Glass composition for glass fiber, glass fiber, glass fiber fabric, and glass fiber-reinforced resin composition

HK40137359APending Publication Date: 2026-09-11NITTO BOSEKI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
HK62026124612
Authority / Receiving Office
HK · HK
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-02-24
Filing Date
2026-06-10
Publication Date
2026-09-11
Patent Text Reader

Abstract

Provided is a glass composition having a sufficient operating temperature range, with which a glass fiber having excellent water resistance and dielectric properties can be obtained. The glass composition contains 59.00 to 65.00% by mass of SiO2, 16.00 to 26.00% by mass of B2O3, 7.00 to 14.00% by mass of Al2O3, 0 to 5.00% by mass of CaO, 0 to 4.00% by mass of MgO, 0 to 6.00% by mass of SrO, 0.10 to 5.00% by mass of TiO2, 0 to 2.00% by mass of F2 and Cl2 in total, less than 0.20% by mass of P2O5, and less than 1.00% by mass of Na2O, K2O and Li2O in total.
Need to check novelty before this filing date? Find Prior Art

Description

(19) State Intellectual Property Office (12) Invention Patent Application (10) Application Publication Number (43) Application Publication Date (21) Application Number 202610214630.1 (22) Application Date 2022.02.09 (30) Priority Data 2021-026997 2021.02.24 JP (62) Divisional Application Data 202280009045.8 2022.02.09 (71) Applicant Nitto Spinning Co., Ltd. Address 1 Higashi, Gonome, Fukushima City, Fukushima Prefecture, Japan (72) Inventors Takayuki Hosokawa, Tadashi Kurita, Takashi Nonaka (74) Patent Agency Beijing Yifeng Intellectual Property Agency Co., Ltd. 11293 Patent Attorney Li Yanli (51) Int.Cl. C03C 13 / 02 (2006.01) C03B 37 / 06(2006.01) C08J 5 / 04(2006.01) C08L 101 / 00(2006.01) C08K 7 / 14(2006.01) D03D 15 / 267(2021.01) (54) Invention Title Glass Composition for Glass Fiber, Glass Fiber, Glass Fiber Fabric and Glass Fiber Reinforced Resin Composition (57) Abstract This invention provides a glass composition having a sufficient operating temperature range, which enables the production of glass fibers with excellent water resistance and dielectric properties. The glass composition contains 59.00–65.00% by mass of SiO2, 16.00–26.00% by mass of B2O3, 7.00–14.00% by mass of Al2O3, 0–5.00% by mass of CaO, 0–4.00% by mass of MgO, 0–6.00% by mass of SrO, 0.10–5.00% by mass of TiO2, a total of 0–2.00% by mass of F2 and Cl2, less than 0.20% by mass of P2O5, and a total content of less than 1.00% by mass of Na2O, K2O, and Li2O.Claims 1 page, Description 22 pages, CN 121929914 A 2026.04.28 CN 1 21 92 99 14 A 1. A glass composition for glass fiber, characterized in that it contains SiO2 in the range of 59.00-65.00% by mass, B2O3 in the range of 16.00-26.00% by mass, Al2O3 in the range of 7.00-14.00% by mass, CaO in the range of 0-5.00% by mass, MgO in the range of 0-4.00% by mass, SrO in the range of 0-6.00% by mass, TiO2 in the range of 0.10-5.00% by mass, and F2 and Cl2 in the range of 0-2.00% by mass, the content of P2O5 is less than 0.20% by mass, and the total content of Na2O, K2O and Li2O is less than 1.00% by mass. 2. A glass fiber, characterized in that it is composed of the glass composition for glass fiber as described in claim 1. 3. A glass fiber fabric, characterized in that it comprises the glass fiber as described in claim 2. 4. A glass fiber reinforcing resin composition, characterized in that it comprises the glass fiber as described in claim 2. Claims 1 / 1 page 2 CN 121929914 A Glass composition for glass fiber, glass fiber, glass fiber fabric and glass fiber reinforcing resin composition

[0001] This application is a divisional application of the invention patent application filed on February 9, 2022, with application number 202280009045.8, PCT international application number PCT / JP2022 / 005085, entitled "Glass composition for glass fiber, glass fiber, glass fiber fabric and glass fiber reinforcing resin composition". Technical Field

[0002] The present invention relates to glass compositions for glass fiber, glass fiber, glass fiber fabric and glass fiber reinforcing resin composition. Background Art

[0003] Glass fibers are manufactured by the following process: molten glass (the melt of the glass composition for glass fibers) is produced by melting glass raw materials in a glass melting furnace to form a glass composition for glass fibers with a desired composition; the molten glass is ejected from a container (sleeve) having a nozzle plate with several to thousands of nozzle chips; and the molten glass is cooled and solidified by high-speed winding while being stretched (hereinafter, this operation is sometimes referred to as "spinning"). The sleeve is formed, for example, from a precious metal such as platinum.

[0004] Conventionally, glass fibers have been widely used in various applications because they can improve the strength of resin molded articles, which are used in the housings or accessories of electronic devices such as servers, smartphones, and laptops.

[0005] Typically, glass absorbs energy as heat from alternating current. Therefore, when the above-mentioned resin molded article is used in the housing or accessories of the above-mentioned electronic device, there is a problem that the resin molded article will generate heat.

[0006] Here, the dielectric loss energy absorbed by the glass is proportional to the dielectric constant and dielectric loss tangent determined by the composition and structure of the glass, and can be expressed by the following formula (A).

[0007] W=kfv2×ε1 / 2×tanδ …(A) Here, W represents the dielectric loss energy, k represents a constant, f represents the frequency, v2 represents the potential gradient, ε represents the dielectric constant, and tanδ represents the dielectric loss tangent. According to formula (A), the larger the dielectric constant and dielectric loss tangent, and the higher the frequency, the greater the dielectric loss, and therefore the greater the heat generated by the above-mentioned resin molded article.

[0008] In recent years, due to the increasing frequency of the alternating current used in the aforementioned electronic devices (f in the above formula (A)), in order to reduce dielectric loss energy, it is required that the glass fiber used in the housing or components of the aforementioned electronic devices have a lower dielectric constant and dielectric loss tangent. In particular, compared with the dielectric constant to the power of 1 / 2, the dielectric loss tangent has a greater impact on the above formula (A), therefore a low dielectric loss tangent is required.

[0009] In view of the above, the applicant has proposed a glass composition for glass fibers that has a low dielectric constant and a low dielectric loss tangent, suppresses phase separation, and further reduces viscosity at high temperatures. The glass composition for glass fibers contains SiO2 in the range of 52.0 to 59.5% by mass, B2O3 in the range of 17.5 to 25.5% by mass, Al2O3 in the range of 9.0 to 14.0% by mass, SrO in the range of 0.5 to 6.0% by mass, MgO in the range of 1.0 to 5.0% by mass, CaO in the range of 1.0 to 5.0% by mass, and F2 and Cl2 in the range of 0.1 to 2.5% by mass (see Patent Document 1).

[0010] Prior Art Document Specification 1 / 22 pages 3 CN 121929914 A Patent Document Patent Document 1: Japanese Patent No. 6468409 Summary of the Invention

[0011] Problem to be Solved by the Invention On the other hand, there is a particular need for a glass composition for glass fibers that can produce glass fibers with lower dielectric constant and dielectric loss tangent in the high frequency region of about 10 GHz. In order to achieve the above problem, it is considered to reduce the content of Al2O3 and alkaline earth metal oxides (CaO, MgO and SrO) in the glass composition for glass fibers relative to the total amount of the glass composition for glass fibers, thereby correspondingly increasing the content of SiO2 and B2O3.

[0012] However, in the above-mentioned glass composition for glass fibers, if the content of SiO2 and B2O3 relative to the total amount of the glass composition for glass fibers is increased to compensate for the content of Al2O3 and alkaline earth metal oxides, the following problems exist: the operating temperature range expressed as the difference between the 1000 poise temperature and the liquidus temperature becomes narrower, the manufacturability of the glass fibers decreases or the water resistance of the glass fibers deteriorates, foreign matter precipitated on the surface of the glass fibers due to the hydrolysis of the glass leads to the deterioration of dielectric properties, and the strength of the glass fibers is greatly reduced.

[0013] The present invention aims to eliminate the above problems and provides a glass composition for glass fibers that has a sufficient operating temperature range, and glass fibers with excellent water resistance and excellent dielectric properties (low dielectric constant and low dielectric loss tangent) in the high-frequency region can be obtained using the glass composition for glass fibers.

[0014] Means for Solving the Problem In order to achieve the above-mentioned objective, the glass composition for glass fibers of the present invention is characterized in that the glass composition for glass fibers contains: SiO2 in the range of 59.00 to 65.00% by mass, B2O3 in the range of 16.00 to 26.00% by mass, Al2O3 in the range of 7.00 to 14.00% by mass, CaO in the range of 0 to 5.00% by mass, MgO in the range of 0 to 4.00% by mass, SrO in the range of 0 to 6.00% by mass, TiO2 in the range of 0.10 to 5.00% by mass, and F2 and Cl2 in the range of 0 to 2.00% by mass, the content of P2O5 is less than 0.20% by mass, the total content of Na2O, K2O and Li2O is less than 1.00% by mass, and the content of TiO2 (by mass) is relative to the total content of CaO, MgO and SrO (by mass). The ratio (TiO2 / (CaO+MgO+SrO)) is in the range of 0.66~4.00, and the content (mass%) of SiO2 (SI) and the content (mass%) of Al2O3 (A) satisfy the following formula (1): 1.00≤1000×A / SI2≤4.65 …(1).

[0015] The glass composition for glass fiber of the present invention contains SiO2, B2O3, Al2O3, CaO, MgO, SrO, TiO2, F2, Cl2, P2O5, Na2O, K2O and Li2O within the above range. The ratio of the content of TiO2 (mass%) to the total content of CaO, MgO and SrO (mass%) (TiO2 / (CaO+MgO+SrO)) is in the range of 0.66 to 4.00. The content of SiO2 (mass%) SI and the content of Al2O3 (mass%) A satisfy the above formula (1). Therefore, the glass composition for glass fiber itself can have a sufficient operating temperature range, and glass fibers with excellent water resistance and excellent dielectric properties (low dielectric constant and low dielectric loss tangent) in the high frequency region can be obtained using this glass composition for glass fiber.

[0016] It should be noted that the glass fiber obtained using the glass composition for glass fiber of the present invention has a low dielectric constant, meaning that the dielectric constant is 4.2 or less at a measurement frequency of 10 GHz, and has a low dielectric loss tangent, meaning that the dielectric loss tangent is 0.0011 or less at a measurement frequency of 10 GHz.

[0017] In addition, the glass fiber obtained using the glass composition for glass fiber of the present invention exhibits excellent water resistance, meaning that when evaluated by the following water resistance evaluation method, the mass reduction rate is 2.0% or less, and almost no components of the glass fiber dissolve in water.

[0018] In the method for evaluating water resistance, firstly, glass raw materials are mixed in such a way that they will have a specified glass fiber composition after melting and solidification to obtain a glass batch. This glass batch is placed in a platinum crucible with a diameter of 80 mm and heated at 1550°C for 4 hours, and then further heated at 1650°C for 2 hours to melt it. Next, the homogeneous glass shavings obtained from the crucible are placed in a small cylindrical platinum sleeve with a circular nozzle at the bottom of the container and heated to a specified temperature to melt it. Then, the molten glass ejected from the nozzle is wound onto a stainless steel sleeve at a specified speed, thereby stretching the molten glass while cooling and solidifying it to obtain glass fibers with a circular cross-section and a fiber diameter of 13 μm. Next, about 1 g (test glass fiber) of the obtained glass fiber is collected from the sleeve, dried at 120°C for 1 hour, and the mass (mass before operation) is measured. Next, the glass fiber for testing was left to stand in 100 ml of distilled water at 80°C for 24 hours. The glass fiber was then obtained using a metal mesh with an opening of approximately 150 μm. After being washed with distilled water, the glass fiber was dried at 120°C for 1 hour, and its mass (post-operation mass) was measured.Then, based on the above-mentioned pre-operation mass and post-operation mass, the mass reduction rate (100 × (1 - (post-operation mass / pre-operation mass)))) is calculated.

[0019] In addition, the glass composition for glass fiber of the present invention having a sufficient operating temperature range means that the operating temperature range is 20°C or higher. It should be noted that the upper limit of the operating temperature range is not particularly limited, and the upper limit is, for example, 500°C or lower, preferably 450°C or lower, and more preferably 400°C or lower.

[0020] Furthermore, in the glass composition for glass fiber of the present invention, the content of SiO2 (mass%) SI, the content of B2O3 (mass%) B, the content of Al2O3 (mass%) A, the content of CaO (mass%) C, the content of MgO (mass%) M, the content of SrO (mass%) SR, the content of TiO2 (mass%) T, and the total content of F2 and Cl2 (mass%) F preferably satisfy the following formula (2), more preferably satisfy the following formula (3), further preferably satisfy the following formula (4), and particularly preferably satisfy the following formula (5).

[0021] 204.00≤Si×B2×T2 / [{C+(40.1 / 87.6)×SR-(40.1 / 24.3)×M-F}1 / 2×A3]≤ 422.40...(2) 244.00≤Si×B2×T2 / [{C+(40.1 / 87.6)×SR-(40.1 / 24.3)×M-F}1 / 2×A3]≤ 410.00…(3) 308.50≤Si×B2×T2 / [{C+(40.1 / 87.6)×SR-(40.1 / 24.3)×M-F}1 / 2×A3]≤ 400.50…(4) 339.60≤Si×B2×T2 / [{C+(40.1 / 87.6)×SR-(40.1 / 24.3)×M-F}1 / 2×A3]≤ 377.80 …(5) In addition, the present invention also relates to: glass fibers characterized by being composed of any of the above-described glass fiber compositions; glass fiber fabrics containing the glass fibers; and glass fiber reinforced resin compositions containing the glass fibers.

[0022] The glass fibers of the present invention can be manufactured, for example, by the following process: melting the above-described glass fiber compositions of the present invention to form a molten material, ejecting the obtained molten material from a sleeve having a nozzle plate having 1 to 8000 nozzle heads or holes, and cooling and solidifying the molten material while stretching it at high speed to form a fibrous shape. Therefore, the glass fibers of the present invention have the same glass composition as the above-described glass fiber compositions of the present invention. Instruction manual 3 / 22 pages 5 CN 121929914 A Detailed Description of Embodiments

[0023] Next, embodiments of the present invention will be described in more detail.

[0024] The glass composition for glass fiber in this embodiment contains: SiO2 in the range of 59.00 to 65.00% by mass relative to the total amount of the glass composition for glass fiber, B2O3 in the range of 16.00 to 26.00% by mass, Al2O3 in the range of 7.00 to 14.00% by mass, CaO in the range of 0 to 5.00% by mass, MgO in the range of 0 to 4.00% by mass, SrO in the range of 0 to 6.00% by mass, and 0.10 to The glass composition for glass fiber of this embodiment contains 5.00% by mass of TiO2 and a total of 0 to 2.00% by mass of F2 and Cl2, with a P2O5 content of less than 0.20% by mass, a total content of Na2O, K2O and Li2O of less than 1.00% by mass, and the ratio of the TiO2 content (by mass) to the total content (by mass) of CaO, MgO and SrO (TiO2 / (CaO+MgO+SrO)) is in the range of 0.66 to 4.00, and the SiO2 content (by mass) SI and the Al2O3 content (by mass) A satisfy the following formula (1).

[0025] 1.00≤1000×A / SI2≤4.65 …(1) The glass composition for glass fiber of this embodiment contains SiO2, B2O3, Al2O3, CaO, MgO, and The glass composition for glass fiber contains SrO, TiO2, F2, Cl2, P2O5, Na2O, K2O, and Li2O, and the ratio of the content (mass%) of TiO2 to the total content (mass%) of CaO, MgO, and SrO (TiO2 / (CaO+MgO+SrO)) is in the range of 0.66 to 4.00. The content (mass%) of SiO2 (SI) and the content (mass%) of Al2O3 (A) satisfy the above formula (1). Thus, a glass composition for glass fiber with a sufficient operating temperature range can be obtained, and glass fiber with excellent water resistance and excellent dielectric properties (low dielectric constant and low dielectric loss tangent) in the high frequency region can be obtained using this glass composition for glass fiber.

[0026] In the glass composition for glass fibers of this embodiment, if the content of SiO2 relative to the total amount of the glass composition for glass fibers is less than 59.00% by mass, the mechanical strength of the glass fibers obtained using this glass composition is significantly reduced, and the function of the glass fiber as a reinforcing material in the glass fiber reinforcing resin composition is impaired. In addition, the glass fibers are prone to deterioration in acidic environments. On the other hand, if the content of SiO2 relative to the total amount of the glass composition for glass fibers exceeds 65.00% by mass, the viscosity at high temperatures increases, thus increasing the melting temperature of the glass raw materials. From the viewpoint of manufacturing cost, this is not suitable for industrial glass fiber manufacturing.

[0027] In the glass composition for glass fibers of this embodiment, the content of SiO2 relative to the total amount of the glass composition for glass fibers is preferably in the range of 59.20 to 64.50% by mass, more preferably in the range of 59.30 to 64.00% by mass, further preferably in the range of 59.40 to 63.50% by mass, particularly preferably in the range of 59.50 to 63.00% by mass, extremely preferably in the range of 59.60 to 62.80% by mass, and most preferably in the range of 60.10 to 62.60% by mass.

[0028] In the glass composition for glass fibers of this embodiment, if the content of B2O3 relative to the total amount of the glass composition for glass fibers is less than 16.00% by mass, the dielectric loss tangent of the glass fibers obtained using this glass composition for glass fibers cannot be sufficiently reduced. On the other hand, if the content of B2O3 relative to the total amount of the glass composition for glass fibers exceeds 26.00% by mass, the glass fibers obtained using this glass composition for glass fibers will undergo phase separation, and the chemical durability of the glass fibers may decrease.

[0029] In the glass composition for glass fibers of this embodiment, the content of B2O3 relative to the total amount of the glass composition for glass fibers is preferably in the range of 18.00 to 24.90% by mass, more preferably in the range of 19.00 to 24.50% by mass, further preferably in the range of 19.60 to 24.00% by mass, particularly preferably in the range of 20.10 to 23.50% by mass, and most preferably in the range of 20.50 to 23.00% by mass.

[0030] In the glass composition for glass fibers of this embodiment, if the content of Al2O3 relative to the total amount of the glass composition for glass fibers is less than 7.00% by mass, the glass fibers obtained using this glass composition for glass fibers will undergo phase separation, which may lead to a decrease in the chemical durability of the glass fibers. On the other hand, if the content of Al2O3 relative to the total amount of glass composition for glass fiber exceeds 14.00% by mass, the dielectric loss tangent of the glass fiber obtained using this glass composition for glass fiber cannot be sufficiently reduced.

[0031] In the glass composition for glass fiber of this embodiment, the content of Al2O3 relative to the total amount of glass composition for glass fiber is preferably in the range of 7.20 to 13.50% by mass, more preferably in the range of 7.40 to 13.00% by mass, further preferably in the range of 7.60 to 12.50% by mass, particularly preferably in the range of 7.80 to 12.00% by mass, extremely preferably in the range of 8.00 to 11.80% by mass, and most preferably in the range of 8.20 to 9.90% by mass.

[0032] In the glass composition for glass fibers of this embodiment, if the content of CaO relative to the total amount of the glass composition for glass fibers exceeds 5.00% by mass, the dielectric loss tangent of the glass fibers obtained using this glass composition for glass fibers cannot be sufficiently reduced.

[0033] In the glass composition for glass fibers of this embodiment, the content of CaO relative to the total amount of the glass composition for glass fibers is preferably in the range of 0.60 to 4.80% by mass, more preferably in the range of 1.10 to 4.60% by mass, further preferably in the range of 1.60 to 4.40% by mass, particularly preferably in the range of 1.80 to 4.20% by mass, especially preferably in the range of 2.00 to 4.00% by mass, and most preferably in the range of 2.10 to 3.60% by mass.

[0034] In the glass composition for glass fibers of this embodiment, if the content of MgO relative to the total amount of the glass composition for glass fibers exceeds 4.00% by mass, ripples are generated in the melt of the glass composition for glass fibers, which may lead to easy breakage of the glass fibers during spinning. Furthermore, it may lead to a deterioration in the water resistance of the glass fibers obtained using this glass fiber composition.

[0035] In the glass fiber composition of this embodiment, the content of MgO relative to the total amount of the glass fiber composition is preferably less than 3.00% by mass, more preferably less than 2.00% by mass, further preferably less than 1.50% by mass, particularly preferably less than 1.00% by mass, especially preferably less than 0.95% by mass, and most preferably less than 0.50% by mass.

[0036] In the glass fiber composition of this embodiment, if the content of SrO relative to the total amount of the glass fiber composition exceeds 6.00% by mass, the dielectric properties of the glass fibers obtained using this glass fiber composition deteriorate and cannot meet the target dielectric properties.

[0037] In the glass composition for glass fiber of this embodiment, the content of SrO relative to the total amount of the glass composition for glass fiber is preferably less than 4.00% by mass, more preferably less than 3.00% by mass, further preferably less than 2.00% by mass, particularly preferably less than 1.00% by mass, extremely preferably less than 0.50% by mass, and most preferably less than 0.45% by mass.

[0038] In the glass composition for glass fiber of this embodiment, when the content of TiO2 relative to the total amount of the glass composition for glass fiber is less than 0.10% by mass, the viscosity at high temperature increases, thus increasing the melting temperature of the glass raw materials. From the viewpoint of manufacturing cost, this is not suitable for industrial glass fiber manufacturing.On the other hand, when the content of TiO2 relative to the total amount of the glass composition for glass fiber exceeds 5.00% by mass, the dielectric loss tangent of the glass fiber obtained using the glass composition for glass fiber cannot be sufficiently reduced. In addition, due to the significant increase in the liquidus temperature of the glass composition for glass fiber, stable glass fiber manufacturing is not possible.

[0039] In the glass composition for glass fiber of this embodiment, the content of TiO2 relative to the total amount of the glass composition for glass fiber is preferably in the range of 0.60 to 4.90% by mass, more preferably in the range of 1.60 to 4.70% by mass, further preferably in the range of 2.10 to 4.60% by mass, particularly preferably in the range of 2.50 to 4.50% by mass, and most preferably in the range of 2.80 to 4.40% by mass.

[0040] In the glass composition for glass fibers of this embodiment, if the total content of F2 and Cl2 relative to the total amount of the glass composition for glass fibers (page 5 / 22, CN 121929914 A) exceeds 2.00% by mass, the chemical durability of the glass fibers obtained using this glass composition for glass fibers is reduced.

[0041] In the glass composition for glass fibers of this embodiment, the total content of F2 and Cl2 relative to the total amount of the glass composition for glass fibers is preferably in the range of 0.10 to 1.80% by mass, more preferably in the range of 0.30 to 1.60% by mass, and even more preferably in the range of 0.50 to 1.50% by mass.

[0042] In the glass composition for glass fibers of this embodiment, if the content of P2O5 relative to the total amount of the glass composition for glass fibers exceeds 0.20% by mass and the content of SiO2 is within the above range, the presence of P2O5 does not help improve the dielectric properties of the glass fibers obtained using the glass composition for glass fibers. On the other hand, it cannot suppress the phase separation of the glass fibers, and the chemical durability of the glass fibers deteriorates.

[0043] In the glass composition for glass fibers of this embodiment, the content of P2O5 relative to the total amount of the glass composition for glass fibers is preferably less than 0.10% by mass, and more preferably less than 0.05% by mass.

[0044] Furthermore, in the glass composition for glass fibers of this embodiment, if the combined content of Na2O, K2O, and Li2O relative to the total amount of the glass composition for glass fibers exceeds 1.00% by mass, the dielectric properties of the glass fibers obtained using the glass composition for glass fibers deteriorate significantly and cannot meet the target dielectric properties.

[0045] In the glass composition for glass fibers of this embodiment, the total content of Na2O, K2O and Li2O relative to the total amount of the glass composition for glass fibers is preferably less than 0.80% by mass, more preferably less than 0.50% by mass, further preferably less than 0.20% by mass, particularly preferably less than 0.10% by mass, and most preferably less than 0.05% by mass.

[0046] In the glass composition for glass fibers of this embodiment, if the ratio of the content of TiO2 (by mass) to the total content of CaO, MgO and SrO (by mass) (TiO2 / (CaO+MgO+SrO)) is less than 0.66, the deterioration of the dielectric loss tangent caused by the presence of alkaline earth metal oxides cannot be sufficiently suppressed. Therefore, the dielectric loss tangent of the glass fiber obtained using the glass composition for glass fibers cannot be sufficiently reduced, and the water resistance of the glass fiber may deteriorate. If the above ratio exceeds 4.00, it is impossible to suppress the generation of ripples in the glass. In addition, the liquid phase temperature increases significantly, making it impossible to manufacture stable glass fibers.

[0047] In the glass composition for glass fibers of this embodiment, the ratio of the content of TiO2 (mass%) to the total content of CaO, MgO and SrO (mass%) (TiO2 / (CaO+MgO+SrO)) is preferably in the range of 0.67 to 2.15, more preferably in the range of 0.85 to 2.00, further preferably in the range of 0.90 to 1.80, particularly preferably in the range of 0.95 to 1.70, and most preferably in the range of 0.98 to 1.60.

[0048] Here, the ratio of the TiO2 content (mass%) to the total content (mass%) of CaO, MgO and SrO can be inferred to reflect a balance between the deterioration of the glass fiber manufacturing stability and the decrease of the dielectric loss tangent caused by the increase in the liquid phase temperature of the glass composition for glass fibers and the improvement of the glass fiber manufacturing stability and the deterioration of the dielectric loss tangent and water resistance caused by the decrease in the liquid phase temperature of the glass composition for glass fibers. The glass composition for glass fibers contains TiO2 as an intermediate oxide, which causes the increase in the liquid phase temperature of the glass composition for glass fibers; the glass composition for glass fibers contains oxides of alkaline earth metals as mesh-modifying oxides, which causes the decrease in the liquid phase temperature of the glass composition for glass fibers.

[0049] In the glass composition for glass fibers of this embodiment, if the value of the above formula (1) is less than 1.00, it is impossible to suppress the deterioration of the water resistance and the deterioration of the manufacturability of the glass fibers obtained using the glass composition for glass fibers. The deterioration of the manufacturability of the glass fibers is caused by the increase in the manufacturing cost of the glass fibers due to the increased viscosity of the glass composition for glass fibers at high temperatures, and the increase in the number of burrs generated during the manufacturing process of the glass fibers. Specification 6 / 22 pages 8 CN 121929914 A On the other hand, if the value of the above formula (1) exceeds 4.65, it is impossible to suppress the deterioration of the manufacturing stability of the glass fibers due to the increase in the liquidus temperature of the glass composition for glass fibers, and the deterioration of the dielectric properties of the glass fibers obtained using the glass composition for glass fibers.

[0050] In the glass composition for glass fiber of this embodiment, the value of the above formula (1) is preferably in the range of 1.50 to 4.50, more preferably in the range of 1.80 to 4.20, even more preferably in the range of 2.00 to 4.00, particularly preferably in the range of 2.05 to 3.80, especially preferably in the range of 2.10 to 3.60, and most preferably in the range of 2.11 to 3.35.

[0051] Here, the above formula (1) tends to have the following tendency: the higher the Al2O3 content A, the lower the viscosity of the glass composition for glass fiber at high temperature, thereby reducing the manufacturing cost of glass fiber. However, if this value becomes too high, it will promote the formation of mullite-based crystals, and there is a tendency to be unable to suppress the deterioration of the glass fiber manufacturing stability caused by the rise in the liquid phase temperature of the glass composition for glass fiber, and the deterioration of the dielectric properties of the glass fiber obtained using the glass composition for glass fiber. On the other hand, there is a tendency that the lower the value, the better the stability of glass fiber manufacturing and the dielectric properties of the glass fiber composition, which are associated with a decrease in the liquidus temperature of the glass fiber composition. However, if the value is too low, the water resistance of the glass fiber obtained using the glass fiber composition deteriorates, and the fiber strength decreases, making it easier to generate fuzz that hinders glass fiber manufacturing. Furthermore, there is a tendency that the higher the SiO2 content (SI), the better the dielectric properties of the glass fiber obtained using the glass fiber composition; however, the viscosity of the glass fiber composition increases at high temperatures, leading to increased glass fiber manufacturing costs. On the other hand, there is a tendency that the lower the value, the lower the viscosity of the glass fiber composition at high temperatures, thereby reducing glass fiber manufacturing costs; however, the dielectric properties of the glass fiber obtained using the glass fiber composition deteriorate.Therefore, it can be inferred that the above formula (1) is a balance between the comprehensive glass fiber manufacturability and the dielectric properties obtained by the glass fiber composition. It should be noted that the tendency to generate the above-mentioned burrs will also hinder the processing of glass fibers into glass fiber products (e.g., glass fiber fabrics, chopped strands, rovings).

[0052] In addition, in the glass fiber composition of this embodiment, the content of SiO2 (mass%) SI, the content of B2O3 (mass%) B, the content of Al2O3 (mass%) A, the content of CaO (mass%) C, the content of MgO (mass%) M, the content of SrO (mass%) SR, the content of TiO2 (mass%) T, and the total content of F2 and Cl2 (mass%) F preferably satisfy the following formula (2), more preferably satisfy the following formula (3), further preferably satisfy the following formula (4), and particularly preferably satisfy the following formula (5).

[0053] 204.00≤SI×B2×T2 / [{C+(40.1 / 87.6)×SR-(40.1 / 24.3)×M-F}1 / 2×A3]≤ 422.40...(2), 244.00≤SI×B2×T2 / [{C+(40.1 / 87.6)×SR-(40.1 / 24.3)×M-F}1 / 2×A3]≤ 410.00…(3), 308.50≤SI×B2×T2 / [{C+(40.1 / 87.6)×SR-(40.1 / 24.3)×M-F}1 / 2×A3]≤ 400.50…(4), 339.60≤SI×B2×T2 / [{C+(40.1 / 87.6)×SR-(40.1 / 24.3)×M-F}1 / 2×A3]≤ 377.80 …(5)。

[0054] In the glass composition for glass fiber of this embodiment, by making SI, B, A, C, M, SR, T and F satisfy formula (2), the glass composition for glass fiber itself has a sufficient operating temperature range, and glass fiber with excellent water resistance and excellent dielectric properties in the high frequency region can be obtained by using the glass composition for glass fiber. Instruction manual 7 / 22 pages 9 CN 121929914 A

[0055] In addition, in the glass composition for glass fiber in this embodiment, by making the above SI, B, A, C, M, SR, T and F satisfy formula (3), the glass composition for glass fiber itself has a sufficient operating temperature range, and glass fiber with excellent water resistance and better dielectric properties in the high frequency region can be obtained by using the glass composition for glass fiber.Here, the superior dielectric properties of the glass fiber refer to a dielectric constant of 4.1 or less and a dielectric loss tangent of 0.0010 or less at a measurement frequency of 10 GHz.

[0056] Furthermore, in the glass composition for glass fiber of this embodiment, by making the above SI, B, A, C, M, SR, T and F satisfy formula (4), the glass composition for glass fiber itself has an excellent operating temperature range of 120°C or more, and glass fibers with excellent water resistance and excellent dielectric properties in the high-frequency region can be obtained using this glass composition for glass fiber.

[0057] Furthermore, in the glass composition for glass fiber of this embodiment, by making the above SI, B, A, C, M, SR, T and F satisfy formula (5), the glass composition for glass fiber itself has an even superior operating temperature range of 200°C or more, and glass fibers with excellent water resistance and extremely excellent dielectric properties in the high-frequency region can be obtained using this glass composition for glass fiber. Here, the excellent dielectric properties of the aforementioned glass fiber refer to a dielectric constant of 4.0 or less and a dielectric loss tangent of less than 0.0010 at a measurement frequency of 10 GHz.

[0058] In addition, in the glass composition for glass fiber of this embodiment, the ratio of the content of MgO (mass%) to the total content of CaO and SrO (mass%) (MgO / (CaO+SrO)) is, for example, less than 0.60. As a result, it is possible to suppress phase separation caused by MgO in the glass fiber obtained using the glass composition for glass fiber, and to reduce the viscosity of the glass composition for glass fiber at high temperatures. Furthermore, by lowering the liquidus temperature of the glass composition for glass fiber, it is possible to improve the overall glass fiber manufacturability of the glass composition for glass fiber. In the glass composition for glass fiber of this embodiment, the ratio of the content of MgO (mass%) to the total content of CaO and SrO (mass%) (MgO / (CaO+SrO)) is preferably less than 0.40, more preferably less than 0.30, further preferably less than 0.20, particularly preferably less than 0.10, and most preferably less than 0.05.

[0059] In addition, in the glass composition for glass fiber of this embodiment, the ratio of the content of TiO2 (mass%) to the content of Al2O3 (mass%) (TiO2 / Al2O3) is, for example, in the range of 0.24 to 0.72. Therefore, it is possible to suppress the rise in liquid phase temperature of the glass composition for glass fiber caused by the crystallization promoted by TiO2, while taking into account the effect of reducing the dielectric loss tangent brought about by the presence of TiO2 and the effect of improving water resistance brought about by the presence of Al2O3.In the glass composition for glass fiber of this embodiment, the ratio of TiO2 content (mass%) to Al2O3 content (mass%) (TiO2 / Al2O3) is preferably in the range of 0.28 to 0.56, more preferably in the range of 0.29 to 0.50, further preferably in the range of 0.30 to 0.45, and most preferably in the range of 0.35 to 0.44.

[0060] In addition, in the glass composition for glass fiber of this embodiment, by making the content (mass%) P of B, A, C, M, SR, T, F and P2O5 satisfy the following formula (6), the glass composition for glass fiber itself has a sufficient operating temperature range, and glass fibers with excellent water resistance and excellent dielectric properties in the high frequency region can be obtained using this glass composition for glass fiber.

[0061] 1.08≤{2×(0.72×C+M+0.39×SR)-1.06×F}×(B / 1.2+A / 1.7+P / 1.3+T / 4.7) / (1.37×B / 1.2+1.77×A / 1.7+1.63×P / 1.3+1.96×T / 4.7)≤2.34 …(6)。

[0062] In the glass composition for glass fiber of this embodiment, B, A, C, M, SR, T, F and P are preferably satisfied by the following formula (7), more preferably satisfied by the following formula (8), and particularly preferably satisfied by the following formula (9).

[0063] 1.47≤{2×(0.72×C+M+0.39×SR)-1.06×F}×(B / 1.2+A / 1.7+P / 1.3+T / 4.7) / (1.37×B / 1.2+1.77×A / 1.7+1.63×P / 1.3+1.96×T / 4.7)≤2.33 …(7), 1.47≤{2×(0.72×C+M+0.39×SR)-1.06×F}×(B / 1.2+A / 1.7+P / 1.3+T / 4.7) / (1.37×B / 1.2+1.77×A / 1.7+1.63×P / 1.3+1.96×T / 4.7)≤2.32…(8), 2.14≤{2×(0.72×C+M+0.39×SR)-1.06×F}×(B / 1.2+A / 1.7+P / 1.3+T / 4.7) / (1.37×B / 1.2+1.77×A / 1.7+1.63×P / 1.3+1.96×T / 4.7)≤2.32…(9).

[0064] In the glass composition for glass fiber of this embodiment, by making B, A, C, M, SR, T, F and P satisfy the above formula (7), the glass composition for glass fiber itself has a sufficient operating temperature range, and glass fibers with excellent water resistance and superior dielectric properties in the high-frequency region can be obtained using this glass composition for glass fiber.

[0065] In addition, in the glass composition for glass fiber of this embodiment, by making B, A, C, M, SR, T, F and P satisfy the above formula (8), the glass composition for glass fiber itself has an excellent operating temperature range of 120°C or more, and glass fibers with excellent water resistance and superior dielectric properties in the high-frequency region can be obtained using this glass composition for glass fiber.

[0066] Furthermore, in the glass composition for glass fibers of this embodiment, by making B, A, C, M, SR, T, F, and P satisfy the above formula (9), the glass composition for glass fibers itself has a more superior operating temperature range of 200°C or higher, and glass fibers with excellent water resistance and extremely excellent dielectric properties in the high-frequency region can be obtained using this glass composition for glass fibers.

[0067] In addition, the glass composition for glass fibers of this embodiment may contain ZnO in the range of 0 to 3.00% by mass relative to the total amount of the glass composition for glass fibers. When the glass composition for glass fibers of this embodiment contains ZnO, if the ZnO content exceeds 3.00% by mass, devitrification is easily generated, making it impossible to manufacture stable glass fibers.

[0068] When the glass composition for glass fiber in this embodiment contains ZnO, the content of ZnO relative to the total amount of the glass composition for glass fiber is preferably in the range of 2.50% by mass or less, more preferably in the range of 1.50% by mass or less, and even more preferably in the range of 0.50% by mass or less.

[0069] In addition, the glass composition for glass fiber in this embodiment may contain MnO2 in the range of 0 to 3.00% by mass relative to the total amount of the glass composition for glass fiber. When the glass composition for glass fiber in this embodiment contains MnO2, if the content of MnO2 exceeds 3.00% by mass, the dielectric properties deteriorate, and the desired dielectric properties cannot be obtained.

[0070] When the glass composition for glass fiber in this embodiment contains MnO2, the content of MnO2 relative to the total amount of the glass composition for glass fiber is preferably 2.50% by mass or less, more preferably 1.50% by mass or less, and even more preferably 0.50% by mass or less.

[0071] In addition, the glass composition for glass fiber in this embodiment may contain Fe2O3 in the range of 0% by mass or more and 1.00% by mass or less relative to the total amount of the glass composition for glass fiber.In the case where the glass composition for glass fiber in this embodiment contains Fe2O3, from the viewpoint of suppressing the generation of bubbles in the glass fiber, it is effective to set the content of Fe2O3 to a range of 0.10% by mass or more and 0.60% by mass or less.

[0072] In addition, the glass composition for glass fiber in this embodiment may contain SnO2 in the range of 0% by mass or more and 1.00% by mass or less relative to the total amount of the glass composition for glass fiber. In the case where the glass composition for glass fiber in this embodiment contains SnO2, from the viewpoint of suppressing the generation of bubbles in the glass fiber, it is effective to set the content of SnO2 to a range of 0.10% by mass or more and 0.60% by mass or less.

[0073] In addition, in the glass composition for glass fiber in this embodiment, ZrO2 may also be contained as long as the content of ZrO2 relative to the total amount of the glass composition for glass fiber is less than 0.50% by mass. If the content of ZrO2 relative to the total amount of the glass composition for glass fiber is 0.50% by mass or more, devitrification is easily generated, making stable glass fiber manufacturing impossible.

[0074] In the case where the glass composition for glass fiber in this embodiment contains ZrO2, the content of ZrO2 relative to the total amount of the glass composition for glass fiber is preferably less than 0.45% by mass, more preferably less than 0.40% by mass, further preferably less than 0.20% by mass, particularly preferably less than 0.10% by mass, and most preferably less than 0.05% by mass.

[0075] In addition, in the glass composition for glass fiber in this embodiment, as long as the content of Cr2O3 relative to the total amount of the glass composition for glass fiber is less than 0.05% by mass, the glass composition for glass fiber in this embodiment may also contain Cr2O3. If the content of Cr2O3 relative to the total amount of the glass composition for glass fiber is 0.05% by mass or more, devitrification is easily generated, making stable glass fiber manufacturing impossible.

[0076] In addition, in the glass composition for glass fiber in this embodiment, as impurities derived from raw materials, oxides of Ba, Co, Ni, Cu, Mo, W, Ce, Y, La, Bi, Gd, Pr, Sc or Yb may be contained in a total content of less than 1.00% by mass relative to the total amount of the glass composition for glass fiber.Especially when the glass composition for glass fiber in this embodiment contains BaO, CeO2, Y2O3, La2O3, Bi2O3, Gd2O3, Pr2O3, Sc2O3 or Yb2O3 as impurities, the content of each is preferably less than 0.40% by mass, more preferably less than 0.20% by mass, further preferably less than 0.10% by mass, particularly preferably less than 0.05% by mass, and most preferably less than 0.01% by mass.

[0077] It should be noted that, regarding the content of each of the above components in the glass composition for glass fiber in this embodiment, Li, as a light element, can be determined using an ICP emission spectrophotometer, and other elements can be determined using a wavelength dispersive X-ray fluorescence analyzer.

[0078] The determination method is as follows: First, glass batch (glass batch prepared by mixing glass raw materials) or glass fiber (in the case where organic matter is attached to the surface of the glass fiber, or in the case where the glass fiber is mainly contained in organic matter (resin) as a reinforcing material, for example, it is heated in a muffle furnace at 300-650°C for about 0.5-24 hours to remove the organic matter before use) is placed in a platinum crucible. When glass batch is used, it is held at 1550°C for 4 hours in an electric furnace, and then held at 1650°C for 2 hours while stirring to melt it; when glass fiber is used, it is held at 1550°C for 6 hours in an electric furnace while stirring to melt it, thereby obtaining homogeneous molten glass. Next, the obtained molten glass is poured onto a carbon plate to form glass shavings, which are then crushed and pulverized to form glass powder. After the glass powder obtained above is heated and decomposed with acid, Li, as a light element, is quantitatively analyzed using an ICP-based luminescence spectrophotometer. After the glass powder is formed into a disc shape using a press, other elements are quantitatively analyzed using a wavelength dispersive fluorescence X-ray analyzer. Specifically, the quantitative analysis using the wavelength dispersive fluorescence X-ray analyzer is based on the results determined by the basic parameter method to prepare a standard curve sample, and the analysis is performed using the standard curve method. It should be noted that the content of each component in the calibration curve sample can be quantitatively analyzed using an ICP emission spectrophotometer. The content and total amount of each component can be calculated by oxide conversion of these quantitative analysis results, and the content rate of each component can be determined based on these values.

[0079] The glass composition for glass fiber of this embodiment can be obtained by melting and solidifying a glass raw material (glass batch) that will become the above composition after melting and solidification, and then cooling and solidifying it.

[0080] When forming the glass fiber of this embodiment using the glass composition for glass fiber of this embodiment, firstly, the glass raw material prepared in the above manner is supplied to a glass melting furnace and melted at a temperature in the temperature range of 1000 poise or higher, specifically in the range of 1400°C to 1700°C. Then, molten glass melted to the specified temperature is ejected from 1 to 8000 nozzles or holes controlled to a specified temperature, and is cooled while being stretched by high-speed winding, and is solidified to form glass fiber.

[0081] Here, the glass monofiber (glass filament) ejected from one nozzle or hole and cooled and solidified generally has a circular cross-sectional shape and a diameter in the range of 3.0 to 35.0 μm. In applications requiring low dielectric properties, the glass filaments described above preferably have a diameter in the range of 3.0 to 6.0 μm, and more preferably a diameter in the range of 3.0 to 4.5 μm. On the other hand, when the nozzle head has a non-circular shape and has a protrusion or cut for quenching the molten glass, by controlling the temperature conditions, glass filaments with a non-circular (e.g., elliptical, oblong) cross-sectional shape can be obtained. When the glass filaments have an elliptical or oblong cross-sectional shape, the ratio of the major axis to the minor axis of the cross-sectional shape (major axis / minor axis) is, for example, in the range of 2.0 to 10.0, and the fiber diameter when the cross-sectional area is converted to a perfect circle (converted fiber diameter) is in the range of 3.0 to 35.0 μm.

[0082] The glass fibers of this embodiment are generally in the shape of a glass fiber bundle (glass filament) formed by bundling 10 to 8000 of the above-mentioned glass filaments, and have a weight in the range of 1 to 10000 tex (g / km). It should be noted that glass filaments ejected from multiple nozzles or orifices may sometimes be bundled into a single glass fiber bundle, and sometimes into multiple glass fiber bundles.

[0083] The glass fiber of this embodiment can take various forms, such as yarn, fabric, braided fabric, nonwoven fabric (including chopped strand mat, multi-axis nonwoven fabric), chopped strands, roving, powder, etc., obtained by further processing the above-mentioned glass filaments.

[0084] With the aim of improving the bundleability of glass filaments, improving the adhesion between glass fiber and resin, and improving the uniform dispersion of glass fiber in mixtures of glass fiber and resin or inorganic materials, the surface of the glass fiber of this embodiment can be coated with an organic material. Examples of such organic materials include: starch, polyurethane resin, epoxy resin, vinyl acetate resin, acrylic resin, modified polypropylene (especially carboxylic acid modified polypropylene), copolymers of (poly)carboxylic acid (especially maleic acid) and unsaturated monomers, etc.In addition to these resins, the glass fibers of this embodiment can also be coated with a resin composition containing silane coupling agents, lubricants, surfactants, etc. Alternatively, the glass fibers of this embodiment may not contain the aforementioned resins, but may be coated with a treatment agent composition containing silane coupling agents, surfactants, etc. Based on the mass of the glass fibers of this embodiment in their uncoated state by the resin composition or treatment agent composition, such resin compositions or treatment agent compositions coat the glass fibers at a ratio ranging from 0.03% to 2.0% by mass. It should be noted that coating the glass fibers with organic matter can be performed, for example, by applying a resin solution or resin composition solution to the glass fibers using a known method such as a roller coater during the glass fiber manufacturing process, and then drying the glass fibers coated with the resin solution or resin composition solution. Alternatively, coating the glass fibers with organic matter can also be performed, for example, by immersing the glass fibers of this embodiment in a fabric form into a treatment agent composition solution, and then drying the glass fibers coated with the treatment agent composition.

[0085] Here, examples of silane coupling agents include: aminosilanes, chlorosilanes, epoxysilanes, mercaptosilanes, vinylsilanes, and (meth)acrylate silanes.

[0086] Examples of aminosilanes include: γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-N'-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and γ-anilinepropyltrimethoxysilane.

[0087] Examples of chlorosilanes include γ-chloropropyltrimethoxysilane.

[0088] Examples of epoxy silanes include (β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-epoxypropoxypropyltrimethoxysilane, etc. (See specification 11 / 22 pages 13 CN 121929914 A)

[0089] Examples of mercaptosilanes include γ-mercaptotrimethoxysilane, etc.

[0090] Examples of vinyl silanes include vinyltrimethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane.

[0091] Examples of (meth)acrylate silanes include γ-methacryloyloxypropyltrimethoxysilane, etc.

[0092] In this embodiment, the above-mentioned silane coupling agents can be used alone, or two or more of the above-mentioned silane coupling agents can be used in combination.

[0093] Examples of lubricants include: modified silicone oils, animal oils and their hydrogenated derivatives, vegetable oils and their hydrogenated derivatives, animal waxes, vegetable waxes, mineral waxes, condensates of higher saturated fatty acids and higher saturated alcohols, polyethyleneimine, polyalkyl polyamine alkyl linolenic acid derivatives, fatty acid amides, and quaternary ammonium salts.

[0094] Examples of animal fats include tallow.

[0095] Examples of vegetable oils include soybean oil, coconut oil, rapeseed oil, palm oil, and castor oil.

[0096] Examples of animal waxes include beeswax and wool.

[0097] Examples of vegetable waxes include candelilla wax and carnauba wax.

[0098] Examples of mineral waxes include paraffin wax and lignite wax.

[0099] Examples of stearates, such as lauryl stearate, are condensates of higher saturated fatty acids and higher saturated alcohols.

[0100] Examples of fatty acid amides include dehydration condensates of polyvinylpolyamines such as diethylenetriamine, triethylenetetramine, and tetraethylenepentamine with fatty acids such as lauric acid, myristic acid, palmitic acid, and stearic acid.

[0101] Examples of quaternary ammonium salts include alkyltrimethylammonium salts such as lauryltrimethylammonium chloride.

[0102] In this embodiment, the above-mentioned lubricant can be used alone, or two or more of the above-mentioned lubricants can be used in combination.

[0103] Examples of surfactants include nonionic surfactants, cationic surfactants, anionic surfactants, and amphoteric surfactants. In this embodiment, the above-mentioned surfactants can be used alone, or two or more of the above-mentioned surfactants can be used in combination.

[0104] Examples of nonionic surfactants include ethylene oxide propylene alkyl ethers, polyoxyethylene alkyl ethers, polyoxyethylene-polyoxypropylene-block copolymers, alkyl polyoxyethylene-polyoxypropylene-block copolymer ethers, polyoxyethylene fatty acid esters, polyoxyethylene fatty acid monoesters, polyoxyethylene fatty acid diesters, polyoxyethylene sorbitan fatty acid esters, glycerol fatty acid ester ethylene oxide adducts, polyoxyethylene stearyl ethers, hydrogenated castor oil ethylene oxide adducts, alkylamine ethylene oxide adducts, fatty acid amide ethylene oxide adducts, glycerol fatty acid esters, polyglycerol fatty acid esters, pentaerythritol fatty acid esters, sorbitol fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, polyol alkyl ethers, fatty acid alkanolamides, acetylenol, ethylene oxide adducts of acetylenol, and ethylene oxide adducts of acetylenol.

[0105] Examples of cationic surfactants include: alkyl dimethyl benzyl ammonium chloride, alkyl trimethyl ammonium chloride, alkyl dimethyl ethyl ammonium ethyl sulfate, higher alkylamine salts (acetate or hydrochloride, etc.), ethylene oxide adducts of higher alkylamines, condensates of higher fatty acids and polyalkylene polyamines, ester salts of higher fatty acids and alkanolamines, salts of higher fatty acid amides, imidazoline-type cationic surfactants, and alkylpyridine salts.

[0106] Examples of anionic surfactants include higher alcohol sulfates, higher alkyl ether sulfates, α-olefin sulfates, alkylbenzene sulfonates, α-olefin sulfonates, reaction products of fatty acid halides and N-methyl taurine, dialkyl sulfosuccinates, higher alcohol phosphates, and phosphates of higher alcohol ethylene oxide adducts.

[0107] Examples of amphoteric surfactants include amino acid-type amphoteric surfactants such as alkali metal salts of alkylaminopropionates (see page 12 / 22, CN 121929914 A), betaine-type amphoteric surfactants such as alkyl dimethyl betaine, and imidazoline-type amphoteric surfactants.

[0108] The glass fiber fabric of this embodiment includes the glass fiber of this embodiment described above. Specifically, the glass fiber fabric of this embodiment can be woven by using a known loom as at least part of the warp or weft yarns. Examples of the aforementioned looms include: air-jet looms, water-jet looms, shuttle looms, rapier looms, etc. Furthermore, examples of weaving methods for the aforementioned looms include plain weave, satin weave, square weave, twill weave, etc., and from the viewpoint of manufacturing efficiency, plain weave is preferred. The glass fiber fabric of this embodiment preferably uses the aforementioned glass fiber of this embodiment as both warp and weft yarns.

[0109] In the glass fiber fabric of this embodiment, it is preferable that the aforementioned glass fiber of this embodiment is a bundle of 35 to 400 glass filaments with a diameter in the range of 3.0 to 9.0 μm, to which a twist in the range of 0 to 1.0 times / 25 mm is applied, with a mass in the range of 0.9 to 69.0 tex (g / km).

[0110] In the glass fiber fabric of this embodiment, when the aforementioned glass fiber of this embodiment is used as warp or weft, it is preferable that the warp yarn density is in the range of 40 to 120 threads / 25 mm and the weft yarn density is in the range of 40 to 120 threads / 25 mm.

[0111] The glass fiber fabric of this embodiment may also undergo degreasing treatment, surface treatment, and fiber opening treatment after weaving.

[0112] As a degreasing treatment, the following treatment can be cited: placing the glass fiber fabric in a heating furnace with an atmosphere temperature in the range of 350°C to 400°C for a period of 40 to 80 hours, and performing a heat decomposition treatment on the organic matter attached to the glass fiber.

[0113] As a surface treatment, the following treatment can be cited: impregnating the glass fiber fabric in a solution containing the above-mentioned silane coupling agent or a solution containing the above-mentioned silane coupling agent and the above-mentioned surfactant, and after removing excess water, heating and drying at a temperature range of 80 to 180°C for a period of 1 to 30 minutes.

[0114] As a fiber-opening process, examples include the following: fiber opening using water pressure while applying a tension of 30 to 200 N to the warp yarns of the glass fiber fabric; fiber opening using high-frequency vibration with a liquid as the medium; fiber opening using fluid pressure with surface pressure; and fiber opening using pressure from rollers, etc., to widen the line width of the warp and weft yarns.

[0115] The glass fiber fabric of this embodiment preferably has a unit area mass in the range of 7.0 to 190.0 g / m2 and a thickness in the range of 8.0 to 200.0 μm.

[0116] The yarn width of the warp yarns of the glass fiber fabric of this embodiment is preferably in the range of 110 to 600 μm, and the yarn width of the weft yarns is preferably in the range of 110 to 600 μm.

[0117] The glass fiber fabric of this embodiment may also have a surface treatment layer containing the above-mentioned silane coupling agent or a surface treatment layer containing the above-mentioned silane coupling agent and the above-mentioned surfactant. In the case where the glass fiber fabric of this embodiment includes the surface treatment layer, the surface treatment layer may, for example, have a mass percentage ranging from 0.03% to 1.50% by mass relative to the total amount of the glass fiber fabric including the surface treatment layer.

[0118] The glass fiber reinforced resin composition of this embodiment includes the glass fiber described above in this embodiment. Specifically, in a glass fiber reinforced resin composition comprising resin (thermoplastic resin or thermosetting resin), glass fiber, and other additives, the glass fiber reinforced resin composition of this embodiment contains glass fiber ranging from 10% to 90% by mass relative to the total amount of the glass fiber reinforced resin composition. In addition, the glass fiber reinforced resin composition of this embodiment contains resin ranging from 90% to 10% by mass relative to the total amount of the glass fiber reinforced resin composition, and contains other additives ranging from 0% to 40% by mass.Instruction manual, pages 13 / 22, 15 CN 121929914 A

[0119] Here, examples of the above-mentioned thermoplastic resins include: polyethylene, polypropylene, polystyrene, styrene / maleic anhydride resin, styrene / maleimide resin, polyacrylonitrile, acrylonitrile / styrene (AS) resin, acrylonitrile / butadiene / styrene (ABS) resin, chlorinated polyethylene / acrylonitrile / styrene (ACS) resin, acrylonitrile / ethylene / styrene (AES) resin, Acrylonitrile / styrene / methyl acrylate (ASA) resin, styrene / acrylonitrile (SAN) resin, methacrylic acid resin, polyvinyl chloride (PVC), polyvinylidene chloride (PVDC), polyamide, polyacetal, polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polypropylene terephthalate (PTT), polycarbonate, polysulfide, polyethersulfone (PES), polyphenylene sulfone (PPSU), polyphenylene ether (PPE), modified polyphenylene ether (m-PPE), polyaryl ether ketone, liquid crystal polymer (LCP), fluoropolymers, polyetherimide (PEI), polyarylate (PAR), polysulfone (PSF), polyamide-imide (PAI), polyaminobismaleimide (PABM), thermoplastic polyimide (TPI), polyethylene naphthalate (PEN), ethylene / vinyl acetate (EVA) resin, Ionomer (IO) resins, polybutadiene, styrene / butadiene resins, polybutene, polymethylpentene, olefin / vinyl alcohol resins, cyclic olefin resins, cellulose resins, polylactic acid, etc.

[0120] Specifically, as polyethylene, examples include: high-density polyethylene (HDPE), medium-density polyethylene, low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), ultra-high molecular weight polyethylene, etc.

[0121] As polypropylene, examples include: isotactic polypropylene, atactic polypropylene, syndiotactic polypropylene, and mixtures of the above polypropylenes, etc.

[0122] As polystyrene, examples include general-purpose polystyrene (GPPS) as atactic polystyrene having an atactic structure, impact-resistant polystyrene (HIPS) with rubber components added to GPPS, syndiotactic polystyrene having a syndiotactic structure, etc.

[0123] Examples of methacrylic resins include polymers formed by polymerizing one of the following methacrylic resins: acrylic acid, methacrylic acid, styrene, methyl acrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, and ethylene fatty acid esters; or polymers formed by copolymerizing two or more of the above-mentioned methacrylic resins.

[0124] Examples of polyvinyl chloride include: homopolymers of vinyl chloride polymerized using known methods such as emulsion polymerization, suspension polymerization, micro-suspension polymerization, and bulk polymerization; copolymers of vinyl chloride monomers; and graft copolymers of polymers in which vinyl chloride monomers have been grafted onto the polymer.

[0125] Examples of polyamides include: polycaprolactam (Nylon 6), polyhexamethylene adipamide (Nylon 66), polytetramethylene adipamide (Nylon 46), polyhexamethylene sebacamide (Nylon 410), polypentamethylene adipamide (Nylon 56), polypentamethylene sebacamide (Nylon 510), polyhexamethylene sebacamide (Nylon 610), polyhexamethylene dodecylamide (Nylon 612), polydecamethylene adipamide (Nylon 106), polydecamethylene sebacamide (Nylon 1010), polydecamethylene dodecylamide (Nylon 1012), polyundecylamide (Nylon 11), polyhexamethylene adipamide (Nylon 116), and polydodecylamide. Amide (Nylon 12), Polyxylhexadiamide (Nylon D6), Polyxylhexadiamide (Nylon MXD10), Poly(m-phenylene adipamide) (Nylon MXD6), Poly(p-xylhexadiamide) (Nylon PXD6), Poly(terephthalamide) (Nylon 4T), Polypentamethylene terephthalamide (Nylon 5T), Polyhexamethylene terephthalamide (Nylon 6T), Polyhexamethylene isophthalamide (Nylon 6I), Polynonamethylene terephthalamide (Nylon 9T), Poly(terephthaloylmethyl terephthalamide) (Nylon 10T), Polyhexamethylene terephthalamide (Nylon 11T), Polydodecyl terephthalamide (Nylon 12T) The copolymer of one or more of the following components: polytetramethylene polyphthalamide (Nylon 4I), polybis(3-methyl-4-aminohexyl)methane terephthalamide (Nylon PACMT), polybis(3-methyl-4-aminohexyl)methane isophthalamide (Nylon PACMI), polybis(3-methyl-4-aminohexyl)methane dodecylamide (Nylon PACM12), and polybis(3-methyl-4-aminohexyl)methane tetradecylamide (Nylon PACM14), or a mixture of the above components and the copolymers mentioned above in the specification (page 14 / 22, CN 121929914 A).

[0126] Examples of polyacetals include homopolymers with oxymethylene units as the main repeating units, and copolymers mainly composed of oxymethylene units and containing oxyalkylene units having 2 to 8 adjacent carbon atoms in the main chain.

[0127] Examples of polyethylene terephthalate include polymers obtained by polycondensation of ethylene glycol with terephthalic acid or its derivatives.

[0128] Examples of polybutylene terephthalate include polymers obtained by polycondensation of 1,4-butanediol with terephthalic acid or its derivatives.

[0129] Examples of polypropylene terephthalate include polymers obtained by polycondensation of 1,3-propanediol with terephthalic acid or its derivatives.

[0130] Examples of polycarbonate include polymers obtained by transesterification in which a dihydroxy aryl compound is reacted with a carbonate such as diphenyl carbonate in the molten state, or polymers obtained by phosgene reaction in which a dihydroxy aryl compound is reacted with phosgene.

[0131] Examples of polyaryl sulfides include linear polyphenylene sulfides, cross-linked polyphenylene sulfides that are polymerized by curing after polymerization, polyphenylene sulfide sulfones, polyphenylene sulfide ethers, and polyphenylene sulfide ketones.

[0132] Examples of polyphenylene ethers include: poly(2,3-dimethyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-chloromethyl-1,4-phenylene ether), poly(2-methyl-6-hydroxyethyl-1,4-phenylene ether), poly(2-methyl-6-n-butyl-1,4-phenylene ether), poly(2-ethyl-6-isopropyl-1,4-phenylene ether), poly(2-ethyl-6-n-propyl-1,4-phenylene ether), poly(2,3,6-trimethyl-1,4-phenylene ether), poly[2-(4'-methylphenyl)-1,4-phenylene ether], poly(2-bromo-6-phenyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), poly(2-phenyl-1,4-phenylene ether), poly(2-chloro-1,4-phenylene ether), poly(2- Methyl-1,4-phenylene ether), poly(2-chloro-6-ethyl-1,4-phenylene ether), poly(2-chloro-6-bromo-1,4-phenylene ether), poly(2,6-di-n-propyl-1,4-phenylene ether), poly(2-methyl-6-isopropyl-1,4-phenylene ether), poly(2-chloro-6-methyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2,6-dibromo-1,4-phenylene ether), poly(2,6-dichloro-1,4-phenylene ether), poly(2,6-diethyl-1,4-phenylene ether), poly(2,6-dimethyl-1,4-phenylene ether), etc.

[0133] Examples of modified polyphenylene ethers include: polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and polystyrene; polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and styrene / butadiene copolymer; polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and styrene / maleic anhydride copolymer; polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and polyamide; polymer alloys of poly(2,6-dimethyl-1,4-phenylene) ether and styrene / butadiene / acrylonitrile copolymer; modified polyphenylene ethers in which functional groups such as amino, epoxy, carboxyl, and styrene groups are introduced at the polymer chain ends of the above-mentioned polyphenylene ethers; and modified polyphenylene ethers in which functional groups such as amino, epoxy, carboxyl, styrene, and methacryloyl groups are introduced into the side chains of the polymer of the above-mentioned polyphenylene ethers.

[0134] Examples of polyarylether ketones include: polyether ketone (PEK), polyether ether ketone (PEEK), polyether ketone ketone (PEKK), polyether ether ketone ketone (PEEKK), etc.

[0135] Examples of liquid crystal polymers (LCPs) include (co)polymers composed of one or more structural units selected from the following components: aromatic hydroxy carbonyl units, aromatic dihydroxy units, aromatic dicarbonyl units, aliphatic dihydroxy units, aliphatic dicarbonyl units, etc., which are thermotropic liquid crystal polyesters.

[0136] Examples of fluoropolymers include: polytetrafluoroethylene (PTFE), perfluoroalkoxy resin (PFA), fluorinated ethylene propylene resin (FEP), fluorinated ethylene tetrafluoroethylene resin (ETFE), polyethylene fluoride (PVF), polyvinylidene fluoride (PVDF), polyvinyl chloride (PCTFE), ethylene / trifluorochloroethylene resin (ECTFE), etc.

[0137] Examples of ionomer (IO) resins include copolymers of olefins or styrene with unsaturated carboxylic acids, wherein a portion of the carboxyl group is neutralized with metal ions.

[0138] Examples of olefin / vinyl alcohol resins include ethylene / vinyl alcohol copolymers, propylene / vinyl alcohol copolymers, ethylene / vinyl acetate copolymer saponifications, propylene / vinyl acetate copolymer saponifications, etc.

[0139] Examples of cyclic olefin resins include polymers of monocyclic monomers such as cyclohexene, polycyclic monomers such as tetracyclic cyclic olefins, and cyclic olefin monomers.

[0140] Examples of polylactic acid include poly-L-lactic acid as an L-body homopolymer, poly-D-lactic acid as a D-body homopolymer, or stereocomposite polylactic acid as a mixture thereof.

[0141] Examples of cellulose resins include: methylcellulose, ethylcellulose, hydroxycellulose, hydroxymethylcellulose, hydroxyethylcellulose, hydroxyethylmethylcellulose, hydroxypropylmethylcellulose, cellulose acetate, cellulose propionate, cellulose butyrate, etc.

[0142] In addition, examples of the above-mentioned thermosetting resins include: unsaturated polyester resins, vinyl ester resins, epoxy (EP) resins, melamine (MF) resins, phenolic resins (PF), polyurethane resins (PU), polyisocyanates, polyisocyanurates, polyimide (PI), urea (UF) resins, silicone (SI) resins, furan (FR) resins, benzoguanamine (BR) resins, alkyd resins, xylene resins, bismaleimide triazine (BT) resins, diallyl phthalate resins (PDAP), etc.

[0143] Specifically, examples of unsaturated polyester resins include resins obtained by esterification of aliphatic unsaturated dicarboxylic acids with aliphatic diols.

[0144] Examples of vinyl ester resins include: divinyl ester resins and phenolic varnish-based vinyl ester resins.

[0145] Examples of epoxy resins include: bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol E type epoxy resins, bisphenol S type epoxy resins, bisphenol M type epoxy resins (4,4'-(1,3-phenylene diisopropylidene) bisphenol type epoxy resins), bisphenol P type epoxy resins (4,4'-(1,4-phenylene diisopropylidene) bisphenol type epoxy resins), bisphenol Z type epoxy resins (4,4'-cyclohexylene diphenol type epoxy resins), phenolic varnish type epoxy resins, cresol varnish type epoxy resins, and tetraphenolic ethane type epoxy resins. Aldehyde varnish-type epoxy resin, phenolic varnish-type epoxy resin with a fused ring aromatic hydrocarbon structure, biphenyl-type epoxy resin, xylene-type epoxy resin or phenylarylene-type epoxy resin and other aralkyl-type epoxy resins, naphthylene ether-type epoxy resin, naphthol-type epoxy resin, naphthalene glycol-type epoxy resin, difunctional or tetrafunctional naphthalene epoxy resin, binatyl-type epoxy resin, naphthalene aralkyl-type epoxy resin, anthracene-type epoxy resin, phenoxy-type epoxy resin, dicyclopentadiene-type epoxy resin, norbornene-type epoxy resin, adamantane-type epoxy resin, fluorene-type epoxy resin, etc.

[0146] As melamine resin, polymers composed of melamine (2,4,6-triamino-1,3,5-triazine) and formaldehyde can be cited as examples.

[0147] Examples of phenolic resins include: phenolic varnish resins such as phenolic varnish resins, cresol varnish resins, and bisphenol A varnish resins; methyl phenolic resins such as hydroxymethyl methyl phenolic resins and dimethylene ether methyl phenolic resins; and arylalkylene phenolic resins, or resins composed of one or more of these resins.

[0148] Examples of urea-formaldehyde resins include resins obtained by the condensation of urea and formaldehyde.

[0149] The above-mentioned thermoplastic resin or thermosetting resin can be used alone or in combination of two or more resins.

[0150] The glass fiber reinforced resin composition of this embodiment is used for applications requiring low dielectric properties. Therefore, epoxy resin, modified polyphenylene ether, polybutylene terephthalate, polypropylene, fluoropolymer, and liquid crystal polymer (LCP) are preferred as the above-mentioned resins.

[0151] Other additives mentioned above may include: reinforcing fibers other than glass fibers (e.g., carbon fibers, metal fibers), fillers other than glass fibers (e.g., glass powder, talc, mica), flame retardants, ultraviolet absorbers, heat stabilizers, antioxidants, antistatic agents, flow modifiers, antiblocking agents, lubricants, nucleating agents, antibacterial agents, pigments, etc.

[0152] The glass fiber reinforced resin composition of this embodiment can be a prepreg obtained by impregnating the above-mentioned resin into the glass fiber fabric of this embodiment and semi-curing it using a known method.

[0153] The glass fiber reinforced resin composition of this embodiment can be molded by known molding methods such as injection molding, injection compression molding, two-color molding, hollow molding, foaming molding (including supercritical fluid), insert molding, in-mold coating molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, compression molding, blow molding, stamping molding, melt molding, hand lay-up molding, spraying, resin transfer molding, sheet molding, bulk molding, pultrusion molding, and filament winding to obtain various glass fiber reinforced resin molded articles. In addition, glass fiber reinforced resin molded articles can also be obtained by curing the above-mentioned prepreg.

[0154] Examples of uses for such molded articles include: electronic device housings, electronic components, vehicle exterior parts, vehicle interior parts, vehicle engine peripheral parts, muffler-related parts, high-pressure tanks, etc.

[0155] Examples of electronic accessories include printed wiring boards.

[0156] Examples of vehicle exterior parts include bumpers, mudguards, engine hoods, air deflectors, wheel covers, etc.

[0157] Examples of vehicle interior parts include door trim, headliner materials, etc.

[0158] Examples of vehicle engine peripheral parts include oil pans, engine hoods, intake manifolds, exhaust manifolds, etc.

[0159] Examples of muffler-related parts include muffler components, etc.

[0160] It should be noted that the glass fiber of this embodiment can be used not only in the glass fiber reinforced resin composition of this embodiment, but also as a reinforcing material for inorganic materials such as gypsum and cement.For example, when used as a reinforcing material for gypsum (especially gypsum board with a thickness in the range of 4 to 60 mm), the gypsum contains glass fibers having a glass composition in the range of 0.1 to 4.0% by mass relative to the total mass of the gypsum.

[0161] Next, embodiments and comparative examples of the present invention are shown.

[0162] Embodiment First, glass raw materials were mixed to obtain a glass batch such that the glass composition after melting and solidification would be the composition of Examples 1 to 4 shown in Table 1 and Comparative Examples 1 to 10 shown in Tables 2 and 3.

[0163] Next, the glass batch corresponding to the glass fiber composition of Examples 1 to 4 or Comparative Examples 1 to 10 was placed in a platinum crucible with a diameter of 80 mm, heated at a temperature of 1550°C for 4 hours, and then further melted at a temperature of 1650°C for 2 hours. After that, it was taken out of the crucible to obtain homogeneous glass blocks and glass shavings. Next, the obtained glass blocks and glass shavings were annealed at a temperature of 620°C for 8 hours to obtain test pieces. The dielectric constant and dielectric loss tangent of the test piece obtained above were evaluated using the method shown below. Additionally, the water resistance was evaluated using glass shavings obtained during the test piece manufacturing process using the method shown below. Furthermore, the operating temperature range was calculated using glass shavings obtained during the test piece manufacturing process using the method shown below. The results of Examples 1-4 are shown in Table 1, the results of Comparative Examples 1-5 are shown in Table 2, and the results of Comparative Examples 6-10 are shown in Table 3.

[0164] [Method for evaluating water resistance] The glass shavings obtained in the above manner were placed in a small cylindrical platinum sleeve with a circular nozzle head at the bottom of a container. After being heated to a specified temperature to melt it, the molten glass ejected from the nozzle head was wound onto a stainless steel sleeve at a specified speed. It was then stretched and cooled to solidify, resulting in glass fibers with a perfectly circular cross-section and a fiber diameter of 13 μm. Approximately 1g of the glass fiber obtained above (test glass fiber) was collected from the clamp and dried at 120°C for 1 hour. The mass (mass before operation) was measured. Next, the test glass fiber was placed in 100ml of distilled water at 80°C for 24 hours. Then, the test glass fiber was obtained using a metal mesh with an opening of approximately 150μm, washed with distilled water, dried at 120°C for 1 hour, and the mass (mass after operation) was measured.

[0165] Based on the above-mentioned mass before operation and mass after operation, the mass reduction rate (100×(1-(mass after operation / mass before operation))) was calculated. The case where the mass reduction rate is less than 2.0% and the glass fiber components hardly dissolve in water is set as OK; the case where the mass reduction rate exceeds 2.0% and the glass fiber components dissolve significantly in water is set as NG.

[0166] [Method for measuring dielectric constant and dielectric loss tangent] A polishing test piece was prepared, measuring 80 mm × 3 mm (1 mm thickness). The prepared polishing test piece was then oven-dried and stored indoors at 23°C and 60% humidity for 24 hours. Next, according to JIS C 2565:1992, the dielectric constant (dielectric constant Dk) and dielectric loss tangent (dissipation rate Df) of the obtained polishing test piece at 10 GHz were measured using a cavity resonator method dielectric constant measuring apparatus ADM01Oc1 (trade name) manufactured by AET Corporation.

[0167] 〔Calculation Method for Operating Temperature Range〕 First, using a high-temperature electric furnace equipped with a rotational viscometer (manufactured by Shibaura Systems Co., Ltd.), glass shavings were melted in a platinum crucible. While changing the melting temperature, the viscosity of the molten glass was continuously measured using a rotational Brinell viscometer. The temperature corresponding to a rotational viscosity of 1000 poise was measured, thereby determining the 1000 poise temperature.

[0168] Next, the glass shavings were crushed, and 40g of glass particles with a particle size in the range of 0.5 to 1.5 mm were placed in a platinum vessel of 180×20×15 mm. After heating in a tubular electric furnace with a temperature gradient in the range of 1000 to 1400 °C for more than 8 hours, the particles were removed from the tubular electric furnace and observed using a polarizing microscope to determine the location where crystallization (devitrification) originating from the glass began to precipitate. The temperature inside the tubular electric furnace was measured using a type B thermocouple, and the temperature at which the above-mentioned crystallization began to precipitate was determined and taken as the liquid phase temperature.

[0169] Next, the operating temperature range is calculated using the difference between the 1000 poise temperature and the liquid phase temperature.

[0170] [Table 1] Specification 18 / 22 pages 20 CN 121929914 A [Table 2] Specification 19 / 22 pages 21 CN 121929914 A [Table 3] Specification 20 / 22 pages 22 CN 121929914 A As can be clearly seen from Table 1, the glass compositions for glass fibers according to Examples 1 to 4 below have a sufficient operating temperature range of 26°C or higher, and glass fibers with excellent water resistance, a dielectric constant of 4.2 or less in the high-frequency region of 10 GHz, and a dielectric loss tangent of 0.0011 or less can be obtained using this glass composition for glass fibers.In Examples 1-4, the glass composition for glass fiber contains SiO2 in the range of 59.00-65.00% by mass, B2O3 in the range of 16.00-26.00% by mass, Al2O3 in the range of 7.00-14.00% by mass, CaO in the range of 0-5.00% by mass, MgO in the range of 0-4.00% by mass, SrO in the range of 0-6.00% by mass, TiO2 in the range of 0.10-5.00% by mass, F2 and Cl2 in the range of 0-2.00% by mass, P2O5 content less than 0.20% by mass, Na2O, K2O and Li2O combined content less than 1.00% by mass, and the ratio of TiO2 content (by mass) to the combined content (by mass) of CaO, MgO and SrO (TiO2 / (CaO+)) is given by the following formula: The content of MgO + SrO is in the range of 0.66 to 4.00, and the content of SiO2 (mass %) SI and the content of Al2O3 (mass %) A satisfy the above formula (1).

[0171] On the other hand, it is obvious from Table 2 that glass fibers with sufficient water resistance cannot be obtained according to the glass composition for glass fiber of Comparative Example 1 below. In Comparative Example 1, the glass composition for glass fiber contains SiO2 with a content of less than 59.00% by mass relative to the total amount of the glass composition for glass fiber, B2O3 with a content of more than 26.00% by mass, Al2O3 with a content of less than 7.00% by mass, and TiO2 with a content of less than 0.10% by mass.

[0172] In addition, it is obvious that glass fibers with sufficient water resistance cannot be obtained using the glass composition for glass fiber of Comparative Example 2 below. In Comparative Example 2, the glass composition for glass fiber contained SiO2 at a rate of less than 59.00% by mass relative to the total amount of the glass composition for glass fiber, B2O3 at a rate of more than 26.00% by mass, and Al2O3 at a rate of less than 7.00% by mass.

[0173] Furthermore, it is evident that glass fibers with sufficient water resistance cannot be obtained using the glass composition for glass fiber of Comparative Example 3 described below. In Comparative Example 3, the glass composition for glass fiber contained SiO2 at a rate of less than 59.00% by mass relative to the total amount of the glass composition for glass fiber, B2O3 at a rate of more than 26.00% by mass, and Al2O3 at a rate of less than 7.00% by mass.

[0174] Furthermore, it is evident that, in addition to failing to obtain glass fibers with sufficient water resistance, crystallization also occurred using the glass composition for glass fiber of Comparative Example 4 described below.In Comparative Example 4, the glass composition for glass fiber contained SiO2 at a rate of less than 59.00% by mass relative to the total amount of the glass composition for glass fiber, B2O3 at a rate of more than 26.00% by mass, Al2O3 at a rate of less than 7.00% by mass, and TiO2 at a rate of more than 5.00% by mass.

[0175] Furthermore, it is evident that glass fibers with sufficient water resistance cannot be obtained using the glass composition for glass fiber of Comparative Example 5 below. In Comparative Example 5, the glass composition for glass fiber contained SiO2 at a rate of less than 59.00% by mass relative to the total amount of the glass composition for glass fiber, and B2O3 at a rate of more than 26.00% by mass.

[0176] Furthermore, it is evident from Table 3 that, in addition to failing to obtain glass fibers with sufficient water resistance, phase separation also occurred using the glass composition for glass fiber of Comparative Example 6 below. In Comparative Example 6, the glass composition for glass fiber contained SiO2 at a content of less than 59.00% by mass relative to the total amount of the glass composition for glass fiber and Al2O3 at a content of more than 14.00% by mass, and the value of the above formula (1) exceeded 4.65.

[0177] In addition, it is obvious that glass fibers with sufficient water resistance cannot be obtained using the glass composition for glass fiber of Comparative Example 7. In Comparative Example 7, the glass composition for glass fiber contained SiO2 at a content of less than 59.00% by mass relative to the total amount of the glass composition for glass fiber and B2O3 at a content of more than 26.00% by mass.

[0178] In addition, it is obvious that glass fibers with a sufficient operating temperature range and a sufficiently low dielectric loss tangent in the high-frequency region of the measurement frequency of 10 GHz cannot be obtained using the glass composition for glass fiber of Comparative Example 8, which contained Al2O3 at a content of more than 14.00% by mass relative to the total amount of the glass composition for glass fiber.

[0179] Furthermore, it is evident that the glass fiber composition of Comparative Example 9, in which the content of P2O5 relative to the total amount of the glass fiber composition exceeds 0.20% by mass, cannot produce glass fibers with sufficiently low dielectric constant and dielectric loss tangent in the high-frequency region of 10 GHz.

[0180] Furthermore, it is evident that the glass fiber composition of Comparative Example 10, in which the ratio of the content of TiO2 relative to the total amount of the glass fiber composition (by mass) to the total content of CaO, MgO, and SrO (by mass) (TiO2 / (CaO+MgO+SrO)) is less than 0.66, cannot produce glass fibers with sufficient water resistance and sufficiently low dielectric loss tangent in the high-frequency region of 10 GHz. Specification 22 / 22 pages 24 CN 121929914 A.

Claims

1. A glass composition for glass fiber, characterized in that, It contains SiO2 in the range of 59.00 to 65.00% by mass, B2O3 in the range of 16.00 to 26.00% by mass, Al2O3 in the range of 7.00 to 14.00% by mass, CaO in the range of 0 to 5.00% by mass, MgO in the range of 0 to 4.00% by mass, SrO in the range of 0 to 6.00% by mass, TiO2 in the range of 0.10 to 5.00% by mass, and F2 and Cl2 in the range of 0 to 2.00% by mass, relative to the total amount of the glass composition for glass fiber. The content of P2O5 is less than 0.20% by mass, and the total content of Na2O, K2O and Li2O is less than 1.00% by mass.

2. A type of glass fiber, characterized in that, It is composed of the glass composition for glass fiber as described in claim 1.

3. A glass fiber fabric, characterized in that, It contains the glass fiber as described in claim 2.

4. A glass fiber reinforced resin composition, characterized in that, It contains the glass fiber as described in claim 2.