Electrophoretic media comprising a cationic charge control agent

HK40137546APending Publication Date: 2026-09-11E INK CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
HK62026127214
Authority / Receiving Office
HK · HK
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-01-02
Filing Date
2026-08-07
Publication Date
2026-09-11

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

An electrophoretic medium is disclosed that includes a plurality of charged pigment particles, a charge control agent, and a nonpolar liquid. The molecular structure of the charge control agent includes two quaternary ammonium functional groups, two or more amide functional groups or two or more ester functional groups, and two or more aliphatic diradical units, each of the two or more aliphatic diradical units including a ring structure.
Need to check novelty before this filing date? Find Prior Art

Description

(19) State Intellectual Property Office (12) Invention Patent Application (10) Application Publication Number (43) Application Publication Date (21) Application Number 202480083031.X (22) Application Date 2024.12.23 (30) Priority Data 63 / 616,957 2024.01.02 US (85) PCT International Application Entering National Phase Date 2026.06.29 (86) PCT International Application Application Data PCT / US2024 / 061641 2024.12.23 (87) PCT International Application Publication Data WO2025 / 147410 EN 2025.07.10 (71) Applicant Eink Company Address Massachusetts, USA (72) Inventors E. Buzovje D.S. Bull (74) Patent Agency Beijing Panhua Weiye Intellectual Property Agency Co., Ltd. 11280 Patent Attorney Guo Guangxun (51) Int.Cl. C09B 67 / 22 (2006.01) G02F 1 / 167 (2019.01) G02F 1 / 1675 (2019.01) (54) Invention Title: Electrophoretic Medium Containing Cationic Charge Control Agent (57) Abstract: An electrophoretic medium comprising a plurality of charged pigment particles, a charge control agent, and a nonpolar liquid is disclosed. The molecular structure of the charge control agent comprises two quaternary ammonium functional groups, two or more amide functional groups, or two or more ester functional groups, and two or more aliphatic biradical units, each of which comprises a ring structure. Claims (3 pages), Description (17 pages), Drawings (3 pages), CN 122514573 A, 2026.08.04, CN 1 22 51 45 73 A 1. An electrophoretic medium comprising a plurality of charged pigment particles, a charge control agent, and a nonpolar liquid, wherein the charge control agent has a molecular structure comprising at least two quaternary ammonium functional groups, at least two amide functional groups, or at least two ester functional groups, and two or more aliphatic biradical units, each aliphatic biradical unit comprising a ring structure. 2. The electrophoretic medium of claim 1, wherein each of the two or more aliphatic biradical units contains 28 to 40 carbon atoms. 3. The electrophoretic medium of claim 1 or claim 2, wherein the ring structure comprises a six-membered ring. 4. The electrophoretic medium of claim 3, wherein the six-membered ring comprises a double bond, or wherein the six-membered ring comprises only carbon-carbon single bonds. 5. The electrophoretic medium of claim 4, wherein the six-membered ring has four aliphatic substituents. 6. The electrophoretic medium of claim 5, wherein the substituent of the six-membered ring is alkenyl. 7. The electrophoretic medium of any one of claims 1, 2, 3, 4, and 5, wherein the two or more aliphatic bimetallic rings...Each of the free radical units is independently selected from the molecular structures represented by Formula I and Formula II, Formula I, Formula II. 8. The electrophoretic medium of claim 7, wherein the molecular structure of the charge control agent comprises a group represented by Formula III, Formula III. (Claims 1 / 3 page 2 CN 122514573 A) wherein each Q is independently selected from oxygen and NH groups, each -Z- is independently selected from aliphatic biradical unit -A- and aliphatic biradical unit -B-, -A- is represented by Formula I, and -B- is represented by Formula II, and r is an integer from 1 to 20. 9. The electrophoretic medium of claim 7 or claim 8, wherein the molecular structure of the charge control agent is represented by formula IV, wherein R1, R2 and R3 are independently selected from alkyl, aryl and alkenyl groups, each Q is independently selected from oxygen and NH groups, each -Z- is independently selected from aliphatic diradical unit -A- and aliphatic diradical unit -B-, -A- is represented by formula I and -B- is represented by formula II, and r is an integer from 1 to 20. 10. The electrophoretic medium of claim 7 or claim 8, wherein the molecular structure of the charge control agent is represented by formula V, wherein R1, R2 and R3 are independently selected from alkyl, aryl and alkenyl groups, each Q is independently selected from oxygen and NH groups, each G is independently selected from oxygen, sulfur and NH groups, D is -(CH2)t-, where t is an integer from 3 to 6, each -Z- is independently selected from aliphatic diradical unit -A- and aliphatic diradical unit -B-, -A- is represented by formula I and -B- is represented by formula II, and r is an integer from 1 to 20. 11. The electrophoretic medium of claim 7 or claim 8, wherein the molecular structure of the charge control agent is represented by formula VI, wherein R1, R2, and R3 are independently selected from alkyl, aryl, and alkenyl groups, each Q is independently selected from oxygen and NH groups, each -Z- is independently selected from aliphatic biradical unit -A- and aliphatic biradical unit -B-, -A- is represented by formula I, and -B- is represented by formula II, and r is an integer from 1 to 20. 12. The electrophoretic medium of claim 10, wherein the molecular structure of the charge control agent is represented by formula V, wherein R1, R2, and R3 are methyl groups, G is oxygen or NH, Q is oxygen, D is -(CH2)3-, and -Z- is an aliphatic biradical unit represented by formula I. 13. The electrophoretic medium according to any one of claims 1 to 12, comprising a plurality of charged pigment particles of first, second, and third types, wherein each type of charged pigment particle has a different color from each of the other types of charged pigment particles. 14. The electrophoretic medium according to any one of claims 1 to 13, wherein the weight-average molecular weight of the charge control agent is greater than or equal to 1000.15. The electrophoretic medium according to any one of claims 1 to 14, wherein the weight-average molecular weight of the charge control agent is from 1000 g / mol to 8000 g / mol. 16. The electrophoretic medium according to any one of claims 1 to 15, further comprising a second charge control agent, wherein the second charge control agent comprises a hydrophobic portion and a head group selected from anionic, nonionic, and cationic functional groups. 17. The electrophoretic medium according to any one of claims 1 to 16, wherein the plurality of charged pigment particles are capable of moving through the nonpolar liquid when an electric field is applied. 18. An electro-optic display comprising a light-transmitting conductive layer, an electro-optic material layer, and a substrate comprising a plurality of pixel electrodes, wherein the electro-optic material layer comprises the electrophoretic medium according to any one of claims 1 to 17. 19. The electro-optic display of claim 18, wherein the electrophoretic medium is encapsulated in a plurality of microcapsules or a plurality of microunits. 20. The electro-optic display of claim 19, wherein each of the plurality of microunits comprises a bottom layer, a partition wall, an opening, and a sealing layer, the sealing layer spanning the opening of each microunit. Claims 3 / 3 Page 4 CN 122514573 A Electrophoretic Medium Containing a Cationic Charge Control Agent

[0001] Related Applications

[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 616,957, filed January 2, 2024, which, along with all other patents and patent applications disclosed herein, are incorporated herein by reference in their entirety. Field of the Invention

[0003] The present invention relates to an electrophoretic medium for electro-optic devices, the electrophoretic medium comprising a plurality of charged pigment particles and a cationic charge control agent in a nonpolar liquid. The molecular structure of the charge control agent comprises two quaternary ammonium functional groups, two or more amide functional groups, or two or more ester functional groups, and two or more aliphatic biradical units, each of the two or more aliphatic biradical units comprising a ring structure.

[0004] Background of the Invention

[0005] The term "electro-optic," applied to materials or displays, is used herein in its conventional meaning in the field of imaging to refer to a material having a first display state and a second display state that differ in at least one optical property, said material changing from its first display state to its second display state by applying an electric field to the material. Although the optical property is generally color perceptible to the human eye, it can also be other optical properties, such as optical transmittance, reflectance, brightness, or, in the case of a display intended for machine reading, in the sense of a change in reflectance at electromagnetic wavelengths outside the visible light range, it can be false color.

[0006] For many years, particle-based electrophoretic displays have been a subject of in-depth research and development. In such displays...In electrophoretic displays, multiple charged pigment particles (sometimes referred to as charged particles or pigment particles) move through a fluid under the influence of an electric field. The electric field is typically provided by a conductive film or a transistor, such as a field-effect transistor. Compared to liquid crystal displays (LCDs), electrophoretic displays offer good brightness and contrast, wide viewing angles, bistable states, and low power consumption. However, such electrophoretic displays have a slower switching speed than LCDs, and are generally too slow to display live video. Additionally, electrophoretic displays can be hysteretic at low temperatures because the viscosity of the fluid restricts the movement of charged pigment particles. Despite these drawbacks, electrophoretic displays can be found in everyday items such as e-books (e-readers), mobile phones and mobile phone covers, smart cards, signage, watches, shelf labels, and flash drives.

[0007] The term “gray state” is used herein in its conventional sense in the field of imaging to refer to a state that is between two extreme optical states of a pixel and does not necessarily imply a black-to-white transition between these two extreme states. For example, several E Ink patents and published applications describe electrophoretic displays in which the extreme states are white and dark blue, such that the intermediate "gray state" is light blue. In fact, as already mentioned, the change in optical state may not be a color change at all. The terms "black" and "white" as used below refer to the two extreme optical states of the display and should be understood to generally include extreme optical states that are not strictly black and white, such as the white and dark blue states mentioned above. The term "monochrome" as used below refers to a driving scheme that drives pixels only to their two extreme optical states without an intermediate gray state.

[0008] Many commercial electrophoretic media essentially display only two colors, with a gradient between the black and white extremes, referred to as "grayscale". Such electrophoretic media use a single type of electrophoretic particles of a first color in a coloring fluid with a different second color, or first and second types of charged pigment particles of different first and second colors in an uncolored fluid. In the former case, the first color is displayed when the charged pigment particles are near the viewing surface of the display, and the second color is displayed when the charged pigment particles are spaced apart from the viewing surface. In the latter case, a first color is displayed when charged pigment particles of the first type (page 1 / 17, CN 122514573 A) are near the viewing surface of the display, and a second color is displayed when charged pigment particles of the second type are near the viewing surface. Typically, these two colors are black and white.

[0009] Some electro-optic materials are solid in the sense that the material has a solid outer surface, although the material may and often does have an internal space filled with liquid or gas. Such a display using solid electro-optic materials may, for convenience, be referred to below as a "solid-state electro-optic display." Therefore, the term "solid-state electro-optic display" includes rotating dual-color component displays, encapsulated...Electrophoretic displays, microcell electrophoretic displays, and packaged liquid crystal displays.

[0010] The terms “bistable” and “bistable” are used herein in their conventional meaning in the art to refer to a display comprising display elements having a first display state and a second display state that are different in at least one optical property, and such that after any given element has been driven to present its first or second display state by an addressing pulse of finite duration, the state will persist for at least several times, for example, at least four times, the minimum duration of the addressing pulse required to change the state of the display element after the addressing pulse has terminated. U.S. Patent No. 7,170,670 shows that some particle-based electrophoretic displays capable of having grayscale are stable not only in their extreme black and white states but also in their intermediate gray states, and so are some other types of electro-optical displays. This type of display is more suitably referred to as “multistable” than bistable, but for convenience, the term “bistable” may be used herein to encompass both bistable and multistable displays.

[0011] One type of electro-optic display is a particle-based electrophoretic display, which has been the subject of intensive research and development for many years, in which multiple charged pigment particles move through a fluid under the influence of an electric field. Compared to liquid crystal displays, electrophoretic displays can have properties such as good brightness and contrast, wide viewing angle, bistable state, and low power consumption. Nevertheless, long-term image quality issues of these displays have hindered their widespread use. For example, the charged pigment particles constituting an electrophoretic display tend to settle, resulting in a short lifespan for these displays.

[0012] Numerous patents and applications assigned to or in the name of Massachusetts Institute of Technology (MIT), E Ink Corporation, E Ink California, LLC, and related companies describe various techniques for encapsulated and micro-unit electrophoresis and other electro-optic media. Encapsulated electrophoretic media comprise a plurality of small capsules, each of which contains an electrophoretic medium and a capsule wall surrounding the electrophoretic medium, the electrophoretic medium containing electrophoretically moving pigment particles in a fluid medium. Generally, the capsule itself is held within a polymeric adhesive to form a coherent layer between the two electrodes. In microcell electrophoresis displays, charged pigment particles and fluid are not encapsulated within microcapsules but are retained within a carrier medium, typically multiple cavities formed within a polymeric membrane. [[The following may be used...]]The term "microcavity electrophoretic display" is used to encompass both packaged electrophoretic displays and microcell electrophoretic displays. The technologies described in these patents and applications include:

[0013] (a) electrophoretic particles, fluids, and fluid additives; see, for example, 5,961,804; 6,017,584; 6,120,588; 6,120,839; 6,262,706; 6,262,833; 6,300,932; 6,323,989; 6,377,387; 6,515,649; 6,538,801; 6,580,545; 6,652,075; 6,693,620; 6,721,083; 6,727,881; 6,822,782; 6,831,771; 6,870,661; 6,927 ,892;6,956,690;6,958,849;7,002,728;7,038,655;7,052,766;7,110,162;7,113,323;7,141,688;7,142,351;7,170,670;7,226,550;7,230,750;7,230,751;7,236,290;7,277,218;7,286,279;7,312,916;7,382,514;7,390,901;7,473,782;7,561, 324; 7,583,251; 7,572,394; 7,576,904; 7,580,180; 7,679,814; 7,848,006; 7,903,319; 8,018,640; 8,115,729; 8,257,614; 8,270,064; 8,363,306; 8,390,918; 8,582,196; 8,654,436; 8,902,491; 8,961,831; 9,052,564; 9,341,915; 9,348,193; 9,361,836; 9,366,935; 9, Instruction manual 2 / 17 pages 6 CN 122514573 A 372,380; 9,382,427; 9,423,666; 9,428,649; 9,557,623; 9,670,367; 9,671,667; 9,688,859; 9,726,957; 9,752,034; 9,765,015; 9,778,535; 9,778,537; 9,835,926; 9,953,588; 9,995,987; 10,025,157; ​​10,031,394; 10,040,954; 10,061,123; 10,062,337; 10,147,366; and 10U.S. Patents 514,583; and 2003 / 0048522; 2003 / 0151029; 2003 / 0164480; 2004 / 0030125; 2004 / 0105036; 2005 / 0012980; 2009 / 0009852; 2011 / 0217639; 2012 / 0049125; 2013 / 0161565; 2013 / 0193385; 2013 / 0244149; 2013 / 0063333; 2014 / 0011913; 2014 / 0078576; 2014 / 0104674; 2014 / 0231728; 2015 / 0177590; 2015 / 0185509; 2015 / 0241754; 2015 / 0301425; and 2016 / 0170106 U.S. Patent Application Publications;

[0014] (b) Encapsulation, adhesive, and encapsulation process; see, for example, U.S. Patent Application Publications 5,930,026; 6,067,185; 6,130,774; 6,262,706; 6,327,072; 6,392,786; 6,459,418; 6,727,881, 6,839,158; 6,866,760; 6,922,276; 6, U.S. Patent Nos. 958,848; 6,987,603; 7,110,164; 7,148,128; 7,184,197; 7,304,634; 7,327,511, 7,339, 715; 7,411,719; 7,477,444; 7,561,324; 7,910,175; 7,952,790; 8,129,655; 8,446,664; and U.S. Patent Application Publications Nos. 2005 / 0156340; 2007 / 0091417; and 2009 / 0122389;

[0015] (c) Microunit structures, wall materials, and methods of forming microunits; see, for example, Nos. 6,672,921; 6,751,007; 6,753,067;6,781,745;6,788,452;6,795,229;6,806,995;6,829,078;6,850,355;6,865,012;6,870,662;6,885,495;6,930,818;6,933,098;6,947,202;7,046,228;7,072,095;7,079,303;7,141,279;7,156,945;7,205,355;7,233,429;7,261,920;7,271,947;7,304,780; 7,307,778; 7,327,346; 7,347,957; 7,470,386; 7,504,050; 7,580,180; 7,715,087; 7,767,126; 7,880,958; 8,002,948; 8,154,790; 8,169,690; 8,441,432; 8,891,156; 9,279,906; 9,291,872; 9,388,307; 9,436,057; 9,436,058; 9,470,917; 9,919,553; and 10,401,668 U.S. Patent No. 2003 / 0203101; and U.S. Patent Application Publications Nos. 2003 / 0203101, 2014 / 0050814, and 2016 / 0059442;

[0016] (d) Methods for filling and sealing microcells; see, for example, U.S. Patent Nos. 6,545,797; 6,788,449; 6,831,770; 6,833,943; 6,930,818; 7,046,228; 7,052,571; 7,166,182; 7,347,957; 7,374,634; 7,385,751; 7,408,696; 7,557,981; 7,560,004; 7,564,614; 7 U.S. Patent Nos. 572,491; 7,616,374; 7,715,087; 7,715,088; 8,361,356; 8,625,188; 8,830,561; 9,346,987; and 9,759,978; and U.S. Patent Application Publications Nos. 2002 / 0188053; 2004 / 0120024; 2004 / 0219306; and 2015 / 0098124;

[0017] (e) Films and subassemblies containing electro-optic materials; see, for example, Nos. 6,825,829; 6,982,178; 7,110,164; U.S. Patent Nos. 7,158,282; 7,554,712; 7,561,324; 7,649,666; 7,728,811; 7,826,129; 7,839,564; 7,843,621; 7,843,624; 7,952,790; 8,034,209; 8,177,942; 8,390,301; 9,238,340; 9,470,950; 9,835,925; and U.S. Patent Application Publications Nos. 2005 / 0122563; 2007 / 0237962; and 2011 / 0164301;

[0018] (f) Back panel, adhesive layer, and other auxiliary layers and methods for use in the display; see, for example, section D485,294;5,930,026;6,120,588;6,124,851;6,177,921;6,232,950;6,252,564;6,312,304;6,312,971;6,376,828;6,392,786;6,413,790;6,480,182;6,498,114;6,506,438;6,518,949;6,545,291;6,639,578;6,657,772;6,664,944;6,683,333;6,710,540;6,724,519;6,816, 147; 6,819,471; 6,825,068; 6,831,769; 6,842,279; 6,842,657; 6,865,010; 6,873,452; 6,909,532; 6,967,640; 7,012,600; 7,012,735; 7,030,412; 7,075,703; 7,106,296; 7,110, Instruction manual 3 / 17 pages 7 CN 122514573 A 163; 7,116,318; 7,148,128; 7,167,155; 7,173,752; 7,176,880; 7,190,008; 7,206,119; 7,223,672; 7,230,751; 7,256,766; 7,259,744; 7,301,693; 7,304,780; 7,327,346; 7,327,511; 7,347,957; 7,365,733; 7,388,572; 7,401,758; 7,492,497; 7,535,624; 7,551,346; 7,554 712;7 ,560,004;7 ,583,427;7 ,649,674;7 ,667 ,886;7 ,672,040;7 ,688,497;7 ,826, 129;7,830,592;7,839,564;7,880,958;7,893,435;7,905,977;7,952,790;7,986,450;8, 034 ,209;8,049,947;8,072,675;8,120,836;8,159,636;8,177 ,942;8,237 ,892;8,362, 488; 8,395,836; 8,437,069; 8,441,414; 8,456,589; 8,514,168; 8,547,628; 8,576,162; 8,610,988; 8,714780;8,743,077;8,754 ,859;8,797 ,258;8,797 ,633;8,797 ,636;9,147 , 364;9,025,234;9,025,238;9,030,374;9,140,952;9,201,279;9,223,164;9,238,340;9, 285,648;9,454,057;9,529,240;9,620,066;9,632,373;9,666,142;9,671 ,635;9,715, U.S. Patents Nos. 155; 9,777,201; 9,897,891; 10,037,735; 10,190,743; 10,324,577; 10,365,533; 10,372,008; 10,446,585; 10,466,565; 10,495,941; 10,503,041; 10,509,294; and 10,613,407; and U.S. Patents Nos. 2002 / 0060321; 2004 / 0085619; 2004 / 0105036; 2005 / 0122306; and 2005 / 0122563; U.S. Patent Application Publications Nos. 2006 / 0255322; 2009 / 0122389; 2010 / 0177396; 2011 / 0164301; 2011 / 0292319; 2014 / 0192000; 2014 / 0210701; 2014 / 0368753; and 2016 / 0077375; and International Application Publications Nos. WO2000 / 038000; WO2000 / 005704; and WO1999 / 067678;

[0019] (g) Color formation and color adjustment; see, for example, Nos. 6,017,584; 6,545,797; 6,664,944; 6,788, 452;6,864,875;6,914,714;6,972,893;7,038,656;7,038,670;7,046,228;7,052,571;7,075,502;7,167,155;7,385,751;7,492,505;7,667,684;7,684,108;7,791,789;7,800,813;7,821,702;7,839,564;7,910,175;7,952,790;7,956,841;7,982,941;8,040,594;8,054 ,526;8,098,418;8,159,636;8,213,076;8,363,299;8,422,116;8,441714;8,441 , 716;8,466,852;8,503,063;8,576,470;8,576,475;8,593,721;8,605,354;8,649,084;8, 670,174;8,704 ,756;8,717 ,664;8,786,935;8,797 ,634;8,810,899;8,830,559;8,873, 129;8,902,153;8,902,491;8,917,439;8,964,282;9,013,783;9,116,412;9,146,439;9, U.S. Patents Nos. 164,207; 9,170,467; 9,170,468; 9,182,646; 9,195,111; 9,199,441; 9,268,191; 9,285,649; 9,293,511; 9,341,916; 9,360,733; 9,361,836; 9,383,623; and 9,423,666; and U.S. Patents Nos. 2008 / 0043318; 2008 / 0048970; 2009 / 0225398; 2010 / 0156780; 2011 / 0043543; 2012 / 0326957; 2013 / 0242378; 2013 / 0278995; 2014 / 0055840; 2014 / 0078576; 2014 / 0340430; 2014 / 0340736; 2014 / 0362213; 2015 / 0103394; 2015 / 0118390; 2015 / 0124345; 2015 / 0198858; 2015 / 0234250; 2015 / 0268531; 2015 / 0301246; 2016 / 0011484; 2016 / 0026062; U.S. Patent Application Publications Nos. 2016 / 0048054, 2016 / 0116816, 2016 / 0116818, and 2016 / 0140909;

[0020] (h) A method for driving a display; see, for example, U.S. Patent Application Publications Nos. 5,930,026, 6,445,489, 6,504,524, 6,512,354, 6,531,997, 6,753,999, 6,825,970, 6,900,851, 6,995,550, 7,012,600, 7,023, 420; 7,034,783; 7,061,166; 7,061,662; 7,116,466; 7,119,772; 7,177,066; 7,193,625; 7,202,847; 7,242,514; 7,259,744;7 ,304 ,787;7 ,312,794;7 ,327 ,511;7 ,408,699;7 ,453, 445;7,492,339;7,528,822;7,545,358;7,583,251;7,602,374;7,612,760;7,679,599;7, 679,813;7 ,683,606;7 ,688,297;7 ,729,039;7 ,733,311;7 ,733,335;7 ,787 ,169;7 ,859, 742; 7,952,557; 7,956,841; 7,982,479; 7,999,787; 8,077,141; 8,125,501; 8,139,050; 8,174,490; 8,243,013; 8,274,472; 8,289,250; 8,300,006; 8,305,341; 8,314,784; 8,373, Instruction manual 4 / 17 pages 8 CN 122514573 A 649;8,384,658;8,456,414;8,462,102;8,514,168;8,537,105;8,558,783;8,558,785;8, 558,786;8,558,855;8,576,164;8,576,259;8,593,396;8,605,032;8,643,595;8,665, 206;8,681,191;8,730,153;8,810,525;8,928,562;8,928,641;8,976,444;9,013,394;9, U.S. Patents Nos. 019,197; 9,019,198; 9,019,318; 9,082,352; 9,171,508; 9,218,773; 9,224,338; 9,224,342; 9,224,344; 9,230,492; 9,251,736; 9,262,973; 9,269,311; 9,299,294; 9,373,289; 9,390,066; 9,390,661; and 9,412,314; and U.S. Patents Nos. 2003 / 0102858; 2004 / 0246562; and 2005 / 0253777; 2007 / 0091418; 2007 / 0103427; 2007 / 0176912; 2008 / 0024429; 2008 / 0024482;2008 / 0136774; 2008 / 0291129; 2008 / 0303780; 2009 / 0174651; 2009 / 0195568; 2009 / 0322721; 2010 / 0194733; 2010 / 0194789; 2010 / 0220121; 2010 / 0265561; 2010 / 0283804; 2011 / 0063314; 2011 / 0175875; 2011 / 0193840; 2011 / 0193841; 2011 / 0199671; 2011 / 0221740; 2012 / 0001957; 2012 / 0098740; 2013 / 0063333; 2013 / 0194250; 2013 / 0249782; 2013 / 0321278; 2014 / 0009817; 2014 / 0085355; 2014 / 0204012; 2014 / 0218277; 2014 / 0240210; 2014 / 0240373; 2014 / 0253425; 2014 / 0292830; 2014 / 0293398; 2014 / 0333685; U.S. Patent Application Publications Nos. 2014 / 0340734; 2015 / 0070744; 2015 / 0097877; 2015 / 0109283; 2015 / 0213749; 2015 / 0213765; 2015 / 0221257; 2015 / 0262255; 2015 / 0262551; 2016 / 0071465; 2016 / 0078820; 2016 / 0093253; 2016 / 0140910; and 2016 / 0180777;

[0021] (i) Applications of displays; see, for example, U.S. Patents 6,118,426; 6,473,072; 6,704,133; 6,710,540; 6,738,050; 6,825,829; 7,030,854; 7,119,759; 7,312,784; 7,705,824; 8,009,348; 8,011,592; 8,064,962; 8,162,212; 8,553,012; 8,973,837; 9,188,829; and 9,197,704; and Nos. 2002 / 0090980; 2004 / 0119681; 2007 / 0285385; 2013 / 0176288; 2013 / 0221112; 2013 / 0233930; 2013 / 0235536; 2014 / 0049808; 2014 / 0062391; 2014 / 0206292; and 2016 / 0035291U.S. patent application publication text; and international application publication text WO 00 / 36560; and

[0022] (j) non-electrophoretic displays, such as those in 6,241,921; 6,784,953; 6,795,138; 6,914,713; 6,950,220; 7,095,477; 7,182,830; 7,245,414; 7,420,549; 7,471,369; 7,576,904; 7,580,180; 7, U.S. Patent Nos. 850,867; 8,018,643; 8,023,071; 8,282,762; 8,319,759; and 8,994,705; and U.S. Patent Application Publications Nos. 2005 / 0099575; 2006 / 0262249; 2007 / 0042135; 2007 / 0153360; 2008 / 0020007; 2012 / 0293858; and 2015 / 0277160; and applications of packaging and microcell technologies other than displays; see, for example, U.S. Patent No. 7,615,325; and U.S. Patent Application Publications Nos. 2015 / 0005720 and 2016 / 0012710.

[0023] Although electrophoretic media are often opaque (because, for example, in many types of electrophoretic media, charged pigment particles substantially block visible light from passing through the display) and operate in reflective mode, many types of electrophoretic displays can be operated in so-called “shutter mode,” where one display state is substantially opaque and the other is translucent. See, for example, U.S. Patents 5,872,552; 6,130,774; 6,144,361; 6,172,798; 6,271,823; 6,225,971 and 6,184,856. Dielectrophoretic displays, similar to electrophoretic displays but dependent on changes in electric field strength, can operate in a similar mode; see U.S. Patent 4,418,346. Other types of electro-optic displays may also be able to operate in shutter mode. Electro-optic media operating in shutter mode are useful in multilayer structures of full-color displays; in such structures, at least one layer adjacent to the viewing surface of the display operates in shutter mode to expose or conceal a second layer farther from the viewing surface.

[0024] Encapsulated electrophoretic displays generally do not suffer from the problems of aggregation and sedimentation failure modes of conventional electrophoretic equipment and offer further advantages such as the ability to print or coat the display on a wide variety of flexible and rigid substrates. (Glossary 5 / 17 pages 9 CN 122514573 A The use of “printing” is intended to include all forms of printing and coating, including but not limited to: pre-quantity coating, such as patch die coating)Coating), slot or extrusion coating, ramp or step coating, curtain coating; roll coating, such as roll-lined doctor blade coating, forward and reverse roll coating; gravure coating; dip coating; spray coating; meniscus coating; spin coating; brush coating; air knife coating; screen printing; electrostatic printing; thermal printing; inkjet printing; electrophoretic deposition (see U.S. Patent No. 7,339,715); and other similar techniques). Therefore, the resulting display can be flexible. Furthermore, because the display medium can be printed (using various methods), the display itself can be manufactured at low cost.

[0025] Electrophoretic displays typically comprise an electrophoretic material layer and at least two other layers disposed on opposite sides of the electrophoretic material, one of which is an electrode layer. In most such displays, both layers are electrode layers, and one or both electrode layers are patterned to define the pixels of the display. For example, one electrode layer may be patterned as an elongated row electrode, and another may be patterned as an elongated column electrode extending perpendicularly to the row electrode, the pixel being defined by the intersection of the row and column electrodes. Alternatively and more generally, one electrode layer may have the form of a single continuous electrode, while the other electrode layer may be patterned as a matrix of pixel electrodes, each defining a pixel of the display. In another type of electrophoretic display intended for use with a stylus, the printhead or similar movable electrode is separate from the display, only one of these layers adjacent to the electrophoretic layer includes an electrode, and the layers on the opposite side of the electrophoretic layer are generally protective layers intended to prevent damage to the electrophoretic layer by the movable electrode.

[0026] Manufacturing a three-layer electrophoretic display typically involves at least one lamination operation. For example, many of the aforementioned MIT and E Ink patents and applications describe a method for manufacturing an encapsulated electrophoretic display, wherein an encapsulated electrophoretic medium containing a capsule in an adhesive is coated onto a flexible substrate, the flexible substrate containing an indium tin oxide (ITO) or similar conductive coating on a plastic film (which serves as an electrode of the final display), and the capsule / adhesive coating is dried to form a coherent layer of electrophoretic medium firmly adhered to the substrate. A backplate containing a pixel electrode array and conductors connecting the pixel electrodes to driving circuitry is fabricated separately. To form the final display, the substrate with the capsule / adhesive layer on it is laminated to the backplate using a laminating adhesive. (An electrophoretic display usable with a stylus or similar movable electrode can be fabricated using a very similar method by replacing the backplate with a simple protective layer, such as a plastic film, on which a stylus or other movable electrode can slide). In a preferred form of this method, the backplate itself is flexible and is fabricated by printing the pixel electrodes and conductors onto a plastic film or other flexible substrate. The obvious lamination technique for mass-producing displays using this method is roller lamination, which uses laminating adhesives.

[0027] As discussed in the aforementioned U.S. Patent No. 6,982,178 (see column 3, lines 63 through 5, lines 46), many of the components used in electrophoretic displays, as well as the methods for manufacturing such displays, are derived from technologies used in liquid crystal displays (LCDs). For example, an electrophoretic display may use an active matrix backplane comprising an array of transistors or diodes and corresponding pixel electrode arrays, and “continuous” front electrodes on a transparent substrate (in the sense that the electrodes extend to cover multiple pixels and typically cover the entire display), components that are substantially the same as those in an LCD. However, the methods used to assemble LCDs cannot be used for encapsulated electrophoretic displays. The conventional assembly method for LCDs is as follows: a backplane and front electrodes are formed on separate glass substrates, and the two components are then held together with adhesive, leaving a small hole between them. The resulting assembly is placed under vacuum and immersed in a liquid crystal bath, allowing liquid crystal to flow in through the hole between the backplane and the front electrodes. Finally, after the liquid crystal is in place, the hole is sealed to provide the final display.

[0028] This LCD assembly process cannot be easily transferred to encapsulated displays. Because the electrophoretic material is solid, it must exist between the two components before the backplate and the front electrode are fixed to each other. Furthermore, encapsulated electrophoretic media typically need to be fixed to both, compared to liquid crystal materials that are simply placed between the front electrode and the backplate without being attached to either; in most cases, the electrophoretic media is formed on the front electrode, as this is generally easier than forming the media on the backplate containing the circuitry. The front electrode / electrophoretic media combination is then laminated to the backplate, typically by covering the entire surface of the electrophoretic media with an adhesive and laminating under heat, pressure, and possibly a vacuum. Therefore, the methods for final lamination of solid-state electrophoretic displays in the prior art are essentially batch methods, where the electro-optic media, laminating adhesive, and backplate are (typically) combined before final assembly, with the aim of providing a method more suitable for mass production.

[0029] Electro-optic displays, including electrophoretic displays, can be expensive; for example, the cost of a color LCD found in portable computers typically accounts for a large portion of the overall computer cost. As the use of such displays expands to devices much cheaper than portable computers, such as mobile phones and personal digital assistants (PDAs), the pressure to reduce the cost of such displays is significant. As discussed above, the ability to form an electrophoretic dielectric layer on a flexible substrate using printing technology makes it possible to reduce the cost of the electrophoretic components of the display by using mass production technologies, such as roll-to-roll coating using commercial equipment for producing coated paper, polymer films, and similar media.

[0030] Electro-optic displays typically include an electro-optic material layer and at least two [unclear text - likely referring to two different types of electro-optic displays disposed on opposite sides of the electro-optic material].Other layers, one of which is an electrode layer. In most such displays, both layers are electrode layers, and one or both electrode layers are patterned to define pixels of the display. For example, one electrode layer may be patterned as an elongated row electrode, and the other as an elongated column electrode extending at right angles to the row electrode, the pixel being defined by the intersection of the row and column electrodes. Alternatively and more generally, one electrode layer has the form of a single continuous electrode, while the other electrode layer is patterned as a pixel electrode matrix, each of which defines a pixel of the display. In another type of electro-optic display intended for use with a stylus, a printhead or similar movable electrode is separate from the display, only one of these layers adjacent to the electro-optic layer includes an electrode, and the layers on the opposite side of the electro-optic layer are generally protective layers intended to prevent damage to the electro-optic layer by the movable electrode.

[0031] The aforementioned U.S. Patent No. 6,982,178 describes a method of assembling solid-state electro-optic displays (including encapsulated electrophoretic displays) that is very suitable for mass production. This patent essentially describes a so-called "front panel laminate" ("FPL"), which sequentially comprises a light-transmitting conductive layer, a solid electro-optic dielectric layer electrically in contact with the conductive layer, an adhesive layer, and a release sheet. Generally, the light-transmitting conductive layer is carried by a light-transmitting substrate, preferably flexible in the sense that the substrate can be manually wound onto a roller with a diameter of, for example, 10 inches (254 mm) without permanent deformation. The term "light-transmitting" is used in this patent and herein to indicate that the layer transmission is designed to allow a viewer to see through the layer to observe changes in the display state of the electro-optic dielectric, typically viewed through the conductive layer and adjacent substrates (if present); where the electro-optic dielectric displays changes in reflectivity at non-visible wavelengths, the term "light-transmitting" should of course be interpreted as referring to the transmission of the relevant non-visible wavelengths. The substrate is generally a polymer film and typically ranges in thickness from about 1 to about 25 mil (25 to 634 µm), preferably from about 2 to about 10 mil (51 to 254 µm). The conductive layer is preferably a thin metal or metal oxide layer such as aluminum or ITO, or it may be a conductive polymer. Poly(ethylene terephthalate) (PET) films coated with aluminum or ITO are commercially available, for example, “Aluminized Mylar” (“Mylar” is a registered trademark) from E.I. du Pont de Nemours & Company of Wilmington DE, and this commercial material can be used in the front panel laminate with good results.

[0032] Assembly of an electro-optic display using such a front panel laminate can be achieved by removing the release sheet from the front panel laminate and contacting the adhesive layer with the back panel under conditions that effectively adhere the adhesive layer to the back panel, thereby bonding the adhesive layer, the electro-optic dielectric...The material layer and conductive layer are fixed to the backsheet. This method is well-suited for mass production because the front sheet laminate can be mass-produced, typically using roll-to-roll coating technology, and then cut into sheets of any size required for use with a specific backsheet.

[0033] U.S. Patent No. 7,561,324 describes a so-called “double-sided release sheet,” which is essentially a simplified version of the front sheet laminate of the aforementioned U.S. Patent No. 6,982,178. One form of double-sided release sheet comprises a solid electro-optic dielectric layer sandwiched between two adhesive layers, one or both of which are covered by the release sheet. Another form of double-sided release sheet comprises a solid electro-optic dielectric layer sandwiched between two release sheets. Both forms of double-sided release films are intended for use in a manner generally similar to the described method for assembling an electro-optic display from a front-plane laminate, but involve two separate laminations; generally, in a first lamination, the double-sided release sheet is laminated to the front electrode to form a front sub-assembly, and then in a second lamination, the front sub-assembly is laminated to the backplane to form the final display, although the order of these two laminations can be reversed if desired.

[0034] U.S. Patent No. 7,839,564 describes a so-called “inverted front plane laminate,” a variant of the front plane laminate described in the aforementioned U.S. Patent No. 6,982,178. The inverted front plane laminate sequentially comprises at least one of a light-transmitting protective layer and a light-transmitting conductive layer, an adhesive layer, a solid electro-optic dielectric layer, and a release sheet. The inverted front plate laminate is used to form an electro-optic display with a laminated adhesive layer between the electro-optic layer and the front electrode or front substrate; a second adhesive layer may or may not be present between the electro-optic layer and the back plate, typically a thin adhesive layer. Such an electro-optic display can achieve both good resolution and good low-temperature performance.

[0035] Optical modulators represent a potentially important market for electro-optic media. As the energy performance of buildings and vehicles becomes increasingly important, electro-optic media can be used as coatings on windows (including skylights and sunroofs) to electronically control the proportion of incident radiation transmitted through the window by changing the optical state of the electro-optic media. It is expected that the effective implementation of this “variable transmittance” (“VT”) technology in buildings will achieve: (1) reducing the undesirable heating effect in hot weather, thereby reducing the energy required for cooling, reducing the size of air conditioning equipment, and reducing peak power demand; (2) increasing the use of natural light, thereby reducing lighting power consumption and peak power demand; and (3) increasing the comfort of occupants by improving thermal and visual comfort. In vehicles, the ratio of glass surface area to enclosed volume is expected to yield even greater benefits.Significantly larger than typical buildings. Specifically, the effective implementation of VT technology in vehicles is expected to provide not only the aforementioned benefits, but also: (1) improved driving safety; (2) reduced glare; (3) enhanced rearview mirror performance (by using an electro-optic coating on the rearview mirror); and (4) improved ability to use head-up displays. Other potential applications of VT technology include privacy glass in electronic devices and anti-glare devices.

[0036] If a full-color display is required, an array of color filters can be deposited on the viewing surface of a monochrome (black and white) display. Displays with an array of color filters rely on area sharing and color mixing to produce color stimulation. Available display areas are shared among three or four primary colors such as red / green / blue (RGB) or red / green / blue / white (RGBW), and the color filters can be arranged in a one-dimensional (stripes) or two-dimensional (2×2) repeating pattern. Other options for primary colors or more than three primary colors are also known in the art. Three (in the case of an RGB monitor) or four (in the case of an RGBW monitor) subpixels are chosen to be small enough that at the intended viewing distance, they visually blend together to become a single pixel with uniform color stimulation (“color blending”). An inherent drawback of area sharing is that colorants are always present and can only be modulated by switching the corresponding pixel of the underlying monochrome display to white or black (turning the corresponding primary color on or off). For example, in an ideal RGBW monitor, each of the red, green, blue, and white primary colors occupies one-quarter of the display area (one of the four subpixels), the white subpixel is as bright as the white of the underlying monochrome display, and each of the tinted subpixels is no brighter than one-third of the white of the monochrome display. The overall brightness of white displayed by the monitor cannot exceed half the brightness of the white subpixel. This is due to the fact that the white area of ​​the monitor is produced by displaying one of the four white subpixels plus each tinted subpixel, which exists in its tinted form and is equal to one-third of the white subpixel. Therefore, the combined contribution of the three tinted subpixels does not exceed that of a single white subpixel. The brightness and saturation of the color are reduced due to sharing with the color pixel area switched to black. When mixing yellow, area sharing is particularly problematic because it is brighter than any other color of the same brightness, and saturated yellow is almost as bright as white. Switching blue pixels (a quarter of the display area) to black makes the yellow too dark.

[0037] Alternatively, full-color displays can be provided by using an electrophoretic medium containing multiple colored charged pigment particles with different electrophoretic mobilities. For example, U.S. Patent No. 9,921,451 teaches a colorA color electrophoretic display comprises an electrophoretic medium containing: (a) one type of light-scattering charged pigment particles (typically white); and (b) three substantially non-light-scattering charged pigment particles that provide three subtractive primary colors. Using a substantially non-light-scattering particle type with subtractive primary colors allows for color mixing and provides more color effects on a single pixel than that achieved using color filters. Electrophoretic media and electrophoretic devices exhibit complex properties, especially those containing multiple sets of charged pigments with different charges and mobilities. An important aspect of display operation is the interaction between charge control agents and charged pigment particles. Charge control agents alter the surface charge of the charged pigment particles, enabling them to move selectively under the influence of an applied electric field. Furthermore, charge control agents contribute to the stabilization of charged pigment particles, in terms of particle aggregation. Charge control agents are surfactant-type polymer molecules with one or more polar functional groups (heads) and hydrophobic functional groups (tails). Charge control agents can form reverse micelles in the electrophoretic medium of a display, with the head positioned as a strongly polar core facing the reverse micelle and the tail positioned as a strongly nonpolar outer surface facing the reverse micelle, directly contacting the nonpolar liquid of the electrophoretic medium. Given the structure and function of typical charge control agents, their effectiveness is likely determined by three physical properties: hydrophobicity, charge, and hydrogen bonding ability. The charge control agent should have adequate solubility in the nonpolar liquid of the electrophoretic medium. A commonly used charge control agent has a quaternary ammonium functional group head and a polyester tail, which is formed by the polymerization of aliphatic hydroxycarboxylic acid monomers such as 12-hydroxystearic acid or unsaturated hydroxycarboxylic acid monomers. The inventors of this invention have surprisingly discovered that electrophoretic media containing such cationic charge control agents provide improved electro-optic properties compared to commonly used cationic charge control agents containing linear hydrophobic tails, namely, the molecular structure of said cationic charge control agent comprising two quaternary ammonium functional groups, two or more amide functional groups or two or more ester functional groups, and two or more aliphatic biradical units, each of said two or more aliphatic biradical units comprising a ring structure.

[0038] In one aspect, the present invention provides an electrophoretic medium comprising a plurality of charged pigment particles, a charge control agent, and a nonpolar liquid, wherein the molecular structure of said charge control agent comprises two or more quaternary ammonium functional groups, two or more amide functional groups or two or more ester functional groups, and two or more aliphatic biradical units, each of said two or more aliphatic biradical units comprising a ring structure. Each of said two or more aliphatic biradical units may contain 28 to 40 carbon atoms. The ring structure may include a six-membered ring. The six-membered ring may contain a double bond.The ring may contain only carbon-carbon single bonds. The six-membered ring may have four aliphatic substituents. The substituents of the six-membered ring may be alkenyl.

[0039] Each of the two or more aliphatic biradical units may be selected from the molecular structures represented by Formula I and Formula II. Specification 9 / 17 pages 13 CN 122514573 A

[0040]

[0041] Formula I

[0042]

[0043] Formula II

[0044] The molecular structure of the charge control agent may contain a group represented by Formula III, wherein each Q is independently selected from oxygen and NH groups, wherein each -Z- is independently selected from aliphatic biradical unit -A- and aliphatic biradical unit -B-, -A- is represented by Formula I and -B- is represented by Formula II, and wherein r is an integer from 1 to 20.

[0045]

[0046] Formula III

[0047] The molecular structure of the charge control agent can be represented by Formula IV, wherein R1, R2 and R3 are independently selected from alkyl, aryl and alkenyl groups, wherein each Q is independently selected from oxygen and NH groups, wherein each -Z- is independently selected from aliphatic diradical unit -A- and aliphatic diradical unit -B-, -A- is represented by Formula I and -B- is represented by Formula II, and wherein r is an integer from 1 to 20.

[0048]

[0049] Formula IV

[0050] The molecular structure of the charge control agent can be represented by Formula V, wherein R1, R2 and R3 are independently selected from alkyl, aryl and alkenyl groups, wherein each Q is independently selected from oxygen and NH groups, wherein each G is independently selected from oxygen, sulfur and NH groups, wherein D is -(CH2)t-, wherein t is an integer from 3 to 6, wherein each -Z- is independently selected from aliphatic diradical unit -A- and aliphatic diradical unit -B-, -A- is represented by Formula I and -B- is represented by Formula II, and wherein r is an integer from 1 to 20.

[0051]

[0052] Formula V

[0053] The molecular structure of the charge control agent can be represented by Formula V, wherein R1, R2, and R3 are methyl groups, G is oxygen or NH, Q is oxygen, D is -(CH2)3-, and -Z- is an aliphatic biradical unit represented by Formula I or Formula II. The molecular structure of the charge control agent can be represented by Formula V, wherein R1, R2, and R3 are methyl groups, G is oxygen or NH, and -Z- is an aliphatic biradical unit represented by Formula I. The molecular structure of the charge control agent can be represented by Formula V, wherein R1, R2, and R3 are methyl groups, G is NH, and -Z- is an aliphatic biradical unit represented by Formula I.

[0054] The molecular structure of the charge control agent can be represented by Formula VI, wherein R1, R2, and R3 are independently selected from alkyl, aryl, and alkenyl groups, wherein each Q is independently selected from oxygen and NH groups, and wherein each -Z- is independently selected from an aliphatic diradical unit -A-The aliphatic biradical units -B- and -A- are represented by Formula I, and -B- is represented by Formula II, where r is an integer from 1 to 20.

[0055]

[0056] Formula VI

[0057] The weight-average molecular weight of the charge control agent may be greater than or equal to 1000 g / mol, or from 1000 g / mol to 8000 g / mol.

[0058] The electrophoretic medium of the present invention may further comprise a second charge control agent. The second charge control agent may comprise a hydrophobic portion and a head group selected from anionic, nonionic, and cationic functional groups.

[0059] A plurality of charged pigment particles are capable of moving through a nonpolar liquid when an electric field is applied.

[0060] The electrophoretic medium of the present invention may comprise a plurality of first, second, and third type charged pigment particles, wherein each type of charged pigment particle has a different color than each other type of charged pigment particle. The plurality of charged pigment particles are capable of moving through a nonpolar liquid when an electric field is applied. The electrophoretic medium of the present invention may further comprise a plurality of fourth-type charged pigment particles, each of which has a different color from each of the plurality of first, second, and third-type charged pigment particles. Each of the plurality of first and second-type charged pigment particles may have a negative charge, while each of the plurality of third and fourth-type charged pigment particles may have a positive charge. Each of the plurality of first-type charged pigment particles may have a first charge polarity, while each of the plurality of second, third, and fourth-type charged pigment particles may have a second charge polarity, the second charge polarity being opposite to the first charge polarity.

[0061] On the other hand, the present invention provides an electro-optic display comprising a light-transmitting conductive layer, an electro-optic material layer, and a substrate comprising a plurality of pixel electrodes. The electro-optic material layer comprises an electrophoretic medium containing multiple charged pigment particles, a charge control agent, and a nonpolar liquid. The charge control agent has a molecular structure comprising two quaternary ammonium functional groups, two or more amide functional groups, or two or more ester functional groups, and two or more aliphatic biradical units, each of which contains a ring structure. Each of the two or more aliphatic biradical units may contain 28 to 40 carbon atoms. The ring structure may contain a six-membered ring. The six-membered ring may contain a double bond. The six-membered ring may contain only a carbon-carbon single bond. The six-membered ring may have four aliphatic substituents. The substituents of the six-membered ring may be alkenyl. Each of the two or more aliphatic biradical units may be independently selected from the molecular structures represented by Formula I and Formula II.

[0062] The molecular structure of the charge control agent may contain a group represented by Formula III, wherein each Q is independently selected from oxygen.The charge control agent has an NH group, wherein each -Z- is independently selected from an aliphatic biradical unit -A- and an aliphatic biradical unit -B-, -A- is represented by Formula I, -B- is represented by Formula II, and r is an integer from 1 to 20. The molecular structure of the charge control agent can be represented by Formula IV, wherein R1, R2 and R3 are independently selected from alkyl, aryl and alkenyl groups, wherein each Q is independently selected from an oxygen and an NH group, wherein each -Z- is independently selected from an aliphatic biradical unit -A- and an aliphatic biradical unit -B-, -A- is represented by Formula I, -B- is represented by Formula II, and r is an integer from 1 to 20. The molecular structure of the charge control agent can be represented by formula V, wherein R1, R2 and R3 are independently selected from alkyl, aryl and alkenyl groups, wherein each Q is independently selected from oxygen and NH groups, wherein each G is independently selected from oxygen, sulfur and NH groups, wherein D is -(CH2)t-, wherein t is an integer from 3 to 6, wherein each -Z- is independently selected from aliphatic diradical unit -A- and aliphatic diradical unit -B-, -A- is represented by formula I, -B- is represented by formula II, and wherein r is an integer from 1 to 20. The electrophoretic medium of the electro-optic display can be encapsulated in multiple microcapsules or multiple microunits. The multiple microunits include a bottom layer, a partition wall, an opening and a sealing layer, wherein the sealing layer spans the opening of each microunit.

[0063] Brief Description of the Drawings

[0064] Figure 1 is a side view of a color electro-optic display containing an electrophoretic medium encapsulated in microcapsules. The color electro-optic display sequentially includes: a first electrode layer, an electro-optic material layer, a first adhesive layer and a second electrode layer.

[0065] FIG2 is a side view of a color electro-optic display comprising an electrophoretic medium encapsulated in microcapsules. The color electrophoretic display sequentially comprises: a first electrode layer, a second adhesive layer, an electro-optic material layer, a first adhesive layer, and a second electrode layer.

[0066] FIG3 is a side view of a color electro-optic display comprising an electrophoretic medium encapsulated in microcells. The color electrophoretic display sequentially comprises: a first electrode layer, an electro-optic material layer including a sealing layer, a first adhesive layer, and a second electrode layer.

[0067] FIG4 is a color gamut diagram of an electro-optic display comprising the electrophoretic medium of the present invention and a color gamut diagram of an electro-optic display comprising a contrasting electrophoretic medium.

[0068] Detailed Description of the Invention

[0069] In the following detailed description, many specific details are set forth by way of example in order to provide a thorough understanding of the relevant teachings. However, it will be apparent to those skilled in the art that the present teachings can be practiced without these details.

[0070] The present invention provides an electrophoretic medium comprising charged pigment particles, a charge control agent, and a nonpolar liquid. Particles that absorb, scatter, or reflect light over a wide band or at a selected wavelength are referred to herein as colored particles or pigment particles. The electrophoretic medium can be incorporated into a display, or into a front-panel laminate or an inverted front-panel laminate; the front-panel laminate...The pressure plate and the inverted front plate laminate are combined with the back plate to form a display.

[0071] As used herein, a “head group” of a molecule containing both a hydrophilic and a hydrophobic portion is a functional group of the hydrophilic portion of the molecule. The molecule may have one or more head groups.

[0072] Unless otherwise stated, the term “molecular weight” or “MW” as used herein refers to weight-average molecular weight. Weight-average molecular weight specification 12 / 17 pages 16 CN 122514573 A The amount is measured by gel permeation chromatography.

[0073] As used herein, the term “aliphatic diradical unit” is a molecular structure that is part of a larger molecule, wherein the molecular structure of the diradical unit has two or more terminal atoms, each of which is bonded to another molecular segment or functional group to form a larger molecule. That is, a larger molecule containing the “aliphatic diradical unit”, such as the charge control agent here, does not contain single-electron material (reactive radical). For example, in the literature, ethylene-CH2CH2- (or methylene-CH2-) is sometimes referred to as a diradical, even though it is part of a molecule such as dichloroethane (Cl-CH2CH2-Cl), which does not contain any radicals in its unexcited state. In the case of diradical units represented by Formula I and Formula II, the terminal atom of the diradical unit is a carbon atom (part of the terminal -CH2- group).

[0074] An “amide functional group” can be represented by the formula -NC(O)-, and an “ester functional group” by the formula -OC(O)-, both of which contain a carbonyl group (-C=O).

[0075] The electrophoretic medium according to various embodiments of the invention comprises a plurality of charged pigment particles, a charge control agent, and a nonpolar liquid. The molecular structure of the charge control agent comprises two or more quaternary ammonium functional groups, two or more amide functional groups, or two or more ester functional groups, and two or more aliphatic diradical units, each of which contains a ring structure. Each of the two or more aliphatic biradical units may contain 28 to 40 carbon atoms.

[0076] The ring structure may comprise a six-membered ring. The six-membered ring may comprise a double bond. The six-membered ring may comprise only a carbon-carbon single bond. The six-membered ring may comprise a double bond. The six-membered ring may have four aliphatic substituents. Each of the two or more aliphatic biradical units may be a molecular structure represented by Formula I or Formula II.

[0077] The molecular structure of the charge control agent may comprise one or more groups represented by Formula III. In Formula III, each Q is independently selected from oxygen and NH groups, and each -Z- is independently selected from aliphatic biradical unit -A- and aliphatic biradical unit -B-, -A- is represented by Formula I, and -B- is represented by Formula II. In Formula III, r may be an integer from 1 to 20. In Formula II, r may be an integer from 1 to 20.The values ​​are integers from 1 to 18, 2 to 16, 2 to 14, 3 to 20, 4 to 18, 5 to 16, or 5 to 14. Oxygen is divalent (-O-). The NH group is also divalent (-N(H)-).

[0078] The molecular structure of the charge control agent can be represented by Formula IV. In Formula IV, R1, R2, and R3 are independently selected from alkyl, aryl, and alkenyl groups, each Q is independently selected from oxygen and NH groups, each -Z- group in Formula IV is independently selected from aliphatic biradical unit -A- and aliphatic biradical unit -B-, -A- is represented by Formula I, -B- is represented by Formula II, and r can be an integer from 1 to 20. In Formula IV, r can be an integer from 1 to 18, 2 to 16, 2 to 14, 3 to 20, 4 to 18, 5 to 16, or 5 to 14.

[0079] The molecular structure of the charge control agent can be represented by Formula V. In Formula V, R1, R2, and R3 are independently selected from alkyl, aryl, and alkenyl groups; each Q is independently selected from oxygen and NH groups; each G is independently selected from oxygen, sulfur, and NH groups; D is -(CH2)t-, where t is an integer from 3 to 6; each -Z- in Formula V is independently selected from aliphatic diradical unit -A- and aliphatic diradical unit -B-, -A- is represented by Formula I, -B- is represented by Formula II, and r is an integer from 1 to 20. In Formula V, r can be an integer from 1 to 18, 2 to 16, 2 to 14, 3 to 20, 4 to 18, 5 to 16, or 5 to 14. In Formula V, t can be an integer from 3 to 6, 3 to 5, or 3 to 4. In Formula V, t can be 3, 4, 5, or 6. Oxygen and sulfur are divalent (-O-; -S-). NH groups are also divalent (-N(H)-).

[0080] The molecular structure of the charge control agent can be represented by Formula VI. In Formula VI, R1, R2, and R3 are independently selected from alkyl, aryl, and alkenyl groups, each Q is independently selected from oxygen and NH groups, each -Z- group in Formula VI is independently selected from aliphatic biradical unit -A- and aliphatic biradical unit -B-, -A- is represented by Formula I, -B- is represented by Formula II, and r is an integer from 1 to 20. In Formula VI, r can be an integer from 1 to 18, 2 to 16, 2 to 14, 3 to 20, 4 to 18, 5 to 16, or 5 to 14.

[0081] The weight-average molecular weight of the charge control agent can be greater than or equal to 500 g / mol, 1000 g / mol, 2000 g / mol, or 3000 g / mol. The weight-average molecular weight of the charge control agent can be from 500 g / mol to 10000 g / mol, 1000 g / mol to 9000 g / mol, 1000 g / mol to 8000 g / mol, 1500 g / mol to 8000 g / mol, or 2000 g / mol to 7000 g / mol.g / mol, or 2000 g / mol to 6000 g / mol.

[0082] Commercially available materials important for forming the charge control agents of the present invention are available from Cargill under the trade codes Pripol™, Priamine™, and Priplast™. Specifically, Cargill supplies: (a) dimeric acids HOOC-A-COOH and HOOC-B-COOH, (b) dimeramines H2N-A-NH2 and H2N-B-NH2, (c) dimerols HO-A-OH and HO-B-OH, and (d) polyesters formed from dimeric acids and dimerols, wherein -A- is a diradical represented by Formula I and -B- is a diradical represented by Formula II. These high-purity dimer products are commercially prepared as Diels-Alder adducts of tall oil fatty acids. These commercial products provide a very useful platform for manufacturing condensation polymers with controlled hydrophobicity, charge, and hydrogen bonding by varying the molecular weight, the conversion from primary amine to quaternary ammonium, and the ester to amide ratio. Therefore, they can be used as charge control agents. That is, for a given set of pigments used in color electro-optic displays, the structure of the polymer can be tailored to achieve an optimal balance of hydrophobicity, charge, and hydrogen bonding. This, in turn, allows for more precise control of pigment aggregation. Another potential benefit of dimer-based charge control agents is that high levels of branching can lead to improved low-temperature performance. The resulting charge control agents can have two or more amide functional groups or two or more ester functional groups. That is, charge control agents can have two, three, four, five, or more amide or ester functional groups. Amide groups are useful because they can form hydrogen bonds with polar functional groups present on the surface of pigment particles, which can improve the effectiveness of the charge control agent in controlling particle charge and particle aggregation stability. On the other hand, if the number of amide groups in the charge control agent is large, its solubility in the nonpolar liquid of the electrophoretic medium may be reduced, thus affecting its effectiveness.

[0083] Dicarboxylic acids and diamines (or diols) can react via a condensation reaction to form oligomers or polymers containing amide bonds (or ester bonds). Dicarboxylic acids can react with mixtures of diamines and diols via a condensation reaction to form oligomers or polymers containing both amide and ester bonds. Depending on the stoichiometry of the reaction, the oligomer or polymer may contain terminal amine functional groups or terminal carboxylic acid functional groups. In the case of oligomers or polymers containing terminal amine functional groups, the two or more terminal amine functional groups can be converted to two or more quaternary ammonium functional groups after reacting with an alkylating agent in one or more steps. Depending on the alkylating agent used, the quaternary ammonium functional groups may contain substituents having one or more carbon-carbon double bonds. The molecular structure of the cationic polymer prepared by the above method is generally represented by Formula IV.

[0084] Another method for forming charge control agents with improved properties is to employ the structure of an oligomer or polymer with carboxylic acid-terminated ends. Specifically, as discussed above, the stoichiometry of the reaction between a dicarboxylic acid and a diamine (or a diol, or a mixture of diamines and diols) can be controlled to form an oligomer or polymer containing terminal carboxyl functional groups. Two or more carboxyl functional groups of this oligomer or polymer can be further reacted with a reagent containing a primary (or secondary) amine and a tertiary amine to form an amide bond, followed by alkylation of the tertiary amine to obtain a quaternary ammonium functional group. An example of such a reagent is 3-(dimethylamino)-1-propanol. Another example is 3-(dimethylamino)-1-propanol, or more generally, a reagent containing a hydroxyl group and a tertiary amine. The product of this method is a charge control agent containing two or more quaternary ammonium functional groups. Various alkylating agents can be used to form the quaternary ammonium functional groups. Depending on the alkylating agent used, the quaternary ammonium functional group may contain substituents having one or more carbon-carbon double bonds. The molecular structure of the cationic polymer prepared by the method described herein can generally be represented by Formula V.

[0085] A typical color electro-optic display may have an electro-optic material layer containing an electrophoretic medium encapsulated in microcapsules or microunits, as described in U.S. Patent No. 6,982,178. Figure 1 shows an example side view of a portion of the basic structure of a color electro-optic display with microcapsules. The color electro-optic display 100 includes: a first electrode layer 101 containing a light-transmitting electrode, an electro-optic material layer 102, a first adhesive layer 104, and a second electrode layer 103, the second electrode layer containing a plurality of pixel electrodes. The first adhesive layer 104 connects the electro-optic material layer 102 to the second electrode layer. The electro-optic material layer 102 contains a plurality of microcapsules 112. Each microcapsule has a microcapsule wall and contains an electrophoretic medium 122 having charged pigment particles and a charge control agent in a nonpolar liquid. Electrophoretic medium 122 contains a plurality of first-type charged pigment particles and a plurality of second-type charged pigment particles. Electrophoretic medium 122 may also contain a plurality of third-type charged pigment particles. Electrophoretic medium 122 may also contain a plurality of fourth-type charged pigment particles. Electrophoretic medium 122 may also contain a plurality of fifth-type charged pigment particles. Typically, multiple microcapsules are retained within a polymer binder 132. A viewer can view the image of display 100 from viewing side 150. At least one type of charged pigment particle may contain an organic pigment. The molecular structure of the charge control agent comprises two quaternary ammonium functional groups, two or more amide functional groups, or two or more ester functional groups, and two or more aliphatic biradical units, each of which comprises a ring structure.Each of the base units may contain 28 to 40 carbon atoms. The ring structure may contain a six-membered ring. The six-membered ring may contain double bonds. The six-membered ring may contain only carbon-carbon single bonds. The six-membered ring may have four aliphatic substituents.

[0086] Another example of a color electro-optic display is shown in FIG2. FIG2 shows an example side view of a portion of the basic structure of a color electro-optic display with microcapsules. The electro-optic display 200 has a viewing side 150. It sequentially includes: a first electrode layer 101 containing light-transmitting electrodes, a second adhesive layer 105, an electro-optic material layer 102, a first adhesive layer 104, and a second electrode layer 103, the second electrode layer containing a plurality of pixel electrodes. The second adhesive layer 105 connects the first electrode layer 101 and the electro-optic material layer 102. The first adhesive layer 104 connects the electro-optic material layer 102 and the second electrode layer. The electro-optic material layer 102 contains a plurality of microcapsules 112. Each microcapsule has a microcapsule wall and contains an electrophoretic medium 122 having charged pigment particles and a charge control agent in a nonpolar liquid. The electrophoretic medium 122 contains a plurality of first-type charged pigment particles and a plurality of second-type charged pigment particles. The electrophoretic medium may also contain a plurality of third-type charged pigment particles. The electrophoretic medium 122 may also contain a plurality of fourth-type charged pigment particles. The electrophoretic medium 122 may also contain a plurality of fifth-type charged pigment particles. The molecular structure of the charge control agent contains two quaternary ammonium functional groups, two or more amide functional groups, or two or more ester functional groups, and two or more aliphatic biradical units, each of which contains a ring structure. Each of the two or more aliphatic biradical units may contain 28 to 40 carbon atoms. The ring structure may contain a six-membered ring. The six-membered ring may contain double bonds. The six-membered ring may contain only carbon-carbon single bonds. The six-membered ring may have four aliphatic substituents. Typically, multiple microcapsules are retained within a polymer adhesive 132. The color electro-optic material layer 100 may be constructed from a dual-release sheet as described in the background section of this invention.

[0087] The microcapsule color electro-optic display in Figures 1 and 2 may further include a light-transmitting front substrate (not shown in Figures 1 and 2) adjacent to a first electrode layer 101, wherein the electrode layer is disposed between the front substrate and the electro-optic material layer (for the display of Figure 1) or between the front substrate and a second adhesive layer (for the display of Figure 1). The front substrate may be a plastic film, such as a polyethylene terephthalate (PET) sheet with a thickness of 25 to 200 µm. The front substrate may also include one or more other layers, such as a protective layer for absorbing ultraviolet radiation, a barrier layer for preventing oxygen or moisture from entering the display, and an anti-reflective coating for improving the optical properties of the display.

[0088] Figure 3 illustrates an example of a color electro-optic display containing microcells. The color electro-optic display 300 of Figure 3 is based on...The display 300 comprises: a first electrode layer 201, an electro-optic material layer 202, an adhesive layer 204, and a second electrode layer 203, the second electrode layer 203 including a plurality of pixel electrodes. The adhesive layer 204 connects the sealing layer 232 of the electro-optic material layer 202 to the second electrode layer 203. The electro-optic material layer 202 of the color electro-optic display 300 includes a plurality of microcells 212 and a sealing layer 232. Each of the plurality of microcells 212 has a bottom 242, a partition wall 252, and an opening, and the sealing layer 232 spans the opening of each microcell. Each of the plurality of microcells 212 includes an electrophoretic medium 222. The electrophoretic medium 222 includes a plurality of first-type charged pigment particles 272, a plurality of second-type charged pigment particles 262, and a charge control agent in a non-polar liquid. The electrophoretic medium 222 may also include a plurality of third-type charged pigment particles. Electrophoretic medium 222 may also contain multiple type IV charged pigment particles. Electrophoretic medium 222 may also contain multiple type V charged pigment particles. The molecular structure of the charge control agent comprises two quaternary ammonium functional groups, two or more amide functional groups or two or more ester functional groups, and two or more aliphatic biradical units, each of which contains a ring structure. Each of the two or more aliphatic biradical units may contain 28 to 40 carbon atoms. The ring structure may contain a six-membered ring. The six-membered ring may contain double bonds. The six-membered ring may contain only carbon-carbon single bonds. The six-membered ring may have four aliphatic substituents. The colored electro-optic material layer 100 may be constructed from the front-plate laminate described in the background section of this invention. A viewer can view the image of the display 300 from the viewing side 350.

[0089] The micro-unit color electro-optic display of FIG3 may further include a light-transmitting front substrate (not shown in FIG3) adjacent to the first electrode layer 201, wherein the electrode layer is disposed between the front substrate and the electro-optic material layer. The front substrate may be a plastic film, such as a polyethylene terephthalate (PET) sheet with a thickness of 25 to 200 µm. The front substrate may also include one or more other layers, such as a protective layer for absorbing ultraviolet radiation, a barrier layer for preventing oxygen or moisture from entering the display, and an anti-reflective coating for improving the optical properties of the display.

[0090] In the electro-optic displays of FIG1, FIG2 and FIG3, the first electrode layer may be a conductive layer having a thin continuous coating of a conductive material having minimal inherent absorption of electromagnetic radiation in the visible spectrum, such as indium tin oxide (ITO), poly(3,4-ethylenedioxythiophene) poly(styrene sulfonate) (PEDOT: PSS), graphene, etc.

[0091] The micro-units can be manufactured using a batch process as disclosed in U.S. Patent No. 6,933,098 or a continuous roll-to-roll process.The latter provides a continuous, low-cost, high-volume manufacturing technology for producing compartments for a variety of applications, including electro-optical display devices. The micro-unit arrays suitable for the present invention can be manufactured by microimprinting. Examples

[0092] Preparation of Charge Control Agent Examples

[0093] Comparative Example 1

[0094] A charge control agent having a polyricinoleic acid tail and a quaternary ammonium salt head was prepared using the method described in Example 1 of U.S. Patent Application Publication No. 2020 / 0355978A1. The ricinoleic acid monomer was reacted with 3-(dimethylamino)-1-propylamine to generate a polymer having a polyricinoleic acid and an amine head. The amine was methylated with dimethyl sulfate to form a charge control agent of formula XXI, with a weight-average molecular weight of 9038 g / mol (CCA111).

[0095]

[0096] Formula XXI

[0097] Example 2

[0098] Polymerization: 22.72 g of Pripol™ 1009, 62.1 g of Priplast™ 3238, and 15.4 g of toluene (15.4 g) were mixed in a round-bottom flask equipped with a mechanical stirrer, a nitrogen inlet, and a Dean-Stark separator. The mixture was refluxed under nitrogen to 175°C for 3 hours, and water was collected. The mixture was cooled to ambient temperature, at which point 1.313 g of 3-(dimethylamino)-1-propylamine was added, and the resulting mixture was refluxed to 200°C for a total of 11.5 hours. Toluene was added or removed as needed to control the reflux temperature. After cooling, stannous(II) octoate (0.1 g) was added, and the mixture was refluxed again for 4 hours. The resulting polymer mixture was separated (117.2 g), and the solids content was measured to be 70.2%. Pripol™ 1009, page 16 / 17, CN 122514573 A (provided by Cargill), is a dimer acid HOOC-X-COOH, where X is represented by a diradical unit of formula II. Priplast™ 3238 (provided by Cargill) is an amorphous polyester polyol with a molecular weight of 2000 g / mol.

[0099] Quaternization: 86.50 g of a separated polymer mixture was mixed with 50.0 g of toluene and stirred under nitrogen. 1.107 g of dimethyl sulfate was added, and the mixture was stirred at ambient temperature to complete the quaternization reaction. The product was vacuum stripped to remove volatiles, yielding the quaternized polymer. Such quaternized polymers are usually represented by formula V.

[0100] Comparative Example 3

[0101] Preparation of Electrophoretic Medium and Electro-optic Display

[0102] Using white, cyan, magenta and yellow charged pigment particles, charge control agent from Comparative Example 1 and IsoparE was used to prepare the electrophoretic medium. White charged pigment particles carried a negative charge, while cyan, magenta, and yellow charged pigment particles carried a positive charge. The electro-optic display illustrated in FIG3 was prepared using the electrophoretic medium.

[0103] Example 4

[0104] Preparation of electrophoretic medium and electro-optic display

[0105] An electrophoretic medium was prepared using white, cyan, magenta, and yellow charged pigment particles, a charge control agent from Example 2, and Isopar E. White charged pigment particles carried a negative charge, while cyan, magenta, and yellow charged pigment particles carried a positive charge. The electro-optic display illustrated in FIG3 was prepared using the electrophoretic medium.

[0106] Measurement of color gamut of electro-optic display

[0107] Each electro-optic display from Comparative Example 3 and Example 4 was electrically driven at 25°C to produce various optical states, and its reflectance spectrum was acquired using a spectrophotometer. The CIE L*, a*, and b* values ​​of the reflected light from each electrophoretic display were measured. For each spectral sample, the minimum distance, in units of ΔE*, between the display's color in the L*a*b* color space and each of the eight SNAP (Newsprint Advertising Production Specification) standard primary colors was calculated. The complete color gamut of all measurement points was extracted. The primary colors are red, green, blue, yellow, cyan, magenta, white, and black (R, G, B, Y, C, M, W, and K). The smaller this distance, the closer the performance of the electrophoretic display is to the SNAP target, indicating better color saturation in the display's optical state. The color gamut results of the embodiments and comparative embodiments of the present invention are summarized in Figure 4. The solid lines in the figure correspond to the color gamut of the electro-optic display of the present invention from Example 4, the wide dashed lines correspond to the color gamut of the comparative electro-optic display from Example 3, and the narrow dashed lines correspond to the color standard (SNAP).

[0108] From the color gamut diagram in Figure 4, it can be concluded that the electrophoretic medium containing the charge control agent of the present invention provides a wider total color gamut volume (58100) compared to the system containing the control charge control agent (45000).

[0109] The improved performance of the charge control agent of the present invention is likely due to the presence of (a) two cationic groups (quaternary ammonium groups) and (b) branched alkyl groups in the molecular structure of the charge control agent. This structure may provide reverse micelles with branched hydrophobic rings on their surface, thereby increasing the stability of the micelles in nonpolar liquids of the electrophoretic medium. Furthermore, the branched structure of the charge control agent of the present invention is expected to improve its solubility and its low-temperature electro-optic properties, even at low temperatures. (See Figures 1-3, 22, CN 122514573 A, 23, CN 122514573 A, 24, CN 122514573 A)

Claims

1. An electrophoretic medium comprising a plurality of charged pigment particles, a charge control agent, and a nonpolar liquid, wherein the molecular structure of the charge control agent comprises at least two quaternary ammonium functional groups, at least two amide functional groups, or at least two ester functional groups, and two or more aliphatic diradical units, each aliphatic diradical unit comprising a ring structure.

2. The electrophoretic medium of claim 1, wherein each of the two or more aliphatic diradical units contains 28 to 40 carbon atoms.

3. The electrophoretic medium according to claim 1 or claim 2, wherein the ring structure comprises a six-membered ring.

4. The electrophoretic medium of claim 3, wherein the six-membered ring comprises a double bond, or wherein the six-membered ring comprises only carbon-carbon single bonds.

5. The electrophoretic medium of claim 4, wherein the six-membered ring has four aliphatic substituents.

6. The electrophoretic medium of claim 5, wherein the substituent of the six-membered ring is an alkenyl group.

7. The electrophoretic medium according to any one of claims 1, 2, 3, 4, and 5, wherein each of the two or more aliphatic biradical units is independently selected from the molecular structures represented by formulas I and II. Formula I, Formula II.

8. The electrophoretic medium of claim 7, wherein the molecular structure of the charge control agent comprises a group represented by formula III. Formula III in Each Q is independently selected from oxygen and NH groups. Each -Z- is independently selected from the aliphatic bisradical unit -A- and the aliphatic bisradical unit -B-, where -A- is represented by Equation I and -B- is represented by Equation II, and r is an integer from 1 to 20.

9. The electrophoretic medium of claim 7 or claim 8, wherein the molecular structure of the charge control agent is represented by formula IV. Formula IV in R1, R2, and R3 are independently selected from alkyl, aryl, and alkenyl groups. Each Q is independently selected from oxygen and NH groups. Each -Z- is independently selected from the aliphatic bisradical unit -A- and the aliphatic bisradical unit -B-, where -A- is represented by Equation I and -B- is represented by Equation II, and r is an integer from 1 to 20.

10. The electrophoretic medium of claim 7 or claim 8, wherein the molecular structure of the charge control agent is represented by formula V. Formula V in R1, R2, and R3 are independently selected from alkyl, aryl, and alkenyl groups. Each Q is independently selected from oxygen and NH groups. Each G is independently selected from oxygen, sulfur, and NH groups. D stands for -(CH2) t -, where t is an integer from 3 to 6, Each -Z- is independently selected from the aliphatic bisradical unit -A- and the aliphatic bisradical unit -B-, where -A- is represented by Equation I and -B- is represented by Equation II, and r is an integer from 1 to 20.

11. The electrophoretic medium of claim 7 or claim 8, wherein the molecular structure of the charge control agent is represented by formula VI. Style VI in R1, R2, and R3 are independently selected from alkyl, aryl, and alkenyl groups. Each Q is independently selected from oxygen and NH groups. Each -Z- is independently selected from the aliphatic bisradical unit -A- and the aliphatic bisradical unit -B-, where -A- is represented by Equation I and -B- is represented by Equation II, and r is an integer from 1 to 20.

12. The electrophoretic medium of claim 10, wherein the molecular structure of the charge control agent is represented by formula V, wherein R1, R2, and R3 are methyl groups, G is oxygen or NH, Q is oxygen, D is -(CH2)3-, and -Z- is an aliphatic diradical unit represented by formula I.

13. The electrophoretic medium according to any one of claims 1 to 12, comprising a plurality of charged pigment particles of first, second and third types, wherein each type of charged pigment particle has a different color than each of the other types of charged pigment particles.

14. The electrophoretic medium according to any one of claims 1 to 13, wherein the weight-average molecular weight of the charge control agent is greater than or equal to 1000 g / mol.

15. The electrophoretic medium according to any one of claims 1 to 14, wherein the weight-average molecular weight of the charge control agent is from 1000 g / mol to 8000 g / mol.

16. The electrophoretic medium according to any one of claims 1 to 15, further comprising a second charge control agent, wherein the second charge control agent comprises a hydrophobic portion and a head group selected from anionic, nonionic, and cationic functional groups.

17. The electrophoretic medium according to any one of claims 1 to 16, wherein the plurality of charged pigment particles are capable of moving through the nonpolar liquid when an electric field is applied.

18. An electro-optic display comprising a light-transmitting conductive layer, an electro-optic material layer, and a substrate containing a plurality of pixel electrodes, wherein the electro-optic material layer comprises an electrophoretic medium according to any one of claims 1 to 17.

19. The electro-optic display of claim 18, wherein the electrophoretic medium is encapsulated in a plurality of microcapsules or a plurality of microunits.

20. The electro-optic display of claim 19, wherein each of the plurality of microcells includes a bottom layer, a partition wall, an opening, and a sealing layer, the sealing layer spanning the opening of each microcell.