METHOD FOR PRODUCE A PART FROM A COMPOSITE MATERIAL USING AN ADHESIVE AGENT CONTAINING A LEWIS ACID OR A COMPLEX
Patent Information
- Application Number
- DE602021021429
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-09
- Filing Date
- 2021-06-02
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-06-02
AI Technical Summary
The mechanical properties of composite materials with a ceramic matrix formed by the Polymer Impregnation and Pyrolysis (PIP) technique are limited due to adhesion issues at the interfaces, leading to suboptimal load transfer and thermal resistance problems, particularly at high temperatures.
Introducing a Lewis complex or Lewis acid adhesion promoter with reactive S1 or S2 structures into the porosity of a fibrous preform, grafting it to the surface, and chemically binding it to the ceramic precursor resin to enhance adhesion between the matrix and the fibrous reinforcement, thereby improving mechanical properties and thermal resistance.
The proposed method improves the adhesion between the ceramic matrix and the fibrous reinforcement, enhancing mechanical properties and increasing the thermal resistance of the composite material to temperatures above 1500°C, while reducing volume shrinkage and increasing mass yield.
Description
Technical Field
[0001] The present invention relates to a method for manufacturing a part made of at least partially ceramic matrix composite material having improved mechanical properties. Prior art
[0002] Parts made of composite material with an at least partially ceramic matrix can conventionally be obtained by a polymer impregnation and pyrolysis technique (“Polymer Impregnation and Pyrolysis”; “PIP”).
[0003] According to such a technique, a liquid composition of a ceramic precursor polymer is introduced into the porosity of a fiber preform. The composition thus introduced is then polymerized and then pyrolyzed in order to form the ceramic matrix phase. Various types of ceramic matrices can be formed by this method depending on the choice of precursor used. In particular, a polysilazane polymer can be used to obtain a SiCN matrix, a polycarbosilane polymer can be used to obtain a SiC matrix or a polysiloxane polymer can be used to obtain a SiCO matrix.
[0004] It is usual to repeat these infiltration and pyrolysis cycles several times in a row in order to obtain the desired porosity rate for the densified part, given that the transformation into ceramic by pyrolysis involves volume shrinkage.
[0005] One of the limitations of the mechanical properties of parts having a matrix obtained by a PIP technique comes from a problem of adhesion to the interfaces of the PIP matrix.
[0006] We also know application WO 2018 / 229428 which discloses the use of silane adhesion promoters to improve adhesion between the fibrous reinforcement and the ceramic matrix.
[0007] It is desirable to have new solutions to improve the mechanical properties presented by composite material parts whose matrix has been at least partly formed by a PIP technique. It is also desirable to improve the thermal resistance of matrices formed by the PIP technique, particularly at temperatures of around 1500°C. Statement of the invention
[0008] The invention relates, according to a first aspect, to a method for manufacturing a part made of composite material comprising at least the following steps: a) introducing an adhesion promoter into the porosity of a fiber preform formed by yarns coated with a coating having -OH groups on its surface, the adhesion promoter being a Lewis complex or a Lewis acid, the Lewis complex adhesion promoter comprising a reactive S1 structure of formula B1-XH where B1 is a Lewis base, the Lewis acid adhesion promoter comprising a reactive S2 structure of formula XH with atom X having an electronic gap, in these two alternatives X denotes boron or aluminum, b) grafting the adhesion promoter to the surface of the coating by addition to the -OH groups at atom X, c) introducing a ceramic precursor resin into the porosity of the fiber preform, after the adhesion promoter grafting step,d) polymerization of the introduced resin and bonding of the grafted adhesion promoter to the resin by chemical reaction between these two compounds at an XH bond of the grafted promoter, this polymerization and this bonding being carried out by heating the fiber preform into which the resin has been introduced, and e) formation of a ceramic matrix phase in the porosity of the fiber preform by pyrolysis of the polymerized resin.
[0009] One of the limitations of the mechanical properties of parts having a matrix obtained by a PIP technique comes from a problem of adhesion to the interfaces of the PIP matrix. The inventors have, in fact, noted the existence of decohesions between the ceramic precursor in the polymerized state and a coating previously formed on the wires (see figure 1 ). In the test associated with the figure 1 , the coating was a pyrolytic carbon (PyC) interphase layer covering the wires. The figure 2 shows, for its part, the existence of decohesions between the matrix phase obtained after pyrolysis of the precursor and a silicon carbide (SiC) coating formed, beforehand, on the wires. The existence of these decohesions results in suboptimal mechanical properties for the parts obtained, due to a limitation of the transfer of charges between the matrix and the fiber reinforcement. The present invention was developed in order to solve this problem and thus implements an adhesion promoter making it possible to improve the adhesion between the PIP matrix phase and a coating formed beforehand on the wires. This coating formed beforehand can be of different natures, as will be described below.
[0010] When the adhesion promoter is a Lewis acid, it has an electron vacancy at the X atom that is intended to be filled by the oxygen electrons of the pendant -OH groups present on the surface of the underlying coating. A covalent bond is thus formed between the oxygen atom of the -OH groups and the X atom during grafting. It should be noted that the -OH groups are naturally present after exposure of the coating to ambient air. Once grafting is carried out, the XH bonds of the promoter are able to react chemically with the resin. This reaction allows the promoter to be covalently bonded to the ceramic precursor resin.
[0011] When the adhesion promoter is a Lewis complex, the Lewis base B1 constitutes a leaving group during grafting. This forms a covalent bond between the oxygen atom of the -OH groups and the X atom. The XH bonds of the promoter are then able to react chemically with the resin as in the case of the Lewis acid.
[0012] The adhesion promoter thus constitutes a bonding intermediary between the resin, that is to say ultimately the PIP matrix phase, and the underlying coating, thus making it possible to improve the adhesion of this matrix phase to this coating. The use of the adhesion promoter proposed by the present invention thus contributes to improving the mechanical properties of the composite material part obtained. In addition, the reaction of the adhesion promoter with the ceramic precursor resin makes it possible to increase its degree of crosslinking and its density, thus making it possible to increase the mass yield of this resin and reduce its volume shrinkage.
[0013] In an exemplary embodiment, X is boron.
[0014] Such a feature is advantageous because it allows boron to be obtained in the ceramic matrix phase after pyrolysis, thus improving the thermal resistance of the matrix. In particular, a ceramic matrix can be obtained that is thermostable at 1500°C, for example of the SiBCN type.
[0015] Alternatively, X can be aluminum.
[0016] Such a feature is advantageous in order to improve the oxidation resistance of the formed matrix.
[0017] In an exemplary embodiment, the adhesion promoter is a Lewis complex of general formula B1-BH 3 or B1-AlH 3 . B1 may for example be an aliphatic or aromatic hydrocarbon chain having from 1 to 12 carbon atoms, for example from 1 to 4 carbon atoms. B1 may be a linear or branched hydrocarbon chain having from 1 to 12 carbon atoms, for example from 1 to 4 carbon atoms. The adhesion promoter may be a Lewis complex and the Lewis base B1 may be of formula *-SR 2 or *-NR 3 , with *- denoting the bond to the X atom and in each of these formulas the R groups being identical or different and being a hydrocarbon chain comprising from 1 to 12 carbon atoms, for example from 1 to 4 carbon atoms, saturated or unsaturated.
[0018] The R groups can in particular be chosen from: a methyl group or an ethyl group.
[0019] The adhesion promoter may in particular be borane dimethylsulfide (“borane dimethylsulfide”) having the formula below:
[0020] The adhesion promoter may in particular be Alane NN dimethyl amine having the formula below:
[0021] Alternatively, the adhesion promoter is a Lewis acid of general formula R' 2 -BH or R' 2 -AlH, in each of these formulas the R' groups being identical or different and being a hydrogen atom, a hydrocarbon chain comprising from 1 to 12 carbon atoms, for example from 1 to 4 carbon atoms, saturated or unsaturated, the R' groups possibly together defining the same cyclic hydrocarbon chain. In this case, the adhesion promoter may in particular be 9-Borabicyclo[3.3.1]nonane having the formula below:
[0022] In an exemplary embodiment, the ceramic precursor resin comprises at least one reactive function reacting with the XH bond of the adhesion promoter grafted during step d) and chosen from: a carbon-carbon double bond, an NH group, an Si-H group, an -OH group.
[0023] In particular, the reactive function can be an allyl group or a vinyl group.
[0024] In an exemplary embodiment, the method further comprises, before introducing the promoter, a step of forming the coating on the wires by chemical vapor deposition or infiltration (“Chemical Vapor Deposition” or “Chemical Vapor Infiltration”; “CVD” or “CVI”).
[0025] In this case, the coating may be an interphase or a preliminary matrix phase. In this example, the use of the adhesion promoter improves the adhesion of the PIP matrix phase formed directly on this coating.
[0026] Alternatively, the method further comprises, before introducing the promoter, a step of forming the coating on the wires by introducing a precursor compound into the porosity of the preform and pyrolyzing this precursor compound. In this case, the coating constitutes a preliminary PIP matrix phase and the use of the adhesion promoter improves the adhesion between two successively formed PIP matrix blocks. It will be noted that when the matrix is formed from a plurality of PIP matrix blocks, it is possible to implement the method described above in order to improve the adhesion between each of these blocks.
[0027] In an exemplary embodiment, the material forming the surface of the coating is chosen from: carbon, boron-doped carbon, silicon carbide, boron nitride, silicon-doped boron nitride or silicon nitride.
[0028] In an exemplary embodiment, the resin is chosen from: polysiloxane resins, polysilazane resins, polycarbosiloxane resins, polycarbosilane resins, polycarbosilazane resins and mixtures of such resins. Brief description of the drawings
[0029] [ Fig. 1 ] There figure 1 is a photograph showing the existence of decohesions between a ceramic precursor in the polymerized state and a PyC coating formed on wires (outside the invention). [ Fig. 2 ] There figure 2 is a photograph showing the existence of decohesions between a PIP matrix phase and a SiC coating formed on wires (outside the invention). [ Fig. 3 ] There figure 3 schematically illustrates a step of a first example of a method according to the invention. Fig. 4 ] There figure 4 schematically illustrates a step of the first example of the method according to the invention. Fig. 5 ] There figure 5 schematically illustrates a step of the first example of the method according to the invention. Fig. 6 ] There figure 6 schematically illustrates a step of the first example of the method according to the invention. Fig. 7 ] There figure 7 schematically illustrates a step of a second example of a method according to the invention. Fig. 8 ] There figure 8 schematically illustrates a step of the second example of the method according to the invention. Fig. 9 ] There figure 9 schematically illustrates a step of the second example of the method according to the invention. Fig. 10 ] There figure 10 schematically illustrates a step of the second example of the method according to the invention. Description of the embodiments
[0030] First, a fiber preform made of refractory yarns, such as ceramic or carbon yarns, is formed.
[0031] The preform can, for example, be formed from silicon carbide wires supplied by the Japanese company NGS under the reference “Nicalon”, “Hi-Nicalon” or “Hi-Nicalon Type S”. The carbon wires that can be used to form this preform are, for example, supplied under the name Torayca T300 3K by the Toray company.
[0032] The fiber preform is obtained from at least one textile operation. The fiber preform is intended to constitute the fiber reinforcement of the part to be obtained. The fiber preform can, in particular, be obtained by multi-layer or three-dimensional weaving.
[0033] By "three-dimensional weaving" or "3D weaving" is meant a weaving method by which at least some of the warp threads bind weft threads over several weft layers. A reversal of roles between warp and weft is possible in the present text and must be considered as also covered by the claims.
[0034] The fiber preform may, for example, have a multi-satin weave, i.e., be a fabric obtained by three-dimensional weaving with several layers of weft yarns, the basic weave of each layer of which is equivalent to a conventional satin weave but with certain points of the weave that bind the layers of weft yarns together. Alternatively, the fiber preform may have an interlock weave. By "interlock weave or fabric" is meant a 3D weave weave in which each layer of warp yarns binds several layers of weft yarns with all the yarns of the same warp column having the same movement in the plane of the weave. Different multi-layer weaving methods that can be used to form the fiber preform are described in WO 2006 / 136755.
[0035] It is also possible to first form fiber textures such as two-dimensional fabrics or unidirectional webs, and to obtain the fiber preform by draping such fiber textures onto a form. These textures can optionally be linked together, for example by sewing or implantation of threads to form the fiber preform.
[0036] The coating is then formed on the preform yarns. This coating may be an interphase or comprise one or more matrix phases partially densifying the fiber preform. The coating may be made of carbon, in particular PyC, boron-doped carbon (BC, with boron in an atomic proportion of between 5% and 20%, the remainder being carbon) or ceramic material, such as silicon carbide, boron nitride (BN), silicon-doped boron nitride (BN(Si), with silicon in a mass proportion of between 5% and 40%, the remainder being boron nitride) or silicon nitride (Si 3 N 4 ).
[0037] The coating can thus be formed by a single-layer or multi-layer interphase. In this case, the surface of the interphase has -OH groups intended to allow the grafting of the adhesion promoter. This interphase can comprise at least one layer of pyrolytic carbon, boron nitride, silicon-doped boron nitride or boron-doped carbon.
[0038] The interphase here has a function of weakening the composite material which promotes the deflection of any cracks reaching the interphase after having propagated in the matrix, preventing or delaying the rupture of the wires by such cracks. The thickness of the interphase can be between 10 nm and 1000 nm, and for example between 10 nm and 100 nm. The interphase can be formed by CVI on the wires of the preform.
[0039] Alternatively, the interphase could be formed by chemical vapor deposition on the wires before forming the preform, and then forming the preform from the coated wires.
[0040] Alternatively, the coating may comprise at least one preliminary matrix phase and optionally an interphase interposed between said at least one preliminary matrix phase and the wires. In which case, the external preliminary matrix phase, i.e. the one furthest from the wires of the preform, has on its surface the -OH groups intended to allow the grafting of the adhesion promoter.
[0041] The external preliminary matrix phase can be formed by various methods known per se, such as CVI, infiltration of silicon in the molten state (melt-infiltration process) or by a PIP technique. It will therefore be noted that, in the latter case, the adhesion promoter makes it possible to improve the adhesion between two successive PIP matrix blocks. The external preliminary matrix phase can be ceramic or carbon. The external preliminary matrix phase can be carbon, or even PyC, silicon carbide, boron nitride or silicon nitride.
[0042] Of course, the fiber preform remains porous, after formation of the coating, in order to allow the formation of a PIP ceramic matrix phase linked to the coating via the adhesion promoter. This aspect will now be described through a first example of a method according to the invention, illustrated in figures 3 à 6 .
[0043] After formation of the coating 1 on the fibers, the adhesion promoter 10 is introduced into the residual porosity of the fiber preform (see figure 3 ). The adhesion promoter 10 can be introduced in the liquid state into the porosity of the fiber preform. The adhesion promoter 10 can be injected into the porosity of the fiber preform. The introduced liquid medium comprising the adhesion promoter 10 can fill the entire accessible porosity of the fiber preform. The introduced adhesion promoter 10 is in contact with the surface S of the coating 1 carrying the -OH groups. This surface S corresponds to the external surface of the coating 1, i.e. to the surface furthest from the wires forming the preform. In the example illustrated, the adhesion promoter 10 is a boron-based Lewis complex of general formula B1-BH 3 where B1 denotes a Lewis base. Other possible examples of Lewis complexes have been indicated above. For reasons of brevity, the figures only illustrate a boron-based adhesion promoter, but the same principle remains applicable when the promoter is aluminum-based.
[0044] The adhesion promoter comprises in particular a reactive structure S1 of formula B1-BH. The B1-B part (boron - Lewis base bond) is intended to react with the oxygen of the -OH groups, and the BH part (boron - hydrogen bond) is intended to react with the ceramic precursor resin.
[0045] A first heating can be carried out in order to graft the promoter 10 onto the surface S of the coating 1. This heating is however not obligatory, contact at room temperature (20°C) or at a lower temperature can be sufficient to graft the promoter to the coating of the fibers. The temperature imposed during the grafting can be between -50°C and +60°C, for example between -20°C and +30°C. The promoter 10 and the -OH groups are brought into contact for a sufficient time to carry out the grafting. This time depends on the chemical nature of the promoter chosen. For example, the promoter 10 and the -OH groups can be brought into contact for a time greater than or equal to 2 hours, for example greater than or equal to 3 hours, to carry out the grafting. The introduction of the adhesion promoter 10 and the grafting can be carried out under an inert atmosphere or under vacuum.During this grafting, boron is added to the oxygen of the -OH groups and there is departure of the Lewis base B1. The grafted promoter 20 is linked to the surface S of the coating 1 by a covalent bond between the oxygen of the -OH groups and the boron (see . figure 4 ).
[0046] After grafting, the grafted promoter 20 always has at least one dangling boron-hydrogen (BH) bond intended to react with the ceramic precursor resin (see figure 4 ).
[0047] Once the adhesion promoter 20 is grafted, a ceramic precursor resin 4 is introduced into the porosity of the fiber preform (see figure 5 ). The introduced resin 4 is in contact with the grafted promoter 20. The resin 4 can be introduced in the liquid state into the porosity of the fiber preform. The resin 4 can be injected into the porosity of the fiber preform. This resin 4 is known per se, and can be chosen from: polysiloxane resins, polysilazane resins, polycarbosiloxane resins, polycarbosilane resins, polycarbosilazane resins and mixtures of such resins.
[0048] Once the resin 4 is introduced, it will bind covalently to the grafted promoter 20. This bond is achieved by a chemical reaction between the BH bond and a reactive function carried by the resin 4. For example, the reactive function of the resin may be an NH group which can react with the BH bond of the promoter by a dehydrocoupling reaction to form a BN bond. This is the case, for example, when the resin is a polysilazane resin, such as that marketed under the reference “Durazane 1800” marketed by Merck. According to another example, a resin comprising a carbon-carbon double bond may be used as a reactive function which is capable of reacting with the BH bond of the promoter by a hydroboration reaction followed by dehydrocoupling in order to form a BC bond.This is the case, for example, when the resin is a polycarbosilane resin, such as that marketed under the reference "SMP-10" by Starfire ®< Systems. Whatever the embodiment considered, the chemical reaction between the resin introduced and the grafted adhesion promoter may comprise a dehydrocoupling reaction, possibly preceded by a hydroboration reaction.
[0049] The bonding of the resin 4 to the grafted promoter 20 is carried out by carrying out a second heating. The second heating makes it possible, at the same time, to polymerize the resin 4 and to activate the bonding reaction of the latter to the grafted promoter 20. It is within the general knowledge of the person skilled in the art to determine the temperature value to be imposed during the second heating depending on the resin and the grafted promoter 20 used. A temperature between 90°C and 250°C can typically be imposed during the second heating.
[0050] There figure 6 shows the bonding of the polymerized resin 40 to the grafted promoter 30. The grafted promoter 30 forms a bonding arm between the polymerized resin 40 and the coating 1. The polymerized resin 40 is then pyrolyzed to form a ceramic matrix phase in the porosity of the fiber preform.
[0051] It should be noted that the formation of the part matrix may involve carrying out several PIP cycles of introduction and pyrolysis of a ceramic precursor resin. In this case, an adhesion promoter can be grafted onto a matrix block obtained by PIP before each new introduction of the ceramic precursor resin. In this case, the adhesion promoter links the different PIP matrix blocks, in order to improve the adhesion of these blocks to each other.
[0052] THE figures 7 à 10 are analogous to figures 3 à 6 and relate to the case where the adhesion promoter 100 is a Lewis acid, here BH 3 . The adhesion promoter 100 comprises a reactive structure S2 of formula BH with B having an electronic gap represented diagrammatically by the empty rectangle at figure 7 The oxygen of the -OH groups is intended to fill this electronic gap, and the BH part is intended to react with the ceramic precursor resin. We thus obtain a promoter 20 grafted to the surface of the coating 1 ( figure 8 ). The interaction and reaction of the grafted promoter 20 with the resin 4 illustrated in figures 9 et 10 takes place in the same way as described previously.
[0053] Once obtained, the part thus manufactured may be a part for aeronautical or aerospace applications. The part may be a hot end part of a gas turbine of an aeronautical or aerospace engine or of an industrial turbine. The part may be a turbomachine part. The part may constitute at least part of a distributor, at least part of a nozzle or a thermal protection coating, a wall of a combustion chamber, a turbine ring sector or a turbomachine blade. Example
[0054] During the impregnation process, the fiber preform is kept in a sealed mold under an inert atmosphere. The fiber preform was made of SiC fibers (Hi-Nicalon S) coated with a SiC matrix obtained by CVI. Prior to the addition of the polymer, the fiber preform is impregnated with a controlled quantity of borane dimethylsulfide (2M in toluene, Sigma Aldrich). The borane dimethylsulfide is kept in contact with the coated fibers for 12 hours at 20°C and then the assembly is placed under dynamic vacuum to evacuate the solvent, i.e., toluene, which is condensed in a trap immersed in liquid nitrogen. After evaporation of the solvent, the mold is placed under static vacuum to impregnate the fiber preform with the preceramic polymer (Durazane 1800).After impregnation of the polymer, the assembly is maintained under dynamic vacuum and then placed under argon to be heat treated up to 130°C (solidification temperature of the polymer) before cooling to demould the fibrous preform impregnated with the polymer.
[0055] The expression "between ... and ..." must be understood as including the limits.
Claims
1. A method for manufacturing a part made of composite material comprising at least the following steps: a) introducing an adhesion promoter (10; 100) into the pores of a fibrous preform formed by yarns coated by a coating (1) having -OH groups at its surface (S), the adhesion promoter being a Lewis complex or a Lewis acid, the Lewis complex adhesion promoter (10) comprising a reactive structure S1 of formula B1-X-H, where B1 is a Lewis base, the Lewis acid adhesion promoter (100) comprising a reactive structure S2 of formula X-H with the atom X having an empty orbital, in these two alternatives, X designates boron or aluminium, b) grafting the adhesion promoter to the surface of the coating by addition on the -OH groups at the atom X, c) introducing a ceramic precursor resin (4) into the pores of the fibrous preform, after the step of grafting the adhesion promoter, d) polymerising the introduced resin and bonding the grafted adhesion promoter to the resin by chemical reaction between these two compounds at the X-H bond of the grafted promoter, this polymerisation and this bonding being carried out by heating the fibrous preform into which the resin has been introduced, e) forming a ceramic matrix phase in the pores of the fibrous preform by pyrolysis of the polymerised resin (40).
2. The method according to claim 1, wherein X is boron.
3. The method according to claim 1 or 2, wherein the adhesion promoter is a Lewis complex of general formula B1-BH3 or B1-AlH3.
4. The method according to any one of claims 1 to 3, wherein the adhesion promoter (10) is a Lewis complex and wherein the Lewis base B1 is of formula *-S-R2 or *-N-R3, with *- designating the bond to the atom X and in each of these formulas the R groups being identical or different and being a saturated or unsaturated hydrocarbon chain containing 1 to 12 carbon atoms.
5. The method according to any one of claims 1 to 3, wherein the adhesion promoter (100) is a Lewis acid of general formula R'2-BH or R'2-AlH, in each of these formulas the R' groups being identical or different and being a hydrogen atom, a saturated or unsaturated hydrocarbon chain containing 1 to 12 carbon atoms, the R' groups optionally together defining a same cyclic hydrocarbon chain.
6. The method according to any one of claims 1 to 5, wherein the ceramic precursor resin (4) comprises at least one reactive function reacting with the X-H bond of the adhesion promoter grafted during step d) and chosen from: a carbon-carbon double bond, an N-H group, an Si-H group or an OH group.
7. The method according to claim 6, wherein the reactive function is an allyl group or a vinyl group.
8. The method according to any one of claims 1 to 7, wherein the material forming the surface (S) of the coating (1) is chosen from: carbon, boron-doped carbon, silicon carbide, boron nitride, boron nitride doped with silicon or silicon nitride.
9. The method according to any one of claims 1 to 8, wherein the resin (4) is chosen from: polysiloxane resins, polysilazane resins, polycarbosiloxane resins, polycarbosilane resins, polycarbosilazane resins and the mixtures of such resins.