Modified bone replacement material
Patent Information
- Application Number
- ES2023218159T
- Authority / Receiving Office
- ES · ES
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-12-19
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-19
AI Technical Summary
Current bone substitute materials, such as hydroxyapatite and calcium phosphate, primarily exhibit osteoconductive properties and lack the ability to directly stimulate bone regeneration or proliferation, with additional osteoinductive substances like growth factors often being washed away quickly and causing systemic effects.
A method to modify bone replacement materials or implant surfaces by incorporating strontium, fluorine, magnesium, manganese, and/or gallium ions into the hydroxyapatite lattice through a controlled thermal treatment process, ensuring these ions are concentrated at the surface for sustained osteotropic and osteoinductive effects.
The modified materials provide long-lasting, localized osteotropic and osteoinductive properties, enhancing bone healing and integration without systemic effects, and are applicable to bone defects and implant surfaces.
Smart Images

Figure 00000013_0000 
Figure 00000013_0001 
Figure 00000014_0000
Abstract
Description
[0001] The invention relates to a method for modifying a bone replacement material or a surface coating of an implant to a product with osteotropic properties from a solid, microporous starting material comprising essentially hydroxyapatite (Ca 5 [OH|(PO 4 ) 3 ].
[0002] Within the scope of the invention, the starting materials mentioned can also include materials which have a structure analogous to the starting materials, but are synthetically produced.
[0003] Many currently used bone substitute materials derived from natural bone, whether autologous, allogeneic, or xenogeneic, coral, algae, or fully synthetic hydroxyapatite bone substitutes, which are used as bone implants or as bone substitutes in bone augmentation procedures, only possess osteoconductive properties. This means that while existing calcium phosphate or hydroxyapatite bone substitute materials offer a suitable biocompatible surface for the direct growth of bone tissue onto the implant surface, they do not directly stimulate bone regeneration in the immediate vicinity of the implant.
[0004] Hydroxyapatite or calcium phosphate materials are fundamentally only osteoconductive. They thus allow bone growth and serve as a guiding structure, but do not themselves stimulate the proliferation or differentiation of bone-forming cells, such as osteoblasts or their precursors. Direct growth, as defined by the invention, can be understood in particular as growth without an "intermediate tissue layer" between the implant surface and the bone tissue.
[0005] To exert an osteoinductive effect, bone substitute materials or organic substances such as collagen are currently supplemented with additional proteins, peptides, or other molecules. Examples include growth factors such as various BMPs, IGF1 / 2, FGF, etc., or serum products. The problem here is that these substances often remain in the implant or at the implant site for unpredictable periods, as they are usually quickly washed away or broken down from the implant bed. As a result, the osteoinductive properties are only present for a short time and cannot be precisely controlled. Furthermore, systemic effects throughout the entire organism are possible, which are generally undesirable.
[0006] Natural bone contains trace elements of certain ions within the crystalline structure of calcium phosphate, which ultimately constitute the inorganic composition of bone hard tissue. These incorporated ions, such as strontium (Sr), magnesium (Mg), manganese (Mn), and zinc (Zn), are known to play a fundamental role in bone development, either individually or in combination. Strontium is present in natural bone in considerable quantities, particularly in regions of increased metabolic activity. Its presence is associated with increased osteoclast apoptosis and enhanced osteoblastic cell proliferation and collagen synthesis, which subsequently maintain bone formation and inhibit bone resorption.
[0007] Strontium has been shown to possess osteotropic and osteoinductive properties. Therefore, increasing the proportion of strontium as a natural trace element in bone substitute materials or implant surfaces to stimulate bone-forming cells is of great interest. Such an increase in strontium imparts the desired osteotropic and osteoinductive properties to a bone substitute material or implant surface.
[0008] The same applies to the elements zinc, magnesium, manganese, gallium, and fluorine, whose bone-growth-stimulating properties are also described in the literature. Two methods exist for producing such strontium-enriched bone substitute materials. EP 3,777,904 A1 describes the production of a bone substitute material from calcifying algae or mammalian bones as the starting material, while US 10,688,218 B2 describes the production of a bone substitute material from wood as the starting material. Both methods are based on a known, very energy-intensive hydrothermal process, which was first described in US 3,929,971 and EP 230,570 B1.The further development of the teachings of the methods of the first-mentioned publications EP 3 777 904 A1 and US 10,688,218 B2 consists in the additional incorporation of strontium ions into the crystal lattice by a modification of the original method from publications US 3,929,971 and EP 230 570 B1.
[0009] All of the above-mentioned processes describe a technically and energetically very complex hydrothermal process. In this process, the starting material, after the addition of chemical additives and sometimes highly toxic solutions, is exposed in a closed container to temperatures of up to approximately 230 °C and the resulting pressure for an extended period. This can last from several hours, or even days depending on the temperature applied. Under these conditions, the desired ion exchange of calcium ions for strontium ions within the crystal lattice of the starting material is achieved. In this process, the strontium ions are absorbed into the starting material in a relatively homogeneous manner, but only in very small quantities. Consequently, only a small amount of strontium is available at the surface of the treated starting material to stimulate bone cells.This therefore only involves the occasional exchange of calcium ions by strontium ions; there is no question of a conversion of hydroxyapatite into strontium apatite.
[0010] Nevertheless, a bone substitute material manufactured in this way exerts a local osteotropic and osteoinductive effect, which occurs primarily and essentially only within the implant bed. Thus, such a bone substitute material has a local, but not a systemic, effect. A further advantage is that such a bone substitute material exerts its osteoinductive and osteotropic effects throughout its entire time in the implant bed and only ceases once it is replaced by autochthonous bone tissue. Therefore, even a slight increase in the strontium content can achieve faster and more sustained bone healing of a bone defect.
[0011] The invention therefore lies in the TaskThe basis is to specify a method for modifying a bone replacement material or surface coating of an implant to a product with osteotropic properties, as well as an osteotropic bone replacement material or osteotropic surface coating which has long-acting, locally limited osteotropic and osteoinductive properties.
[0012] This problem is solved according to the invention by a method for modifying a bone replacement material or a surface coating of an implant with the features of claim 1 and an osteotropic bone replacement material or an osteotropic surface coating with the features of claim 11.
[0013] Advantageous embodiments of the invention are specified in the dependent claims.
[0014] According to the invention, a bone substitute material or a surface coating of an implant is to be modified into a product with osteotropic properties. The product is to be made from a solid, microporous starting material comprising essentially hydroxyapatite (Ca5[OH|(PO4)3]).
[0015] The starting material of the invention consists of small porous solids in the form of granules measuring approximately 0.2 to 2.0 mm or larger shaped bodies, which are synthetically produced or of natural origin. They are already present in a macroscopically visible crystalline form, and this macroscopic form is not altered by the application of the process.
[0016] Its structure acts as a volume carrier and a kind of "lattice" or "guiding structure" for bone growth and should therefore retain its shape even during clinical use. This material should not be confused with the bone cements often described in the literature. These are used to fix, for example, orthopedic prostheses such as hip or femoral neck prostheses and, furthermore, to stabilize fractured vertebrae by "injection." Bone cements consist of finely ground powders mixed with solutions immediately before application to the patient and then injected with the prosthesis in low or high viscosity (liquid or paste). Under a chemical exothermic reaction generating heat, they set and harden, forming the finest crystalline structures.
[0017] These types of bone cements are used to compensate for gaps or inaccuracies in the fit between the bone and the prosthesis, such as a titanium hip prosthesis. This ensures a stable fit of the prosthesis within the bone. Furthermore, they can be used to fill cavities in osteoporotic fractured vertebrae, thus preventing further fractures by restabilizing the vertebral body.
[0018] Such stabilization cannot be achieved with bone substitute materials, as bone formation must first develop around the material. The material itself does not provide stability in the same way as bone cement. Bone substitute materials, as described and used here, consist of small solid particles whose porous and interconnected structures are utilized to enable ingrowth onto and between the granular solids. The bone substitute material is ultimately completely incorporated into the newly formed bone and, if necessary, resorbed over the years as part of the natural bone remodeling processes and replaced by genuine bone. Its crystalline microstructure and macroscopic form are already present before application and should be preserved as much as possible after application. Unlike bone cements, no new crystals form here through a chemical reaction generating heat during application to the patient.
[0019] In summary, bone cements are powders that, at the time of application, are mixed with solutions to form a liquid to pasty mass. They then set and harden through a chemical reaction that generates heat and forms minute crystalline structures. They compensate for inconsistencies in the fit between two materials or serve as an immediately load-bearing support in vertebral fractures. Ingrown bone is virtually impossible. In contrast, bone substitute materials are already in crystalline form as granules, do not react chemically upon application, and have no stabilizing function, but merely a volume-enhancing and conductive one during bone regeneration.
[0020] According to the inventive method, a modification material from a solid source containing strontium, fluorine, magnesium, manganese, zinc, and / or gallium atoms is ground to an average diameter of no more than 1.0 mm or less, and the ground modification material is applied to the starting material to produce an intermediate product. Subsequently, the intermediate product is thermally treated in an open atmosphere at a treatment temperature below the melting point of the modification material and the bone substitute material or the surface coating of the implant for a treatment period, allowing moisture to escape, to produce the product in which some calcium atoms of the hydroxyapatite are replaced by atoms of the modification material.The modification material of the intermediate product has a maximum moisture content of 10%, and the treatment temperature and time are within a range whose lower limit is a treatment temperature of at least 400°C and a treatment time of at least 30 minutes. This range is further defined by the following combinations: a treatment temperature of at least 500°C and a treatment time of at least 10 minutes; a treatment temperature of at least 600°C and a treatment time of at least 7 minutes; a treatment temperature of at least 700°C and a treatment time of at least 5 minutes; a treatment temperature of at least 900°C and a treatment time of at least 3 minutes; and a treatment temperature of at least 1150°C and a treatment time of at least 2 minutes. Finally, the product is cleaned of any remaining modification material by mechanical, chemical, or physical cleaning processes.
[0021] With the method according to the invention, it has been possible for the first time to incorporate strontium, fluorine, magnesium, manganese, zinc, and / or gallium ions into the surface of apatite, particularly hydroxyapatite, facing bone growth, rather than merely depositing them or distributing them in low concentrations throughout the entire solid. This ensures that the ions are available in increased concentrations directly on the surface of the bone substitute material, especially during the crucial initial phase of bone growth in the first days and weeks. With purely superficial deposition, as described, for example, in JP 2021029750, where crystal growth of strontium apatite on a surface is described, detachment of the deposited substances could occur. With a uniform distribution throughout the entire solid, as in the known hydrothermal method of EP 3 777 904 A1, the distribution of the ions is homogeneous, and the concentration at the surface is very low.However, the inventive method makes it possible to bind the aforementioned ions, which have osteotropic (i.e., osteoinductive), antiresorptive, and / or bone-forming properties, to the resulting apatite structure in such a way that they cannot be readily released. This is achieved by the described method because the chemical composition of the apatite surfaces, particularly those of hydroxyapatite, that have come into contact with the strontium, fluorine, magnesium, manganese, zinc, and / or gallium sources is selectively altered.
[0022] In the process according to the invention, for example, when strontium fluoride is used as the strontium source in the contact area on the surface of a hydroxyapatite after heat treatment according to the described process, superficial "islands" and "band-like areas" of strontium phosphate are formed, which are firmly integrated into the surface of the hydroxyapatite. These "islands" represent areas in which a conversion of calcium phosphate to strontium phosphate has taken place through ion exchange. In these clearly demarcated areas, hydroxyapatite has thus been converted into the bioactive strontium phosphate by the input of energy.
[0023] Treatment time and treatment temperature are interrelated. This means that a lower treatment temperature can be selected for a longer treatment time than for a shorter treatment time. According to the invention, this physicochemical relationship between time and energy input is clarified by specifying the treatment time and treatment temperature according to the invention by means of a range defined by its limits. The lowest described combination is a treatment temperature of 400°C and a treatment time of at least 30 minutes. If the treatment temperature is increased, the treatment time can be reduced. This means that the invention cannot be successfully implemented with a treatment temperature of 400°C and a treatment time of only 20 minutes.Further points defining the possible combinations are a minimum treatment temperature of 500°C and a minimum treatment time of 10 minutes, a minimum treatment temperature of 600°C and a minimum treatment time of 7 minutes, a minimum treatment temperature of 700°C and a minimum treatment time of 5 minutes, a minimum treatment temperature of 900°C and a minimum treatment time of 3 minutes, and a minimum treatment temperature of 1150°C and a minimum treatment time of 2 minutes. This is described in the figure description. Figure 45 To explain further: Below 400°C, no or virtually no reaction takes place. Above 1150°C, depending on the chosen modification material, it either melts or sinters.
[0024] In principle, the application of the comminuted modification material to the starting material can be carried out in any way. However, it has been found that certain methods yield particularly good results. For example, the comminuted modification material can be at least partially dissolved in a liquid, preferably water, and applied to the starting material, followed by drying to remove the liquid. The liquid thus serves as a carrier medium for the modification material. After drying, the modification material remains on the starting material.
[0025] Another possibility is to mix the crushed modification material with small amounts of liquid to create a slurry-like consistency and then apply this slurry to the starting material. Here too, the liquid acts as a carrier medium, and the resulting slurry-like consistency ensures sufficiently good application to the starting material.
[0026] If a liquid is used to apply the modification material to the starting material, it can be helpful to remove excess pulverized modification material by physical means before thermally treating the intermediate. This has been shown to lead to better results in the final product.
[0027] However, it is not absolutely necessary to use a liquid to apply the modification material to the starting material. It is also possible to embed the starting material in the pulverized modification material and then thermally treat it. Alternatively, dry, pulverized modification material can be applied to the starting material.
[0028] Preferably, the sources of strontium, fluorine, magnesium, manganese, zinc and / or gallium atoms are the respective substances themselves or chemical compounds, preferably their salts, containing these atoms, in particular selected from: strontium fluoride, magnesium fluoride, zinc fluoride, manganese, gallium oxide. In this process, good incorporation or exchange of the atoms with the atoms of the starting material can occur.
[0029] Furthermore, it is advantageous to select compounds as sources of strontium, fluorine, magnesium, manganese, zinc, and / or gallium that are non-toxic for processing, have sufficient solubility in a non-toxic solution, or can be present in fine powder form, have melting points that are as low as possible and ideally below the melting point of the starting material, and whose residual products and residues after annealing are also non-toxic and can be readily removed by mechanical, physical, or chemical purification methods. In the case of strontium, a salt of strontium, namely strontium fluoride, has proven effective. Strontium fluoride dissolved moderately well in distilled water in the experiments. This solubility could be improved by applying heat up to the boiling point of the distilled water.
[0030] In principle, the thermal treatment of the intermediate product can be carried out in any way desired. Heating and / or cooling intervals can be incorporated to achieve the desired treatment temperature or room temperature.
[0031] It is preferred that the heating and / or cooling temperature change is a maximum of 10°C per minute, preferably less than 5°C per minute. Such temperature changes have been shown to have the least impact on the durability of the final product. A cooling interval of one hour at room temperature has also proven to be gentle on the material.
[0032] This gentle approach prevents embrittlement or the transition to a glassy phase of the materials. Lower temperatures are associated with longer annealing times and a less pronounced effect on the desired surface change, but this also allows for precise control of the composition of the new material.
[0033] Generally, longer heating of the material to be modified at relatively low temperatures is preferred in order to modify the starting material gently. According to the invention, it has been found that heating to 900°C for 30 minutes already yields excellent results, so that even longer heating or higher temperatures do not necessarily lead to significantly better results.
[0034] In the case of using hydroxyapatite in the form of bone substitute material from bovine bone or algae as the starting material and strontium fluoride as the strontium source, temperatures of 400°C to 1150°C and an annealing time of at least 2 min to a maximum of 300 min have proven effective in achieving the desired result, namely a conversion of hydroxyapatite (calcium phosphate) into the desired strontium phosphate in the direct contact area with the ion source strontium fluoride, without causing damage to the starting material.
[0035] However, it is also possible to introduce the intermediate product directly into a treatment unit that essentially operates at the treatment temperature. Particularly good results were achieved, according to the investigations on which the invention is based, when the treatment temperature was below the melting point of the starting material and the ion source.
[0036] The bone substitute material used is a starting material which essentially contains hydroxyapatite (Ca 5 [OH(PO 4 ) 3 ]); other known bone substitute materials are calcium phosphate, tricalcium orthophosphate or tricalcium phosphate, calcium hydroxide, calcium oxide, aragonite, calcite in the form of calcined, uncalcined and / or chemically processed biological skeletons or vertebrate or mammalian bones after or before pyrolytic or chemical maceration.
[0037] Aragonite or calcite, e.g., from calcareous algae, can be used in calcined, uncalcined, and / or chemically processed form. When using vertebrate or mammalian bones, they are advantageously subjected beforehand to pyrolytic or chemical maceration, that is, the removal of immunogenic material.
[0038] It is preferable if the starting material, in the case of organic origin, has already been subjected to pyrolytic treatment and / or chemical purification prior to treatment according to the invention and thus freed from organic components. This does not apply to synthetically produced materials.
[0039] Furthermore, the invention relates to an osteotropic bone substitute material or an osteotropic surface coating of an implant, which were produced according to the inventive method. In this case, calcium atoms of the hydroxyapatite are partially replaced by strontium, fluorine, magnesium, manganese, zinc and / or gallium atoms.
[0040] The osteotropic and osteoinductive surface of such a bone substitute material or implant, which essentially consists of apatite, exhibits, on the surface facing bone growth, island-like or band-like, sharply defined areas of crystal transformations of hydroxyapatite into specific crystals of the corresponding ions from the strontium, fluorine, magnesium, manganese, zinc, and / or gallium sources. These areas exhibit osteotropic and osteoinductive properties after implantation into an animal or human body. In addition to apatite, particularly hydroxyapatite, small amounts of calcium phosphate, especially tricalcium phosphate, and calcium carbonate, especially calcite or aragonite, may also be present.
[0041] The osteotropic and osteoinductive bone substitute material produced according to the inventive method can, for example, be used to manufacture dimensionally stable blocks. Since the resulting osteotropic bone substitute material has a granular to powder-like form, the dimensionally stable blocks produced from it can be custom-made and thus adapted to bone defects. Furthermore, the surfaces of implants, whether metallic or ceramic, can be subjected to surface treatment in this way, provided they contain apatite, preferably hydroxyapatite or calcium phosphate. This results in a bioactive, osteotropic, and osteoinductive surface, which promotes faster and more likely osseointegration of the respective implant into the bone.For example, hydroxylapatite-coated titanium dental implants or all-ceramic dental implants could be subjected to such heat treatment for the incorporation of bone cell-stimulating strontium, fluorine, magnesium, manganese, zinc and / or gallium ions to improve osseointegration into the jawbone.
[0042] Through the surface modification of a starting material according to the invention, this material, whether in the form of bone substitute material or as surfaces on implants, exerts a local osteotropic and osteoinductive effect, which occurs mainly and essentially only in or at the implant site. Thus, the bone substitute material according to the invention has no systemic effect. A further advantage is that the surface modification of a starting material according to the invention, whether in the form of bone substitute material or as surfaces on implants, exerts its osteotropic and osteoinductive effects throughout the entire time it remains in the implant site and only ceases once it is replaced by autochthonous bone tissue. This results in faster and more sustainable bone healing of a bone defect or the integration of an implant into the bone.
[0043] Another application example for the osteotropic bone substitute material according to the invention is the acceleration of healing in osteoporotic, traumatic and / or malignant vertebral fractures or compression fractures after their stabilization by stimulating bone regeneration. A further possibility would be to use the material produced according to the invention as a starting material for 3D printing processes.
[0044] In the following, we will describe the execution of the inventive method by way of example and finally explain the corresponding analysis results.
[0045] The characters are also referenced here. This shows: Fig. 1 a secondary electron image of a first embodiment of the method according to the invention; Fig. 2 material contrasts of the first embodiment of the method according to the invention; Figures 3 to 8 elemental distribution maps of the first embodiment of the method according to the invention; Figures 9 and 10 single-point and small-area analyses of the first embodiment of the method according to the invention; Fig. 11 a secondary electron image of a second embodiment of the method according to the invention; Fig. 12 material contrasts of the second embodiment of the method according to the invention; Figures 13 to 18 elemental distribution maps of the second embodiment of the method according to the invention; Figures 19 and 20 single-point and small-area analyses of the second embodiment of the method according to the invention; Fig. 21 a secondary electron image of a third embodiment of the method according to the invention; Fig.Figures 22: Material contrasts of the third embodiment of the method according to the invention; Figures 23 to 30: Elemental distribution maps of the third embodiment of the method according to the invention; Figures 31 and 32: Single-point and small-area analyses of the third embodiment of the method according to the invention; Figure 33: A secondary electron image of a fourth embodiment of the method according to the invention; Figure 34: Material contrasts of the fourth embodiment of the method according to the invention; Figures 35 to 42: Elemental distribution maps of the fourth embodiment of the method according to the invention; Figures 43 and 44: Single-point and small-area analyses of the fourth embodiment of the method according to the invention; and Figure 45: A diagram illustrating the treatment temperature and time.
[0046] For this purpose, strontium fluoride was dissolved in distilled water, with the release behavior being improved by applying heat up to the boiling point of the distilled water. Subsequently, a starting material consisting of hydroxyapatite in the form of granules of the bone substitute material BioOss from Geistlich and Algipore from Dentsply Sirona was introduced into the strontium fluoride solution.
[0047] Thorough wetting with the strontium source was achieved by stirring and heating. Excess water was removed by pouring it off through a sieve. The treated material was then dried by evaporation by placing it in a heating oven at 180°C until sufficiently dry.
[0048] The removal of the coarsest excesses of the strontium source was achieved by simple sieving. The material, thus dried and freed from coarse excesses of the strontium source, was then subjected to a thermal treatment, which can also be described as an annealing process, and after cooling, was again freed from coarse and loose excesses and residues of the strontium source by washing and sieving in distilled water.
[0049] During the annealing process, a high-temperature furnace for the dental sector with a combustion chamber of approximately 15 x 10 x 17 cm and a heating module for programming heating intervals and holding stages as well as temperature control was used.
[0050] The pre-treated and dried material was placed in a refractory ceramic dish in the combustion chamber, the air-permeable combustion chamber was closed, and the annealing program was started. The end products analyzed below were produced at holding temperatures of 900°C for 30 or 60 minutes without a heating interval and without a defined cooling interval, simply cooling to room temperature. At these temperatures and annealing times, a sufficiently good conversion of the starting material was achieved, whereby, as already described, the aforementioned ions were incorporated and bonded to the crystal lattice of the apatite. Material analyses showed that the hydroxyapatite (calcium phosphate) of the starting material was converted to strontium apatite (strontium phosphate) on the surface precisely at those points where contact areas with the strontium fluoride had existed.The lower the oven temperature, the slower and less pronounced this phenomenon became. This fact could be used to control the composition of the desired end product.
[0051] For analysis, the samples prepared as described were embedded in epoxy resin. Since the samples were intended for analysis in a scanning electron microscope, these non-conductive preparations were first made conductive with a thin layer of carbon.
[0052] The samples were placed in a scanning electron microscope (LEO 440) with a tungsten cathode. Images were acquired at an excitation voltage of 20 kV and various beam currents. The shown SE images (secondary electron images) depict topographic contrasts.
[0053] The BSE (backscattered electron) images shown in the figures illustrate material contrasts. The brighter a pixel is in the BSE image, the higher the average atomic number of the material found at that location.
[0054] For example, in the samples presented here, one area is significantly lighter where the Ca present in the apatite has been replaced in significant amounts by Sr.
[0055] Chemical analysis in the SEM was performed using an X-Max 150 detector. This is an SDD detector that can simultaneously detect the analyzable elements using energy dispersion.
[0056] To characterize the samples, element distribution maps were first created for each location. Here, an area of the sample that appeared interesting was "mapped" at a resolution of 1024 * 768 pixels.
[0057] Based on these element distribution maps, targeted individual analyses were then carried out at specific points. This resulted in spectra with very good statistics, enabling the generation of meaningful chemical analysis data. The element distribution maps shown in the figures were selected selectively. Although other elements were also included, they proved irrelevant to the research question under consideration. Sample bone material 0.5h / 900°C
[0058] The in the Figures 1-10 The analyses shown relate to bovine bone which was treated according to the inventive method for 0.5 h / 900°C. Here, it shows Fig. 1A secondary electron micrograph shows that the polished sample has almost no relief. The majority of the sample consists of the bone material used here, which appears in medium gray tones. The dark areas originate from the locations of the epoxy resin. The light gray grains are embedded in this epoxy resin and are located close to the bone material.
[0059] Fig. 2 The image shows material contrasts. Within the bone material, clearly distinguishable areas with slight differences are visible in the grayscale. This is likely due to slight variations in the chemical composition or density of the apatite in these areas.
[0060] The grains appear so bright in the BSE image because they contain large amounts of the heavy element strontium (Sr). Several bright areas can also be seen in the upper part of the image, which originate from grains containing Sr.
[0061] Upon closer inspection, several light-colored areas can be seen within the bone material. This occurs primarily where the SrF2 granules are located close to the bone. However, there are also light-colored areas where no SrF2 is visible. It could be assumed that SrF2 was present there once as well (before preparation).
[0062] The following section explains the element distribution maps that are included in the Figures 3 to 8 are shown. In the images for the elements P ( Fig 3 ) and Ca ( Fig 4 The bone material is immediately apparent. The concentrations of the elements appear to vary locally – as already explained in the discussion of the BSE image. It seems that both elements exhibit higher and lower concentrations at the same locations. It is assumed that the bone material may exhibit variations in density at these locations.
[0063] However, another fact is striking. If one examines the areas in the elemental distribution map where the BSE image was lighter in the bone material, the phosphorus image suggests that there is less phosphorus there. As will become clear later, this is only partially true. Simultaneously, the calcium image shows that the calcium is practically no longer visible in these areas. Something has clearly changed.
[0064] In the images for the Sr ( Fig 5 ) and the F ( Fig 6 ) one can recognize the position of the SrF 2 grains. Simultaneously, considering the elemental distribution for oxygen (O) ( Fig 7At these points, it can be seen that some of the grains in the center of the image exhibit a slight rim with increased oxygen concentrations. This is more pronounced in the upper middle area of the image. There, fluorine is hardly visible, but oxygen is much more abundant. Since the strontium was introduced in the form of SrF₂ at the beginning of the experiment, it can be assumed that oxidation of the material occurred during the experiment. Fig. 8 shows an element distribution map for carbon (C).
[0065] Furthermore, it can be observed that significant concentrations of strontium are present in areas where calcium and phosphorus levels are lower in the bone material. These are primarily the areas that—as already mentioned—are located close to the strontium-rich fluoride (SrF2) grains or their oxygen-rich conversion products. It is particularly important to document and characterize these areas in more detail using point analyses. Single-point analyses
[0066] Using single-point and small-area analyses, as described in the Figures 9 and 10 The findings resulting from the element distribution maps have now been substantiated in more detail, as previously shown.
[0067] For this sample, points 1 to 4 (small area analyses) show that it consists of "normal" apatites containing Ca and P. Significant amounts of F and some Cl are also present. The Sr is at the detection limit.
[0068] This also applies to analysis point 5, which represents the beginning of a small profile extending to point 9. Here, the Sr content increases significantly, while the Ca value decreases accordingly. At the last point of the profile (point 9), 71 wt% SrO is found. Looking at the atomic composition, it appears that the P content remains approximately constant. Likewise, the sum of Ca and Sr seems to remain roughly the same. This could mean that even in the Sr-rich areas, there is a phase that stoichiometrically corresponds to apatite, but in which the Ca is successively replaced by Sr.
[0069] Another profile (points 10 to 15) shows identical behavior.
[0070] Analysis 17 shows a nearly ideal grain of SrF 2, while analysis 16 already suggests some oxidation of SrF 2.
[0071] Analysis points 18 to 23 show SrF₂ grains that have undergone varying degrees of transformation. It is not possible to determine what these grains are. Analysis points 20 and 21, for example, show significantly more oxygen than the known divalent cations Ca and Sr would normally exhibit. Bone sample 1.0h / 900°C
[0072] The in the Figures 11-20 The analyses shown relate to beef bones treated according to the inventive method for 1 hour at 900°C. The figures show analyses analogous to those described previously.
[0073] The sample processed for one hour showed conditions not much different from the sample treated for only half an hour. However, fewer residual grains of SrF₂ were found. Where reactions involving the incorporation of Sr occurred, these grains appear to penetrate somewhat further.
[0074] The area of the sample shown in the figures contains no relict SrF 2 .
[0075] The elemental distribution map of Sr clearly shows that significant amounts of SrF₂ must have been present. However, they appear not to have survived the experiment and to have left behind only massive concentrations of Sr in the apatite.
[0076] The three single-point profiles produced (from 1 to 6, from 7 to 11 and from 12 to 16) each clearly show the increase in the concentration of Sr towards the edge.
[0077] The content of C also appears to increase slightly towards the edges of these profiles. This behavior was already indicated in the previous sections, but is most noticeable here. Sample algae material 0.5h / 900°C
[0078] The in the Figures 21-32The analyses shown refer to algal material which was treated according to the inventive method for 0.5h / 900°C.
[0079] Fig. 21 shows a secondary electron image and Fig. 22 Again, material contrasts. In Fig. 23 is an element distribution map for P, in Fig. 24 an elemental distribution map for Ca, in Fig. 25 an elemental distribution map for Mg, in Fig. 26 an element distribution map for Na, in Fig. 27 an element distribution map for Sr, in Fig. 28 an element distribution map for F, in Fig. 29 an element distribution map for O, in Fig. 30 An element distribution map for C is shown. Figures 31 and 32 Single-point and small-area analyses, in turn, show this.
[0080] The algal material in this sample consists of calcium phosphate.
[0081] While chemical inhomogeneities can only be vaguely discerned in the BSE image, the element distribution maps are significantly more informative.
[0082] Firstly, it is evident that there are local concentrations of magnesium in the calcium phosphate. Here, the magnesium is likely incorporated as a substitute for the calcium. It is also striking that the magnesium is sometimes concentrated at the edges of the grains. This indicates significant mobilization of the magnesium during the heating process. It is quite possible that this mobilization only occurs when approaching the melting point of the material. However, no definitive statement can be made here.
[0083] Similar statements can be made for Na, which also has its highest concentrations at the edge of the algal material.
[0084] The elemental distribution map clearly shows the enrichment of Sr at the edge of the algal material. Four profiles (1 to 5, 8 to 11, 12 to 15, and 16 to 20) were analyzed. All of these profiles show a significant increase in Sr at the expense of Ca.
[0085] The element chlorine plays no role in this algal material. In contrast, fluorine is prominently represented. Sample: Algae material 1.0h / 900°C
[0086] Finally, the following concern the Figures 33-44 The algal material shown was treated according to the inventive method for 1 hour at 900°C. The figures show the analyses analogous to those described previously.
[0087] Here again, the same phenomena can be seen as already mentioned above in the sample with a treatment duration of 0.5 hours.
[0088] The profiles (points 1 to 4, 6 to 8 and 19 to 23) each show the increase in the concentrations of Sr.
[0089] For profiles 19 to 23, small areas were analyzed instead of points, thus representing an integral analysis of the area. Here too, the increase in Sr is evident.
[0090] In both SrF 2 grains shown in the image, it can be seen that the Sr penetrates the porous algal material to a depth of approximately 50 µm. This is significantly more than in the compact bone material.
[0091] In summary, it can be stated that in the present samples, the incorporation of Sr into the bone material and into the algae material occurred to a very pronounced extent under the present experimental conditions.
[0092] It can be seen that the sr sometimes penetrates quite deeply into the material, displacing the ca from the lattice. The stoichiometric calculation of the atomic fractions suggests that a simple exchange of the two elements for each other is taking place.
[0093] The formation of oxygen-rich rims around the SrF₂ grains can be clearly demonstrated. This extends to the complete displacement of SrF₂. Whether this effect represents an intermediate stage in the displacement of Ca from the apatite lattice cannot be determined.
[0094] Figure 45 Figure 1 shows a diagram illustrating the temperature and treatment time range according to the invention. According to the invention, the thermal treatment takes place under specific conditions. These are defined by a range determined by the treatment temperature and treatment time, as shown in Figure 2. Figure 45 This is illustrated. The maximum temperature is determined by the melting point of the products used. Thus, the temperature and treatment time range in which the reaction according to the invention proceeds successfully is located to the right above the curve shown in the figure.
[0095] According to the invention, the inventive method can be carried out when the combination of treatment temperature and treatment time lies within the range whose lower limit is defined by the points 1150°C / 2 min, 900°C / 3 min, 700°C / 5 min, 600°C / 7 min, 500°C / 10 min, and 400°C / 30 min. In other words, the invention can be carried out, for example, at 500°C and 20 min, but at least not with the exceptionally good results achieved with a treatment at 550°C and 30 min. Conversely, the invention cannot be successfully carried out with a treatment at 400°C and 20 min.
Claims
1. Method for modifying a bone replacement material or a surface coating of an implant into a product having osteotropic properties, from a solid, microporous starting material which substantially comprises hydroxyapatite (Ca5[OH|(PO4)3] and is present in crystalline form so as to be macroscopically visible, with the steps to be carried out in the following order: - comminuting a modification material from a solid source of strontium, fluorine, magnesium, manganese, zinc and / or gallium atoms to an average diameter of at most 1.0 mm or smaller, - applying the comminuted modification material to the starting material in order to produce an intermediate product, - thermally treating the intermediate product at a treatment temperature below the melting point of the modification material and of the bone replacement material or of the surface coating of the implant, for a treatment time, in a device for thermal treatment in an open atmosphere, so that moisture can escape, in order to produce the product, wherein calcium atoms of the hydroxyapatite are partially replaced by atoms of the modification material, - wherein the modification material of the intermediate product exhibits a maximum moisture of 10% and - wherein the treatment temperature and the treatment time lie within a range whose lower limit is at least 400 °C treatment temperature and at least 30 min treatment time, and wherein the range is further defined by the combinations of at least 500 °C treatment temperature and at least 10 min treatment time, at least 600 °C treatment temperature and at least 7 min treatment time, at least 700 °C treatment temperature and at least 5 min treatment time, at least 900 °C treatment temperature and at least 3 min treatment time, and at least 1150 °C treatment temperature and at least 2 min treatment time, - cleaning the product of non-incorporated modification material by mechanical, chemical or physical cleaning methods.
2. Method according to claim 1, characterized in that for applying the comminuted modification material to the starting material, the comminuted modification material is at least partially dissolved in a liquid, preferably water, and is applied to the starting material, wherein a subsequent drying is carried out in order to remove the liquid.
3. Method according to claim 1, characterized in that for applying the comminuted modification material to the starting material, the comminuted modification material is admixed with small amounts of a liquid in order to produce a slurry-like consistency, and this slurry is deposited on the starting material.
4. Method according to any one of claims 1 to 3, characterized in that before the thermal treatment of the intermediate product, excess comminuted modification material is removed by means of physical steps.
5. Method according to any one of claims 1 to 4, characterized in that for applying the comminuted modification material to the starting material, the starting material is embedded in the comminuted modification material and is thermally treated in this manner.
6. Method according to any one of claims 1 to 4, characterized in that for applying the comminuted modification material to the starting material, dry comminuted modification material is deposited.
7. Method according to any one of claims 1 to 6, characterized in that the sources used for strontium, fluorine, magnesium, manganese, zinc and / or gallium atoms are the respective substances themselves or chemical compounds, preferably salts thereof, which comprise these atoms, in particular selected from: strontium fluoride, magnesium fluoride, zinc fluoride, manganese, gallium oxide.
8. Method according to any one of claims 1 to 7, characterized in that for thermally treating the intermediate product, heating and / or cooling intervals are provided in order to reach the desired treatment temperature or room temperature.
9. Method according to any one of claims 1 to 8, characterized in that the heating and / or cooling temperature change is at most 10 °C per minute, preferably less than 5 °C per minute.
10. Method according to any one of claims 1 to 7, characterized in that for thermally treating the intermediate product, the latter is introduced directly into a treatment device which substantially exhibits the treatment temperature.
11. Osteotropic bone replacement material or osteotropic surface coating of an implant produced by one of the methods 1 to 10, characterized in that calcium atoms of the hydroxyapatite are partially replaced by strontium, fluorine, magnesium, manganese, zinc and / or gallium atoms.