AI Technical Summary
Reducing the clinker content in cementitious compositions to minimize carbon impact while maintaining mechanical and rheological properties is challenging due to deterioration in fluidity, as existing adjuvants are not effective enough for compositions with reduced cement content.
A polymer adjuvant comprising specific units, such as those defined by formulas (I) and (II), is used to improve the fluidity of cementitious compositions with reduced clinker content, incorporating ether-linked comb polymer structures that enhance workability and delay setting, thereby maintaining fluidity over extended periods.
The polymer adjuvant significantly improves the maintenance of fluidity and workability of cement compositions with reduced clinker content, extending the period of effective fluidity to over 90 minutes and delaying setting time, outperforming other setting retarding agents and polymer types.
Description
[0001] The present invention relates to the use of an adjuvant for improving the fluidity maintenance of a cementitious composition with a reduced clinker content, an adjuvanted cementitious composition and its uses.
[0002] Common cement compositions include a significant proportion of clinker. For example, a cement composition according to the NF EN 197-1 standard of 2012 includes at least 65% by weight of clinker.
[0003] Research is underway to reduce the clinker content of cementitious compositions in order to reduce their carbon footprint, while maintaining their mechanical and rheological properties. New cementitious compositions in which part of the clinker is replaced by activated clays and limestones are beginning to emerge.
[0004] Patent application WO 2010 / 130511 describes a cementitious composition comprising activated clay.
[0005] One of the obstacles to the development of such compositions is that lowering the clinker content leads to a deterioration in the fluidity maintenance of the cement composition.
[0006] Most of the admixtures known to improve the fluidity maintenance of a cementitious composition with a usual cement content are not effective enough to improve that of a cementitious composition with a reduced cement content.
[0007] Application WO 2010 / 040915 teaches that adding a specific water-soluble cationic polymer to a hydraulic composition comprising calcined clays, and possibly a plasticizer, allows for better maintenance of workability.
[0008] Application WO 2019 / 094060 describes a cementitious composition comprising: from 30 to 95% by weight of hydratable cement, limestone or mixtures thereof, from 5 to 70% by weight of calcined clay comprising from 1 to 15% by weight of Fe 2 O 3 , from 0.002 to 0.2% by weight of a tertiary alkanolamine, the proportions being in relation to the dry weight of cement composition. The tertiary alkanolamine makes it possible to improve the pozzolanic reactivity of the activated clay and thus to improve the maintenance of fluidity at early and late ages.
[0009] There is a need to develop alternative methods to improve the fluidity maintenance of reduced clinker cementitious compositions.
[0010] One of the objectives of the present application is to provide an adjuvant which can be used as a fluidifier for such cementitious compositions.
[0011] Another objective is to provide a composition with a low clinker content and including activated clays whose mechanical and rheological properties allow its use as a cementitious composition.
[0012] According to a first subject, the invention relates to the use of an adjuvant comprising a polymer comprising units of the following formulae (I) and (II): in which: R 1< and R 2< independently represent hydrogen or methyl, R 3< represents hydrogen or a group of formula -COO(M) 1 / m R 4< represents a group of formula -(CH 2 ) p -(OAlk) q -R 5 in which: p represents 1 or 2, q represents an integer from 3 to 300, the Alk of each OAlk unit of the group -(OAlk) q - independently represents a linear or branched alkylene comprising from 2 to 4 carbon atoms, R 5< represents -OH or a linear or branched alkoxyl comprising from 1 to 4 carbon atoms, R 11< and R 12< independently represent hydrogen or methyl, R 13< represents hydrogen or a group of formula -COO(M) 1 / m , M represents H or a cation of valence m, when M represents H, m represents 1 and when M represents a cation, m is the valence of the cation M, a is a number from 0.05 to 0.25, such that (100 x a) represents the molar percentage of units of formula (I) within the polymer, and b is a number from 0.75 to 0.95,such that (100 xb) represents the molar percentage of units of formula (II) within the polymer, , as a fluidifier for a cementitious composition comprising: from 20 to 64% by weight of clinker, from 5 to 60% by weight of activated clay, from 0 to 35% by weight of limestone, from 0 to 10% by weight of calcium sulfate, the proportions being relative to the dry weight of the cement composition.
[0013] The following embodiments for formulas (I) and (II) of the polymer units can be considered independently or combined with each other: R 1< represents H, R 3< represents H, R 1< and R 3< represent H, R 2< represents a methyl, p represents 1, Alk represents -CH 2 -CH 2 -, -CH 2 -CH 2 -CH 2 -CH 2 -, -CH 2 -CH 2 -CH 2 -CH 2 -, -CH 2 -CHMe-, - CHMe-CH 2 -, at least 80% of the Alk of the group -(OAlk) q - represent -CH 2 -CH 2 -, or even all the Alk of the group -(OAlk) q - represent -CH 2 -CH 2 -, q represents an integer from 5 to 200, in particular from 10 to 100, preferably from 25 to 75, R 5< represents -OH or -OMe, preferably R 5< represents -OH, the sum of a and b is 1, R 11< represents H, R 13< represents H, R 11< and R 13< represent H, R 12< represents H, and / or M represents H or a monovalent or bivalent cation, m then representing 1 or 2, the monovalent cation preferably being chosen from an ammonium salt NH 4 +< , a primary, secondary, tertiary or quaternary ammonium cation and a cation of an alkali metal, such as a sodium, lithium or potassium ion,and the divalent cation preferably being a cation of an alkaline earth metal, such as a magnesium or calcium ion, a is a number from 0.05 to 0.20, preferably a represents a number between 0.10 and 0.20, b is a number from 0.80 to 0.95, preferably b represents a number between 0.80 and 0.90. ,
[0014] Preferably, the units of formula (I) of the polymer have the following formula (I'): in which: R 2< independently represents hydrogen or methyl, preferably methyl, R' 4< represents a group of formula -CH 2 -(O-CH 2 -CH 2 ) q -R 5 in which: q represents an integer from 3 to 500, R 5< represents -OH or -OMe, preferably -OH, a is a number from 0.05 to 0.25, such that (100 x a) represents the molar percentage of units of formula (I') within the polymer.
[0015] Preferably, the units of formula (II) of the polymer have the following formula (II'): in which: R 12< represents hydrogen or methyl, preferably hydrogen, M represents H or a cation of valence m, when M represents H, m represents 1 and when M represents a cation, m is the valence of the cation M, b is a number from 0.75 to 0.95, such that (100 xb) represents the molar percentage of units of formula (II') within the polymer.
[0016] Preferably, the polymer of the adjuvant used comprises units of formulas (I') and (II').
[0017] The following embodiments for formulas (I') and (II') of the adjuvant polymer may be considered independently or combined with each other: q represents an integer from 5 to 200, in particular from 10 to 100, preferably from 25 to 75, R 5< represents -OH or -OMe, preferably R 5< represents -OH, a is a number from 0.05 to 0.20, preferably a represents a number between 0.10 and 0.20, b is a number from 0.80 to 0.95, preferably b represents a number between 0.80 and 0.90, the sum of a and b is 1 (which implies that the polymer is made up of the units of formulae (I) and (II)), and / or M represents H or a monovalent or bivalent cation, m then representing 1 or 2, the monovalent cation preferably being chosen from an ammonium salt NH 4 +< , a primary, secondary, tertiary or quaternary ammonium cation and a cation of an alkali metal, such as a sodium, lithium or potassium ion, and the divalent cation preferably being a cation of an alkaline earth metal, such as a magnesium or calcium ion.
[0018] The polymer may comprise one or more additional units in addition to those of formula (I) and (II). Preferably, the polymer is free from the following unit of formula (V): wherein M represents H or a cation, such as sodium. Particularly preferably, the polymer is free of sulfonic acid and sulfonate groups.
[0019] Preferably, the polymer of the adjuvant used consists of the units of formulas (I) and (II). It does not include any additional units in addition to those of formulas (I) and (II). The sum of a and b is then 1.
[0020] The weight average molar mass of the polymer is generally 10,000 to 200,000 g / mol, especially 10,000 to 100,000 g / mol.
[0021] Generally, the polymer is obtained by free radical polymerization.
[0022] The polymer used is therefore a comb polymer whose pendant groups are linked to the main carbon chain by ether groups. The inventors observed that the polymer as defined above is capable of fluidifying a cementitious composition comprising: from 20 to 64% by weight of clinker, from 5 to 60% by weight of activated clay, from 0 to 35% by weight of limestone, from 0 to 10% by weight of calcium sulfate, the proportions being relative to the dry weight of the cementitious composition. This polymer makes it possible in particular to fluidify such a cementitious composition more effectively than a comb polymer whose pendant groups are linked to the main carbon chain by ester groups.
[0023] Furthermore, the inventors have observed that a polymer, the molar percentage of which in units of formula (I) is from 5 to 25% (therefore a from 0.05 to 0.25), in particular from 5 to 20% (therefore a from 0.05 to 0.20), preferably from 10 to 20% (therefore a from 0.10 to 0.20), is a more effective fluidifier of such cementitious compositions than when this molar percentage is higher.
[0024] The admixture comprising the polymer defined in the application makes it possible to increase the fluidity maintenance (also called workability maintenance) of a cementitious composition as defined above. The fluidity maintenance can in particular be measured using a rheometer by carrying out several measurements of the applied stress to obtain each strain rate value. Preferably, the admixture makes it possible to improve the fluidity maintenance of the cementitious composition over a period greater than or equal to 90 minutes, in particular greater than 120 minutes, or even greater than 240 minutes.
[0025] The adjuvant is generally used so that the proportion of polymer is from 0.001% to 5% by weight, in particular from 0.005% to 1%, preferably from 0.01% to 0.2% relative to the dry weight of the cementitious composition to be fluidized.
[0026] The adjuvant may further comprise a setting retarding agent.
[0027] In the context of this application, the term "setting retarder" is understood to mean a compound having the effect of delaying the setting of the cementitious composition, that is to say of delaying or inhibiting the phenomena linked to this setting such as hydration phenomena, thereby inducing later hardening of the composition. Generally, a setting retarder delays the setting time of a cementitious composition into which it has been introduced at a dosage of at most 5% by dry weight relative to the weight of the clinker, the setting time being measured according to the EN480-2 (2006) test. Preferably, the setting time is delayed by at least 30 minutes compared to a control cementitious composition.
[0028] The setting retardant is chosen in particular from: a carboxylic or hydroxycarboxylic acid in neutral form or a salt thereof, those having a pK A of 2 to 5 being preferred. The carboxylic acid being chosen in particular from acetic acid, gluconic acid, citric acid, tartaric acid, malic acid or a mixture thereof, a phosphonic acid in neutral form or a salt thereof, chosen in particular from those comprising a group -N[-(CH 2 )-PO(OH) 2 ] 2 or a group >C[-PO(OH) 2 ] 2 , preferably chosen from amino tri methylene phosphonic acid (ATMP), ethylene diamine tetra methylene phosphonic acid (EDTMP), 1-hydroxyethylidene -1,1,-diphosphonic acid (HEDP), and their salts, in particular sodium.a sugar, in particular chosen from glucose, gluconic acid in neutral form or a salt thereof or in lactone form, dextrose, fructose, galactose, sucrose, maltose, lactose and mannose and mixtures thereof, a phosphate, in particular chosen from sodium tripolyphosphate and tetrapotassium pyrophosphate and mixtures thereof. and mixtures thereof.
[0029] The salt of the carboxylic acid is preferably an alkali metal salt, such as sodium, lithium or potassium, an alkaline earth metal salt, such as a magnesium or calcium salt or an ammonium salt NH 4 +< or primary, secondary, tertiary or quaternary ammonium cation.
[0030] The preferred setting retarding agent is a phosphonic acid in neutral form or a salt thereof, preferably one of those described above, gluconic acid in neutral form or a salt thereof, preferably sodium gluconate, or a mixture thereof. The inventors have in fact observed that an adjuvant comprising, in addition to the polymer defined above, one of these preferred retarding agents, makes it possible to more effectively fluidify the cementitious composition defined in the application than other setting retarding agents.
[0031] Generally, within the admixture, the ratio of the weight of polymer to the weight of the setting retarding agent is 1 / 2 to 2 / 1, preferably 2 / 3 to 3 / 2.
[0032] The adjuvant used may further comprise an anti-foam additive and / or an air-entraining additive, and one or more solvents such as water.
[0033] The adjuvant may consist of the polymer defined above and possibly a setting retardant.
[0034] The cement composition to be fluidified by the adjuvant includes: from 20 to 64% by weight, preferably from 35 to 60% by weight, of clinker, from 5 to 60% by weight of activated clay, from 0 to 35% of limestone, from 0 to 10% of calcium sulfate, the proportions being by weight relative to the dry weight of the cement composition.
[0035] Such a cement composition is not usual in that its proportion of clinker is low and its proportion of activated clay is high. The cement composition is notably of type LC 3< (“limestone calcined clay cement” in English), and / or it can be a CEM II / CM Q -L or LL of the provisional standard prEN 197-5.
[0036] The clinker is in particular Portland clinker, preferably Portland clinker as defined in the book "Cement Chemistry". Harry FW Taylor. Edition, 2., Academic Press, 1990).
[0037] The cementitious composition comprises from 0 to 35% by weight, preferably from 10 to 30% by weight of limestone, the proportions being by weight relative to the dry weight of the cementitious composition.
[0038] The limestone is preferably as defined in the Cement standard NF EN 197-1(2012) paragraph 5.2.6.
[0039] The cementitious composition comprises from 0 to 10% by weight, preferably from 1 to 5% by weight of calcium sulfate, the proportions being by weight relative to the dry weight of the cementitious composition.
[0040] Calcium sulfate can be in dehydrated, hydrated form, or a mixture of these. Hydrated calcium sulfate can be monohydrate, dihydrate, or a mixture of these. Dihydrated calcium sulfate with the formula CaSO 4 .2H 2 O is gypsum. Gypsum is therefore an example of calcium sulfate.
[0041] "Activated clay" means a clay that has undergone dehydroxylation. As used herein, the term "dehydroxylation" refers to the loss of one or more hydroxyl (OH) groups in the form of water (H 2 O) from a clay.
[0042] Preferably, the activated clay is a kaolinic (also called kaolinitic) clay that has been activated. A “kaolinic clay” means a clay that includes kaolinite. A “kaolinic clay that has been activated” is a kaolinic clay, at least a portion of the kaolinite of which has been dehydroxylated to metakaolin. For example, upon heating the clay mineral kaolinite from 300 to 600°C, water is lost according to the following reaction. Al 2 Si 2 O 5 (OH) 4 → Al 2 Si 2 O 7 + 2H 2 O
[0043] Thus, an activated kaolin clay includes, or even consists of, metakaolin. Metakaolin is very reactive in the presence of water and portlandite to form hydrated phases, including calcium aluminosilicate hydrate (CASH) and stratlingite.
[0044] For the purposes of the application, the activated kaolin clay may comprise residual kaolinite (which has not been dehydroxylated during activation) in a content, as measured by thermogravimetric analysis (TGA), typically by raising the temperature between 30 and 900°C, with, for example, a heating rate of 10°C / min, which makes it possible to quantify the loss of mass corresponding to the water released by the clay. This residual kaolinite content is generally less than or equal to 50% by weight, typically less than or equal to 40% by weight, in particular less than or equal to 30% by weight, preferably less than or equal to 20% by weight, particularly preferably less than or equal to 10% by weight, relative to the weight of the activated clay. The activated kaolin clay may be free of kaolinite (the dehydroxylation has then been complete).
[0045] Dehydroxylation can be carried out by thermal, mechanical and / or chemical treatment.
[0046] Mechanical treatment can be, for example, that described in the article "Preparation of pozzolanic addition by mechanical treatment of kaolin clay" Aleksandra Mitrović, Miodrag Zdujić. International Journal of Mineral Processing 132 (2014) 59-66.
[0047] Heat treatment is calcination, generally at a temperature between 400 and 700°C (dehydroxylation temperature). We then speak of kaolin clay having been calcined.
[0048] Calcination is most often carried out in a rotary kiln into which the clay is introduced. The kaolin is transformed at least partially into an amorphous and reactive phase, with a strong pozzolanic power, called metakaolin. The calcined clay is then ground. Calcination can be carried out by the "flash" method where the clay is ground and the fine particles are calcined in a few seconds in a kiln.
[0049] Regardless of the activation method used (in particular mechanical or thermal), the activated clay can undergo additional activation chemically using compounds capable of complexing cations, preferably compounds capable of complexing calcium.
[0050] The activated kaolin clay can be, for example, ARGICAL 1000 from AGS.
[0051] The cementitious composition may comprise one or more additives, for example an antifoam additive, an air-entraining additive and / or a grinding agent.
[0052] The milling agent may or may not be an alkanolamine.
[0053] Preferably, the cementitious composition comprises less than 0.001% by cumulative weight of diethanolisopropanolamine (DEIPA), triisopropanolamine (TIPA), N,N-bis(2-hydroxypropyl)-N-(hydroxyethyl)amine (EDIPA) and triethanolamine (TEA) relative to the dry weight of the cementitious composition. Particularly preferably, the cementitious composition and / or the admixture is (are) free of DEIPA, TIPA, EDIPA and TEA.
[0054] Preferably, the cementitious composition comprises less than 0.001% by weight of tertiary alkanolamine comprising from 1 to 6 carbon atoms relative to the dry weight of the cementitious composition. The cementitious composition and / or the admixture is (are) generally free of tertiary alkanolamine comprising from 1 to 6 carbon atoms, or even of alkanolamine comprising from 1 to 6 carbon atoms, or even of alkanolamine.
[0055] Preferably, the cementitious composition and / or the admixture are free of cationic polymer having a cationic charge density greater than 0.5 meq / g and an intrinsic viscosity less than 1 dl / g, or even of cationic polymer. The intrinsic viscosity and the cationic charge density are as measured in application WO 2010 / 040915. The cationic charge density is measured by colloidal titration with an anionic polymer in the presence of a colored indicator sensitive to the ionicity of the excess polymer. The intrinsic viscosity measurements of the cationic polymers are carried out in a 3 M NaCl solution, with a Ubbelhode type capillary viscometer, at 25°C. The flow time in the capillary tube is measured between 2 marks for the solvent and solutions of the polymer at different concentrations. The reduced viscosity is calculated by dividing the specific viscosity by the concentration of the polymer solution.The specific viscosity is obtained for each concentration by dividing the difference between the flow times of the polymer solution and the solvent by the flow time of the solvent. By plotting the reduced viscosity line as a function of the concentration of the polymer solution, a straight line is obtained. The intersection with the ordinate of this line corresponds to the intrinsic viscosity for a concentration equal to zero.
[0056] In one embodiment, the cementitious composition consists of: from 20 to 64% by weight of clinker, from 5 to 60% by weight of activated clay, from 0 to 35% by weight of limestone, from 0 to 10% by weight of calcium sulfate, from 0 to 5% by weight of a grinding agent, from 0 to 5% by weight of anti-foam additive, and from 0 to 5% by weight of air-entraining additive, the proportions being relative to the dry weight of the cement composition.
[0057] Preferably, within the cementitious composition, the mass ratio of the weight of calcined clay to the weight of limestone is from 1 / 2 to 5 / 1, preferably from 1 / 1 to 3 / 1, particularly preferably from 3 / 2 to 5 / 2.
[0058] Preferably, within the cementitious composition, the mass ratio of the weight of clinker relative to the weight of activated clay is from 1 / 4 to 4 / 1, in particular from 1 / 1 to 3 / 1, preferably from 3 / 2 to 5 / 2.
[0059] Preferably, within the cementitious composition, the mass ratio of the weight of clinker to the weight of limestone is from 1 / 1 to 10 / 1, in particular from 3 / 1 to 5 / 1.
[0060] Preferably, the cementitious composition contains: from 5 to 25% by weight, preferably from 6 to 20% by weight, of Al 2 O 3 , from 25 to 55% by weight, preferably from 40 to 50% by weight, of CaO, from 20 to 40% by weight, preferably from 22 to 35% by weight, of SiO 2 , from 2 to 10% by weight, preferably from 2 to 5% by weight of SO 3 , and / or from 0.1 to 10% by weight, preferably from 0.5 to 8% by weight, of Fe 2 O 3 , relative to the sum of the dry weights of clinker, activated clay, limestone and calcium sulfate.
[0061] According to a second subject, the invention relates to an adjuvanted cementitious composition comprising: a cementitious composition comprising: from 20 to 64% by weight of clinker, from 5 to 60% by weight of activated clay, from 0 to 35% by weight of limestone, from 0 to 10% by weight of calcium sulfate, the proportions of clinker, activated clay, limestone and calcium sulfate being relative to the dry weight of the cementitious composition, and the admixture as defined above, the proportion of polymer in the adjuvant being from 0.001% to 5% by weight, in particular from 0.005% to 1%, preferably from 0.01% to 0.2% relative to the dry weight of the cementitious composition.
[0062] For the purposes of the application, the term "adjuvanted cementitious composition" means a composition comprising the cementitious composition as defined above and the adjuvant as defined above, and the term "cementitious composition" means the cementitious composition free of adjuvant (this is the cementitious composition to be fluidified).
[0063] The embodiments defined above for the cementitious composition are applicable for the admixed cementitious composition.
[0064] The admixed cementitious composition may include or be free of a grinding agent. The grinding agent may or may not be an alkanolamine.
[0065] Preferably, the admixed cementitious composition comprises less than 0.001% by cumulative weight of diethanolisopropanolamine (DEIPA), triisopropanolamine (TIPA), N,N-bis(2-hydroxypropyl)-N-(hydroxyethyl)amine (EDIPA) and triethanolamine (TEA) relative to the dry weight of the admixed cementitious composition. Particularly preferably, the admixed cementitious composition is free of DEIPA, TIPA, EDIPA and TEA.
[0066] Preferably, the admixed cementitious composition comprises less than 0.001% by weight of tertiary alkanolamine comprising from 1 to 6 carbon atoms relative to the dry weight of the cementitious composition. The admixed cementitious composition is generally free of tertiary alkanolamine comprising from 1 to 6 carbon atoms, or even alkanolamine.
[0067] Preferably, in addition to the adjuvant defined above, the adjuvanted cementitious composition is free of fluidifying adjuvant and / or adjuvant capable of delaying the setting of the adjuvanted cementitious composition.
[0068] Preferably, the admixed cementitious composition is free of cationic polymer having a cationic charge density greater than 0.5 meq / g and an intrinsic viscosity less than 1 dl / g, or even of cationic polymer.
[0069] The admixed cementitious composition preferably consists of the cementitious composition defined above and the admixture defined above.
[0070] Preferably, the admixed cementitious composition meets the criteria defined in ASTM C1157 of 2020.
[0071] According to a third subject, the invention relates to a method for improving the fluidity maintenance (also called workability maintenance) over time of a cementitious composition comprising bringing the cementitious composition defined above into contact with an adjuvant as defined above. This improvement is preferably long-term, namely over a period greater than or equal to 90 minutes, in particular greater than 120 minutes, or even greater than 240 minutes.
[0072] According to a fourth subject, the invention relates to a process for preparing the admixed cementitious composition comprising the step of mixing the cementitious composition as defined above, the admixture as defined above and water.
[0073] According to a fifth object, the invention relates to the use of the adjuvanted cementitious composition defined above for the preparation of a hydraulic composition.
[0074] According to a sixth subject, the invention relates to a hydraulic composition comprising (or even consisting of) the admixed cementitious composition defined above, water, an aggregate and optionally one or more mineral additions. The hydraulic composition is preferably a concrete, mortar or screed composition.
[0075] Aggregates are defined as a set of mineral grains with an average diameter of between 0 and 125 mm. Depending on their diameter, aggregates are classified into one of the following six families: fillers, sand, gravel, gravel and ballast (standard XP P 18-545). The most commonly used aggregates are: fillers, which have a diameter less than 2 mm and for which at least 85% of the aggregates have a diameter less than 1.25 mm and at least 70% of the aggregates have a diameter less than 0.063 mm, sands with a diameter between 0 and 4 mm (in standard 13-242, the diameter can go up to 6 mm), gravel with a diameter greater than 6.3 mm, gravel with a diameter between 2 mm and 63 mm. Sands are therefore included in the definition of aggregate according to the invention. Fillers can be of limestone or dolomitic origin.
[0076] The term "mineral additions" means slags (as defined in the Cement standard NF EN 197-1(2012) paragraph 5.2.2), steelworks slags, pozzolanic materials (as defined in the Cement standard NF EN 197-1(2012) paragraph 5.2.3), fly ash (as defined in the Cement standard NF EN 197-1(2012) paragraph 5.2.4), calcined schists (as defined in the Cement standard NF EN 197-1(2012) paragraph 5.2.5), or silica fumes (as defined in the Cement standard NF EN 197-1(2012) paragraph 5.2.7 or the prEN 197-5 standard paragraph 5), limestones or their mixtures.
[0077] The invention is illustrated in the following examples and figures.
[0078] [ Fig 1 ] There figure 1 represents the hydration kinetics of a cement composition (heat flow in mW / g of cement composition as a function of time in hours): of a cementitious composition without admixture (reference) (solid line), of an admixed cementitious composition, the admixture comprising polymer 5 at a dosage of 0.15% by weight relative to the dry weight of the cementitious composition (the admixed cementitious composition being free of setting retarder) (dotted line), or of an admixed cementitious composition, the admixture comprising polymer 5 at 0.1% by weight and sodium gluconate at 0.08% by weight relative to the dry weight of the cementitious composition (mixed line) (example 3). EXAMPLE 1: Impact of the nature of the polymer and the presence of a setting retarding agent on the fluidification of a cement composition.
[0079] The polymers described below were tested on a mixture of cementitious composition and water (cement paste). A rheological study with 2 hours of hydration was carried out.
[0080] The cement composition used was composed of approximately 50% clinker and approximately 50% of a mixture of metakaolin, limestone and gypsum (Table 1). [Table 1] Table 1-Mineralogical analysis by X-ray diffraction of the cement composition used Phase name Formula Mass content (%) Alite Ca 3 SiO 5 25,3-32,7 Belite Ca 2 SiO 5 5,7-15,2 Aluminate Ca 3 Al 2 O 6 0,3-2,5 Ferrite Ca 4 Al 2 Fe 2 O 10 6,8-8,1 Total clinker phases 37,6-59,1 Calcium sulfate 7,6-8,1 Quartz* SiO 2 1,2-1,6 Free lime* CaO 0,1-0,4 Portlandite Ca(OH) 2 0-1,3 Calcite* CaCO 3 13,5-15 Aragonite* CaCO 3 0,0-1,3 Periclase* MgO 0,0-1,7 Dolomite CaMgCO 3 2,2-3,4 Aphthitalitis K 3 Na(SO 4 ) 2 0,0-0,5 Thenardite* Na 2 SO 4 0,2-0,3 Syngenite K 2 Ca(SO 4 ) 2 H 2 0 0,0-0,7 Mullite Al 6 Si 2 O 13 1,8-2,0 Hematite Fe 2 O 3 0,0-0,7 Amorphous phases 16,2-17,4 Kaolinite Al 2 Si 2 O 5 (OH) 4 2,7-3,4 Description of the polymers used:
[0081] The polymers used in the examples are comb polymers whose pendant groups are linked to the main carbon chain either by ether groups (polymers 5 and 6) or by ester groups (polymers 1 to 4 and 7).
[0082] Comb polymers whose pendant groups are linked to the main carbon chain by ether groups were obtained by free radical polymerization with HPEG 2400 and consist of the units of the following formulas: where a, b and q are as defined in Table 2 below. The average total number of units in the polymer is the sum of the average number of units of formula (I") and the average number of units of formula (II").
[0083] Polymer 5 is a polymer as defined in the application.
[0084] The percentage in formula unit (I") of polymer 6 is greater than 30%. It is therefore a comparative polymer.
[0085] Comb polymers whose pendant groups are linked to the main carbon chain by ester groups (comparative) were obtained by polymerization then post-esterification to graft the pendant groups, for example with MPEG 750 for polymer 7, or a mixture of MPEG for polymers 1 and 4 (two values of "q" in Table 2 below). They consist of the following units of formulas (XI) and (XII): in which R represents H or methyl.
[0086] The average total number of units in the polymer is the sum of the average number of units of formula (XI) and the average number of units of formula (XII). [Table 2] Table 2: q, a, b and average total number of units in each polymer tested, and preparation method. Polymer Made up of formula units q a* b* Preparation process 1 (comparative) (XI) and (XII) with R = Me q1 = 114 = 0,20 0,80 Polymerization then post-esterification q2 = 45 2 (comparative) (XI) and (XII) with R = Me 17 0,25 0,75 Polymerization then post-esterification 3 (comparative) (XI) and (XII) with R = Me 45 0,20 0,80 Polymerization then post-esterification 4 (comparative) (XI) and (XII) with R = Me 31 0,40 0,60 Polymerization then post-esterification q1 = 45 q2 = 17 5 (invention) (I") and (II") 50 0,18 0,82 Free radical polymerization 6 (comparative) (I") and (II") 50 0,33 0,67 Free radical polymerization 7 (comparative) (XI) and (XII) with R = H 17 0,47 0,53 Polymerization then post-esterification *: determined by gel permeation chromatography (GPC). Whether during free radical polymerization or post-esterification, a certain amount of residual monomer remains in solution after synthesis. These residual monomers can be quantified by GPC. The difference between this residual amount and the starting amount of monomer is the amount of monomer that has been polymerized, and therefore a, then b = 1 - a. Experimental protocol:
[0087] The cementitious composition was prepared as follows, using a KENWOOD KM011 CHEF TITANIUM mixer with a stainless steel bowl (capacity 4.6 liters) and a sage leaf-shaped metal stirring blade (height 13 cm and width 13.6 cm), and its fluidity was measured as follows: 1. Water and admixture are weighed into the mixer bowl, then the mixer is started at a speed of 43 rpm. 2. The timer is started and the cementitious composition is introduced into the bowl in 30 seconds. 3. The speed is increased to 96 rpm and the mixture is mixed for one minute. 4. The mixer is stopped for 30 seconds, any admixed cementitious composition projected onto the walls is scraped towards the center with a spatula. 5. The admixed cementitious composition is mixed for one minute at 96 rpm. At the end of mixing, the resulting cementitious admixture composition, which is in the form of a paste, is poured into the cylindrical measuring cell of a Kinexus Pro rheometer (Netzsch) equipped with a fin-type measuring geometry.
[0088] Five minutes after the start of mixing, the admixed cementitious composition is subjected to a one-minute pre-shear at a strain rate of 200 s -1< . The admixed cementitious composition is then subjected to a series of decreasing strain rate steps, in logarithmic jumps from 200 to 0.01 s -1< and the rheometer records the stress to be applied at each point. This makes it possible to develop a flow curve linking the applied stress to obtain each strain rate value. These flow curves present a minimum stress which is interpreted as a threshold stress, i.e. a minimum stress to be applied to cause flow. This value varies inversely with the fluidity, so we seek to reduce it as much as possible.
[0089] A flow curve measurement is then carried out every 30 min up to 120 min after the start of mixing to check the evolution of fluidity over time.
[0090] In a first series of tests, the ratio of water weight to the weight of the cementitious composition (dry weight) was 0.45. The admixture consisted of one of the polymers (no retarding agent). For each test, the proportion of polymer was 0.1% by weight relative to the dry weight of the cementitious composition to be fluidized. The results are provided in Table 3. [Table 3] Table 3: threshold stress of the admixed cement composition according to the nature of the admixture polymer. Threshold stresses (Pa) Polymer 5 min 30 min 60 min 90 min 120 min 1 (comparative) 6,7 19,2 37,2 45,9 54,3 2 (comparative) 20,9 23,5 34,7 41,3 48,8 3 (comparative) 11,4 22,6 35,0 42,6 49,7 4 (comparative) 32,8 23,2 36,4 45,9 59,4 5 (invention) 0,8 2,6 5,8 12,1 17,8
[0091] These results demonstrate that polymer 5 according to the invention is by far the best fluidifier. It allows a significant reduction in the initial threshold stress and an improvement in maintaining the fluidity of the admixed cementitious composition over a period greater than or equal to 120 minutes.
[0092] In a second series of tests, the ratio of water weight to the weight of the cementitious composition (dry weight) was 0.35. The admixture consisted of polymer 5 (no setting retarder). Given the lower quantity of water compared to the first series of tests, the dosage of polymer 5 was increased to 0.15% by weight relative to the dry weight of the cementitious composition to be fluidized, in order to obtain the desired threshold stresses. The results are provided in Table 4 (row "polymer 5").
[0093] In a third series of tests, the ratio of water weight to cementitious composition weight (dry weight) was maintained at 0.35. The admixture consisted of polymer 5 and a sodium gluconate solution as a setting retarding agent. The dosage of polymer 5 was reduced to 0.10% by weight relative to the dry weight of the cementitious composition to be fluidized. The dosage of sodium gluconate was 0.08% by weight relative to the dry weight of the cementitious composition to be fluidized. The results are provided in Table 4 (row "polymer 5 + sodium gluconate"). [Table 4] Table 4: threshold stress of the admixed cement composition according to the nature of the admixture. Threshold stresses (Pa) Adjuvant 5 min 30 min 60 min 90 min 120 min Polymer 5 (invention) 3,5 9,8 17,4 22,8 28,6 Polymer 5 + sodium gluconate (invention) 1,0 2,9 5,1 8,0 9,5
[0094] The results show that the addition of a setting retarding agent improves the fluidity of the admixed cement composition, even when reducing the polymer dosage 5.
[0095] In a fourth series of tests, the ratio of water weight to cementitious composition weight (dry weight) was maintained at 0.35. The admixture consisted of one of the polymers and a sodium gluconate solution as a setting retarding agent. The polymer dosage was 0.125% by weight relative to the dry weight of the cementitious composition to be fluidized. The sodium gluconate dosage was 0.1% by weight relative to the dry weight of the cementitious composition to be fluidized. The results are provided in Table 5. [Table 5] Table 5: threshold stress of the admixed cement composition according to the nature of the admixture. Threshold stresses (Pa) Adjuvant 5 min 30 min 60 min 90 min 120 min Polymer 5 + sodium gluconate (invention) 5,2 4,8 4,9 4,8 5,4 Polymer 6 + sodium gluconate (comparison) 76,8 57,1 95,8 115,1 120,7 Polymer 7 + sodium gluconate (comparison) 68,1 49,7 61,8 72,9 87,3
[0096] These results show that an adjuvant comprising polymer 5 according to the invention and sodium gluconate as a setting retarding agent is by far the best fluidifier compared to adjuvants comprising other polymers and the same setting retarding agent. EXAMPLE 2: Impact of the nature of the setting retarding agent of the admixture on the fluidification of a cementitious composition
[0097] The polymer 5 described above was tested with different setting retarding agents on a cementitious composition to be fluidized. A rheological study with 2 hours of hydration was carried out.
[0098] The cement composition and experimental protocol are identical to those described in example 1.
[0099] The selected setting retarding agents are conventional retarders used to reduce the hydration kinetics of cement. Among these, carboxylic acids (citric acid, tartaric acid, salicylic acid), a phosphonic acid in neutral form or a salt thereof and a sucrose-type sugar were evaluated.
[0100] The ratio of water weight to cementitious composition weight (dry weight) was 0.35. The admixture consisted of polymer 5 and the setting retarder. The dosage of polymer 5 was 0.125% by weight relative to the dry weight of the cementitious composition to be fluidized. The dosage of setting retarder was 0.1% by weight relative to the dry weight of the cementitious composition to be fluidized. The results are provided in Table 6. [Table 6] Table 6: threshold stress of the admixed cementitious composition according to the nature of the admixture comprising polymer 5 and a setting retarding agent of a different nature. Threshold stresses (Pa) Adjuvant 5 min 30 min 60 min 90 min 120 min Polymer 5 + sodium gluconate 5,2 4,8 4,9 4,8 5,4 Polymer 5 + citric acid 5,9 49,0 76,7 71,4 68,8 Polymer 5 + tartaric acid 9,6 164,8 256,3 280,7 258,3 Polymer 5 + salicylic acid 70,7 111,2 92,1 81,0 78,1 Polymer 5 + sugar (sucrose) 18,0 49,2 43,2 37,4 34,0 Polymer 5 + phosphonic acid (ATMP) 2,1 3,1 4,4 5,7 6,8
[0101] These results show that adjuvants comprising, in addition to polymer 5, sodium gluconate or phosphonate allow better fluidification than those comprising other setting-retarding agents. EXAMPLE 3: Impact of admixtures on the hydration kinetics of the cement composition
[0102] Isothermal microcalorimetry tests (TAM Air calorimeter, TA Instruments) were used to assess the impact of admixtures on the hydration kinetics of the cement composition. Since hydration of the cement composition is an exothermic reaction, isothermal calorimetry allows us to obtain the evolution of the heat flux released per gram of the cement composition as a function of time.
[0103] The cement paste is prepared from a mixture of cementitious material, admixtures and water. A water to binder ratio (W / B) of 0.35 is set for all pastes. The agitation system consists of a turbine stirring blade (diameter 2.5 cm) attached to an IKA mixer and a 50 mL stainless steel beaker. The admixtures and water are first weighed and mixed in the stainless steel beaker. The water provided by the admixture is subtracted from the mixing water. The cementitious composition powder is added to the water, which marks the start of hydration. The suspension is mixed for one minute at a speed of 500 rotations per minute. Then the mixing is stopped, the edges of the beaker and the blade are scraped for one minute. Finally, the agitation is restarted at a speed of 1000 rotations per minute for one minute. The cement paste is then ready for analysis.
[0104] To reproduce the same experimental conditions as those of the rheological tests, the cement pastes were prepared: without adjuvant (reference), with polymer 5 at a dosage of 0.15% by weight relative to the dry weight of the cementitious composition (without setting retarder), or with a mixture of polymer 5 at 0.1% and sodium gluconate at 0.08% by weight relative to the dry weight of the cementitious composition. The results are illustrated in the figure 1 and show that polymer 5 at a dosage of 0.15% by weight relative to the dry weight of the cementitious composition provides a delay of approximately 30 minutes compared to the reference containing the cementitious composition without admixture. Polymer 5 at a dosage of 0.1% by weight relative to the dry weight of the cementitious composition in combination with sodium gluconate at a dosage of 0.08% by weight relative to the dry weight of the cementitious composition delays the hydration kinetics of the cementitious compositions by approximately 6 hours compared to the reference containing the cementitious composition without admixture. However, the setting retarder has no impact on the intensity of the main hydration peak of the cementitious composition. EXAMPLE 4: Example with another cement composition: Impact of the nature of the polymer and the presence of a setting retarding agent on the fluidification of a cement composition 2.
[0105] Tests are carried out with a cement composition 2 comprising a clinker of a different nature from that previously used (out of stock), but whose metakaolin, limestone and gypsum mixture is as described in Table 1. In view of the different nature of the clinker, the following results cannot strictly be compared with those in Tables 4 and 5 above.
[0106] The cement composition 2 used was composed of approximately 50% clinker and approximately 50% of the metakaolin, limestone and gypsum mixture (Table 7). [Table 7] Table 7-Mineralogical analysis by X-ray diffraction of the cement composition 2 used Phase name Formula Mass content (%) Alite Ca 3 SiO 5 24,7-25,7 Belite Ca 2 SiO 5 11,6-12,6 Aluminate Ca 3 Al 2 O 6 0,9-1,9 Ferrite Ca 4 Al 2 Fe 2 O 10 5,9-9,9 Total clinker phases 44,1-51,1 Calcium sulfate 7,6-8,1 Quartz* SiO 2 1,2-1,6 Free lime* CaO 0,1-0,3 Portlandite Ca(OH) 2 0,0-0,5 Calcite* CaCO 3 13,5-15,0 Aragonite* CaCO 3 0,0-0,2 Periclase* MgO 0,0-0,2 Dolomite CaMgCO 3 2,2-3,4 Aphthitalitis K 3 Na(SO 4 ) 2 0,0 Thenardite* Na 2 SO 4 0,2-0,3 Syngenite K 2 Ca(SO 4 ) 2 H 2 0 0,0-0,7 Mullite Al g Si 2 O 13 1,8-2,0 Hematite Fe 2 O 3 0,0 Amorphous phases 16 ,< 2-17,4 Kaolinite Al 2 Si 2 O 5 (OH) 4 2,7-3,4
[0107] The experimental protocol is identical to those described in examples 1 and 2.
[0108] The ratio of water weight to cement composition 2 weight (dry weight) was 0.35.
[0109] The adjuvant was: either polymer 5 (free of retarding agent) with a dosage of 0.1% by weight relative to the dry weight of the cementitious composition 2 to be fluidized, or polymer 5 and sodium gluconate as a setting retarding agent, with a dosage of 0.1% by weight of polymer 5 and 0.08% by weight of sodium gluconate, each relative to the dry weight of the cementitious composition 2 to be fluidized, or polymer 6 (comparative) (free of retarding agent) with a dosage of 0.1% by weight relative to the dry weight of the cementitious composition 2 to be fluidized.
[0110] The results are provided in Table 8. [Table 8] Table 8: threshold stress of the cement composition 2 admixed according to the nature of the admixture. Threshold stresses (Pa) Adjuvant setting retardant 5 min 30 min 60 min 90 min 120 min invention 0.1% polymer 5 none 20,0 35,2 53,9 68,6 86,6 invention 0.1% polymer 5 0.08% sodium gluconate 1,6 0,7 0,8 1,0 1,0 comparative 0.1% polymer 6 none 24,6 56,2 93,2 125,0 160,2
[0111] The use of 0.1% of polymer 5 by weight relative to the dry weight of the cementitious composition 2 to be fluidized, leads to an increase in the threshold stress of the admixed cementitious composition 2 whereas the use of 0.1% by weight of polymer 5 and 0.08% by weight of sodium gluconate, each relative to the dry weight of the cementitious composition 2 to be fluidized, makes it possible to maintain a threshold stress at a low and constant level.
[0112] The use of 0.1% of polymer 6 (comparative) by weight relative to the dry weight of the cementitious composition 2 to be fluidized, leads to a greater increase in the threshold stress of the admixed cementitious composition 2 than that obtained by the use of 0.1% of polymer 5 (invention) by weight relative to the dry weight of the cementitious composition 2 to be fluidized. Polymer 6 is less efficient than polymer 5.
Claims
1. An admixed cement composition comprising: - a cement composition comprising: - from 20 to 64 weight % clinker, - from 5 to 60 weight % activated clay, - from 0 to 35 weight % limestone, - from 0 to 10 weight % calcium sulfate, the proportions of clinker, activated clay, limestone and calcium sulfate being relative to the dry weight of the cement composition and - an admixture comprising a polymer comprising units of following formulas (I) and (II): where: - R1 and R2 are each independently a hydrogen or a methyl, - R3 is a hydrogen or a group of formula -COO(M)1 / m - R4 is a group of formula -(CH2)p-(OAlk)q-R5 where: - p is 1 or 2, - q is an integer of 3 to 300, - the Alk in each OAlk unit of the group -(OAlk)q- is independently a linear or branched alkylene having 2 to 4 carbon atoms, - R5 is -OH or a linear or branched alkoxyl having 1 to 4 carbon atoms, - R11 and R12 are each independently a hydrogen or a methyl, - R13 is a hydrogen or a group of formula -COO(M)1 / m, - M is H or a cation of valence m, - when M is H, m is 1 and when M is a cation, m is the valence of the cation M, - a is a number from 0.05 to 0.25, such that (100 x a) represents the molar percentage of units of formula (I) within the polymer, and - b is a number from 0.75 to 0.95, such that (100 x b) represents the molar percentage of units of formula (II) within the polymer, the proportion of polymer in the admixture being from 0.001 weight % to 5 weight %, in particular from 0.005 weight % to 1 weight %, preferably from 0.01 weight % to 0.2 weight % relative to the dry weight of the cement composition.
2. The admixed cement composition according to claim 1, wherein the polymer of the admixture comprises units of following formulas (I') and (II'): where: - R2 is independently a hydrogen or a methyl, preferably a methyl, - R'4 is a group of formula -CH2-(O-CH2-CH2)q-R5 where: - q is an integer of 3 to 500, - R5 is -OH or -OMe, preferably -OH, - a is a number from 0.05 to 0.25, such that (100 x a) represents the molar percentage of units of formula (I') within the polymer, - R12 is a hydrogen or a methyl, preferably a hydrogen, - M is H or a cation of valence m, - when M is H, m is 1 and when M is a cation, m is the valence of the cation M, - b is a number from 0.75 to 0.95, such that (100 x b) represents the molar percentage of units of formula (II') within the polymer.
3. The admixed cement composition according to claim 1 or 2 wherein, in the formulae of the polymer of the admixture: - a is a number from 0.05 to 0.20, preferably a is a number of between 0.10 and 0.20, and - b is a number from 0.80 to 0.95, preferably b is a number between 0.80 and 0.90.
4. The admixed cement composition according to anyone of claims 1 to 3 wherein, in the formulae of the polymer of the admixture: - q is an integer of 5 to 200, in particular of 10 to 100, preferably of 25 to 75, - R5 is -OH or -OMe, preferably R5 is -OH, - a is a number from 0.05 to 0.20, preferably a is a number between 0.10 and 0.20, - b is a number from 0.80 to 0.95, preferably b is a number between 0.80 and 0.90, and / or - M is H or a monovalent or bivalent cation, m then being 1 or 2, the monovalent cation preferably being selected from among an ammonium salt NH4+, a primary, secondary, tertiary or quaternary ammonium cation, and a cation of an alkali metal such as a sodium, lithium or potassium ion, and the bivalent cation preferably being a cation of an alkaline-earth metal such as a magnesium or calcium ion.
5. The admixed cement composition according to any of claims 1 to 4, wherein the admixture comprises a set retarding agent.
6. The admixed cement composition according to claim 5, wherein the set retarding agent is chosen among: - a phosphonic acid in neutral form or a salt thereof, - a phosphate, - and mixtures thereof.
7. The admixed cement composition according to claim 6, wherein the set retarding agent is amino tri methylene phosphonic acid (ATMP).
8. The admixed cement composition according to claim 5, wherein the set retarding agent is gluconic acid in neutral form or a salt thereof, a phosphonic acid in neutral form or a salt thereof, or a mixture thereof.
9. The admixed cement composition according to any of claims 1 to 8, comprising less than 0.001 weight % of tertiary alkanolamine having 1 to 6 carbon atoms relative to the dry weight of the admixed cement composition.
10. A hydraulic composition comprising the admixed cement composition according to any of claims 1 to 9, water, an aggregate and optionally a mineral addition.
11. Use of an admixture such as defined in any of claims 1 to 8 as fluidifier of a cement composition comprising: - from 20 to 64 weight % clinker, - from 5 to 60 weight % activated clay, - from 0 to 35 weight % limestone, - from 0 to 10 weight % calcium sulfate, the proportions being relative to the dry weight of the cement composition.
12. The use according to claim 11, wherein the admixture is used so that the proportion of polymer is from 0.001 weight % to 5 weight %, in particular from 0.005 weight % to 1 weight %, preferably from 0.01 weight % to 0.2 weight % relative to the dry weight of the cement composition.
13. The use according to any of claims 11 to 12, wherein the cement composition comprises less than 0.001 weight % of tertiary alkanolamine having 1 to 6 carbon atoms relative to the dry weight of the cement composition.