High strength glass-ceramics having petalite and lithium silicate structures

HK40137277APending Publication Date: 2026-09-11CORNING INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
HK42026125514
Authority / Receiving Office
HK · HK
Patent Type
Applications
Current Assignee / Owner
Priority Date
2015-08-14
Filing Date
2026-06-30
Publication Date
2026-09-11

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Glass and glass ceramic compositions having a combination of a lithium silicate crystalline phase and a petalite crystalline phase, and methods of making the glass and glass ceramic compositions, are described. The compositions are compatible with conventional rolling and float processes, are transparent or translucent, and have high mechanical strength and fracture resistance. In addition, the composition can be chemically tempered into even higher strength glass ceramics, which can be used as large substrates in a variety of applications.
Need to check novelty before this filing date? Find Prior Art

Description

(19) State Intellectual Property Office (12) Invention Patent Application (10) Application Publication Number (43) Application Publication Date (21) Application Number 202511495772.1 (22) Application Date 2015.10.08 (30) Priority Data 62 / 061,385 2014.10.08 US 62 / 205,120 2015.08.14 US (62) Divisional Application Data 201580065414.5 2015.10.08 (71) Applicant Corning Incorporated Address New York, USA (72) Inventors G.H. Bill, F.C., C.M. Smith (74) Patent Agency King & Wood Mallesons, Beijing 11256 Patent Attorneys Tai Hong, Mao Yunbei (51) Int.Cl. C03C 10 / 04 (2006.01) C03C 10 / 12 (2006.01) C03C 3 / 097 (2006.01) (54) Invention Title: High-Strength Glass-Ceramics with Lithium Feldspar and Lithium Silicate Structures (57) Abstract: This paper describes glass and glass-ceramic compositions having a combination of lithium silicate and lithium feldspar crystalline phases, and methods for preparing the glass and glass-ceramic compositions. The compositions are compatible with conventional rolling and float processes, are transparent or translucent, and have high mechanical strength and fracture resistance. Furthermore, the compositions can be chemically tempered into glass-ceramics with even higher strength, which can be used as large substrates in a variety of applications. Claims (4 pages), Description (31 pages), Drawings (15 pages), CN 121318156 A 2026.01.13 CN 1 21 31 81 56 A 1. A glass-ceramic article comprising, by weight percentage: 55 wt% to 80 wt% SiO2; 2 wt% to 20 wt% Al2O3; 5 wt% to 20 wt% Li2O; 0 wt% to 10 wt% B2O3; 0 wt% to 5 wt% Na2O; 0 wt% to 10 wt% ZnO; 0.5 wt% to 6 wt% P2O5; and 0.2 wt% to 15 wt% ZrO2, wherein the sum of P2O5 and ZrO2 is greater than or equal to 3 wt%. 2. The glass-ceramic article of claim 1, comprising: 65 wt% to 75 wt% SiO2; 2 wt% to 8 wt% Al2O3; 10 wt% to 16 wt% Li2O; >0 wt% to 1 wt% R2O, wherein R is Na and K; 0 wt% to 1 wt% B2O3; 3 wt% to 5 wt% P2O5; and 4 wt% to 12 wt% ZrO2, wherein the sum of P2O5 and ZrO2 is greater than or equal to 5 wt%. 3. The glass-ceramic article of claim 2, comprising: 65 wt% to 73 wt% SiO2;2 wt% to 5 wt% Al2O3; and 12 wt% to 16 wt% Li2O, wherein the sum of P2O5 and ZrO2 is greater than or equal to 7 wt%. 4. The glass-ceramic article of claim 2, comprising: 69 wt% to 75 wt% SiO2; 6 wt% to 8 wt% Al2O3; 10 wt% to 12 wt% Li2O; and 4 wt% to 8 wt% ZrO2. 5. The glass-ceramic article of claim 1, comprising: 0 wt% to 4 wt% K2O; 0 wt% to 8 wt% MgO; 0 wt% to 5 wt% TiO2; 0 wt% to 0.4 wt% CeO2; and 0.05 wt% to 0.5 wt% SnO2. 6. The glass-ceramic article according to any one of claims 1-5, wherein the glass-ceramic article is transparent, has a thickness of 0.8 mm to 6 mm, and has a transmittance of at least 85% for light in the wavelength range of 400 nm to 1,000 nm. 7. The glass-ceramic article according to any one of claims 1-5, wherein the glass-ceramic article is chemically strengthened and contains a surface compressive stress of 300 MPa or greater. 8. The glass-ceramic article according to claim 7, comprising a thickness of 200 micrometers to 5 mm, a central tension of at least 10 MPa, and an ion-exchange layer depth of 30 micrometers or greater. 9. The glass-ceramic article according to any one of claims 1-5, wherein the glass-ceramic article has a fracture toughness of 1 MPa·m1 / 2 or greater. 10. The glass-ceramic article according to any one of claims 1-5, wherein the glass-ceramic article has a Vickers hardness of 600 kgf / mm2 or greater. 11. The glass-ceramic article according to any one of claims 1-5, wherein the glass-ceramic article has a ring-strand strength of at least 300 MPa. 12. The glass-ceramic article according to any one of claims 1-5, comprising grains having a longest dimension of 100 nm or less. 13. The glass-ceramic article according to any one of claims 1-5, comprising grains having an aspect ratio of 2 or greater, wherein the glass-ceramic article is transparent. 14. The glass-ceramic article according to any one of claims 1-5, comprising 20 wt% to 60 wt% of a lithium silicate crystalline phase. 15. The glass-ceramic article according to claim 14, wherein the lithium silicate crystalline phase is the dominant crystalline phase, and the glass-ceramic article has one or more minor phases comprising one or more of β-spodumene solid solution, β-quartz solid solution, lithium phosphate, cristobalite, or rutile.16. The glass-ceramic article according to any one of claims 1-5, wherein the lepidolite phase comprises 20% to 70% by weight of the glass-ceramic article. 17. The glass-ceramic article according to claim 14, wherein the lepidolite phase is the dominant phase, and the glass-ceramic article has one or more minor phases, the minor phases comprising one or more of β-spodumene solid solution, β-quartz solid solution, lithium phosphate, cristobalite, or rutile. 18. The glass-ceramic article according to claim 14, wherein the lepidolite phase comprises 20% to 70% by weight of the glass-ceramic article, and the lithium silicate phase comprises 20% to 60% by weight of the glass-ceramic article. 19. A precursor glass composition comprising, by weight percentage: 55 wt% to 80 wt% SiO2; 2 wt% to 20 wt% Al2O3; 5 wt% to 20 wt% Li2O; 0 wt% to 10 wt% B2O3; 0 wt% to 5 wt% Na2O; 0 wt% to 10 wt% ZnO; 0.5 wt% to 6 wt% P2O5; and 0.2 wt% to 15 wt% ZrO2, wherein the sum of P2O5 and ZrO2 is greater than or equal to 3 wt%. 20. The precursor glass composition of claim 19, comprising: 65 wt% to 75 wt% SiO2; 2 wt% to 8 wt% Al2O3; 10 wt% to 16 wt% Li2O; >0 wt% to 1 wt% R2O, wherein R is Na and K; 0 wt% to 1 wt% B2O3; 3 wt% to 5 wt% P2O5; and 4 wt% to 12 wt% ZrO2, wherein the sum of P2O5 and ZrO2 is greater than or equal to 5 wt%. 21. The precursor glass composition of claim 20, comprising: 65 wt% to 73 wt% SiO2; 2 wt% to 5 wt% Al2O3; and 12 wt% to 16 wt% Li2O, wherein the sum of P2O5 and ZrO2 is greater than or equal to 7 wt%. 22. The precursor glass composition of claim 20, comprising: 69 wt% to 75 wt% SiO2; 6 wt% to 8 wt% Al2O3; 10 wt% to 12 wt% Li2O; and 4 wt% to 8 wt% ZrO2. 23. The precursor glass composition of claim 19, comprising: 0 wt% to 4 wt% K2O; 0 wt% to 8 wt% MgO; 0 wt% to 5 wt% TiO2; 0 wt% to 0.4 wt% CeO2; and 0.05 wt% to 0.5 wt% SnO2.24. The glass-ceramic article according to any one of claims 19-23, wherein the glass-ceramic article has a fracture toughness of 1 MPa·m1 / 2 or greater. 25. A method of manufacturing a glass-ceramic, comprising: heat-treating a precursor glass by the following steps: (i) heating the glass to a pre-nucleation temperature at a rate of 1 to 10 °C / min; (ii) holding the glass at the pre-nucleation temperature for 1 / 4 hour to 4 hours; (iii) heating the glass to a nucleation temperature at a rate of 1 to 10 °C / min; (iv) holding the glass at the nucleation temperature for 1 / 4 hour to 4 hours; (v) heating the glass to a crystallization temperature at a rate of 1 °C / min to 10 °C / min; and (vi) holding the glass at the crystallization temperature for 1 / 4 hour to 4 hours, thereby forming the glass-ceramic. 26. The method according to claim 25, further comprising cooling the glass-ceramic to room temperature. 27. The method of claim 26, wherein the crystallization temperature is in the range of 630°C to 730°C. 28. The method of claim 27, wherein the pre-nucleation temperature is 540°C. 29. The method of any one of claims 25-28, wherein the precursor glass comprises a composition, by weight percentage, comprising: 55 wt% to 80 wt% SiO2; 2 wt% to 20 wt% Al2O3; 5 wt% to 20 wt% Li2O; 0 wt% to 10 wt% B2O3; 0 wt% to 5 wt% Na2O; 0 wt% to 10 wt% ZnO; 0.5 wt% to 6 wt% P2O5; and 0.2 wt% to 15 wt% ZrO2, wherein the sum of P2O5 and ZrO2 is greater than or equal to 3 wt%. 30. The method of claim 29, wherein the composition comprises: 65 wt% to 75 wt% SiO2; 2 wt% to 8 wt% Al2O3; 10 wt% to 16 wt% Li2O; >0 wt% to 1 wt% R2O, wherein R is Na and K; 0 wt% to 1 wt% B2O3; 3 wt% to 5 wt% P2O5; and 4 wt% to 12 wt% ZrO2, wherein the sum of P2O5 and ZrO2 is greater than or equal to 5 wt%. 31. The method of claim 30, wherein the composition comprises: 65 wt% to 73 wt% SiO2; 2 wt% to 5 wt% Al2O3; and 12 wt% to 16 wt% Li2O, wherein the sum of P2O5 and ZrO2 is greater than or equal to 7 wt%.32. The method according to claim 30, wherein the composition comprises: 69% to 75% by weight of SiO2; 6% to 8% by weight of Al2O3; 10% to 12% by weight of Li2O; and 4% to 8% by weight of ZrO2. Claims 4 / 4 Page 5 CN 121318156 A High-strength glass-ceramics having a lithium feldspar and lithium silicate structure

[0001] This patent application is a divisional application of the international application PCT / US2015 / 054615, filed on October 8, 2015, entering the Chinese national phase with application number 201580065414.5, entitled "High-strength glass-ceramics having a lithium feldspar and lithium silicate structure" with application number 201910849140.9.

[0002] Cross-Reference to Related Applications

[0003] This application claims priority to U.S. Provisional Application Serial No. 62 / 061,385, filed October 8, 2014, and U.S. Provisional Application Serial No. 62 / 205,120, filed August 14, 2015, the contents of which are incorporated herein by reference in their entirety. Technical Field

[0004] Embodiments relate to glass and glass-ceramic compositions, and more particularly, to high-strength glass-ceramic compositions having a combination of a lithium feldspar phase and a lithium silicate phase. Background Art

[0005] Lithium pyrosilicate glass-ceramics in the SiO2-Li2O-K2O-ZnO-P2O5-Al2O3-ZrO2 system have been developed and marketed for use as dental crowns, dental bridges, and dental overlays. Their interlocking, flattened crystalline microstructure provides high mechanical strength and fracture toughness as well as excellent chemical durability. Compositions in this field were invented by Corning, Inc. and are protected by patent in US 5,219,799 (“'799 Patent”) by Beall et al.

[0006] Furthermore, known glass-based materials often exhibit inherent brittleness or low resistance to crack propagation. For example, the inherently low fracture toughness (e.g., 0.5–1.0 MPa•m1 / 2 for oxide glasses and glass ceramics) makes oxide glasses more sensitive to the presence of small defects and imperfections. By comparison, commercially available monocrystalline substrates exhibit fracture toughness values ​​of about 2.4–about 4.5 MPa•m1 / 2. Chemical strengthening, for example, through ion exchange processes, can provide some resistance to crack penetration at the surface of the glass or glass ceramic by applying a compressive stress layer at a certain depth (e.g., 50–100 micrometers) from the surface in the glass or glass ceramic; however, the resistance to crack penetration can be limited, and once the crack propagates through the compressive stress layer into the glass or glass ceramic…The bulk of the glass or glass-ceramic is no longer effective. While reinforcement provides some resistance to crack penetration, the inherent properties (k1c) of the material are unaffected by ion exchange. Improving the mechanical properties of glass-based materials, particularly in terms of damage resistance and fracture toughness, is a continuing focus of attention. Therefore, there is a need in the art to provide materials with improved damage resistance and fracture toughness.

[0007] It is known that ion-exchangeable lithium-containing aluminosilicate glass-ceramic articles in the β-spodumene family provide damage resistance and fracture toughness. However, β-spodumene-based glass-ceramics are typically opaque, which limits their use in display-related applications or other applications requiring transparency or translucency. Therefore, there is a need in the art for transparent or translucent glass-ceramic materials with rapid ion exchange capability and high fracture toughness.

[0008] The first aspect comprises a glass-ceramic article having a lithium feldspar crystalline phase and a lithium silicate crystalline phase, wherein the lithium feldspar crystalline phase and the lithium silicate crystalline phase have a higher weight percentage than other crystalline phases present in the glass-ceramic article. In some embodiments, the lithium feldspar crystalline phase accounts for 20-70% by weight of the glass-ceramic article, and the lithium silicate crystalline phase accounts for 20-60% by weight of the glass-ceramic article. In some embodiments, the lithium feldspar crystalline phase accounts for 45-70% by weight of the glass-ceramic article, and the lithium silicate crystalline phase accounts for 20-50% by weight of the glass-ceramic article. In some embodiments, the lithium feldspar crystalline phase accounts for 40-60% by weight of the glass-ceramic article, and the lithium silicate crystalline phase accounts for 20-50% by weight of the glass-ceramic article.

[0009] In some embodiments, the glass-ceramic article is transparent. In some embodiments, the glass-ceramic article has a transmittance of at least 85% for light in the wavelength range of 400 nm to 1,000 nm. In some embodiments, the glass-ceramic article has a transmittance of at least 90% for light in the wavelength range of 400 nm to 1,000 nm. In some embodiments, the glass-ceramic article is transparent. In some embodiments, the glass-ceramic article comprises grains having a longest dimension of 500 nm or less or 100 nm or less.

[0010] In some embodiments, the glass-ceramic has the following composition by weight percent: SiO2: 55-80%; Al2O3: 2-20%; Li2O: 5-20%; B2O3: 0-10%; Na2O: 0-5%; ZnO: 0-10%; P2O5: 0.5-6%; and ZrO2: 0.2-15%.

[0011] In some embodiments, the glass-ceramic article, by weight percent, has a composition that also includes the following optional additional components: K2O:0-4%; MgO: 0-8%; TiO2: 0-5%; CeO2: 0-0.4% and SnO2: 0.05-0.5%.

[0012] In some embodiments, the glass-ceramic article has the following composition by weight %: SiO2: 69-80%; Al2O3: 6-9%; Li2O: 10-14%; B2O3: 0-2%; P2O5: 1.5-2.5%; and ZrO2: 2-4%.

[0013] In some embodiments, the glass-ceramic article has the following composition by weight percent: SiO2: 69-80%; Al2O3: 6-9%; Li2O: 10-14%; Na2O: 1-2%; K2O: 1-2%; B2O3: 0-12%; P2O5: 1.5-2.5%; and ZrO2: 2-4%.

[0014] In some embodiments, the glass-ceramic article has the following composition by weight percent: SiO2: 65-80%; Al2O3: 5-16%; Li2O: 8-15%; Na2O: 0-3%; K2O: 0-3%; B2O3: 0-6%; ZnO: 0-2%; P2O5: 0.5-4%; and ZrO2: 0.2-6%.

[0015] In some embodiments, the glass-ceramic article has the following composition by weight percent: SiO2: 60-80%; Al2O3: 5-20%; Li2O: 5-20%; Na2O: 0-3%; K2O: 0-3%; B2O3: 0-6%; ZnO: 0-4%; P2O5: 0.5-4%; and ZrO2: 0.2-8%.

[0016] In some embodiments, the sum of the weight percentages of P2O5 and ZrO2 in the glass-ceramic composition is greater than 3.

[0017] In some embodiments, the glass-ceramic article has one or more of the following: a fracture toughness of 1 MPa•m1 / 2 or greater, a Vickers hardness of about 600 kgf / mm2 or greater, or a ring-on-ring strength of at least 300 MPa. In some embodiments, the glass-ceramic article has a compressive stress layer formed by ion exchange, having a layer depth (DOL) of at least about 30 micrometers. In some embodiments, the ion-exchanged glass-ceramic article is not brittle.

[0018] A second aspect includes a method of forming a glass-ceramic article, the method comprising forming a glass composition, by weight percent, the glass composition comprising: SiO2: 55-80%; Al2O3:2-20%; Li2O: 5-20%; B2O3: 0-10%; Na2O: 0-5%; ZnO: 0-10%; P2O5: 0.5-6%; and ZrO2: 0.2-15%; and page 3 / 31 of the specification, CN 121318156 A, to ceramicize the glass composition to form a glass-ceramic article having a lithium feldspar crystalline phase and a lithium silicate crystalline phase, wherein the lithium feldspar crystalline phase and the lithium silicate crystalline phase have a higher weight percentage than other crystalline phases present in the glass-ceramic article.

[0019] In some embodiments, the method further includes forming a glass composition comprising, by weight percent: K2O: 0-4%; MgO: 0-8%; TiO2: 0-5%; CeO2: 0-0.4% and SnO2: 0.05-0.5%.

[0020] In some embodiments, the method further includes forming a glass composition comprising, by weight percent: SiO2: 69-80%; Al2O3: 6-9%; Li2O: 10-14%; B2O3: 0-2%; P2O5: 1.5-2.5%; and ZrO2: 2-4%.

[0021] In some embodiments, the method further includes forming a glass composition comprising, by weight percent: SiO2: 69-80%; Al2O3: 6-9%; Li2O: 10-14%; Na2O: 1-2%; K2O: 1-2%; B2O3: 0-12%; P2O5: 1.5-2.5%; and ZrO2: 2-4%.

[0022] In some embodiments, the method further includes forming a glass composition comprising, by weight percent: SiO2: 65-80%; Al2O3: 5-16%; Li2O: 8-15%; Na2O: 0-3%; K2O: 0-3%; B2O3: 0-6%; ZnO: 0-2%; P2O5: 0.5-4%; and ZrO2: 0.2-6%. Specification 4 / 31 page 9 CN 121318156 A

[0023] In some embodiments, the method further includes forming a glass composition comprising, by weight percent: SiO2: 60-80%; Al2O3: 5-20%; Li2O: 5-20%; Na2O: 0-3%; K2O: 0-3%; B2O3: 0-6%; ZnO: 0-4%; P2O5: 0.5-4%; and ZrO2: 0.2-8%.

[0024] In some embodiments, the sum of the weight percentages of P2O5 and ZrO2 in the glass composition is greater than 3.

[0025] In some embodiments, the method further includes ion-exchanging the glass-ceramic article to form a compressive stress layer having a layer depth of at least 30 micrometers. In some embodiments, the ion-exchanged glass-ceramic article is not brittle.

[0026] In some embodiments, ceramization includes the following sequential steps: heating the glass composition to a glass pre-nucleation temperature; holding the glass pre-nucleation temperature for a predetermined time; heating the composition to a nucleation temperature; holding the nucleation temperature for a predetermined time; heating the composition to a crystallization temperature; and holding the crystallization temperature for a predetermined time.

[0027] In some embodiments, ceramization includes the following sequential steps: heating the composition to a nucleation temperature; holding the nucleation temperature for a predetermined time; heating the composition to a crystallization temperature; and holding the crystallization temperature for a predetermined time.

[0028] In some embodiments, the method forms a glass-ceramic article wherein the lithium feldspar crystal phase accounts for 20-70% by weight of the glass-ceramic article, and the lithium silicate crystal phase accounts for 20-60% by weight of the glass-ceramic article.

[0029] The above and other aspects, advantages, and salient features of the invention will become apparent from the following detailed description, the accompanying drawings, and the appended claims. Brief Description of the Drawings

[0030] FIG1 is a graph of differential scanning calorimetry (DSC) traces for an exemplary glass-ceramic composition.

[0031] FIG2 is a graph of transmittance for an exemplary glass-ceramic composition with wavelengths from 400 nm to 1,000 nm at a sample thickness of 1 mm.

[0032] FIG3A is a scanning electron microscope (SEM) image of an exemplary glass-ceramic composition on a 200 nm scale.

[0033] FIG3B is a scanning electron microscope (SEM) image of an exemplary glass-ceramic composition on a 100 nm scale.

[0034] FIG4 shows the results of a ring-over-ring (RoR) test and an abraded ring-over-ring (aRoR) test for an exemplary non-ion-exchanged glass-ceramic composition.

[0035] FIG5 shows a graph of Na2O concentration, in molar percentage, as a function of sample thickness for an exemplary glass-ceramic composition.

[0036] Figure 6 shows the RoR test results of the exemplary glass-ceramic composition before and after ion exchange.

[0037] Figure 7 shows the aRoR test results of the exemplary glass-ceramic composition after ion exchange.

[0038] Figure 8 shows the RoR test results of the exemplary glass-ceramic composition after ion exchange for different durations.

[0039] Figure 9 shows the aRoR test results of the exemplary glass-ceramic composition after ion exchange and wear under different pressures.

[0040] The optical photograph in Figure 10 shows ion-exchanged glass-ceramic sheets with different fracture patterns.

[0041] Figure 11 is a graph of the differential scanning calorimetry (DSC) traces for the exemplary glass-ceramic composition.

[0042] Figure 12 shows the X-ray diffraction (XRD) pattern of the crystalline phase of the exemplary glass-ceramic composition.

[0043] Figure 13 shows the ring-on-ring (RoR) test results for the exemplary glass-ceramic composition.

[0044] Figure 14 shows a graph of the Na₂O concentration, by weight percentage, as a function of sample thickness for the exemplary glass-ceramic composition.

[0045] Detailed Description

[0046] In the following detailed description, numerous specific details are set forth in order to provide a thorough understanding of the embodiments described herein. However, it will be apparent to those skilled in the art that embodiments may be practiced without some or all of these specific details. In other instances, well-known features or processes have not been described in detail so as not to obscure the invention. Furthermore, similar or identical drawing numbers may be used to identify common or similar parts. Moreover, unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. In case of conflict, this specification (including the definitions herein) shall prevail.

[0047] Although other methods and materials may be used in the implementation or testing of embodiments of the invention, some suitable methods and materials are described below.

[0048] Materials, compounds, compositions, and components that can be used in the disclosed methods and compositions, in combination with the disclosed methods and / or compositions, in the preparation of the disclosed methods and compositions, or in embodiments of the disclosed methods and compositions are disclosed. These and other materials are disclosed herein, and it should be understood that each of them is specifically contemplated and described herein when specific references to combinations, subsets, interactions, groups, etc., of these materials are disclosed without explicitly disclosing specific references to each different individual and group combination and arrangement of these compounds.

[0049] Thus, each can be contemplated individually and collectively if examples of embodiments A-D, which disclose a class of substitutes A, B, and C and also disclose examples of a class of substitutes D, E, and F and combinations thereof, are disclosed. Therefore, in this example, each of the following combinations A-E, A-F, B-D, B-E, B-F, C-D, C-E, and C-F is specifically conceived, and these should be considered as being revealed from the content of A, B, and / or C; D, E, and / or F; and the instance combination A-D. Similarly, any subsets of the above or combinations of such subsets are also specifically conceived and revealed. Thus, for example, subgroups of A-E, B-F, and C-E are specifically conceived, and they should be considered as being revealed from the content of A, B, and / or C; D, E, and / or F; and the instance combination A-D. This concept applies to all aspects of this content, including but not limited to…This is not limited to any component of the composition or any step in the disclosed methods of preparing and using the composition. Specifically, the exemplary composition ranges given herein are to be considered part of the specification, and it is further considered that providing exemplary numerical range endpoints is equivalent in all respects to their inclusion in the text, and all combinations are specifically contemplated and disclosed. Furthermore, if multiple additional steps are possible, it should be understood that each of these additional steps can be performed by any particular embodiment or combination of embodiments of the disclosed method, and each such combination is specifically contemplated and should be considered as disclosed.

[0050] Unless otherwise indicated in specific circumstances, the numerical ranges listed herein include upper and lower limits and are intended to include the endpoints of the range, all integers and fractions within which the range is defined. The scope of the invention is not limited to the specific values ​​listed when defining the range. Furthermore, when a quantity, concentration, or other value or parameter is expressed as a range, one or more preferred ranges, or a preferred upper limit and a preferred lower limit, it should be understood that this is equivalent to specifically disclosing any range by combining any pair of upper or preferred values ​​with any pair of lower or preferred values, as specified in CN 121318156 A on page 6 / 31 of the specification, regardless of whether such pairing is specifically disclosed. Finally, when the term “about” is used to describe the value or endpoint of a range, it should be understood that the invention includes the specific value or endpoint referenced.

[0051] As used herein, the term “about” means that a quantity, size, formulation, parameter, or other quantity or feature is not and need not be precise, but may be approximate and / or larger or lower if necessary, reflecting tolerances, conversion factors, rounding off, measurement errors, etc. Generally, whether explicitly stated or not, a quantity, size, formulation, parameter, or other quantity or feature is “about” or “approximate”.

[0052] As used herein, the term “or” is inclusive; specifically, the phrase “A or B” means “A, B, or A and B”. In this document, for example, an exclusive “or” is specified by terms such as “either A or B” and “one of A or B”.

[0053] Elements and components of this disclosure are described using the indefinite articles “a” or “an”. The use of these articles indicates the presence of one or at least one of these elements or components. Although these articles are generally used to indicate that the noun being modified is singular, the articles “a” or “an” as used herein also include plural nouns unless otherwise stated. Similarly, the definite article “the” as used herein also indicates that the noun being modified may be singular or plural, unless otherwise stated.

[0054] For the purpose of describing embodiments of the invention, it should be noted that one variable referred to herein is a parameter.The term "function" of a number or another variable is not intended to mean that the variable is merely a function of the listed parameters or variables. Rather, the use of "function" of a variable as a function of the listed parameters is open-ended, meaning that the variable can be a single parameter or a function of multiple parameters.

[0055] It should be noted that words such as "preferred," "common," and "usually" as used herein are not intended to limit the scope of the invention, nor do they indicate that certain features are important, critical, or even essential to the structure or function of the embodiments described herein. Rather, these terms are used merely to indicate specific aspects of embodiments of the invention, or to emphasize alternative or additional features that may or may not be used in a particular embodiment of the invention.

[0056] It should be noted that one or more claims in the claims use the term "characterized by" as a transitional phrase. For the purpose of limiting the invention, it should be noted that the use of this term as an open-ended transitional phrase in the claims to introduce a description of a series of structural features should be interpreted similarly to the more commonly used open-ended introductory phrase "comprising."

[0057] As a result of the raw materials and / or equipment used in the production of glass compositions, certain impurities or components that are not intentionally added may be present in the final glass composition. This material is present in small amounts in glass or glass-ceramic compositions and is referred to herein as “indeterminate material”.

[0058] As used herein, a glass or glass-ceramic composition comprising 0% by weight of a compound is defined as not having intentionally added to the composition, but the composition may still contain the compound, typically in an indeterminate amount or trace amounts. Similarly, “iron-free,” “sodium-free,” “lithium-free,” “zirconium-free,” “alkaline earth metal-free,” “heavy metal-free,” etc., are defined as not having intentionally added to the composition, but the composition may still contain iron, sodium, lithium, zirconium, alkaline earth metals, or heavy metals, but in close to an indeterminate amount or trace amounts.

[0059] Unless otherwise stated, the concentrations of all components referenced herein are expressed as weight percentages (wt%).

[0060] As described above, it is desirable to obtain transparent or translucent lithium-containing aluminum silicate glass-ceramic compositions having lithium feldspar and lithium silicate as the main crystalline phases. The lithium silicate crystalline phase may be lithium pyrosilicate or lithium metasilicate. The improved properties of the glass and glass-ceramic compositions described herein (page 7 / 31, CN 121318156 A) include: 1) the glass retains a low melting temperature (below 1500°C) but provides a higher liquidus viscosity (>2000 poise) and a long operating range compatible with conventional rolling, molding, and float processes; 2) lithium silicate is retained as the dominant crystalline phase, providing the glass-ceramic with inherently high mechanical strength and fracture toughness; and 3) lithium feldspar is the second dominant crystalline phase.It also has a fine grain size, which contributes to the transparency or translucency of the glass-ceramic, and can also be ion-exchanged for additional mechanical strength. In addition, the material can be ceramicized into shapes with very little deformation, is easy to process into precise shapes, cut, drill, chamfer, tapped, polished to high gloss using conventional ceramic processing tools, and even exhibits different degrees of translucency based on composition and heat treatment. These properties make glass-ceramics suitable for many applications, such as worktops and other surfaces, handheld, desktop and wall-mounted consumer electronics device covers, appliance doors and exteriors, floor tiles, wall panels, ceiling tiles, whiteboards, material storage containers (plates) such as beverage bottles, food sales and storage containers, and mechanical parts requiring lightweight, good wear resistance and precise dimensions. Because of the lower viscosity of glass-ceramics, various methods can be used to form glass-ceramics in three-dimensional articles.

[0061] Lithium feldspar LiAlSi4O10 is a monoclinic crystal with a three-dimensional framework structure comprising a layered structure with folded Si2O5 layers connected by Li and Al tetrahedra. Li is coordinated with oxygen tetrahedra. The mineral petalite is a lithium source and is used as a low-thermal-expansion phase to improve the thermal shock resistance of glass-ceramics or ceramic parts. Furthermore, glass-ceramic products based on the petalite phase can be chemically strengthened in a salt bath, where Na+ (and / or K+) replace Li+ in the petalite structure, resulting in surface compression and strengthening. In some embodiments, the weight percentage of the lithopone crystalline phase in the glass-ceramic composition may be about 20-about 70 wt%, about 20-about 65 wt%, about 20-about 60 wt%, about 20-about 55 wt%, about 20-about 50 wt%, about 20-about 45 wt%, about 20-about 40 wt%, about 20-about 35 wt%, about 20-about 30 wt%, about 20-about 25 wt%, about 25-about 70 wt%, about 25-about 65 wt%, about 25-about 60 wt%, about 25-about 55 wt%, about 25-about 50 wt%, about 25-about 45 wt%, about 25-about 40 wt%. Approximately 25–35% by weight, approximately 25–30% by weight, approximately 30–70% by weight, approximately 30–65% by weight, approximately 30–60% by weight, approximately 30–55% by weight, approximately 30–45% by weight, approximately 30–40% by weight, approximately 30–35% by weight, approximately 35–70% by weight, approximately 35–65% by weight, approximately 35–60% by weight, approximately 35–55% by weight, approximately 35–50% by weight, approximately 35–45% by weight, approximately 35–40% by weight% by weight, approximately 40–70% by weight, approximately 40–65% by weight, approximately 40–60% by weight, approximately 40–55% by weight, approximately 40–50% by weight, approximately 40–45% by weight, approximately 45–70% by weight, approximately 45–65% by weight, approximately 45–60% by weight, approximately 45–55% by weight, approximately 45–50% by weight, approximately 50–70% by weight, approximately 50–65% by weight, approximately 50–60% by weight, approximately 50–55% by weight, approximately 55–70% by weight, approximately 55–65% by weight, approximately 55–60% by weight, approximately 60% by weight - Approximately 70% by weight, approximately 60-65% by weight, or approximately 65-70% by weight. In some embodiments, the glass-ceramic has about 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, or 70% by weight of a lithium feldspar crystal phase.

[0062] As described above, the lithium silicate crystal phase can be lithium pyrosilicate or lithium metasilicate. Lithium pyrosilicate Li2Si2O5 is an orthorhombic crystal based on a corrugated sheet of {Si2O5} tetrahedral array. The crystal shape is typically flat or plate-like and has distinct dissociation surfaces. Due to the microstructure of the randomly oriented interlocking crystals—a crystal structure that forces cracks to propagate through the material via a twisted path around these crystals—lithium pyrosilicate-based glass-ceramics provide highly desirable mechanical properties, including high bulk strength and fracture toughness. Lithium metasilicate Li2SiO3 has orthorhombic symmetry, and the (Si2O6) chains are parallel to the c-axis and linked together by lithium ions. In dilute hydrofluoric acid, lithium metasilicate crystals can be readily dissolved from glass-ceramics. In some embodiments, the weight percentage of the lithium silicate crystalline phase in the glass-ceramic composition may be about 20-about 60% by weight, about 20-about 55% by weight, about 20-about 50% by weight, about 20-about 45% by weight, about 20-about 40% by weight, about 20-about 35% by weight, about 20-about 30% by weight, about 20-about 25% by weight, about 25-about 60% by weight, or about 25-about 55% by weight.% by weight, approximately 25–50% by weight, approximately 25–45% by weight, approximately 25–40% by weight, approximately 25–35% by weight, approximately 25–30% by weight, approximately 30–60% by weight, approximately 30–55% by weight, approximately 30–45% by weight, approximately 30–40% by weight, approximately 30–35% by weight, approximately 35–60% by weight, approximately 35–55% by weight, approximately 35–50% by weight, approximately 35–45% by weight, approximately 35–40% by weight, approximately 40–60% by weight, approximately 40–55% by weight, approximately 40 - Approximately 50% by weight, approximately 40-approximately 45% by weight, approximately 45-approximately 60% by weight, approximately 45-approximately 55% by weight, approximately 45-approximately 50% by weight, approximately 50-approximately 60% by weight, approximately 50-approximately 55% by weight, or approximately 55-approximately 60% by weight. In some embodiments, the glass-ceramic has 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, or 60 wt% lithium silicate crystalline phase.

[0063] There are two main families of lithium pyrosilicate glass-ceramics. The first group includes those doped with cerium dioxide and noble metals such as silver. These can be nucleated by UV light and subsequently heat-treated to prepare high-strength glass-ceramics, such as Fotoceram®. The second family of lithium pyrosilicate glass-ceramics is nucleated by the addition of P2O5, where the nucleating phase is Li3PO4. P2O5-nucleated lithium pyrosilicate glass-ceramics have been developed for various applications, such as high-temperature sealing materials, computer hard drive disks, transparent armor, and dental applications.

[0064] The glasses and glass-ceramics described herein can be broadly described as lithium-containing aluminosilicate glasses or glass-ceramics containing SiO2, Al2O3, and Li2O. In addition to SiO2, Al2O3, and Li2O, the glasses and glass-ceramics described herein may also contain basic salts such as Na2O, K2O, Rb2O, or Cs2O, as well as P2O5, ZrO2, and a variety of other components as described below. In one or more embodiments, depending on the composition of the precursor glass, the primary crystalline phases include pyrite and lithium silicate, but β-spodumene (SS), β-quartz (SS), and lithium phosphate may also be present as secondary crystalline phases.Scaflopous quartz and rutile. In some embodiments, the glass-ceramic composition has the following residual glass content: about 5 to about 30 wt%, about 5 to about 25 wt%, about 5 to about 20 wt%, about 5 to about 15 wt%, about 5 to about 10 wt%, about 10 to about 30 wt%, about 10 to about 25 wt%, about 10 to about 20 wt%, about 10 to about 15 wt%, about 15 to about 30 wt%, about 15 to about 25 wt%, about 15 to about 20 wt%, about 20 to about 30 wt%, about 20 to about 25 wt%, or about 25 to about 30 wt%. In some embodiments, the residual glass content may be 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by weight.

[0065] SiO2 is an oxide involved in glass forming and can be used to stabilize glass and glass-ceramic network structures. In some embodiments, the glass or glass-ceramic composition contains about 55 to about 80% by weight of SiO2. In some embodiments, the glass or glass-ceramic composition contains 69 to about 80% by weight of SiO2. In some embodiments, the glass or glass-ceramic composition may contain about 55-about 80% by weight, about 55-about 77% by weight, about 55-about 75% by weight, about 55-about 73% by weight, 60-about 80% by weight, about 60-about 77% by weight, about 60-about 75% by weight, about 60-about 73% by weight, 65-about 80% by weight, about 65-about 77% by weight, about 65-about 75% by weight, about 65-about 73% by weight, 69-about 80% by weight, about 69-about 77% by weight, about 69-about 75% by weight, about 69-about 73% by weight, about 70-about 80% by weight, about 70-about 77% by weight. About 70-about 75% by weight, about 70-about 73% by weight, about 73-about 80% by weight, about 73-about 77% by weight, about 73-about 75% by weight, about 75-about 80% by weight, about 75-about 77% by weight, or about 77-about 80% by weight, SiO2. In some embodiments, the glass or glass-ceramic composition contains about 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68,69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, or 80, wt% SiO2.

[0066] Regarding viscosity and mechanical properties, viscosity and mechanical properties are affected by the glass composition. In glasses and glass-ceramics, SiO2 is used as the main glass-forming oxide for precursor glasses and can be used to stabilize the network structure of glasses and glass-ceramics. When the precursor glass is heat-treated to convert to glass-ceramics, the concentration of SiO2 should be high enough to form the lithium feldspar crystalline phase. The amount of SiO2 can be limited to control the melting temperature (200 poise temperature) because the melting temperature of pure SiO2 or high-SiO2 glasses is undesirably high.

[0067] Al2O3 can also stabilize the network and provides improved mechanical properties and chemical durability. However, if the amount of Al2O3 is too high, it can reduce the fraction of lithium silicate, possibly to the point where interlocking structures cannot be formed. The viscosity can be controlled by adjusting the amount of Al2O3. Furthermore, excessively high amounts of Al2O3 generally increase the viscosity of the melt. In some embodiments, the glass or glass-ceramic composition may contain about 2 to about 20 wt% Al2O3. In some embodiments, the glass or glass-ceramic composition may contain about 6 to about 9 wt% Al2O3. In some embodiments, the glass or glass-ceramic composition may contain about 2-about 20%, about 2-about 18% by weight, about 2-about 15% by weight, about 2-about 12% by weight, about 2-about 10% by weight, about 2-about 9% by weight, about 2-about 8% by weight, about 2-about 5% by weight, about 5-about 20%, about 5-about 18% by weight, about 5-about 15% by weight, about 5-about 12% by weight, about 5-about 10% by weight, about 5-about 9% by weight, about 5-about 8% by weight, about 6-about 20%, about 6-about 18% by weight, about 6-about 15% by weight, about 6-about 12% by weight, about 6-about 10% by weight, about 6-about 9% by weight. wt%, about 8-about 20%, about 8-about 18 wt%, about 8-about 15 wt%, about 8-about 12 wt%, about 8-about 10 wt%, about 10-about 20%, about 10-about 18 wt%, about 10-about 15 wt%, about 10-about 12 wt%, about 12-about 20%, about 12-about 18 wt%, or about 12-about 15 wt%, Al2O3. In some embodiments, the glass or glass-ceramic composition may contain about 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 wt% Al2O3.

[0068] In the glasses and glass-ceramics described herein, Li₂O contributes to the formation of the lithium feldspar and lithium silicate crystalline phases. In fact, to achieve lithium feldspar and lithium silicate as the dominant crystalline phases, it is ideal to have at least about 7 wt% Li₂O in the composition. Furthermore, it has been found that once the Li₂O content becomes too high – greater than about 15 wt% – the composition becomes very fluid. In some embodiments of the composition, the glass or glass-ceramic may contain about 5 wt% to about 20 wt% Li₂O. In other embodiments, the glass or glass-ceramic may contain about 10 wt% to about 14 wt% Li₂O. In some embodiments, the glass or glass-ceramic composition may contain about 5-about 20% by weight, about 5-about 18% by weight, about 5-about 16% by weight, about 5-about 14% by weight, about 5-about 12% by weight, about 5-about 10% by weight, about 5-about 8% by weight, 7-about 20% by weight, about 7-about 18% by weight, about 7-about 16% by weight, about 7-about 14% by weight, about 7-about 12% by weight, about 7-about 10% by weight, 10-about 20% by weight, about 10-about 18% by weight, about 10-about 16% by weight, about 10-about 14% by weight, about 10-about 12% by weight, and 12-about 20% by weight. About 12-about 18 wt%, about 12-about 16 wt%, about 12-about 14 wt%, 14-about 20 wt%, about 14-about 18 wt%, about 14-about 16 wt%, about 16-about 20 wt%, about 16-about 18 wt%, or about 18-about 20 wt% Li2O. In some embodiments, the glass or glass-ceramic composition may contain about 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 wt% Li2O.

[0069] As mentioned above, Li2O is generally used to form the glass-ceramic of the embodiment, but other basic oxides tend to reduce the formation of glass-ceramics and form aluminosilicate residual glass in the glass-ceramic. Greater than about 5% by weight of Na₂O or K₂O, or combinations thereof, has been found to result in undesirable amounts of residual glass, which can lead to deformation during crystallization and unfavorable microstructures from a mechanical property perspective. The composition of the residual glass can be adjusted to control the viscosity during crystallization, minimize deformation or undesirable thermal expansion, or control microstructural properties. Therefore, the compositions described herein generally have low amounts of non-lithium alkaline oxides. In some embodiments, the glass or glass-ceramic composition may contain about 0% by weight of Na₂O or K₂O, or combinations thereof.- About 5% by weight of R₂O, wherein R is one or more basic cations Na and K. In some embodiments, the glass or glass-ceramic composition may contain about 1 to about 3% by weight of R₂O, wherein R is one or more basic cations Na and K. In some embodiments, the glass or glass-ceramic composition may contain 0 to about 5 wt%, 0 to 4 wt%, 0 to 3 wt%, 0 to about 2 wt%, 0 to about 1 wt%, >0 to about 5 wt%, >0 to about 4 wt%, >0 to about 3 wt%, >0 to about 2 wt%, >0 to about 1 wt%, about 1 to about 5 wt%, about 1 to about 4 wt%, about 1 to about 3 wt%, about 1 to about 2 wt%, about 2 to about 5 wt%, about 2 to about 4 wt%, about 2 to about 3 wt%, about 3 to about 5 wt%, about 3 to about 4 wt%, or about 4 to about 5 wt% Na₂O or K₂O, or combinations thereof. In some embodiments, the glass or glass-ceramic composition may contain about 0, >0, 1, 2, 3, 4, or 5 wt% R2O.

[0070] The glass and glass-ceramic composition may include P2O5. P2O5 can be used as a nucleating agent to form bulk nucleation. If the P2O5 concentration is too low, the precursor glass does not crystallize, but only forms a weak and often deformable bulk at higher temperatures (because of lower viscosity) and from the surface inward; however, if the P2O5 concentration is too high, devitrification is difficult to control during cooling in the precursor glass formation process. Embodiments may contain >0 to about 6 wt% P2O5. Other embodiments may contain about 2 to about 4 wt% P2O5. Still other embodiments may contain about 1.5 to about 2.5 wt% P2O5. The implemented composition may contain 0-about 6 wt%, 0-about 5.5 wt%, 0-about 5 wt%, 0-about 4.5 wt%, 0-about 4 wt%, 0-about 3.5 wt%, 0-about 3 wt%, 0-about 2.5 wt%, 0-about 2 wt%, 0-about 1.5 wt%, 0-about 1 wt%, >0-about 6 wt%, >0-about 5.5 wt%, >0-about 5 wt%, >0-about 4.5 wt%, >0-about 4 wt%, >0-about 3.5 wt%, >0-about 3 wt%, >0-about 2.5 wt%, >0-about 2 wt%, >0-about 1.5 wt%, >0 - Approximately 1% by weight, approximately 0.5% - Approximately 6% by weight, approximately 0.5% - Approximately 5.5% by weight, approximately 0.5% - Approximately 5% by weight, approximately 0.5% - Approximately 4.5% by weight, approximately 0.5% - Approximately 4% by weight, approximately 0.5% - Approximately 3% by weight0.5% by weight, about 0.5-3% by weight, about 0.5-2.5% by weight, about 0.5-2% by weight, about 0.5-1.5% by weight, about 0.5-1% by weight, about 1-6% by weight, about 1-5.5% by weight, about 1-5% by weight, about 1-4.5% by weight, about 1-4% by weight, about 1-3.5% by weight, about 1-3% by weight, about 1-2.5% by weight, about 1-2% by weight, about 1-1.5% by weight, about 1.5-6% by weight, about 1.5-5.5% by weight, about 1.5-5% by weight. Approximately 1.5–4.5 wt%, approximately 1.5–4 wt%, approximately 1.5–3.5 wt%, approximately 1.5–3 wt%, approximately 1.5–2.5 wt%, approximately 1.5–2 wt%, approximately 2–6 wt%, approximately 2–5.5 wt%, approximately 2–5 wt%, approximately 2–4.5 wt%, approximately 2–4 wt%, approximately 2–3.5 wt%, approximately 2–3 wt%, approximately 2–2.5 wt%, approximately 2.5–6 wt%, approximately 2.5–5.5 wt%, approximately 2.5–5 wt%, approximately 2.5–4.5 wt%. Approximately 2.5–4 wt%, approximately 2.5–3.5 wt%, approximately 2.5–3 wt%, approximately 3–6 wt%, approximately 3–5.5 wt%, approximately 3–5 wt%, approximately 3–4.5 wt%, approximately 3–4 wt%, approximately 3–3.5 wt%, approximately 3.5–6 wt%, approximately 3.5–5.5 wt%, approximately 3.5–5 wt%, approximately 3.5–4.5 wt%, approximately 3.5–4 wt%, approximately 4–6 wt%, approximately 4–5.5 wt%, approximately 4–4.5 wt%, approximately 4.5–6 wt%. About 4.5 to about 5.5% by weight, about 4.5 to about 5% by weight, about 5 to about 6% by weight, about 5 to about 5.5% by weight, or about 5.5 to about 6% by weight of P2O5. In some embodiments, the glass or glass-ceramic composition may contain about 0, >0, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, or 6% by weight of P2O5.

[0071] In the glasses and glass-ceramics described herein, ZrO2 is generally found to improve the stability of Li2O-Al2O3-SiO2-P2O5 glasses by significantly reducing glass devitrification and lowering the liquidus temperature during formation. At concentrations of 8% by weight or higher, ZrSiO4 can form the dominant liquidus phase at high temperatures, significantly reducing the liquidus viscosity. When the glass contains more than 2% by weight of ZrO2, a transparent glass can be formed. The addition of ZrO2 can also help reduce the grain size of transparent lithium feldspar, which facilitates the formation of transparent glass-ceramics. In some embodiments, the glass or glass-ceramic composition may contain about 0.2% to about 15% by weight of ZrO2. In some embodiments, the glass or glass-ceramic composition may contain about 2% to about 4% by weight of ZrO2. In some embodiments, the glass or glass-ceramic composition may contain about 0.2-about 15% by weight, about 0.2-about 12% by weight, about 0.2-about 10% by weight, about 0.2-about 8% by weight, about 0.2-6% by weight, about 0.2-about 4% by weight, 0.5-about 15% by weight, about 0.5-about 12% by weight, about 0.5-about 10% by weight, about 0.5-about 8% by weight, about 0.5-6% by weight, about 0.5-about 4% by weight, 1-about 15% by weight, about 1-about 12% by weight, about 1-about 10% by weight, about 1-about 8% by weight, about 1-6% by weight, about 1-about 4% by weight, 2 - Approximately 15% by weight, approximately 2% - Approximately 12% by weight, approximately 2% - Approximately 10% by weight, approximately 2% - Approximately 8% by weight, approximately 2% - 6% by weight, approximately 2% - Approximately 4% by weight, approximately 3% - Approximately 15% by weight, approximately 3% - Approximately 12% by weight, approximately 3% - Approximately 10% by weight, approximately 3% - Approximately 8% by weight, approximately 3% - 6% by weight, approximately 3% - Approximately 4% by weight, approximately 4% - Approximately 15% by weight, approximately 4% - Approximately 12% by weight, approximately 4% - Approximately 10% by weight, approximately 10% - Approximately 15% by weight, approximately 10% - Approximately 10 ... - About 12% by weight, or about 12 to about 15% by weight ZrO2. In some embodiments, the glass or glass-ceramic composition may contain about 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15% by weight ZrO2.

[0072] B2O3 helps to provide a precursor glass with a low melting temperature. Furthermore, the addition of B2O3 to the precursor glass therefore...Glass-ceramics facilitate the attainment of interlocked crystalline microstructures and improve the damage resistance of glass-ceramics. When boron in the residual glass is not balanced by the charge of basic oxides or divalent cation oxides, it will be in a trigonal-coordinated state (or triple-coordinated boron), which opens the glass structure. The network around these triple-coordinated borons is not as rigid as that of tetrahedral (or tetrahedral) coordinated boron. While not intended to be theoretically deficient, precursor glasses and glass-ceramics containing triple-coordinated boron are believed to tolerate a certain degree of deformation before crack formation. By tolerating some deformation, the Vickers indentation crack initiation value is increased. The fracture toughness of precursor glasses and glass-ceramics containing triple-coordinated boron is also increased. While not intended to be theoretically deficient, the presence of boron in the residual glass (and precursor glass) of glass-ceramics is believed to reduce the viscosity of the residual glass (or precursor glass), which promotes the growth of lithium silicate crystals, especially large crystals with high aspect ratios. It is believed that a larger amount of triple-coordinated boron (as opposed to quadruple-coordinated boron) results in glass-ceramics exhibiting greater Vickers indentation crack initiation load. In some embodiments, the amount of triple-coordinated boron (based on the percentage of total B2O3) can be about 40% or more, 50% or more, 75% or more, about 85% or more, or even about 95% or more. Generally, the amount of boron should be controlled to maintain the chemical durability and mechanical strength of the ceramicized bulk glass-ceramic.

[0073] In one or more embodiments, the glass and glass-ceramics described herein may contain 0 to about 10 wt% or 0 to about 2 wt% B2O3. In some embodiments, the glass or glass-ceramic composition may contain 0-about 10 wt%, 0-about 9 wt%, 0-about 8 wt%, 0-about 7 wt%, 0-about 6 wt%, 0-about 5 wt%, 0-about 4 wt%, 0-about 3 wt%, 0-about 2 wt%, 0-about 1 wt%, >0-about 10 wt%, >0-about 9 wt%, >0-about 8 wt%, >0-about 7 wt%, >0-about 6 wt%, >0-about 5 wt%, >0-about 4 wt%, >0-about 3 wt%, >0-about 2 wt%, >0-about 1 wt%, about 1-about 10 wt%, about 1-about 8 wt%, about 1-about 6 wt%, and so on. % by weight, about 1-5% by weight, about 1-4% by weight, 12 / 31 pages, CN 121318156 A, about 1-2% by weight, about 2-10% by weight, about 2-8% by weight, about 2-6% by weight, about 2-4% by weight, about 3-10% by weight, about 3-8% by weight, about 3-6% by weight, about 3-4% by weight.About 4 to about 5 wt%, about 5 wt% to about 8 wt%, about 5 wt% to about 7.5 wt%, about 5 wt% to about 6 wt%, or about 5 wt% to about 5.5 wt% B2O3. In some embodiments, the glass or glass-ceramic composition may contain about 0, >0, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 wt% B2O3.

[0074] MgO may be incorporated into the penelopeite crystals in the form of a partial solid solution. In one or more embodiments, the glass and glass-ceramic described herein may contain 0 to about 8 wt% MgO. In some embodiments, the glass or glass-ceramic composition may contain 0-about 8 wt%, 0-about 7 wt%, 0-about 6 wt%, 0-about 5 wt%, 0-about 4 wt%, 0-about 3 wt%, 0-about 2 wt%, 0-about 1 wt%, about 1-about 8 wt%, about 1-about 7 wt%, about 1-about 6 wt%, about 1-about 5 wt%, about 1-about 4 wt%, about 1-about 3 wt%, about 1-about 2 wt%, about 2-about 8 wt%, about 2-about 7 wt%, about 2-about 6 wt%, about 2-about 5 wt%, about 2-about 4 wt%, about 2-about 3 wt%, about 3-about 8 wt%. About 3 to about 7 wt%, about 3 to about 6 wt%, about 3 to about 5 wt%, about 3 to about 4 wt%, about 4 to about 8 wt%, about 4 to about 7 wt%, about 4 to about 6 wt%, about 4 to about 5 wt%, about 5 to about 8 wt%, about 5 to about 7 wt%, about 5 to about 6 wt%, about 6 to about 8 wt%, about 6 to about 7 wt%, or about 7 wt% to about 8 wt% MgO. In some embodiments, the glass or glass-ceramic composition may contain about 0, >0, 1, 2, 3, 4, 5, 6, 7, or 8 wt% MgO.

[0075] ZnO may be incorporated into the lepidolite crystals in the form of a partial solid solution. In one or more embodiments, the glass and glass-ceramic described herein may contain 0 to about 10 wt% ZnO. In some embodiments, the glass or glass-ceramic composition may contain 0 to about 10 wt%, 0 to about 9 wt%, 0 to about 8 wt%, 0 to about 7 wt%, 0 to about 6 wt%, 0 to about 5 wt%, 0 to about 4 wt%, 0 to about 3 wt%, 0 to about 2 wt%, 0 to about 1 wt%, about 1 to about 10 wt%, about 1 to about 9 wt%, about 1 to about 8 wt%, about 1 to about 7 wt%.% by weight, approximately 1-6% by weight, approximately 1-5% by weight, approximately 1-4% by weight, approximately 1-3% by weight, approximately 1-2% by weight, approximately 2-10% by weight, approximately 2-9% by weight, approximately 2-8% by weight, approximately 2-7% by weight, approximately 2-6% by weight, approximately 2-5% by weight, approximately 2-4% by weight, approximately 2-3% by weight, approximately 3-10% by weight, approximately 3-9% by weight, approximately 3-8% by weight, approximately 3-7% by weight, approximately 3-6% by weight, approximately 3-5% by weight, approximately 3-4% by weight, approximately 4-10% by weight, approximately 4% by weight - Approximately 9% by weight, approximately 4% - Approximately 8% by weight, approximately 4% - Approximately 7% by weight, approximately 4% - Approximately 6% by weight, approximately 4% - Approximately 5% by weight, approximately 5% - Approximately 10% by weight, approximately 5% - Approximately 9% by weight, approximately 5% - Approximately 8% by weight, approximately 5% - Approximately 7% by weight, approximately 5% - Approximately 6% by weight, approximately 6% - Approximately 10% by weight, approximately 6% - Approximately 9% by weight, approximately 6% - Approximately 8% by weight, approximately 6% - Approximately 7% by weight, approximately 7% - Approximately 10% by weight, approximately 7% - Approximately 9% by weight, approximately 7% - Approximately 8% by weight, approximately 8% - Approximately 10% by weight, approximately 8% - Approximately 9% by weight, or approximately 9% - Approximately 10% by weight ZnO. In some embodiments, the glass or glass-ceramic composition may contain about 0, >0, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 wt% ZnO.

[0076] In one or more embodiments, the glass and glass-ceramic described herein may contain 0 to about 5 wt% TiO2. In some embodiments, the glass or glass-ceramic composition may contain 0 to about 5 wt%, 0 to about 4 wt%, 0 to about 3 wt%, 0 to about 2 wt%, 0 to about 1 wt%, about 1 to about 5 wt%, about 1 to about 4 wt%, about 1 to about 3 wt%, about 1 to about 2 wt%, about 2 to about 5 wt%, about 2 to about 4 wt%, about 2 to about 3 wt%, about 3 to about 5 wt%, about 3 to about 4 wt%, or about 4 to about 5 wt% TiO2. In some embodiments, the glass or glass-ceramic composition may contain about 0, >0, 1, 2, 3, 4, or 5 wt% TiO2. Specification page 13 / 31 18 CN 121318156 A

[0077] In one or more embodiments, the glass and glass-ceramic described herein may contain 0 to about 0.4% by weight CeO2. In some embodiments,The glass or glass-ceramic composition may contain 0 to about 0.4 wt%, 0 to about 0.3 wt%, 0 to about 0.2 wt%, 0 to about 0.1 wt%, about 0.1 to about 0.4 wt%, about 1 to about 0.3 wt%, about 1 to about 0.2 wt%, about 0.2 to about 0.4 wt%, about 0.2 to about 0.3 wt%, or about 0.3 to about 0.4 wt% CeO2. In some embodiments, the glass or glass-ceramic composition may contain about 0, >0, 0.1, 0.2, 0.3, or 0.4 wt% CeO2.

[0078] In one or more embodiments, the glass and glass-ceramic described herein may contain 0 to about 0.5 wt% SnO2. In some embodiments, the glass or glass-ceramic composition may contain 0 to about 0.5% by weight, 0 to about 0.4% by weight, 0 to about 0.3% by weight, 0 to about 0.2% by weight, 0 to about 0.1% by weight, about 0.05 to about 0.5% by weight, 0.05 to about 0.4% by weight, 0.05 to about 0.3% by weight, 0.05 to about 0.2% by weight, 0.05 to about 0.1% by weight, about 0.1 to about 0.5% by weight, about 0.1 to about 0.4% by weight, about 0.1 to about 0.3% by weight, about 0.1 to about 0.2% by weight, about 0.2 to about 0.5% by weight, about 0.2 to about 0.4% by weight, about 0.2% by weight, and about 0.2% by weight. - About 0.3 wt%, about 0.3 to about 0.5 wt%, about 0.3 to about 0.4 wt%, or about 0.4 to about 0.5 wt% SnO2. In some embodiments, the glass or glass-ceramic composition may contain about 0, >0, 0.05, 0.1, 0.2, 0.3, 0.4, or 0.5 wt% SnO2.

[0079] In some embodiments, the sum of the weight percentages of P2O5 and ZrO2 in the glass and glass-ceramic described herein may be greater than or equal to about 3 wt%, 4 wt%, or 5 wt%, thereby increasing nucleation. Increased nucleation can lead to the formation of finer grains.

[0080] In some embodiments, the glass-ceramic exhibits transparency in the visible light range (i.e., the glass-ceramic is transparent). In some embodiments, the transparency of the glass-ceramic can be achieved by preparing a crystal smaller than the demodulation wavelength of light, and by matching the refractive index of the residual glass with the refractive index of lithium feldspar (1.51) and the refractive index of lithium pyrosilicate (1.55). In some embodiments, a transparent glass-ceramic with a thickness of 1 mm can have a wavelength range of about 400 nm to about 1,000 nm.90% transmittance (including surface reflection loss). In one or more embodiments, for a glass-ceramic article with a thickness of 1 mm, the average transmittance of the transparent glass-ceramic article in the wavelength range of about 400 nm to about 1000 nm is about 85% or greater, about 86% or greater, about 87% or greater, about 88% or greater, about 89% or greater, about 90% or greater, about 91% or greater, about 92% or greater, or about 93% or greater (including surface reflection loss). In other embodiments, the glass-ceramic may be translucent in the visible light range. In some embodiments, for a glass-ceramic article with a thickness of 1 mm, the translucent glass-ceramic may have an average transmittance of about 20% to less than about 85% in the wavelength range of about 400 nm to about 1000 nm. In embodiments where the glass-ceramic is translucent, the glass-ceramic may be white.

[0081] In some embodiments, the grain size in the glass-ceramic can affect transparency or translucency. In some embodiments, the grains of transparent glass-ceramics may have a longest dimension of less than about 100 nm. In some embodiments, the grains of translucent glass-ceramics may have a longest dimension of about 100 nm to about 500 nm. In some embodiments, the grains of transparent glass-ceramics may have an aspect ratio of about 2 or greater. In some embodiments, the grains of translucent glass-ceramics may have an aspect ratio of about 2 or less.

[0082] As a result of the raw materials and / or equipment used to produce the glass compositions of this disclosure, certain impurities or components that are not intentionally added may be present in the final glass composition. Such materials are present in small amounts in the glass or glass-ceramic composition and are referred to herein as indeterminate "materials".

[0083] As used herein, a glass or glass-ceramic composition comprising 0% by weight of a certain compound is defined as not having intentionally added that compound, molecule, or element to the composition, but the composition may still contain that compound, typically in an indeterminate amount or trace amounts. Similarly, "free of iron," "free of sodium," "free of lithium," "free of zirconium," "free of alkaline earth metals," "free of heavy metals," etc., is defined as not having intentionally added that compound, molecule, or element to the composition, but the composition may still contain iron, sodium, lithium, zirconium, alkaline earth metals, or heavy metals, but in an indeterminate amount or trace amounts. Indeterminate compounds that may be found in the glass or glass-ceramic described herein include, but are not limited to, Na₂O, TiO₂, MnO, ZnO, Nb₂O₅, MoO₃, Ta₂O₅, WO₃, ZrO₂, Y₂O₃, La₂O₃, HfO₂, CdO.SnO2, Fe2O3, CeO2, As2O3, Sb2O3, sulfur-based compounds such as sulfates, halogens, or combinations thereof.

[0084] In some embodiments, an antimicrobial component may be added to the glass or glass-ceramic composition. This is particularly preferred because the glass-ceramics described herein can be used in applications such as kitchen or catering countertops, where exposure to harmful bacteria is likely. Antimicrobial components that may be added to the glass or glass-ceramics include, but are not limited to, Ag, AgO, Cu, CuO, Cu2O, etc. In some embodiments, the concentration of the antimicrobial component may be maintained at the following levels: about 3, 2, 1, or 0.5, >0 wt%. In some embodiments, the antimicrobial component is >0 to about 3 wt%. In some embodiments, the antimicrobial component is >0 to about 1 wt%.

[0085] In some embodiments, the glass or glass-ceramic may also include a chemical clarifying agent. Such clarifying agents include, but are not limited to, SnO2, As2O3, Sb2O3, F, Cl, and Br. In some embodiments, the concentration of the chemical clarifying agent is maintained at the following levels: 3, 2, 1, or 0.5, >0 wt%. In some embodiments, the clarifying agent dosage is >0 to about 3 wt%. The chemical clarifying agent may also include CeO2, Fe2O3, and other transition metal oxides such as MnO2. These oxides introduce unwanted colors into the glass or glass ceramic by absorbing visible light in the final valence state of the oxides in the glass, and therefore, when present, the concentration of these oxides is typically maintained at the following levels: 0.5, 0.4, 0.3, 0.2, 0.1, or >0 wt%.

[0086] The glass or glass ceramic may also contain SnO2 as a result of Joule melting when using tin-oxide electrodes; by formulation with tin-containing materials such as SnO2, SnO, SnCO3, SnC2O2, etc., or by adding SnO2 as a reagent to adjust various physical, melting, color, or forming characteristics. The glass or glass-ceramic may contain 0 to about 3% by weight, 0 to about 2% by weight, 0 to about 1% by weight, 0 to 0.5% by weight, or 0 to 0.1% by weight of SnO2.

[0087] In some embodiments, the glass or glass-ceramic may be substantially free of Sb2O3, As2O3, or combinations thereof. For example, the glass or glass-ceramic may contain 0.05% by weight or less of Sb2O3 or As2O3, or combinations thereof; the glass or glass-ceramic may contain 0% by weight of Sb2O3 or As2O3, or combinations thereof; or the glass or glass-ceramic may, for example, be free of any intentionally added Sb2O3, As2O3, or combinations thereof.

[0088] Additional components can be incorporated into the glass composition to provide additional benefits, or contaminants commonly found in commercially prepared glasses can be included. For example, additional components can be added to modulate various physical, melting, and forming characteristics. Glasses according to some embodiments may also contain batch-related contaminants and / or contaminants (such as ZrO2) introduced by the melting, refining, and / or forming equipment used in glass production. In some embodiments, the glass may contain one or more compounds that act as ultraviolet radiation absorbers. In some embodiments, the glass may also contain equal to or less than 3% by weight of TiO2, MnO, ZnO, Nb2O5, MoO3, Ta2O5, WO3, ZrO2, Y2O3, La2O3, HfO2, CdO, Fe2O3, CeO2, or combinations thereof. In some embodiments, the glass may contain 0 to about 3 wt%, 0 to about 2 wt%, 0 to about 1 wt%, 0 to 0.5 wt%, 0 to 0.1 wt%, 0 to 0.05 wt%, or 0 to 0.01 wt% TiO2, MnO, ZnO, Nb2O5, MoO3, Ta2O5, WO3, ZrO2, Y2O3, La2O3, HfO2, CdO, SnO2, Fe2O3, CeO2, As2O3, Sb2O3, or combinations thereof.

[0089] In some embodiments, the glass described herein can be manufactured into sheets by various processes, including but not limited to slot drawing, float glass, roll forming, and other sheet forming processes known in the art. Alternatively, the glass composition can be formed using float or roll forming methods known in the art, as described on pages 15 / 31 of the specification (20 CN 121318156 A).

[0090] In some embodiments, the glass composition described herein can be compatible with float-type forming processes by adjusting the liquidus viscosity. In some embodiments, the glass composition may have a liquidus viscosity of about 1500 P to about 3000 P. In some embodiments, the glass composition may have a liquidus viscosity of about 1000, 1200, 1500, 2000, 2500, or 3000 P.

[0091] In some embodiments, the glass may have the following coefficients of thermal expansion: about 50 x 10⁻⁷ / K or greater, about 50 x 10⁻⁷ / K or greater, about 60 x 10⁻⁷ / K or greater, about 61 x 10⁻⁷ / K or greater, about 62 x 10⁻⁷ / K or greater, about 63 x 10⁻⁷ / K or greater, about 64 x 10⁻⁷ / K or greater, about 65 x 10⁻⁷ / K or greater, about 66 x10⁻⁷ / K or greater, about 67 x 10⁻⁷ / K or greater, about 68 x 10⁻⁷ / K or greater, about 69 x 10⁻⁷ / K or greater, about 70 x 10⁻⁷ / K or greater, about 71 x 10⁻⁷ / K or greater, about 72 x 10⁻⁷ / K or greater, about 73 x 10⁻⁷ / K or greater, about 74 x 10⁻⁷ / K or greater, about 75 x 10⁻⁷ / K or greater, about 76 x 10⁻⁷ / K or greater, about 77 x 10⁻⁷ / K or greater, about 78 x 10⁻⁷ / K or greater, about 79 x 10⁻⁷ / K or greater, or about 80 x 10⁻⁷ / K or greater.

[0092] Articles formed from the glass and glass-ceramics described herein may have any reasonably useful thickness. Embodiments of glass sheets and / or glass-ceramic materials may have any thickness ranging from about 0.8 mm to about 10 mm. Some embodiments have thicknesses of about 6 mm or less, about 5 mm or less, about 3 mm or less, about 1.0 mm or less, about 750 µm or less, about 500 µm or less, or about 250 µm or less. Some glass or glass-ceramic sheet embodiments may have thicknesses of about 200 µm to about 5 mm, about 500 µm to about 5 mm, about 200 µm to about 4 mm, about 200 µm to about 2 mm, about 400 µm to about 5 mm, or about 400 µm to about 2 mm. In some embodiments, the thickness may be about 3 mm to about 6 mm or about 0.8 mm to about 3 mm.

[0093] In some embodiments, on a 1 mm thick glass-ceramic substrate, the glass-ceramic has the following equiaxed flexural strength: about 300 MPa or greater, about 325 MPa or greater, about 350 MPa or greater, about 375 MPa or greater, about 400 MPa or greater, about 425 MPa or greater, or about 450 MPa or greater. The equiaxed flexural strength may also be referred to as the ring-over-ring (RoR) strength, which is measured according to the procedures detailed in ASTM: C1499-05, with some modifications to the test fixture and test conditions, as described in U.S. Patent Application Publication No. 2013 / 0045375, paragraph

[0027] , the entire contents of which are incorporated herein by reference. If the glass-ceramic is first worn (typically using silicon carbide particles), the worn ring-over-ring (aRoR) strength may also be measured using the procedures described above. Some embodiments also include chemically strengthened glass-ceramics having a lithopone phase that provides increased flexural strength. In such embodiments, the RoR strength can be about 500 MPa or greater, about 550 MPa or greater, or about 600 MPa.MPa or greater, about 650 MPa or greater, about 700 MPa or greater, about 750 MPa or greater, or about 800 MPa or greater.

[0094] Some embodiments of glass-ceramics exhibit high fracture toughness and inherent damage resistance. As described above, some embodiments of glass-ceramics include interlocked lithium silicate crystals, which contribute to high fracture toughness. One or more embodiments of glass-ceramics may include boron, which may be present as triple-coordinated boron in the residual glass phase of the glass-ceramic. In this embodiment, triple-coordinated boron is provided by including B2O3 in the precursor glass. Triple-coordinated boron provides a densification mechanism when the glass or glass-ceramic is subjected to indentation load.

[0095] In one or more embodiments, the glass-ceramic exhibits the following fracture toughness: about 1.0 MPa•m1 / 2 or greater, about 1.1 MPa•m1 / 2 or greater, 1.2 MPa•m1 / 2 or greater, 1.3 MPa•m1 / 2 or greater, 1.4 MPa•m1 / 2 or greater, 1.5 MPa•m1 / 2 or greater, 1.6 MPa•m1 / 2 or greater, 1.7 MPa•m1 / 2 or greater, 1.8 MPa•m1 / 2 or greater, 1.9 MPa•m1 / 2 or greater, or about 2.0 MPa•m1 / 2. In some embodiments, the fracture toughness is about 1 to about 2 MPa•m1 / 2. Fracture toughness can be measured using methods known in the art, such as using a V-notch short beam, according to ASTM specification 16 / 31, page 21, CN 121318156 A C1421 – 10, “Standard Test Method for Determining Fracture Toughness of Advanced Ceramics at Ambient Temperatures”.

[0096] In one or more embodiments, glass-ceramics exhibit high crack resistance and scratch resistance by exhibiting Vickers hardness. In some embodiments, the non-ion-exchanged glass-ceramic exhibits the following Vickers hardness: about 600–about 900 kgf / mm², about 600–about 875 kgf / mm², about 600–about 850 kgf / mm², about 600–about 825 kgf / mm², about 600–about 800 kgf / mm², about 600–about 775 kgf / mm², about 600–about 750 kgf / mm², about 600–about 725 kgf / mm², about 600–about 700 kgf / mm², about 700–about 900 kgf / mm², about 700–about 875 kgf / mm², about 700–about 850 kgf / mm², about 700–about 825 kgf / mm², or about 700 kgf / mm². - Approximately 800 kgf / mm². In some embodiments, the Vickers hardness is 600 kgf / mm² or greater, 625kgf / mm² or greater, 650 kgf / mm² or greater, 675 kgf / mm² or greater, 700 kgf / mm² or greater, 725 kgf / mm² or greater, 750 kgf / mm² or greater, 775 kgf / mm² or greater, 800 kgf / mm² or greater, 825 kgf / mm² or greater, 850 kgf / mm² or greater, 875 kgf / mm² or greater, or 900 kgf / mm² or greater. Vickers hardness can be measured using ASTM C1326 and C1327 (and subsequent versions, the entire contents of which are incorporated herein by reference) "Standard Test Methods for Vickers Indentation Hardness in Advanced Ceramics," ASTM International, Conseke Hill, PA, USA. In some embodiments, glass-ceramics exhibit this Vickers indentation crack initiation load value after chemical strengthening by ion exchange.

[0097] In some embodiments, the glass-ceramic described herein is not brittle during ion exchange. Hereinafter, the terms "brittle" and "fragile" mean that a glass-ceramic plate or sheet, when subjected to a force sufficient to break into multiple small pieces upon impact with a sharp object or upon landing on a solid surface, exhibits strong fracturing, which may include: multiple cracks branching out in the glass (i.e., more than five cracks branching from the initial crack), fragments detaching from their initial position by a distance of at least 2 inches (approximately 5 centimeters), a fragmentation density of approximately greater than 5 fragments / cm² glass plate, or any combination of these three conditions. Conversely, if a glass-ceramic plate, when subjected to a force sufficient to break upon impact with a sharp object or upon landing on a solid surface, does not break, or breaks into fewer than five branching cracks from the initial crack, and the fragments detach from their initial position by a distance of less than 2 inches, then the glass is considered non-brittle.

[0098] Figure 10 shows examples of brittleness and non-brittleness observed in 5 cm × 5 cm glass-ceramic plates with a thickness of 0.5 mm. Glass-ceramic plate a is brittle, evidenced by multiple small fragments breaking off more than 2 inches apart, with significant crack branching from the initial crack, producing small fragments. Glass-ceramic plates b, c, and d are not brittle compared to glass-ceramic plate a. In these cases, the glass-ceramic plate breaks into a few large fragments that do not break off forcefully from the initial position more than 2 inches apart (“X” is the approximate center of the glass plate before breakage). Glass-ceramic plate b breaks into two large fragments without crack branching; glass-ceramic plate c breaks into four fragments with two cracks branching from the initial crack; glass-ceramic plate d breaks into four fragments with two cracks branching from the initial crack.

[0099] Furthermore, all compositions and glass and / or glass-ceramic compositions can be ion-exchanged using methods known in the art. In a typical ion-exchange process, smaller metal ions in the glass are replaced or "exchanged" by larger metal ions of the same valence state within a layer adjacent to the outer surface of the glass and / or glass-ceramic. The replacement of smaller ions with larger ions creates compressive stress within the layers of the glass and / or glass-ceramic. In one embodiment, the metal ions are monovalent alkali metal ions (e.g., Na+, K+, Rb+, Cs+, etc.), and the ion exchange is carried out by immersing the glass and / or glass-ceramic in a bath containing at least one molten salt containing larger metal ions, which replace the smaller metal ions in the glass. Alternatively, other monovalent metal ions such as Ag+, Tl+, Cu+, etc., can also be used to exchange monovalent ions. One or more ion exchange processes used to strengthen glass and / or glass-ceramics may include, but are not limited to: immersion in a single bath, or immersion in multiple baths having the same or different compositions, with washing and / or annealing steps between immersions. In one or more embodiments, the glass and / or glass-ceramics may be ion exchanged by exposure to molten NaNO3 at a temperature of about 430°C. In this embodiment, Na+ ions replace some of the Li ions in the glass-ceramic, thereby forming a surface compressive stress layer and exhibiting high crack resistance. After about 2 hours, the resulting compressive stress layer may have a depth of at least 100 micrometers (also referred to as "layer depth") on the glass surface. In this embodiment, the layer depth may be determined from the Na2O concentration distribution. In other embodiments, the embodiment may be ion exchanged by exposure to molten KNO3 at a temperature of 410°C for 2 hours, thereby forming a compressive stress layer with a layer depth of at least about 100 micrometers. In some embodiments, the glass-ceramic may undergo ion exchange to obtain layer depths of approximately 30 µm or greater, approximately 40 µm or greater, approximately 50 µm or greater, approximately 60 µm or greater, approximately 70 µm or greater, approximately 80 µm or greater, approximately 90 µm or greater, or approximately 100 µm or greater. In other embodiments, the glass undergoes ion exchange to obtain a central tension of at least 10 MPa. Forming such a surface compression layer is advantageous for obtaining better crack resistance and higher flexural strength compared to non-ion-exchanged materials. The surface compression layer has a higher concentration of ions exchanged into the glass-ceramic article compared to the body of the glass-ceramic article (i.e., excluding the surface compression region).

[0100] In some embodiments, the glass-ceramic may have surface compressive stresses of approximately 100 MPa to approximately 500 MPa, approximately 100...MPa - approximately 450 MPa, approximately 100 MPa - approximately 400 MPa, approximately 100 MPa - approximately 350 MPa, approximately 100 MPa - approximately 300 MPa, approximately 100 MPa - approximately 250 MPa, approximately 100 MPa - approximately 200 MPa, approximately 100 MPa - approximately 150 MPa, 150 MPa - approximately 500 MPa, approximately 150 MPa - approximately 450 MPa, approximately 150 MPa - approximately 400 MPa, approximately 150 MPa - approximately 350 MPa, approximately 150 MPa - approximately 300 MPa, approximately 150 MPa - approximately 250 MPa, approximately 150 MPa - approximately 200 MPa, 200 MPa - approximately 500 MPa, approximately 200 MPa - approximately 450 MPa, approximately 200 MPa - approximately 400 MPa, approximately 200 MPa - approximately 350 MPa, approximately 200 MPa - approximately 300 MPa, approximately 200 MPa - approximately 250 MPa, 250 MPa - approximately 500 MPa, approximately 250 MPa - approximately 450 MPa, approximately 250 MPa - approximately 400 MPa, approximately 250 MPa - approximately 350 MPa, approximately 250 MPa - approximately 300 MPa, 300 MPa - approximately 500 MPa, approximately 300 MPa - approximately 450 MPa, approximately 300 MPa - approximately 400 MPa, approximately 300 MPa - approximately 350 MPa, 350 MPa - approximately 500 MPa Approximately 350 MPa to approximately 450 MPa, approximately 350 MPa to approximately 400 MPa, 400 MPa to approximately 500 MPa, approximately 400 MPa to approximately 450 MPa, or approximately 450 MPa to approximately 500 MPa. In some embodiments, the glass-ceramic may have surface compressive stresses of approximately 100 MPa or greater, approximately 150 MPa or greater, approximately 200 MPa or greater, approximately 250 MPa or greater, approximately 300 MPa or greater, approximately 350 MPa or greater, approximately 400 MPa or greater, approximately 450 MPa or greater, or approximately 500 MPa or greater. The compressive stress and the depth of the compressive stress layer (“DOL”) are measured using methods known in the art. DOL is determined by measuring surface stress (FSM) using a commercial instrument such as the FSM-6000 manufactured by Luceo Ltd. (Tokyo, Japan) or a similar instrument, and by methods for measuring compressive stress and layer depth such as ASTM.The standard specification for chemically strengthened flat glass, ASTM 1422C-99, entitled "Standard Test Method for Nondestructive Photoelastic Measurement of Edge and Surface Stress in Annealed, Heat-Strengthened, Fully Tempered Flat Glass," is incorporated herein by reference in its entirety. Surface stress measurement relies on the accurate measurement of the stress-optic coefficient (SOC), which is related to the birefringence of the glass. SOC is then measured by methods known in the art, such as fiber and four-point bending methods (both described in ASTM Standard C770-98 (2008), entitled "Standard Test Method for Measurement of Stress-Optical Coefficient of Glass," which is incorporated herein by reference in its entirety) and block cylinder methods.

[0101] In one or more embodiments, the method for preparing glass ceramics includes heat-treating a precursor glass at one or more pre-selected temperatures for one or more pre-selected times to induce glass homogenization and crystallization (i.e., nucleation and growth) of one or more crystalline phases (e.g., having one or more compositions, amounts, morphologies, size distributions, etc.). In some embodiments, the heat treatment may include (i) heating the precursor glass to a prenucleation temperature at a rate of 1–10 °C / min; (ii) holding the crystallizable glass at the prenucleation temperature for about 1 / 4 hour to about 4 hours to form a prenucleated crystallizable glass; (iii) heating the prenucleated crystallizable glass to a nucleation temperature (Tn) at a rate of 1–10 °C / min; (iv) holding the crystallizable glass at the nucleation temperature for about 1 / 4 hour to about 4 hours to form a nucleated crystallizable glass; (v) heating the nucleated crystallizable glass to a crystallization temperature (Tc) at a rate of 1 °C / min to about 10 °C / min; (vi) holding the nucleated crystallizable glass at the crystallization temperature for about 1 / 4 hour to about 4 hours to form the glass-ceramic described herein; and (vii) cooling the formed glass-ceramic to room temperature. As used herein, the term crystallization temperature may be used interchangeably with ceramic temperature or ceramization temperature. Furthermore, in these embodiments, the terms "ceramic" or "ceramization" may be used to uniformly refer to steps (v), (vi), and optionally (vii). In some embodiments, the glass pre-nucleation temperature may be 540°C, the nucleation temperature may be 600°C, and the crystallization temperature may be 630°C–730°C. In other embodiments, the heat treatment does not include holding the crystallizable glass at the glass pre-nucleation temperature. Therefore, the heat treatment may include (i) heating the precursor glass to the nucleation temperature (Tn) at a rate of 1–10°C / min; and (ii) holding the crystallizable glass at the nucleation temperature for approximately ¼ hour.(iii) The nucleated crystallizable glass is heated to the crystallization temperature (Tc) at a rate of about 1 °C / min to about 10 °C / min; (iv) The nucleated crystallizable glass is held at the crystallization temperature for about ¼ hour to about 4 hours to form the glass-ceramic described herein; and (v) The formed glass-ceramic is cooled to room temperature. Furthermore, in these embodiments, the terms "ceramic" or "ceramization" may be used to uniformly refer to steps (iii), (iv), and optionally (v). In some embodiments, the nucleation temperature may be about 700 °C, and the crystallization temperature may be about 800 °C. In some embodiments, a higher crystallization temperature results in the formation of more β-spodumene ss as a secondary crystalline phase.

[0102] The temperature-time distribution of the heat treatment step and the composition of the precursor glass are wisely defined when heating to the crystallization temperature and maintaining the temperature at the crystallization temperature, thereby producing one or more of the following desired performance characteristics: the crystalline phase of the glass-ceramic, the ratio of one or more dominant crystalline phases and / or one or more secondary crystalline phases to the residual glass, the crystalline phase aggregate of one or more dominant crystalline phases and / or one or more secondary crystalline phases to the residual glass, and the grain size or grain size distribution of one or more dominant crystalline phases and / or one or more secondary crystalline phases, which in turn can affect the final integrity, quality, color, and / or opacity of the resulting glass-ceramic.

[0103] The resulting glass-ceramic can then be provided as sheets, which can be reshaped into curved or bent workpieces of uniform thickness by pressing, blow molding, bending, sag, vacuum forming, or other means. Reshaping can be performed before heat treatment, or the shaping step can also be used as a heat treatment step, wherein the shaping step and heat treatment are performed substantially simultaneously.

[0104] In other embodiments, a precursor glass composition for forming a glass-ceramic can be prepared, for example, so that the glass-ceramic can be chemically strengthened using one or more ion exchange techniques. In these embodiments, ion exchange can be performed by exposing one or more surfaces of such glass-ceramic to one or more ion exchange baths having a specific composition and temperature for a specified time, thereby imparting a compressive stress layer to one or more surfaces. The compressive stress layer may contain one or more average surface compressive stresses (CS), and / or one or more layer depths.

[0105] Many efforts have been made to ensure the accuracy of numerical values ​​(e.g., quantities, temperatures, etc.), but some errors and deviations must be taken into account. Unless otherwise stated, temperatures are expressed in °C or ambient temperature, and pressures are atmospheric pressure or near atmospheric pressure. The composition itself is given in wt% based on oxides and has been normalized to 100%. There are many variations and combinations of reaction conditions, such as component concentrations, temperatures, and pressures, and these can be used to optimize the purity of the product obtained from the described process.Other reaction ranges and conditions for clarity and yield. Only reasonable and conventional experimental methods are required to optimize such process conditions. Specification 19 / 31 pages 24 CN 121318156 A

[0106] Example 1 Example glass and glass-ceramic composition (expressed in wt%) and the properties for obtaining transparent glass-ceramics are shown in Table 1 and determined according to conventional techniques in the glass industry. Precursor glasses having compositions 1-16 listed in Table 1 were formed. The precursor glasses were then exposed to a ceramicization cycle having a glass homogenization hold of 4 hours at 540°C, a nucleation hold of 4 hours at 600°C, and a crystallization hold of 4 hours at a temperature of 630-730°C. In Table 1, the ceramicization cycle is described using the following terms: glass homogenization temperature - hold time / nucleation temperature - hold time / crystallization temperature - hold time.

[0107] The liquidus temperature is the temperature at which the first crystal is observed in a standard gradient boat liquidus measurement (ASTM C829-81 and subsequent versions). This method involves placing pulverized glass particles in a platinum boat, immersing the boat in a furnace with a gradient temperature zone, heating the boat at an appropriate temperature range for 24 or 72 hours, and determining the temperature by microscopically detecting the highest temperature at which crystals appear inside the glass. Specifically, the glass sample is removed intact from the Pt boat, and then polarized optical microscopy is used to determine the location and nature of crystals forming near the Pt-air interface and inside the sample. Because the furnace gradient is well-known, the temperature-relative-position relationship can be estimated relatively well, within 5–10 °C. The temperature of the crystals observed inside the sample is considered representative of the liquidus of the glass (for the corresponding test period). Tests are sometimes conducted for longer periods (e.g., 72 hours) to observe a slower growth phase. The liquidus viscosity, in poise, is determined from the liquidus temperature and the coefficients of the Fulcher equation.

[0108] Table 1 Specification 20 / 31 Page 25 CN 121318156 A

[0109] Table 1 (continued) Specification 21 / 31 Page 26 CN 121318156 A Specification 22 / 31 Page 27 CN 121318156 A

[0110] After ceramization, various tests were performed on composition 2 to determine various properties of the glass-ceramic of composition 2. As shown in Figure 1, the differential scanning calorimetry (DSC) trace of composition 2 was measured, and DSC / (mW / mg) was plotted against temperature in degrees Celsius. The trace is used to indicate that a fine grain microstructure can be achieved by ceramization at a lower temperature relative to the crystallization temperature.

[0111] The transmittance of the glass-ceramic composition 2 with a thickness of 1 mm for light with wavelengths of 400 nm to 1,000 nm was measured. As shown in Figure 2, the average transmittance of the glass-ceramic composition 2 in the visible light wavelength range is greater than 90%.

[0112] The glass-ceramic composition 2 samples were observed using scanning electron microscopy (SEM) to determine the grain size of the lepidolite. Figure 3A shows the SEM at a 200 nm scale, and Figure 3B shows the SEM at a 100 nm scale. The lepidolite grains were in the 50–100 nm range. It is believed that the grain fineness contributes to the transparency of the glass-ceramic as confirmed in Figure 2.

[0113] Two 50 mm × 50 mm × 1 mm samples of glass-ceramic composition 2 were subjected to the ring stacking test as described above to determine the sample strength. One sample was worn (15 psi), and the other sample was not worn. Figure 4 shows the results of the ring stacking test. For the ring stacking test, a strength of 514 MPa was obtained.

[0114] The fracture toughness of the glass-ceramic composition 2 samples was measured using a V-notch short beam measurement. The fracture toughness was 1.13 MPa•m1 / 2.

[0115] The hardness of the glass-ceramic sample was measured using a MicroTester (model 5948) available from Instron to determine the Vickers hardness as described above. The Vickers hardness is approximately 750 kgf / mm².

[0116] The glass-ceramic of composition 2 was subjected to an ion exchange process in which the sample was placed in a molten NaNO₃ bath at 430°C for 2 hours, 4 hours, 8 hours, and 16 hours. As shown in Figure 5, a layer depth exceeding 100 micrometers was obtained. Figure 5 also shows a graph of the Na₂O concentration (in mol%) versus sample thickness for each ion exchange treatment. As can be seen from the graph, the layer depth increases with the duration of the ion exchange treatment. Furthermore, a parabolic Na₂O concentration was obtained after 16 hours of ion exchange.

[0117] Ion exchange was performed on two 50 mm × 50 mm × 1 mm samples of the glass-ceramic of composition 2. One sample was ion-exchanged in a molten NaNO3 bath at 430°C for 2 hours, and another sample was ion-exchanged in a molten KNO3 bath at 430°C for 2 hours. The two ion-exchanged samples, as well as a 50 mm × 50 mm × 1 mm glass-ceramic sample of composition 2 that was not ion-exchanged, were subjected to the ring-chain test as described above. The results are shown in Figure 6. After ion exchange with NaNO3, the strength of the glass-ceramic increased by approximately 30%, and approximately doubled after ion exchange with KNO3. It is believed that ion exchange using a KNO3 bath results in a larger layer depth (DOL) for the compressive stress layer formed on the sample surface during ion exchange.

[0118] A 50 mm × 50 mm × 1 mm glass-ceramic sample of composition 2 was ion-exchanged in a molten NaNO3 bath at 430°C for 2 hours. A 50 mm × 50 mm × 1 mm glass-ceramic sample of composition 2 was ion-exchanged in a molten NaNO3 bath at 430°C for 2 hours.The 50 mm × 50 mm × 1 mm sample of glass B was ion-exchanged at 420°C for 5.5 hours in a molten KNO3 bath. The 50 mm × 50 mm × 1 mm sample of glass B was ion-exchanged at 540°C for 8 hours in a 32% KNO3 molten bath, and then ion-exchanged at 390°C for 15 minutes in a 100% KNO3 molten bath. All samples were worn at 15 psi and subjected to the wear ring stacking test as described above. The results are shown in Figure 7. The glass ceramic has a higher strength than glass A and a strength close to that of glass B. Therefore, the strength of the ion-exchanged glass ceramic can be exactly the same as or higher than that of the ion-exchanged glass.

[0119] The 50 mm × 50 mm × 1 mm sample of glass ceramic of composition 2 was ion-exchanged at 430°C for 2 hours, 4 hours, 8 hours, and 16 hours in a molten NaNO3 bath. Then, the ring stacking test as described above was performed on the ion-exchanged sample and the union-exchanged glass ceramic sample of composition 2. The results are shown in Figure 8. The strength of the glass-ceramic increases based on the duration of ion exchange.

[0120] A 50 mm × 50 mm × 1 mm sample of the glass-ceramic of composition 2 was ion-exchanged in a molten NaNO3 bath at 430°C for 16 hours. The samples were worn at 15 psi, 25 psi, or 45 psi, and the wear ring stacking test as described above was performed. The results are shown in Figure 9. The sample worn at 15 psi had a load failure of about 253 MPa, the sample worn at 25 psi had a load failure of about 240 MPa, and the sample worn at 45 psi had a load failure of about 201 MPa.

[0121] Example 2 Example glass and glass-ceramic composition (in weight %) and the properties of the translucent glass-ceramic used to obtain it are shown in Table 2 and determined according to conventional techniques in the glass industry. A precursor glass having compositions 17-29 listed in Table 2 was formed. The precursor glass was then subjected to the ceramicization cycle shown in Table 2 below.

[0122] Table 2, Specification 24 / 31, Page 29, CN 121318156 A

[0123] Table 2 (continued), Specification 25 / 31, Page 30, CN 121318156 A

[0124] The fracture toughness of samples of glass-ceramic compositions 17, 18, and 22 was measured using a V-notch short beam measurement. The fracture toughnesses were 1.2 MPa•m1 / 2, 1.13 MPa•m1 / 2, and 1.2 MPa•m1 / 2, respectively.

[0125] As shown in Figure 11, the differential scanning calorimetry (DSC) trace of composition 18 was measured, and DSC / (mW / mg) was plotted against temperature in degrees Celsius. Figure 12 is the X-ray diffraction (XRD) pattern of the crystalline phase formed in composition 18. From the XRD...As can be seen from the spectra, lithium feldspar and lithium pyrosilicate are the main crystalline phases.

[0126] Two 50 mm 50 mm 1 mm samples of glass-ceramic compositions 19, 20 and 21 were subjected to the ring stacking test as described above to determine the sample strength. Figure 13 shows the results of the ring stacking test. For the ring stacking test, strengths of 352 MPa, 304 MPa and 313 MPa were obtained, respectively. Therefore, for the translucent glass-ceramic described herein, a strength of more than 300 MPa can be obtained. Specification 26 / 31 pages 31 CN 121318156 A

[0127] An ion exchange process was performed on the glass-ceramic of composition 18 formed by adding a Na2O concentration of 1.4 mol% to the bulk glass, wherein the sample was placed in a NaNO3 bath at 430°C for 4 hours. As shown in Figure 14, a layer depth of more than 100 micrometers was obtained. Figure 14 also shows a graph of the relationship between the Na2O concentration and the sample thickness, expressed as wt%.

[0128] Although typical embodiments have been given for illustrative purposes, the foregoing description should not be considered as a limitation on the scope of this specification or the appended claims. Therefore, various modifications, alterations, and substitutions will be apparent to those skilled in the art without departing from the spirit and scope of this specification or the appended claims.

[0129] This application also relates to the following technical solutions.

[0130] 1. A glass-ceramic article comprising: a lithium feldspar crystal phase; and a lithium silicate crystal phase, wherein the lithium feldspar crystal phase and the lithium silicate crystal phase have a higher weight percentage than other crystal phases present in the glass-ceramic article.

[0131] 2. The glass-ceramic article according to technical solution 1, characterized in that the lithium feldspar crystal phase accounts for 20-70% by weight of the glass-ceramic article, and the lithium silicate crystal phase accounts for 20-60% by weight of the glass-ceramic article.

[0132] 3. The glass-ceramic article as described in technical solution 2, characterized in that the transparent lithium feldspar crystal phase accounts for 45-70% by weight of the glass-ceramic article, and the lithium silicate crystal phase accounts for 20-50% by weight of the glass-ceramic article.

[0133] 4. The glass-ceramic article as described in technical solution 2, characterized in that the transparent lithium feldspar crystal phase accounts for 40-60% by weight of the glass-ceramic article, and the lithium silicate crystal phase accounts for 20-50% by weight of the glass-ceramic article.

[0134] 5. The glass-ceramic article as described in any one of technical solutions 1-4, characterized in that the lithium silicate crystal phase is a lithium pyrosilicate crystal phase or a lithium metasilicate crystal phase.

[0135] 6. The glass-ceramic article as described in any one of technical solutions 1-5, characterized in that the article is transparent.

[0136] 7. The glass-ceramic article as described in technical solution 6, characterized in that, at a thickness of 1 mm, for 400 nm - 1,000 nmFor light within the wavelength range, the article has a transmittance of at least 85%.

[0137] 8. The glass-ceramic article as described in claim 6, characterized in that, at a thickness of 1 mm, for light within the wavelength range of 400 nm to 1,000 nm, the article has a transmittance of at least 90%.

[0138] 9. The glass-ceramic article as described in any one of claims 1-5, characterized in that the article is translucent, and at a thickness of 1 mm, for light within the wavelength range of 400 nm to 1,000 nm, the article has a transmittance of from 20% to less than 85%.

[0139] 10. The glass-ceramic article according to any one of technical solutions 1-9, characterized in that, by weight percent, the glass-ceramic article has a composition comprising the following components: SiO2: 55-80%; Al2O3: 2-20%; Li2O: 5-20%; B2O3: 0-10%; Na2O: 0-5%; ZnO: 0-10%; P2O5: 0.5-6%; and ZrO2: 0.2-15%. Specification 27 / 31 pages 32 CN 121318156 A

[0140] 11. The glass-ceramic article as described in technical solution 10, characterized in that, by weight %, the glass-ceramic article has a composition further comprising the following components: K2O: 0-4%; MgO: 0-8%; TiO2: 0-5%; CeO2: 0-0.4%; and SnO2: 0.05-0.5%.

[0141] 12. The glass-ceramic article as described in technical solution 10, characterized in that, by weight %, the glass-ceramic article has a composition comprising the following components: SiO2: 69-80%; Al2O3: 6-9%; Li2O: 10-14%; B2O3: 0-12%; P2O5: 1.5-2.5%; and ZrO2: 2-4%.

[0142] 13. The glass-ceramic article as described in technical solution 10, characterized in that, by weight %, the glass-ceramic article has a composition comprising the following components: SiO2: 69-80%; Al2O3: 6-9%; Li2O: 10-14%; Na2O: 1-2%; K2O: 1-2%; B2O3: 0-12%; P2O5: 1.5-2.5%; and ZrO2: 2-4%.

[0143] 14. The glass-ceramic article as described in technical solution 10, characterized in that, by weight %, the glass-ceramic article has a composition comprising the following components: SiO2: 65-80%; Al2O3: 5-16%; Li2O: 8-15%; Na2O: 0-3%;K2O: 0-3%; B2O3: 0-6%; ZnO: 0-2%; P2O5: 0.5-4%; and ZrO2: 0.2-6%.

[0144] 15. The glass-ceramic article as described in technical solution 10, characterized in that, by weight %, the glass-ceramic article has a composition comprising the following components: SiO2: 60-80%; Al2O3: 5-20%; Li2O: 5-20%; Na2O: 0-3%; K2O: 0-3%; B2O3: 0-6%; ZnO: 0-4%; P2O5: 0.5-4%; and ZrO2: 0.2-8%.

[0145] 16. The glass-ceramic article as described in claim 10, characterized in that the sum of the weight percentages of P2O5 and ZrO2 is greater than 3.

[0146] 17. The glass-ceramic article as described in any one of claims 1-16, characterized in that the glass-ceramic article has a fracture toughness of 1 MPa•m1 / 2 or greater.

[0147] 18. The glass-ceramic article as described in any one of claims 1-17, characterized in that the glass-ceramic article has a Vickers hardness of about 600 kgf / mm2 or greater.

[0148] 19. The glass-ceramic article as described in any one of claims 1-18, characterized in that the glass-ceramic article has a surface compressive stress of about 100 MPa to about 500 MPa.

[0149] 20. The glass-ceramic article as described in any one of claims 1-19, characterized in that it further comprises a compressive stress layer having a layer depth (DOL) of at least about 30 micrometers.

[0150] 21. The glass-ceramic article as described in claim 20, characterized in that the glass-ceramic article is not brittle.

[0151] 22. The glass-ceramic article as described in any one of claims 1-21, characterized in that it further comprises grains having a longest dimension of 500 nm or less.

[0152] 23. The glass-ceramic article as described in any one of claims 1-22, characterized in that it further comprises grains having a longest dimension of 100 nm or less.

[0153] 24. The glass-ceramic article as described in any one of claims 1-23, characterized in that the glass-ceramic article has a ring-stack strength of at least 300 MPa.

[0154] 25. A method of forming a glass-ceramic article, the method comprising the steps of: forming a glass composition, the glass composition comprising, by weight percent: SiO2: 55-80%; Al2O3: 2-20%; Li2O: 5-20%;B2O3: 0-10%; Na2O: 0-5%; ZnO: 0-10%; P2O5: 0.5-6%; and ZrO2: 0.2-15%; and the glass composition is ceramicized to form a glass-ceramic article having a lithium feldspar crystal phase and a lithium silicate crystal phase, wherein the lithium feldspar crystal phase and the lithium silicate crystal phase have a higher weight percentage than other crystal phases present in the glass-ceramic article. Specification 29 / 31 pages 34 CN 121318156 A

[0155] 26. The method of claim 25, characterized in that, by weight %, the glass composition further comprises: K2O: 0-4%; MgO: 0-8%; TiO2: 0-5%; CeO2: 0-0.4%; and SnO2: 0.05-0.5%.

[0156] 27. The method of claim 25, wherein, by weight percent, the glass composition comprises: SiO2: 69-80%; Al2O3: 6-9%; Li2O: 10-14%; B2O3: 0-12%; P2O5: 1.5-2.5%; and ZrO2: 2-4%.

[0157] 28. The method of claim 25, wherein, by weight percent, the glass composition comprises: SiO2: 69-80%; Al2O3: 6-9%; Li2O: 10-14%; Na2O: 1-2%; K2O: 1-2%; B2O3: 0-12%; P2O5: 1.5-2.5%; and ZrO2: 2-4%.

[0158] 29. The method of claim 25, wherein, by weight percent, the glass composition comprises: SiO2: 65-80%; Al2O3: 5-16%; Li2O: 8-15%; Na2O: 0-3%; K2O: 0-3%; B2O3: 0-6%; ZnO: 0-2%; P2O5: 0.5-4%; and ZrO2: 0.2-6%.

[0159] 30. The method of claim 25, characterized in that, by weight percent, the glass composition comprises: SiO2: 60-80%; Al2O3: 5-20%; Li2O: 5-20%; Na2O: 0-3%; K2O: 0-3%; B2O3: 0-6%; ZnO: 0-4%; P2O5: 0.5-4%; and ZrO2: 0.2-8%.

[0160] 31.The method of any one of technical solutions 25-30 is characterized in that the sum of the weight percentages of P2O5 and ZrO2 is greater than 3.

[0161] 32. The method of any one of technical solutions 25-31 is characterized in that the method further comprises ion-exchanging the glass-ceramic article to form a compressive stress layer having a layer depth of at least 30 micrometers.

[0162] 33. The method of any one of technical solutions 25-32 is characterized in that the ceramization comprises the following sequential steps: heating the glass composition to a glass pre-nucleation temperature; holding the glass pre-nucleation temperature for a predetermined time; heating the composition to a nucleation temperature; holding the nucleation temperature for a predetermined time; heating the composition to a crystallization temperature; and holding the crystallization temperature for a predetermined time.

[0163] 34. The method of any one of technical solutions 25-30 is characterized in that the ceramization comprises the following sequential steps: heating the composition to a nucleation temperature; holding the nucleation temperature for a predetermined time; heating the composition to a crystallization temperature; and holding the crystallization temperature for a predetermined time.

[0164] 35. The method according to any one of technical solutions 25-33, characterized in that the lithium feldspar crystal phase accounts for 20-70% by weight of the glass-ceramic article, and the lithium silicate crystal phase accounts for 20-60% by weight of the glass-ceramic article. Instruction manual page 31 / 31, page 36, CN 121318156 A, Figure 1; Instruction manual figure 1 / 15, page 37, CN 121318156 A, Figure 2; Instruction manual figure 2 / 15, page 38, CN 121318156 A, Figure 3A; Instruction manual figure 3 / 15, page 39, CN 121318156 A, Figure 3B; Instruction manual figure 4 / 15, page 40, CN 121318156 A, Figure 4; Instruction manual figure 5 / 15, page 41, CN 121318156 A, Figure 5; Instruction manual figure 6 / 15, page 42, CN 121318156 A, Figure 6; Instruction manual figure 7 / 15, page 43, CN 121318156 A, Figure 7; Instruction manual figure 8 / 15, page 44, CN 121318156 A, Figure 8; Instruction manual figure 9 / 15, page 45, CN 121318156 A, Figure 9. Instruction manual, Figure 10 / 15, page 46, CN 121318156 A, Figure 10; Instruction manual, Figure 11 / 15, page 47, CN 121318156 A, Figure 11; Instruction manual, Figure 12 / 15, page 48, CN 121318156 A, Figure 12; Instruction manual, Figure 13 / 15, page 49, CN 121318156 A, Figure 13.Description Drawings Page 14 / 15 50 CN 121318156 A Figure 14 Description Drawings Page 15 / 15 51 CN 121318156 A Abstract Glass and glass ceramic compositions having a combination of lithium silicate and petalite crystalline phases along with methods of making the glass and glass ceramic compositions are described. The compositions are compatible with conventional rolling and float processes, are transparent or translucent, and have high mechanical strength and fracture resistance. Further, the compositions are able to be chemically tempered to even higher strength glass ceramics that are useful as large substrates in multiple applications.

Claims

1. A glass-ceramic article, comprising, by weight percentage: 55% to 80% by weight of SiO2; 2% to 20% by weight of Al2O3; 5% to 20% by weight of Li₂O; 0% to 10% by weight of B2O3; 0% to 5% by weight of Na₂O; 0% to 10% ZnO; 0.5 wt% to 6 wt% of P2O5; and 0.2% to 15% by weight of ZrO2, The sum of P2O5 and ZrO2 is greater than or equal to 3 by weight.

2. The glass-ceramic article according to claim 1, comprising: 65% to 75% by weight of SiO2; 2% to 8% by weight of Al2O3; 10% to 16% by weight of Li₂O; >0% to 1% by weight of R2O, where R is Na and K; 0% to 1% by weight of B2O3; 3% to 5% by weight of P2O5; and 4% to 12% by weight of ZrO2, The sum of P2O5 and ZrO2 is greater than or equal to 5% by weight.

3. The glass-ceramic article according to claim 2, comprising: 65% to 73% by weight of SiO2; 2% to 5% by weight of Al2O3; and 12% to 16% by weight of Li₂O, The sum of P2O5 and ZrO2 is greater than or equal to 7 by weight.

4. The glass-ceramic article according to claim 2, comprising: 69% to 75% by weight of SiO2; 6% to 8% by weight of Al2O3; 10 wt% to 12 wt% Li₂O; and 4% to 8% by weight of ZrO2.

5. The glass-ceramic article according to claim 1, comprising: 0% to 4% by weight of K2O; 0% to 8% by weight of MgO; 0% to 5% by weight of TiO2; 0% to 0.4% by weight of CeO2; and 0.05% to 0.5% by weight of SnO2.

6. The glass-ceramic article according to any one of claims 1-5, wherein the glass-ceramic article is transparent, has a thickness of 0.8 mm to 6 mm, and has a transmittance of at least 85% for light in the wavelength range of 400 nm to 1,000 nm.

7. The glass-ceramic article according to any one of claims 1-5, wherein the glass-ceramic article is chemically strengthened and contains a surface compressive stress of 300 MPa or greater.

8. The glass-ceramic article of claim 7, comprising a thickness of 200 micrometers to 5 mm, a central tension of at least 10 MPa, and an ion-exchange layer depth of 30 micrometers or greater.

9. The glass-ceramic article according to any one of claims 1-5, wherein, The glass-ceramic product has a strength of 1 MPa·m 1 / 2 Or greater fracture toughness.

10. The glass-ceramic article according to any one of claims 1-5, wherein, The glass-ceramic product has a strength of 600 kgf / mm². 2 Or a higher Vickers hardness.

11. The glass-ceramic article according to any one of claims 1-5, wherein, The glass-ceramic article has a ring-to-ring strength of at least 300 MPa.

12. The glass-ceramic article according to any one of claims 1-5, comprising grains having a longest dimension of 100 nm or less.

13. The glass-ceramic article according to any one of claims 1-5, comprising grains having an aspect ratio of 2 or greater, wherein, The glass-ceramic product is transparent.

14. The glass-ceramic article according to any one of claims 1-5, comprising 20% ​​to 60% by weight of lithium silicate crystalline phase.

15. The glass-ceramic article according to claim 14, wherein, The lithium silicate crystal phase is the primary crystal phase, and the glass-ceramic article has one or more secondary phases, the secondary phases comprising one or more of β-spodumene solid solution, β-quartz solid solution, lithium phosphate, cristobalite, or rutile.

16. The glass-ceramic article according to any one of claims 1-5, wherein, The lithium feldspar crystal phase accounts for 20% to 70% by weight of the glass-ceramic article.

17. The glass-ceramic article as claimed in claim 14, wherein, The spodumene crystal phase is the primary crystalline phase, and the glass-ceramic article has one or more secondary phases, the secondary phases comprising one or more of β-spodumene solid solution, β-quartz solid solution, lithium phosphate, cristobalite, or rutile.

18. The glass-ceramic article as claimed in claim 14, wherein, The lithium feldspar crystal phase accounts for 20% to 70% by weight of the glass-ceramic article, while the lithium silicate crystal phase accounts for 20% to 60% by weight of the glass-ceramic article.

19. A precursor glass composition, comprising, by weight percentage: 55% to 80% by weight of SiO2; 2% to 20% by weight of Al2O3; 5% to 20% by weight of Li₂O; 0% to 10% by weight of B2O3; 0% to 5% by weight of Na₂O; 0% to 10% ZnO; 0.5 wt% to 6 wt% of P2O5; and 0.2 wt% to 15 wt% ZrO2, The sum of P2O5 and ZrO2 is greater than or equal to 3 by weight.

20. The precursor glass composition according to claim 19, comprising: 65% to 75% by weight of SiO2; 2% to 8% by weight of Al2O3; 10% to 16% by weight of Li₂O; >0% to 1% by weight of R2O, where R is Na and K; 0% to 1% by weight of B2O3; 3% to 5% by weight of P2O5; and 4% to 12% by weight of ZrO2, The sum of P2O5 and ZrO2 is greater than or equal to 5% by weight.

21. The precursor glass composition according to claim 20, comprising: 65% to 73% by weight of SiO2; 2% to 5% by weight of Al2O3; and 12% to 16% by weight of Li₂O, The sum of P2O5 and ZrO2 is greater than or equal to 7 by weight.

22. The precursor glass composition according to claim 20, comprising: 69% to 75% by weight of SiO2; 6% to 8% by weight of Al2O3; 10 wt% to 12 wt% Li₂O; and 4% to 8% by weight of ZrO2.

23. The precursor glass composition according to claim 19, comprising: 0% to 4% by weight of K2O; 0% to 8% by weight of MgO; 0% to 5% by weight of TiO2; 0% to 0.4% by weight of CeO2; and 0.05% to 0.5% by weight of SnO2.

24. The glass-ceramic article according to any one of claims 19-23, wherein, The glass-ceramic product has a strength of 1 MPa·m 1 / 2 Or greater fracture toughness.

25. A method for manufacturing glass-ceramics, comprising: The precursor glass is heat-treated using the following steps: (i) The glass is heated to the pre-nucleation temperature at a rate of 1 to 10 °C / min; (ii) The glass is held at the prenucleation temperature for 1 / 4 hour to 4 hours; (iii) The glass is heated to the nucleation temperature at a rate of 1 to 10 °C / min; (iv) The glass is held at the nucleation temperature for 1 / 4 hour to 4 hours; (v) The glass is heated to its crystallization temperature at a rate of 1 °C / min to 10 °C / min; as well as (vi) Hold the glass at the crystallization temperature for 1 / 4 hour to 4 hours. This forms the glass-ceramic material.

26. The method of claim 25, further comprising cooling the glass-ceramic to room temperature.

27. The method according to claim 26, wherein, The crystallization temperature is in the range of 630°C to 730°C.

28. The method according to claim 27, wherein, The pre-nucleation temperature is 540℃.

29. The method according to any one of claims 25-28, wherein, The precursor glass comprises a composition, which, by weight percentage, comprises: 55% to 80% by weight of SiO2; 2% to 20% by weight of Al2O3; 5% to 20% by weight of Li₂O; 0% to 10% by weight of B2O3; 0% to 5% by weight of Na₂O; 0% to 10% ZnO; 0.5 wt% to 6 wt% of P2O5; and 0.2 wt% to 15 wt% ZrO2, The sum of P2O5 and ZrO2 is greater than or equal to 3 by weight.

30. The method of claim 29, wherein the composition comprises: 65% to 75% by weight of SiO2; 2% to 8% by weight of Al2O3; 10% to 16% by weight of Li₂O; >0% to 1% by weight of R2O, where R is Na and K; 0% to 1% by weight of B2O3; 3% to 5% by weight of P2O5; and 4% to 12% by weight of ZrO2, The sum of P2O5 and ZrO2 is greater than or equal to 5% by weight.

31. The method of claim 30, wherein the composition comprises: 65% to 73% by weight of SiO2; 2% to 5% by weight of Al2O3; and 12% to 16% by weight of Li₂O, The sum of P2O5 and ZrO2 is greater than or equal to 7 by weight.

32. The method of claim 30, wherein the composition comprises: 69% to 75% by weight of SiO2; 6% to 8% by weight of Al2O3; 10 wt% to 12 wt% Li₂O; and 4% to 8% by weight of ZrO2.