Colloidal silica and method for producing colloidal silica
Patent Information
- Application Number
- HK62026125074
- Authority / Receiving Office
- HK · HK
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-21
- Filing Date
- 2026-06-22
- Publication Date
- 2026-09-11
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
(19) State Intellectual Property Office (12) Invention Patent Application (10) Application Publication Number (43) Application Publication Date (21) Application Number 202480072374.6 (22) Application Date 2024.11.29 (30) Priority Data 2023-215881 2023.12.21 JP (85) PCT International Application Entering National Phase Date 2026.05.14 (86) PCT International Application Application Data PCT / JP2024 / 042396 2024.11.29 (87) PCT International Application Publication Data WO2025 / 134733 JA 2025.06.26 (71) Applicant Tama Chemical Industry Co., Ltd. Address Japan (72) Inventors Ryuichi Oyama, Yojin Yashiro, Tsukasa Nishimori, Itsuki Murayama (74) Patent Agency China Council for the Promotion of International Trade Patent & Trademark Office Co., Ltd. 11038 Patent Attorney Du Lili (51) Int.Cl. C01B 33 / 141 (2006.01) H10P 52 / 00 (2026.01) (54) Invention Title Colloidal Silica and Method for Manufacturing Colloidal Silica (57) Abstract Provides colloidal silica with the characteristics of smooth surface, low alkali metal impurities, and preferably low surface changes over time, and a method for manufacturing the same. It relates to colloidal silica, characterized in that it simultaneously satisfies the following (1) and (2): (1) The roughness expressed by the following formula (i) is 1.0740 or less, roughness = equivalent circle diameter converted from perimeter obtained by image analysis of an electron microscope (perimeter equivalent circle diameter) / equivalent circle diameter converted from projected area obtained by image analysis of an electron microscope (area equivalent circle diameter) (i) (2) Metal impurities are 1 ppm or less. Claims 1 page, Description 20 pages, Drawings 9 pages, CN 122228218 A 2026.06.16 CN 1 22 22 82 18 A 1. Colloidal silica, characterized in that it simultaneously satisfies the following (1) and (2): (1) The roughness expressed by the following formula (i) is 1.0740 or less, Roughness = Equivalent circle diameter converted from circumference obtained by image analysis of the projection image obtained by electron microscope / Equivalent circle diameter converted from projection area obtained by image analysis of electron microscope (i) (2) Metal impurities are 1 ppm or less. 2. Colloidal silica according to claim 1, characterized in that, after being kept at a temperature of 60°C for 7 days, the change rate of silanol group density is -5% or more.3. The colloidal silica according to claim 1, characterized in that the change rate of the transverse relaxation time of the seed nucleus 1H, measured by time-domain nuclear magnetic resonance, after being kept at 60°C for 7 days, is less than 24%. 4. The colloidal silica according to claim 1, characterized in that the silanol group density is less than 3 groups / nm². 5. The colloidal silica according to claim 1, characterized in that the transverse relaxation time of the seed nucleus 1H, measured by time-domain nuclear magnetic resonance, is greater than 650 ms and less than 1300 ms. 6. The colloidal silica according to claim 1, characterized in that the electron microscope is any one or more of scanning electron microscopy (SEM), scanning transmission electron microscopy (STEM), and transmission electron microscopy (TEM). 7. An abrasive comprising the colloidal silica according to any one of claims 1 to 6. 8. A method for manufacturing colloidal silica, comprising supplying a hydrolyzable organosilicon ester to a reaction solution containing a hydrolysis catalyst composed of one or more organic amines and reacting it to manufacture colloidal silica, characterized in that the manufacturing condition constant represented by the following formula (ii) is 0.024 or less, manufacturing condition constant = silica concentration after reaction (mass%) / supply time of the hydrolyzable organosilicon ester (hr) / reaction temperature (°C) (ii). Claims 1 / 1 page 2 CN 122228218 A Colloidal silica and method for manufacturing colloidal silica Technical Field
[0001] The present invention relates to colloidal silica and a method for manufacturing colloidal silica, and particularly to colloidal silica with smooth particle surface and a method for manufacturing the same. Background Art
[0002] As a method for industrially manufacturing high-purity colloidal silica, methods such as ion exchange of sodium silicate aqueous solution, thermal decomposition of silicon tetrachloride, and hydrolysis of organosilicon esters in a water-alcohol mixed solvent in the presence of an acid catalyst or a base catalyst have been proposed and implemented. Regarding the method of hydrolyzing organosilicon esters, high-purity substances can be used as the organosilicon esters, catalysts, and solvents used in the reaction, so there are very few impurities from these raw materials, which is particularly suitable as a method for manufacturing high-purity colloidal silica with low metal impurity content. Several methods related to the hydrolysis of organosilicon esters have been proposed so far.
[0003] Among them, for colloidal silica used for various purposes, especially colloidal silica used in the field of polishing agents for semiconductor wafers, with the current high integration of LSI, various metal wirings, oxide films, etc. exist on a single wafer. In addition, for each semiconductor wafer, polishing performance suitable for each is required, so colloidal silica with subtle differences in composition and properties is needed.
[0004] In addition, for colloidal silica used in applications such as hard coatings, ceramics, adhesives, chromic acid-based metal surface treatment agents, and foundation improvement injection agents where the presence of small amounts of alkali metal impurities is undesirable, acidic colloidal silica is required, and several proposals are known for manufacturing methods of such acidic colloidal silica.
[0005] For example, the applicant of this application has studied a method that can easily produce colloidal silica with specified properties, such as spherical colloidal silica, without the need for special post-treatment such as acid treatment, ion exchange treatment, or modification treatment. In addition, the content of metal impurities, mainly alkali metals, is extremely low, and the average particle size obtained by particle size distribution analysis using electron microscopy is in the range of 5 to 500 nm, with a standard deviation of 20 or less and a polydispersity index of 0.15 or less. As a result, it was proposed to use a fast-hydrolyzing organosilicon ester and an organic hydrolysis catalyst such as a quaternary ammonium to add the hydrolysis catalyst such that the ratio of the hydrolysis catalyst (A) to the silica (B) in the reaction mixture at the end of the reaction, {catalyst residual molar ratio (A / B)}, is at least below a specified value, so that neutral colloidal silica with pH 5 to 8 can be easily produced without special post-treatment such as acid treatment or ion exchange treatment (Patent Document 1). According to the manufacturing method of Patent Document 1, it is said that neutral colloidal silica with a large SEM average particle size, large BET specific surface area, high particle density (true specific gravity), excellent grinding speed, and suitability for use as a polishing compound in CMP can be easily manufactured.
[0006] In addition, for colloidal silica manufactured using the method of Patent Document 1, a polishing composition that appropriately adjusts the protrusions on the particle surface has been proposed (Patent Document 2) to achieve a higher grinding speed.
[0007] Furthermore, for colloidal silica manufactured using the method of Patent Document 1, a colloidal silica with excellent surface irregularity maintenance under alkaline conditions has been proposed (Patent Document 3).
[0008] Thus, various studies have been conducted on colloidal silica with irregularities and protrusions on the surface.
[0009] For example, in the field of polishing compounds for semiconductor wafers, various requirements have been needed in recent years. For example, in the grinding process described on page 1 / 20 of the specification, CN 122228218 A, colloidal silica is used in various liquid forms, including acidic, neutral, and alkaline forms, with a slurry using neutral to alkaline colloidal silica being particularly preferred.The reason is that, especially in silicon wafer polishing, it has the effect of chemically acting on the surface of the silicon wafer, promoting etching, and increasing the polishing rate; in addition, it has the effect of removing impurities such as abrasive particles and chelating agents adsorbed on the surface of the silicon wafer; furthermore, it can improve the flatness and defect performance of the wafer; and thus it has the effect of reducing the coefficient of friction with the polishing pad, thereby suppressing heat generation and wear during polishing and stabilizing the polishing quality. Therefore, colloidal silica that does not change much over time under neutral to alkaline conditions is particularly preferred. In addition, as mentioned in Patent Documents 1 to 3 above, colloidal silica with an uneven surface has a high physical polishing rate for the polishing object, raising concerns about the possibility of damage to the polishing object.
[0010] Colloidal silica with a smooth surface has a relatively low physical polishing rate for the polishing object. However, the polishing rate can be met by chemical polishing (chemical polishing), so colloidal silica with a smooth surface is advantageous for polishing objects that are considered to be harmless as long as they are unlikely to be damaged, and can be used as colloidal silica with polishing abrasive particles that have a smooth surface. In addition, particles with small surface roughness generally have the advantage of less change over time due to unevenness.
[0011] In general, when colloidal silica is manufactured using catalysts derived from alkali metals such as NaOH and KOH, the catalysts derived from alkali metals are highly alkaline, resulting in high solubility of the silica source, low growth rate, and easy uniform particle growth, thus tending to result in smaller surface roughness of the obtained silica particles. However, when using such catalysts derived from alkali metals, the alkali metals become impurities, making them unsuitable for semiconductor manufacturing.
[0012] Therefore, in order to obtain colloidal silica suitable for semiconductor manufacturing, catalysts derived from alkali metals are preferred to be avoided. For example, a manufacturing method using an organic hydrolysis catalyst, as described in Patent Document 1 above, has been proposed. However, in organic hydrolysis catalysts, low-boiling-point ammonia and organic amines are prone to volatilization during reactions in aqueous solvents at high temperatures, raising concerns about unstable reactions.
[0013] Based on this actual situation, and from the viewpoint of producing colloidal silica with few alkali metal impurities and stability, it can be said that an organic amine catalyst with a relatively high boiling point is preferred. However, in conventional reaction methods using high-boiling-point organic amine catalysts, the organic amine catalysts are weakly alkaline, resulting in low solubility of the silica source, high growth rate, and particles that tend not to easily form a stable configuration, thus resulting in colloidal silica with relatively large surface roughness.
[0014] That is, colloidal silica with a smooth surface and few alkali metal impurities has not yet been discovered.
[0015] Prior Art Documents
[0016] Patent Documents
[0017] Patent Document 1: Japanese Patent Application Publication No. 2007-153732
[0018] Patent Document 2: Japanese Patent Application Publication No. 2012-104800
[0019] Patent Document 3: WO2020 / 179558 Summary of the Invention
[0020] Problems to be Solved by the Invention
[0021] Therefore, in order to develop colloidal silica with the characteristics of smooth surface and low alkali metal impurities, the inventors of this application conducted in-depth research and found that by adjusting the reaction conditions when adding the silica source in the method of reacting the silica source with a hydrolysis catalyst selected from organic amines, it is possible to achieve this, thus completing the present invention. At this time, the characteristics related to the time-dependent changes of the colloidal silica surface were also studied in depth, and in addition to the above, it was further successfully discovered that a preferred embodiment is one with low time-dependent changes. Specification 2 / 20 pages 4 CN 122228218 A
[0022] Therefore, the object of the present invention is to provide colloidal silica that combines the characteristics of smooth surface and low alkali metal impurities, preferably with low surface changes over time, and a method for manufacturing the same.
[0023] Furthermore, the object of the present invention is also to specify the characteristics of the surface changes of such colloidal silica over time and to provide a method for evaluating them over a specified time.
[0024] Means for solving the problem
[0025] That is, the gist of the present invention is as follows.
[0026] [1] Colloidal silica, characterized in that it simultaneously satisfies the following (1) and (2):
[0027] (1) The roughness expressed by the following formula (i) is 1.0740 or less,
[0028] Roughness = equivalent circle diameter converted from the perimeter obtained by image analysis of the projection image obtained by electron microscope (circumference converted equivalent circle diameter) / equivalent circle diameter converted from the projection area obtained by image analysis of electron microscope (area converted equivalent circle diameter) (i)
[0029] (2) The metallic impurity is 1 ppm or less.
[0030] [2] Colloidal silica according to [1], characterized in that, after being kept at a temperature of 60°C for 7 days, the change rate of silanol group density is -5% or more.
[0031] [3] According to [1], the colloidal silica is characterized in that the change rate of the transverse relaxation time of the seed 1H, measured by time-domain nuclear magnetic resonance, after being kept at a temperature of 60°C for 7 days is less than 24%.
[0032] [4] According to [1], the colloidal silica is characterized in that the silanol group density is less than 3 groups / nm2.
[0033] [5] According to [1], the colloidal silica is characterized in that the transverse relaxation time of the seed 1H, measured by time-domain nuclear magnetic resonance, is more than 650ms and less than 1300ms.
[0034] [6] The colloidal silica according to [1] is characterized in that the electron microscope is any one or more of a scanning electron microscope (SEM), a scanning transmission electron microscope (STEM), and a transmission electron microscope (TEM).
[0035] [7] An abrasive comprising colloidal silica according to any one of [1] to [6].
[0036] [8] A method for manufacturing colloidal silica, comprising supplying a hydrolyzable organosilicon ester to a reaction solution comprising a hydrolysis catalyst composed of one or more of organic amines and reacting it to manufacture colloidal silica, characterized in that the manufacturing condition constant represented by the following formula (ii) is 0.024 or less,
[0037] Manufacturing condition constant = silica concentration after reaction (mass%) / supply time of the hydrolyzable organosilicon ester (hr) / reaction temperature (°C) (ii).
[0038] Effects of the Invention
[0039] According to the present invention, it is possible to provide colloidal silica that has the characteristics of smooth surface and low alkali metal impurities. Furthermore, as a preferred embodiment, colloidal silica with minimal changes in surface properties over time, other than those described above, can be obtained. Additionally, a method for manufacturing such colloidal silica can be provided. Brief Description of the Drawings
[0040] FIG1 shows a SEM image (200,000x magnification) of the colloidal silica obtained in Example 1.
[0041] FIG2 shows a STEM image (200,000x magnification) of the colloidal silica obtained in Example 1.
[0042] FIG3 shows a SEM image (200,000x magnification) of the colloidal silica obtained in Example 3.
[0043] FIG4 shows a STEM image (200,000x magnification) of the colloidal silica obtained in Example 3.
[0044] FIG5 shows a SEM image (200,000x magnification) of the colloidal silica obtained in Comparative Example 1.
[0045] FIG6 shows a STEM image (200,000x magnification) of the colloidal silica obtained in Comparative Example 1. Instruction manual 3 / 20 pages 5 CN 122228218 A
[0046] FIG7 shows a SEM image (200,000x magnification) of colloidal silica obtained in Comparative Example 3.
[0047] FIG8 shows a STEM image (200,000x magnification) of colloidal silica obtained in Comparative Example 3.
[0048] FIG9 is an analytical image of the STEM images of colloidal silica of Examples 1 to 6 and Comparative Examples 1 to 4. Detailed Description
[0049] <Colloidal Silica>
[0050] As described above, the colloidal silica of the present invention is characterized by simultaneously satisfying the following (1) and (2).
[0051] (1) The roughness expressed by the following formula (i) is 1.0740 or less.
[0052] Roughness = Equivalent circle diameter converted from the perimeter obtained by image analysis of an electron microscope (circumference converted to equivalent circle diameter) / Equivalent circle diameter converted from the projected area obtained by image analysis of an electron microscope (area converted to equivalent circle diameter) (i)
[0053] (2) Metal impurities are 1 ppm or less.
[0054] The above explanation is based on (1).
[0055] The roughness of the colloidal silica of the present invention is 1.0740 or less. By satisfying the roughness defined in this way, it is possible to specify that the surface roughness of the colloidal silica particles is relatively small and smooth. The reason is as follows.
[0056] That is, as far as the particles of colloidal silica are concerned, due to manufacturing methods, etc., the shape is not a perfect sphere, and the surface shape is also varied, so it is difficult to immediately determine whether the surface is smooth. Therefore, in this invention, it is envisioned that, as described above, the degree of unevenness of the particle surface of colloidal silica can be determined by calculating the ratio of the equivalent circle diameter converted from the projected area obtained from image analysis by an electron microscope (area-converted equivalent circle diameter) to the equivalent circle diameter converted from the circumference obtained from the projected image obtained from image analysis by an electron microscope (circumference-converted equivalent circle diameter). That is, it is assumed that as the degree of unevenness of the particle surface increases, the circumference of the particle seen in the projected image by an electron microscope increases, and therefore the diameter of the circle with the same circumference also increases. In this invention, the circumference is defined as the circumference obtained from the projected image obtained from image analysis by an electron microscope. Therefore, it is known that by comparing the particle surface unevenness with the area-converted equivalent circle diameter, which is considered to differ from the degree of unevenness and is particularly insensitive to the degree of unevenness, the degree of unevenness of the particle surface can be relatively grasped, thus providing a preferred method and benchmark for determining whether a surface is smooth.
[0057] In this respect, if the spherical monodisperse particles have approximately the same degree of unevenness, the larger the BET specific surface area, the smaller the particle size tends to be. Therefore, the tendency for the BET specific surface area and the aforementioned unevenness not to be the same is an unexpected technical matter learned in this invention.
[0058] Here, firstly, the aforementioned perimeter-equivalent circle diameter is also called the projected perimeter-equivalent circle diameter, which is the diameter of a circle with the same perimeter as the circumference. This perimeter-equivalent circle diameter is determined taking into account the surface shape of the particles and is one of the parameters that affect the shape and contour of the particles.
[0059] In addition, the aforementioned area-equivalent circle diameter is also commonly referred to as the Heywood diameter, which can be obtained according to JIS Z 8827-1:2018 Particle Size Analysis - Image Analysis Method.When measuring particles of various shapes, such as those with uneven surfaces or particles that taper in the middle, on the surface of colloidal silica particles, there are problems with the ease of measurement by hand and the time required for measurement. Therefore, it is preferable to use a standardized equivalent circle diameter to objectively evaluate the outer diameter of the particles.
[0060] It should be noted that the above-mentioned unevenness is preferably 1.0735 or less, more preferably 1.0730 or less, and even more preferably 1.0725 or less. On the other hand, there is no limitation on the lower limit of this unevenness. The theoretical lower limit of unevenness is greater than 1.0000, preferably 1.0300 or more, more preferably 1.0400 or more, and even more preferably 1.0500 or more.
[0061] As for the electron microscope used, there are no limitations as long as it can acquire images applicable to the measurement and analysis of the equivalent diameter described above. For example, known electron microscopes such as scanning electron microscopes (SEM), transmission electron microscopes (TEM), and scanning transmission electron microscopes (STEM) can be used without limitation. Preferably, SEM or TEM can be used in combination with STEM, more preferably, SEM and STEM can be used in combination, and even more preferably, STEM. In the analysis of particles, binarization is performed to separate the black part of the particle and the white part outside the particle to identify the particle. For example, when observing particles with unevenness with SEM, the unevenness on the particle becomes black and white, so there is a tendency to make it difficult to determine the boundary of the particle. Therefore, it becomes necessary to use TEM or STEM observations where unevenness and black and white are not generated. This is because, with TEM observation alone, there is a tendency to make it difficult to determine whether it is a particle formed by the aggregation of particles or whether it is just particles overlapping to appear as a particle. Therefore, when taking STEM images and analyzing the images, the shape of the particles can be accurately captured, and a more accurate equivalent circle diameter and area equivalent circle diameter can be obtained.
[0062] Specifically, in any image analysis software used in the embodiments, STEM images are imported to measure the area of the particles. The results are imported into the calculation software, overlapping particle data are removed, and the perimeter-to-equivalent circle diameter and area-to-equivalent circle diameter are determined from the images of the remaining particles. After summing the equivalent diameters of all particles, the roughness can be calculated from the ratio of the two according to the above formula (i).
[0063] In addition, the colloidal silica of the present invention, as described above, has a metal impurity of 1 ppm or less. Preferably, it is 0.01 ppm or less, more preferably 0.001 ppm or less, and even more preferably 0.0001 ppm or less.In order to obtain colloidal silica with low metal impurities, in methods using sodium silicate as a raw material and methods using NaOH or KOH as hydrolysis catalysts, alkali metals such as sodium from the raw materials remain, making it difficult to reduce the metal impurities in the manufactured colloidal silica to below 1 ppm. Therefore, in the colloidal silica of the present invention, there are no limitations on achieving the aforementioned metal impurity content of below 1 ppm. For example, a preferred embodiment is to use a high-purity substance with a metal impurity content of below 1 ppm, preferably below 0.01 ppm, as the silica source, hydrolysis catalyst, and water used as raw materials for manufacturing.
[0064] Among these, regarding the colloidal silica of the present invention having the aforementioned characteristics of unevenness and metal impurities, it is preferable that the particle surface exhibits minimal changes over time. Minimal changes over time in the particle surface tend to reveal its usefulness in actual use, for example, reduced fluctuations in the grinding rate, which is therefore preferable. While several main reasons are considered for this change over time, one of them is due to the silanol groups (Si-OH) on the particle surface. If a large number of silanol groups are present, the adjacent silanol groups become more prone to condensation due to the closer distance between them. This is because, especially under neutral and alkaline conditions, protons easily detach from the silanol groups, making them more prone to condensation and resulting in changes over time. Furthermore, fewer silanol groups also lead to lower roughness, resulting in a smoother texture and less change over time, which is preferable.
[0065] In this invention, the low change over time can be confirmed by measuring the change in the density of silanol groups (unit: groups / nm2) of colloidal silica over time. Specifically, the change in the density of silanol groups after holding under heating conditions for a certain period can be used. There are no limitations on the pH conditions; the pH of the manufactured product can be used. Specifically, as also performed in the embodiments described later, a minimum temperature of 60°C or higher is used as a severe condition to prevent phase changes such as water evaporation. Furthermore, the change in silanol density after maintaining this condition for 7 days is confirmed, and if the change rate is -5% or higher, it can be determined that there is no change in silanol density. There is no limitation on the concentration of solid components during this measurement; it is preferable to measure the silanol density using a concentration of solid components consistent with the intended use and actual application.
[0066] The reason for preferably using the method of maintaining at 60°C or higher for 7 days is that by setting the condition at 60°C for 7 days, it is known that this is roughly equivalent to a time-varying test maintained at room temperature for 1 year. Therefore, it can be confirmed, as per specification page 5 / 20, 7 CN 122228218 A, that there is no time-varying change in silanol density in a time-varying test maintained at room temperature for at least 1 year. Moreover, it is preferable that the change rate is -4% or higher, more preferably -3% or higher. On the other hand, there is no limitation on the upper limit of this change rate.The reason is believed to be that, regarding the change in the density of silanol groups, although it is assumed that it will decrease due to condensation reactions of silanol groups, etc., the number of silanol groups will not increase significantly under the measurement conditions. Therefore, considering the variation in the rate of change (variance coefficient) based on the measured value, the upper limit of the rate of change is generally preferably +10% or less, more preferably +7% or less, and even more preferably +5% or less.
[0067] In addition, the density of silanol groups on the surface of the colloidal silica particles of the present invention is preferably 3 or less per nm2. This is because, as described above, when the density of silanol groups is high, condensation between silanol groups and a decrease in silanol groups are likely to occur over time in neutral to alkaline conditions. More preferably, it is 2.7 or less per nm2. On the other hand, there is no limitation on the lower limit, but it is preferably 1 or more per nm2, more preferably 1.5 or more per nm2. If there are too few silanol groups, the affinity with water decreases, and therefore the sedimentation of colloidal silica particles is likely to occur.
[0068] Furthermore, the colloidal silica of the present invention preferably has a silanol group number of 2.70 × 10²⁰ per g or less per unit mass. This is because, with a high number of silanol groups, condensation between silanol groups in a liquid under neutral to alkaline conditions and a decrease in the number of silanol groups over time are more likely to occur, as described above. More preferably, it is 2.50 × 10²⁰ per g or less. On the other hand, there is no limitation on the lower limit, but it is preferably 1.00 × 10²⁰ per g or more, and more preferably 1.20 × 10²⁰ per g or more. If there are too few silanol groups, the affinity with water decreases, and therefore the colloidal silica particles are more likely to settle.
[0069] Furthermore, regarding the number of silanol groups per unit mass, the change rate when maintained for 7 days under the same conditions, preferably at a temperature of 60°C, is preferably -7% or more, and more preferably -5% or more. On the other hand, regarding the upper limit of this rate of change, similarly to the above, it is assumed that there is essentially no new increase in silanol groups. Therefore, considering the variation (variance coefficient) of this rate of change based on the measured value, the upper limit of this rate of change is generally preferably +10% or less, more preferably +5% or less, and even more preferably +3% or less.
[0070] In addition, in the present invention, for the above-mentioned small change over time, the so-called change in silanol group density and silanol group number can also be measured by another method. As one of them, the change over time can be confirmed by measuring the rate of change of the transverse relaxation time [unit: milliseconds (ms)] of the nucleus seed 1H measured by time-domain nuclear magnetic resonance (TD-NMR). Regarding the measurement using TD-NMR, it is described below.
[0071] That is, based on the measurement using TD-NMR, information on the relaxation time can be obtained. The smaller the change in relaxation time, the smaller the change over time on the particle surface.Relaxation, in this context, refers to the process of temporarily absorbed energy decay. Nuclear spins excited by radio waves relax through energy exchange with the surrounding environment and nuclear spins. The time required for this process is called the relaxation time, which can be quantified as T1 (longitudinal relaxation time, spin-lattice relaxation time) and T2 (lateral relaxation time, spin-spin relaxation time). For example, in the case of particles dispersed in water, the response to changes in the magnetic field differs for water in contact with or adsorbed on the particle surface (bound water) and for water in a free state (bulk water) not in contact with the particle surface, resulting in different relaxation times.
[0072] The temporal changes in the particle surface of the colloidal silica of the present invention can be evaluated based on the changes in wettability caused by the silanol groups present on the particle surface, i.e., the aforementioned changes in relaxation time. In the evaluation of wettability, it is suitable to observe the most prevalent nucleus species 1H, and the observed nucleus species is 1H. It is believed that the silanol groups present on the surface of colloidal silica particles interact with the water molecules of the bound water on the particle surface through hydrogen bonds, etc. On the other hand, free water, which has little or no direct interaction with the silanol groups, is also present. Bound water is prone to energy exchange and has a short 1H relaxation time, while free water in a free state has a long 1H relaxation time. That is, under the condition of good wettability, as indicated on page 6 / 20 of the specification (CN 122228218 A), a state with a large number of hydrogen bonds and a large amount of bound water indicates a shorter relaxation time. Moreover, regarding the relaxation time mentioned here, since it is easily affected by molecular mobility and interactions, it is suitable for evaluating the physical properties of the sample, so the transverse relaxation time is preferred. In addition, for the determination of transverse relaxation time, the Carr-Purcell-Meiboom-Gill method (CPMG method) is preferred for theoretical reasons. Although there are no restrictions on other conditions for the determination of transverse relaxation time, it is preferred to perform the measurement at a temperature of 40°C. The reason for preferring 40°C is that it is the temperature at which the molecular motion of many organic and polymeric compounds becomes active. Furthermore, its lower boiling point than water makes it suitable for measuring samples containing moisture. Moreover, it is a temperature where temperature control is easy. At excessively low temperatures, molecular motion may be inhibited, resulting in excessively prolonged relaxation times. Conversely, at excessively high temperatures, moisture may evaporate easily, potentially altering the composition and properties of the sample and reducing measurement accuracy. It should be noted that other measurement conditions besides these can be appropriately determined.
[0073] Furthermore, for the colloidal silica of the present invention, similar to the conditions for the change in silanol group density over time described above, the rate of change in the transverse relaxation time of the seed 1H, measured by time-domain nuclear magnetic resonance (TD-NMR), after being kept at a temperature of 60°C for 7 days is preferably 24% or less. The colloidal silica of the present invention exhibiting such characteristics has good wettability, meaning that the particle dispersibility and the change in silanol groups over time are small. The rate of change in the transverse relaxation time of the seed 1H, measured by TD-NMR, is more preferably 23% or less, and even more preferably 22% or less. On the other hand, for the lower limit of this rate of change in transverse relaxation time, the rate of change is preferably as small as possible, and therefore more preferably 0% or more.
[0074] The transverse relaxation time of the seed 1H, measured by TD-NMR, is preferably less than 1300 ms. More preferably 1100 ms or less, even more preferably 1050 ms or less, and even more preferably 1010 ms or less. On the other hand, for the lower limit value, 650 ms or more is preferred, and 700 ms or more is more preferred. If the transverse relaxation time is too long, it tends to have low wettability to particles in the dispersion medium such as water, which is not preferred. In addition, if the transverse relaxation time is too short, it tends to have high wettability to particles in the dispersion medium such as water and more silanol groups, and therefore tends to increase over time, which is not preferred.
[0075] As for the colloidal silica of the present invention, the silica concentration can be appropriately set according to the application and actual use. As for the concentration of concentrated silica, the preferred embodiment is 1% by mass or more and 40% by mass or less, the more preferred embodiment is 5% by mass or more and 35% by mass or less, and the even more preferred embodiment is 10% by mass or more and 30% by mass or less. In addition, there is no limitation on the pH value. In the actual use, such as in grinding, it is used in both acidic and alkaline conditions, so it is preferred to adjust the colloidal silica itself to a neutral pH of 6.0 or more and 9.0 or less in the pH range of both. Furthermore, due to the aforementioned characteristics, it typically exhibits excellent dispersion stability for several weeks or even years, with very little second-layer separation.
[0076] Regarding the colloidal silica of the present invention, since it can also handle a wide range of particle sizes, the BET specific surface area is preferably 1 to 3000 m² / g, more preferably 2 to 2000 m² / g, and even more preferably 5 to 2700 m² / g. This is because, if the BET specific surface area is too small, the colloidal silica is prone to sedimentation; on the other hand, if the BET specific surface area is too large, it is difficult to determine the smoothness of the particle surface.
[0077] In addition, regarding the colloidal silica of the present invention, there is no limitation on the particle size; it is preferably within the range that allows for the image resolution of the electron microscope described above.Regarding particle size, for example, the BET particle size (nm) obtained from the BET specific surface area is preferably 1nm to 500nm, more preferably 5nm to 300nm, and even more preferably 10nm to 200nm.
[0078] As for the shape of the colloidal silica particles of the present invention, depending on the feed composition, it is possible to produce monodisperse spherical particles (spherical products) or to control the shape of the particles being aggregated together (aggregated products). For example, by using a slightly larger amount of catalyst and slowly introducing the organosilicon ester as a silica raw material into the reaction field, the organosilicon ester is rapidly and uniformly hydrolyzed and gently grown. Therefore, the particles are slowly grown while maintaining a spherical shape, and spherical products can be obtained as described on page 7 / 20 of the specification, CN 122228218 A. Additionally, for example, by using a slightly smaller amount of catalyst and rapidly introducing the organosilicone ester as a silica raw material into the reaction field, the organosilicone ester is hydrolyzed unevenly, thus acting as a binder between particles. The result can be a composite product (cocoon-shaped, chain-like, branched) with a shape that appears to be formed by multiple particles being joined together in two or three dimensions when observed under an electron microscope. The manufacturing method described above can also be used within the scope of the manufacturing method described later.
[0079] Furthermore, regarding the colloidal silica of the present invention, colloidal silica that has undergone known treatments can be used without impairing the purpose of the present invention. For example, dispersion stabilization treatment, surface treatment (e.g., modification treatment, silane coupling agent, polymer, metal oxide, etc.), pH adjustment, ionic strength adjustment, etc., described later can be listed.
[0080] The colloidal silica of the present invention has the above-described characteristics and is therefore suitable for applications such as abrasives (silicon wafers, hard disks, etc.), coatings (eyeglasses, displays, building materials, paper, etc.), and binders (ceramics, catalysts, etc.).
[0081] <Method for Manufacturing Colloidal Silica>
[0082] There are no limitations on the method for manufacturing the colloidal silica of the present invention. In order to give it the above-mentioned characteristics, it is preferable to use a method in which a silica source is reacted with a hydrolysis catalyst selected from organic amines. That is, it is preferable to supply a readily hydrolyzable organosilicon ester to a reaction solution containing a hydrolysis catalyst composed of a mixture of one or more organic amines and react it therewith.
[0083] In the present invention, in the preferred manufacturing method described above, by adjusting the conditions for supplying the readily hydrolyzable organosilicon ester and reacting it therewith, the manufacturing condition constant represented by the following formula (ii) is 0.024 or less.
[0084] Manufacturing condition constant = silica concentration after reaction (mass%) / supply time of easily hydrolyzable organosilicone ester (hr) / reaction temperature (°C) (ii)
[0085] By adjusting in a way that satisfies such a manufacturing condition constant, as described above, it is possible to manufacture colloidal silica particles with less unevenness and smoothness. In addition, preferably, as described above, it is possible to obtain colloidal silica with less change over time on the particle surface. Furthermore, it is preferable to satisfy the above-described silanol group density on the surface of colloidal silica particles, the number of silanol groups per unit mass of colloidal silica, the transverse relaxation time of 1H nuclei determined by TD-NMR, and their rate of change. The above-described manufacturing condition constant is preferably 0.022 or less, more preferably 0.020 or less. There is no limitation on the lower limit value, but the most preferred value is as small as possible. If based on the preferred ranges of silica concentration after reaction, supply time of easily hydrolyzable organosilicone ester, and reaction temperature described later, it is preferably 0.0001 or more. A more preferred lower limit is 0.001 or more, further preferably 0.002 or more, and even more preferably 0.005 or more.
[0086] Regarding the silica concentration after the reaction, it is preferably set to 1 to 40% by mass or less, depending on the intended use and actual application. The silica concentration after the reaction can be adjusted by adjusting the concentration of the readily hydrolyzable organosilicon ester. When the silica concentration is relatively low, the hydrolysis reaction becomes better, so it is preferable that the yield tends to decrease when the concentration is too low. Conversely, when the silica concentration is too high, the hydrolysis reaction tends to be difficult to proceed, so the alkoxy groups of the readily hydrolyzable organosilicon ester tend to remain in large quantities. Therefore, the preferred lower limit of the silica concentration after the reaction is 2% by mass or more, more preferably 4% by mass or more, further preferably 6% by mass or more, and even more preferably 8% by mass or more. On the other hand, the preferred upper limit of the silica concentration after the reaction is 30% by mass or less, more preferably 20% by mass or less, further preferably 15% by mass or less, and even more preferably 12% by mass or less.
[0087] Furthermore, the supply time (hr) of the readily hydrolyzable organosilicone ester is the time required to supply the readily hydrolyzable organosilicone ester to the reaction solution containing a hydrolysis catalyst composed of one or more organic amines. In this invention, the supply time refers to the actual time required for the growth reaction of colloidal silica. For example, in a method where readily hydrolyzable organosilicone ester is further supplied to a reaction solution containing seed particles of colloidal silica with particle growth properties for particle growth, as described in part of the embodiments below, the supply time until the seed particles are obtained is assumed to be excluded from the supply time when the manufacturing condition constant is calculated.That is, in this method, the actual time for supplying the hydrolyzable organosilicon ester to the reaction solution containing the seed particles is set as the supply time when the manufacturing condition constant is calculated. Here, the reason for not including the supply time involved in the reaction until the seed particles are obtained is that, at least within the range of roughness characterized in this invention, since the roughness of the surface where the seed particles are present is completely covered during the subsequent growth reaction, it has no effect on the roughness of the final colloidal silica surface. Similarly, when using seed particles for growing the seed particles (grown seed particles) and carrying out a reaction to further grow the grown seed particles, the time involved in the reaction until the grown seed particles are obtained is not included in the supply time when the manufacturing condition constant is calculated. Moreover, the supply time for calculating the manufacturing condition constant is preferably set to 1 to 100 hours. A longer supply time results in a better hydrolysis reaction, which is preferred, but an excessively long supply time tends to reduce yield. Conversely, a shorter supply time tends to make the hydrolysis reaction difficult to carry out, thus easily leading to a large amount of alkoxy groups remaining in the hydrolyzable organosilicon ester. Therefore, the upper limit of the preferred supply time is more preferably 50 hours or less, and even more preferably 20 hours or less.
[0088] In addition, the reaction temperature (°C) is preferably 40°C or higher and 100°C or lower, more preferably 55°C or higher and 80°C or lower. At low temperatures, the particle size becomes smaller and tends to become larger and more uneven. At excessively low temperatures, the hydrolysis reaction becomes slower and thus agglomerates are formed, which is not preferred. At high reaction temperatures, the hydrolysis reaction proceeds faster and thus the particle size becomes larger and the unevenness tends to become smaller. At excessively high temperatures, the reaction liquid boils and thus side reactions are prone to occur, and small particles are easily formed. It should be noted that, similar to the supply time mentioned above, the reaction temperature is not the reaction temperature involved in the reaction until the seed particles are obtained, but the reaction temperature in the growth reaction of colloidal silica, especially the highest temperature of the reaction, is the reaction temperature at which the manufacturing condition constant is calculated.
[0089] Specifically, regarding the readily hydrolyzable organosilicon esters preferred for use in this invention, it is preferable to use a substance in which 10g of the organosilicon ester and 100g of pure water with impurities of less than 0.1ppb are subjected to a hydrolysis reaction at 25°C under stirring, and the hydrolysis reaction is completed within 1 hour. Examples of such readily hydrolyzable organosilicon esters include trimethyl silicate (hydrolysis reaction time until completion: approximately 3 minutes), tetramethyl silicate (hydrolysis reaction time: approximately 5 minutes), triethyl silicate (hydrolysis reaction time: approximately 5 minutes), and trimethyl methyl silicate (hydrolysis reaction time: approximately 7 minutes), etc.Tetraethyl silicate and organosilicon esters with more carbon atoms tend to gel easily due to their slow hydrolysis rate (hydrolysis reaction time is 24 hours or more), therefore, the above-mentioned easily decomposable organosilicon esters are preferred.
[0090] In addition, there are no limitations on the organic amines preferred as hydrolysis catalysts in this invention, and one or more of the following can be widely used: quaternary ammonium hydroxide, tertiary amines, secondary amines and primary amines, and their carbonates, bicarbonates and silicates. Among them, for example, for quaternary ammonium hydroxide, tetramethylammonium hydroxide (TMAH), tetraethylammonium hydroxide (TEAH), trimethylethylammonium hydroxide, trimethylethanolammonium hydroxide (choline), triethylethanolammonium hydroxide, tetrapropylammonium hydroxide, butylammonium hydroxide, and other quaternary ammonium hydroxides, as well as their carbonates, bicarbonates and silicates. A higher pH is preferred in the hydrolysis reaction, therefore tetramethylammonium hydroxide (TMAH), choline, or tetraethylammonium hydroxide (TEAH) are preferred.
[0091] Furthermore, there are no limitations on the primary, secondary, and tertiary amines used as hydrolysis catalysts, such as amino alcohols, morpholines, piperazines, aliphatic amines, and aliphatic ether amines. Among these, ethanolamine derivatives are preferred, with various amino alcohols being the most common. Examples include monoethanolamine, diethanolamine, triethanolamine, N,N-dimethylethanolamine, N,N-diethylethanolamine, N,N-di-n-butylethanolamine, N-(β-aminoethyl)ethanolamine, N-methylethanolamine, N-methyldiethanolamine, N-ethylethanolamine, N-n-butylethanolamine, N-n-butyldiethanolamine, N-tert-butylethanolamine, and N-tert-butyldiethanolamine.
[0092] Furthermore, regarding morpholine-type organic amines used as hydrolysis catalysts, various morpholine derivatives can be used, preferably including morpholine, N-methylmorpholine, N-ethylmorpholine, etc. Furthermore, regarding piperazine-type organic amines used as hydrolysis catalysts, various piperazine derivatives can be used, preferably including piperazine, hydroxyethylpiperazine, etc. Additionally, regarding aliphatic amines and aliphatic ether amines used as hydrolysis catalysts, as aliphatic amines, alkylamines with 1 to 8 carbon atoms such as triethylamine, dipropylamine, pentylamine, hexylamine, heptylamine, and octylamine are preferably included. Additionally, as aliphatic ether amines, aliphatic ether amines with 1 to 8 carbon atoms such as 2-methoxyethylamine, 3-methoxypropylamine, 3-ethoxypropylamine, 3-propoxypropylamine, 3-isopropoxypropylamine, and 3-butoxypropylamine are preferably included.
[0093] In addition to being used alone, these organic amines used as hydrolysis catalysts can be used in mixtures of two or more as needed.
[0094] Regarding the reaction solution, it comprises the readily hydrolyzable organosilicon ester and the hydrolysis catalyst as described above. In addition, water, alcohols, aldehydes, ketones, surfactants, etc., can be used. Preferably, it comprises a total of 90% by mass or more of the readily hydrolyzable organosilicon ester, the hydrolysis catalyst, and water. More preferably, these are 95% by mass or more.
[0095] In the mixture after the reaction of the readily hydrolyzable organosilicon ester and the hydrolysis catalyst described above (hereinafter sometimes referred to as the "reaction mixture") or in the reaction mixture after the removal of alcohol and dispersion stabilization treatment described later (hereinafter sometimes specifically referred to as the "reaction concentrate"), it is preferable to add the hydrolysis catalyst to the reaction system to carry out the hydrolysis reaction in such a way that the ratio of the hydrolysis catalyst (A) to the readily hydrolyzable organosilicon ester (B) {catalyst residual molar ratio (A / B)} is 0.012 or less, more preferably in the range of 0.00035 to 0.012, and even more preferably in the range of 0.0035 to 0.011. By doing so, the pH of the reaction mixture and the reaction concentrate can be appropriately adjusted, and thickening and gelation can be suppressed, which is therefore preferred.
[0096] There are no particular limitations on the method for achieving such a catalyst residual molar ratio. For example, a method can be listed where a hydrolyzable organosilicon ester is continuously or intermittently introduced into a reaction vessel containing water and hydrolysis catalyst (A) in such a way that the catalyst residual molar ratio (A / B) finally becomes within the range described above. In addition, if the method involves introducing the hydrolysis catalyst and the hydrolyzable organosilicon ester from separate supply routes, methods can be listed where a hydrolysis catalyst and a hydrolyzable organosilicon ester are continuously or intermittently introduced into a reaction vessel containing only water in such a way that the final catalyst residual molar ratio is within the range described above; methods can be listed where a hydrolysis catalyst and a hydrolyzable organosilicon ester are continuously or intermittently introduced into a reaction vessel containing water and a small amount of hydrolysis catalyst (A) in such a way that the final catalyst residual molar ratio is within the range described above, etc.
[0097] Furthermore, seeds of colloidal silica that have particle growth properties obtained by hydrolysis of the silica source prior to the hydrolysis reaction can be introduced into the hydrolysis reaction system. The silica source and hydrolysis catalyst are then slowly added to the reaction system until the catalyst residual molar ratio (A / B) is within the aforementioned range. This allows for the production of colloidal silica with uniform particles, which is therefore preferable.
[0098] It should be noted that, as described above, the readily hydrolyzable organosilicon ester, hydrolysis catalyst, and water used as raw materials for the hydrolysis reaction are substances with low metal impurity content.
[0099] In this invention, it is preferable to remove the alcohol generated from the hydrolyzable organosilicon ester after the reaction of the readily hydrolyzable organosilicon ester with the hydrolysis catalyst.There are no particular limitations on the method for such alcohol removal treatment. For example, methods such as using a distillation tube equipped with a condenser or heating to distill off the alcohol can be listed. By performing such alcohol removal treatment, the alcohol resistance of the materials used in subsequent processes does not need to be considered. Since highly volatile alcohols disappear, it is preferable in terms of stabilizing the concentration of colloidal silica.
[0100] Next, it is preferable to use an acid to stabilize the dispersion of the reaction mixture after the above-described alcohol removal treatment. As such dispersion stabilization treatment, carbon dioxide blowing method or acid solution addition method under stirring can be used. In addition to either carbon dioxide blowing method or acid solution addition method, these methods can be used in combination. In any case, during dispersion stabilization treatment, it is necessary to maintain the reaction mixture in a stirred state by using operations such as carbon dioxide bubbling and stirring.
[0101] When using a carbon dioxide blowing method for dispersion stabilization treatment, the carbon dioxide blown into the reaction mixture can be 100% by volume, or it can be carbon dioxide diluted to about 0.1% by volume with an inactive gas such as nitrogen. Alternatively, it can be air, preferably 100% by volume or more of carbon dioxide diluted with an inactive gas.
[0102] Moreover, regarding the processing conditions of this carbon dioxide blowing method, since the carbon dioxide blowing itself has a stirring effect, it is generally advisable to introduce carbon dioxide into the reaction mixture at a temperature higher than 0°C but less than 100°C, preferably 5°C or higher but less than 80°C, with stirring at a rate preferably greater than 0 mL / min but less than 100,000 mL / min, and more preferably 1 mL / min or more but less than 10,000 mL / min, under a stirring rate of 0 rpm to 3000 rpm, preferably 0 rpm to 1000 rpm.
[0103] In addition, when using an acid solution addition method for dispersion stabilization treatment, the acid solution used is preferably an aqueous acid solution with a concentration of 20% by weight or less, and is a mixture of one or more selected from an aqueous carbonic acid solution, an aqueous dilute inorganic acid solution with a concentration of 20% by weight or less, and an aqueous dilute organic acid solution with a concentration of 20% by weight or less. It is more preferably a mixture of one or more selected from an aqueous dilute inorganic acid solution with a concentration of 10% by weight or less and an aqueous dilute organic acid solution with a concentration of 10% by weight or less.Specifically, the following can be listed: inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid; and organic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylvaleric acid, heptanoic acid, 2-methylhexanoic acid, octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, diethanolic acid, 2-furanic acid, 2,5-furanic acid, 3-furanic acid, 2-tetrahydrofuranic acid, methoxyacetic acid, methoxyphenylacetic acid, phenoxyacetic acid, methanesulfonic acid, ethanesulfonic acid, and hydroxyethanesulfonic acid. The appropriate choice should be made based on the intended use.
[0104] Regarding the processing conditions for adding the acid solution, it is generally advisable to add an acid solution in the range of 0.0001 mol to 10 mol, preferably 0.001 mol to 1 mol, based on acid, to 1 mol of catalyst in the reaction mixture of the object being processed, under stirring at a speed of 1 rpm to 3000 rpm, preferably 10 rpm to 1000 rpm, and preferably 0.001 mol to 1 mol, based on acid, at a temperature of 0°C to 100°C, preferably 5°C to 80°C.
[0105] Furthermore, in the manufacturing method of the present invention, it is preferable to prevent the scattering of the easily hydrolyzable organosilicone ester during supply, and to prevent scattering to the walls or surrounding surfaces of the reaction vessel, and the occurrence of side reactions. This is because if the scattering of the easily hydrolyzable organosilicone ester scatters to the walls or surrounding surfaces of the reaction vessel, it will come into contact with water droplets adhering to the surrounding walls, and a side reaction will occur, thereby potentially introducing unwanted colloidal silica into the reaction solution.
[0106] Therefore, in the manufacturing method of the present invention, it is preferable to supply the silica source to the reaction liquid in a state where the supply port is immersed in the surface of the reaction liquid. This is because: by immersing the supply port in the surface of the reaction liquid, the silica source is supplied (discharged) within the reaction liquid, thereby preventing the silica source from scattering at the supply port and the surface of the reaction liquid as much as possible compared to supplying it from outside the reaction liquid (in the air above the surface of the reaction liquid). At this time, regarding the degree of immersion of the supply port, it is preferable to immerse it for a sufficient length so that the easily hydrolyzable organosilicon ester supplied (discharged) from the supply port does not fly out from the surface of the reaction liquid. More preferably, the length of the immersed supply port can be at least three times the outer diameter of the supply port (or the outer diameter of the outer tube in the case of a nozzle with a double tube structure described later). The upper limit of the length of the impregnation supply port, as specified in the instruction manual (page 11 / 20, CN 122228218 A), can be determined taking into account contact with other equipment (such as stirrers, walls of reaction vessels, bottom surfaces, etc.), and preferably, it can be a length that does not contact the bottom surface inside the reaction vessel.It should be noted that, as long as the purpose of the present invention is not impaired, any known supply port with any shape and size can be used without limitation, such as a commonly used nozzle or pipe with a circular or rectangular discharge portion. There is no limitation on the outer diameter of the supply port; it can typically be set to about 1 mm to 100 mm. Similarly, regarding the reaction vessel for carrying out the reaction, any known reaction vessel with any shape and size can be used without limitation.
[0107] Furthermore, when supplying (discharging) the easily hydrolyzable organosilicon ester while the supply port is immersed in the reaction liquid, it is preferable to have a means to promote or assist the supply (discharge). Examples of such means include using an inactive gas, using a neutral gas that does not react with the easily hydrolyzable organosilicon ester, water, or catalyst. More preferably, by providing a supply port for supplying an inactive gas alongside or separately from the supply port for the easily hydrolyzable organosilicon ester, an inactive gas can be used to promote or assist the supply (discharge) of the easily hydrolyzable organosilicon ester in the reaction liquid. Depending on the purpose, inert gases such as nitrogen, argon, and helium can be used appropriately. By employing such methods, problems such as stagnation near the supply port of the supplied hydrolyzable organosilicon ester and blockage caused by side reactions are avoided, allowing the hydrolysis reaction to proceed sufficiently, which is therefore preferable.
[0108] To more reliably supply the hydrolyzable organosilicon ester to the reaction liquid, from the perspective of reliability and efficiency, the preferred embodiment for supplying the hydrolyzable organosilicon ester is to use a nozzle with an inner and outer double-tube structure, including an outer tube and an inner tube inserted into the outer tube, to supply a silica source or inert gas from each tube. In this case, to suppress the scattering of the hydrolyzable organosilicon ester from the supply port, it is preferable to allow the hydrolyzable organosilicon ester to flow in the inner tube and the inert gas to flow in the outer tube. Regarding such a double-tube structure, any known nozzle with a double-tube structure can be used without limitation. It should be noted that in this case, as long as it includes at least a double tube for supplying easily hydrolyzable organosilicon esters and inactive gases, the pipeline can be multiple.
[0109] Regarding the diameter of the tubes through which the various substances flow using nozzles with such double tube structures, it is preferable that the ratio O / I of the inner diameter (O) of the outer tube supplying the inactive gas relative to the outer diameter (I) of the inner tube supplying the silica source is 1 to 10. This is because by setting such an O / I ratio, the supply effect and efficiency of the inactive gas from the outer tube are improved, and stagnation and blockage near the silica source supply port can be suppressed, tending to achieve a more reliable supply of the silica source.
[0110] Regarding the inner diameter of each tube, it can be appropriately set according to the scale of manufacturing, supply volume, flow rate, etc. Regarding the outer diameter (I) of the inner tube supplying the silica source, it can generally be set to 5 to 96 mm, and more preferably to 4 to 99 mm.Regarding the inner diameter (O) of the outer tube supplying the inactive gas, it can generally be set to 4 to 99 mm, and more preferably to 6 to 98 mm.
[0111] Furthermore, in such an embodiment, it is preferable that the length of the outer tube through which the inactive gas flows is greater than the length of the inner tube through which the easily hydrolyzable organosilicon ester flows. This is because the supply effect and efficiency of the inactive gas from the outer tube are improved, and stagnation and blockage near the supply port of the easily hydrolyzable organosilicon ester can be suppressed, and there is a tendency to achieve a reliable supply.
[0112] Examples
[0113] The preferred embodiments of the present invention will be specifically described below based on examples and comparative examples.
[0114] [Example 1]
[0115] In a 1000-liter (L) stainless steel reaction vessel equipped with a stirrer, a temperature sensor, a heating steam pipe, a cooling water pipe, an exhaust pipe, and an organosilicon ester inlet pipe with a double pipe, 542.58 kg of pure water with a metal impurity content of less than 0.1 ppb and 0.84 kg of triethanolamine were added. Instruction manual, pages 12 / 20, CN 122228218 A
[0116] After loading, it was confirmed that the immersion length of the organosilicon ester inlet tube of the double tube was 20 cm from the liquid surface to the liquid center under stirring. Regarding the double tube, the outer tube has an outer diameter of 25.4 mm, an inner diameter of 22 mm, and a length inside the vessel of 723 mm. The inner tube has an outer diameter of 6.35 mm, an inner diameter of 3.5 mm, and a length inside the vessel of 553 mm.
[0117] After confirmation, using steam and cooling water, while maintaining the liquid temperature in the reaction vessel at 70°C, 198.19 kg of tetramethyl silicate (silica source; manufactured by Tama Chemical Industry Co., Ltd.) with a metal impurity content of less than 10 ppb was continuously supplied to the inside of the double tube, and nitrogen at a flow rate of 0.5 L / min was continuously supplied to the outside tube side under stirring for 10 hours.
[0118] Then, the temperature inside the reaction vessel was reduced to 40°C to produce a 12% by mass product. This product was then transferred to an 800L stainless steel distillation vessel and a 500L stainless steel intermediate vessel, which included a stirrer, a temperature sensor, a pressure sensor, a liquid level control sensor, heating steam piping, cooling water piping, and an exhaust pipe connected to a condenser. The evaporated gas was then heated and cooled by the condenser and distilled off into the distillate receiver. As the liquid level in the distillation vessel decreased, the crude reaction product was supplied from the intermediate vessel. After the crude reaction product was used up from the intermediate vessel, 125.2 kg of pure water was supplied to replace the solvent, yielding a concentrated 20% by mass colloidal silica.
[0119] Carbon dioxide was blown into the concentrate at 1.2 L / min for 10 minutes for dispersion stabilization. Electron microscopy confirmed that the concentrate consisted of smooth, spherical particles with uniform particle size.Image analysis was performed using the steps described later, and the projected area [A] and perimeter [L] of the particles were measured. Using these measurements, the concavity and convexity were calculated using the formula described later. SEM images are shown in Figure 1, STEM images are shown in Figures 2 and 9, and other analytical results are shown in Tables 1 to 3.
[0120] [Example 2]
[0121] In the same apparatus as in Example 1, 179.78 kg of the reaction product of Example 1 as seed particles, 392.47 kg of pure water with a metal impurity content of less than 0.1 ppb and 1.24 kg of triethanolamine were loaded.
[0122] After loading, while maintaining the liquid temperature in the reaction vessel at 80°C, 42.04 kg of tetramethyl silicate (silica source; manufactured by Tama Chemical Industry Co., Ltd.) with a metal impurity content of less than 10 ppb was flowed inside the double tube, and nitrogen at a flow rate of 0.5 L / min was flowed on the outer tube. The mixture was continuously supplied for 10 hours with stirring to obtain 12% by mass of the reaction product. The product was then subjected to the same distillation process as in Example 1. After dispersion stabilization treatment of the concentrate, it was observed under an electron microscope, which confirmed that the particles were smooth spherical particles with uniform particle size. The analysis was performed in the same manner as in Example 1. The STEM image is shown in Figure 9, and the other analytical results are shown in Tables 1 to 3.
[0123] [Example 3]
[0124] In the same apparatus as in Example 1, 73.39 kg of the reaction product of Example 1 as seed particles, 386.45 kg of pure water with a metal impurity content of less than 0.1 ppb and 1.21 kg of triethanolamine were loaded.
[0125] After loading, while maintaining the liquid temperature in the reaction vessel at 80°C, 167.72 kg of tetramethyl silicate (silica source; manufactured by Tama Chemical Industry Co., Ltd.) with a metal impurity content of less than 10 ppb was continuously supplied to the inner side of the double tube while nitrogen at a flow rate of 0.5 L / min was supplied to the outer tube. This process was repeated for 10 hours with stirring to obtain 12% by mass of the reaction product. The product was then subjected to the same distillation process as in Example 1. After dispersion stabilization treatment of the concentrate, electron microscopy was performed, confirming that the particles were uniformly sized, smooth, spherical. The following analysis is the same as in Example 1. SEM images are shown in Figure 3, STEM images in Figures 4 and 9, and other analytical results are shown in Tables 1-3.
[0126] [Example 4]
[0127] In the same apparatus as Example 1, 66.71 kg of the reaction product of Example 1 as seed particles, 507.04 kg of pure water with a metal impurity content of less than 0.1 ppb and 1.30 kg of triethanolamine were loaded.
[0128] After loading, while maintaining the liquid temperature in the reaction vessel at 80°C, 166.57 kg of tetramethyl silicate (silica source; manufactured by Tama Chemical Industry Co., Ltd.) with a metal impurity content of less than 10 ppb was flowed inside the double tube, while 0.5 L / min of nitrogen was flowed on the outer tube. This was continuously supplied for 6 hours with stirring, resulting in a 10% by mass product. The product was then subjected to the same distillation process as in Example 1. After dispersion stabilization treatment of the concentrate, electron microscopy was performed, confirming that the particles were uniformly sized, smooth, spherical. The following analysis is the same as in Example 1. The STEM image is shown in Figure 9, and other analytical results are shown in Tables 1-3.
[0129] [Example 5]
[0130] In the same apparatus as Example 1, 53.36 kg of the reaction product of Example 1 as seed particles, 553.64 kg of pure water with a metal impurity content of less than 0.1 ppb, and 1.31 kg of triethanolamine were loaded.
[0131] After loading, while maintaining the liquid temperature in the reaction vessel at 80°C, 133.25 kg of tetramethyl silicate (silica source; manufactured by Tama Chemical Industry Co., Ltd.) with a metal impurity content of less than 10 ppb was flowed inside the double tube, and nitrogen was continuously supplied at a rate of 0.5 L / min to the outer tube while stirring for 10 hours. After obtaining 8% by mass of the reaction product, the same distillation process as in Example 1 was performed. After dispersion stabilization treatment of the concentrate, electron microscopy was performed to confirm that the particles were smooth spherical particles with uniform particle size. The following analysis was performed in the same manner as in Example 1. The STEM image is shown in Figure 9, and other analytical results are shown in Tables 1 to 3.
[0132] [Example 6]
[0133] In the same apparatus as in Example 1, 437.51 kg of pure water with a metal impurity content of less than 0.1 ppb and 0.32 kg of 3-ethoxypropylamine were charged.
[0134] After charging, while maintaining the liquid temperature in the reaction vessel at 70°C, 190.92 kg of tetramethyl silicate (silica source; manufactured by Tama Chemical Industry Co., Ltd.) with a metal impurity content of less than 10 ppb was flowed inside the double tube, and nitrogen at 0.5 L / min was flowed on the outer tube, and the mixture was continuously supplied with stirring for 6 hours.
[0135] Then, the temperature in the reaction vessel was reduced to 40°C to produce a 12% by mass product. 96.54 kg of this product as seed particles, 486.87 kg of pure water with a metal impurity content of less than 0.1 ppb and 0.88 kg of 3-ethoxypropylamine were charged into the same apparatus as in Example 1.
[0136] After loading, while maintaining the liquid temperature in the reaction vessel at 85°C, 157.34 kg of tetramethyl silicate (silica source; manufactured by Tama Chemical Industry Co., Ltd.) with a metal impurity content of less than 10 ppb was flowed inside the double tube, and nitrogen at a flow rate of 0.5 L / min was flowed on the outer tube. The mixture was continuously supplied for 6 hours with stirring to obtain 10% by mass of the reaction product. After distillation treatment as in Example 1, the concentrate was dispersed and stabilized, and then observed under an electron microscope to confirm that it consisted of smooth spherical particles with uniform particle size. The following analysis was performed in the same manner as in Example 1. The STEM image is shown in Figure 9, and the other analytical results are shown in Tables 1 to 3.
[0137] [Comparative Example 1]
[0138] In the same apparatus as in Example 1, 521.23 kg of pure water with a metal impurity content of less than 0.1 ppb and 0.56 kg of triethanolamine were loaded. Then, while maintaining the liquid temperature in the reaction vessel at 70°C, 227.45 kg of tetramethyl silicate (silica source; manufactured by Tama Chemical Industry Co., Ltd.) with a metal impurity content of less than 10 ppb was continuously supplied to the inner side of the double tube while nitrogen flowed at a rate of 0.5 L / min to the outer tube, under stirring for 6 hours. After obtaining 12% by mass of the reaction product, the same distillation process as in Example 1 was performed. After dispersion stabilization treatment of the concentrate, electron microscopy was performed to confirm that it consisted of uniformly sized, spherical particles with protrusions. The following analysis was performed in the same manner as in Example 1. SEM images are shown in Figure 5, STEM images are shown in Figures 6 and 9, and other analytical results are shown in Tables 1-3.
[0139] [Comparative Example 2]
[0140] 181.73 kg of the reaction liquid of Comparative Example 1 (as seed particles), 396.73 kg of pure water with a metal impurity content of 0.1 ppb or less, and 1.23 kg of triethanolamine were loaded into the same apparatus as in Example 1. Then, while maintaining the liquid temperature in the reaction vessel at 70°C, 170.00 kg of tetramethyl silicate (silica source; manufactured by Tama Chemical Industry Co., Ltd.) with a metal impurity content of 10 ppb or less was continuously supplied to the inner side of the double tube while the nitrogen at 0.5 L / min was continuously supplied to the outer tube side under stirring for 6 hours to obtain 12% by mass of the reaction product. After obtaining the product, the same distillation process as in Example 1 was performed. After dispersion stabilization treatment of the concentrate, the product was observed under an electron microscope, and it was confirmed that the particles were spherical with uniform particle size and protrusions. The following analysis is the same as in Example 1. The STEM image is shown in Figure 9, and the other analysis results are shown in Tables 1 to 3.
[0141] [Comparative Example 3]
[0142] 87.50 kg of the reaction liquid of Comparative Example 1 (as seed particles), 458.07 kg of pure water with a metal impurity content of 0.1 ppb or less, and 1.44 kg of triethanolamine were loaded into the same apparatus as in Example 1.
[0143] After loading, using steam and cooling water, while maintaining the liquid temperature in the reaction vessel at 80°C, 199.88 kg of tetramethyl silicate (silica source; manufactured by Tama Chemical Industry Co., Ltd.) with a metal impurity content of 10 ppb or less was flowed inside the double tube, and nitrogen at 0.5 L / min was flowed on the outer tube side, and the mixture was continuously supplied with stirring for 6 hours. After obtaining 12% by mass of the reaction product, the product was subjected to the same distillation process as in Example 1. After dispersion stabilization treatment of the concentrate, it was observed under an electron microscope, and it was confirmed to be spherical particles with uniform particle size and protrusions. The following analysis is performed in the same manner as in Example 1. SEM images are shown in Figure 7, STEM images are shown in Figures 8 and 9, and other analytical results are shown in Tables 1 to 3.
[0144] [Comparative Example 4]
[0145] 526.45 kg of seed particles of the reaction product obtained under the same conditions as in Example 6, 2218.66 kg of pure water with a metal impurity content of less than 0.1 ppb, and 2.36 kg of 3-ethoxypropylamine were loaded into the same apparatus as in Example 1.
[0146] After loading, while maintaining the liquid temperature in the reaction vessel at 80°C, 180.04 kg of tetramethyl silicate (silica source; manufactured by Tama Chemical Industry Co., Ltd.) with a metal impurity content of less than 10 ppb was continuously supplied to the inner side of the double tube while nitrogen at a flow rate of 0.5 L / min was supplied to the outer tube. This process was repeated for 3 hours with stirring to obtain 12% by mass of the reaction product. The product was then subjected to the same distillation process as in Example 1. After dispersion stabilization treatment of the concentrate, electron microscopy was performed, confirming that the particles were uniform in size and had protrusions, forming spherical particles. The following analysis was performed in the same manner as in Example 1. The STEM image is shown in Figure 9, and other analytical results are shown in Tables 1-3.
[0147] [Table 1] Specification 15 / 20 pages 17 CN 122228218 A
[0148]
[0149] [Table 2] Specification 16 / 20 pages 18 CN 122228218 A
[0150]
[0151] [Table 3] Specification 17 / 20 pages 19 CN 122228218 A
[0152]
[0153] It should be noted that the physical properties of the obtained colloidal silica are evaluated by the following method.
[0154] (1) Silica concentration: The silica concentration is defined as the residue component containing water that has been evaporated.Instruction manual 18 / 20 pages 20 CN 122228218 A
[0155] (2) pH: Measured at 25℃.
[0156] (3) Average particle size nm: The median value of the particle size distribution measured using a disc centrifugal particle size distribution measuring device manufactured by CPS Instruments, USA, is set as the average particle size (nm).
[0157] (4) Electron microscopy (SEM, STEM) observation: The colloidal silica is diluted with water, placed on a TEM indicator film, dried, and observed using a Hitachi High-tech SU9000 ultra-high resolution field emission scanning electron microscope with an observation magnification of 200,000 to 500,000 times, containing more than 20 particles in 1 field of view. The obtained STEM image is read into the Image-Pro software of Bodong Company, the projected area [A] and perimeter [L] of the particles are measured, and the results are read into the calculation software. At the same time, it is compared with the captured SEM image to remove overlapping particle data and particle data that have cut off the surrounding particles. The diameter calculated by assuming the projected area A of the remaining particles as an ideal circle [r1=2(A / π)0.5] is used as the area conversion equivalent circle diameter (r1). In addition, the diameter calculated by assuming the circumference L as an ideal circle [r2=L / π] is used as the circumference conversion equivalent circle diameter (r2), and the average value of r2 / r1 of any 300 particles in the remaining particles is set as the concavity. Figure 9 shows a photograph of each particle being extracted and adjusted to the same size.
[0158] (5) BET specific surface area: The BET specific surface area of the spherical colloidal silica particles constituting the colloidal silica particles is determined by nitrogen adsorption method (BET method).
[0159] (6) BET method particle size: The particle size D2 is derived from the BET specific surface area Sm2 / g in (5) according to the formula D2=2720 / S.
[0160] (7) Silanol (SiOH) density: Take 1.5g of the sample as silica into a beaker. Using a constant temperature bath, while maintaining 25°C, add pure water to make the liquid volume 90mL.
[0161] Add 0.1mol / L hydrochloric acid to make the pH 3.6-3.7.
[0162] Add 30g of sodium chloride, dilute with pure water to 150mL, and stir for 10 minutes.
[0163] Set a pH electrode, and add 0.1mol / L sodium hydroxide solution dropwise while stirring to adjust the pH to 4.0.
[0164] The sample adjusted to pH 4.0 was titrated with 0.1 mol / L sodium hydroxide solution. The titration amount and pH value in the range of pH 8.7 to 9.3 above 4 points were recorded. The titration amount of 0.1 mol / L sodium hydroxide solution was set as X, and the pH value at this time was set as Y. A calibration curve was made, and the titration amount V (mL) to pH 4.0 to 9.0 was calculated by the following formula.
[0165] V = (A × f × 100 × 1.5) / (W × C)
[0166] Where, A is the titration amount (mL) of 0.1 mol / L sodium hydroxide solution required to bring 1.5 g SiO2 to pH 4.0–9.0, f is the potency of 0.1 mol / L sodium hydroxide solution, C is the SiO2 concentration (%) of the sample, and W is the sample amount (g).
[0167] The sodium hydroxide consumption (mmol / g) per 1 g of silicon dioxide is calculated using the following formula.
[0168] Titration amount of sodium hydroxide solution to pH 4.0–9.0: V (mL) / 1.5 (g) × 0.1 (mol / L)
[0169] The mass of silanol per unit surface area (mmol / m2) is calculated using the following formula.
[0170] Sodium hydroxide consumption per 1g of silica (mmol / g) / BET specific surface area (m2 / g)
[0171] The density of silanol groups per unit surface area (units / nm2) is calculated by the following formula.
[0172] Silanol mass per unit surface area (mmol / m2) × 10⁻³ × 10⁻¹⁸ × 6.02 × 10²³ (units / mol)
[0173] In addition, the number of silanol groups per 1g (×10²⁰ units / g) is calculated by the following formula.
[0174] Sodium hydroxide consumption per 1g of silica (mmol / g) × 10⁻³ × 6.02 × 10²³ (units / mol)
[0175] (8) TD-NMR: The transverse relaxation time T2 of the colloidal silica solution was measured using a minispec mq20 TD-NMR instrument from Bruker Corporation. As for the measurement conditions, the measurement was performed under the following conditions: magnetic field: 0.47T, measurement frequency: 20MHz, measurement nucleus: 1H NMR, measurement method: CPMG pulse sequence method, and temperature: 40℃.
[0176] (9) Metal impurity content: The metal impurities (the total of Na, Fe, Cu, Al, K, Cr, Ni, Pb, Mn, Mg, Zn and Ca) were determined using an atomic absorption spectrophotometer with a sample volume of 10g. Instruction manual, pages 19 / 20, 21 CN 122228218 A
[0177] (10) Method for determining changes over time: Each liquid from Examples 1 to 6 and Comparative Examples 1 to 4 was dispensed into three 250 mL polypropylene containers for STEM observation, silica concentration and pH determination, TD-NMR determination, and BET specific surface area, average particle size and silanol group density determination. The containers were then placed in a constant temperature desiccator at 60°C and allowed to return to room temperature for 7 days before each analysis was performed.
[0178] Industrial applicability
[0179] The colloidal silica of the present invention is suitable for applications such as abrasives (silicon wafers, hard disks, etc.), coatings (eyeglasses, displays, building materials, paper, etc.), and adhesives (ceramics, catalysts, etc.).Instruction manual 20 / 20 pages 22 CN 122228218 A Figure 1 Instruction manual Figure 1 / 9 pages 23 CN 122228218 A Figure 2 Instruction manual Figure 2 / 9 pages 24 CN 122228218 A Figure 3 Instruction manual Figure 3 / 9 pages 25 CN 122228218 A Figure 4 Instruction manual Figure 4 / 9 pages 26 CN 122228218 A Figure 5 Instruction manual Figure 5 / 9 pages 27 CN 122228218 A Figure 6 Instruction manual Figure 6 / 9 pages 28 CN 122228218 A Figure 7 Instruction manual Figure 7 / 9 pages 29 CN 122228218 A Figure 8 Instruction manual Figure 8 / 9 pages 30 CN 122228218 A Figure 9 Instruction manual Figure 9 / 9 pages 31 CN 122228218 A.
Claims
1. Colloidal silica, characterized in that, Both of the following conditions must be met: (1) The concavity or convexity expressed by the following formula (i) is 1.0740 or less. Concavity / convexity = Equivalent circle diameter converted from the circumference of the projected image obtained from electron microscope image analysis (i.e., circumference-to-equivalent circle diameter) / Equivalent circle diameter converted from the projected area obtained from electron microscope image analysis (i.e., area-to-equivalent circle diameter) (i) (2) The metal impurities are less than 1 ppm.
2. The colloidal silica according to claim 1, characterized in that, After being kept at 60℃ for 7 days, the change rate of silanol group density was more than -5%.
3. The colloidal silica according to claim 1, characterized in that, Nuclear species were analyzed by time-domain nuclear magnetic resonance after being kept at 60°C for 7 days. 1 The rate of change of the transverse relaxation time of H is less than 24%.
4. The colloidal silica according to claim 1, characterized in that, The density of silanol groups is 3 per nm. 2 the following.
5. The colloidal silica according to claim 1, characterized in that, Nuclear species determined by time-domain nuclear magnetic resonance 1 The transverse relaxation time of H is greater than 650ms but less than 1300ms.
6. The colloidal silica according to claim 1, characterized in that, The electron microscope can be any one or more of the scanning electron microscope (SEM), scanning transmission electron microscope (STEM), and transmission electron microscope (TEM).
7. An abrasive comprising colloidal silica according to any one of claims 1 to 6.
8. A method for producing colloidal silica, comprising supplying a readily hydrolyzable organosilicon ester to a reaction solution containing a hydrolysis catalyst composed of one or more organic amines and reacting it to produce colloidal silica, characterized in that... The manufacturing condition constant represented by the following equation (ii) is 0.024 or less. Manufacturing condition constant = silica concentration after reaction (mass%) / supply time of easily hydrolyzable organosilicone ester (hr) / reaction temperature (°C) (ii).