Insulating panel of composite materials and its manufacturing process

ES3084771T3Undetermined Publication Date: 2026-11-16VIDALS ACIER (25 00) +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
ES2022813419T
Authority / Receiving Office
ES · ES
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-10-20
Publication Date
2026-11-16
Estimated Expiration
2042-10-20

AI Technical Summary

Technical Problem

Existing polyurethane and polyisocyanurate insulation boards are environmentally unfriendly and exhibit poor thermal performance in summer, leading to increased carbon footprint due to the need for air conditioning.

Method used

A composite insulating panel comprising a mixture of cork and a binder, such as polyurethane or polyepoxide, applied to a metal sheet, which provides improved thermal phase shift and insulation properties.

Benefits of technology

The panel achieves enhanced thermal insulation and reduced carbon footprint by smoothing temperature variations, using environmentally friendly bio-based materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000009_0000
    Figure 00000009_0000
  • Figure 00000009_0001
    Figure 00000009_0001
  • Figure 00000009_0002
    Figure 00000009_0002
Patent Text Reader

Abstract

The present invention relates to an insulating panel (1) based on composite materials, characterized in that it comprises at least: - a layer (2) comprising a mixture of at least one binder and cork, and - a flat or profiled metal sheet (3).
Need to check novelty before this filing date? Find Prior Art

Description

Technical field of the invention

[0001] The present invention relates to the field of panels for thermal and acoustic insulation and, more particularly, to insulating panels based on environmentally friendly bio-sourced materials. State of the art

[0002] In the field of insulating panels (building envelope insulation), polyurethane and polyisocyanurate insulation boards are commonly used. The drawbacks of these boards are that they are made of environmentally unfriendly materials and have poor performance in summer. While they effectively retain heat inside buildings in winter, in summer, at nightfall, when the outside temperature drops below the inside temperature, these boards do not allow buildings to cool down. Their use therefore often necessitates the use of an indoor air conditioning system; this is known as thermal lag. The negative environmental impact of this type of insulation is thus twofold: the significant use of petroleum-based insulation and the need for air conditioning in summer increase the carbon footprint.An insulating panel featuring a layer of cork / binder mixture is described in US document 2017 / 226749 A1. Summary of the invention

[0003] The aim of the present invention is therefore to overcome the aforementioned disadvantages and to propose a panel and a manufacturing process for an insulating panel containing more than 50% bio-based materials that are more environmentally friendly and have good phase shift.

[0004] The term "phase shift" refers to the ability of a material used in a building's envelope to slow down the penetration of heat. Phase shift thus helps to smooth out variations in indoor temperatures caused by changes in outdoor temperatures.

[0005] In accordance with the invention, a manufacturing process according to claim 1 and an insulating panel according to claim 2, based on composite materials, are therefore proposed, remarkable in that it comprises at least: a layer comprising a mixture of at least one binder and cork, a flat or profiled metal sheet.

[0006] A "panel" is a composite assembly consisting of a substrate (here sheet metal) covered with one or more layers of another material or mixture of materials.

[0007] A composite material is defined as an assembly of at least two immiscible components (materials) (but with a high capacity for interpenetration) whose properties complement each other. The resulting heterogeneous material possesses properties that the individual components do not possess.

[0008] Cork is a material found in the bark of some trees, particularly the cork oak. The term "cork" refers to the material in its raw or pre-treated form (pre-treatments are the processes applied to raw cork to enable its use in insulation, for example).

[0009] A rolled metal sheet is called a "flat metal sheet".

[0010] A metal sheet manufactured with a specific profile is called a "profiled metal sheet" (for example: a ribbed or corrugated metal sheet).

[0011] A product used to bind together solid particles in powder or granule form (for example, glue) is called a "binder".

[0012] Advantageously, metal sheeting is steel sheeting.

[0013] Preferably, the binder is an organic binder.

[0014] "Organic" binders are hydrocarbon binders based on hydrogen carbides whose hardening is reversible and temperature-dependent (e.g., tar, bitumen) and resin or polymer type binders.

[0015] Even more preferably, the binder is a polymer or a mixture of polymers.

[0016] Preferably, the binder is a polyurethane, a polyepoxide, or a non-isocyanate polyurethane (NIPU).

[0017] Preferably, the binder is a polyurethane.

[0018] Preferably, the said binder is a polyepoxide.

[0019] The polyepoxide binder preferably comprises one or more polyepoxides resulting from the mixing of one or more compounds (A) comprising two or more epoxy groups with one or more compounds (B) comprising two or more amine groups.

[0020] Where x and y are greater than or equal to two and R1 and R2 denote independently of each other, a divalent hydrocarbon chain, saturated or unsaturated aliphatic, linear or branched, or cycloaliphatic or aromatic, which may include at least one heteroatom such as O, N and S.

[0021] This reaction can be carried out at a temperature ranging from -20 to 250°C, preferably from 50 to 150°C, under atmospheric pressure.

[0022] This reaction can be carried out in the presence of a catalyst such as a tertiary amine like triethylamine, or an aminopheno, or a catalyst well known in the technique.

[0023] According to a preferred embodiment, the layer comprises between 10 and 99% by mass of cork and between 90 and 1% by mass of polyepoxide.

[0024] According to an even more preferred embodiment, the layer comprises between 50 and 95% by mass of cork and between 50 and 5% by mass of polyepoxide.

[0025] According to a highly preferred embodiment, the layer comprises between 70 and 90% by mass of cork and between 30 and 10% by mass of polyepoxide.

[0026] In the case where the binder is polyurethane, the binder is produced by a polyaddition reaction of a polyisocyanate with a polyol.

[0027] Preferably, the layer comprises between 20 and 80% by mass of cork and between 80 and 20% by mass of polyurethane.

[0028] Preferably, the layer comprises between 35 and 65% cork by mass and between 65 and 35% polyurethane by mass.

[0029] Even more preferably, the layer comprises between 45 and 55% by mass of cork and between 55 and 45% by mass of polyurethane.

[0030] Advantageously, the binder is derived from a polyaddition reaction between a diisocyanate and a polyol.

[0031] A molecule with the following structure is designated as "diisocyanate": with R containing linear and cyclic aliphatic structures and / or aromatic structures (e.g., MDI, HDI, TDI, HMDI, IPDI, LDI...) or resulting from its self-condensation with R containing, for example, isocyanurate, biurea allophanate functions..., a functionality of n=2 or n >2, and a mass less than 10000 g.mol⁻¹, or resulting from the prepolymerization of a deficient polyol with a diisocyanate, a functionality of n=2 or n>2 and a mass less than 10000 g.mol⁻¹

[0032] More advantageously, the binder is obtained from the polyaddition reaction between a 1,6-diisocyanatohexane-based diisocyanate containing allophanate functions and a polyol.

[0033] More advantageously, the binder is obtained from a polyaddition reaction between a 1,6-diisocyanatohexane-based diisocyanate containing allophane functions and a diol chosen from the following diols: ethylene glycol or 1,4-butanediol or 1,3-propanediol.

[0034] Even more advantageously, the binder is derived from a polyaddition reaction between a 1,6-diisocyanatohexane-based diisocyanate containing allophanate functions and 1,3-propanediol.

[0035] Preferably, cork is in powder form.

[0036] Cork is called "powder" when it is in the form of pieces smaller than 100 micrometers.

[0037] The cork that can be used in the invention is preferably in the form of flour, granules preferably having a particle size of 0.01 mm up to 20 mm.

[0038] Particle size can be measured for example by the sieve method, at room temperature (20-25 °C).

[0039] The invention also relates to a method for manufacturing an insulating panel as described above, remarkable in that it comprises at least the following successive steps: Coating of a metal sheet with a layer of cork / binder mixture, Passing through an oven at a temperature between 40 and 150°C.

[0040] According to a preferred embodiment of the invention, said process is a semi-continuous process in which the coating precedes the oven passage. Brief description of the figures

[0041] Other advantages and features will become clearer from the following description of an embodiment of a panel according to the invention, with reference to the attached figure in which: [ Fig.1 ] is a cross-sectional view of a panel according to the invention, [ Fig. 2 ] is a perspective view of a panel with an example of profiled sheet metal according to the invention, [ Fig.3 [ ] is a cross-sectional view of a panel, another example of profiled sheet metal according to the invention, Description of the implementation methods

[0042] In accordance with the [ Fig.1 ], therefore, an insulating panel 1 made of composite materials is described, remarkable in that it comprises at least: a layer 2 comprising a mixture of at least one binder and cork, a flat or profiled metal sheet 3.

[0043] Cork is a natural product derived from the outer bark of the cork oak tree, found primarily in the Mediterranean basin. Cork is a renewable resource because it can be harvested from the tree trunk without affecting its health, especially since the bark regrows continuously. It has numerous properties: it is lightweight, absorbs little to no water, is rot-proof, has very low thermal conductivity (making it a good thermal insulator), and is compressible and impermeable to liquids. One of its main known applications is for wine bottle stoppers. It can also be used in expanded form.

[0044] Known for its excellent thermal and acoustic insulation properties, traditional cork has a thermal conductivity (lambda) between 0.040 and 0.045 W / mK and a thermal diffusivity (alpha) between 10⁻⁷ and 1.5 x 10⁻⁷ m² / s, while expanded cork has a thermal conductivity between 0.035 and 0.070 W / mK and a thermal diffusivity between 1.5 x 10⁻⁷ and 3.5 x 10⁻⁷ m² / s (for comparison, polyisocyanurate foam has a thermal conductivity of 0.023 W / mK). Cork's excellent thermal properties are largely due to the air trapped within its cells. To create a rigid cork-based material, a binder is used to bond the cork granules together.

[0045] Advantageously, metal sheet 3 is a steel sheet. This sheet can be flat or profiled. It will serve as cladding or roofing in the insulation of a building. Cladding refers to a covering or layer covering the exterior surface of a building.

[0046] Preferably, the binder is an organic binder. This could include, for example, natural glues of plant or animal origin, resins, or polymers.

[0047] Even more preferably, the binder is a polymer or a mixture of polymers.

[0048] Preferably, the binder is a polyurethane, a polyepoxide, or a non-isocyanate polyurethane (NIPU). Binders based on these polymers are well known for their ability to bond wood and metal together with strong adhesion. Other binders that provide this type of bond may also be used.

[0049] Preferably, the binder is polyurethane. Polyurethane is well known for its diverse applications; the variety of reagents that can be used for its synthesis and its resulting structure make it a material found in very different fields: it can be found in the form of adhesives and coatings, thermoplastics (automotive parts, seals, cables, extruded films, electronics, etc.), flexible foams (cushions, car seats, mattresses, etc.), or rigid foams (thermal and acoustic insulation panels).

[0050] Even more preferentially, the binder is obtained from a polyaddition reaction of a polyisocyanate with a polyol.

[0051] The diol or polyol has the following structure: R being an organic molecule or polymer containing repeating units (Alkyls, ethers, esters, carbonates, urethanes, hydroxyurethanes, ureas) R having linear, cyclic, and aromatic aliphatic structures R with a mass between 20 and 20,000 g.mol-1 With R possibly bearing heteroatoms (O, N, S, Si...) With R of bio- or petroleum-based origin R with a functionality n=2 or n >2

[0052] Advantageously, the binder is derived from a polyaddition reaction between a diisocyanate and a polyol.

[0053] Diisocyanate is commercially available from bio- or petroleum-based sources with R containing linear and cyclic aliphatic structures and / or aromatic structures (e.g., MDI, HDI, TDI, HMDI, IPDI, LDI...) or resulting from its self-condensation with R containing, for example, isocyanurate, biurea, allophane, etc. functions, a functionality of n=2 or n >2, and a mass less than 10000 g.mol -1< or resulting from the prepolymerization of a polyol (previous) in deficiency with a diisocyanate, a functionality of n=2 or n>2 and a mass less than 10000 g.mol -1<

[0054] Preferably, layer 2 comprises between 20 and 80% cork by mass and between 80 and 20% polyurethane by mass. These specific proportions ensure good adhesion of the binder / cork mixture to the metal plate, without an excess of binder or uncrosslinked cork.

[0055] Preferably, layer 2 comprises between 35 and 65% by mass of cork and between 65 and 35% by mass of polyurethane.

[0056] Even more preferably, layer 2 comprises between 45 and 55% by mass of cork and between 55 and 45% by mass of polyurethane.

[0057] Advantageously, the binder is derived from a polyaddition reaction between a diisocyanate and a polyol.

[0058] More advantageously, the binder is produced by a polyaddition reaction between a 1,6-diisocyanatohexane-based diisocyanate containing allophane groups and a polyol. The physicochemical properties of polyurethane can be modulated depending on the chemical nature of the polyols (primary or secondary hydroxyl group, for example). It can be prepared from both petroleum-based and bio-based polyols (for example, from rapeseed, castor, palm, or soybean oils). Two main methods are used for this: either epoxidation with oxirane ring opening, or transesterification with triethanolamine. One study highlights the use of cork residues as bio-polyols. For this, the residues undergo liquefaction in a mixture of diethylene glycol and 2-ethyl hexanol.These bio-based polyol preparations are promising and could reduce the environmental impact of polyurethane foams; however, they require chemical preparation steps. The polyol is chosen so that its combination with diisocyanate allows for the cross-linking of cork.

[0059] More advantageously, the binder is produced by a polyaddition reaction between a 1,6-diisocyanatohexane-based diisocyanate containing allophane groups and a diol chosen from the following: ethylene glycol, 1,4-butanediol, or 1,3-propanediol. Here, the polyisocyanate is a diisocyanate containing isocyanurate groups, specifically the trimer of HDI (1,6-diisocyanatohexane), marketed under the name Tolonate HDT by Vencorex. Two versions can be used: Tolonate HDT (T3HDT) and Tolonate HDT LV (T3HDT LV), which has a lower viscosity than the former and releases fewer volatile organic compounds. Tolonate HDT LV is preferred. Since Tolonate has a functionality of 3, the polyol used can be a diol (functionality of 2). Several other diols combined with this diisocyanate allow the crosslinking of cork, for example: Poly (propylene glycol), a mixture of Sorbitol + water (in proportions 50 / 50).The advantage of HDI is that it is among the least toxic isocyanate monomers.

[0060] Even more advantageously, the binder is derived from a polyaddition reaction between a 1,6-diisocyanatohexane-based diisocyanate containing al-lophane functions and 1,3-propanediol.

[0061] Preferably, layer 2 comprises between 10 and 99% cork by mass and between 90 and 1% polyepoxide by mass. These specific proportions ensure good adhesion of the binder / cork mixture to the metal plate, without an excess of binder or uncrosslinked cork.

[0062] Preferably, layer 2 comprises between 50 and 95% by mass of cork and between 50 and 5% by mass of polyepoxide.

[0063] Even more preferably, layer 2 comprises between 70 and 90% by mass of cork and between 30 and 10% by mass of polyepoxide.

[0064] Ideally, the cork should be in powder form. Using powdered cork ensures a completely homogeneous binder / cork foam and avoids binder settling problems. The cork / binder mixture should be prepared in a universal mixer.

[0065] Preferably, a catalyst is used to accelerate crosslinking. For example, the saturated bicyclic diamine known commercially as DABCO is used. Indeed, an addition of only 0.05% by mass reduces the crosslinking temperature by approximately 10°C. Preferably, an amount of DABCO less than 1% by mass is used. Other tertiary amine catalysts can be used: triethylamine, dimethyl cyclohexane amine, tetramethyl ethylene diamine, etc.

[0066] The invention also relates to a method for manufacturing an insulating panel 1 according to claim 1, as described above, remarkable in that it comprises at least the following successive steps: Continuous coating of a metal sheet 3 by pouring a layer 2 of cork / binder mixture, Crosslinking of said mixture by passing through a continuous oven at a temperature between 40 and 150°C.

[0067] Preferably, the manufacturing process is a semi-continuous process.

[0068] Preferably, the coating step is carried out in a mold.

[0069] Preferably, the oven temperature should be between 70 and 130°C. Even more preferably, the oven temperature should be between 90 and 110°C.

[0070] The panel manufacturing process is preferably a semi-continuous process in which the metal sheet is positioned in a mold and a layer of cork / binder mixture is poured over the moving metal sheet to cover it. The mold supporting the panel then passes through an oven. The oven can hold several molds simultaneously. The operating parameters of the oven (time, temperature) depend on the number of molds present in the oven, as well as the desired thickness of the cork / binder mixture on the metal sheet, to ensure proper cross-linking of the mixture.

[0071] Advantageously, the time spent in the oven will last between 3 and 12 hours.

[0072] More advantageously, the time spent in the oven will last between 3 and 5 hours.

[0073] Even more advantageously, the time spent in the oven will last between 3h30 and 4h30.

[0074] To illustrate the advantages of the invention in terms of thermal insulation, the results of thermal tests carried out on panel 1 specimens according to the invention may be cited as an example. The following example illustrates the invention without limiting it. Examples has. Samples

[0075] Two test specimens of panels made of 2 / 5 mm grain size cork mixed with a binder and bonded to a steel sheet were tested. The first specimen was 100 mm thick, the second 120 mm thick. In the second specimen, intermediate thermocouple probes were placed in the material as follows: the first probe 30 mm from the steel face, the second probe 60 mm from the steel face, and the third probe 90 mm from the steel face. has. Experimental conditions

[0076] The test specimens are placed in a wooden frame and surrounded on both sides by crossbeams around which airtight seals have been installed. This frame is designed to be inserted into measurement tunnels. A Compriband-type compression seal is also positioned on the four sides of the frame, and the same seal is placed on the bottom of the measurement tunnels; these seals are compressed by a pressure plate. All of these elements are designed to prevent any thermal leakage or risk of thermal migration that could disrupt the experiment.

[0077] Two types of experimental chambers are used: one allowing measurements for temperatures ranging from -20°C to 0°C in ventilated or static cold (source type negative cold group), the other allowing measurements for temperatures ranging from +40°C to +120°C (temperature source infrared radiation). has. Taking measurements

[0078] A phase shift measurement is taken every half hour to determine when the measurements are stable and without variation. Here, measurement stability is reached after 7 hours and 30 minutes.

[0079] For the two test specimens two measurements are carried out: the first at 0°C serving as a reference for thermal classification, the second at + 60°C allowing to evaluate the behavior of the material or complex in summer comfort under strong solar radiation (Infrared). has. Calculation method

[0080] The calculation formula used is the industrial measurement formula approved by COFRAC, THERMAL TESTS ACCORDING TO FORMULA U: U = TI − TSI * 0,125 / T 1 − TE

[0081] This formula allows us to determine the U coefficient, which corresponds to the material's conductive heat loss rate. This is inversely proportional to the R coefficient, which is the thermal resistance coefficient. Note: U = 1 / R R = 1 / U

[0082] The lambda of a product (thermal migration coefficient) is determined by dividing the thickness expressed in meters by the coefficient R.

[0083] Note that, unlike the calculation rules of software, lambda is not a constant value and can vary due to temperature differences, material thickness, humidity levels, and even, in some cases, pressure differences. has. Results of thermal behavior for the 100mm specimen and conclusions:

[0084] We can observe good stability of the material to thermal changes although we observe a minor loss of performance when hot. -Behavior in cold conditions (at 0°C):

[0085] We observe excellent resistance to standard cold with the following for the 100mm specimen: a lambda of 0.0246, an R coefficient of 4.06 and a U coefficient of 0.25.

[0086] We note very good cold behavior of the test specimen with a very low lambda compared to the lambdas of existing insulating panels. -Behavior in hot conditions (at +60°C):

[0087] For the 100mm test specimen: a lambda of 0.0346, an R coefficient of 2.89, and a U coefficient of 0.35.

[0088] There is a variation depending on the thicknesses and the thermal deltas. -Results of thermal migration on the 120mm specimen:

[0089] [Table 1] outdoor surf temperature A 30mm A 60mm A 90 mm Indoor surf temperature 0°C 15.00° 19.80° 20.90° 21.20° +60°C 41.80° 35.70° 29.90° 24.80°

Claims

1. Method for manufacturing an insulating panel (1), characterised in that it comprises at least the following successive steps: - covering a metal sheet (3) by pouring a layer (2) of cork / binder mixture onto the metal sheet and, - cross-linking said mixture by moving it into an oven at a temperature between 40 and 150°C.

2. Insulating panel (1) obtained by the method according to claim 1 based on composite materials, characterised in that it comprises at least: - one layer (2) comprising a mixture of at least one binder and cork, - a planar or profiled metal sheet (3).

3. Panel (1) according to claim 2, characterised in that the metal sheet (3) is a steel sheet.

4. Panel (1) according to either claim 2 or 3, characterised in that the binder is an organic binder.

5. Panel (1) according to any one of claims 2 to 4, characterised in that the binder is a polymer or a mixture of polymers.

6. Panel (1) according to any one of claims 2 to 6, characterised in that the binder is a polyurethane, a polyepoxide or a non-isocyanate polyurethane (NIPU).

7. Panel (1) according to the preceding claim, characterised in that the binder is a polyepoxide.

8. Panel (1) according to claim 7, characterised in that the binder is derived from a polyaddition reaction of a polyepoxide with a polyamine.

9. Panel (1) according to claim 7, characterised in that the layer (2) comprises between 10 and 99% by mass of cork and between 90 and 1% by mass of polyepoxide, respectively.

10. Panel (1) according to claim 7, characterised in that the layer (2) comprises between 50 and 95% by mass of cork and between 50 and 5% by mass of polyepoxide, respectively.

11. Panel (1) according to claim 7, characterised in that the layer (2) comprises between 70 and 90% by mass of cork and between 30 and 10% by mass of polyepoxide, respectively.

12. Panel (1) according to any one of the preceding claims, characterised in that the cork is taken as powder or chips.