Temperature-adaptive electric double-layer capacitor with Anti-freeze electrolyte

IN595199BActive Publication Date: 2026-07-13INDIAN INST OF TECH MADRAS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202541057175
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Filing Date
2025-06-13
Publication Date
2026-07-13
Estimated Expiration
2045-06-13

AI Technical Summary

Technical Problem

Conventional aqueous electrolytes in supercapacitors freeze at low temperatures, leading to increased internal resistance, reduced capacitance, and poor energy density, limiting their use in cold environments, while alternative electrolytes like organic and ionic liquids suffer from drawbacks such as high cost or reduced conductivity.

Method used

Incorporating potassium acetate as an antifreeze additive in a KOH-based electrolyte, maintaining a mole ratio of 1:2 to 1:3, to create an electrolyte system that depresses the freezing point and maintains ionic conductivity across a wide temperature range.

Benefits of technology

The potassium acetate-enhanced electrolyte system enables reliable supercapacitor operation from -60°C to +50°C, improving both low-temperature performance and maintaining high-temperature stability, suitable for automotive, aerospace, and outdoor electronics applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

ABSTRACT TEMPERATURE-ADAPTIVE ELECTRIC DOUBLE-LAYER CAPACITOR WITH ANTI-FREEZE ELECTROLYTE The present disclosure provides an electric double-layer capacitor (EDLC) comprising a pair of carbon electrodes and an aqueous electrolyte comprising potassium hydroxide (KOH) and 5 potassium acetate (CH3COOK). The potassium hydroxide and potassium acetate are present in a mole ratio range of 1:2 to 1:3. The EDLC maintains electrochemical stability across a temperature range of -60°C to +50°C. The aqueous electrolyte exhibits a freezing point in a range of -40°C to -60°C. The EDLC retains at least 72% stability at -60°C and at least 90% capacitance retention at +50°C. The carbon electrodes comprise activated carbon. A separator 10 is sandwiched between the pair of carbon electrodes.
Need to check novelty before this filing date? Find Prior Art

Description

FIELD OF THE INVENTION

[0001] The present disclosure relates to energy storage devices, and more particularly toan electric double-layer capacitor with improved temperature adaptability using an antifreezeelectrolyte composition.The present disclosure relates to energy storage devices, and more particularly to an electricdouble layer capacitor with improved electrolyte composition.BACKGROUND OF THE INVENTION

[0002] Supercapacitors, also known as electric double-layer capacitors (EDLCs), havegained significant attention in recent years due to their high power density, rapid chargedcharge capabilities, and long cycle life. These characteristics make them promising energystorage devices for applications ranging from consumer electronics to automotive systems andgrid-scale energy storage. However, one major limitation in their broader application is thetemperature sensitivity of aqueous electrolytes, particularly at sub-zero temperatures.

[0003] Conventional aqueous electrolytes, such as those based on potassium hydroxide(KOH), tend to freeze at low temperatures, severely limiting the performance and reliability ofsupercapacitors in cold environments. This freezing leads to increased internal resistance,reduced capacitance, and poor energy density, restricting their use in applications exposed toextreme temperature variations. Several strategies have been explored to address thislimitation:1. Organic Electrolytes: Researchers have investigated organic electrolytes, whichtypically have lower freezing points than aqueous systems. For example, a researchgroup demonstrated the use of propylene carbonate-based electrolytes insupercapacitors, achieving operation down to -40°C. However, organic electrolytesoften suffer from lower ionic conductivity and higher cost compared to aqueoussystems.2. Ionic Liquids: Ionic liquids have been proposed as alternative electrolytes due to theirwide electrochemical window and low volatility. Another research group reported onan ionic liquid electrolyte that enabled supercapacitor operation at temperatures as lowas -50°C. Despite these advantages, ionic liquids are generally expensive and can havehigh viscosity, limiting power performance.3. Aqueous Electrolyte Modifications: Efforts to improve the low-temperatureperformance of aqueous electrolytes have included the use of various additives such asinvestigation with the addition of ethylene glycol to KOH electrolytes, demonstratingimproved performance down to -20°C. However, organic additives like ethylene glycolcan lead to decreased conductivity and potential electrochemical instability at highertemperatures.4. Salt-based Additives: Inorganic salt additives have shown promise in depressing thefreezing point of aqueous electrolytes without significantly compromisingconductivity. A research group explored the use of potassium formate as an additive inKOH electrolytes, achieving stable operation down to -30°C. This approachdemonstrated the potential of using compatible salt additives to enhance lowtemperature performance.5. Electrode Material Optimization: Some researchers have focused on modifyingelectrode materials to improve low-temperature performance. Wang et al. (2019)developed nitrogen-doped porous carbon electrodes that showed enhanced capacitanceretention at low temperatures. While effective, this approach does not address thefundamental limitations of electrolyte freezing.

[0004] Despite these advancements, there remains a significant need for a simple, costeffective solution that can enhance supercapacitor performance across a wide temperaturerange, particularly at extremely low temperatures, without compromising high-temperatureperformance or long-term stability.SUMMARY OF THE INVENTION

[0005] This summary is provided to introduce a selection of concepts in a simplified formthat are further described below in the detailed description. This summary is not intended toidentify key features or essential features of the claimed subject matter, nor is it intended to beused as an aid in determining the scope of the claimed subject matter.

[0006] In a first aspect of the present disclosure, there is provided an electric doublelayer capacitor (EDLC) comprising: a pair of carbon electrodes; and an aqueous electrolytecomprising potassium hydroxide (KOH) and potassium acetate (CH3COOK), whereinpotassium hydroxide and potassium acetate are present in a mole ratio range of 1:2 to 1:3.

[0007] In a second aspect of the present disclosure, there is provided a method of preparingthe electric double-layer capacitor as provided herein, the method comprising: dissolvingpotassium hydroxide and potassium acetate in water to obtain the aqueous electrolyte, whereinpotassium hydroxide and potassium acetate are present in a mole ratio range of 1:2 to 1:3; andassembling a pair of electrodes in the presence of a separator soaked in the aqueous electrolyteto obtain the electric double-layer capacitor, wherein the separator is sandwiched between thepair of electrodes.

[0008] In a third aspect of the present disclosure, there is provided an energy storagedevice comprising: at least one electric double-layer capacitor as provided herein; and electricalconnections configured for energy storage and discharge, wherein the device is operable inextreme temperature environments ranging from -60°C to +50°C.

[0009] These and other features, aspects, and advantages of the present subject matter will bebetter understood with reference to the following detailed description and appended claims.This summary is provided to introduce a selection of concepts in a simplified form.BRIEF DESCRIPTION OF THE DRAWINGS

[0010] The following drawings form a part of the present specification and are included tofurther illustrate aspects of the present disclosure. The disclosure may be better understood byreference to the drawings in combination with the detailed description of the specificembodiments presented herein.

[0011] Figure 1 illustrates room temperature capacitance variation with and withoutantifreezant, in accordance with an embodiment of the present disclosure.

[0012] Figure 2 illustrates room temperature GCD measurements with and withoutantifreezant, in accordance with an embodiment of the present disclosure.

[0013] Figure 3 illustrates CV at a scan rate of 10 mV / s at varying temperature, inaccordance with an embodiment of the present disclosure.

[0014] Figure 4 illustrates Low temperature charge discharge behaviour of symmetricelectric double-layer capacitor (EDLC), in accordance with an embodiment of the presentdisclosure.

[0015] Figure 5 shows a Nyquist plot derived using EIS technique, in accordance with anembodiment of the present disclosure.

[0016] Figure 6 depicts graph showing Variation in specific capacitance at lowtemperatures, in accordance with an embodiment of the present disclosure.

[0017] Figure 7 depicts a graph showing Variation in specific capacitance at hightemperatures, in accordance with an embodiment of the present disclosure.

[0018] Figure 8 depicts a graph showing stability of the symmetric AC electric doublelayer capacitor (EDLC) at 50°C, in accordance with an embodiment of the present disclosure.DESCRIPTION OF THE INVENTION

[0019] Those skilled in the art will be aware that the present disclosure is subject tovariations and modifications other than those specifically described. It is to be understood thatthe present disclosure includes all such variations and modifications. The disclosure alsoincludes all such steps, features, compositions, and compounds referred to or indicated in thisspecification, individually or collectively, and any and all combinations of any or more of suchsteps or features.Definitions

[0020] For convenience, before further description of the present disclosure, certain termsemployed in the specification, and examples are delineated here. These definitions should beread in the light of the remainder of the disclosure and understood as by a person of skill in theart. The terms used herein have the meanings recognized and known to those of skill in the art,however, for convenience and completeness, particular terms and their meanings are set forthbelow.

[0021] The articles "a", "an" and "the" are used to refer to one or to more than one (i.e.,to at least one) of the grammatical object of the article.

[0022] The terms "comprise" and "comprising" are used in the inclusive, open sense,meaning that additional elements may be included. It is not intended to be construed as"consists of only".

[0023] Throughout this specification, unless the context requires otherwise the word"comprise", and variations such as "comprises" and "comprising", will be understood to implythe inclusion of a stated element or step or group of elements or steps but not the exclusion ofany other element or step or group of element or steps.

[0024] The term "including" is used to mean "including but not limited to". "Including"and "including but not limited to" are used interchangeably.

[0025] The term "electric double-layer capacitor" or "EDLC" as used herein refers to anenergy storage device that stores electrical charge in an electric double layer at the interfacebetween a high surface area electrode, typically made of activated carbon, and an electrolytesolution. This type of capacitor utilizes the separation of charge in a Helmholtz double layer atthe electrode-electrolyte interface to store energy electrostatically, rather than throughelectrochemical reactions as in batteries.

[0026] Ratios, concentrations, amounts, and other numerical data may be presented hereinin a range format. It is to be understood that such range format is used merely for convenienceand brevity and should be interpreted flexibly to include not only the numerical valuesexplicitly recited as the limits of the range, but also to include all the individual numericalvalues or sub-ranges encompassed within that range as if each numerical value and sub-rangeis explicitly recited. For example, concenteration in a range of 3M to 9M should be interpretedto include not only the explicitly recited limits of 3M to 9M, but also to include subranges, suchas 4 to 9 M, 5 to 7 M and so forth, as well as individual values, including fractional values,within the specified ranges, such as 3.1 M, 5.6 M, and 7.5 M.

[0027] Unless defined otherwise, all technical and scientific terms used herein have thesame meaning as commonly understood by one of ordinary skill in the art to which thisdisclosure belongs. Although any methods and materials similar or equivalent to thosedescribed herein can be used in the practice or testing of the disclosure, the preferred methods,and materials are now described. All publications mentioned herein are incorporated herein byreference.

[0028] The present disclosure is not to be limited in scope by the specific embodimentsdescribed herein, which are intended for the purposes of exemplification only. Functionallyequivalent products, compositions, formulations, and methods are clearly within the scope ofthe disclosure, as described herein.

[0029] As discussed in the background section standard water-based electrolytes likepotassium hydroxide (KOH) tend to freeze at low temperatures, which significantly hampersthe efficiency and dependability of supercapacitors in cold climates. This freezing effectincreases internal resistance, lowers capacitance, and diminishes energy density, making themunsuitable for environments with extreme temperature fluctuations. Further the alternativeapproaches also have certain drawbacks apart from few advantage. For e.g. In case of organicelectrolytes, the advantages include that these have lower freezing points than aqueous ones.For instance, propylene carbonate-based systems have been shown to function at -40°C,whereas the drawback is that they typically offer lower ionic conductivity and are moreexpensive. With respect to ionic liquids, the advanatge is that they are known for their broadelectrochemical stability and low evaporation rates, they can operate at temperatures as low as-50°C. However the drawback is their high cost and viscosity can hinder power output. Furtherthe modified aqueous electrolytes with organic additives like ethylene glycol can enhancecold-weather performance (down to -20°C). However the drawback is that these additives mayreduce conductivity and become unstable at higher temperatures. Additionally, the inorganicsalt additives, such as potassium formate can lower the freezing point without greatly affectingconductivity, enabling operation at -30°C, but further research is needed to confirm long-termeffectiveness and compatibility. Moreover, enhancing the electrode materials like usingnitrogen-doped porous carbon, can help retain capacitance in cold conditions, however thismethod doesn't resolve the core issue of electrolyte freezing.

[0030] To overcome this limitation, the present disclosure builds upon the concept of saltbased additives, specifically focusing on potassium acetate (KAc) as an antifreeze agent inKOH-based electrolytes. Potassium acetate has been widely used as a de-icing agent in variousapplications due to its excellent freezing point depression properties. Its compatibility withpotassium-based systems and its ability to maintain high ionic conductivity make it a promisingcandidate for supercapacitor electrolyte modification. Thus the present disclosure aims toaddress the limitations of previous approaches by:1. Providing a simple and cost-effective method to significantly lower the freezing point ofaqueous KOH electrolytes.2. Maintaining or improving ionic conductivity across a wide temperature range.3. Enhancing both low-temperature and high-temperature performance of supercapacitors.4. Ensuring long-term stability and compatibility with activated carbon electrodes.

[0031] By incorporating potassium acetate as an antifreeze additive, this invention seeksto develop a next-generation electrolyte system that enables reliable supercapacitor operationin extreme temperature conditions, thus expanding their potential applications in automotive,aerospace, and outdoor electronics sectors.

[0032] In conclusion the present disclosure electric double-layer capacitor (EDLC)employs potassium acetate as a co-solute in the KOH electrolyte. This binary KOH-CH3COOKsystem effectively depresses the electrolyte's freezing point, thereby maintaining ionic mobilityand preventing electrolyte solidification at sub-zero temperatures. Furthermore, potassiumacetate enhances the electrochemical stability of the electrolyte without compromisingconductivity. The present disclosure thus, delivers a bifunctional electrolyte solution thatsignificantly improves both low- and high-temperature performance in KOH-based aqueoussupercapacitor systems, offering a robust and scalable solution for real-world energy storageapplications.

[0033] The present disclosure relates to electric double-layer capacitors (EDLCs) withimproved temperature adaptability. EDLCs are energy storage devices that store electricalcharge in an electric double layer at the interface between high surface area electrodes and anelectrolyte solution. The EDLCs described herein comprise carbon electrodes and an aqueouselectrolyte containing potassium hydroxide and potassium acetate. The addition of potassiumacetate to the electrolyte enhances the low-temperature performance of the EDLC bysuppressing electrolyte freezing while maintaining electrochemical functionality across a broadtemperature range. This configuration enables more reliable operation of EDLC systems incold climates or fluctuating temperature conditions, making them suitable for variousapplications including automotive, grid storage, and portable electronics.

[0034] The present disclosure is not to be limited in scope by the specific embodimentsdescribed herein, which are intended for the purposes of exemplification only. Functionallyequivalent products, compositions, and methods are clearly within the scope of the disclosure,as described herein.

[0035] In an embodiment of the present disclosure, there is provided an electric doublelayer capacitor (EDLC) comprising: (i) a pair of carbon electrodes; and (ii) an aqueouselectrolyte comprising potassium hydroxide (KOH) and potassium acetate (CH3COOK),wherein potassium hydroxide and potassium acetate are present in a mole ratio range of 1:2 to1:3. The carbon electrodes are composed of activated carbon, which serves as the primaryelectrode material. Activated carbon is selected due to its high surface area and chemicalstability, which are beneficial for charge storage in EDLCs. The activated carbon may bederived from various precursor materials such as coconut shells, wood, or synthetic polymers,and may undergo different activation processes to achieve the desired porosity and surfacecharacteristics. In an embodiment, the carbon electrodes are prepared by mixing activatedcarbon with a binder. Specifically, activated carbon is mixed with polyvinylidene fluoride(PVDF) binder in a ratio of 95:5. This mixture forms an electrode slurry that can be applied toa current collector. The current collector for the carbon electrodes may be carbon cloth. Theelectrode slurry is coated onto the carbon cloth current collector to form the final electrodestructure. The use of carbon cloth as a current collector provides good electrical conductivityand mechanical support for the activated carbon layer. The current collector may also beselected from carbon paper, nickel foam and the like. The EDLC employs a symmetricalconfiguration of the carbon electrodes, often referred to as an AC / / AC configuration. In thisarrangement, both the positive and negative electrodes are made from the same activatedcarbon material. The symmetrical arrangement of activated carbon electrodes allows forefficient charge storage and distribution within the EDLC. During operation, chargeaccumulates at the interface between the activated carbon electrodes and the electrolyte,forming the electric double layer that gives the EDLC its name and charge storage capability.The aqueous electrolyte of the electric double-layer capacitor (EDLC) comprises potassiumhydroxide (KOH) and potassium acetate (CH3COOK). The aqueous electrolyte of the electricdouble-layer capacitor (EDLC) comprises potassium hydroxide (KOH) and potassium acetate(CH3COOK). The potassium hydroxide and potassium acetate are present in the aqueouselectrolyte in a mole ratio range of 1:2 to 1:3. This specific mole ratio range has beendetermined to provide an optimal balance between electrolyte conductivity and freezing pointdepression.

[0036] In an embodiment of the present disclosure, there is provided an electric doublelayer capacitor (EDLC) as described herein, wherein potassium acetate is present in aconcentration in a range of 3 M to 9 M. This specific mole ratio range has been determined toprovide an optimal balance between electrolyte conductivity and freezing point depression.The concentration of potassium acetate in the aqueous electrolyte ranges from 3 M to 9 M. Thisconcentration range of potassium acetate has been found to effectively lower the freezing pointof the electrolyte without significantly increasing its viscosity or compromising its ionicconductivity.

[0037] In an embodiment of the present disclosure, there is provided an electric doublelayer capacitor (EDLC) as described herein, wherein EDLC comprises a separator selectedfrom the group consisting of Polyacrylonitrile (PAN), Nylon, Glass Fiber, Celgard separators,Whatman filter paper, and combinations thereof. The separator serves multiple functions in theEDLC. A primary function of the separator is to prevent direct electrical contact between thepositive and negative electrodes while allowing ion transport through the electrolyte. Thisphysical separation is crucial for maintaining the charge separation that enables the EDLC tostore energy. Additionally, the separator helps retain the electrolyte within its porous structure,ensuring consistent ionic conductivity throughout the device. These materials are selectedbased on their porosity, chemical stability, and compatibility with the aqueous electrolyte usedin the EDLC. Polyacrylonitrile (PAN) separators offer good chemical stability and mechanicalstrength. Nylon separators provide excellent durability and resistance to degradation in alkalineenvironments. Glass Fiber separators are known for their high porosity and thermal stability.Celgard separators, typically made from polypropylene or polyethylene, offer controlledporosity and thin profiles. Whatman filter paper, composed of cellulose fibers, provides a costeffective option with good electrolyte absorption properties. The choice of separator materialmay depend on factors such as the specific electrolyte composition, operating temperaturerange, and desired EDLC performance characteristics. For example, in applications requiringoperation at elevated temperatures, Glass Fiber or Celgard separators may be preferred due totheir thermal stability. During the assembly of the EDLC, the separator is soaked in the aqueouselectrolyte containing potassium hydroxide and potassium acetate. This soaking processensures that the pores of the separator are filled with electrolyte, facilitating ion transportbetween the electrodes during EDLC operation. The electrolyte-soaked separator is then placedbetween the pair of carbon electrodes to complete the EDLC cell assembly. The thickness ofthe separator may be selected based on the desired balance between ionic conductivity andmechanical strength. Thinner separators generally allow for lower internal resistance andhigher power density, while thicker separators may provide enhanced mechanical stability andsafety.

[0038] In an embodiment of the present disclosure, there is provided an electric doublelayer capacitor (EDLC) as described herein, wherein the aqueous electrolyte exhibits a freezingpoint in a range of -40°C to -60°C. The combination of potassium hydroxide and potassiumacetate in these specific concentration ranges results in an aqueous electrolyte with a freezingpoint in the range of -40°C to -60°C. This lowered freezing point enables the EDLC to maintainelectrochemical functionality at temperatures well below the freezing point of conventionalaqueous electrolytes. The aqueous electrolyte may be prepared by dissolving potassiumhydroxide and potassium acetate in water. In an embodiment, a predetermined amount ofpotassium hydroxide is first dissolved in deionized water to create a base solution.Subsequently, potassium acetate is added to the base solution and dissolved to achieve thedesired final concentrations and mole ratio. The resulting solution may be stirred or agitated toensure complete dissolution and homogeneity of the electrolyte components. The use ofpotassium acetate as an antifreeze additive in the aqueous electrolyte provides severaladvantages over conventional organic antifreeze agents such as ethylene glycol or glycerol.Potassium acetate does not significantly increase the viscosity of the electrolyte, which helpsmaintain good ion mobility. Additionally, potassium acetate exhibits high thermal stability anddoes not undergo decomposition or volatilization at elevated temperatures, contributing to theoverall stability and performance of the EDLC across a wide temperature range.

[0039] In an embodiment of the present disclosure, there is provided an electric doublelayer capacitor (EDLC) as described herein, wherein the EDLC maintains electrochemicalstability across a temperature range of -60°C to +50°C. The aqueous electrolyte, containingpotassium hydroxide and potassium acetate, facilitates ion transport between the electrodes.The potassium hydroxide provides high ionic conductivity, while the potassium acetate acts asan antifreeze additive, lowering the freezing point of the electrolyte. This combination allowsfor efficient charge transport across a wide temperature range, from -60°C to +50°C. This broadtemperature range enables operation in diverse environmental conditions.

[0040] In an embodiment of the present disclosure, there is provided an electric double-layercapacitor (EDLC) as described herein, wherein the EDLC retains at least 72% stability at -60°C and at least 90% capacitance retention at +50°C.

[0041] In an embodiment of the present disclosure, there is provided an electric double-layercapacitor (EDLC) as described herein, wherein the electrode comprises activated carbon. Thecarbon electrodes, composed of activated carbon, provide a high surface area for chargestorage. When a voltage is applied to the EDLC, ions from the aqueous electrolyte accumulateat the electrode-electrolyte interface, forming an electric double layer. This double layer storeselectrical charge through electrostatic adsorption of ions onto the electrode surface.

[0042] In an embodiment of the present disclosure, there is provided an electric double-layercapacitor (EDLC) as described herein, wherein the EDLC is operated in applications selectedfrom the group consisting of electric vehicles, aerospace systems, military equipment, coldclimate energy systems, and remote sensing devices. The energy storage devices may comprisea single EDLC or multiple EDLCs connected in series or parallel configurations. In electricvehicles, the EDLC may provide reliable energy storage and power delivery in cold climates,enhancing overall vehicle performance and range. Aerospace systems may benefit from theEDLC's ability to operate across the temperature fluctuations encountered during flight.Military equipment deployed in diverse environmental conditions may utilize the EDLC forconsistent energy storage and rapid power delivery. In cold-climate energy systems, the EDLCmay serve as a reliable energy storage component, maintaining functionality in regions withprolonged periods of sub-zero temperatures. Remote sensing devices deployed in harshenvironments may incorporate the EDLC to ensure consistent power supply and data collectioncapabilities across varying temperature conditions. The EDLC's extended operating range andimproved low-temperature performance offer advantages in terms of reliability, efficiency, andversatility across multiple applications. The use of readily available and cost-effectivematerials, such as activated carbon electrodes and aqueous electrolytes, allows for scalablemanufacturing and integration into existing energy storage systems.

[0043] In an embodiment of the present disclosure, there is provided a method of preparing theelectric double-layer capacitor as described herein, the method comprising: dissolvingpotassium hydroxide and potassium acetate in water to obtain the aqueous electrolyte, whereinpotassium hydroxide and potassium acetate are present in a mole ratio range of 1:2 to 1:3; andassembling a pair of electrodes in the presence of a separator soaked in the aqueous electrolyteto obtain the electric double-layer capacitor, wherein the separator is sandwiched between thepair of electrodes.

[0044] In an embodiment of the present disclosure, there is provided a energy storage devicecomprising: at least one electric double-layer capacitor as described herein ; and electricalconnections configured for energy storage and discharge, wherein the device is operable inextreme temperature environments ranging from -60°C to +50°C.

[0045] In an embodiment of the present disclosure, there is provided a energy storage deviceas described herein, wherein the device comprises a plurality of electric double-layer capacitorsconnected in a series or parallel configuration.

[0046] In an embodiment of the present disclosure, there is provided a energy storage deviceas described herein, wherein the device is configured for high-power applications requiringrapid energy discharge.

[0047] In an embodiment of the present disclosure, there is provided a energy storage deviceas described herein, wherein the energy storage device is configured for use in applicationsselected from the group consisting of electric vehicles, aerospace systems, military equipment,cold-climate energy systems, and remote sensing devices.

[0048] Although the subject matter has been described in considerable detail withreference to certain examples and implementations thereof, other implementations are possible.EXAMPLES

[0049] The disclosure will now be illustrated with working examples, which is intendedto illustrate the working of disclosure and not intended to take restrictively to imply anylimitations on the scope of the present disclosure. Unless defined otherwise, all technical andscientific terms used herein have the same meaning as commonly understood to one of ordinaryskill in the art to which this disclosure belongs. Although methods and materials similar orequivalent to those described herein can be used in the practice of the disclosed methods andcompositions, the exemplary methods, devices and materials are described herein. It is to beunderstood that this disclosure is not limited to particular methods, and experimental conditionsdescribed, as such methods and conditions may apply.Example 1: Electrode Preparation

[0050] A slurry was prepared by thoroughly grinding 9.5 mg of activated carbon with 0.5mg of polyvinylidene fluoride (PVDF) and 30 μL of N-methyl-2-pyrrolidone (NMP) for 30minutes. The weight of the carbon cloth (12 mm diameter) was recorded prior to coating. Theprepared slurry was uniformly brush-coated onto the carbon cloth. The coated cloth was thendried overnight at 80°C in a hot air oven. After drying, the cloth was weighed again todetermine the active material loading. The electrode was subsequently used for the fabricationof a symmetric device.Example 2: Electrolyte Preparation

[0051] For the control electrolyte, 336.6 g of KOH was dissolved in 1 L of deionized waterto prepare a 6 M KOH solution.

[0052] For the test electrolyte, 294.4 g of potassium acetate was added to 500 mL of the 6M KOH solution, resulting in a 6 M KOH + 6 M CH3COOK mixture.

[0053] Applying the above preparation methods multiple electrolyte compositions wereprepared wherein Potassium acetate is added in varying molar ratios (3-9 M) to evaluate itsconductivity, and overall electrochemical performance.(a) 6M KOH (control)(b) 6M KOH + 3M KAc(c) 6M KOH + 6M KAc(d) 6M KOH + 9M KAc

[0054] Room temperature measurements were conducted for all the differentcombinations of KOH and KAc concentrations. Upon analyzing the results, it was found thatthe combination of 6M KOH and 9M KAc exhibited the most favorable performance orcharacteristics at room temperature. Based on this observation, the specific combination of 6MKOH + 9M KAc was further studied involving temperature-dependent behavior, as it showedthe most promising results under standard conditions (Refer Figure 1, Figure 2(a) and Figure2(b)).

[0055] Figure 1 presents a comparative analysis of specific capacitance at roomtemperature for 6M KOH and 6M KOH + 9M KAc electrolytes. The addition of KAcsignificantly enhances performance, with the 6M KOH + 9M KAc system exhibiting a specificcapacitance of 167.3 mF / cm², compared to 61.1 mF / cm² for 6M KOH alone. This representsnearly a threefold improvement, highlighting the beneficial role of KAc as an antifreezingadditive in the conventional KOH electrolyte.

[0056] Figure 2(a) displays the Galvanostatic charge-discharge (GCD) performance of thesupercapacitor device using a 6M KOH + 9M KAc electrolyte at room temperature undervarying current densities. In contrast, Figure 2(b) shows the GCD performance of the devicewith a 6M KOH electrolyte under the same conditions. The comparison reveals that the devicewith the KAc additive delivers longer discharge times and improved charge-storage behavioracross all current densities.

[0057] These results confirm that the 6M KOH + 9M KAc electrolyte combinationexhibits enhanced electrochemical performance at room temperature, supporting its potentialfor further development and broader practical applications.Example 3: Cell assembly

[0058] In this experiment, a symmetric electric double-layer capacitor (EDLC) cell isassembled using activated carbon (AC) electrodes. The electrodes are prepared by coatingactivated carbon onto a suitable current collector, often with the help of a binder, and then driedthoroughly. These electrodes are arranged in a symmetric configuration (AC / / AC), meaningboth the positive and negative electrodes are identical in composition. A Whatman filter paperis used as the separator between the electrodes to prevent electrical short circuits while allowingionic movement. This separator is thoroughly soaked in a modified electrolyte composed ofpotassium hydroxide (KOH) and potassium acetate, which enhances the ionic conductivity andelectrochemical stability of the system. The components are then stacked in a sandwich-likestructure-electrode, soaked separator, and electrode-and assembled into a cell housing. Afterassembly, the cell is typically rested to ensure proper electrolyte penetration before undergoingelectrochemical testing to evaluate its performance.TESTING AND CHARACTERIZATION

[0059] After assembling the symmetric electric double-layer capacitor (EDLC) cell,electrochemical testing is carried out to evaluate its performance under various temperatureconditions. For instance, cyclic voltammetry (CV) is performed by sweeping the voltagebetween two set limits (e.g., 0 to 1 V) at different scan rates to observe the capacitive behaviorof the device. A nearly rectangular CV curve indicates ideal capacitive performance.Galvanostatic charge-discharge (GCD) tests are then conducted by charging and dischargingthe cell at constant current densities (e.g., 1 A / g), and the resulting triangular curves areanalyzed to calculate the specific capacitance using the discharge time.

[0060] To assess the internal resistance and ion transport characteristics, electrochemicalimpedance spectroscopy (EIS) is performed over a frequency range (typically from 100 kHz to0.01 Hz). The resulting Nyquist plot helps determine the charge transfer resistance andequivalent series resistance (ESR). These tests are repeated across a wide temperature range,from -60°C to 50°C, using a temperature-controlled chamber.

[0061] For example, at room temperature (25°C), the device might show a specificcapacitance of 180 F / g, a low charge transfer resistance of 0.8 Ω, and excellent capacitanceretention. However, at -40°C, the specific capacitance might drop to 120 F / g, and resistancecould increase due to slower ion mobility. Despite this, if the device retains over 80% of itsoriginal capacitance at sub-zero temperatures, it demonstrates strong capacitance retention,indicating good low-temperature performance-an essential metric for applications in coldenvironments.

[0062] To evaluate the performance of electric double-layer capacitor (EDLC) of thepresent disclosure under varying thermal conditions, three primary electrochemical techniqueswere employed:

[0063] Cyclic Voltammetry (CV): CV was used to assess the capacitive behavior andelectrochemical stability of the electrodes. The potential window was typically set between 0and 1.6 V, and measurements were conducted at a scan rate of 10 mV / s. CV curves wererecorded at multiple temperatures ranging from-60°C to 50°C. The shape and area under theCV curves provided insights into the charge storage mechanism and the effect of temperatureon ion mobility and electrode kinetics (Refer Figure 3).

[0064] Galvanostatic Charge-Discharge (GCD): GCD tests were performed todetermine the specific capacitance and rate capability of the electric double-layer capacitor(EDLC). The current was set to 2 mA / cm² (e.g., 2 mA for a 1 cm² electrode). The cell wascharged to 1.6 V and discharged to 0 V. Voltage versus time was recorded. These measurementswere repeated across the full temperature range to observe thermal effects on energy storageperformance.

[0065] Graphs illustrated in Figure 4(a) and Figure 4(b) show the potential (voltage)versus time for a galvanostatic charge-discharge (GCD) cycle of an electric double-layercapacitor (EDLC) at lower temperatures of symmetric commercial AC-based electric doublelayer capacitor (EDLC) without and with antifreezant respectively.

[0066] Both plots show galvanostatic charge-discharge curves at different temperatures(0°C, -10°C, -40°C, and -60°C). The results are tabulated in the Table 1 and Table 2 below.a) Without antifreezant: The curves show significant distortion and reduced dischargetime as temperature decreases. At -60°C, the curve is highly compressed, indicating very poorcapacitance. The voltage drop at the beginning of discharge (IR drop) increases with decreasingtemperature, suggesting higher internal resistance.b) With antifreezant: The curves maintain a more triangular shape even at lowertemperatures. Discharge times are longer compared to the system without antifreezant at alltemperatures. The IR drop is smaller and increases less dramatically with decreasingtemperature. It can be inferred that the antifreezant (potassium acetate) significantly improveslow-temperature performance. It helps maintain capacitance and reduces internal resistance atsub-zero temperatures. The electric double-layer capacitor (EDLC) with antifreezant remainsfunctional even at -60°C, while the one without shows severe performance degradation.

[0067] Electrochemical Impedance Spectroscopy (EIS): EIS was conducted to analyzethe internal resistance and charge transfer characteristics of the cell. EIS is performed atrespective open circuit potential over a frequency range from 100 kHz to 0.01 Hz. The resultingNyquist plots were used to extract parameters such as solution resistance (Rs) and chargetransfer resistance (Rct). The diameter of the semicircle in the high-frequency region indicatedRct, which is sensitive to temperature-induced changes in electrolyte conductivity andelectrode / electrolyte interface behavior. Figure 5 shows Nyquist plot derived using EIStechnique. This figure shows Nyquist plots for two systems:- KOH+KAc (blue curve)- KOH (red curve)

[0068] Both curves show a semicircle in the high-frequency region followed by a slopedline in the low-frequency region. The KOH+KAc curve has a smaller semicircle diameter andis shifted left compared to the KOH curve. The sloped portion of the KOH+KAc curve is morevertical than the KOH curve. It is clear from Figure 5 that the smaller semicircle of KOH+KAcindicates lower charge transfer resistance. The leftward shift suggests lower equivalent seriesresistance (ESR) for KOH+KAc. The more vertical low-frequency portion for KOH+KAcindicates better capacitive behavior. Overall, the KOH+KAc system shows improved iontransport and charge storage characteristics.

[0069] Charge Transfer Resistance (Rct): Extracted from EIS data, Rct indicates the easewith which electrons and ions move across the electrode / electrolyte interface. A lower Rct atlow temperatures suggests better ionic conductivity and interfacial kinetics, which are crucialfor cold-weather applications. Table 1 and Table 2 show the Rct values for KOH+Kac andcomparative KOH at low temperatures and high temperatures.Table 1: Low temperature electrochemical performance of AC based symmetricelectric double-layer capacitor (EDLC) with and without antifreezantTable 2: High temperature electrochemical performance of AC based symmetricelectric double-layer capacitor (EDLC) with and without antifreezantElectrolyte Temperature (°C) Specific

[0070] Table 1 compares the performance of electric double-layer capacitor (EDLC)comprising two electrolyte systems (KOH+KAc and KOH alone) at four low temperatures.The inference drawn from Table 1 is as below:1. Superior low-temperature performance: The KOH+KAc electrolyte consistently showshigher specific capacitance and lower resistance across all temperatures compared to KOHalone.2. Freezing point depression: The KOH+KAc system maintains functionality even at -60°C,while the KOH system shows significant performance degradation below -10°C.3. Temperature sensitivity: Both systems show decreased capacitance and increased resistanceas temperature drops, but the KOH+KAc system degrades more gradually.4. Extreme cold performance: At -60°C, the KOH+KAc system retains 18.5% of its 0°Ccapacitance, while the KOH system retains only 14.9%.5. Resistance behavior: The KOH+KAc system shows lower resistance at all temperatures,indicating better ion mobility and charge transfer.

[0071] Table 2 compares the performance of electric double-layer capacitor (EDLC)comprising the two electrolyte systems at three higher temperatures. The inference drawn fromTable 2 is as below:1. Enhanced high-temperature performance: The KOH+KAc system shows significantly higherspecific capacitance and lower resistance across all temperatures compared to KOH alone.2. Temperature-dependent improvement: The performance gap between the two systemswidens as temperature increases, with the KOH+KAc system showing more pronouncedimprovement.3. Thermal stability: The KOH+KAc system maintains consistent performance improvementfrom 10°C to 50°C, while the KOH system shows erratic behavior, particularly at 10°C.4. Resistance trends: Both systems show decreased resistance as temperature increases, but theKOH+KAc system maintains consistently lower resistance values.5. Capacitance enhancement: At 50°C, the KOH+KAc system shows a 60% higher specificcapacitance compared to the KOH system.PERFORMANCE METRICS:

[0072] The following key performance indicators were used to quantify theelectrochemical behavior of the electric double-layer capacitor (EDLC) of the presentdisclosure, especially under sub-zero conditions:

[0073] Specific Capacitance (Cs): This metric reflects the charge storage capacity perunit mass of active material. It was derived from GCD data and used to compare performanceacross different temperatures and electrolyte compositions. Figure 6 graph plots specificcapacitance (mF / cm²) against temperature (°C) from 0°C to -60°C for two systems:- KOH-KAc (blue line)- KOH (red line)

[0074] Both the above lines show a downward trend as temperature decreases, indicatingcapacitance loss. The KOH-KAc system starts at a higher capacitance (~220 mF / cm² at 0°C)and maintains higher values throughout. The KOH system starts lower (~170 mF / cm² at 0°C)and drops more steeply. At -60°C, KOH-KAc retains about 40 mF / cm², while KOH drops toaround 30 mF / cm². It is amply clear from Figure 6 that the antifreezant (KAc) improves overallcapacitance across all temperatures. It also reduces the rate of capacitance loss as temperaturedecreases. The performance gap between the two systems widens at extremely lowtemperatures.

[0075] Further Figure 7 illustrates variation in specific capacitance at high temperatures:This graph plots specific capacitance (mF / cm²) against temperature (°C) from 10°C to 50°Cfor two systems:- KOH+KAc (blue line)- KOH (red line)

[0076] Both the above lines show an upward trend as temperature increases. TheKOH+KAc system starts higher (~150 mF / cm² at 10°C) and increases more steeply. The KOHsystem starts much lower (~20 mF / cm² at 10°C) and shows a more gradual increase. At 50°C,KOH+KAc reaches about 320 mF / cm², while KOH reaches about 200 mF / cm². It is clear fromFigure 7 that the antifreezant (KAc) significantly improves capacitance at all temperatures.The performance gap between the two systems widens as temperature increases. KOH+KAcshows better thermal stability and enhanced high-temperature performance.

[0077] Capacitance Retention: This parameter measures the percentage of capacitanceretained at low temperatures compared to room temperature. It is a critical indicator of thedevice's reliability and efficiency in cold environments. For example, a retention of 90% at-40°C implies strong thermal stability of the electrolyte and electrode materials. Figure 8shows the stability of the symmetric AC electric double-layer capacitor (EDLC) at 50°C. Thisgraph shows capacitance retention (%) versus number of cycles for the KOH+KAc system at50°C and 6mA current. The curve starts at 100% capacitance retention and shows a gradualdecrease over 1000 cycles. By the end of 1000 cycles, the capacitance retention is around 85-90%. It is clear from Figure 8 that the KOH+KAc system demonstrates good cycling stabilityat elevated temperatures. The gradual slope indicates a slow, steady degradation rather thanrapid failure. Retaining 85-90% capacitance after 1000 cycles at 50°C suggests good long-termperformance in high-temperature environments.

[0078] Overall, these figures collectively demonstrate the superior performance of theelectric double-layer capacitor (EDLC) comprising the aqueous electrolyte of the presentdisclosure. KOH+KAc electrolyte system across a wide temperature range, its improvedelectrochemical characteristics, and its stability under various operating conditions. This datastrongly supports the effectiveness of the potassium acetate antifreeze additive in enhancingelectric double-layer capacitor (EDLC) performance.

[0079] Based on the detailed analysis of Figures 1-5, the following inferences may bedrawn:1. Enhanced Low-Temperature Performance: The KOH+KAc system maintains functionalityand higher capacitance at temperatures as low as -60°C, while the KOH-only system showssevere performance degradation. This indicates that the potassium acetate additive effectivelyprevents electrolyte freezing and maintains ion mobility at extremely low temperatures.2. Improved High-Temperature Performance: The KOH+KAc system shows significantlyhigher specific capacitance at elevated temperatures (up to 50°C) compared to the KOH-onlysystem. This suggests that the additive not only works as an antifreeze agent but also enhancesoverall electrochemical performance across a wide temperature range.3. Reduced Internal Resistance: The Nyquist plots and charge-discharge curves indicate lowerinternal resistance for the KOH+KAc system across all temperatures. This implies better iontransport and charge transfer efficiency in the modified electrolyte.4. Broader Operating Temperature Range: The KOH+KAc system maintains superiorperformance from -60°C to 50°C, significantly expanding the usable temperature range of theelectric double-layer capacitor (EDLC). This makes the device suitable for applications indiverse and extreme environments.5. Enhanced Capacitance and Energy Storage: Consistently higher specific capacitance valuesfor the KOH+KAc system indicate improved energy storage capability across all temperatures.This translates to higher energy density and potentially better overall device performance.6. Improved Cycling Stability: The stability test at 50°C shows good capacitance retention (85-90%) after 1000 cycles. This indicates that the KOH+KAc system is suitable for long-termoperation in high-temperature environments.7. Electrochemical Behavior Optimization: The more ideal shape of charge-discharge curvesand Nyquist plots for the KOH+KAc system suggests optimized electrochemical behavior.This includes better double-layer formation, more efficient charge storage, and improved iondiffusion.8. Potential for Practical Applications: The consistent performance improvements acrossvarious conditions indicate that this system could be valuable for real-world applicationsrequiring reliable energy storage in fluctuating or extreme temperatures.9. Synergistic Effects: The improvements seen are not just additive but appear synergistic, withthe KOH+KAc system outperforming the KOH system more significantly as conditionsbecome more extreme (very low or high temperatures).10. Material Compatibility: The stable performance and lack of adverse effects suggest goodcompatibility between the potassium acetate additive and the activated carbon electrodes.11. Cost-Effective Performance Enhancement: Given that potassium acetate is a relativelyinexpensive and common material, this method provides a cost-effective way to significantlyenhance electric double-layer capacitor (EDLC) performance.Example 4: Energy storage Device

[0080] An energy storage device was developed incorporating at least one electric doublelayer capacitor (EDLC) as described in claim 1. The device includes robust electricalconnections designed to facilitate efficient energy storage and rapid discharge. To evaluate itsperformance under extreme environmental conditions, the device was subjected to a series oftests across a wide temperature range, from -60°C to +50°C.

[0081] During testing, the device maintained stable capacitance, low internal resistance,and consistent charge-discharge cycles throughout the entire temperature spectrum. The seriesparallel configuration enabled scalable energy output, while the EDLCs ensured fast chargedischarge cycles critical for high-power demands. These results confirm the device's suitabilityfor deployment in aerospace, defense, and industrial sectors where both environmentalresilience and high power density are essential.

[0082] The results presented herein demonstrate that the incorporation of potassiumacetate into KOH-based electrolytes contributes to improved electrochemical performance andenhanced operational stability of electric double-layer capacitor (EDLC). This approachenables effective functioning of the device under low-temperature conditions, therebyextending the range of environments in which such electric double-layer capacitor (EDLC) canbe reliably deployed.

Claims

1. An electric double-layer capacitor (EDLC) comprising: i. a pair of carbon electrodes; and ii. an aqueous electrolyte comprising potassium hydroxide (KOH) and potassium acetate (CH3COOK), wherein potassium hydroxide and potassium acetate are present in a mole ratio range of 1:2 to 1:3.

2. The electric double-layer capacitor as claimed in claim 1, wherein potassium acetate is present in a concentration in a range of 3 M to 9 M, and the potassium hydroxide is present in a concentration in a range of 3 M to 9 M.

3. The electric double-layer capacitor as claimed in claim 1, wherein EDLC comprises a separator selected from the group consisting of Whatman filter paper, Polyacrylonitrile (PAN), Nylon,Glass Fiber, Celgard separators, and combinations thereof.

4. The electric double-layer capacitor as claimed in claim 1, wherein the aqueous electrolyte exhibits a freezing point in a range of -40°C to -60°C.

5. The electric double-layer capacitor as claimed in claim 1, wherein the EDLC maintains electrochemical stability across a temperature range of -60°C to +50°C.

6. The electric double-layer capacitor as claimed in claim 1, wherein the EDLC retains at least 72% stability at -60°C and at least 90% capacitance retention at +50°C.

7. The electric double-layer capacitor as claimed in claim 1, wherein the electrode comprises activated carbon.

8. The electric double-layer capacitor as claimed in claim 1, wherein the EDLC is operated in applications selected from the group consisting of electric vehicles, aerospace systems, military equipment, cold-climate energy systems, and remote sensing devices.

9. A method of preparing the electric double-layer capacitor as claimed in claim 1, the method comprising: - dissolving potassium hydroxide and potassium acetate in water to obtain the aqueous electrolyte, wherein potassium hydroxide and potassium acetate are present in a mole ratio range of 1:2 to 1:3; and - assembling a pair of electrodes in the presence of a separator soaked in the aqueous electrolyte to obtain the electric double-layer capacitor, wherein the separator is sandwiched between the pair of electrodes.

10. An energy storage device comprising: - at least one electric double-layer capacitor as claimed in claim 1; and - electrical connections configured for energy storage and discharge, wherein the device is operable in extreme temperature environments ranging from -60°C to +50°C.

11. The energy storage device as claimed in claim 10, wherein the device comprises a plurality of electric double-layer capacitors connected in a series or parallel configuration.

12. The energy storage device as claimed in claim 10, wherein the device is configured for high-power applications requiring rapid energy discharge.