Amino derivatives as an additive in rubbers
Patent Information
- Application Number
- ES2023211747T
- Authority / Receiving Office
- ES · ES
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-11-23
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-23
AI Technical Summary
Modern vehicle tires face challenges in achieving low rolling resistance, high abrasion resistance, and maintaining grip under varying conditions while ensuring sustainability, with existing additives like carbon black and silicates having poor miscibility and compatibility due to polarity differences, and silanes causing alcohol emissions during processing.
The use of amine derivatives with specific molecular structures, such as polyisobutenyl-substituted succinic acid amine derivatives, to improve dispersion and compatibility of fillers and additives in rubber compounds, enhancing properties like dispersion coefficient, particle size, wet grip, abrasion resistance, and rolling resistance.
The amine derivatives enhance the incorporation of fillers and additives in rubber compounds, improving tire performance while reducing emissions and ensuring consistent functionality, thereby enhancing tire durability and environmental sustainability.
Abstract
Description
[0001] The present invention relates to the use of various amine derivatives as additives in rubbers to improve the properties of vehicle tires.
[0002] Modern vehicle tires are subject to increased demands on their properties, not least from a sustainability perspective, particularly regarding low rolling resistance to reduce fuel consumption and associated emissions, and high abrasion resistance to reduce the emission of tire abrasion into the environment and increase the service life of the tires, without simultaneously impairing the grip of the tires on the surface under various conditions (e.g. temperature, weather conditions, road conditions).
[0003] To improve the properties of vehicle tires, the rubber compounds can contain various fillers and vulcanization accelerators. The fillers are often inorganic materials such as carbon black, silicates, or zinc oxide, while the rubber itself consists of nonpolar polymers. Consequently, the miscibility and compatibility of these components are often poor due to their differing polarities. Other additives, such as vulcanization accelerators and activators, antioxidants, and plasticizers, require a uniform distribution within the rubber compound to ensure they exert their effects consistently.
[0004] Therefore, there is a need for additives that allow filler materials, such as carbon black, silicates or zinc oxide, as well as the other additives mentioned, to be better incorporated into rubbers and to fulfill their functions in the rubbers or in their production, for example as antioxidants, activators or plasticizers.
[0005] Furthermore, in the production of rubber compounds for tires, silanes are often used as processing aids to improve the mixing of carbon black or silica. These silanes release alcohols, especially ethanol, during the process. From both occupational safety and environmental perspectives, this represents an emission that should be avoided or reduced.
[0006] US 2008 / 0214718 A1 describes the use of polyisobutene derivatives for the dispersion of metal oxides, such as ZnO, in polymers, e.g., polychloroprene, urethane-acrylic, or acrylate polymers. Examples of such polyisobutene derivatives are reaction products of polyisobutenyl-substituted succinic acid (PIBSA) with polyamines, such as triethylenetetraamine, for the hydrophobization of zinc oxide in dispersions. Applications in rubber are not described.
[0007] Rubber differs from the described dispersions simply in that it consists of a continuous hydrophobic and organic matrix, whereas in dispersions aqueous and organic phases alternate and are separated from each other by phase boundaries.
[0008] The problem was solved by using amine derivatives of the formula wherein X a single bond or an organic spacer, R1< a straight-chain or branched alkenyl residue with a molecular weight Mn of 104 to 100,000 g / mol, preferably of 104 to 10,000 g / mol, particularly preferably of 156 to 5,000 g / mol and most preferably of 500 to 2,500 g / mol, R2< and R3< independently a further single bond to the organic spacer X, hydrogen, C1- to C4-alkyl, a group -R-NR, R5< or a repeating residue -[-R-NH-], x -H, x a positive integer from 1 to 4, R a divalent organic residue having 2 to 6 carbon atoms, which may optionally be interrupted by oxygen atoms, preferably selected from the group consisting of 1,2-ethylene, 1,2-propylene and 1,3-propylene.R4< and R5<, regardless of whether hydrogen or C1- to C4-alkyl, are used to improve at least one of the following properties: dispersion coefficient, particle size, wet grip, abrasion resistance, rolling resistance, vulcanization rate of rubber-containing tires.
[0009] In a preferred embodiment, the spacer X comprises a structural unit of the formula or where the bonding sites are each connected to the nitrogen atom and the residue R 1<.
[0010] In another preferred embodiment, the spacer X is a single bond.
[0011] The residue R 1< is a straight-chain or branched, preferably branched, alkenyl residue with a molecular weight Mn of 104 to 100000 g / mol, preferably of 104 to 10000 g / mol, particularly preferably of 156 to 5000 g / mol and most preferably of 500 to 2500 g / mol. Examples of R 1< are
[0012] linear C 10 - to C 30 -alkenyl branched C 9 - to C 30 -alkenyl obtainable by polymerization of C 3 - and / or C 4 -alkenes branched alkenyl derived from homo- and copolymers containing iso-butene in polymerized form with a number-average molecular weight Mn of 104 to 100000 g / mol, preferably of 104 to 10000 g / mol, particularly preferably of 156 to 5000 g / mol and most preferably of 500 to 2500 g / mol.
[0013] In a preferred embodiment, R1< comprises a structural unit from the polymerization of isobutene or an isobutene-containing monomer mixture, as described below. Ideally, the homopolymer at R1< is then a residue. wherein n is from 0 to 960, preferably from 0 to 94, particularly preferably from 1 to 46 and most particularly preferably from 3 to 22.
[0014] In a further preferred embodiment, R 1< comprises a structural unit from the polymerization of 1- and / or 2-butene, particularly 1-butene or a butene-containing monomer mixture.
[0015] In a further preferred embodiment, R 1< comprises a structural unit from the polymerization of propene or a propene-containing monomer mixture.
[0016] Unless expressly stated otherwise, in this application C 1 - to C 4 -alkyl preferably stands for methyl, ethyl, n-propyl or n-butyl, preferably methyl, ethyl or n-butyl, particularly preferably methyl or n-butyl and most particularly preferably methyl.
[0017] In a preferred embodiment, X is a single bond and R 2< and R 3< are simultaneously hydrogen.
[0018] In another preferred embodiment, the amine derivative fulfills the formula where R, R 1< and x have the above meanings.
[0019] In this preferred embodiment, X is an organic spacer derived from succinic acid, and R 2< is another single bond to the organic spacer X and R 3< is a repeating residue -[-R-NH-] x -H with R preferably 1,2-ethylene and x a positive integer from 1 to 4.
[0020] In another preferred embodiment, the amine derivative fulfills the formula or or or mixtures thereof, wherein R a divalent alkylene residue, which may optionally be interrupted by oxygen atoms; R 1< a straight-chain or branched alkenyl residue with 9 to 200 carbon atoms; R 4< and R 5< independently hydrogen or C 1 to C 4 alkyl is.
[0021] In this embodiment, X is an organic spacer, R 2< hydrogen, R 3< a group -R-NR 4< R 5< , in which R is preferably 1,3-propylene and R 4< and R 5< are each methyl.
[0022] In the last embodiment, the product is often also present in a mixture with a compound in which X is an organic spacer, R 2< is another single bond to the organic spacer X, R 3< is a group -R-NR 4< R 5< , in which R is preferably 1,3-propylene and R 4< and R 5< are each methyl.
[0023] The invention is explained in more detail below: rubber
[0024] In vehicle tire compounds, especially for the treads, mixtures of butyl rubber with diene elastomers and other components are used, for example.
[0025] Such mixtures are described, for example, in WO2019 / 199839 A1, paragraphs
[0008] to
[0070] , which are incorporated by reference into the present disclosure.
[0026] In this document, the term "rubbers" refers to diene elastomers, i.e., homo- and copolymers of diene monomers, preferably natural rubber, polybutadienes, styrene-butadiene copolymers and polyisoprene and their mixtures, for example, mixtures of natural rubber and styrene-butadiene copolymers, of natural rubber and polybutadienes or natural rubber and polyisoprene.
[0027] Diene elastomers typically have a glass transition temperature Tg of -75 to 0 °C. Polybutadiene
[0028] These are polymers of 1,3-dienes, preferably buta-1,3-diene with a cis-1,4 linkage of at least 90%, preferably at least 95%.
[0029] Other comonomers can be polymerized in small quantities.
[0030] The elastomer used is preferably polybutadiene with more than 90% cis-1,4 linkages, obtained by known catalytic processes with transition metal compounds, as described, for example, in French patent application FR-A-1436607.
[0031] Examples of suitable conjugated dienes include, in particular, 1,3-butadiene, isoprene, and 2,3-dimethyl-1,3-butadiene. Aromatic vinyl compounds can also be incorporated; suitable aromatic vinyl compounds include, in particular, styrene, o-, m-, and p-methylstyrene, or the commercially available "vinyltoluene" mixture. Styrene-butadiene copolymers
[0032] Typical styrene-butadiene copolymers have a styrene content of 5 to 60, preferably 20 to 50 wt%, with the remaining comonomers being predominantly 1,3-butadiene. The content of 1,2-units is generally 4 to 80 mol% and that of cis-1,4-units more than 80 mol%.
[0033] Styrene-butadiene-isoprene terpolymers are also conceivable. Polyisoprene
[0034] This includes homo- and copolymers of isoprene, which can be of natural or preferably synthetic origin.
[0035] In these, the proportion of cis-1,4 units is at least 90 mol%, preferably at least 98 mol%. Butyl rubber
[0036] These are copolymers of 85 to 99.5 mol%, preferably 90 to 99.5, particularly preferably 95 to 99.5 mol% C 4 -C 7 -isoolefins with 0.5 to 15 mol%, preferably 0.5 to 10, particularly preferably 0.5 to 5 mol% C 4 -C 14 -conjugated dienes.
[0037] The preferred isoolefin is isobutene, preferred conjugated dienes are 1,3-butadiene and isoprene, isoprene being particularly preferred.
[0038] The butyl rubber has a viscosity-average molecular weight of 100000 to 1500000, preferably 250000 to 800000.
[0039] The starting materials for the synthetic rubbers, preferably 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, styrene, and / or isobutene, and particularly preferably 1,3-butadiene, isoprene, and / or isobutene, can be derived at least partially, preferably entirely, from renewable sources. Their proportion of the total monomers used, measured according to ASTM D 6866 (see below), is advantageously at least 1 wt%, preferably at least 2 wt%, particularly preferably at least 10 wt%, very preferably at least 25 wt%, and particularly at least 50 wt%. The proportion of monomers from renewable sources can be up to 100 wt%, preferably up to 95 wt%, particularly preferably up to 90 wt%, very preferably up to 85 wt%, and particularly up to 80 wt%. Plasticizer
[0040] Plasticizers (process oils) improve the processability of the composition; these are mostly esters of aliphatic acids, for example fatty acid esters and fatty acid glycerides, preferably naturally occurring oils such as sunflower oil or rapeseed oil, or hydrocarbons such as paraffinic oils, aromatic oils, napthenic petroleum oils and polybutene oils.
[0041] Resins such as those known as tackifiers for adhesives and paints are also suitable as plasticizers. These are preferably copolymers of C5 fractions of naphtha or steam cracker residues with vinyl aromatics, especially copolymers of 1,3-butadiene, 1-butene, 2-butenes, 1,2-butadiene, 3-methyl-1-butene, 1,4-pentadiene, 1-pentene, 2-methyl-1-butene, 2-pentenes, isoprene, cyclopentadiene (which can also exist as a dicyclopentadiene dimer), piperylene, cyclopentene, 1-methylcyclopentene, 1-hexene, methylcyclopentadiene, or cyclohexene. These are primarily copolymers of cyclopentadiene and / or dicyclopentadiene with vinyl aromatics, especially styrene, α-methylstyrene, o-, m- or p-methylstyrene or divinylstyrene. These vinyl aromatics are components of the C9 fractions of naphtha or steam cracker residues.
[0042] Preferred resins as plasticizers are cyclopentadiene and / or dicyclopentadiene copolymers, cyclopentadiene and / or dicyclopentadiene styrene copolymers, polylimonenes, limonene styrene copolymers, limonene cyclopentadiene and / or dicyclopentadiene copolymers, C5 fraction styrene copolymers, and C5 fraction C9 fraction copolymers. Filler
[0043] Examples of fillers include calcium carbonate, clays, mica, silica, silicates, talc, bentonite, titanium dioxide, aluminum oxide, zinc oxide and carbon black, preferably zinc oxide, silicates and carbon black.
[0044] Typical particle sizes range from 0.0001 to 100 µm.
[0045] Silicates, as used here, are derivatives of silicic acid, including its calcium and aluminum compounds. Silicates can be obtained from solution or as pyrogenic substances and can exist in colloidal or precipitated form. Highly dispersible silicates are preferred.
[0046] The BET surface area is typically less than 450 m² / g, preferably 30 to 400 m² / g, particularly preferably 100 to 250 m² / g, and preferably 130 to 220 m² / g; the CTAB surface area is 100 to 250 m² / g, and preferably 150 to 200 m² / g; the DBP oil absorption is 150 to 250 ml / 100 g; and the aggregates have a mean projection area of more than 8500 nm², and preferably 9000 to 11000 nm², before use and 7000 to 8400 nm² after thermomechanical mixing with an elastomer. The selected special silicon dioxide can be used alone or in the presence of other fillers, such as carbon black or another conventional silicon dioxide.
[0047] Silicon dioxide obtained according to the method described in European patent application EP-A-157703 is particularly suitable, for example.
[0048] The BET surface area, the CTAB surface area, and the oil absorption are measured according to the methods described in European patent application EP-A-157703. The mean projection area of the silicon dioxide is determined according to the method described in DE 69206445 T2, page 8, last paragraph to page 9, first paragraph. antioxidant
[0049] Antioxidants counteract oxidative degradation, in particular p-phenylenediamines should be mentioned, for example N,N'-alkyl- or aryldisubstituted p-phenylenediamines, especially preferred is N-(1,3-Dimethylbutyl)-N'-phenyl-1,4-phenylenediamine. Hardeners, crosslinkers, activators
[0050] The rubber compositions are produced using at least one hardener and at least one crosslinking agent, which are known to those skilled in the art in this field.
[0051] Examples include organic peroxides and polyamines.
[0052] In particular, sulfur is used as a vulcanizing agent.
[0053] Amines, diamines, guanidines, thioureas, thiatols, thirams, sulfenamides, sulfenimides, thiocarbamates, and xanthates are used as activators for the vulcanization process. N-cyclohexylbenzothiazole-2-sulfenamide (CBS) is particularly suitable.
[0054] Sulfur, metal oxides, fatty acids, especially stearic acid, and especially organosilane crosslinkers (see below under silane coupling agents) can be used, for example vinyl triethoxysilane, vinyl-tris-(beta-methoxyethoxy)silane, methacryloylpropyltrimethoxysilane, gamma-amino-propyl triethoxysilane, gamma-mercaptopropyltrimethoxysilane and the like.
[0055] In a particular embodiment, bis-(3-triethoxysilylpropyl)tetrasulfide is used.
[0056] Suitable metal oxides include ZnO, CaO, MgO, Al₂O₃, CrO₃, TiO₂, FeO, Fe₂O₃, and NiO. These can be used as oxides or as the corresponding fatty acid compounds, preferably as stearate.
[0057] Zinc oxide is preferred among these. Silane coupling agent
[0058] Typical coupling agents ensure a stable chemical and / or physical interaction between the individual components, for example fillers and rubbers.
[0059] These are typically sulfur-containing compounds, organosilanes, or polysiloxanes.
[0060] Preferably, coupling agents are those bearing a polysulfide group and an alkoxysilyl group; silane polysulfides are particularly preferred, for example, bis((C₁-C₄)alkoxy(C₁-C₄)alkylsilyl(C₁-C₄)alkyl)polysulfides (especially disulfides, trisulfides, or tetrasulfides), such as bis(3-trimethoxysilylpropyl) polysulfide or bis(3-triethoxysilylpropyl) polysulfide. Further examples are bis(3-triethoxysilylpropyl)tetrasulfide (TESPT) of the formula [(C₂H₅O)₃Si(CH₂)₃S₂]₂, or bis(triethoxysilylpropyl)disulfide (TESPD) of the formula [(C₂H₅O)₃Si(CH₂)₃S]₂. Other examples are bis(mono(C 1 -C 4 )alkoxy di(C 1 -C 4 )alkylsilylpropyl)polysulfide, especially disulfides, trisulfides or tetrasulfides), in particular bis(monoethoxydimethylsilylpropyl)tetrasulfide. composition
[0061] Butyl rubber, for example, makes up 5 to 40, preferably 5 to 25 phr in the tread compound of a vehicle tire. "phr" (parts per hundred rubber) indicates the composition based on the 100 parts by mass of the polymer blend.
[0062] Polybutadiene can constitute 30 to 50 phr, styrene-butadiene copolymers 40 to 70 phr, and polyisoprene 0 to 20 phr, with the provision that the sum of these polymers equals 100 phr. All non-rubber components are related to the sum of these polymers.
[0063] The proportion of fillers, especially carbon black and silicates, is generally 20 to 200 phr, preferably 30 to 150 phr.
[0064] The proportion of plasticizers is usually 10 to 30 phr.
[0065] According to the invention, the above-mentioned amine derivatives are added to these rubbers, which in a preferred embodiment may be polyisobutenyl substituted: The polyisobutene underlying the chain is a homo- and copolymer containing iso-butene in polymerized form with a number-average molecular weight Mn of 500 to 50000, preferably 550 to 40000, particularly preferably 650 to 30000, most preferably 750 to 20000 and particularly 900 to 15000.
[0066] In a preferred embodiment, the polyisobutene has a manganese content of 950 to 1050 mg / L. Among these polyisobutenes, those with a high content of terminally arranged ethylenic double bonds (α-double bonds) are preferred, particularly those with an α-double bond content of at least 50 mol%, preferably at least 60 mol%, more preferably at least 70 mol%, and most preferably at least 80 mol%. These are referred to as highly reactive polyisobutenes.
[0067] In another preferred embodiment, the polyisobutene is one with a Mn value of 2300 to 10000.
[0068] For the production of such isobutene-containing homo- or copolymers in polymerized form, both pure isobutene and isobutene-containing C4 hydrocarbon streams are suitable as isobutene sources. Examples include C4 raffinates, particularly "Raffinate 1," C4 sections from isobutane dehydrogenation, C4 sections from steam crackers, and C4 sections from FCC (fluid-catalyzed cracking) crackers, provided they are largely free of the 1,3-butadiene they contain. A C4 hydrocarbon stream from an FCC refinery unit is also known as a "b / b" stream. Other suitable isobutene-containing C4 hydrocarbon streams include, for example, the product stream from a propylene-isobutane co-oxidation or the product stream from a metathesis unit, which are generally used after standard purification and / or concentration. Suitable C4 hydrocarbon streams typically contain less than 500 ppm, preferably less than 200 ppm, of butadiene.The presence of 1-butene as well as cis- and trans-2-butene is largely uncritical. Typically, the isobutene concentration in the aforementioned C4 hydrocarbon streams is in the range of 40 to 60 wt.%. Thus, raffinate 1 generally consists essentially of 30 to 50 wt.% isobutene, 10 to 50 wt.% 1-butene, 10 to 40 wt.% cis- and trans-2-butene, and 2 to 35 wt.% butanes; in the polymerization process according to the invention, the unbranched butenes in raffinate 1 generally behave practically inertly, and only the isobutene is polymerized. In a preferred embodiment, a technical-grade C4 hydrocarbon stream with an isobutene content of 1 to 100 wt.%, in particular 1 to 99 wt.%, especially 1 to 90 wt.%, and most preferably 30 to 60 wt.%, is used as the monomer source for the polymerization.-%, in particular a raffinate 1 stream, a b / b stream from an FCC refinery unit, a product stream from a propylene-isobutane co-oxidation or a product stream from a metathesis unit.
[0069] Especially when using a raffinate 1 stream as the isobutene source, the use of water as the sole or additional initiator has proven effective, particularly when polymerizing at temperatures from -20°C to +30°C, and especially from 0°C to +20°C. However, at temperatures from -20°C to +30°C, and especially from 0°C to +20°C, the use of an initiator can also be omitted when using a raffinate 1 stream as the isobutene source.
[0070] The isobutene or the isobutene-containing C4 hydrocarbon stream can originate at least partially, preferably entirely, from renewable sources, as described, for example, in WO 2012 / 40859 A1, particularly from page 5, line 9 to page 6, line 24. The proportion of isobutene from renewable sources in the total isobutene used, measured according to ASTM D 6866, as described in WO 2012 / 40859 A1, is advantageously at least 1 wt%, preferably at least 2 wt%, particularly preferably at least 10 wt%, very preferably at least 25 wt%, and particularly at least 50 wt%. The proportion of isobutene from renewable sources can be up to 100 wt%, preferably up to 95 wt%, particularly preferably up to 90 wt%, very preferably up to 85 wt%, and particularly up to 80 wt%.
[0071] Isobutene obtained from renewable raw materials can be characterized by determining the 14< C / 12< C isotope ratio, preferably according to ASTM D 6866 ("Determining the Biobased Content of Natural Range Materials Using Radiocarbon and Isotope Ratio Mass Spectrometry Analysis").
[0072] According to this test method, the 14<C / 12<C isotope ratio of a sample is measured and compared to the 14<C / 12<C isotope ratio in a standardized 100% bio-based material. The result is the bio-based content of the sample.
[0073] The application of ASTM D6866 to derive the "bio-based content" is based on the same concepts as radiocarbon dating, but without using the age equations. The analysis is performed by determining the ratio of the amount of radiocarbon (1414C) in an unknown sample compared to that of a modern reference standard. This value is expressed as a percentage with the unit "pMC" (percent modern carbon). If the material being analyzed is a mixture of modern radiocarbon and fossil carbon (with very low radiocarbon content), the obtained pMC value correlates directly with the amount of biomass material present in the sample.
[0074] Bio-based materials are organic materials made from carbon derived from CO₂ recently (on a human timescale) fixed from the atmosphere using solar energy (photosynthesis). On land, this CO₂ is absorbed or fixed by plants (e.g., agricultural crops or forestry plantations). In the oceans, CO₂ is bound or fixed by photosynthesis in bacteria or phytoplankton. Thus, a bio-based material has a ¹⁴C / ¹²C isotope ratio greater than 0. In contrast, a fossil material has a ¹⁴C / ¹²C isotope ratio of approximately 0.
[0075] A small fraction of the carbon atoms in atmospheric carbon dioxide is the radioactive isotope 14C, which is formed when atmospheric nitrogen is struck by a neutron produced by cosmic radiation. This causes the nitrogen to lose a proton, forming carbon with an atomic mass of 14 (14C), which is then immediately oxidized to carbon dioxide. A small but measurable fraction of atmospheric carbon exists in the form of 14CO₂. Atmospheric carbon dioxide is assimilated by green plants to produce organic molecules during the process known as photosynthesis. Virtually all life forms on Earth depend on the production of organic molecules by green plants to generate the chemical energy that enables growth and reproduction.Therefore, the 14C that forms in the atmosphere eventually becomes part of all life forms and their biological products, enriching biomass and organisms that feed on biomass containing 14C. In contrast, carbon from fossil sources, especially petroleum or coal, does not exhibit the characteristic 14C: 12C ratio of renewable organic molecules derived from atmospheric carbon dioxide.
[0076] In a preferred embodiment of the present invention, the isobutene used in the polyisobutene has a bio-based content, measured as a 14< C: 12< C ratio ASTM-D6866 of more than 0%, preferably at least 1%, particularly preferably at least 5%, most preferably at least 10%, particularly at least 20% and especially at least 25%.
[0077] Advantageously, this bio-based content can be at least 30%, preferably at least 40%, particularly preferably at least 50%, most preferably at least 66%, in particular at least 75% and especially at least 85%.
[0078] With a proportion of at least 90%, preferably at least 95%, particularly preferably at least 98% and even 100%, this can be described as predominantly or completely bio-based isobutene.
[0079] According to this embodiment, resources are conserved and the product is manufactured at least partially with renewable raw materials.
[0080] In another embodiment of the present invention, the isobutene used in the polymerization can be obtained entirely from renewable raw materials or can consist of mixtures of isobutene from renewable and fossil sources.
[0081] This embodiment is particularly preferred where and for as long as isobutene from renewable sources is not available in industrially sufficient quantities and economically.
[0082] The aforementioned isobutene-containing monomer mixture can contain small amounts of contaminants such as water, carboxylic acids, or mineral acids without causing critical losses in yield or selectivity. It is advantageous to prevent the accumulation of these impurities by removing them from the isobutene-containing monomer mixture, for example, by adsorption onto solid adsorbents such as activated carbon, molecular sieves, or ion exchangers.
[0083] Monomer mixtures of isobutene or the isobutene-containing hydrocarbon mixture with olefinically unsaturated monomers that are copolymerizable with isobutene can also be reacted, although less preferably. If monomer mixtures of isobutene are to be copolymerized with suitable comonomers, the monomer mixture preferably contains at least 5 wt.%, more preferably at least 10 wt.%, and particularly at least 20 wt.% isobutene, and preferably at most 95 wt.%, more preferably at most 90 wt.%, and particularly at most 80 wt.% comonomers.
[0084] In a preferred embodiment, the amine derivatives that can be used according to the invention are polyisobutene derivatives containing at least one amino group (-NR 2< R 3< ). This means
[0085] R 2< and R 3< can each independently form hydrogen or C 1 -C 4 -alkyl or, although less preferably, together with the central nitrogen atom form a five- to seven-membered ring which may optionally contain another heteroatom.
[0086] Preferably, R 2< and R 3< are independently hydrogen, methyl, ethyl, n-propyl or n-butyl or together 1,4-butylene, 1,5-pentylene or 3-oxa-1,5-pentylene, particularly preferably hydrogen or methyl and most preferably hydrogen.
[0087] In a preferred embodiment, these are so-called polyisobutenamines (PIBA), which can be produced from highly reactive polyisobutene by hydroformylation and reductive amination with ammonia, monoamines, or polyamines such as dimethylaminopropylamine, ethylenediamine, diethylenetriamine, triethylenetetramine, or tetraethylenepentamine, as is known in particular from EP-A 244 616. Preferably, the reaction is carried out with ammonia. Thus, the residue R< 1< contains one more carbon atom than the underlying polyisobutene, which was introduced by the hydroformylation.
[0088] Due to its manufacturing process, polyisobutene is a mixture of double bond isomers, which determine its properties and especially its chemical reactivity. The most important of these are: Isomers with alpha double bonds as well as isomers with beta double bonds where the remainder PIB stands for the remainder of the polyisobutene without the substructure shown.
[0089] Furthermore, other isomers are conceivable, such as those shown in WO 2023 / 152258, which, however, play only a subordinate role according to the invention.
[0090] In a preferred embodiment of the invention, the polyisobutene used for hydroformylation has an alpha double bond content of at least 70%, preferably at least 75%, particularly preferably at least 80%, most preferably at least 85%, and particularly preferably at least 90%. Such polyisobutene is also referred to as highly reactive polyisobutene.
[0091] The content of beta double bonds can be up to 25%, preferably up to 20%, particularly preferably up to 15%, most preferably up to 10% and particularly up to 5%.
[0092] The content of isomers other than those with alpha or beta double bonds is usually no more than 5%.
[0093] The isomer content is determined using 1H NMR spectroscopy, with the sensitivity being determined by the frequency of the instrument. 1H NMR spectroscopy is preferably performed at 700 MHz at 25 °C. Particularly preferably, the isomers are identified according to the method described in Guo et al., Journal of Polymer Science, Part A: Polymer Chemistry, 2013, 51, 4200-4212.
[0094] In a preferred embodiment, the polyisobutene has a number-average molecular weight Mn of 104 to 10000 g / mol with the above-mentioned contents of alpha and beta double bonds, preferably from 156 to 5000, particularly preferably from 500 to 2500.
[0095] In a further, less preferred embodiment, the polyisobutene (A) has a number-average molecular weight Mn of more than 10,000 up to 100,000 g / mol, preferably from 11,000 to 90,000, particularly preferably from 12,000 to 80,000, most preferably from 13,000 to 75,000, and particularly from 14,000 to 70,000, and an alpha double bond content of at least 20 to 60%, preferably at least 25 to 45%, and particularly preferably at least 30 to 40%. Such a polyisobutene is also referred to as medium molecular weight polyisobutene.
[0096] The use of high molecular weight polyisobutene with a number-average molecular weight of more than 100,000 up to 5,000,000 g / mol is conceivable, although less preferred, and typically has an alpha double bond content of no more than 50%, preferably no more than 40%, and most preferably no more than 30%.
[0097] The molecular weight is determined by gel permeation chromatography using polystyrene as a standard.
[0098] The idealized structure of a polyisobutenamine is
[0099] The number of loops n is defined as above.
[0100] For a number-mean molecular weight Mn of the preferably underlying polyisobutene of 168 to 2300, n is from 1 to 39, for an Mn of 224 to 1500, n is from 2 to 25, for an Mn of 550 to 1300, n is from 8 to 21, for an Mn of 700 to 1300, n is from 10 to 21, and for an Mn of 950 to 1050, n is from 15 to 17.
[0101] If the underlying polyisobutene is produced from isobutene-containing C4 hydrocarbon streams (so) containing monomers other than isobutene, the polymeric backbone comprises other monomers in polymerized form, e.g. 1-butene and cis- and trans-2-butene, in particular 1-butene.
[0102] Such a polyisobutenamine is obtained by polymerizing isobutene to a polyisobutene with an (idealized) terminal double bond, which is then subjected to hydroformylation and subsequent amination with ammonia. This process is described by way of example in Example 1 of US 4832702. The parameter n corresponds to the degree of polymerization of the isobutene in the polyisobutene minus 2; the polyisobutene used preferably has a molecular weight of approximately 1000 g / mol.
[0103] In a further preferred embodiment, these are compounds containing free amino and imido groups, such preferably reaction products of alkyl- or alkenyl-substituted succinic anhydride with aliphatic polyamines (polyalkylenemines) such as, in particular, ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine and hexaethyleneheptamine, which have an imide structure.
[0104] Such polyisobutenylsuccinimides have the formula up, in which R 1< represents a polyisobutenyl residue with a number-average molecular weight Mn of 104 to 100000 g / mol, preferably of 104 to 10000 g / mol, particularly preferably of 156 to 5000 g / mol and most preferably of 500 to 2500 g / mol, and x represents a positive integer of, for example, 1 to 4, preferably 2 to 4, particularly preferably 3 or 4.
[0105] Preferably, the residue R 1< has a molecular weight of 550 to 2300, preferably of 650 to 1500 and particularly preferably of 750 to 1300 g / mol.
[0106] In a further preferred embodiment, the reaction products of alkyl- or alkenyl-substituted succinic anhydride with N-single- or double-substituted 1,ω-alkylenediamines, preferably 1,3-propylenediamines, are used as amine derivatives that can be employed according to the invention.
[0107] Beispiele dafür sind N-Cyclohexylpropylendiamin-1,3; N-2-Ethylhexylpropylendiamin-1,3; N-Dodecyl-1,3-Propylendiamin; N-Stearylpropylendiamin-1,3; N-Oleylpropylendiamin-1,3; N-3-Aminopropyltalgfettamin; N-Arachidylpropylendiamin-1,3; N-Behenylpropylendiamin-1,3; N-Benzyl-propylendiamin-1,3; N-Phenylpropylendiamin-1,3; 2-Aminoethylstearylamin; 2-Aminoethylbehenylamin; 2-Aminoethyloleylamin; 2-Aminoethyltalgfettamin; N-Stearylbishexamethylendiamin-1,6; N-Stearyldipropylentriamin; N-Dodecyldipropylentriamin; N,N-Dimethylaminopropylamin-1,3; N,N-Ditridecylpropylendiamin-1,3; N,N-Bis(2-Ethylhexyl)-3-Aminopropylenamin; Bis-aminopropyltalgfettamin; Bis-aminopropyllaurylamin, 1-(2-Aminopropyl)-stearylamin; 1-(2-Aminopropyl)-piperazin; N-2-Aminoethyl-piperidin; N-3-Aminopropylimidazol.
[0108] Bevorzugt ist N,N-Dimethylaminopropylamin-1,3.
[0109] As a rule, when the anhydride functionalities open, the respective amides are formed first, or at higher reaction temperatures, ring closure to the respective imides occurs.
[0110] The preparation is described, for example, in WO 2012 / 004300. If the temperature in the reaction of the alkyl- or alkenyl-substituted succinic anhydride with the N-single- or double-substituted 1,ω-alkylenediamines is kept below about 80 °C, predominantly an amide is formed, with minor amounts of imide also being formed under these reaction conditions.
[0111] The compounds that can be used according to the invention, which contain a spacer X derived from succinic acid, are generally based on polyisobutenyl-substituted succinic anhydrides (PIBSA), which are obtainable by ene reaction of highly reactive polyisobutenes with maleic anhydride and serve as starting materials for the amides or imides.
[0112] In a preferred embodiment, highly reactive polyisobutenes with the number-average molecular weight Mn specified above are used for these polyisobutenyl-substituted succinic anhydrides.
[0113] In a preferred embodiment, the polyisobutenyl-substituted succinic anhydrides (PIBSA) to be used also have more than simply substituted products.
[0114] The ratio of the more highly maleated to the simply maleated components can be expressed by the "degree of bismalination" (BMG). The BMG is known per se (see also US 5,883,196) and can be determined using the following formula: BMG = 100 % × wt − % BM PIBSA / wt − % BM PIBSA + wt − % PIBSA where wt-%(X) represents the respective weight fraction of component X (X = PIBSA (simply maleated polyisobutene) or BM PIBSA (more than simply maleated polyisobutene)) in the reaction product of polyisobutene with maleic anhydride.
[0115] The degree of bismaleitization is preferably calculated from the saponification value according to DIN 53401: 1988-06 of the sample. The sample must be solubilized with a suitable solvent if necessary, preferably a 2:1 mixture of toluene and ethanol.
[0116] It should be noted that only the ratio of the more highly maleated components to the simply maleated components is considered, whereas unreacted polyisobutene present in the reaction mixture, for example, polyisobutene without reactive double bonds, is not included in the determination of the degree of bismaleitization. Therefore, the reaction mixture may still contain unreacted polyisobutene, which usually corresponds to the portion of the polyisobutene used that does not contain reactive double bonds, whereas the portion of the polyisobutene containing reactive double bonds preferentially reacts completely or almost completely.
[0117] In a preferred embodiment, the PIBSA have a bismaleitization level of at least 5%, preferably at least 8%, particularly preferably at least 10%.
[0118] A further advantage is that such conversion products of polyisobutene with a bismaleitization level of at least 12%, preferably at least 15%, particularly preferably at least 20% can be used.
[0119] The degree of bismaleination can be up to 60%, preferably up to 55%, particularly preferably up to 50%, especially up to 45%, and specifically up to 40%. By selecting suitable reaction conditions, especially a high excess of maleic anhydride, the degree of bismaleination can be increased to up to 80% and even up to 100%.
[0120] The best results are achieved with a bismaleitization level of 10 to 50%, preferably 12 to 45% and particularly preferably 15 to 40%.
[0121] The amine derivatives according to the invention are generally added to the rubber mixture in amounts of 2 to 20, preferably 4 to 14, particularly preferably 5 to 10 phr.
[0122] These compounds are typically added to the rubber compound along with the other components and heated in a kneader or extruder to initiate vulcanization. It can also be advantageous to first thoroughly mix the rubber compound and fillers together with the amine derivatives and then add the other components, especially antioxidants, activators, and / or plasticizers, later.
[0123] Accordingly, a further embodiment of the present invention is a method for lowering the viscosity of rubber masses in the manufacture of rubber-containing tires, in which one at least one rubber containing carbon black and / or silicates and at least one processing aid and / or additive to improve at least one performance characteristic of the tire mixed in a kneader and / or extruder, whereby at least one amine derivative as described above is added to the rubber mass before and / or during processing.
[0124] The processes for vulcanization and production of rubber compounds are known in themselves and can be applied to the use of amine derivatives.
[0125] One advantage of amine derivatives is that they have a beneficial effect on improving at least one of the following properties. Dispersion coefficient, particle size, wet adhesion, abrasion resistance, rolling resistance have rubber-containing tires.
[0126] The amine derivatives are particularly suitable for improving the dispersion of fillers, especially silica, in rubber compounds.
[0127] Furthermore, they offer a particular advantage in reducing rolling resistance.
[0128] During the production of rubber compounds, the use of amine derivatives continues to show the advantage of significantly reducing the viscosity of the rubber compounds during the processing and manufacture of rubber-containing tires.
[0129] Accordingly, a further object of the present invention is a method for lowering the viscosity of rubber masses in the manufacture of rubber-containing tires, in which one at least one rubber containing carbon black and / or silicates and at least one processing aid and / or additive to improve at least one performance characteristic of the tire mixed in a kneader and / or extruder, in which at least one amine derivative is added to the rubber mass before and / or during processing as described.
[0130] Furthermore, these compounds offer advantages in terms of wet grip at low temperatures (-10 °C) and / or rolling resistance and / or abrasion resistance of the tires containing them. Preferably, the amine derivatives improve at least two of these three properties. It is a particular advantage that the amine derivatives simultaneously offer advantages in terms of wet grip at low temperatures (-10 °C) and the rolling resistance and abrasion resistance of the tires.
[0131] Increasing the abrasion resistance of tires reduces the release of microplastics from tire abrasion during the operation of motor vehicles.
[0132] Another item is rubber compounds containing at least one rubber selected from the group consisting of isobutene-isoprene rubber, styrene-butadiene rubber and natural rubber, at least one filler selected from the group consisting of calcium carbonate, clays, mica, silica, silicates, talc, bentonite, titanium dioxide, aluminum oxide, zinc oxide and carbon black, at least one antioxidant, preferably a p-phenylenediamine, at least one peroxide and / or polyamine as a hardener and / or crosslinker, at least one activator for the vulcanization process selected from the group consisting of amines, diamines, guanidines, thioureas, thiatols, thirames, sulfenamides, sulfenimides, thiocarbamates and xanthates, at least one silane crosslinker selected from the group consisting of bis((C 1 -C 4 )alkoxy(C 1 -C 4 )alkylsilyl(C 1 -C 4 ) )alkyl)polysulfides, (especially disulfides, trisulfides or tetrasulfides), bis(3-trimethoxysilylpropyl) polysulfide, bis(3-triethoxysilylpropyl) polysulfide,Bis(3-triethoxysilylpropyl)tetrasulfide (TESPT) of the formula [(C 2 H 5 O) 3 Si(CH 2 ) 3 S 2 ] 2 , and bis(triethoxysilylpropyl)disulfide (TESPD) of the formula [(C 2 H 5 O) 3 Si(CH 2 ) 3 S] 2 , and at least one amine derivative of the formula ,
[0133] A further object of the present invention is, for cases in which at least one of the two residues R 2< and R 3< is hydrogen, preferably if both are hydrogen, compounds of the formula R 1< -X-NR 3< -Si(OC 2 H 5 ) 2 -(CH 2 ) 3 -S 4 -(CH 2 ) 3 -Si(OC 2 H 5 ) 3 and R 1< -X-NR 3< -Si(OC 2 H 5 ) 2 -(CH 2 ) 3 -S 2 -(CH 2 ) 3 -Si(OC 2 H 5 ) 3 , in which R 1< , X and R 3< have the above meanings, as well as rubber compounds containing at least one of these compounds, the use of which in rubber-containing tires, especially for improving the compatibility of silicates in rubber-containing tires and their use for improving at least one of the following properties: dispersion coefficient, particle size, wet grip, abrasion resistance, rolling resistance, vulcanization rate of rubber-containing tires.
[0134] Another object of the present invention is derivatives of polyisobutenamine with the silane coupling agent having the idealized structure as follows: wherein the number n is as defined above and Y represents -(S) y -R 25< -Si(OR 26< ) 3 and y represents 1, 2, 3 or 4 and R 25< is an alkylene residue with 1 to 6 carbon atoms, preferably 1 to 4 carbon atoms, particularly preferably 2 or 3 carbon atoms and is most preferably selected from the group consisting of methylene, 1,2-ethylene, 1,2-propylene, 1,3-propylene, 1,4-butylene, 5-oxa-1,5-pentylene and 1,6-hexylene, in particular 1,3-propylene, and R 26< is a C 1 to C 6 alkyl, preferably a C 1 to C 4 alkyl, particularly preferably methyl, ethyl, n-propyl, isopropyl, n-butyl or tert-butyl, most preferably Methyl, ethyl or n-butyl, especially methyl or ethyl and specifically methyl.
[0135] These compounds, as well as rubber compounds containing at least one of these compounds, the use of which in rubber-containing tires, especially to improve the compatibility of silicates or as coupling agents in rubber-containing tires, and their use to improve at least one of the following properties Dispersion coefficient, particle size, wet adhesion, abrasion resistance, rolling resistance, vulcanization rate Rubber-containing tires are also the subject of the present invention.
[0136] A further object of the present invention for cases in which at least one of the two residues R 2< and R 3< is hydrogen, preferably if both are hydrogen, are derivatives of the amine compounds with the fatty acids used as activators, especially stearic acid, with the structure as follows: R 1< -X-NR 3< -(C=O)-R 10< in which R 1< , X and R 3< have the above meanings and R 10< denote the residue of a fatty acid, preferably a saturated alkyl residue or a mono- or polyunsaturated alkenyl residue with 9 to 19 carbon atoms.
[0137] Preferably the residue R 10< -(C=O)- is derived from fatty acids such as lauric acid, myristic acid, stearic acid, palmitic acid, lauric acid, oleic acid, linoleic acid and linolenic acid or mixtures thereof.
[0138] Technically common fatty acid mixtures are preferably tallow fatty acid, coconut oil fatty acid, trans fatty acid, coconut palm kernel oil fatty acid, soybean oil fatty acid, rapeseed oil fatty acid, peanut oil fatty acid or palm oil fatty acid, which contain oleic acid and palmitic acid as their main components.
[0139] These compounds, as well as rubber compounds containing at least one of these compounds, their use in rubber-containing tires, especially vulcanization activators or accelerators in rubber-containing tires, and their use to improve at least one of the following properties Dispersion coefficient, particle size, wet adhesion, abrasion resistance, rolling resistance, vulcanization rate Rubber-containing tires are also the subject of the present invention.
[0140] Furthermore, the compounds according to the invention are suitable for binding alcohols, especially ethanol, released during the production of rubber compounds for tires, so that lower emissions are released during production.
[0141] Without wishing to be bound to any one theory, it is assumed that alcohols R 6< OH, especially ethanol, released during the production of rubber compounds for tires, react with previously unreacted succinic anhydride or carboxylic acid groups and are bound as carboxylic acid esters. It is also conceivable that the released alcohol R 6< OH, especially ethanol, displaces alcohols or amines from the existing carboxylic acid ester, amide, or imide bond in a transesterification or transamidation reaction.
[0142] The following combinations, for example, can be formed: From the connections or or can be formed or or From the connection can be formed or or in which the variables each have their above meaning.
[0143] In the case of amine derivatives of the formula wherein R 2< and R 3< are hydrogen, one of the residues R 2< and R 3< or both can be replaced by R 6< , preferably by ethyl.
[0144] These compounds, which are formed from the reaction with released alcohol, as well as rubber masses containing at least one of these compounds, their use in rubber-containing tires, especially to improve the compatibility of silicates or as coupling agents in rubber-containing tires, and their use to improve at least one of the following properties Dispersion coefficient, particle size, wet adhesion, abrasion resistance, rolling resistance, vulcanization rate Rubber-containing tires are also the subject of the present invention.
[0145] The present invention is illustrated by the following examples, without being limited thereto. Examples Production examples Connection 1
[0146] Polyisobutenamine with a number-average molecular weight Mn of approximately 1000 g / mol, commercially available as Kerocom PIBA 03 from BASF SE, Ludwigshafen, dissolved in Mihagol. Connection 2
[0147] 150.20 g of Glissopal® < 1000 from BASF SE, Ludwigshafen, with a number-average molecular weight of Mn (determined by GPC) of approximately 1000 g / mol, polydispersity of approximately 1.6, alpha double bond content (determined by < 13C NMR) of approximately 88%, and beta double bond content of 6%, were heated to 225 °C with 29.4 g (0.30 mol, 2 eq.) of maleic anhydride in an autoclave and stirred for 7 h. The reaction mixture was then cooled to 80 °C and 150 mL of heptane was added. The solution was stirred at 100 °C for 1 h and then filtered. The solvent was removed under vacuum (yield = 164.00 g). (SV: 175 mg KOH / g). A polyisobutenyl succinic anhydride (PIBSA) with a bismaleitization level of approximately 100% was obtained. Connection 3
[0148] 122.2 g of a polyisobutenyl succinic anhydride obtained analogously to compound 2, with a salinity of 91.8 mg KOH / g, were dissolved in 100.60 g of toluene. The reaction mixture was treated with 11.20 g (0.11 mol) of 3-dimethylaminopropylamine and stirred for 2 h at 120 °C. The reaction mixture was then cooled to room temperature and the solvent was removed under vacuum (yield = 130.50 g). Connection 4
[0149] 126.10 g of a polyisobutenyl succinic anhydride obtained analogously to compound 2, with a solubility of 89.0 mg KOH / g, were dissolved in 100.00 g of toluene. The reaction mixture was treated with 18.90 g (0.10 mol) of tetraethylenepentamine and stirred for 2 h at 120 °C. The reaction mixture was then cooled to room temperature and the solvent was removed under vacuum (yield = 142.10 g). Method description Improvement of the dispersion coefficient
[0150] The macrodispersion (Dispersion Index Analysis System, DIAS) of undivided filler agglomerates (particles) is determined by comparing the reflectance of the particle surfaces with the total observation area using a light microscope at 125x magnification and at least 10 images. This yields the degree of dispersion (expressed as a percentage), taking into account the filler volume fraction and the void volume of the fillers via correction factors. A high dispersion coefficient is the desired result. Determination of particle size
[0151] The mean diameter of the particles was determined optically together with the calculation of the dispersion coefficient.
[0152] A small particle size is advantageous. Wet grip at low temperatures (-10 °C) and rolling resistance
[0153] A strip test specimen (40 × 10 × 2 mm) of the manufactured rubber mass is subjected to dynamic mechanical analysis (DMA) in an ARES testing device from Rheometric Scientific ™.
[0154] Measurement parameters: Temperature range -60 to 80 °C, frequency 1 Hz, amplitude 0.5%
[0155] The tan(δ) value at -10 °C is considered a measure of traction on wet roads at low temperatures, while the tan(δ) value at +60 °C is a measure of rolling resistance. High tan(δ) values at -10 °C indicate high wet grip and are advantageous, while low tan(δ) values at +60 °C indicate low rolling resistance and are desirable. Abrasion resistance
[0156] The abrasion was determined according to DIN ISO 4649 in an abrasion test apparatus from Frank GmbH under a load of 10 N over a sliding length of 40 m and a rotation of 40 m. The abrasion index is given as a percentage [%]; higher values are positive. Reduction of viscosity during processing
[0157] The components of the rubber masses were mixed together in the specified ratios and the Mooney viscosity of the mass was determined at a temperature of 100 °C at 2 revolutions / min in a Mooney meter Alpha Technologies MV 2000 E (Mooney ML (1+4) 100 °C).
[0158] Viscosity is measured in Mooney units (ME). Vulcanization acceleration
[0159] A silica-containing rubber compound, as described below, was treated at 160 °C with an amplitude of 0.5% and a frequency of 1.67 Hz in a Monsanto MDR 2000E vulcanizer, with the torque being monitored over time. The increase in torque indicates the progress of vulcanization.
[0160] Furthermore, the rubber mass was vulcanized at 160 °C under a load of 280 bar in an apparatus from Rucks Maschinenbau KV 207.00 to determine the t 90 value.
[0161] A reduction in the t90 time is advantageous. Application examples
[0162] Silica-containing ("reference") rubber compounds were produced for comparison and with the additives according to the invention, with the following composition: Quantity [phr] function Designation reference rubber SBR (high-Tg) NS616 1)< 100 Silica U7000 GR 2)< 80 Silane Si 69 3)< 8 Plasticizers Vivatec 500 37,5 activator ZnO 2,5 activator Stearic acid 1 Antioxidant IPPD 4)< 2 accelerator DPG 5)< 2 accelerator CBS 6)< 1,7 Networker sulfur 1,4 1) Nipol NS616 rubber (modified S-SBR, styrene content: 20 wt%, vinyl group content: 67 mol%, SP value: 17.25 (J / cm³< ) 1 / 2< , Tg: -25°C, Mw: 510,000, non-oil-extended) manufactured by ZEON CORPORATION (SBR1 in EP 3263360 A1, paragraph
[0054] ) 2) Amorphous SiO₂, Ultrasil 7000 GR from Evonik 3) Bis(triethoxysilylpropyl)tetrasulfide 4) IPPD: N-Isopropyl-N'-phenyl-1,4-phenylenediamine 5) DPG: N,N'-Diphenylguanidine 6) CBS: N-Cyclohexylbenzothiazole-2-sulfenamide Rubber compounds according to the invention
[0163] By adding the specified amount of the compounds according to the invention, silica-containing rubber compounds K1 to K5 were produced analogously to the silica-containing reference rubber compound "Reference". To compensate, the proportion of plasticizer was partially reduced accordingly. Quantity [phr] function Designation K1 K3 K4 rubber SBR (high-Tg) NS616 100 100 100 Silica U7000 GR 80 80 80 Silane Si 69 8 8 8 Connection 1 5 Connection 3 5 Connection 4 5 Plasticizers Vivatec 500 32,5 32,5 32,5 activator ZnO 2,5 2,5 2,5 activator Stearic acid 1 1 1 Antioxidant IPPD 2 2 2 accelerator DPG 2 2 2 accelerator CBS 1,7 1,7 1,7 Networker sulfur 1,4 1,4 1,4 Example 1 (Improvement of the dispersion coefficient)
[0164] Dispersion coefficient [%] reference 61 K1 72 K3 70 K4 78 Example 2 (reduction of particle size)
[0165] Particle size reference 180 K1 115 K3 158 K4 119 Example 3 (Wet grip at low temperatures (-10 °C))
[0166] Wet grip (tan(δ) -10°C ) reference 0,83 K3 1,07 K4 1,00 Example 4 (rolling resistance)
[0167] Rolling resistance tan(δ) 60°C reference 0,14 K1 0,056 K3 0,037 K4 0,04 Example 5 (Abrasion resistance)
[0168] Abrasion resistance reference 129 K3 134 K4 146 PIBA 142 Example 6 (Shore A hardness)
[0169] The Shore A hardness was determined using a Zwick digitest device according to DIN ISO 48-4. Dispersion coefficient [%] reference 64 K1 67 K3 64 K4 65 Example 7 (Acceleration of vulcanization)
[0170] t90 [min] reference 18,60 K1 19,16 K3 17,86 K4 18,37
Claims
1. Use of amine derivatives of the formula wherein X is a single bond or an organic spacer, R1 is a linear or branched alkenyl radical having a molecular weight Mn of 104to 100000 g / mol, preferably from 104 to 10000 g / mol, particularly preferably from 156 to 5000 g / mol and very particularly preferably from 500 to 2500 g / mol R2 and R3 independently of one another are a further single bond to the organic spacer X, hydrogen, C1- to C4-alkyl, a group -R-NR4R5 or a repeating radical -[-R-NH-]x--H, x being a positive integer from 1 to4 R is a divalent organic radical having 2 to 6 carbon atoms, radical, preferably selected from the group consisting of 1,2-ethylene, 1,2-propylene and 1,3-propylene, R4 and R5 is independently hydrogen or C1- to C4-alkyl for improving at least one of the following properties - dispersion coefficient - particle size - wet grip - abrasion resistance - rolling resistance - vulcanization speed of rubber-containing tires.
2. Use according to claim 1, characterized in that the amine derivative is a polyisobutene amine of the formula is, wherein n is a positive integer from 0 to 960, preferably from 0 to 94, particularly preferably from 1 to 46 and very particularly preferably from 3 to 22.
3. Use according to claim 1, characterized in that the amine derivative has the formula oder oder satisfies, wherein R is a divalent alkylene radical, which may optionally be interrupted by oxygen atoms R4 and R5 are independently of one another hydrogen or C1- to C4-alkyl.
4. Use according to claim 3, characterized in that - R is 1,3-propylene and - R4 and R5 are each C1- to C4-alkyl.
5. Use according to claim 1, characterized in that the amine derivative has the formula satisfies, wherein R is a divalent alkylene radical, which is optionally interrupted by oxygen atoms can be and x is a positive integer from 1 to 4.
6. Use according to claim 5, characterized in that - R is 1,2-ethylene and - x is a positive integer from 1 to 4, preferably 2 or 3.
7. Use according to one of claims 1 or 3 to 6, characterized in that R1 is selected from the group consisting of - linear C10- to C30-alkenyl - branched C9- to C30-alkenyl, obtainable by polymerization of C3 and / or C4 alkenes - branched alkenyl, derived from homo- and copolymers containing iso-butene in copolymerized form homo- and copolymers with a number-average molecular weight Mn of 104 to 100000 g / mol, preferably from 104 to 10000 g / mol, particularly preferably from 156 to 5000 g / mol and very particularly preferably from 500 to 2500 g / mol.
8. Use according to one of claims 1 or 3 to 6, characterized in that the radical R1 is a radical wherein n is from 0 to 960, preferably from 0 to 94, particularly preferably from 1 to 46 and very particularly preferably from 3 to 22.
9. Use according to one of the preceding claims for simultaneously improving at least two, preferably all three, of the following properties - wet grip - abrasion resistance - rolling resistance of rubber-containing tires.
10. Use according to one of claims 1 to 9 for reducing microplastics from tire abrasion.
11. Use according to one of claims 1 to 9 for reducing fuel consumption and associated emissions by reducing the rolling resistance of rubber-containing tires.
12. Use according to one of the preceding claims, characterized in that the rubber is an isobutene-isoprene rubber.
13. Use according to one of claims 1 to 11, characterized in that the rubber is a styrene-butadiene rubber.
14. Process for lowering the viscosity of rubber compounds in the manufacture of rubber-containing tires, in which - at least one rubber with - carbon black and / or silicates and - at least one processing aid and / or additive for improving at least one service property of the tire is mixed in an internal mixer and / or extruder, characterized in that at least one amine derivative as described in one of claims 1 to 8 is added to the rubber compound before and / or during processing.
15. Use of amine derivatives as described in one of claims 1 to 8 for lowering the viscosity of rubber compounds in the manufacture of rubber-containing tires.
16. Rubber compound, containing - at least one rubber, selected from the group consisting of natural rubber, polybutadienes, styrene-butadiene copolymers and polyisoprene and mixtures thereof, preferably mixtures of natural rubber and styrene-butadiene copolymers, of natural rubber and polybutadienes, or natural rubber and polyisoprenes, - at least one filler, selected from the group consisting of calcium carbonate, clays, mica, silica, silicates, talc, bentonite, titanium dioxide, aluminum oxide, zinc oxide and carbon black, - at least one antioxidant, preferably a p-phenylenediamine, - at least one peroxide and / or polyamine as hardener and / or crosslinker, - at least one activator for the vulcanization process selected from the group consisting of amines, diamines, guanidines, thioureas, thiazoles, thiurams, sulfenamides, sulfenimides, thiocarbamates and xanthates, - at least one silane crosslinker selected from the group consisting of bis((C1-C4)alkoxy(C1-C4)alkylsilyl(C1-C4)alkyl) polysulfides (especially disulfides, trisulfides or tetrasulfides), bis(3-trimethoxysilylpropyl), bis(3-triethoxysilylpropyl)polysulfide, bis(3-triethoxysilylpropyl)tetrasulfide (TESPT) of the formula [(C2H5O)3Si(CH2)3S2]2, and bis(triethoxysilylpropyl)disulfide (TESPD) of the formula [(C2H5O)3Si(CH2)3S2]2, and at least one amine derivative as described in one of claims 1 to 8.