Method for obtaining a purified diester effluent by depolymerising a polyester comprising opaque polyethylene terephthalate

FI4077511T3Undetermined Publication Date: 2026-11-05IFP ENERGIES NOUVELLES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
FI2020817361T
Authority / Receiving Office
FI · FI
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-07
Filing Date
2020-12-07
Publication Date
2026-11-05
Estimated Expiration
2040-12-07
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The invention relates to a glycolytic depolymerization process for a polyester, particularly polyester terephthalate, comprising colored and / or opaque and / or multilayer polyethylene terephthalate (PET), for recycling in a polymerization unit. More specifically, the invention relates to a glycolytic depolymerization process for a polyester feedstock comprising at least colored and / or opaque PET, with an optimized final purification step for the resulting biodiesel effluent. Previous technique

[0002] The chemical recycling of polyester, particularly polyethylene terephthalate (PET), has been the subject of much work aimed at breaking down polyester recovered as waste into monomers that can again be used as a filler in a polymerization process.

[0003] Many polyesters are sourced from material collection and sorting systems. In particular, polyester, especially PET, can come from the collection of bottles, trays, films, resins, and / or polyester-based fibers (such as textile fibers or tire fibers). Polyester from these collection and sorting streams is called recyclable polyester.

[0004] Recyclable PET can be classified into four main categories: Clear PET, consisting mainly of colorless transparent PET (generally at least 60% by weight) and azure-colored transparent PET, contains no pigments and can be used in mechanical recycling processes; dark or colored PET (green, red, etc.) can generally contain up to 0.1% by weight of dyes or pigments but remains transparent or translucent; opaque PET contains a significant amount of pigments, typically ranging from 0.25% to 5.0% by weight, to opacify the polymer. Opaque PET is increasingly used, for example, in the manufacture of food containers, such as milk bottles, and in the composition of cosmetic, plant protection product, or dye bottles; multilayer PET consists of layers of polymers other than PET or a layer of recycled PET between layers of virgin PET (i.e., PET that has not undergone recycling), or an aluminum film, for example.Multilayer PET is used after thermoforming to make packaging such as trays.

[0005] The collection systems that feed into the recycling systems are structured differently depending on the country. They evolve to maximize the amount of plastic recovered from waste, taking into account the nature and quantity of the waste streams and the sorting technologies used. The recycling process for these waste streams generally consists of an initial flake-forming stage during which bales of raw packaging are washed, purified, and sorted, then shredded and purified and sorted again to produce a flake stream containing generally less than 1% by mass of "macroscopic" impurities (glass, metals, other plastics, wood, paperboard, mineral elements), preferably less than 0.2% of "macroscopic" impurities, and even more preferably less than 0.05%.

[0006] The clear PET flakes can then undergo an extrusion-filtration process to produce extrudates that can be reused by blending them with virgin PET to make new products (bottles, fibers, films). A solid-state vacuum polymerization (SSP) step is required for food-grade applications. This type of recycling is called mechanical recycling.

[0007] Dark (or colored) PET flakes are also mechanically recyclable. However, the coloring of the extrudates formed from colored streams limits their uses: dark PET is most often used to produce fibers or packaging strips. Therefore, its market opportunities are more limited compared to those of clear PET.

[0008] The presence of opaque PET containing significant amounts of pigments in recycled PET poses problems for recyclers because opaque PET alters the mechanical properties of the recycled PET. Opaque PET is currently collected with colored PET and ends up in the colored PET stream. Given the increasing uses of opaque PET, the levels of opaque PET in the colored PET stream are currently between 5-20% by weight and are tending to increase further. Within a few years, it will be possible to reach opaque PET levels in the colored PET stream exceeding 20-30% by weight. However, it has been shown that beyond 10-15% opaque PET in colored PET streams, the mechanical properties of the recycled PET are altered (see...). "Impact of the development of opaque white PET on the recycling of PET packaging" (preliminary note from COTREP dated 5 / 12 / 13) and prevent recycling in the form of fibers, the main outlet for colored PET in the industry.

[0009] Dyes are natural or synthetic substances, soluble in materials such as polyester, used to color the materials into which they are incorporated. Dyes commonly used are of various types and often contain O and N heteroatoms, and conjugated unsaturates, such as quinone, methine, and azo groups, or molecules like pyrazolone and quinophthalone. Pigments are finely divided substances, insoluble in materials such as polyester, used to color and / or opacify the materials into which they are incorporated. The main pigments used to color and / or opacify polyesters, particularly PET, are metal oxides such as TiO₂, CoAl₂O₄, and Fe₂O₃, as well as silicates, polysulfides, and carbon black. Pigments are particles with a size generally between 0.1 and 10 µm, and mostly between 0.4 and 0.8 µm.The complete removal of these pigments by filtration, necessary to consider recycling opaque PET, is technically difficult because they are extremely clogging.

[0010] Recycling colored and opaque PET is therefore extremely delicate.

[0011] US patent application 2006 / 0074136 describes a glycolysis depolymerization process for colored PET, particularly PET recovered from green-colored PET bottles. The feedstock processed by this method is in the form of PET flakes and is contacted with ethylene glycol in a reactor at a temperature between 180 and 280°C for several hours. The glycolysis product obtained at the end of the depolymerization step is purified over activated carbon at a temperature above 170°C and then by extraction of residual colorants, particularly yellow colorants, using a solvent such as an alcohol like methanol or a glycol like ethylene glycol. The BHET crystallizes in the extraction solvent and is then separated by filtration.

[0012] In US patent application 2015 / 0105532, post-consumer PET comprising a mixture of different colored PETs, such as clear PET, blue PET, green PET, and / or amber PET, in flake form, is depolymerized by glycolysis in the presence of ethylene glycol, an amine catalyst, and alcohol, in a batch reactor at 150-250°C. The resulting diester monomer is purified by filtration, ion exchange, and / or passage through activated carbon, particularly at a temperature of 80-90°C, before being crystallized and recovered by filtration.

[0013] US patent 6,642,350 describes the purification of a crude BHET solution, comprising at least a series of contacting steps involving activated carbon, an anion exchange resin, and a cation exchange resin, specifically at temperatures of 60°C, 65°C, or 80°C. This patent demonstrates that simple contact with activated carbon alone is insufficient to completely decolorize the solution, as a residual color, particularly yellow, is observed when the crude BHET solution is contacted solely with activated carbon.

[0014] Other earlier techniques are known from WO2018 / 007356.

[0015] Finally, patent application FR 3053691 describes a process for depolymerizing a polyester filler comprising opaque PET and, in particular, 0.1 to 10 wt% pigments, by glycolysis in the presence of ethylene glycol. A purified bis-(2-hydroxyethyl) terephthalate (BHET) effluent is obtained after specific separation and purification steps by adsorption. However, the BHET effluent obtained by the process described in application FR 3053691 can exhibit imperfections: in particular, the BHET effluent becomes discolored rapidly despite passing through an adsorbent column.

[0016] The present invention seeks to improve the glycolytic depolymerization processes of polyester fillers comprising colored and / or opaque PET, and in particular the process described in French patent application FR 3053691, specifically to improve the purification, and more particularly the decolorization, of the diester effluent obtained after separation of heavy and solid impurities, such as oligomers and pigments. The objective of the invention is indeed to obtain a diester stream, in particular a BHET stream, by depolymerizing a polyester filler comprising colored and / or opaque PET, with high purity and, in particular, being colorless or practically colorless. Summary of the invention

[0017] The invention therefore relates to a process for depolymerizing a polyester filler comprising opaque polyethylene terephthalate (PET), said process comprising: a) a conditioning step comprising a conditioning section fed at least by said polyester feed, to produce a conditioned stream; b) a glycolysis depolymerization step fed at least by the conditioned stream and by a diol supplement such that the molar quantity of diol is adjusted between 1 and 20 moles of diol per mole of diester of said polyester feed, operated at a temperature between 180 and 400°C, and a residence time between 0.1 and 10 h;(c) a diol separation step fed at least by the effluent from step (b), operated at a temperature between 100 and 250°C, at a pressure lower than that of step (b) and producing a diol effluent and a liquid monomer-rich effluent, said diol separation step being implemented in 1 to 5 successive gas-liquid separation sections, each producing a gas effluent and a liquid effluent, the liquid effluent from the earlier section feeding the later section, the liquid effluent from the last gas-liquid separation section constituting the liquid monomer-rich effluent, all the gas effluents being recovered to constitute the diol effluent;d) a step of separating the liquid monomer-rich effluent from step c) into a heavy impurity effluent and a pre-purified monomer effluent, operated at a temperature below 250°C and a pressure below 0.001 MPa with a liquid residence time of less than 10 min, and e) a step of decolorizing the pre-purified monomer effluent, comprising at least a mixing section of the pre-purified monomer effluent from step d) with a solvent such that the pre-purified monomer effluent represents between 20 and 90% by weight of the total weight of the mixture, and an adsorption section operated at a temperature between 100 and 200°C, and at a pressure between 0.1 and 1.0 MPa, in the presence of at least one adsorbent selected from activated carbons, aluminas and clays, to produce a purified monomer effluent.

[0018] An advantage of the present invention lies in obtaining, from a polyester feed comprising at least PET, in particular colored and / or opaque PET, a purified diester effluent, in particular a BHET stream, being in particular colorless, or even almost colorless.

[0019] One advantage of the invention is its ability to process all types of polyester waste, which increasingly contains pigments and dyes, such as colored, opaque, or even multi-layered PET. The process according to the invention, suitable for processing opaque PET, removes the pigments and dyes and returns the material to the diester monomer through a chemical reaction. This monomer can then be repolymerized into a polymer that is indistinguishable from virgin polyester, particularly virgin PET, thus enabling all the uses of virgin PET. Description methods of implementation

[0020] According to the invention, polyethylene terephthalate or poly(ethylene terephthalate), also simply called PET, has an elementary repeating formula motif:

[0021] Traditionally, PET is obtained by polycondensation of terephthalic acid (PTA), or dimethyl terephthalate (DMT), with ethylene glycol. In the following text, the expression "per mole of diester in said polyester filler" corresponds to the number of moles of the repeating unit -[O-CO-O-(C6H4)-CO-O-CH2-CH2]-, which is the diester repeating unit resulting from the reaction of PTA and ethylene glycol, in the PET contained in said polyester filler.

[0022] According to the invention, the term "monomer" or "diester monomer" advantageously designates bis(2-hydroxyethyl) terephthalate (BHET) of chemical formula HOC 2 H 4 -CO 2 -(C 6 H 4 )-CO 2 -C 2 H 4 OH, in which -(C 6 H 4 )- represents an aromatic ring, and which is the diester motif resulting from the reaction of PTA and ethylene glycol, in the PET included in said polyester filler.

[0023] The term "oligomer" typically refers to a small polymer, generally consisting of 2 to 20 repeating elementary units. According to the invention, the term "ester oligomer" or "BHET oligomer" refers to a terephthalate ester oligomer, comprising between 2 and 20, preferably between 2 and 5, repeating elementary units of formula -[O-CO-(C6H4)-CO-OC2H4]-, with -(C6H4)- an aromatic ring.

[0024] According to the invention, the terms "diol" and "glycol" are used interchangeably and refer to compounds comprising two hydroxyl groups (-OH). The preferred diol is ethylene glycol, also called monoethylene glycol or MEG.

[0025] Thus, the diol streams or diol effluents involved in the steps of the process of the invention preferably comprise ethylene glycol (or MEG) in a very large quantity, that is to say, such that MEG represents 95% by weight or more of the total weight of said diol stream or diol effluent.

[0026] The term "dye" defines a substance soluble in polyester material and used to color it. Dyes can be of natural or synthetic origin.

[0027] According to the invention, the term "pigment," more specifically coloring and / or opacifying pigment, defines a finely divided substance, insoluble in particular in polyester material. Pigments are in the form of solid particles, generally ranging in size from 0.1 to 10 µm, and predominantly between 0.4 and 0.8 µm. They are often mineral in nature. Pigments commonly used, particularly for opacification, are metal oxides such as TiO₂, CoAl₂O₄, Fe₂O₃, silicates, polysulfides, and carbon black.

[0028] According to the present invention, the expressions "between ... and ..." and "between ... and ..." mean that the limit values ​​of the interval are included within the described range of values. If this were not the case and the limit values ​​were not included within the described range, this clarification will be provided by the present invention.

[0029] In the following, specific and / or preferred embodiments of the invention may be described. They may be implemented separately or in combination without limitation of combination where technically feasible. Charge

[0030] The process according to the invention is fed with a polyester charge comprising at least one polyester, i.e. a polymer whose main chain repeating motif contains an ester function, and comprising polyethylene terephthalate (PET), preferably comprising at least opaque PET, and advantageously colored PET, and preferably opaque PET and colored PET.

[0031] The polyester filler in question is advantageously a recyclable polyester filler, sourced from waste collection and sorting channels, particularly for plastic waste. This polyester filler may originate, for example, from the collection of bottles, trays, films, resins, and / or fibers made of polyethylene terephthalate.

[0032] Advantageously, the polyester filling comprises at least 50% by weight, preferably at least 70% by weight, preferably at least 90% by weight of polyethylene terephthalate (PET).

[0033] Preferably, said polyester filler comprises at least one PET selected from opaque, dark or colored PET, multilayer PET and their mixtures. In particular, said polyester filler comprises at least 10% by weight of opaque PET, and most preferably at least 15% by weight of opaque PET, said opaque PET advantageously being recyclable opaque PET, i.e., sourced from collection and sorting channels.

[0034] The polyester filler advantageously comprises between 0.1% and 10% by weight of pigments, advantageously between 0.1% and 5% by weight. It also preferably comprises between 0.05% and 1% of colorants, in particular between 0.05% and 0.2% by weight.

[0035] In the collection and sorting channels, polyester waste is washed and shredded before forming the polyester feedstock of the process according to the invention.

[0036] The polyester filler may be, in whole or in part, in the form of flakes (or sequins), the longest of which is less than 10 cm, preferably between 5 and 25 mm, or in the form of a micronized solid, i.e., in the form of particles preferably between 10 microns and 1 mm in size. The filler may also include "macroscopic" impurities, preferably less than 5% by weight, preferably less than 3% by weight of "macroscopic" impurities, such as glass, metal, plastics other than polyester (e.g., PP, HDPE...), wood, cardboard, and mineral elements.The polyester filler may also be, in whole or in part, in the form of fibers, such as textile fibers, possibly pre-treated to remove cotton, polyamide, or any other non-polyester textile fibers, or tire fibers, possibly pre-treated to remove, in particular, polyamide fibers or rubber or polybutadiene residues. The polyester filler may also include polyester from production waste from the polymerization and / or processing of polyester material. The polyester filler may also include elements used as polymerization catalysts and stabilizing agents in PET production processes, such as antimony, titanium, and tin. Step a) of conditioning

[0037] The said process according to the invention includes a conditioning step a) which includes at least one conditioning section fed at least by said polyester charge, producing a conditioned flow.

[0038] The said conditioning section of step a) allows the said polyester charge to be heated and pressurized to the operating conditions of step b) of depolymerization.

[0039] In the conditioning section, the polyester filler is gradually heated to a temperature close to, or even slightly above, its melting point so as to become at least partially liquid. Advantageously, at least 70% by weight of the polyester filler, very advantageously at least 80% by weight, preferably at least 90% by weight, and preferably at least 95% by weight of the polyester filler is in liquid form at the end of the conditioning section (step a). The temperature at which the conditioning section of step a) is carried out is advantageously between 225 and 275°C. This temperature is kept as low as possible to minimize the thermal degradation of the polyester.

[0040] According to a preferred embodiment of the invention, said conditioning section is an extrusion section that corresponds to a screw conveyor section. In other words, the conditioning section is operated within an extruder.

[0041] The residence time in said extrusion section, defined as the volume of said section divided by the volumetric flow rate of the charge, is advantageously less than 15 min, preferably less than 10 min, and preferably less than 2 min. Advantageously, the extrusion section allows the polyester charge to be conditioned such that the conditioned flow is at a temperature between 150-300°C, preferably between 225 and 275°C, and at a pressure between atmospheric pressure (i.e., 0.1 MPa) and 20 MPa.

[0042] The extrusion section is advantageously connected to a vacuum extraction system to remove impurities such as dissolved gases, light organic compounds, and / or moisture present in the feed. The extrusion section may also advantageously include a filtration system to remove solid particles larger than 40 µm, preferably smaller than 2 cm, such as sand particles.

[0043] According to a possible embodiment of the invention, the conditioning section may comprise a conditioning zone, advantageously implemented at a temperature between 225 and 275°C, preferably in an extruder, and then a filler-diol contact phase in which the polyester filler is advantageously brought into contact with a diol stream, preferably with a fraction of the diol effluent from step c), preferably such that the number of moles of diol of said diol stream, preferably of said fraction of the diol effluent from step c), per mole of diester in said polyester filler is less than 1.0, preferably less than 0.5, and advantageously at least 0.05. This contacting has the effect of initiating the depolymerization reaction of the polyester filler, before introduction into the depolymerization step b).It also reduces the viscosity of the polyester filler, facilitating its transport, particularly to step b) of depolymerization. This optional filler-diol contact phase can be implemented in a static or dynamic mixer. When the conditioning zone is implemented in an extruder, the filler-diol contact phase can be carried out within the extruder; in this case, it is a reactive extrusion phase. Preferably, the diol stream, especially the fraction of diol effluent from step c), can advantageously be superheated prior to being fed into the filler-diol contact phase to facilitate the heating of the polyester filler.

[0044] The polyester feed can also advantageously be mixed, before or in the conditioning section, with at least a fraction of the heavy impurities effluent from step d), said fraction having preferably been purified beforehand.

[0045] The conditioned flow from the conditioning section is advantageously sent to step b) of depolymerization. Step b) of depolymerization

[0046] The process according to the invention comprises a glycolysis depolymerization step fed at least by the conditioned stream from step a), and by a diol supplement, carried out, in particular in the liquid phase, advantageously at a temperature between 180 and 400°C, preferably between 200 and 300°C, preferably between 210°C and 280°C, with a residence time in said step b) of between 0.1 and 10 h, preferably between 0.25 and 8 h, preferably between 0.5 and 6 h, and such that the total quantity of diol is adjusted between 1 and 20 moles, preferably between 3 and 15 moles, preferably between 5 and 10 moles of diol per mole of diester of said polyester filler (corresponding to a weight ratio of diol introduced relative to the weight of polyester filler of between 0.3 and 6.7, preferably between 1, 0 and 5.0, preferably between 1.7 and 3.3).

[0047] The operating pressure of said step b) is determined so as to maintain the reaction system in the liquid phase. This pressure is advantageously at least 0.1 MPa, preferably at least 0.4 MPa. By reaction system is meant all the components and phases present within said step b).

[0048] The residence time is defined as the ratio of the volume of liquid in said reaction section to the sum of the volumetric flow rate of the polyester feed and the diol make-up.

[0049] The diol is advantageously monoethylene glycol.

[0050] The depolymerization step (b) advantageously comprises one or more reaction sections, preferably at least two, and preferably between two and four, operating in series. Each reaction section can be implemented in any type of reactor known to those skilled in the art for carrying out a depolymerization or transesterification reaction, preferably in a reactor stirred by a mechanical stirring system and / or by a recirculation loop and / or by fluidization. The reactor may include a conical bottom for purging impurities.Preferably, said depolymerization step b) comprises at least two reaction sections, preferably between 2 and 4 reaction sections, operating in series, the reaction section(s) from the second reaction section being operated at the same or different temperature between them and lower than or equal to the temperature of the first reaction section, preferably lower, and preferably lower by 10 to 50°C, or even lower by 20 to 40°C, compared to the temperature of the first operating section.

[0051] The glycolysis reaction can be carried out in the presence or absence of a catalyst.

[0052] When the glycolysis reaction is carried out in the presence of a catalyst, the latter may be homogeneous or heterogeneous and chosen from among the esterification catalysts known to those skilled in the art, such as the oxide and salt complexes of antimony, tin, titanium, the alkoxides of metals from groups (I) and (IV) of the periodic table of elements, organic peroxides, and acid-base metal oxides.

[0053] A preferred heterogeneous catalyst advantageously comprises at least 50% by mass relative to the total mass of the catalyst, preferably at least 70% by mass, advantageously at least 80% by mass, most advantageously at least 90% by mass, and even more advantageously at least 95% by mass of a solid solution consisting of at least one spinel of formula ZxAl2O(3+x) in which x is between 0 (exclusive limit) and 1, and Z is selected from Co, Fe, Mg, Mn, Ti, Zn, and comprising at most 50% by mass of alumina and oxide of element Z. Said preferred heterogeneous catalyst advantageously contains at most 10% by mass of dopants selected from silicon, phosphorus, and boron taken alone or in mixtures.For example, and without limitation, said solid solution may consist of a mixture of ZnAl 2 O 4 spinel and CoAl 2 O 4 spinel, or may consist of a mixture of ZnAl 2 O 4 spinel, MgAl 2 O 4 spinel and FeAl 2 O 4 spinel, or may consist solely of ZnAl 2 O 4 spinel.

[0054] The particular embodiment in which the preferred heterogeneous catalyst is implemented has the advantage of exhibiting excellent conversion of PET to BHET by glycolysis. Furthermore, the heterogeneous catalyst in this particular embodiment has the remarkable property of capturing impurities, especially dyes, additives, and catalytic substances used for polymerization and present in the PET treated in the process according to the invention, such as antimony, magnesium, manganese, zinc, titanium, and phosphorus, thereby simplifying subsequent BHET purification steps for reuse in a polymerization process.

[0055] Preferably, the said depolymerization step is carried out without adding any external catalyst to the feed.

[0056] The depolymerization step can advantageously be carried out in the presence of a solid adsorbent in powder or molded form, the function of which is to capture at least some of the colored impurities, thus relieving the decolorization step (e). The solid adsorbent is advantageously activated carbon.

[0057] The glycolysis reaction converts the polyester feedstock into ester monomers and oligomers, advantageously PET into Bis(2-Hydroxyethyl) terephthalate (BHET) monomer and BHET oligomers. The conversion of the polyester feedstock in said depolymerization step is greater than 50%, preferably greater than 70%, and preferably greater than 85%. The molar yield of BHET is greater than 50%, preferably greater than 70%, and preferably greater than 85%. The molar yield of BHET corresponds to the molar flow rate of BHET exiting said step b) divided by the number of moles of diester in the polyester feedstock entering said step b).

[0058] An internal recirculation loop is advantageously implemented in step b), i.e. the withdrawal of a fraction of the reaction system, the filtration of this fraction, and the reinjection of said fraction into said step b). This internal loop makes it possible to eliminate any solid, "macroscopic" impurities possibly contained in the reaction liquid.

[0059] Advantageously, step b) of depolymerization makes it possible to obtain a reaction effluent which is sent to a step c) of diol separation. Step c) of diol separation

[0060] The process according to the invention includes a step c) of diol separation, fed at least by the effluent from step b), operated at a temperature between 100 and 250°C, at a pressure lower than that of step b) and producing a diol effluent and a liquid monomer-rich effluent.

[0061] The main function of step c) is to recover all or part of the unreacted diol.

[0062] Step c) is carried out at a lower pressure than in step b) so as to vaporize a fraction of the effluent from step b) into a gaseous effluent and a liquid effluent. This liquid effluent constitutes the liquid monomer-rich effluent. The gaseous effluent, consisting of more than 50% by weight of diol, preferably more than 70% by weight, and preferably more than 90% by weight, constitutes a diol effluent.

[0063] Step c) is advantageously implemented in one or more gas-liquid separation sections, advantageously in 2 to 5 successive separation sections, and most advantageously in 3 to 5 successive separation sections. Each gas-liquid separation section produces a liquid effluent and a gas effluent. The liquid effluent from the preceding section feeds the subsequent section. All the gas effluents are recovered to constitute the diol effluent. The liquid effluent from the last gas-liquid separation section constitutes the liquid monomer-rich effluent.

[0064] Advantageously, at least one of the gas-liquid separation sections can be implemented in a falling film evaporator or a scraped film evaporator or a short path distillation.

[0065] Step c) is carried out in such a way that the temperature of the liquid effluents is maintained above the value below which the polyester monomer precipitates, and below a high value, dependent on the diol / monomer molar ratio, above which the monomer re-polymerizes significantly. The temperature in step c) is between 100 and 250°C, preferably between 110 and 220°C, and preferably between 120 and 210°C. The operation, consisting of a series of gas-liquid separations, advantageously a series of 2 to 5, preferably 3 to 5 successive separations, is particularly advantageous because it allows the temperature of the liquid effluent to be adjusted in each separation to meet the aforementioned requirements.

[0066] The pressure in step c) is adjusted to allow the diol to evaporate at a temperature that minimizes re-polymerization and enables optimal energy integration. It is generally between 0.00001 and 0.2 MPa, preferably between 0.00004 and 0.15 MPa, and preferably between 0.00004 and 0.1 MPa.

[0067] The separating section(s) are advantageously agitated by any method known to a person skilled in the art.

[0068] The diol effluent may contain other compounds such as dyes, light alcohols, water, and diethylene glycol. At least a fraction of the diol effluent can advantageously be recycled, in liquid form (i.e., after condensation), to step a) and / or step b) and / or step e), possibly mixed with an external diol input to the process according to the invention.

[0069] All or part of the said diol effluent may be treated in a purification step prior to its recycling. This purification step may include, but is not limited to, adsorption onto a solid (for example, onto activated carbon) to remove dyes and one or more distillations to separate impurities such as diethylene glycol, water, and other alcohols. Step d) Monomer separation

[0070] The process according to the invention includes a step d) of separating the monomer-rich effluent from step c) into a heavy impurity effluent and a pre-purified monomer effluent.

[0071] Said step d) is advantageously carried out at a temperature below 250°C, preferably below 230°C, and most preferably below 200°C, and preferably above 110°C, and at a pressure below 0.001 MPa, preferably below 0.0005 MPa, preferably above 0.000001 MPa, with a liquid residence time of less than 10 min, preferably less than 5 min, preferably less than 1 min, and preferably greater than 0.1 second.

[0072] This separation step (d) aims to separate the monomer, particularly BHET, which is vaporized, from the oligomers, which are not fully converted and remain liquid. These oligomers therefore also capture heavy impurities, including pigments, from the unconverted polyester polymer, any other polymers present, and polymerization catalysts, while minimizing monomer loss through repolymerization. Some oligomers, especially small ones, may be carried along with the monomer. These heavy impurities are then collected with the oligomers in the heavy impurities effluent.

[0073] Due to the possible presence of polymerization catalysts in the polyester feedstock, the separation must be carried out with very short liquid residence times and at a temperature not exceeding 250°C, in order to limit any risk of monomer re-polymerization during this step. Therefore, separation by simple atmospheric distillation is not feasible.

[0074] Step d) of separation is advantageously implemented in a separation section comprising a falling film or scraped film evaporation system or a short path falling film or scraped film distillation system, in particular a short path falling film or scraped film distillation system.

[0075] A very low operating pressure is required to be able to carry out step d) at a temperature below 250°C, preferably below 230°C, while allowing vaporization of the monomer.

[0076] A polymerization inhibitor can advantageously be mixed with the liquid monomer-rich effluent before feeding said step d).

[0077] A fluxing agent can also be advantageously mixed with the liquid monomer-rich effluent before feeding into step d), so as to facilitate the removal of heavy impurities, particularly pigments, from the bottom of the evaporation or short-path distillation system. This fluxing agent must have a boiling point much higher than the monomer, especially BHET, under the operating conditions of step d). Examples include polyethylene glycol or PET oligomers.

[0078] The heavy impurities effluent includes, in particular, pigments, oligomers, and possibly unseparated BHET. This heavy impurities effluent is advantageously recycled, in whole or in part, to the conditioning step (a). The heavy impurities effluent may advantageously undergo at least one purification step, preferably a filtration step, prior to recycling, in order to reduce the quantity of pigments and / or other solid impurities. The portion of the heavy impurities effluent that is separated and has a high pigment content may advantageously be purged from the process and sent to an incineration system.

[0079] The said pre-purified monomer effluent from the separation section of step d) is advantageously sent to step e).

[0080] Optionally, the pre-purified monomer effluent from the separation section of step (d) may be sent to a gas-liquid separation section, operated in any equipment known to those skilled in the art, at a temperature between 100 and 250°C, preferably between 110 and 200°C, and preferably between 120 and 180°C, and at a pressure between 0.00001 and 0.1 MPa, preferably between 0.00001 and 0.01 MPa, and preferably between 0.00001 and 0.001 MPa. This optional gas-liquid separation section allows for the separation of a gaseous diol effluent from a liquid pre-purified monomer effluent. The said gas-liquid separation makes it possible to further reduce the quantity of diol remaining in the pre-purified monomer effluent, or even to eliminate the residual diol, by recovering in the said gaseous diol effluent more than 50% wt, preferably more than 70% wt, preferably more than 90% wt of the diol possibly carried along in step d) with the pre-purified monomer effluent.The amount of monomer carried over in said gaseous diol effluent is preferably less than 1 wt%, preferably less than 0.1 wt%, and more preferably less than 0.01 wt% of the amount of monomer present in the pre-purified monomer effluent. Said gaseous diol effluent is then advantageously condensed, optionally pre-treated in a purification step, and recycled with the diol effluent from step c) to step a) and / or step b) and / or mixed in step e). In the case where the process includes this gas-liquid separation section, it is the liquid pre-purified monomer effluent obtained at the end of said optional gas-liquid section that is sent to step e). Step e) of bleaching

[0081] The process according to the invention includes a step of decolorizing the pre-purified monomer effluent from step d), or optionally the liquid pre-purified monomer effluent, producing a purified monomer effluent.

[0082] This step (e) advantageously allows for the removal of residual colorants from the pre-purified monomer effluent, in particular colorants whose boiling point is lower than the cutting point, i.e., the temperature and pressure conditions used, notably, in step (d) of monomer separation. Indeed, these colorants, carried along with the pre-purified monomer effluent which they color, can thus be efficiently removed by adsorption in said step (e).

[0083] Advantageously, said step e) implements at least one mixing section of the pre-purified monomer effluent from step d), or optionally the liquid pre-purified monomer effluent, with a solvent, and an adsorption section.

[0084] The mixing section is fed with the pre-purified liquid monomer effluent from step d), or optionally the pre-purified liquid monomer effluent, and a solvent, preferably selected from diols, for example ethylene glycol. Preferably, the solvent comprises, or preferably consists of, a fraction of the diol effluent from step c), an external diol addition to the process according to the invention, or mixtures thereof. Most advantageously, the solvent is a fraction of the diol effluent from step c).

[0085] Preferably, the amount of solvent introduced into the mixing section is adjusted so that the pre-purified monomer effluent, or optionally the liquid pre-purified monomer effluent, represents between 20 and 90% by weight, preferably between 30 and 80% by weight, and preferably between 50 and 75% by weight, of the total weight of the mixture in said mixing section. Said mixing section is advantageously operated at a temperature between 100 and 250°C, preferably between 110 and 200°C, and preferably between 120 and 180°C, and at a pressure between 0.1 and 1.0 MPa, preferably between 0.1 and 0.8 MPa, and preferably between 0.2 and 0.5 MPa. The solvent may be heated, prior to said mixing section, preferably to the temperature at which the mixing section is operated, in particular to a temperature between 100 and 250°C, preferably between 110 and 200°C, and preferably between 120 and 180°C.

[0086] Preferably, the mixing section employs a static or dynamic mixer, preferably a static mixer. The residence time in the mixing section, defined as the total volume of liquid in said mixing section relative to the liquid mixing flow rate exiting said mixing section, is advantageously between 0.5 seconds and 20 minutes, preferably between 1 second and 5 minutes, preferably between 3 seconds and 1 minute.

[0087] The said mixture from the mixing section advantageously feeds the adsorption section. The adsorption section is operated in the presence of at least one adsorbent, and preferably up to five different adsorbents, at a temperature between 100 and 200°C, preferably between 100 and 170°C, and preferably between 120 and 150°C, and preferably at a pressure between 0.1 and 1.0 MPa, in particular between 0.1 and 0.8 MPa and more particularly between 0.2 and 0.5 MPa.

[0088] The adsorption section advantageously includes at least one adsorber. Most advantageously, the residence time of the mixture in each adsorber of the adsorption section is between 20 minutes and 40 hours, preferably between 1 and 30 hours, and preferably between 1 and 20 hours. The residence time is defined as the ratio of the internal volume of the adsorber to the volumetric flow rate of the mixture from the mixing section.

[0089] Preferably, the adsorption section is operated in the presence of one or two different adsorbents. According to the invention, adsorbents are said to be different when their nature is different and / or their composition and / or their particle size is different and / or their textural characteristics, such as pore volume. More preferably, the different adsorbents are of different natures.

[0090] When the adsorption section comprises two or more different adsorbents, these adsorbents are either mixed or placed in series within the section, preferably in series, and more preferably with each adsorbent in separate adsorbents (e.g., reactors or columns) placed in series. Combining several different adsorbents, particularly those of different types, can be advantageous to optimize the removal of residual dyes, which can also be of very different natures. Indeed, since the polyester feedstock for the process originates from polyester waste, such as PET packaging waste or plastic bottles, it can contain a very large number of colored and / or opaque PET particles and therefore a very large number of different coloring compounds.The colouring of the effluent from step d) may also come from a degradation or transformation of compounds constituting the feed during the conditioning steps a), polymerization b), diol separation c) and monomer separation d).

[0091] Advantageously, the adsorbent(s) is / are selected from among activated carbons, aluminas, and clays. The activated carbons that can be used are, for example, derived from petcoke, coal, or any other fossil source, or from biomass such as wood, coconut, or any other biomass source. Different raw materials can also be mixed to obtain activated carbons that can potentially be used as adsorbents in the adsorption section. The clays can be, for example, lamellar double hydroxides or natural or processed clays such as those known to humankind as bleaching earths. Preferably, at least one adsorbent is an activated carbon.Thus, when the adsorption section comprises a single type of adsorbent, said adsorbent is an activated carbon and, when the adsorption section comprises two or more different adsorbents, one adsorbent is an activated carbon and the other(s) is / are another activated carbon, an alumina or a clay, preferably an activated carbon or a clay, more particularly a clay.

[0092] The adsorption section is advantageously implemented in a flow-through fixed bed configuration, i.e., in at least one fixed-bed adsorbent unit, specifically at least one adsorbent column, which can operate in either upward or downward flow mode, preferably in upward flow mode, or in at least one continuous stirred tank reactor (CSTR). If the section is implemented in at least one CSTR, the reactor(s) is / are followed by a filtration system to recover the adsorbent(s) suspended in the treated liquid. Preferably, the adsorption section is implemented in a flow-through fixed bed configuration.

[0093] Preferably, each adsorbent in the adsorption section has a pore volume (Vp), determined by mercury porosimetry, greater than or equal to 0.25 ml / g, preferably greater than or equal to 0.40 ml / g, preferably greater than or equal to 0.50 ml / g, and preferably less than or equal to 5 ml / g.

[0094] If the adsorption section contains at least two different adsorbents, then the adsorbents can: either all be present in each column of said adsorption section, in mixture or in successive beds, or each be used in an adsorption subsection, the subsections being placed in series with respect to each other, each adsorption subsection being made up of several, preferably between 2 and 4, fixed bed adsorbent columns.

[0095] Advantageously, the adsorption section, or each of its subsections, comprises several fixed-bed adsorbent columns, in particular at least two columns, preferably between two and four columns of the same adsorbent, and especially two columns of the same adsorbent. When the adsorption section or subsection comprises two columns of the same adsorbent, one operating mode may be a "swing" mode, in which one column is in operation while the other is in reserve. When the adsorbent in the in-operation column is depleted, that column is isolated while the reserve column is brought online. The depleted adsorbent can then be regenerated in-situ and / or replaced with fresh adsorbent to be brought online again once the other column has been isolated.Another operating mode for adsorbent columns is to have at least two columns operating in series. When the adsorbent in the leading column (i.e., the first column in the series) is depleted, this first column is isolated, and the depleted adsorbent is either regenerated in-situ or replaced with fresh adsorbent. The column is then placed last in the column series, and so on. This operation is called "lead-lag," using the established English term. Preferably, the adsorption section is implemented in at least two columns of the same adsorbent, preferably in two to four columns of the same adsorbent, operating in a "lead-lag" configuration.

[0096] In a very particular embodiment of the invention in which the adsorption section comprises two different adsorbents, the adsorption section most preferably comprises a first subsection comprising at least two, preferably between 2 and 4, fixed-bed columns of activated carbon operating preferably in swing or lead-lag and a second subsection comprising at least two, preferably between 2 and 4, columns of another adsorbent, preferably chosen from another activated carbon or a clay, operating in swing or lead-lag and placed upstream or downstream of the first subsection of fixed-bed activated carbon columns.

[0097] Combining at least two columns of the same adsorbent helps to mitigate the potential for rapid clogging of the adsorbent, often due to the presence of dyes in the pre-treated monomer effluent. Having at least two adsorbent columns facilitates adsorbent replacement and / or regeneration, ideally without shutting down the bleaching unit or even the entire process. This reduces the risk of clogging, prevents unit downtime due to clogging, controls costs, and limits adsorbent consumption, while ensuring continuous production of purified diester monomers. Combining at least two columns of the same adsorbent, particularly those operating in a lead-lag configuration, also maximizes the adsorption capacity of the adsorbent.

[0098] Preferably, each adsorbent is in the form of granules, extrudates, or powder. Preferably, each adsorbent is in the form of granules or extrudates when the adsorption section is implemented in a flow-through fixed bed configuration, and it is in the form of powder when the adsorption section is implemented in a stirred-tube reactor (STRR) of the CSTR type. The size of said minimum adsorbent, particularly when in the form of granules or extrudates, is such that the smallest dimension of said minimum adsorbent (corresponding to the diameter of the circle circumscribed by the pattern of polylobular granules or extrudates, or to the diameter of the cylinder circumscribed by the cylindrical pattern of cylindrical extrudates; this dimension is also called the "diameter") is preferably between 0.1 and 5 mm, preferably between 0.3 and 2 mm.For example, 0.8 mm diameter activated carbon extrudates marketed by Cabot Norit or granules in the size range between 0.4 and 1.7 mm marketed by Chemviron may be suitable as an adsorbent in the adsorption section of step e) of decolorization.

[0099] Step e) of decolorization may also advantageously include a regeneration phase of said adsorbent(s).

[0100] The purified monomer effluent obtained at the end of step e) of the process of the invention is practically colorless or even colorless to the naked eye. Preferably, the purified monomer effluent is characterized by UV-visible spectrometry to identify the presence of absorption bands in the visible range, i.e., between 400 and 800 nm. Preferably, the purified monomer effluent is characterized according to this method, i.e., by UV-visible spectrometry, between 400 and 800 nm, at a temperature above the melting point of the characterized effluent, i.e., in a liquid medium, preferably between 120°C and 150°C, and with an optical path length of 5 mm. The purified monomer effluent obtained according to the invention exhibits a spectrum showing no significant absorption band (i.e., not distinguishable from background noise) in the visible wavelength range (i.e., between 400 and 800 nm).

[0101] The purified monomer effluent advantageously feeds a polymerization step known to those skilled in the art, producing PET indistinguishable from virgin PET, advantageously downstream of the supply of ethylene glycol, terephthalic acid, or dimethyl terephthalate, depending on the polymerization step selected. Feeding the purified monomer effluent into a polymerization step allows for a reduction in the dimethyl terephthalate or terephthalic acid supply by an equivalent flow rate.

[0102] The following examples illustrate the invention without limiting its scope. Examples

[0103] In the following example, the steps a) conditioning, b) depolymerization, c) diol separation and d) monomer separation are identical and described below.

[0104] A polyester filler, including in particular 20% by weight of opaque PET, is sourced from collection and sorting channels for processing.

[0105] 4 kg / h of flakes of said polyester filler, comprising 20 wt% opaque PET which itself contains 6.2 wt% TiO2 pigment, and 11.5 kg / h of ethylene glycol (MEG), are heated to a temperature of 250°C, injected into a first stirred reactor maintained at 250°C, then into a second and a third stirred reactor maintained at 220°C. The reactors are maintained at a pressure of 0.4 MPa. The residence time, defined as the ratio of the liquid volume in the reactor to the sum of the liquid volumetric flow rates entering the reactor, is set at 20 min in the first reactor and 2.1 h in the second and third reactors.At the outlet of the third reactor, the reaction effluent consists of 67.7% by weight of diol composed very predominantly of MEG (comprising 95% by weight of MEG or more), 25.8% by weight of diester monomer composed very predominantly of BHET (comprising 95% by weight of BHET or more), 0.32% by weight of TiO2, and 6.1% by weight of heavy compounds containing, among other things, dimers and / or oligomers of BHET.

[0106] The ethylene glycol present in the reaction effluent is separated by evaporation in a series of two flash flasks at temperatures ranging from 180°C to 120°C and pressures from 0.04 MPa to 0.004 MPa, and a scraped-film evaporator operated at 175°C and 0.0005 MPa. Following this evaporation step, a MEG-rich stream of 10.46 kg / h and a BHET-rich liquid stream of 5.02 kg / h are recovered. The MEG-rich stream consists primarily of ethylene glycol and can therefore be partially recycled to the depolymerization reactor and partially sent to the decolorization step if necessary, or to a purification step prior to the decolorization step. The BHET-rich liquid stream consists of 79.6% by weight of diester monomer, 0.6% by weight of MEG and 1.0% TiO2 pods and 18.8% by weight of heavy compounds containing, among other things, BHET dimers.

[0107] The BHET-rich liquid stream is then injected into a short-path evaporator, also known as short-path distillation, operated at a pressure of 20 Pa. Hot oil at 215°C evaporates the BHET, which is then condensed in the short-path evaporator at 130°C to produce a pre-purified BHET liquid stream. The residence time in the short-path evaporator is 1 minute. The pre-purified BHET liquid stream has a flow rate of 3.8 kg / h and is collected as the short-path evaporator distillate. It consists of 99% diester monomer by weight and is free of TiO₂. A heavy residue with a flow rate of 1.19 kg / h is recovered as residue from the short-path evaporator and consists of 16.7 wt% diester monomer, 79.2 wt% BHET oligomers and 4.1 wt% TiO2.

[0108] The gas effluent is condensed at 130°C to give a pre-purified BHET liquid stream. EXAMPLE 1 - COMPLIANT

[0109] The pre-purified BHET liquid stream, containing 99% BHET diester by weight, is compressed to 0.15 MPa and fed into a mixing section that also receives a fraction of the MEG stream from the vaporization step. The feed rate of this MEG fraction is adjusted so that the BHET liquid stream represents 50% by weight of the final mixture. This section is operated at 150°C and a pressure of 0.15 MPa.

[0110] The resulting mixture then feeds an adsorption section consisting of two columns, each filled with an adsorbent. The adsorption section is operated at 150°C and a pressure of 0.15 MPa. One column is placed under flow, while the other remains in reserve. The adsorbent used to fill both columns is activated carbon made of cylindrical extrudates 0.8 mm in diameter, reference ROY 0.8 from Cabot Norit.

[0111] The stay time is set at 3 hours.

[0112] The color of the effluent at the column outlet is monitored by in situ UV-visible spectrometry, using a Hellma Falcata series UV-visible probe with a 5 mm optical path length. The color is monitored between 400 and 800 nm, via the appearance of a significant absorption band in this wavelength range.

[0113] The appearance of a color change, identified by the appearance of an absorption band around 450 nm, is observed after 7 days. This time defines the column's operating time before transferring the flow to be treated to the reserve column.

[0114] The column containing the used adsorbent is either discharged or regenerated before being put back into operation on the flow once the reserve column is worn out.

Claims

1. Process for depolymerizing a polyester feedstock comprising opaque polyethylene terephthalate (PET), said process comprising: a) a conditioning step comprising a conditioning section supplied at least with said polyester feedstock, to produce a conditioned stream; b) a step of depolymerization by glycolysis, which is supplied at least with the conditioned stream and with a supplement of diol in a manner such that the molar amount of diol is adjusted to between 1 to 20 moles of diol per mole of diester in said polyester feedstock, conducted at a temperature of between 180 and 400°C and for a residence time of between 0.1 and 10 h; c) a diol separation step, which is supplied at least with the effluent from step b), and is conducted at a temperature of between 100 and 250°C, at a pressure less than that of step b), and which produces a diol effluent and a liquid effluent rich in monomers, where said diol separation step is implemented in 1 to 5 successive gas-liquid separation sections, each producing a gaseous effluent and a liquid effluent, where the liquid effluent from the preceding section supplies the subsequent section, the liquid effluent obtained from the last gas-liquid separation section forms the liquid effluent rich in monomers, and all the gaseous effluents are recovered to form the diol effluent; d) a step of separation of the effluent rich in liquid monomers obtained from step c) into a heavy impurities effluent and a prepurified monomers effluent, which is conducted at a temperature of less than 250°C and a pressure of less than 0.001 MPa with a liquid residence time of less than 10 min, and (e) a step of decolourizing of the prepurified monomers effluent, comprising at least a section for mixing the prepurified monomers effluent obtained in step d) with a solvent in a manner such that the prepurified monomers effluent represents between 20% and 90% by weight of the total weight of the mixture, and an adsorption section operated at a temperature of between 100 and 200°C and at a pressure of between 0.1 and 1.0 MPa in the presence of at least one adsorbent selected from activated carbons, aluminas and clays, to obtain a purified monomers effluent.

2. Process according to Claim 1, wherein said polyester feedstock comprises at least 50% by weight, preferably at least 70% by weight, more preferably at least 90% by weight of polyethylene terephthalate.

3. Process according to Claim 1 or 2, wherein said polyester feedstock comprises at least 10% by weight, preferably at least 15% by weight, of opaque PET.

4. Process according to any of the preceding claims, wherein said polyester feedstock comprises coloured PET.

5. Process according to any of the preceding claims, wherein said polyester feedstock comprises between 0.1% and 10% by weight of pigments, preferably between 0.1% and 5% by weight of pigments.

6. Process according to any of the preceding claims, wherein said polyester feedstock comprises between 0.05% and 1% of dyes, in particular between 0.05% and 0.2% by weight of dyes.

7. Process according to any of the preceding claims, wherein the solvent in decolourizing step e) comprises a fraction of the diol effluent obtained from step c), a supplement of diol external to the process according to the invention, or mixtures thereof.

8. Process according to any of the preceding claims, wherein the prepurified monomers effluent represents between 30% and 80% by weight, preferably between 50% and 75% by weight, of the total weight of the mixture in step e).

9. Process according to any of the preceding claims, wherein at least one adsorbent in step e) is an activated carbon.

10. Process according to any of the preceding claims, wherein the adsorption section in step e) is operated in the presence of an adsorbent or two different adsorbents.

11. Process according to any of the preceding claims, wherein the adsorption section comprises two or more different adsorbents, said different adsorbents being in a mixture or placed in series in said adsorption section.

12. Process according to the preceding claim, wherein each of said different adsorbents are in different reactors placed in series.

13. Process according to any of the preceding claims, wherein the adsorption section of step e) is implemented in fixed bed adsorption mode.

14. Process according to any of the preceding claims, wherein the adsorption section of step e) is operated at a temperature of between 100 and 170°C, preferably between 120°C and 150°C.