MATERIAL CONTAINING A STACK WITH A THIN ZINC-BASED DIELECTRIC OXIDE COATING AND METHOD FOR APPLYING THIS MATERIAL

DE602020041400T2Active Publication Date: 2024-11-13SAINT GOBAIN VITRAGE SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602020041400
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-29
Filing Date
2020-11-27
Publication Date
2024-11-13
Estimated Expiration
2040-11-27

AI Technical Summary

Technical Problem

Existing materials with metallic functional layers for infrared and solar radiation reflection struggle to achieve low resistance per square and high light transmission while maintaining homogeneity in appearance after heat or radiation treatment, without degrading optical and thermal properties.

Method used

A glass substrate coated with a stack of thin layers, including a metallic functional layer sandwiched between anti-reflective coatings, where a thin zinc-based oxide layer is placed under and over the metallic layer, with silicon nitride dielectric layers acting as barriers, optimized for thickness and composition to minimize absorption and prevent substrate penetration.

Benefits of technology

The configuration achieves low resistance per square and high light transmission with improved thermal properties and homogeneity in both transmission and reflection, even after heat or radiation treatment.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a material comprising a glass substrate coated on one side with a stack of thin layers with reflection properties in the infrared and / or in solar radiation comprising at least one metallic functional layer, in particular based on silver or a metallic alloy containing silver and at least two anti-reflective coatings, said anti-reflective coatings each comprising at least one dielectric layer, said functional layer being arranged between the two anti-reflective coatings.

[0002] In this type of stack, the single, or each, metallic functional layer is thus arranged between two anti-reflective coatings, each generally comprising several layers which are each made of a dielectric material of the nitride type, and in particular silicon or aluminum nitride, or oxide. From an optical point of view, the purpose of these coatings which surround the or each metallic functional layer is to "antireflect" this metallic functional layer.

[0003] A prior configuration is known from European patent application No. EP 718 250 in which, on the one hand, a zinc oxide-based layer is located just under and in contact with the metallic functional layer, towards the substrate, then a silicon nitride-based layer under and in contact with this zinc oxide-based layer and in which, on the other hand, a zinc oxide-based layer is located above, opposite the substrate, then a dielectric layer, for example based on silicon nitride, is located on and in contact with this zinc oxide-based layer.

[0004] This document teaches in particular that the material comprising this stack of thin layers and the substrate on one face of which it is located can undergo a stressful heat treatment, such as bending, quenching or annealing, which leads to a structural modification of the substrate without degrading the optical and thermal properties of the stack.

[0005] International patent application No. WO 2018 / 024985 discloses a functional monolayer stack configuration having, under this functional layer, starting from the substrate, a primary dielectric sub-layer of silicon-based nitride Si 3 N 4 or silicon-zirconium having a particular atomic ratio of Zr to the sum of (Si + Zr), then a sub-layer of zinc-based oxide ZnO which is located under and in contact with said functional layer, then the metallic functional layer, then a metallic over-blocking layer of NiCr, then a dielectric coating. International patent application No. WO 2014 / 177798 discloses a functional bilayer stack configuration with a metallic over-blocking layer located just above and in contact with each metallic functional layer.

[0006] It is also known from international patent application No. WO 2010 / 142926 to apply a radiation treatment after the deposition of a stack comprising a functional layer to reduce the emissivity or improve the optical properties of this stack, in particular by providing an absorbent layer in the terminal layer of the stack. The use of an absorbent terminal layer makes it possible to increase the absorption of radiation by the stack and to reduce the power required for the treatment. As the terminal layer oxidizes during the treatment and becomes transparent, the optical characteristics of the stack after treatment are interesting (a high light transmission can in particular be obtained).

[0007] Unlike the heat treatment mentioned above, this radiation treatment of the stack does not structurally modify the substrate.

[0008] The invention is based on the discovery of a particular configuration of layers framing a metallic functional layer which makes it possible to reduce the resistance per square at identical functional layer thickness, or even to reduce the functional layer thickness to obtain improved thermal properties, and this after a heat treatment of the material or a radiation treatment of the stack according to known techniques.

[0009] An aim of the invention is thus to succeed in developing a new type of stack of layers with one or more functional layers, a stack which has, after heat treatment of the material or treatment of the stack by radiation, a low resistance per square (and therefore a low emissivity), a high light transmission, as well as a homogeneity of appearance, both in transmission and in reflection.

[0010] In the particular configuration according to the invention, it is proposed on the one hand to arrange a very thin layer of zinc-based oxide just under and in contact with the metallic functional layer, in the direction of the substrate, then to arrange, in the direction of the substrate, a layer based on silicon nitride under and in contact with this very thin layer of zinc-based oxide and on the other hand to arrange a thin layer of zinc-based oxide just above and in contact with the metallic functional layer, opposite the substrate, then to arrange a dielectric layer, for example of silicon-based nitride, on (in contact or not) this thin layer of zinc-based oxide.

[0011] The invention thus relates, in its broadest sense, to a material according to claim 1. This material comprises a glass substrate coated on one face with a stack of thin layers with reflection properties in the infrared and / or in solar radiation comprising at least one metallic functional layer, in particular based on silver or a metallic alloy containing silver and at least two anti-reflective coatings, said anti-reflective coatings each comprising at least one dielectric layer, said functional layer being arranged between the two anti-reflective coatings, said material being remarkable: on the one hand in that said anti-reflective coating located under said functional layer towards said substrate comprises: a zinc-based oxide sub-layer, ZnO, which is located under and in contact with said functional layer, with a physical thickness of said zinc-based oxide sub-layer ZnO which is between 0.3 and 5.0 nm, or even between 0.3 and 4.4 nm, or even between 0.3 and 2.9 nm, or even between 0.5 and 2.4 nm, or even between 1.0 and 3.0 nm, or even between 1.5 and 2.4 nm; and a silicon-based nitride dielectric sub-layer, Si 3 N 4 , which is located under and in contact with said zinc-based oxide sub-layer ZnO, with a physical thickness of said silicon-based nitride sub-layer Si 3 N 4 which is between 10.0 and 50.0 nm, or even between 22.0 and 45.0 nm, or even between 35.0 and 45.0 nm;on the other hand in that said anti-reflective coating located above said functional layer opposite said substrate comprises: a zinc-based oxide overlayer, ZnO, which is located on and in contact with said functional layer, with a physical thickness of said zinc-based oxide overlayer ZnO which is between 2.0 and 10.0 nm, or even between 2.0 and 8.0 nm, or even between 2.5 and 5.4 nm; and a dielectric overlayer which is located on said zinc-based oxide overlayer ZnO, and preferably a silicon-based nitride dielectric overlayer, Si 3 N 4 .;

[0012] The said zinc-based oxide sub-layer is the very thin layer mentioned above: it has a thickness corresponding to at least a monomolecular layer of Zn 1 O 1 and a maximum thickness of only a few nanometers. In this layer, preferably, the zinc oxide is neither sub-stoichiometric nor super-stoichiometric, in order to have the lowest possible absorption coefficient in the visible range.

[0013] The said silicon-based nitride dielectric underlayer is a barrier layer that prevents the penetration of elements from the substrate towards the metallic functional layer during processing.

[0014] Said stack may comprise a single metal functional layer or may comprise two metal functional layers, or three metal functional layers, or four metal functional layers; the metal functional layers in question here are continuous layers.

[0015] Preferably, when the stack comprises several metallic functional layers, each functional layer is according to the preceding indication, with: on the one hand said anti-reflective coating located under and in contact with each functional layer which comprises, in the direction of said substrate: a sub-layer of zinc-based oxide, ZnO, which is located under and in contact with said functional layer, with a physical thickness of said sub-layer of zinc-based oxide ZnO which is between 0.3 and 5.0 nm, or even between 0.3 and 4.4 nm, or even between 1.0 and 3.0 nm, or even between 1.5 and 2.4 nm; and a silicon-based nitride dielectric sub-layer, Si 3 N 4 , which is located under and in contact with said zinc-based oxide sub-layer ZnO, with a physical thickness of said silicon-based nitride sub-layer Si 3 N 4 which is between 10.0 and 50.0 nm, or even between 22.0 and 45.0 nm, or even between 35.0 and 45.0 nm;on the other hand said antireflective coating located above and in contact with each functional layer which comprises opposite said substrate: a zinc-based oxide overlayer, ZnO, which is located on and in contact with said functional layer, with a physical thickness of said zinc-based oxide overlayer ZnO which is between 2.0 and 10.0 nm, or even between 2.0 and 8.0 nm, or even between 2.5 and 5.4 nm; and a dielectric overlayer which is located on said zinc-based oxide overlayer ZnO, and preferably a silicon-based nitride dielectric overlayer, Si 3 N 4 .;

[0016] Said metal functional layer, or each metal functional, preferably has a physical thickness which is between 8.0 and 22.0 nm, or even between 9.0 and 16.0 nm, or even between 9.5 and 12.4 nm.

[0017] A metallic functional layer preferably comprises, predominantly, at least 50% in atomic percentage, at least one of the metals chosen from the list: Ag, Au, Cu, Pt; one, several, or each metallic functional layer is preferably made of silver.

[0018] By "metal layer" within the meaning of the present invention, it is understood that the layer does not contain oxygen or nitrogen.

[0019] As usual, by "dielectric layer" within the meaning of the present invention, it is to be understood that from the point of view of its nature, the layer is "non-metallic", that is to say that it comprises oxygen or nitrogen, or even both. In the context of the invention, this term means that the material of this layer has an n / k ratio over the entire visible wavelength range (from 380 nm to 780 nm) equal to or greater than 5.

[0020] It is recalled that n designates the real refractive index of the material at a given wavelength and the coefficient k represents the imaginary part of the refractive index at a given wavelength, or absorption coefficient; the ratio n / k being calculated at a given wavelength identical for n and for k.

[0021] For the purposes of the invention, "in contact" means that no layer is interposed between the two layers in question.

[0022] By "based on" is meant for the purposes of the invention that for the composition of this layer, the reactive elements oxygen, or nitrogen, or both if they are both present, are not considered and the non-reactive element (for example silicon or zinc) which is indicated as constituting the base, is present at more than 85 atomic % of the total of the non-reactive elements in the layer. This expression thus includes what is commonly called in the art considered "doping", whereas the doping element, or each doping element, can be present in an amount of up to 10 atomic %, but without the total dopant exceeding 15 atomic % of the non-reactive elements.

[0023] In a particular variant, said anti-reflective coating located under said functional layer and / or said anti-reflective coating located above said functional layer does not comprise any layer in the metallic state. Indeed, it is not desired that such a layer can react, and in particular oxidize, during treatment.

[0024] In a particular variant, said antireflective coating located under said functional layer and / or said antireflective coating located above said functional layer does not comprise any absorbent layer; By "absorbent layer" within the meaning of the present invention, it should be understood that the layer is a material having an average k coefficient, over the entire visible wavelength range (from 380 nm to 780 nm), greater than 0.5 and having an electrical resistivity in the bulk state (as known in the literature) which is greater than 10 -5< Ω.cm. Indeed, it is not desired for such a layer to be able to react, and in particular to oxidize, during treatment.

[0025] It is all the more surprising to achieve the properties targeted by the invention for these two previous variants because similar properties are sometimes obtained in the prior art with these two previous variants.

[0026] Preferably, said silicon-based nitride dielectric sub-layer Si 3 N 4 does not comprise zirconium.

[0027] Preferably, furthermore, said silicon-based nitride dielectric sub-layer Si 3 N 4 does not contain oxygen.

[0028] Said zinc-based oxide ZnO underlayer and / or said zinc-based oxide ZnO overlayer preferably consists of aluminium-doped zinc oxide ZnO, i.e. it does not contain any other elements than Zn, Al and a.

[0029] In a specific variant, said anti-reflective coating located under said functional layer further comprises a dielectric intermediate sub-layer located between said silicon-based nitride dielectric sub-layer Si 3 N 4 and said face, this dielectric intermediate sub-layer being oxidized (i.e. comprising oxygen) and preferably comprising a mixed oxide of zinc and tin.

[0030] In a specific variant, said anti-reflective coating located above said functional layer further comprises a dielectric intermediate overlayer located between said zinc-based oxide ZnO overlayer and said dielectric overlayer, this dielectric intermediate overlayer being oxidized and preferably comprising a titanium oxide.

[0031] The present invention further relates to a multiple glazing unit comprising a material according to the invention, and at least one other substrate, the substrates being held together by a frame structure, said glazing unit providing a separation between an exterior space and an interior space, in which at least one interposed gas layer is arranged between the two substrates.

[0032] Each substrate can be clear or colored. At least one of the substrates can be made of mass-colored glass. The choice of coloring type will depend on the level of light transmission and / or the desired color appearance for the glazing once it is manufactured.

[0033] A glazing substrate, in particular the substrate carrying the stack, may be curved and / or toughened after the stack has been deposited. It is preferable in a multiple glazing configuration for the stack to be arranged so as to be turned towards the interlayer gas gap.

[0034] The glazing can also be triple glazing consisting of three sheets of glass separated two by two by a gas layer. In a triple glazing structure, the substrate carrying the stack can be on face 2 and / or face 5, when we consider that the incident direction of the sunlight passes through the faces in ascending order of their number.

[0035] The present invention also relates to a method for obtaining, or manufacturing, a material comprising a glass substrate coated on one face with a stack of thin layers with reflection properties in the infrared and / or in solar radiation comprising at least one metallic functional layer, in particular based on silver or a metallic alloy containing silver and two anti-reflective coatings, said anti-reflective coatings each comprising at least one dielectric layer, said functional layer being arranged between the two anti-reflective coatings, said method comprising the following steps, in order: the deposition on one face of said substrate of a stack of thin layers with reflection properties in the infrared and / or in solar radiation comprising at least one metallic functional layer, in particular based on silver or a metallic alloy containing silver and at least two anti-reflective coatings, in order to form a material according to the invention, then the treatment of said stack of thin layers using a source producing radiation and in particular infrared radiation, in order to treat the stack of thin layers as such.

[0036] Said treatment is preferably carried out in an atmosphere not comprising oxygen.

[0037] Said zinc-based oxide underlayer ZnO is preferably deposited from a ceramic target comprising ZnO and in an atmosphere containing no oxygen or at most 10.0% oxygen.

[0038] The details and advantageous characteristics of the invention emerge from the following non-limiting examples, illustrated with the aid of the attached figures illustrating: [ fig. 1 ] illustrates a structure of a functional monolayer stack according to the invention, the functional layer being deposited directly on a zinc-based oxide ZnO sublayer and directly under a zinc-based oxide ZnO sublayer, the stack being illustrated during treatment using a source producing radiation; [ fig. 2 ] illustrates a structure of a functional bilayer stack according to the invention, each functional layer being deposited directly on a zinc-based oxide ZnO sublayer and directly under a zinc-based oxide ZnO sublayer, the stack being illustrated during treatment using a source producing radiation; [ fig. 3 ] illustrates double glazing incorporating a stack according to the invention; [ fig. 4 ] illustrates triple glazing incorporating two stacks according to the invention; [ fig. 5 ] illustrates the resistance per square of some examples of thin film stacks as a function of the thickness of a zinc-based oxide underlayer ZnO 129 and without any treatment; [ fig. 6 ] illustrates the resistance per square of the same examples as in figure 5 , depending on the thickness of a zinc-based oxide sublayer ZnO 129 and after AHT heat treatment or after ALT laser treatment; [ fig. 7 ] the solar factor of certain examples of glazing as a function of the thickness of a zinc-based oxide sub-layer ZnO 129 after laser treatment; [ fig. 8 ] illustrates the resistance per square of some examples of thin film stacks as a function of the thickness of the zinc-based oxide sub-layer ZnO 129 and its deposition conditions (nature of the atmosphere) without any WHT heat treatment or after ALT laser treatment, and; [ fig. 9 ] illustrates the resistance per square as well as the mechanical resistance of certain examples as a function of the thickness of the zinc-based oxide underlayer ZnO 129, without any heat treatment (R, EBT100, EBT200, EBT300, EBT400) or after laser treatment (LR, LEBT100, LEBT200, LEBT300, LEBT400).

[0039] In the figures 1 à 4 , the proportions between the thicknesses of the different layers or the different elements are not strictly respected in order to facilitate their reading.

[0040] There figure 1 illustrates a structure of a functional monolayer stack 14 according to the invention deposited on a face 29 of a transparent glass substrate 30, in which the single functional layer 140, in particular based on silver or a metal alloy containing silver, is arranged between two antireflective coatings, the underlying antireflective coating 120 located below the functional layer 140 in the direction of the substrate 30 and the overlying antireflective coating 160 arranged above the functional layer 140 opposite the substrate 30. These two antireflective coatings 120, 160, each comprise at least one dielectric layer 121, 127, 129; 161, 163, 165. On this figure 1 : on the one hand the anti-reflective coating 120 located under and in contact with the functional layer 140 comprises, in the direction of said substrate: a sub-layer of zinc-based oxide, ZnO, 129 which is located under and in contact with said functional layer, with a physical thickness of the sub-layer of zinc-based oxide ZnO which is between 0.3 and 5.0 nm, or even between 0.3 and 4.4 nm, or even between 1.0 and 3.0 nm, or even between 1.5 and 2.4 nm; and a silicon-based nitride dielectric sub-layer, Si 3 N 4 , 127 which is located under and in contact with the zinc-based oxide sub-layer ZnO, respectively 129, with a physical thickness of the silicon-based nitride sub-layer Si 3 N 4 which is between 10.0 and 50.0 nm, or even between 22.0 and 45.0 nm, or even between 35.0 and 45.0 nm;on the other hand, the antireflective coating 160 located above and in contact with the functional layer 140 comprises, opposite the substrate: a zinc-based oxide overlayer, ZnO, 161, which is located on and in contact with the functional layer, with a physical thickness of the zinc-based oxide overlayer ZnO which is between 2.0 and 10.0 nm, or even between 2.0 and 8.0 nm, or even between 2.5 and 5.4 nm; and a dielectric overlayer 165 which is located on the zinc-based oxide overlayer ZnO, 161 and preferably this dielectric overlayer is silicon-based nitride, Si 3 N 4 . ;

[0041] There figure 2 illustrates a structure of a functional bilayer stack 14 according to the invention deposited on a face 29 of a transparent glass substrate 30, in which the functional layers 140, 180, in particular based on silver or a metal alloy containing silver, are arranged between two antireflective coatings, the underlying antireflective coating 120 located below the functional layer 140 closest to the face 29 of the substrate 30, the intermediate antireflective coating 160 is located between the two functional layers and the overlying antireflective coating 200 arranged above the functional layer 180 furthest from the face 29 of the substrate 30. These three antireflective coatings 120, 160, 200 each comprise at least one dielectric layer 127, 129; 161, 167, 169; 201, 205. On this figure 2 : on the one hand, said anti-reflective coating located under and in contact with each functional layer 140, 180 comprises, in the direction of said substrate: a zinc-based oxide sub-layer, ZnO, 129, 169 which is located under and in contact with said functional layer, with a physical thickness of said zinc-based oxide sub-layer ZnO which is between 0.3 and 5.0 nm, or even between 0.3 and 4.4 nm, or even between 1.0 and 3.0 nm, or even between 1.5 and 2.4 nm; and a silicon-based nitride dielectric sub-layer, Si 3 N 4 , 127, 167, which is located under and in contact with said zinc-based oxide sub-layer ZnO, respectively 129, 169, with a physical thickness of said silicon-based nitride sub-layer Si 3 N 4 which is between 10.0 and 50.0 nm, or even between 22.0 and 45.0 nm, or even between 35.0 and 45.0 nm;on the other hand, said antireflective coating located above and in contact with each functional layer 140, 180 comprises, opposite said substrate: a zinc-based oxide overlayer, ZnO, 161, 201, which is located on and in contact with said functional layer, with a physical thickness of said zinc-based oxide overlayer ZnO which is between 2.0 and 10.0 nm, or even between 2.0 and 8.0 nm, or even between 2.5 and 5.4 nm; and a dielectric overlayer 205 which is located on said zinc-based oxide overlayer ZnO, 201 and preferably this dielectric overlayer is silicon-based nitride, Si 3 N 4 .;

[0042] The functional layer 140 is located directly on the underlying anti-reflective coating 120 and directly under the overlying anti-reflective coating 160: there is no under-blocking coating located between the underlying anti-reflective coating 120 and the functional layer 140 nor an over-blocking coating located between the functional layer 140 and the anti-reflective coating 160. The same is preferably true for the other functional layer(s) possibly present: each is, preferably, in direct contact with the anti-reflective coating located directly below and the anti-reflective coating located directly above.

[0043] The 160 anti-reflective coating located above the single metallic functional layer in figure 1 (or which is located above the metal functional layer furthest from the substrate when there are several metal functional layers) can end with a terminal protection layer (not shown), called “overcoat” in English, which is the layer of the stack which is furthest from face 29.

[0044] Such a stack of thin layers can be used in a multiple glazing 100 creating a separation between an exterior space ES and an interior space IS; this glazing can have a structure: double glazing, as shown in figure 3 : this glazing is then made up of two substrates 10, 30 which are held together by a frame structure 90 and which are separated from each other by an interposed gas blade 15; or triple glazing, as illustrated in figure 4 : this glazing is then made up of three substrates 10, 20, 30, separated two by two by an intermediate gas blade 15, 25, the whole being held together by a frame structure 90.

[0045] In the figures 3 et 4 , the incident direction of sunlight entering the building is illustrated by the double arrow, on the left.

[0046] In figure 3 , the stack 14 of thin layers can be positioned on face 3 (on the innermost sheet of the building considering the incident direction of the sunlight entering the building and on its face facing the gas blade), that is to say on an inner face 29 of the substrate 30 in contact with the interposed gas blade 15, the other face 31 of the substrate 30 being in contact with the inner space IS.

[0047] However, it can also be considered that in this double glazing structure, one of the substrates has a laminated structure.

[0048] In figure 4 , there are two stacks of thin layers, preferably identical: a stack 14 of thin layers is positioned on face 2 (on the outermost sheet of the building considering the incident direction of the sunlight entering the building and on its face facing the gas blade), that is to say on an inner face 11 of the substrate 10 in contact with the interposed gas blade 15, the other face 9 of the substrate 10 being in contact with the outer space ES; and a stack 26 of thin layers is positioned on face 5 (on the innermost sheet of the building considering the incident direction of the sunlight entering the building and on its face facing the gas blade), that is to say on an inner face 29 of the substrate 30 in contact with the interposed gas blade 25, the other face 31 of the substrate 30 being in contact with the inner space IS.

[0049] A first series of examples was produced based on the stacking structure illustrated in figure 1 with, starting from surface 29, only the following layers, in this order: a silicon-based nitride dielectric sub-layer, Si 3 N 4 127, with a physical thickness of 20 nm, deposited from an aluminum-doped silicon target, 92 wt% silicon and 8 wt% aluminum in an atmosphere of 45% nitrogen on the total of nitrogen and argon and under a pressure of 1.5.10 -3< mbar; a zinc-based oxide sub-layer, ZnO 129, with a variable physical thickness, ranging from 1.0 nm to more than 7.0 nm, deposited from a ceramic target consisting of 49 atomic % zinc and 49 atomic % oxygen and doped with 2% aluminum, in an argon atmosphere and under a pressure of 2.10 -3< mbar; a metallic functional layer 140 based on silver, and more precisely here in silver, with a physical thickness of 10 nm, deposited from a silver metallic target, in an argon atmosphere and under a pressure of 2.10 -3< mbar; a zinc-based oxide overlayer, ZnO 161, with a physical thickness of 5 nm, deposited from a ceramic target consisting of 49 atomic % zinc and 49 atomic % oxygen and doped with 2% aluminum, in an argon atmosphere and under a pressure of 2.10 -3< mbar; a silicon-based nitride dielectric overlayer 165, Si 3 N 4 , with a physical thickness of 20 nm, deposited from a silicon target doped with aluminum, with 92 wt% silicon and 8 wt% aluminum in an atmosphere of 45% nitrogen on the total of nitrogen and argon and under a pressure of 2.10 -3< mbar. .

[0050] There figure 5 illustrates on the ordinate the resistance per square, Rsq, in ohms per square of the stacks thus deposited as a function of the thickness, t 129 , in nanometers of the zinc-based oxide sub-layer, ZnO 129 on the abscissa, this resistance per square being measured immediately after the deposition of the stacks, that is to say without any heat treatment. This curve shows that there is, a priori, no interest in using a zinc-based oxide sub-layer ZnO 129 with a thickness of less than 5 nm because the resistance per square of the stack tends to be higher in this thickness range.

[0051] There figure 6 illustrates on the ordinate the resistance per square, Rsq, in ohms per square of these stacks as a function of the thickness, t 129 , in nanometers of the zinc-based oxide sub-layer, ZnO 129 on the abscissa, this resistance per square being measured after one or other of these treatments: either an annealing heat treatment, consisting of heating at a temperature of 650°C for 10 minutes then cooling by simply leaving the sample in an environment at 20°C, in order to simulate quenching; the measurements are illustrated by the top curve, AHT; or a laser treatment consisting here of a scrolling of the substrate 30 at a speed of 4 m / min under a laser line 20 of 0.08 mm width, 11.6 mm length and total power of 433 W with the laser line oriented perpendicular to the face 29 and in the direction of the stack 14, that is to say by placing the laser line above the stack, as visible in figure 1 (the right black arrow illustrating the orientation of the emitted light); the measurements are illustrated by the bottom curve, ALT.

[0052] Comparing the top curve, AHT, with the bottom curve, ALT, shows that, with the exception of an artifact at 3.8 nm, the resistance per square inch is even lower after laser treatment than after quenching heat treatment, for a ZnO 129 zinc-based oxide underlayer thickness between 1.0 and 5.0 nm. There is even a particularly favorable plateau, with a particularly low resistance per square inch, for a ZnO 129 zinc-based oxide underlayer thickness between 1.0 and 3.0 nm, or even between 1.5 and 2.4 nm. The improvement is between 5 and 10% compared to quenching heat treatment.

[0053] Such a situation allows in a first approach to increase the solar factor at constant functional layer thickness, or even in a second approach to reduce the thickness of the functional layer to further increase the solar factor without modifying the resistance per square previously obtained.

[0054] A counter-example was made on the basis of this first series, with the same layers (same material, same thickness) 127, 129 of 5 nm, 140, 161 and 165, but with the addition of a NiCr over-blocking layer (1.0 nm thick layer, deposited from a metal target of 80% by mass of Ni and 20% by mass of Cr, in an argon atmosphere and under a pressure of 2.10 -3< mbar) between the metal functional layer 140 and the zinc-based oxide over-layer 161. Before any treatment, the resistance per square was measured at 6.1 ohms / square, more than 10% higher than without over-blocking layer.

[0055] This counterexample underwent the same laser treatment as the previous examples and its resistance per square was then measured at 5.1 ohms / square.

[0056] The presence of an over-blocking layer is thus unfavorable to obtaining a low square resistance; In addition, it was found that this counter-example presented a residual light absorption after laser treatment which was too high and unacceptable for the targeted performances.

[0057] To confirm this effect, a second series of examples was carried out based on the stacking structure illustrated in figure 1 with, starting from surface 29, only the following layers, in this order: a silicon-based nitride dielectric sub-layer, Si 3 N 4 127 with a physical thickness of 40 nm, deposited from an aluminum-doped silicon target, 92% by weight of silicon and 8% by weight of aluminum in an atmosphere of 45% nitrogen on the total of nitrogen and argon and under a pressure of 1.5.10 -3< mbar; a zinc-based oxide sub-layer ZnO 129, with a variable physical thickness, varying from 1 nm to more than 7 nm, deposited from a ceramic target consisting of 49 atomic % zinc and 49 atomic % oxygen and doped with 2% aluminum, in an argon atmosphere and under a pressure of 2.10 -3< mbar; a 140 silver-based metallic functional layer, and even precisely here in silver, with a physical thickness of 10 nm, deposited from a silver metallic target, in an argon atmosphere and under a pressure of 2.10 -3< mbar; a zinc-based oxide overlayer ZnO 161, with a physical thickness of 5 nm, deposited from a ceramic target consisting of 49 atomic % zinc and 49 atomic % oxygen and doped with 2% aluminum, in an argon atmosphere and under a pressure of 2.10 -3< mbar; a dielectric overlayer 163 comprising titanium dioxide TiOz, with a physical thickness of 2 nm, deposited from a titanium target in an atmosphere of 23% oxygen on the total of oxygen and argon and under a pressure of 2.10 -3< mbar; a dielectric overlayer 165 of silicon-based nitride, Si 3 N 4 , with a physical thickness of 30 nm, deposited from an aluminum-doped silicon target, 92% by weight of silicon and 8% by weight of aluminum in an atmosphere of 45% nitrogen on the total of nitrogen and argon and under a pressure of 2.10 -3 < mbar. .

[0058] All of these examples were laser-treated as before and then triple-glazed in a structure of the type shown in figure 4 . For these examples, it is a configuration: 4-16 (Ar 90%)-4-16 (Ar 90%)-4, that is to say that it is made up of three sheets of transparent glass of 4 mm, each producing a substrate 10, 20, 30, separated two by two by an intermediate gas blade 15, 25 at 90% argon and 10% air each with a thickness of 16 mm, the whole being held together by a frame structure 90.

[0059] The two outer substrates 10, 30 of this triple glazing are each coated, on its inner face 11, 29 facing the intermediate gas layer 15, 25, with an insulating coating 14, 26 consisting of the functional single-layer stack described above: the functional single-layer stacks are thus on faces called “face 2” and “face 5”).

[0060] The central substrate 20 of this triple glazing, the one whose two faces 19, 21 are in contact respectively with the intermediate gas blades 15 and 25, is not coated with any coating on either of these faces.

[0061] There figure 7 illustrates the evolution on the ordinate of the solar factor, g, in percent, as a function of the thickness, t 129 , in nanometers of the zinc-based oxide sublayer ZnO 129 on the abscissa, this solar factor being measured immediately after the laser treatment of the two substrates 10, 30, then their integration to form the triple glazing. The solar factor is thus improved when the zinc-based oxide sublayer ZnO 129 is between 0.03 and 5.0 nm. The solar factor is particularly favorable for a thickness of this zinc-based oxide sublayer ZnO 129 between 1.0 and 3.0 nm, or even between 1.5 and 2.4 nm.

[0062] It was measured that for a thickness of the zinc-based oxide underlayer ZnO 129 of 5.0 nm and a thickness of the functional layer 140 of 10.0 nm for both stacks 14, 26, the resistance per square is 3.78 ohms per square and the solar factor of the triple glazing is 57.02%

[0063] It was surprisingly found that for a thickness of the zinc-based oxide underlayer ZnO 129 of 1.0 nm and a thickness of the functional layer 140 of 10.0 nm for both stacks 14, 26, the resistance per square dropped to 3.59 ohms per square and the solar factor of the triple glazing rose to 57.26%.

[0064] By reducing the thickness of the functional layer 140 of the two stacks 14, 26 from 10.0 to 9.6 ohms per square and by keeping the thickness of the zinc-based oxide sublayer ZnO 129 at 1.0 nm, it was thus possible to produce two stacks having substantially the same resistance per square as with 5.0 nm for the zinc-based oxide sublayer ZnO 129 and 10.0 nm for the functional layer 140 (3.80 ohms per square). However, for a resistance per square maintained, it was then found that the triple glazing had a much higher solar factor, at 58.23%.

[0065] A third series of examples was then carried out on the basis of the first series of examples by modifying the deposition conditions of the zinc-based oxide sub-layer ZnO 129: the deposition atmosphere of this layer was tested with: 0% oxygen (and 100% argon); measurements are shown as circles; 5% oxygen (and 95% argon); measurements are shown as triangles; and 10% oxygen (and 90% argon); measurements are shown as squares.

[0066] There figure 8 illustrates on the ordinate the resistance per square Rsq, in ohms per square of these stacks as a function of the thickness in nanometers of the zinc-based oxide sub-layer ZnO 129, t 129 , on the abscissa, this resistance per square being measured after one or other of these treatments: without heat treatment, WHT; the measurements are illustrated by circles, triangles or empty squares; or the same laser treatment as the first series, ALT by the laser line 20 visible in figure 2 ; measurements are illustrated by solid circles, triangles or squares.

[0067] The resistance per square inch may be lower than expected when there is a lot of oxygen in the deposition atmosphere of the zinc-based oxide undercoat, ZnO 129; especially when the content is much higher than 10%.

[0068] A fourth series of examples was then carried out on the basis of the first series of examples by maintaining the most favorable deposition conditions of the zinc-based oxide sub-layer ZnO 129 from the third series of examples (deposition atmosphere of 5% oxygen and 95% argon) and by varying the thickness of this zinc-based oxide sub-layer ZnO 129.

[0069] The table of the figure 9 presents in the first line the essential data for this series of examples no zinc-based oxide sublayer ZnO 129 (ex. 41), or a zinc-based oxide sublayer ZnO 129 of 1.0 nm (ex. 42), or 2.0 nm (ex. 43) or 5.0 nm (ex. 44).

[0070] The next two lines of the table of the figure 9 present: the resistance per square of the complete stack before any heat treatment: R, in ohms per square, and the resistance per square of the complete stack after laser treatment: LR, in ohms per square; this treatment being identical to that carried out previously.

[0071] The following two sets of four lines present the results of the mechanical resistance test called the "Erichsen Brush Test" which consists of applying a brush with nylon dots to the stack immersed in water for 100, 200, 300 or 400 revolutions and noting: the mechanical resistance to this test before any heat treatment: EBT; the mechanical resistance to this test after laser treatment: LEBT; this treatment being identical to that carried out previously.

[0072] In this test, the rating is given as follows: Note 1 when there are no marks on the sample; Note 2 when there are fine scratches on the sample; Note 3 when there are large scratches on the sample or large point defects; Note 4 when there is delamination of the stack.

[0073] Example 41 shows relatively high square strength both without heat treatment and after laser treatment and very poor EBT resistance.

[0074] Examples 42 to 44 all show good mechanical resistance to the EBT test, both without heat treatment and after laser treatment, and the gain (decrease) in resistance per square is significant with examples 42, 43 and 44 (respective gain of 32%, 27% and 20%) whose zinc-based oxide sub-layer ZnO 129 is deposited directly on the dielectric sub-layer comprising silicon nitride Si 3 N 4 127.

[0075] In a variant, it is possible that said anti-reflective coating 120 located under the functional layer 140 further comprises a dielectric intermediate sub-layer 125 located between the silicon-based nitride dielectric sub-layer, Si 3 N 4 127 and the face 29, this dielectric intermediate sub-layer 125 being oxidized and preferably comprising a mixed oxide of zinc and tin.

[0076] The present invention is described in the foregoing by way of example. It is understood that a person skilled in the art is able to carry out different variants of the invention without departing from the scope of the patent as defined by the claims.

Claims

1. A material comprising a glass substrate (30) coated on one face (29) with a stack of thin layers (14) with properties of reflection in the infrared and / or in solar radiation comprising at least one metallic functional layer (140), in particular based on silver or metal alloy containing silver and at least two anti reflective coatings (120, 160), said anti reflective coatings each comprising at least one dielectric layer (127, 165), said functional layer (140) being arranged between the two antireflective coatings (120, 160), characterized in that said anti reflective coating (120) located beneath said functional layer (140) in the direction of said substrate (30) comprises: - a sublayer of zinc-based oxide, ZnO (129) that is located beneath and in contact with said functional layer (140), with a physical thickness of said sublayer based on zinc oxide ZnO (129) that is between 0.3 and 5.0 nm, or between 0.3 and 4.4 nm, or between 0.3 and 2.9 nm, or between 0.5 and 2.4 nm; and - a dielectric sublayer of silicon-based nitride, Si3N4 (127) that is located beneath and in contact with said sublayer of zinc-based oxide, ZnO (129), with a physical thickness of said dielectric sublayer of silicon-based nitride Si3N4 (127) that is between 10.0 and 50.0 nm, or between 22.0 and 45.0 nm, or between 35.0 and 45.0 nm; and in that said antireflective coating (160) located above said functional layer (140) opposite said substrate (30) comprises: - an overlay of zinc-based oxide, ZnO (161) that is located on top of and in contact with said functional layer (140), with a physical thickness of said overlay of zinc-based oxide, ZnO (161) that is between 2.0 and 10.0 nm, or between 2.0 and 8.0 nm, or between 2.5 and 5.4 nm; and - a dielectric overlay (165) that is located on said overlay of zinc-based oxide, ZnO (161) and, preferably a dielectric overlay of silicon-based nitride, Si3N4.

2. The material as claimed in claim 1, in which said metallic functional layer (140), or each metallic functional layer, has a physical thickness that is between 8.0 and 22.0 nm, or between 9.0 and 16.0 nm, or between 9.5 and 12.4 nm.

3. The material as claimed in claim 1 or 2, in which said anti reflective coating (120) located beneath said metallic functional layer (140) and / or said anti reflective coating (160) located above said metallic functional layer (140) does not comprise any layer in the metallic state.

4. The material as claimed in any one of claims 1 to 3, in which said dielectric sublayer of silicon-based nitride, Si3N4 (127) does not comprise zirconium.

5. The material as claimed in any one of claims 1 to 4, in which said dielectric sublayer of silicon-based nitride, Si3N4 (127) does not comprise oxygen.

6. The material as claimed in any one of claims 1 to 5, in which said sublayer of zinc-based oxide, ZnO (129) and / or said overlay of zinc-based oxide, ZnO (161) consists of zinc oxide ZnO doped with aluminum.

7. The material as claimed in any one of claims 1 to 6, in which said anti reflective coating (120) located beneath said functional layer (140) further comprises a dielectric intermediate sublayer (121) located between said dielectric sublayer of silicon-based nitride, Si3N4 (127) and said face (29), this dielectric intermediate sublayer (121) being oxidized and preferably comprising a mixed oxide of zinc and tin.

8. The material as claimed in any one of claims 1 to 7, in which said anti reflective coating (160) located above said functional layer (140) further comprises a dielectric intermediate overlay (163) located between said overlay of zinc-based oxide, ZnO (161) and said dielectric overlay (165), this dielectric intermediate overlay (163) being oxidized and preferably comprising a titanium oxide.

9. A multiple glazing comprising a material as claimed in any one of claims 1 to 8, and at least one other substrate (10), the substrates (10, 30) being held together by a frame structure (90), said glazing providing separation between an exterior space (ES) and an interior space (IS), in which at least one interposed gas gap (15) is arranged between the two substrates.

10. A method of producing a material comprising a glass substrate (30) coated on one face (29) with a stack of thin layers (14) with properties of reflection in the infrared and / or in solar radiation comprising at least one metallic functional layer (140), in particular based on silver or metal alloy containing silver and two antireflective coatings (120, 160), said anti reflective coatings each comprising at least one dielectric layer (127, 165), said functional layer (140) being arranged between the two antireflective coatings (120, 160), said method comprising the following steps, in this order: - depositing, on a face (29) of said substrate (30), a stack of thin layers (14) with properties of reflection in the infrared and / or in solar radiation comprising at least one metallic functional layer (140), in particular based on silver or metal alloy containing silver and at least two anti reflective coatings (120, 160), in order to form a material as claimed in any one of claims 1 to 7, and then - treating said stack of thin layers (14) using a source producing radiation and in particular infrared radiation.

11. The method as claimed in claim 10, in which said treatment is carried out in an atmosphere not comprising oxygen.

12. The method as claimed in claim 10 or 11, in which said sublayer of zinc-based oxide, ZnO (129) is deposited from a ceramic target comprising ZnO, in an atmosphere not comprising oxygen or comprising at most 10.0% oxygen.