Taphole mix

IN595487BActive Publication Date: 2026-07-15KROSAKI HARIMA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202414016487
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-03-16
Filing Date
2024-03-07
Publication Date
2026-07-15
Estimated Expiration
2044-03-07

AI Technical Summary

Technical Problem

The inclusion of zirconia raw material in taphole mixes suppresses hole enlargement during tapping but causes cracking and difficulty in maintaining hole depth due to high thermal expansion and phase transition.

Method used

Incorporating alumina-zirconia or zirconia-mullite raw materials in a taphole mix to mitigate thermal expansion and volume changes, while leveraging their high corrosion resistance, within a specific mass percentage range to ensure hole depth and prevent hole enlargement.

Benefits of technology

The taphole mix effectively suppresses hole enlargement and maintains hole depth, with optimal strength and corrosion resistance, preventing drillability issues and hole disconnection.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a taphole mix capable of suppressing hole enlargement during tapping and ensuring hole depth. [Solution] The taphole mix contains at least one of an alumina-zirconia raw material and a zirconia-mullite raw material in a total amount of 2 % by mass to 30 % by mass, in 100 % by mass of a refractory raw material mixture, wherein a binder is added to the refractory raw material mixture.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a taphole mix which is used for plugging a taphole of a blast furnace.BACKGROUND ART

[0002] In the operation of a blast furnace, a taphole mix is injected and filled into a taphole after completion of tapping. Then, at the next tapping after elapse of a given time (typically, 2 to 5 hours), an operation of drilling a taphole mix burnt by furnace heat until then to form a hot metal passage is performed. In this operation of drilling the burnt taphole mix to form a hot metal passage, it is necessary to ensure the length of the hot metal passage at a certain level or more. Such a length of the hot metal passage is called "hole depth".In recent years, there has been a need to optimize a tapping duration during which tapping is performed. Thus, it is necessary to prevent the hot metal passage from being chipping away and enlarged by hot metal and slag during tapping. The phenomenon that the hot metal passage is chipped away and enlarged by hot metal and slag during tapping is called "hole enlargement".

[0003] Meanwhile, there has been known a taphole mix intended to achieve improved durability by adding a zirconia raw material, as disclosed in the following Patent Document 1.CITATION LIST [Patent Document]

[0004] Patent Document 1: JP-A H08-231276 SUMMARY OF INVENTION[Technical Problem]

[0005] The present inventors conducted various experimental tests on a taphole mix comprising a zirconia raw material, additionally with a view to verifying the technique disclosed in the Patent Document 1. As a result, the present inventors have found that the inclusion of a zirconia raw material makes it possible to suppress the hole enlargement during tapping, but causes the formation of cracks in the taphole mix in the course of burning after the completion of tapping, leading to difficulty in ensuring the hole depth.

[0006] In view of the above situation, a technical problem to be solved by the present invention is to provide a taphole mix capable of suppressing the hole enlargement during tapping and ensuring the hole depth.[Solution to Technical Problem]

[0007] With regard to the above-mentioned test result, the present inventors assumed as follows. Since a ZnO2 component as a primary component of a zirconia raw material exhibits high corrosion resistance to hot metal and slag, the inclusion of the zirconia raw material makes it possible to suppress the hole enlargement during tapping. On the other hand, since the zirconia raw material has a high thermal expansion rate (thermal expansion coefficient) and undergoes a rapid volume change due to a phase transition, cracks are formed in the taphole mix in the course of burning after the completion of tapping, leading to difficulty in ensuring the hole depth.Therefore, in order to solve the above technical problem, the present inventors repeatedly conducted experimental tests and studies on refractory materials to be used in a taphole mix, under a technical idea of suppressing the thermal expansion and the volume change in the course of the burning, while taking advantage of the high corrosion resistance of the ZrO2 component. As a result, the present inventors have obtained a finding that it becomes possible to suppress the hold expansion and ensure the hole depth when an alumina-zirconia raw material or a zirconia-mullite raw material is contained in a taphole mix. That is. it is effective to introduce a ZrO2 component in the form of an alumina-zirconia raw material or a zirconia-mullite raw material, instead of in the form of a zirconia raw material.

[0008] The present invention has been conceived based on the above technical idea and founding, and the subject matter of the present invention is as follows.A taphole mix containing at least one of an alumina-zirconia raw material and a zirconia-mullite raw material in a total amount of 2 % by mass to 30 % by mass, in 100 % by mass of a refractory raw material mixture, wherein a binder is added to the refractory raw material mixture.[Advantageous Effects of Invention]

[0009] The taphole mix of the present invention is capable of suppressing the hole enlargement during tapping and ensuring the hole depth.DESCRIPTION OF EMBODIMENTS

[0010] A taphole mix according to one embodiment of the present invention contains at least one of an alumina-zirconia raw material and a zirconia-mullite raw material in a total amount of 2 % by mass to 30 % by mass, in 100 % by mass of a refractory raw material mixture, wherein a binder is added to the refractory raw material mixture.The content rate of at least one of the alumina-zirconia raw material and the zirconia-mullite raw material (hereinafter referred to collectively as "zirconia-containing composite oxide raw material) is less than 2 % by mass, it is impossible to sufficiently obtain the hole enlargement-suppressing and hole depth-ensuring effects derived from the zirconia-containing composite oxide raw material. On the other hand, since the strength of the taphole mix becomes higher as the content rate of the zirconia-containing composite oxide raw material increases, if the content rate of the zirconia-containing composite oxide raw material exceeds 30 % by mass, the strength of the taphole mix excessively increases, and therefore drillability deteriorates and so-called "hole disconnection phenomenon" becomes likely to occur, resulting in difficulty in ensuring the hole depth. The content rate of the zirconia-containing composite oxide raw material is preferably 5 % by mass to 15 % by mass.

[0011] As the alumina-zirconia raw material in the zirconia-containing composite oxide raw material, fused alumina-zirconia produced by fusing alumina and zirconia in an electric furnace is available as a commercialized product, for example. Examples of commercialized products of the zirconia-mullite raw material include fused zirconia-mullite produced by fusing alumina and zircon in an electric furnace.In addition to the above commercialized products or new (unused) materials, so-called "reused material" derived from an after-use refractory waste may be used as thezirconia-containing composite oxide raw material. The term "after-use refractory waste" here means a refractory material collected after using it in an iron-making process, and the term "reused material derived from this refractory waste" means refractory raw material particles obtained by pulverizing the refractory waste. In a process for obtaining the reused material, the after-use refractory waste is appropriately subjected to processing such as magnetic separation, and classification.

[0012] As the after-use refractory waste, it is possible to use any refractory material as long as it contains a zirconia-containing composite oxide raw material, for example, a refractory material comprising a zirconia-containing composite oxide raw material1 in an amount of 10-60 % by mass, and a remainder comprising: alumina in an amount of 4080 % by mass; at least one of a carbonaceous material and a carbide material in a total amount of 10 % by mass or less (including 0); and a metal in an amount of 10 % by mass or less (including 0). More specifically, it is possible to use alumina-carbon based bricks such as a sliding nozzle plate, an upper nozzle, and an lower plate.In the case where such a reused material is used as the refractory raw material mixture in the present invention, it is used in an amount converted to mass percentage of the zirconia-containing composite oxide raw material.

[0013] A refractory waste generally has, in a refractory microstructure, a carbon bond derived from an organic binder used in production of its original refractory material. Thus, the reused material generally also has a carbon bond in a refractory microstructure. The inclusion of such a reused material having a carbon bond in the refractory raw material mixture of the taphole mix makes it possible to obtain an effect of enhancing the carbon bond in the taphole mix. Consequently, the corrosion resistance of the taphole mix is improved, thereby enhancing the effect of suppressing the hole enlargement and ensuring the hole depth.In the taphole mix of the present invention, the zirconia-containing composite oxide raw material may be in the form of: only a new material; a combination of a new material and a reused material; or only a reused material. However, from a viewpoint of effective utilization of a refractory waste, and obtaining the above advantageous effect due to the carbon bond, it is preferably in the form of only a reused material.

[0014] As above, the taphole mix of the present invention is technically characterized in that it contains a zirconia-containing composite oxide raw material, irrespective of whether the zirconia-containing composite oxide raw material is a new material or areused material, in a total amount of 2 % by mass to 30 % by mass, in 100 % by mass of a refractory raw material mixture. Thus, the remainder of the refractory raw material mixture is not particularly limited, and may be a remainder commonly used as refractory raw materials of taphole mixes. For example, the remainder may comprise one or more primary raw materials selected from the group consisting of alumina, silicon carbide, chamotte, carbon, roseki, clay, silicon nitride, ferrosilicon nitride, and a metal powder. A reused material derived from a after-use refractory waste may also be used as the refractory raw materials constituting the remainder.Further, the particle size composition of the entire refractory raw material mixture including the remainder may be a particle size composition commonly used for refractory raw material mixture of taphole mixes. For example, the maximum particle size may be set to 3 mm, and the particle size composition may be approximately adjusted within the range.

[0015] The binder to be added to the refractory raw material mixture is not particularly limited in terms of type and addition percentage, but may be a binder commonly used in taphole mixes. Examples of the binder include coal tar and phenolic resin. The addition percentage of the binder may be 10 % by mass to 25 % by mass with respect to 100 % by mass of the refractory raw material mixture.EXAMPLES

[0016] Table 1 shows respective compositions and evaluations result of taphole mixes which are inventive examples, together with comparative examples. In Table 1, "others 1" is clay, coke which is a type of carbon, etc. Further, the composition of "reused material" is classified into alumina-zirconia, zirconia-mullite and others, and respective content rates of them are shown. For example, Inventive Example 10 uses a reused material in an amount of 30 % by mass, wherein the reused material contains, in terms of a percentage in 100 % by mass of refractory raw material mixture, alumina-zirconia in an amount of 9 % by mass, and components other than alumina-zirconia and zirconia-mullite ("others 2") in an amount of 21 % by mass.Since a raw material composition of an original refractory material of a reused material at the time of production is generally known, the respective content rates of alumina-zirconia and zirconia-mullite in each reused material used in inventive examples are calculated from a raw material composition ratio. Further, each reused material used in inventive examples is obtained from sliding nozzle plates. In Inventive Example 10, asliding nozzle plate containing 30 % by mass of alumina-zirconia, 60 % by mass of alumina, and 3 % by mass of carbonaceous raw material was used, and in Inventive Example 11, a sliding nozzle plate containing 17 % by mass of zirconia-mullite, 60 % by mass of alumina, and 3 % by mass of carbonaceous raw material was used. Further, in Inventive Example 12, a sliding nozzle plate containing 17 % by mass of alumina-zirconia, 17 % by mass of zirconia-mullite, 60 % by mass of alumina, and 3 % by mass of carbonaceous raw material was used.With regard to the particle size composition of the refractory raw material mixture, a maximum particle size was set to 3 mm, and the particle size composition was appropriately adjusted within this range.

[0017] TABLE 1

[0018] Each of the taphole mixes was evaluated in terms of corrosion resistance and strength, in the following manner.< Corrosion Resistance >Each of the taphole mixes was subjected to pressure forming at 7 MPa and then to baking under heating at 500°C to obtain a test piece. The test piece was lined on a small rotary furnace, and subjected to a corrosion test at 1600°C for 5 hours, using blast furnace slag as corrosive agent. During the corrosion test, the corrosive agent was changed to new one once in every quarter of an hour (10 times).After completion of the corrosion test, a wear size (in a maximum worn region) of the test piece was measured, and a corrosion resistance index with respect to 100 which corresponds to a value of the wear size in Comparative Example 2 was calculated. Then,a test piece having a corrosion resistance index of less than 70 was evaluated as [Encentric Circle](excellent), and a test piece having a corrosion resistance index of 70 to less than 100 was evaluated as o (good). Further, a test piece having a corrosion resistance index of 100 or more was evaluated as x (NG). A smaller corrosion resistance index indicates better corrosion resistance, and contributes particularly to suppression of the hole enlargement.< Strength >Each of the taphole mixes was subjected to pressure forming at 7 MPa and then to baking under heating at 500°C to obtain a test piece. The test piece was subjected to reduction firing at 1200°C for 3 hours to obtain a sample. Then, the compressive strength of the sample was measured. Then, a test piece having a measured strength value of 20MPa to less than 30 MPa was evaluated as [Encentric Circle] (excellent). A test piece having a measuredstrength value of 10 MPa to less than 20 MPa was evaluated as o (low) (good), and a test piece having a measured strength value of 30 MPa to less than 40 MPa was evaluated as o (high) (good). Further, a test piece having a measured strength value of less than 10 was evaluated as x (low) (NG), and a test piece having a measured strength value of 40 or more was evaluated as x (high) (NG). This measured strength value corresponds to strength at the time of drilling after the taphole mix was injected into a taphole and underwent furnace heat. The strength set to fall within an appropriate range makes it possible to reduce the rate of occurrence of hole disconnection, and contributesparticularly to ensuring the hole depth.

[0019] In Table 1, in Inventive Examples 1-12 each falling within the scope of the present invention, the evaluations of corrosion resistance and strength were [Encentric Circle] (excellent)or O (good). Among them, in Inventive Examples 2, 3 and 9-12 in which the content rate of the zirconia-containing composite oxide raw material is in a preferable range of 5 % by mass to 15 % by mass, both the evaluations of corrosion resistance and strengthwere [Encentric Circle] (excellent), i.e., a particularly excellent evaluation result was obtained in termsof both corrosion resistance and strength.Here, in Inventive Examples 9-12 in which a reused material was used as the zirconia-containing composite oxide raw material, a particularly excellent evaluation result was obtained in terms of corrosion resistance, as compared to Inventive Example 2 in which a new material was used as the zirconia-containing composite oxide raw material at approximately the same content rate (although in all Inventive Examples 9-12 andInventive Example 3, the result of evaluation of corrosion resistance in Table 1 was [Encentric Circle](excellent), a significant difference therebetween was found in the corrosion resistance index calculated after the aforementioned corrosion test).In both Inventive Example 9 in which an alumina-zirconia raw material and a zirconia-mullite raw material each as a new material were used in combination as the zirconia-containing composite oxide raw material, and Inventive Example 12 in which an alumina-zirconia raw material and a zirconia-mullite raw material each as a reused material were used in combination as the zirconia-containing composite oxide raw material, an excellent evaluation result was obtained.

[0020] On the other hand, in Comparative Example 1 in which the content rate of an alumina-zirconia raw material as the zirconia-containing composite oxide raw material was less than the lower limit of the present invention, and Comparative Example 2 in which the content rate of a zirconia-mullite raw material as the zirconia-containing composite oxide raw material was less than the lower limit of the present invention, the evaluation of corrosion resistance was x (NG). Thus, it is impossible to suppress the hole enlargement.Further, in Comparative Example 3 in which the content rate of an alumina-zirconia raw material as the zirconia-containing composite oxide raw material was greaterthan the upper limit of the present invention, and Comparative Example 4 in which the content rate of a zirconia-mullite raw material as the zirconia-containing composite oxide raw material was greater than the upper limit of the present invention, the evaluation of strength was x (NG). Thus, it is impossible to ensure the hole depth.Further, in Comparative Example 5 in which a zirconia raw material was used, instead of the zirconia-containing composite oxide raw material, the evaluation of strength was x (high) (NG). Thus, the hole disconnection often occurs, which makes it impossible to ensure the hole depth.

Claims

1. A taphole mix containing at least one of an alumina-zirconia raw material and a zirconia-mullite raw material in a total amount of 2 % by mass to 30 % by mass, in 100 % by mass of a refractory raw material mixture, wherein a binder is added to the refractory raw material mixture.

2. The taphole mix as claimed in claim 1, wherein a total content rate of at least one of the alumina-zirconia raw material and the zirconia-mullite raw material is 5 % by mass to 15 % by mass.

3. The taphole mix as claimed in claim 1 or 2, wherein each of the alumina-zirconia raw material and the zirconia-mullite raw material derives from an after-use refractory waste.

4. The taphole mix as claimed in claim 3, wherein each of the alumina-zirconia raw material and the zirconia-mullite raw material has a carbon bond in a refractory microstructure.