RARE EARTH CONTAINING HEAT-RESISTANT ALLOY STEEL AND METHOD FOR PRODUCEING SHEETS BY CONTINUOUS CASTING
Patent Information
- Application Number
- DE602021022992
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-08
- Filing Date
- 2021-04-27
- Publication Date
- 2024-12-04
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Rare earth-bearing heat-resistant alloys are prone to precipitation of brittle phases during continuous casting, leading to cracks and inclusion defects in slabs, which affects their quality and reliability at high temperatures.
A rare earth-bearing heat-resistant alloy steel with controlled chemical compositions (C: 0
The alloy exhibits excellent heat resistance with electrical resistivity of 1.3-1.5 µΩ•m at room temperature, elongation of 5-25%, and oxidative weight loss of 0.2-8.0 g/(cm²·h at 1000-1300 °C, while the continuous casting process improves slab quality by reducing cracks and recesses, increasing production capacity, and lowering production costs.
Description
TECHNICAL FIELD
[0001] The present invention relates to a metal material and a manufacturing method thereof, in particular to a rare earth-bearing heat-resistant alloy steel and a continuous casting production process therefor.BACKGROUND
[0002] In industrial production, heat-resistant alloys have been produced for many years, and many well-known foreign metallurgical enterprises produce heat-resistant alloys. The heat-resistant alloys have the advantages of high aperture ratio, large specific surface area, low heat capacity, high thermal conductivity and high strength. The heat-resistant alloys can be used as main raw materials for metal carriers in an exhaust gas purification device, and are widely used in automobiles, diesel locomotives, motorcycles, small general machinery and other industries.
[0003] A rare earth-bearing heat-resistant alloy is a material with Fe, Cr and Al as the matrix and adding some alloys such as Mo, Cu, Nb, V and mixed rare earths, which can improve high-temperature performance, electrical resistivity and grain refinement. For the smelting process for the rare earth-bearing heat-resistant alloys, die casting and electroslag processes are mainly used at present, and continuous casting process is used in a few cases, followed by hot rolling and cold rolling.
[0004] In the iron and steel metallurgy industry around the world, with the continuous casting technology being gradually applied to the production of special steels, some enterprises have used slab continuous caster to produce special alloy products. However, the rare earth-bearing heat-resistant alloys are prone to precipitation of brittle phases during the cooling process of continuous casting, resulting in the formation of cracks and inclusion defects in the continuous casting slabs. WO 0100896 discloses a Fe-Cr-Al-Y-Hf alloy.SUMMARY
[0005] One of the objectives of the present invention is to provide a rare earth-bearing heat-resistant alloy steel, which has an electrical resistivity of 1.3-1.5 µΩ•m at room temperature, can withstand an applicable temperature of 1000-1300 °C, and has an elongation of 5-25% and an oxidative weight loss of 0.2-8.0 g / (cm 2< •h) at the applicable temperature of 1000-1300 °C, thus exhibiting good quality and excellent heat resistance.
[0006] In order to achieve the above-mentioned objective, the present invention provides a rare earth-bearing heat-resistant alloy steel according to claim 1.
[0007] The expression "at least one of rare earth elements Nos. 57 to 71 in Periodic Table of Elements: 0.01-0.1%" means that: when the alloy steel comprises one of the rare earth elements Nos. 57 to 71, the content of the rare earth element is 0.01-0.1%; and when the alloy steel comprises more than one of the rare earth elements Nos. 57 to 71, the total content of these rare earth elements is 0.01-0.1%.
[0008] In the rare earth-bearing heat-resistant alloy steel of the present invention, the design principles of each chemical element are as follows: C: In the rare earth-bearing heat-resistant alloy steel of the present invention, carbon can increase the electrical resistance of the steel and increase the strength of the steel.
[0009] However, it should be noted that carbon is prone to be austenitized, which tends to form carbide precipitates with Cr, thereby reducing the service life of the steel. Therefore, the less content of carbon in steel, the property will be better. In the rare earth-bearing heat-resistant alloy steel of the present invention, the content of C in mass percentage is controlled to be 0<C≤0.05%.
[0010] In some preferred embodiments, the content of C in mass percentage can be controlled to be 0.01≤C≤0.05%.
[0011] In some more preferred embodiments, the content of C in mass percentage can be controlled to be 0.01≤C≤0.03%.
[0012] Si: In the rare earth-bearing heat-resistant alloy steel of the present invention, silicon is generally brought in by the raw materials and alloy materials. A high content of silicon in the steel will increase electrical resistance and room-temperature strength; the anti-oxidation effect of silicon at a medium temperature can reduce the loss of aluminum and rare earth; and silicon can reduce nitrogen absorption at a high temperature. However, it should be noted that silicate inclusions will adversely affect the alloy matrix. Especially in a high-temperature anti-oxidation film composition, if there is silicon oxide, the integrity of an Al 2 O 3 oxide film will be affected. Therefore, the silicon content should not be too high. In the rare earth-bearing heat-resistant alloy steel of the present invention, the content of Si in mass percentage is controlled to be 0.02≤Si≤1.0%.
[0013] In some more preferred embodiments, the content of Si in mass percentage can be controlled to be 0.2≤Si≤0.5%.
[0014] Mn: In the rare earth-bearing heat-resistant alloy steel of the present invention, manganese can increase the toughness of the steel, and is prone to be austenitized. However, it should be noted that manganese can form oxides with a low melting point in the rare earth-bearing heat-resistant alloy steel, thereby reducing the thermal stability of the alloy. Therefore, in the rare earth-bearing heat-resistant alloy steel of the present invention, the content of Mn in mass percentage is controlled to be 0.05≤Mn≤1.0%
[0015] In some more preferred embodiments, the content of Mn in mass percentage can be controlled to be 0.2≤Mn≤0.4%.
[0016] Cr: In the rare earth-bearing heat-resistant alloy steel of the present invention, chromium and iron have many properties that are not very different, both of which are body-centered cubic lattices, and their lattice constants are similar. The chromium content in ferrite stainless steel is usually not less than 13%. The addition of chromium to iron can greatly increase the electrical resistivity of iron, and the electrical resistivity of iron will increase rapidly with the increasing content of Cr. However, it should be noted that when the content of chromium in the steel exceeds 28%, a σ brittle phase will precipitate and a hardening phase will be dissolved, and the electrical resistivity will gradually decrease. At the same time, the addition of chromium will cause the strength of the steel to improve rapidly and the brittleness of the steel to increase continuously. Therefore, in the rare earth-bearing heat-resistant alloy steel of the present invention, the content of Cr in mass percentage is controlled to be 13.0-28.0%.
[0017] In some preferred embodiments, the content of Cr in mass percentage can be controlled to be 17.0-25.0%.
[0018] Al: In the rare earth-bearing heat-resistant alloy steel of the present invention, when the content of aluminum in the Fe-Cr alloy is not less than 2%, the anti-oxidation performance will be improved; especially at a high temperature, an oxide film composition can be transformed from Cr 2 O 3 to Al 2 O 3 , so that an oxide film is more stable and firmer, which greatly increases the applicable temperature and prolongs the service life. However, it should be noted that the addition of aluminum will increase the brittleness of the alloy steel. When the content of Al in the steel exceeds 8%, it is difficult to carry out both cold and hot workability. Therefore, in the rare earth-bearing heat-resistant alloy steel of the present invention, the content of Al in mass percentage is controlled to be 2.0-8.0%.
[0019] In some preferred embodiments, the content of Al in mass percentage can be controlled to be 3.0-6.0%.
[0020] Nb: In the rare earth-bearing heat-resistant alloy steel of the present invention, Nb can improve the high-temperature strength, reduce high-temperature creep, and prolong the service life of the rare earth-bearing heat-resistant alloy steel. However, considering that the cost and the production difficulty will increase as the content of Nb increases, the content of Nb in mass percentage in the rare earth-bearing heat-resistant alloy steel of the present invention is controlled to be 0.02≤Nb≤0.50%.
[0021] In some more preferred embodiments, the content of Nb in mass percentage can be controlled to be 0.02≤Nb≤0.40%.
[0022] In the most preferred embodiment, the content of Nb in mass percentage can be controlled to be 0.05≤Nb≤0.40%.
[0023] Co: In the rare earth-bearing heat-resistant alloy steel of the present invention, Co has similar effect with Nb, and Co can also increase the high-temperature strength, reduce high-temperature creep, and prolong the service life of the rare earth-bearing heat-resistant alloy. Similarly, considering that the production cost and the production difficulty will increase as the content of Co increases, the content of Co in mass percentage in the rare earth-bearing heat-resistant alloy steel of the present invention is controlled to be 0.01≤Co≤0.50%.
[0024] In some more preferred embodiments, the content of Co in mass percentage can be controlled to be 0.01≤Co≤0.20%.
[0025] In the most preferred embodiment, the content of Co in mass percentage can be controlled to be 0.05≤Nb≤0.20%.
[0026] Mo, Y: In the rare earth-bearing heat-resistant alloy steel of the present invention, a small amount of molybdenum (Mo) and yttrium (Y) are added. Molybdenum can effectively reduce the high-temperature creep rate and prolong the service life of the steel. Yttrium can refine alloy grains, thereby improving the room-temperature strength and high-temperature strength of the steel, and reducing the brittleness. The affinity of yttrium to oxygen is between that of lanthanum and that of aluminum, and it can form an enamel-like oxide film, thereby improving the high-temperature oxidation resistance and the nitriding resistance of the alloy steel. Like molybdenum, yttrium can effectively reduce the high-temperature creep rate and prolong the service life of the steel. However, it should be noted that when the content of molybdenum in the steel is too high, it is difficult to perform both hot and cold machining. When pickling the oxide scales, peeling or overwashing is common. Correspondingly, it tends to burn during smelting when the content of yttrium in the steel is too high. Therefore, in the rare earth-bearing heat-resistant alloy steel of the present invention, the content of Mo in mass percentage is controlled to be 0.5-6.0%, and the content of Y in mass percentage is controlled to be 0.01-0.2%.
[0027] In some preferred embodiments, the content of Mo in mass percentage can be controlled to be 1.5-5.0%, and the content of Y in mass percentage can be controlled to be 0.05-0.15%.
[0028] It should be noted that in the rare earth-bearing heat-resistant alloy steel of the present invention, the present inventors use lanthanide rare earth elements Nos. 57 to 71 while using Y, which mainly play the role of significantly prolonging the service life. A larger added content of rare earths indicates a higher service life value. However, in practical production, if more rare earths are added, more rare earths will be burned, and the possibility of increasing impurities and hydrogen absorption will be larger, while the increase in the residual content of rare earths in the alloy after burning is less. When the amount of the lanthanide rare earth added in the alloy is greater than 0.1%, the service life value of the steel shows a downward trend. Furthermore, the cost of the lanthanide rare earth is high, and the content should not be too high. Therefore, in the rare earth-bearing heat-resistant alloy steel of the present invention, the added content of at least one of rare earth elements Nos. 57 to 71 in Periodic Table of Elements in mass percentage is controlled to be 0.01-0.1%.
[0029] Preferably, the content of at least one of rare earth elements Nos. 57 to 71 in Periodic Table of Elements in mass percentage can be controlled to be 0.02-0.05%.
[0030] Preferably, in the rare earth-bearing heat-resistant alloy steel of the present invention, the content of Nb and Co in mass percentage further satisfies: Nb+Co≤0.50%, which can increase the high-temperature strength, reduce the high-temperature creep, and prolong the service life of the rare earth-bearing heat-resistant alloy. In case of Nb+Co>0.5%, the continuous casting production is difficult, the crack sensitivity is high, and the alloy cost is increased. Nb and Co in the formula represent the content of each corresponding element in mass percentage respectively.
[0031] In the rare earth-bearing heat-resistant alloy steel of the present invention, in the inevitable impurities, the content of P, S and N satisfies P≤0.040%, S≤0.020%, and N≤0.020%.
[0032] Preferably, in the rare earth-bearing heat-resistant alloy steel of the present invention, in the inevitable impurities, the content of P, S and N satisfies at least one of P≤0.020%, S≤0.010%, and N≤0.010%.
[0033] In the above technical solution, in the rare earth-bearing heat-resistant alloy steel of the present invention, P, N and S are all inevitable impurity elements in the steel, and the content of these impurity elements in the steel should not be too high. Both P and S can generate brittle substances with a low melting point, which tend to cause hot brittleness. Correspondingly, if the content of N in the rare earth-bearing heat-resistant alloy steel is too high, brittle aluminum nitride will be formed, which tend to cause brittle fracture and hinder the formation of Al 2 O 3 oxide film.
[0034] Preferably, in the rare earth-bearing heat-resistant alloy steel of the present invention, the content of chemical elements in mass percentage satisfies at least one of: 0.01≤C≤0.03%, 0.2≤Si≤0.5%, 0.2≤Mn≤0.4%, Cr: 17.0-25.0%, Al: 3.0-6.0%, 0.02≤Nb≤0.40%, 0.01≤Co≤0.20%, Mo: 1.5-5.0%, Y: 0.05-0.15%, and at least one of rare earth elements Nos. 57 to 71 in Periodic Table of Elements: 0.02-0.05%.
[0035] Preferably, in the rare earth-bearing heat-resistant alloy steel of the present invention, the main microstructure is ferrite.
[0036] Preferably, the properties of the rare earth-bearing heat-resistant alloy steel of the present invention satisfy at least one of: being able to withstand an applicable temperature of 1000-1300 °C; having an elongation of 5-25% and an oxidative weight loss of 0.2-8.0 g / (cm 2< •h) at the applicable temperature of 1000-1300 °C; and having an electrical resistivity of 1.3-1.5 µΩ•m at room temperature.
[0037] Correspondingly, another objective of the present invention is to provide a slab continuous casting production process for rare earth-bearing heat-resistant alloy steel. The slab continuous casting production process can effectively improve the quality of the continuous casting slab, and the produced continuous casting slab has excellent characteristics of good quality on a surface and center of the continuous casting slab. It can fully exert the advantages of continuous casting production, can effectively suppress recesses and cracks of the casting slab, significantly improve the surface and center quality of the casting slab and achieve sequence casting. The slab continuous casting production process of the present invention is a key technology for achieving continuous casting production and quality assurance of rare earth-bearing heat-resistant alloy slabs, and has extremely high promotion and application value for the development of rare-earth-bearing varieties and optimization of the process for enterprises that use a continuous casting process to achieve production and testing. It can not only increase production capacity, and but also effectively reduce production cost, so that the comprehensive competitiveness of an enterprise is greatly enhanced.
[0038] In order to achieve the above objectives, the present invention provides the above-mentioned slab continuous casting production process for the rare earth-bearing heat-resistant alloy steel. In the continuous casting process, the specific water ratio of secondary cooling is controlled to be 1.02±0.10 L / kg.
[0039] In the slab continuous casting production process of the present invention, a structure of rare earth-bearing heat-resistant alloy after solidification is mainly ferrite, and the columnar crystals are developed. Through a large number of experiments, the inventors have found that if weak cooling is used, the solidification time will be long, the columnar crystals will fully grow, and transgranular structure will appear in the casting slab at a low magnification, resulting in crack defects after rolling. In the slab continuous casting production process of the present invention, the present inventors have designed that: a strong cooling process is performed on the rare earth-bearing heat-resistant alloy steel in the secondary cooling zone, wherein when the specific water ratio of secondary cooling is controlled to be 1.02±0.10 L / kg, the lengths of primary columnar crystal and the spacing of secondary columnar crystals are the shortest, which are the prerequisites for improving the internal quality of the casting slab; and the electromagnetic stirring and soft reduction process of the present invention is further used to further ensure the internal quality of the casting slab. In some preferred embodiments, in the continuous casting process, the specific water ratio of secondary cooling can be controlled to be 1.02±0.06 L / kg, and the Mannesmann rating of the casting slab at low magnification is M1.7-2.0.
[0040] Preferably, in the slab continuous casting production process of the present invention, in the continuous casting step, a temperature for hot grinding the casting slab is controlled to be 100-600 °C.
[0041] In the slab continuous casting production process of the present invention, the surface of the continuous casting slab of the rare earth-bearing heat-resistant alloy steel will have defects such as local recesses, slag pits and deep vibration marks in different degrees. These defects will affect the surface quality of subsequent hot-rolled and cold-rolled products. At the same time, considering that the brittle phase is precipitated in the cooling process for the rare earth-bearing heat-resistant alloy steel, a hot grinding process can be used for the casting slab to effectively alleviate the above defects.
[0042] However, it should be noted that if the temperature in the hot grinding process is lower than 100 °C, the precipitated brittle phase tends to cause grinding cracks; and if the temperature is higher than 600 °C, it will exceed the capacity of the grinding equipment. Therefore, in the slab continuous casting production process of the present invention, the temperature for hot grinding the casting slab is controlled to be 100-600 °C. In some preferred embodiments, in the slab continuous casting production process of the present invention, the temperature for hot grinding the casting slab can be controlled to be 300-500 °C.
[0043] Preferably, in the slab continuous casting production process of the present invention, process parameters of the continuous casting process are controlled to satisfy at least one of the specific water ratio of secondary cooling is controlled to be 1.02±0.06 L / kg; the temperature for hot grinding the casting slab is 300-500 °C; the electromagnetic stirring current is 1000-2000 A; the soft reduction amount is 3-10 mm; the solid fraction fs of the casting slab center corresponding to a reduction zone is 0.10-0.90; the grinding amount on one casting slab side is 3-10 mm; the superheat degree of molten steel in a tundish is controlled to be 10-50 °C; the average casting speed of continuous casting is controlled to be 0.40-1.50 m / min; and the submerged depth of a continuous casting crystallizer nozzle is controlled to be 90-130 mm.
[0044] In the slab continuous casting production process of the present invention, in order to improve the segregation problem that may be possibly caused by the ferrite in the rare earth-bearing heat-resistant alloy during the continuous casting process, an electromagnetic stirring in the secondary cooling zone and dynamic soft reduction process can be added in the slab continuous casting production process of the present invention.
[0045] When the electromagnetic stirring in the secondary cooling zone and dynamic soft reduction process are used, if the current of electromagnetic stirring is less than 1000 A, and the soft reduction amount is less than 3 mm, it will not be effective in improving the quality of the center of a ferrite slab. If the current of electromagnetic stirring is higher than 2000 A, a liquid level of the crystallizer fluctuates greatly, and the slab is prone to negative segregation. If the soft reduction amount is greater than 10 mm, the narrow side of the casting slab is prone to bulge, and intermediate cracks are prone to be generated in the casting slab. In the ferrite structure of the rare earth-bearing heat-resistant alloy, the columnar crystals are developed; and through a lot of experiments, the results have shown that dynamic soft reduction is suitable for the whole solidification process of the two-phase region. Therefore, in the slab continuous casting production process of the present invention, the current of electromagnetic stirring is controlled to be 1000-2000 A, the soft reduction amount is controlled to be 3-10 mm, and the solid fraction fs of the casting slab center corresponding to a reduction zone is controlled to be 0.10-0.90. If fs corresponding to the reduction zone is less than 0.10, which is equivalent to complete liquid phase reduction, the columnar crystals have not been completely formed, and the effect of improving segregation is not obvious. If fs corresponding to the reduction zone is more than 0.90, the casting slab being nearly completely solidified, the columnar crystals cannot be completely crushed by reduction, and there is risk of internal cracks. Thus, the solid fraction fs in the center of the casting slab corresponding to the reduction zone being 0.10-0.90 is an important condition to control the Mannesmann rating of the casting slab at low magnification to be M1.7-2.0. In some preferred embodiments, the electromagnetic stirring current can be controlled to be 1400-2000 A, the soft reduction amount can be controlled to be 6-9 mm, and the solid fraction fs of the casting slab center corresponding to the reduction zone can be controlled to be 0.20-0.90.
[0046] In addition, it should be noted that when grinding the casting slab, if the grinding amount on one casting slab side is less than 3 mm, the defects may not be completely removed. If the grinding amount on one side is greater than 10 mm, the yield of the casting slab will be affected. Therefore, in the slab continuous casting production process of the present invention, the grinding amount on one casting slab side can be controlled to be 3-10 mm. In some preferred embodiments, the grinding amount on one casting slab side can be controlled to be 5-8 mm.
[0047] In the continuous casting process, if the superheat degree of molten steel is lower than 10 °C, the fluidity of the molten steel is poor, which will easily lead to the freezing of steel at the crystallizer nozzle to force pouring to be interrupted, and the melting effect of covering slag is not good. If the superheat degree of molten steel is higher than 50 °C, the rare earth-bearing heat-resistant alloy steel is prone to segregation, resulting in long solidification time and sufficient selective crystallization, which will exacerbate the quality issues of the casting slab. Therefore, in the slab continuous casting production process of the present invention, the superheat degree of molten steel in the tundish is controlled to be 10-50 °C. In some preferred embodiments, the superheat degree of molten steel in the tundish can be controlled to be 15-30 °C.
[0048] In addition, in the continuous casting process, if the average casting speed of continuous casting is faster than 1.50 m / min, the initial slab shell is thin, and the slab cooling is uneven, which tend to cause longitudinal cracks and even bleed-out. If the average casting speed of continuous casting is slower than 0.40 m / min, the cooling time of the slab in the crystallizer is too long, the molten steel at the meniscus is in a low-temperature state and the melting effect of the covering slag is not good, which tend to cause cracks and affect the overall production capacity of the continuous caster. Therefore, in the slab continuous casting production process of the present invention, the average casting speed of continuous casting is controlled to be 0.40-1.50 m / min. In some preferred embodiments, the average casting speed of continuous casting can be controlled to be 0.80-1.2 m / min.
[0049] Correspondingly, in the continuous casting process, if the submerged depth of the crystallizer nozzle is too shallow, the impact of the nozzle stream on the steel slag interface will be too strong, which will increase the probability of reaction between the molten steel and covering slag in the crystallizer, and increase the probability of slag entrapment on the meniscus. If the submerged depth of the crystallizer nozzle is too deep, the casting slab is prone to cracks. Therefore, in the slab continuous casting production process of the present invention, the submerged depth of the continuous casting crystallizer nozzle is controlled to be 90-130 mm. In some preferred embodiments, the submerged depth of the continuous casting crystallizer nozzle can be controlled to be 100-125 mm.
[0050] Preferably, in the slab continuous casting production process of the present invention, the process parameters of the continuous casting process are controlled to satisfy at least one of: the electromagnetic stirring current is 1400-2000 A; the soft reduction amount is 6-9 mm; the solid fraction fs of casting slab center corresponding to a reduction zone is 0.20-0.90; the grinding amount on one casting slab side is 5-8 mm; the superheat degree of molten steel in the tundish is controlled to be 15-30 °C; the average casting speed of continuous casting is controlled to be 0.80-1.2 m / min; and the submerged depth of the continuous casting crystallizer nozzle is controlled to be 100-125 mm.
[0051] Compared with the prior art, the rare earth-bearing heat-resistant alloy steel and the slab continuous casting production process therefor according to the present invention have the following advantages and beneficial effects:
[0052] The rare earth-bearing heat-resistant alloy steel of the present invention has an electrical resistivity of 1.3-1.5 µΩ•m at room temperature, can withstand an applicable temperature of 1000-1300 °C, and has an elongation of 5-25% and an oxidative weight loss of 0.2-8.0 g / (cm 2< •h) at the applicable temperature of 1000-1300 °C, exhibiting good quality and excellent properties.
[0053] In addition, the slab continuous casting production process for the rare earth-bearing heat-resistant alloy steel of the present invention can effectively improve the quality of a continuous casting slab. The produced continuous casting slab has excellent characteristics such as good quality on the surface and center of the continuous casting slab. It can fully exert the advantages of continuous casting production, can effectively suppress the occurrence of recesses and cracks of the casting slab, significantly improve the surface and center quality of the casting slab and achieve sequence casting. The slab continuous casting production process of the present invention is a key technology for realizing continuous casting production and quality assurance of rare earth-bearing heat-resistant alloy slabs, and has extremely high promotion and application value for the development of rare-earth-bearing varieties and optimization of the process for enterprises that use a continuous casting process to achieve production and testing. It not only increases production capacity, and but also effectively reduces production cost, so that the comprehensive competitiveness of an enterprise can be greatly enhanced.DETAILED DESCRIPTION
[0054] The rare earth-bearing heat-resistant alloy steel and the slab continuous casting production process therefor according to the present invention will be further explained and illustrated below in combination with specific embodiments. However, the technical solution of the present disclosure is not limited to the explanation and illustration.Inventive Examples 1-6 and Comparative Examples 1-4
[0055] Table 1 shows the content of chemical elements in mass percentage in rare earth-bearing heat-resistant alloy steels in Inventive Examples 1-6 and Comparative Examples 1-4. Table 1 (wt%, the balance being Fe and inevitable impurities other than P, S and N)No.Chemical elementsCSiMnCrAlNbCoMoYPSNReNb+CoInventive Example 10.010.380.2722.34.70.190.013.50.10.0170.0010.0080.030.20Inventive Example 20.0120.530.0528.02.00.230.153.00.130.0110.0010.0100.100.38Inventive Example 30.0150.350.317.25.40.020.102.00.20.0160.0020.0130.010.12Inventive Example 40.021.01.013.08.00.500.023.50.090.0140.0020.0020.0250.52Inventive Example 50.030.020.6521.23.20.030.506.00.010.0200.0010.0050.0720.53Inventive Example 60.050.250.1219.62.80.020.060.50.0170.0070.0010.0070.0150.08Comparative Example 10.010.400.2712 1.0 0.100.100.1 0.160.0100.0010.0080 0.20Comparative Example 20.020.80.508 1.8 0.050.050.4 0.120.0080.0020.0030.008 0.10Comparative Example 30.030.20.72208.2 0.55 0.8 3.30.080.0200.0010.0040.21 1.35Comparative Example 40.040.350.815.69.8 0.61 0.63 2.30.030.0070.0010.0090.25 1.24
[0056] It should be noted that Re in Inventive Examples 1-6 and Comparative Examples 1-4 in Table 1 represents the content of any one element or the total content of several elements among elements Nos. 57 to 71 in Periodic Table of Elements in mass percentage.
[0057] The rare earth-bearing heat-resistant alloy steels of Inventive Examples 1-6 of the present invention and Comparative Examples 1-4 were prepared by the following continuous casting production process: In the continuous casting process, firstly, the superheat degree of molten steel in the continuous casting tundish was controlled to be 10-50 °C and the submerged depth of the continuous casting crystallizer nozzle was controlled to be 90-130 mm. Then continuous casting pouring was started, wherein the average casting speed was controlled to be 0.40-1.50 m / min and the specific water ratio of secondary cooling was controlled to be 1.02±0.10 L / kg. After the casting slab entered the secondary cooling zone, electromagnetic stirring was started. The electromagnetic stirring current was 1000-2000 A, the soft reduction amount was controlled to be 3-10 mm, and the solid fraction fs of the casting slab center corresponding to the reduction zone was controlled to be 0.10-0.90. Finally, after the casting slab was released from the caster, the temperature for hot grinding the casting slab was controlled to be 100-600 °C, and the grinding amount on one casting slab side was controlled to be 3-10 mm.
[0058] Table 2 shows specific process parameters of manufacturing methods of the rare earth-bearing heat-resistant alloy steels of Inventive Examples 1-6 and Comparative Examples 1-4. Table 2No.Sectional dimension of slab (mm)Specific water ratio of secondary cooling (L / kg)Temperature for hot grinding (°C)Electromagnetic stirring current (A)Soft reduction amount (mm)Solid fraction fs of casting slab center corresponding to reduction zoneGrinding amount on one casting slab side (mm)Average superheat degree of molten steel in tundish (°C)Average casting speed of continuous casting (m / min)Submerged depth of continuous casting crystallizer nozzle (mm)Inventive Example 1250×12000.9645016008.00.1-0.98260.76120Inventive Example 2200×11400.9833014006.50.1-0.97320.92105Inventive Example 3150×13001.0820012004.50.1-0.93121.2120Inventive Example 4200×12501.0235020007.00.1-0.95391.0125Inventive Example 5150×14501.1228010003.50.1-0.94331.5115Inventive Example 6230×10800.9257018009.00.1-0.910470.490Comparative Example 1150×10001.1055012005.00.1-0.93181.4120Comparative Example 2200×12001.0045016006.00.1-0.95261.2125Comparative Example 3250×13500.9425020008.50.1-0.97400.8105Comparative Example 4230×11000.9630018007.50.1-0.96301.095
[0059] Various performance tests were performed on the rare earth-bearing heat-resistant alloy steels of Inventive Examples 1-6 and Comparative Examples 1-4, and the test results were listed in Table 3. Performance test methods: GB / T 4338-2006 "Metallic materials - Tensile Testing at elevated temperature"; GB / T 13303-1991 "Steels - Determination method of oxidation resistance"; GB / T 351-2019 "Metallic materials - Resistivity measurement method"; and "Mannesmann Demark Steel Corporation - Standard and method for inspection of defects of continuous casting slab".
[0060] Table 3 shows the performance test results of the rare earth-bearing heat-resistant alloy steels of Inventive Examples 1-6 and Comparative Examples 1-4. Table 3No.Elongation at applicable temperature of 1000-1300 °C (%)Oxidative weight loss at applicable temperature of 1000-1300 °C g / (cm 2< ·h)Electrical resistivity at room temperature (µΩ·m)Quality of casting slabInventive Example 117.30.461.303No cracks, casting slab rating at low magnification of M1.8Inventive Example 224.77.981.446No cracks, casting slab rating at low magnification of M2.0Inventive Example 313.50.371.444No cracks, casting slab rating at low magnification of M1.7Inventive Example 45.10.221.499No cracks, casting slab rating at low magnification of M2.0Inventive Example 520.12.331.496No cracks, casting slab rating at low magnification of M2.0Inventive Example 622.76.551.461No cracks, casting slab rating at low magnification of M2.0Comparative Example 18.29.7 1.232 No cracks, casting slab rating at low magnification of M1.8Comparative Example 211.610.1 1.195 No cracks, casting slab rating at low magnification of M1.9Comparative Example 33.4 0.91.356Cracks, casting slab rating at low magnification of M2.4 Comparative Example 42.8 2.91.421Cracks, casting slab rating at low magnification of M2.2
[0061] It can be seen from Table 3 that the rare earth-bearing heat-resistant alloy steel of each Inventive Example of the present invention had an electrical resistivity of 1.3-1.5 µΩ•m at room temperature, was able to withstand an applicable temperature of 1000-1300 °C, and had an elongation of 5-25% at the applicable temperature of 1000-1300 °C. Test results on oxidization resistance of alloys showed that the oxidative weight loss in each Inventive Example at the applicable temperature of 1000-1300 °C was 0.2-8.0 g / (cm 2< •h). Thus, the rare earth-bearing heat-resistant alloy steels in Inventive Examples exhibited excellent heat resistance. Furthermore, the casting slab in each Inventive Example of the present invention exhibited good quality, had no cracks, and had a Mannesmann rating at low magnification of M1.7-2.0.
[0062] In Comparative Examples 1 and 2, the contents of Al, Cr, Mo and Re were lower than the claimed ranges of the present invention, and the "Oxidative weight loss at applicable temperature of 1000-1300 °C" and the "Electrical resistivity at room temperature" in the heat resistance properties did not satisfy the requirements. In Comparative Examples 3 and 4, the contents of Al, Co, Nb and Re were higher than the claimed ranges of the present invention, the "Elongation at applicable temperature of 1000-1300 °C" was less than 5%, and the rating of casting slab at low magnification exceeded M2.0. In Comparative Examples 3 and 4, the contents of Al and Re were high, such that the casting slabs were prone to subcutaneous inclusions, which would become the source of cracks in the continuous casting slab; and the contents of Co and Nb were high, such that the casting slabs fell into the third brittle zone in the high-temperature range, which would increase the crack susceptibility of the casting slab. Therefore, when the contents of Al, Co, Nb and Re were higher than the claimed ranges of the present invention, the casting slab exhibited low quality.
[0063] It should be noted that the above-listed examples are only specific embodiments of the present disclosure. Apparently, the present disclosure is not limited to the above embodiments but by the appended claims.
Claims
1. A rare earth-bearing heat-resistant alloy steel, comprising the following chemical elements in mass percentage: 0<C≤0.05%, 0.02≤Si≤1.0%, 0.05≤Mn≤1.0%, Cr: 13.0-28.0%, Al: 2.0-8.0%, 0.02<Nb<0.50%, 0.01≤Co≤0.50%, Mo: 0.5-6.0%, Y: 0.01-0.2%, and at least one of rare earth elements Nos. 57 to 71 in Periodic Table of Elements: 0.01-0.1%, and the balance being Fe and inevitable impurities; wherein in the inevitable impurities, the content of P, S and N satisfies: P≤0.040%, S≤0.020%, and N≤0.020%.
2. The rare earth-bearing heat-resistant alloy steel according to claim 1, wherein the content of Nb and Co in mass percentage further satisfies: Nb+Co≤0.50%.
3. The rare earth-bearing heat-resistant alloy steel according to claim 1, wherein in the inevitable impurities, the content of P, S and N satisfies at least one of: P≤0.020%, S≤0.010%, and N≤0.010%.
4. The rare earth-bearing heat-resistant alloy steel according to claim 1, wherein the content of chemical elements in mass percentage satisfies at least one of: 0.01≤C≤0.03%, 0.2≤Si≤0.5%, 0.2≤Mn≤0.4%, Cr: 17.0-25.0%, Al: 3.0-6.0%, 0.02≤Nb≤0.40%, 0.01<Co≤0.20%, Mo: 1.5-5.0%, Y: 0.05-0.15%, and at least one of rare earth elements Nos. 57 to 71 in Periodic Table of Elements: 0.02-0.05%.
5. The rare earth-bearing heat-resistant alloy steel according to claim 1, wherein a microstructure of the rare earth-bearing heat-resistant alloy steel comprises ferrite.
6. The rare earth-bearing heat-resistant alloy steel according to claim 1, wherein the properties of the rare earth-bearing heat-resistant alloy steel satisfy at least one of: being able to withstand an applicable temperature of 1000-1300 °C; having an elongation of 5-25% and an oxidative weight loss of 0.2-8.0 g / (cm2•h) at the applicable temperature of 1000-1300 °C; and having an electrical resistivity of 1.3-1.5 µΩ•m at room temperature.
7. A slab continuous casting production process for the rare earth-bearing heat-resistant alloy steel according to any of claims 1 to 6, wherein in a continuous casting step, a specific water ratio of secondary cooling is controlled to be 1.02±0.10 L / kg.
8. The slab continuous casting production process according to claim 7, wherein in the continuous casting step, a temperature for hot grinding a casting slab is controlled to be 100-600 °C.
9. The slab continuous casting production process according to claim 7 or 8, wherein process parameters of the continuous casting step are controlled to satisfy at least one of: the specific water ratio of secondary cooling is controlled to be 1.02±0.06 L / kg; a temperature for hot grinding a casting slab is 300-500 °C; an electromagnetic stirring current is 1000-2000 A; a soft reduction amount is 3-10 mm; a solid fraction fs of casting slab center corresponding to a reduction zone is 0.10-0.90; a grinding amount on one casting slab side is 3-10 mm; a superheat degree of molten steel in a tundish is controlled to be 10-50 °C; an average casting speed of continuous casting is controlled to be 0.40-1.50 m / min; and a submerged depth of a continuous casting crystallizer nozzle is controlled to be 90-130 mm.
10. The slab continuous casting production process according to claim 9, wherein the process parameters of the continuous casting step are controlled to satisfy at least one of: the electromagnetic stirring current is 1400-2000 A; the soft reduction amount is 6-9 mm; the solid fraction fs of casting slab center corresponding to the reduction zone is 0.20-0.90; the grinding amount on one casting slab side is 5-8 mm; the superheat degree of molten steel in the tundish is controlled to be 15-30 °C; the average casting speed of continuous casting is controlled to be 0.80-1.2 m / min; and the submerged depth insertion depth of the continuous casting crystallizer nozzle is controlled to be 100-125 mm.