Polymer compositions with improved scratch resistance, improved mechanical stability and improved turbidity.

DE602010069563T2Active Publication Date: 2024-11-06BASF SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602010069563
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2009-09-18
Filing Date
2010-09-07
Publication Date
2024-11-06
Estimated Expiration
2030-09-07

AI Technical Summary

Technical Problem

Existing polymer compositions lack improved mechanical properties, specifically flexural modulus, scratch resistance, and haze, which are essential for advanced applications.

Method used

A composition comprising a polypropylene polymer blended with 12 to 1000 ppm of an organic compound A carrying at least two amide functionalities, such as 1,3,5-tris[2,2-dimethylpropionylamino]benzene, and 102 to 500 ppm of a compound B like 1,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol, metal salts of 2,2'-methylene bis(4,6-di-tert-butylphenyl)phosphate, or zinc glycerolate, to enhance mechanical properties and scratch resistance.

Benefits of technology

The composition exhibits improved flexural modulus, scratch resistance, and reduced haze, demonstrating synergistic effects that surpass additive improvements in polypropylene copolymers, making them suitable for various applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to compositions comprising a polymer, an organic compound A carrying at least two amide functionalities and a compound B, and to the use of a mixture of an organic compound A carrying at least two amide functionalities and a compound B for improving the scratch resistance of a polymer.

[0002] WO 04 / 072168 describes compositions comprising a polymer and at least one compound carrying three amide functionalities.

[0003] It was an object of the present invention to provide polymer compositions showing improved mechanical properties, in particular an improved flexural (elastic) modulus, and at the same time improved haze and improved scratch resistance.

[0004] It was another object of the present invention to provide polymer compositions showing an improved scratch resistance.

[0005] These objects are solved by the composition of claim 1 and the use of claim 5.

[0006] The composition of the present invention comprises (i) a polymer, wherein the polymer is a polypropylene homopolymer or a polypropylene random copolymer, alternating or segmented copolymer or block copolymer containing one or more comonomers selected from the group consisting of ethylene, C 4 -C 20 -α-olefin, vinylcyclohexane, vinylcyclohexene, C 4 -C 20 alkandiene, C 5 -C 12 cycloalkandiene and norbornene derivatives; the total amount of propylene and the comonomer(s) being 100 %, (ii) 12 to 1000 parts per million (ppm) of an organic compound A carrying at least two amide functionalities which is 1,3,5-tris[2,2-dimethylpropionylamino]benzene, basec on the total weight of the polymer, and (iii) 102 to 500 parts per million (ppm) of a compound B selected from the group consisting of 1,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol, metal salt of 2,2'-methylene bis(4,6-di-tert-butylphenyl)phosphate, and zinc glycerolate, based on the weight of the polymer.

[0007] The organic compound A carrying at least two amide functionalities is 1,3,5-tris-[2,2-dimethylpropionylamino]benzene, sold under the tradename Ciba ®< Irgaclear ®< XT 386 by Ciba.

[0008] Compound B is selected from the group consisting of 1,3:2,4-bis(3,4-dimethyl-benzylidene)sorbitol, metal salt of 2,2'-methylene bis(4,6-di-tert-butylphenyl)phosphate, and zinc glycerolate. 1,3:2,4-bis(3,4-dimethyl-benzylidene)sorbitol, is for example sold under the tradename Millad ®< 3988 by Milliken.

[0009] Sodium 2,2'-methylene bis(4,6-di-tert-butylphenyl)phosphate, is for example sold under the tradename Ciba ®< Irgastab ®< NA 11 by Ciba,.

[0010] Lithium 2,2'-methylene-bis (4,6-di-tert-butylphenyl) phosphate, is for example sold under the tradename ADK Stab NA 71 by Adeka.

[0011] Aluminium-hydroxy-bis [2,2'-methylene-bis (4,6-di-tert-butylphenyl) phosphate, is for example sold under the tradename ADK Stab NA 21 by Adeka.

[0012] Zinc glycerolate, is for example sold under the tradename Ciba ®< Irgastab ®< NA 287 by Ciba.

[0013] The polymer is a polypropylene homopolymer or a polypropylene random copolymer, alternating or segmented copolymer or block copolymer containing one or more comonomers selected from the group consisting of ethylene, C 4 -C 20 -α-olefin, vinylcyclohexane, vinylcyclohexene, C 4 -C 20 alkandiene, C 5 -C 12 cycloalkandiene and norbornene derivatives; the total amount of propylene and the comonomer(s) being 100 %.

[0014] Polypropylene copolymer also covers long chain branched polypropylene copolymer.

[0015] Examples of suitable C 4 -C 20 -α-olefins are 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene and 4-methyl-1-pentene.

[0016] Examples of suitable C 4 -C 20 alkandienes are hexadiene and octadiene.

[0017] Examples of suitable C 5 -C 12 cycloalkandienes are cyclopentadiene, cyclohexadiene and cyclooctadiene.

[0018] Examples of suitable norbornene derivatives are 5-ethylidene-2-norbornene (ENB), dicyclopentadiene (DCP) and methylene-domethylene-hexahydronaphthaline (MEN).

[0019] A propylene random copolymer comprising ethylene is a preferred synthetic polymer. A propylene / ethylene copolymer contains for example 50 to 99.9%, preferably 80 to 99.9%, in particular 90 to 99.9%, by weight of propylene.

[0020] A propylene copolymer wherein the comonomer is a C 9 -C 20 α-olefin such as e.g. 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene or 1-eicosene; C 9 -C 20 alkandiene, C 9 -C 12 cycloalkandiene or a norbornene derivative such as e.g. 5-ethylidene-2-norbornene (ENB) or methylene-domethylene-hexahydronaphthaline (MEN) contains preferably more than 90 mol%, in particular 90 to 99.9 mol% or 90 to 99 mol%, of propylene.

[0021] A propylene copolymer wherein the comonomer is a C 4 -C 8 α-olefin such as e.g. 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene or 4-methyl-1-pentene; vinylcyclohexane, vinylcyclohexene, C 4 -C 8 alkandiene or C 5 -C 8 cycloalkandiene contains preferably more than 80 mol %, in particular 80 to 99.9 mol % or 80 to 99 mol %, of propylene.

[0022] Additional materials can optionally be added to the compositions of the present invention in a concentration range that does not adversely affect the beneficial effects of the invention. These materials may include lubricants, stabilizers, antioxidants, antibacterial agents, ultraviolet absorbers, thermostabilizers, light stabilizers, neutralizers, antistatic agents, antiblocking agents, heavy metal inactivation agents, flame retardants, lubricants, peroxides, hydrotalcite, foaming agents, elastomers, processing aids, nucleating agents, fillers and the like and mixtures thereof. The amount of the additional materials may be 100 to 10'000 parts per million (ppm) based on the weight of the polymer.

[0023] Examples of fillers are fiber glass, natural fibers such as hemp and kenaf, and inorganic materials such as basalt, talc and wollastonite, (fibrous) magnesium oxysulfate, chalk, kaolin, clay, graphite, graphene, carbon black and other organic or inorganic pigments, titanium dioxide and silicon dioxide.

[0024] The composition of the present invention can comprise 12 to 500, 12 tc 98 or 102 to 500 parts per million (ppm) of the organic compound A carrying at least two amide functionalities, based on the weight of the polymer.

[0025] The composition of the present invention comprises from 102 to 500 parts per million (ppm) of compound B, based on the weight of the polymer.

[0026] Also disclosed is a shaped article obtainable from the composition of the present invention.

[0027] The shaped article can be, for example, obtained from the composition of the present invention by injection blow molding, extrusion, blow molding, rotomolding, in mold decoration (back injection), slush molding, injection molding, co-injection molding, forming, compression molding, pressing, film extrusion (cast film; blown film), fiber spinning (woven, non-woven), drawing (uniaxial, biaxial), annealing, deep drawing, calendaring, mechanical transformation, sintering, coextrusion, coating, lamination, crosslinking (radiation, peroxide, silane), vapor deposition, weld together, glue, vulkanization, thermoforming, pipe extrusion, profile extrusion, sheet extrusion; sheet casting, spin coating, strapping, foaming, recycling / rework, extrusion coating, visbreaking (peroxide, thermal), fiber melt blown, spun bonded, surface treatment (corona discharge, flame, plasma), sterilization (by gamma rays, electron beams), gel-coating, tape extrusion, SMC-process or plastisol.

[0028] A molded article is preferred. The molding is in particular affected by injection, blow, compression, roto-molding or slush-molding or extrusion.

[0029] Examples of shaped article are film fibers, profiles, pipes, bottles, tanks and containers.

[0030] The polymer is a polypropylene homopolymer or a polypropylene random copolymer, alternating or segmented copolymer or block copolymer containing one or more comonomers selected from the group consisting of ethylene, C 4 -C 20 -α-olefin, vinylcyclohexane, vinylcyclohexene, C 4 -C 20 alkandiene, C 5 -C 12 cycloalkandiene and norbornene derivatives; the total amount of propylene and the comonomer(s) being 100%.

[0031] Also part of the invention is the use of a mixture consisting of (ii) 12 to 1000 parts per million (ppm) of an organic compound A carrying at least two amide functionalities is 1,3,5-tris[2,2-dimethylpropionylamino]benzene, based on the total weight of the polymer, and (iii) 102 to 500 parts per million (ppm) of a compound B selected from the group consisting of 1,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol, metal salt of 2,2'-methylene bis(4,6-di-tert-butylphenyl)phosphate, and zinc glycerolate, based on the weight of the polymer, for improving the scratch resistance of a polymer, wherein the polymer is a polypropylene homopolymer or a polypropylene random copolymer, alternating or segmented copolymer or block copolymer containing one or more comonomers selected from the group consisting of ethylene, C 4 -C 20 -α-olefin, vinylcyclohexane, vinylcyclohexene, C 4 -C 20 alkandiene, C 5 -C 12 cycloalkandiene and norbornene derivatives; the total amount of propylene and the comonomer(s) being 100 %.

[0032] The polymer is a polypropylene homopolymer or a polypropylene random copolymer, alternating or segmented copolymer or block copolymer containing one or more comonomers selected from the group consisting of ethylene, C 4 -C 20 -α-olefin, vinylcyclohexane, vinylcyclohexene, C 4 -C 20 alkandiene, C 5 -C 12 cycloalkandiene and norbornene derivatives; the total amount of propylene and the comonomer(s) being 100%.

[0033] The definitions and preferences given above for an organic compound A carrying at least two amide functionalities apply accordingly.

[0034] The polymer compositions of the present invention show improved flexural (elastic) modulus, and at the same time an improved scratch resistance and an improved haze.

[0035] The polymer compositions of the present invention show improved scratch resistance.

[0036] Polymer compositions comprising 1,3,5-tris[2,2-dimethylpropionylamino]benzene, for example as sold under the tradename Ciba ®< Irgaclear ®< XT 386 by Ciba, as compound A, and 1,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol, for example as sold under the tradename Millad ®< 3988 by Milliken, as compound B show an improved scratch resistance and at the same time improved transparency.Examples

[0037] Examples 1 to 11 (examples 6, 7 and 11 are reference examples) and comparative examples 1 to 17

[0038] The nucleating agents and mixtures of nucleating agents as indicated in table 1 are mixed with dry powder form polypropylene (PP), random copolymer comprising 4 mole% ethylene (RD 204 CF from Borealis AG, Vienna, Austria) in a high speed mixer (Mixaco Lab CM 12) and are compounded at 230 ° C to pellets in a twin-extruder (Berstorff ZE 25 X 33 D). Polypropylene (PP) random copolymer without nucleating agents is treated analogously (comparative example 1). Table 1. a< by weight based on the weight of the polypropylene (PP) random copolymer. b< Millad ®< 3988 (Milliken) is 1,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol.Example No.Nucleating agent[ppm] a< Comp. ex. 1--Comp. ex. 2Millad ®< 3988 b< 1800Comp. ex. 3Millad ®< 3988 b< 450Comp.ex. 4Millad ®< 3988 b< 300Comp. ex. 5Millad ®< 3988 b< 150Comp. ex. 6Ciba ®< Irgastab ®< NA 11 c< 450Comp. ex. 7Ciba ®< Irgastab ®< NA 11 c< 300Comp. ex. 8Ciba ®< Irgastab ®< NA 11 c< 150Comp. ex. 9Hyperform ®< HPN-68L d< 230Comp. ex. 10Hyperform ®< HPN-68L d< 150Comp. ex. 11Ciba ®< Irgastab ®< NA 287 e< 230Comp. ex. 12Ciba ®< Irgastab ®< NA 287 e< 150Comp. ex. 13Ciba ®< Irgastab ®< NA 04 f< 850Comp.ex. 14Ciba ®< Irgaclear ®< XT 386 g< 450Comp. ex. 15Ciba ®< Irgaclear ®< XT 386 g< 300Comp. ex. 16Ciba ®< Irgaclear ®< XT 386 g< 230Comp. ex. 17Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 1Millad ®< 3988b Ciba ®< Irgaclear ®< XT 386 g< 300 150Ex. 2Millad ®< 3988b150Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 3Ciba ®< Irgastab ®< NA 11 c< 300Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 4Ciba ®< Irgastab ®< NA 11 c< 150Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 6Hyperform ®< HPN-68L d< 75Ciba ®< Irgaclear ®< XT 386 g< 155Ex. 7Hyperform ®< HPN-68L d< 75Ciba ®< Irgaclear ®< XT 386 g< 75Ex. 8Ciba ®< Irgastab ®< NA 287 e< 75Ciba ®< Irgaclear ®< XT 386 g< 75Ex. 9Ciba ®< Irgastab ®< NA 287 e< 75Ciba ®< Irgaclear ®< XT 386 g< 155Ex. 11Ciba ®< Irgastab ®< NA 04 f< 850Ciba ®< Irgaclear ®< XT 386 g< 150 c< Ciba ®< Irgastab ®< NA 11 is sodium 2,2'-methylene bis(4,6-di-tert-butylphenyl)phosphate of formula

[0039]

[0040] d< Hyperform ®< HPN-68L (Milliken) is a blend of the following compounds: 80% by weight cis-endo-bicyclo[2.2.1]heptane-2,3-dicarboxylic acid, disodium salt, 10% by weight (Z)-13-docosenamide and 10% by weight amorphous silicon dioxide. e< Ciba ®< Irgastab ®< NA 287 is zinc glycerolate. f< Ciba ®< Irgastab ®< NA 04 is sodium benzoate. g< Ciba ®< Irgaclear ®< XT 386 is 1,3,5-tris[2,2-dimethylpropionylamino]benzene.Testing of flexural modulus

[0041] The pellets of examples 1 to 4, 6 to 9 and 11, and comparative examples 1 to 4, 6, 7 and 9 to 13, 16 and 17 are injection molded at 200 ° C to obtain 4 mm thick bars of 10 mm width and 80 mm length.

[0042] The bars are subjected to a "3-point bending test" according to ISO 178. The flexural modulus or elastic modulus (E f ) is determined from the linear regime of the stress-strain curves. The flexural or elastic modulus is a measure of the stiffness of the polymer material. The results are outlined in table 2. Table 2. a-g< see table 1.Example No.Nucleating agent[ppm] a< flexural modulus [MPa]Calculated flexural modulus h< [MPa]Comp. ex. 1--1039-Comp. ex. 2Millad ®< 3988 b< 18001239-Comp. ex. 3Millad ®< 3988 b< 4501060Comp.ex. 4Millad ®< 3988 b< 3001075-Comp. ex. 6Ciba ®< Irgastab ®< NA 11 c< 4501415-Comp. ex. 7Ciba ®< Irgastab ®< NA 11 c< 3001411-Comp. ex. 9Hyperform ®< HPN-68L d< 2301249-Comp. ex. 10Hyperform ®< HPN-68L d< 1501250-Comp. ex. 11Ciba ®< Irgastab ®< NA 287 e< 2301170-Comp. ex. 12Ciba ®< Irgastab ®< NA 287 e< 1501166-Comp. ex. 13Ciba ®< Irgastab ®< NA 04 f< 8501275-Comp. ex. 16Ciba ®< Irgaclear ®< XT 386 g< 2301339-Comp. ex. 17Ciba ®< Irgaclear ®< XT 386 g< 1501233-Ex. 1Millad ®< 3988 b< 3001331-Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 2Millad ®< 3988 b< 1501275-Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 3Ciba ®< Irgastab ®< NA 11 c< 3001444-Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 4Ciba ®< Irgastab ®< NA 11 c< 1501434-Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 6Hyperform ®< HPN-68L d< 7513501309.3Ciba ®< Irgaclear ®< XT 386 g< 155Ex. 7Hyperform ®< HPN-68L d< 7512561241.5Ciba ®< Irgaclear ®< XT 386 g< 75Ex. 8Ciba ®< Irgastab ®< NA 287 e< 7512401199.5Ciba ®< Irgaclear ®< XT 386 g< 75Ex. 9Ciba ®< Irgastab ®< NA 287 e< 7513661283.2Ciba ®< Irgaclear ®< XT 386 g< 155Ex. 11Ciba ®< Irgastab ®< NA 04 f< 8501274-Ciba ®< Irgaclear ®< XT 386 g< 150 h< the calculated flexural (elastic) modulus of n ppm of a mixture of a% A and b% B = a% x "flexural (elastic) modulus of n ppm A" + b% x "flexural (elastic) modulus of n ppm B". For example the calculated flexural (elastic) modulus of 230 ppm of a mixture of 33% Hyperform ®< HPN-68L and 67% Ciba ®< Irgaclear ®< XT 386 (example 6) 33% x "flexural (elastic) modulus of 230 ppm Hyperform ®< HPN-68L" + 67% x "flexural (elastic) modulus of 230 ppm Ciba ®< Irgaclear ®< XT 386" = 33% x 1249 + 67% x 1339 = 1309.3.

[0043] As can be seen from table 2 polypropylene copolymer compositions comprising 75 ppm Hyperform ®< HPN-68L and 155 ppm Ciba ®< Irgaclear ®< XT 386 (example 6) show an improved (higher) flexural (elastic) modulus, namely 1350 MPa, compared with the polypropylene copolymer compositions comprising 230 ppm Hyperform ®< HPN-68L (flexural modulus = 1249 MPa, comparative example 9) or 230 ppm Ciba ®< Irgaclear ®< XT 386 (flexural modulus = 1339 MPa, comparative example 16). The effect is not of additive nature, but synergistic as can be seen when comparing the measured flexural (elastic) modulus (1350 MPa) with the calculated flexural (elastic) modulus (1309.3 MPa).

[0044] Table 2 shows the same effect regarding the flexural (elastic) modulus of the polypropylene copolymer compositions comprising 75 ppm Hyperform ®< HPN-68L and 75 ppm Ciba ®< Irgaclear ®< XT 386 (example 7), 75 ppm Ciba ®< Irgastab ®< NA 287 and 75 ppm Ciba ®< Irgaclear ®< XT 386 (example 8), respectively, 75 ppm Ciba ®< Irgastab ®< NA 287 and 155 ppm Ciba ®< Irgaclear ®< XT 386 (example 9).Testing of haze

[0045] The pellets of examples 1 to 4, 6 to 9, and 11, and comparative examples 1 to 7 and 9 to 17 are molded at 230 ° C to plaques with a thickness of 1 mm using a standard injection molding machine (Engel HL 60).

[0046] The hazes the plaques are analysed using a Haze-gard plus instrument (BYK Gardner Gmbh Germany) in accordance with ASTM standard D1003. In this test, haze is commonly defined as that portion of visible light that is scattered at wider angles (2.5° <θ<90° ) and is a measure for the turbidity of a sample.

[0047] The results are outlined in table 3. Table 3. a-g< see table 1.Example No.Nucleating agent[ppm] a< Haze [%]Calculated Haze i< [%]Comp. ex. 1--40.32-Comp. ex. 2Millad ®< 3988 b< 180012.16-Comp. ex. 3Millad ®< 3988 b< 45038.36-Comp.ex. 4Millad ®< 3988 b< 30039.50-Comp. ex. 5Millad ®< 3988 b< 15039.06-Comp. ex. 6Ciba ®< Irgastab ®< NA 11 c< 45023.28-Comp. ex. 7Ciba ®< Irgastab ®< NA 11 c< 30025.74-Comp. ex. 9Hyperform ®< HPN-68L d< 23047.90-Comp. ex. 10Hyperform ®< HPN-68L d< 15052.90-Comp. ex. 11Ciba ®< Irgastab ®< NA 287 e< 23052.16-Comp. ex. 12Ciba ®< Irgastab ®< NA 287 e< 15053.88-Comp. ex. 13Ciba ®< Irgastab ®< NA 04 f< 85039.38-Comp. ex. 14Ciba ®< Irgaclear ®< XT 386 g< 45012.66-Comp. ex. 15Ciba ®< Irgaclear ®< XT 386 g< 30013.28-Comp. ex. 16Ciba ®< Irgaclear ®< XT 386 g< 23014.90-Comp. ex. 17Ciba ®< Irgaclear ®< XT 386 g< 15014.50-Ex. 1Millad ®< 3988 b< 30011.0629.90Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 2Millad ®< 3988 b< 15012.4426.39Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 3Ciba ®< Irgastab ®< NA 11 c< 30018.7219.78Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 4Ciba ®< Irgastab ®< NA 11 c< 15018.6419.51Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 6Hyperform ®< HPN-68L d< 7515.3025.80Ciba ®< Irgaclear ®< XT 386 g< 155Ex. 7Hyperform ®< HPN-68L d< 7533.0033.70Ciba ®< Irgaclear ®< XT 386 g< 75Ex. 8Ciba ®< Irgastab ®< NA 287 e< 7527.4834.19Ciba ®< Irgaclear ®< XT 386 g< 75Ex. 9Ciba ®< Irgastab ®< NA 287 e< 7516.1827.2Ciba ®< Irgaclear ®< XT 386 g< 155Ex. 11Ciba ®< Irgastab ®< NA 04 f< 85030.42-Ciba ®< Irgaclear ®< XT 386 g< 150 i< the calculated Haze of n ppm of a mixture of a% A and b% B = a% x "Haze of n ppm A" + b% x "Haze of n ppm B".

[0048] For example the calculated Haze of 230 ppm of a mixture of 33% Hyperform ®< HPN-68L and 67% Ciba ®< Irgaclear ®< XT 386 (example 6) = 33% x "Haze of 230 ppm Hyperform ®< HPN-68L" + 67% x "Haze of 230 ppm Ciba ®< Irgaclear ®< XT 386" = 33% x 47.90 + 67% x 14.90 = 25.8.

[0049] As can be seen from table 3 polypropylene copolymer compositions comprising 300 ppm Millad ®< 3988 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 1) show an improved (lower) haze, namely 11.06, compared with the polypropylene copolymer compositions comprising 450 ppm Millad ®< 3988 (haze = 38.36, comparative example 3) or 450 ppm Ciba ®< Irgaclear ®< XT 386 (haze = 12.66, comparative example 14). The effect is not of additive nature, but synergistic as can be seen when comparing the measured haze (11.06) with the calculated haze (29.90).

[0050] Table 3 shows the same effect regarding haze of the polypropylene copolymer compositions comprising 150 ppm Millad ®< 3988 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 2), 300 ppm Ciba ®< Irgastab ®< NA 11 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 3), 150 ppm Ciba ®< Irgastab ®< NA 11 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 4), 75 ppm Hyperform ®< HPN-68L and 155 ppm Ciba ®< Irgaclear ®< XT 386 (example 6), 75 ppm Hyperform ®< HPN-68L and 75 ppm Ciba ®< Irgaclear ®< XT 386 (example 7), 75 ppm Ciba ®< Irgastab ®< NA 287 and 75 ppm Ciba ®< Irgaclear ®< XT 386 (example 8), respectively, 75 ppm Ciba ®< Irgastab ®< NA 287 and 155 ppm Ciba ®< Irgaclear ®< XT 386 (example 9).Measurement of Scratch Resistance

[0051] The pellets of examples 1, 2, 4, 5, 10 and 11, and comparative examples 1, 2, 4, 5, 8, 10, 12, 13 and 17 are molded at 230 ° C to plaques with a thickness of 1 mm using a standard injection molding machine (Engel HL 60). The scratch resistance of the plaques is analysed with an Erichson Sratch Tester by moving a sharp tip of 1 mm radius over the plaques at a velocity of 1000 mm / min and a normal force of 10 N. Evaluation of the scratch resistance is assessed by visual inspection as the transparent or translucent nature of the samples prevented changes in L* to be determined. The results are outlined in table 4. The transparency is also analysed by visual inspection. The results are also outlined in table 4. Table 4. a-g< see table 1.Example No.Nucleating agent[ppm] a< Scratch resistanceTransparencyComp. ex. 1--lowlowComp. ex. 2Millad ®< 3988 b< 1800lowhighComp.ex. 4Millad ®< 3988 b< 300mediumlowComp. ex. 5Millad ®< 3988 b< 150mediumlowComp. ex. 8Ciba ®< Irgastab ®< NA 11 c< 150mediumlowComp. ex. 10Hyperform ®< HPN-68L d< 150mediumlowComp. ex. 12Ciba ®< Irgastab ®< NA 287 e< 150mediumlowComp. ex. 13Ciba ®< Irgastab ®< NA 04 f< 850mediumlowComp. ex. 17Ciba ®< Irgaclear ®< XT 386 g< 150mediumhighEx. 1Millad ®< 3988 b< 300highhighCiba ®< Irgaclear ®< XT 386 g< 150Ex. 2Millad ®< 3988 b< 150highhighCiba ®< Irgaclear ®< XT 386 g< 150Ex. 4Ciba ®< Irgastab ®< NA 11 c< 150highmediumCiba ®< Irgaclear ®< XT 386 g< 150Ex. 5Hyperform ®< HPN-68L d< 150highmediumCiba ®< Irgaclear ®< XT 386 g< 150Ex. 10Ciba ®< Irgastab ®< NA 287 e< 150highmediumCiba ®< Irgaclear ®< XT 386 g< 150Ex. 11Ciba ®< Irgastab ®< NA 04 f< 850highmediumCiba ®< Irgaclear ®< XT 386 g< 150

[0052] As can be seen from table 4, polypropylene copolymer compositions comprising 300 ppm Millad ®< 3988 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 1),150 ppm Millad ®< 3988 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 2), 150 ppm Ciba ®< Irgastab ®< NA 11 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 4), 150 ppm Hyperform ®< HPN-68L and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 5), 150ppm Ciba ®< Irgastab ®< NA 287 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 10), respectively, 850 ppm Ciba ®< Irgastab ®< NA 04and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 11) all show a high scratch resistance. The polypropylene copolymer compositions comprising 300 ppm Millad ®< 3988 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 1), respectively, 150 ppm Millad ®< 3988 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 2) also show a high transparency.Examples 12 to 14, and comparative examples 18 to 22

[0053] The nucleating agents and mixtures of nucleating agents as indicated in table 5 are mixed with dry powder form polypropylene (PP) random copolymer comprising 4 mole% ethylene (RD 204 MFI 8 from Borealis AG, Vienna, Austria) in a high speed mixer (Mixaco Lab CM 12) and are compounded at 230 ° C to pellets in a twin-extruder (Berstorff ZE 25 X 46 D). Table 5. a< by weight based on the weight of the polypropylene (PP) random copolymer. g< Ciba ®< Irgaclear ®< XT 386 is 1,3,5-tris[2,2-dimethylpropionyl-amino]benzene. j< ADK Stab NA 71 (Adeka) is lithium 2,2'-methylene-bis (4,6-di-tert-butylphenyl) phosphate of formulaExample No.Nucleating agent[ppm] a< Comp. ex. 18ADK Stab NA 71 j< 450Comp. ex. 19ADK Stab NA 71 j< 300Comp. ex. 20ADK Stab NA 21 k< 450Comp.ex. 21Ciba ®< Irgaclear ®< XT 386 g< 450Comp. ex. 22Ciba ®< Irgaclear ®< XT 386 g< 300Ex. 12ADK Stab NA 71 j< 150Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 13ADK Stab NA 71 j< 300Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 14ADK Stab NA 21 k< 300Ciba ®< Irgaclear ®< XT 386 g< 150

[0054] k< ADK Stab NA 21 (Adeka) is a mixture of 70% aluminium-hydroxy-bis [2,2'-methylene-bis (4,6-di-tert-butylphenyl) phosphate] and 30% lithium myristate.Measurement of flexural modulus

[0055] The pellets of examples 12 to 13, and comparative examples 18 to 22 are injection molded at 200 ° C to obtain 4 mm thick bars of 40 mm width and 80 mm length.

[0056] The bars are subjected to a "3-point bending test" according to ISO 178. The flexural modulus or elastic modulus (E f ) is determined from the linear regime of the stress-strain curves. The flexural or elastic modulus is a measure of the stiffness of the polymer material. The results are outlined in table 6. Table 6. a, g, j and k< see table 5.Example No.Nucleating agent[ppm] a< flexural modulus [MPa]Calculated flexural modulus h< [MPa]Comp. ex. 18ADK Stab NA 71 j< 4501113-Comp. ex. 19ADK Stab NA 71 j< 3001110-Comp. ex. 20ADK Stab NA 21 k< 4501083Comp.ex. 21Ciba ®< Irgaclear ®< XT 386 g< 4501147-Comp. ex. 22Ciba ®< Irgaclear ®< XT 386 g< 3001165-Ex. 12ADK Stab NA 71 j< 15011771137.5Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 13ADK Stab NA 71 j< 30011441124.2Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 14ADK Stab NA 21 k< 30011721104.1Ciba ®< Irgaclear ®< XT 386 g< 150 h< the calculated flexural (elastic) modulus of n ppm of a mixture of a% A and b% B = a% x "flexural (elastic) modulus of n ppm A" + b% x "flexural (elastic) modulus of n ppm B".

[0057] For example the calculated flexural (elastic) modulus of 300 ppm of a mixture of 50% ADK Stab NA 71 j< and 50% Ciba ®< Irgaclear ®< XT 386 (example 12) = 50% x "flexural (elastic) modulus of 300 ppm ADK Stab NA 71 j< " + 50% x "flexural (elastic) modulus of 300 ppm Ciba ®< Irgaclear ®< XT 386" = 50% x 1110 + 50% x 1165 = 1137.5.

[0058] As can be seen from table 6 polypropylene copolymer compositions comprising 150 ppm ADK Stab NA 71 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 12) show an improved (higher) flexural (elastic) modulus, namely 1177 MPa, compared with the polypropylene copolymer compositions comprising 300 ppm ADK Stab NA 71 (flexural modulus = 1110 MPa, comparative example 19) or 300 ppm Ciba ®< Irgaclear ®< XT 386 (flexural modulus = 1165 MPa, comparative example 22). The effect is not of additive nature, but synergistic as can be seen when comparing the measured flexural (elastic) modulus (1177 MPa) with the calculated flexural (elastic) modulus (1137.5 MPa).

[0059] Table 6 shows the same effect regarding the flexural (elastic) modulus of the polypropylene copolymer compositions comprising 300 ppm ADK Stab NA 71 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 13), respectively, 300 ppm ADK Stab NA 21 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 14).Measurement of haze

[0060] The pellets of examples 12 to 13, and comparative examples 18 to 22 are molded at 200 ° C to plaques with a thickness of 2 mm using a standard injection molding machine (Arburg 320S).

[0061] The hazes the plaques are analysed using a Haze-gard plus instrument (BYK Gardner Gmbh Germany) in accordance with ASTM standard D1003. In this test, haze is commonly defined as that portion of visible light that is scattered at wider angles (2.5° <θ<90° ) and is a measure for the turbidity of a sample.

[0062] The results are outlined in table 7. Table 7. a, g, j and k< see table 5.Example No.Nucleating agent[ppm] a< Haze [%]Calculated Haze i< Comp. ex. 18ADK Stab NA 71 j< 45076.46Comp. ex. 19ADK Stab NA 71 j< 30078.60Comp. ex. 20ADK Stab NA 21 k< 45070.04Comp.ex. 21Ciba ®< Irgaclear ®< XT 386 g< 45076.84Comp. ex. 22Ciba ®< Irgaclear ®< XT 386 g< 30059.98Ex. 12ADK Stab NA 71 j< 15041.0069.29Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 13ADK Stab NA 71 j< 30042.9076.58Ciba ®< Irgaclear ®< XT 386 g< 150Ex. 14ADK Stab NA 21 k< 30040.4672.28Ciba ®< Irgaclear ®< XT 386 g< 150 i< the calculated Haze of n ppm of a mixture of a% A and b% B = a% x "Haze of n ppm A" + b% x "Haze of n ppm B".

[0063] For example the calculated Haze of 300 ppm of a mixture of 50% ADK Stab NA 71 and 50% Ciba ®< Irgaclear ®< XT 386 (example 12) = 50% x "Haze of 300 ADK Stab NA 71" + 50% x "Haze of 300 ppm Ciba ®< Irgaclear ®< XT 386" = 50% x 78.60 + 50% x 59.98 = 69.29

[0064] As can be seen from table 7 polypropylene copolymer compositions comprising 150 ppm ADK Stab NA 71 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 12) show an improved (lower) haze, namely 41.00, compared with the polypropylene copolymer compositions comprising 300 ppm ADK Stab NA 71 (haze = 78.60, comparative example 19) or 300 ppm Ciba ®< Irgaclear ®< XT 386 (haze = 59.98, comparative example 22). The effect is not of additive nature, but synergistic as can be seen when comparing the measured haze (41.00) with the calculated haze (69.29).

[0065] Table 7 shows the same effect regarding haze of the polypropylene copolymer compositions comprising 300 ppm ADK Stab NA 71 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 13), respectively, 300 ppm ADK Stab NA 21 and 150 ppm Ciba ®< Irgaclear ®< XT 386 (example 14)Examples 15 to 17, and comparative examples 23 to 27

[0066] The nucleating agents and mixtures of nucleating agents as indicated in table 8 are mixed with dry powder form polypropylene (PP) homopolymer (Moplen HP 500N, MFI 12) in a high speed mixer (Mixaco Lab CM 12) and are compounded at 230 ° C to pellets in a twin-extruder (Berstorff ZE 25 X 46 D). Table 8. a< by weight based on the weight of the polypropylene (PP) homopolymer. g, j and k< see table 5.Example No.Nucleating agent[ppm] a< Comp. ex. 23ADK Stab NA 71 j< 480Comp. ex. 24ADK Stab NA 71 j< 330Comp. ex. 25ADK Stab NA 21 k< 480Comp.ex. 26Ciba ®< Irgaclear ®< XT 386 g< 480Comp. ex. 27Ciba ®< Irgaclear ®< XT 386 g< 330Ex. 15ADK Stab NA 71 j< 150Ciba ®< Irgaclear ®< XT 386 g< 180Ex. 16ADK Stab NA 71 j< 300Ciba ®< Irgaclear ®< XT 386 g< 180Ex. 17ADK Stab NA 21 k< 300Ciba ®< Irgaclear ®< XT 386 g< 180 Measurement of flexural modulus

[0067] The pellets of examples 15 to 17, and comparative examples 23 to 27 are injection molded at 200 ° C (Arburg 320S) to obtain 4 mm thick bars of 40 mm width and 80 mm length.

[0068] The bars are subjected to a "3-point bending test" according to ISO 178. The flexural modulus or elastic modulus (E f ) is determined from the linear regime of the stress-strain curves. The flexural or elastic modulus is a measure of the stiffness of the polymer material. The results are outlined in table 9. Table 9. a< see table 8. g, j and k< see table 5.Example No.Nucleating agent[ppm] a< flexural modulus [M Pa]Calculated flexural modulus h< [MPa]Comp. ex. 23ADK Stab NA 71 j< 4801736Comp. ex. 24ADK Stab NA 71 j< 3301727Comp. ex. 25ADK Stab NA 21 k< 4801714Comp.ex. 26Ciba ®< Irgaclear ®< XT 386 g< 4801803Comp. ex. 27Ciba ®< Irgaclear ®< XT 386 g< 3301786Ex. 15ADK Stab NA 71 j< 15018161759.5Ciba ®< Irgaclear ®< XT 386 g< 180Ex. 16ADK Stab NA 71 j< 30018181760.8Ciba ®< Irgaclear ®< XT 386 g< 180Ex. 17ADK Stab NA 21 k< 30018311746.9Ciba ®< Irgaclear ®< XT 386 g< 180 h< the calculated flexural (elastic) modulus of n ppm of a mixture of a% A and b% B = a% x "flexural (elastic) modulus of n ppm A" + b% x "flexural (elastic) modulus of n ppm B".

[0069] For example the calculated flexural (elastic) modulus of 330 ppm of a mixture of 45% ADK Stab NA 71 and 55% Ciba ®< Irgaclear ®< XT 386 (example 15) = 45% x "flexural (elastic) modulus of 330 ppm ADK Stab NA 71" + 55% x "flexural (elastic) modulus of 330 ppm Ciba ®< Irgaclear ®< XT 386" = 45% x 1727 + 55% x 1786 = 1759.5.

[0070] As can be seen from table 9 polypropylene homopolymer compositions comprising 150 ppm ADK Stab NA 71 and 180 ppm Ciba ®< Irgaclear ®< XT 386 (example 15) show an improved (higher) flexural (elastic) modulus, namely 1816 MPa, compared with the polypropylene homopolymer compositions comprising 330 ppm ADK Stab NA 71 (flexural modulus = 1727 MPa, comparative example 24) or 330 ppm Ciba ®< Irgaclear ®< XT 386 (flexural modulus = 1786 MPa, comparative example 27). The effect is not of additive nature, but synergistic as can be seen when comparing the measured flexural (elastic) modulus (1816 MPa) with the calculated flexural (elastic) modulus (1759.5 MPa).

[0071] Table 9 shows the same effect regarding the flexural (elastic) modulus of the polypropylene homopolymer compositions comprising 150 ppm ADK Stab NA 71 and 180 ppm Ciba ®< Irgaclear ®< XT 386 (example 15), 300 ppm ADK Stab NA 71 and 180 ppm Ciba ®< Irgaclear ®< XT 386 (example 16), respectively, 300 ppm ADK Stab NA 21 and 180 ppm Ciba ®< Irgaclear ®< XT 386 (example 17).Measurement of haze

[0072] The pellets of examples 15 to 17, and comparative examples 23 to 27 are molded at 200 ° C to plaques with a thickness of 2 mm using a standard injection molding machine (Arburg 320S).

[0073] The hazes the plaques are analysed using a Haze-gard plus instrument (BYK Gardner Gmbh Germany) in accordance with ASTM standard D1003. In this test, haze is commonly defined as that portion of visible light that is scattered at wider angles (2.5° <θ<90° ) and is a measure for the turbidity of a sample.

[0074] The results are outlined in table 10. Table 10. a< see table 8. g, j and k< see table 5.Example No.Nucleating agent[ppm] a< Haze [%]Calculated Haze i< [%]Comp. ex. 23ADK Stab NA 71 j< 48083.3-Comp. ex. 24ADK Stab NA 71 j< 33086.5-Comp. ex. 25ADK Stab NA 21 k< 48079.9-Comp.ex. 26Ciba ®< Irgaclear ®< XT 386 g< 48085.5-Comp. ex. 27Ciba ®< Irgaclear ®< XT 386 g< 33086.0-Ex. 15ADK Stab NA 71 j< 15074.186.2Ciba ®< Irgaclear ®< XT 386 g< 180Ex. 16ADK Stab NA 71 j< 30069.784.1Ciba ®< Irgaclear ®< XT 386 g< 180Ex. 17ADK Stab NA 21 k< 30065.382.0Ciba ®< Irgaclear ®< XT 386 g< 180 i< the calculated Haze of n ppm of a mixture of a% A and b% B = a% x "Haze of n ppm A" + b% x "Haze of n ppm B".

[0075] For example the calculated Haze of 330 ppm of a mixture of 45% ADK Stab NA 71 and 55% Ciba ®< Irgaclear ®< XT 386 (example 15) = 45% x "Haze of 300 ADK Stab NA 71" + 55% x "Haze of 300 ppm Ciba ®< Irgaclear ®< XT 386" = 45% x 86.5 + 55% x 86.0 = 86.2

[0076] As can be seen from table 10 polypropylene homopolymer compositions comprising 150 ppm ADK Stab NA 71 and 180 ppm Ciba ®< Irgaclear ®< XT 386 (example 15) show an improved (lower) haze, namely 74.1, compared with the polypropylene homopolymer compositions comprising 330 ppm ADK Stab NA 71 (haze = 86.5, comparative example 24) or 330 ppm Ciba ®< Irgaclear ®< XT 386 (haze = 86.0, comparative example 27). The effect is not of additive nature, but synergistic as can be seen when comparing the measured haze (74.1) with the calculated haze (86.2).

[0077] Table 10 shows the same effect regarding haze of the polypropylene homopolymer compositions comprising 150 ppm ADK Stab NA 71 and 180 ppm Ciba ®< Irgaclear ®< XT 386 (example 15), 300 ppm ADK Stab NA 71 and 180 ppm Ciba ®< Irgaclear ®< XT 386 (example 16), respectively, 300 ppm ADK Stab NA 21 and 180 ppm Ciba ®< Irgaclear ®< XT 386 (example 17).Examples 18 to 21

[0078] The mixtures of nucleating agents as indicated in table 11 are mixed with dry powder form polypropylene (PP) random copolymer comprising 4 mole% ethylene (RD 204 CF from Borealis AG, Vienna, Austria) in a high speed mixer (Mixaco Lab CM 12). Under constant nitrogen purge, the mixture is then intensely melt-compounded at 240 ° C for 3 minutes at 100 rpm screw speed using a co-rotating laboratory twin-screw extruder (15 cm 3< Micro-Compounder of DSM Xplore). The homogeneous melt is subsequently transferred to a 10 cm 3< Micro-Injector (DSM Xplore), where the melt is injected into a polished mold at a pressure of about 8 bars at 50 ° C mold temperature. The resulting circular disks have a diameter of 40 mm and a thickness of 1.0 mm.Measurement of haze

[0079] The hazes the plaques are analysed using a Haze-gard plus instrument (BYK Gardner Gmbh Germany) at room temperature in accordance with ASTM standard D1003. All haze values are measured at least 24 hours after injection molding.

[0080] The results are outlined in table 11. Table 11. a, g and j< see table 5. l< Precursor of ADK Stab NA 71 isExample No.Nucleating agent[ppm] a< Haze [%]Ex. 18Ciba ®< Irgaclear ®< XT 386 g< 10020.1ADK Stab NA 71 j< 600Ex. 19Ciba ®< Irgaclear ®< XT 386 g< 20022.9ADK Stab NA 71 j< 1200Ex. 20Ciba ®< Irgaclear ®< XT 386 g< 10019.6Precursor of ADK Stab NA 71 l< lithium stearate600360Ex. 21Ciba ®< Irgaclear ®< XT 386 g< 20016.7Precursor of ADK Stab NA 71 l< lithium stearate1200720

Claims

1. A composition comprising (i) a polymer, wherein the polymer is a polypropylene homopolymer or a polypropylene random copolymer, alternating or segmented copolymer or block copolymer containing one or more comonomers selected from the group consisting of ethylene, C4-C20-α-olefin, vinylcyclohexane, vinylcyclohexene, C4-C20alkandiene, C5-C12cycloalkandiene and norbornene derivatives; the total amount of propylene and the comonomer(s) being 100 %, (ii) 12 to 1000 parts per million (ppm) of an organic compound A carrying at least two amide functionalities which is 1,3,5-tris[2,2-dimethylpropionylamino]benzene, basec on the total weight of the polymer, and (iii) 102 to 500 parts per million (ppm) of a compound B selected from the group consisting of 1,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol, metal salt of 2,2'-methylene bis(4,6-di-tert-butylphenyl)phosphate, and zinc glycerolate, based on the weight of the polymer.

2. The composition of claim 1, wherein compound B is 1,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol.

3. The composition of claim 1, wherein the metal salt of 2,2'-methylene bis(4,6-di-tert-butyl phenyl) phosphate is lithium 2,2'-methylene bis(4,6-di-tert-butyl phenyl) phosphate.

4. The composition of claim 1, wherein compound B is zinc glycerolate.

5. Use of a mixture consisting of (ii) 12 to 1000 parts per million (ppm) of an organic compound A carrying at least two amide functionalities which is 1,3,5-tris[2,2-dimethylpropionylamino]benzene, basec on the total weight of the polymer, and (iii) 102 to 500 parts per million (ppm) of a compound B selected from the group consisting of 1,3:2,4-bis(3,4-dimethylbenzylidene)sorbitol, metal salt of 2,2'-methylene bis(4,6-di-tert-butylphenyl)phosphate, and zinc glycerolate, based on the weight of the polymer, for improving the scratch resistance of a polymer, wherein the polymer is a polypropylene homopolymer or a polypropylene random copolymer, alternating or segmented copolymer or block copolymer containing one or more comonomers selected from the group consisting of ethylene, C4-C20-α-olefin, vinylcyclohexane, vinylcyclohexene, C4-C20alkandiene, C5-C12cycloalkandiene and norbornene derivatives; the total amount of propylene and the comonomer(s) being 100 %.