AI Technical Summary
Existing electrode materials for lithium-ion, sodium-ion batteries, and supercapacitors face challenges in accommodating ions of varying sizes while maintaining fast charge-discharge dynamics, with conventional methods being costly and non-scalable.
A multifunctional electrode material derived from white chickpeas, synthesized through carbonization and chemical activation in air, offering a scalable and low-cost solution with tailored pore sizes for efficient ion storage.
The electrode material exhibits high specific capacitance and capacity retention across varying current densities, demonstrating excellent long-term stability and fast-charging capabilities in batteries and supercapacitors.
Abstract
Description
FIELD OF INVENTION
[0001] Embodiment of the present invention relates to the field of Physics, more particularly itrelates to the synthesis of multifunctional electrode material from white chickpeas biowastewith tailored pore sizes developed for multi-storage applications in lithium-ion batteries,sodium-ion batteries, and supercapacitors.RELATED ART
[0002] The increasing demand for fast-charging, high-performance energy storage devices hasdriven extensive research into advanced electrode materials for lithium-ion batteries (LIBs),sodium-ion batteries (SIBs), and supercapacitors (SCs). Traditional graphite anodes performwell in LIBs due to the small ionic radius of lithium (Li⁺, ~0.76 Å) but exhibit poor performancein SIBs because of the larger size of sodium ions (Na⁺, ~1.02 Å).
[0003] To overcome these limitations, carbon-based materials-including activated carbons,graphene, and carbon nanotubes-have been explored owing to their high surface area, tunableporosity, and conductivity. Supercapacitors, which rely on surface-driven charge storage,require materials capable of rapid ion adsorption and desorption, particularly for larger ionssuch as potassium (K⁺, ~1.38 Å).
[0004] Conventional preparation of activated carbons often involves high-temperaturecarbonization followed by chemical activation under inert atmospheres (argon, nitrogen),which increases production cost and limits scalability. Recent studies on biomass-derivedcarbons demonstrate potential for low-cost and environmentally benign electrodes, but mostmethods still rely on expensive inert gases or high-energy processes.
[0005] Despite progress, a significant gap remains in developing a scalable, low-cost,multifunctional electrode capable of accommodating ions of varying sizes while sustaining fastcharge-discharge dynamics.SUMMARY
[0006] An electrode material for batteries and supercapacitors comprising an activated carbonderived from white chickpeas. The electrode material for batteries and supercapacitors, whereinthe said activated carbon is formed by carbonisation at 450 °C to 500 °C temperature for 30minutes of white chickpeas and activation by potassium hydroxide (KOH) at 500 °C to 550 °Ctemperature for 1 hour to form ACH-2 electrode. The electrode material exhibits an initialspecific capacitance of 436 F g⁻¹ at 0.5 A g⁻¹ current density and retains 70 F g⁻¹ at high currentdensity of 10 A g⁻¹ after 10,000 cycles for a super capacitors. The electrode material exhibitsan initial specific capacity of 691 mAh g⁻¹ at 100 mA g⁻¹ current density and retains 133 mAhg⁻¹ at 500 mA g⁻¹ current density after 1000 cycles for Li-ion batteries. The electrode materialexhibits an initial specific capacity of 693 mAh g⁻¹ at 100 mA g⁻¹ and retains 90 mAh g⁻¹ at500 mA g⁻¹ current density after 1000 cycles for sodium ion batteries.
[0007] A process of synthesizing a electrode material comprising; preparing activated carbonfrom white chickpeas (101) and preparing an electrode using prepared activated carbon (102).The process, wherein the preparing activated carbon from white chickpeas (101) furthercomprising: soaking the white chickpeas overnight in deionized water to promote poreactivation by inducing cellular swelling through water absorption; subjecting the soaked whitechickpeas to preliminary carbonization in ambient air using a muffle furnace at around 450 °Cto 500 °C for 30 minutes; cooling the carbonised white chickpea at room temperature; mixingthe resulting carbon with KOH at a weight ratio of 1:3, using a few drops of double distilledwater to assist homogenization; stirring the mixture while being heated at 80 °C until completeevaporation of water and to form gel; drying the obtained gel overnight at 100 °C in a vacuumoven to obtain a fine powder; transferring the obtained fine powder into a crucible to minimizemoisture absorption and tightly sealed with aluminum foil to restrict airflow during thesubsequent activation step; introducing the crucible into a preheated muffle furnace and heatedat around 500 °C to 550 °C with a ramp rate of 2 °C per minute, maintained at the targettemperature for 1 hour; cooling and washing the obtained activated carbon multiple times with1 M hydrochloric acid, ethanol, acetone, and double-distilled water to remove residualimpurities; and drying the washed sample at 80 °C overnight.
[0008] The process, wherein the preparing an electrode using prepared activated carbon furthercomprising; preparing a slurry containing 10 wt% carbon black, 80 wt% active material ofclaim 1, and 10 wt% polyvinylidene fluoride (PVDF) with a few drops of N-methyl-pyrrolidinone; and coating the prepared slurry on copper foil for lithium and sodium-ionbatteries to make a working electrode. The process, wherein the preparing an electrode usingprepared activated carbon further comprising; preparing a slurry containing 10 wt% carbonblack, 80 wt% active material of claim 1, and 10 wt% polyvinylidene fluoride (PVDF) with afew drops of N-methyl-pyrrolidinone; and coating the prepared slurry on titanium foil forsupercapacitors to make a working electrode.
[0009] Several aspects are described below, concerning diagrams. It should be understood thannumerous specific details, relationships and methods are set forth to provide a completeunderstanding of the present disclosure. Skilled personnel in the relevant art, however, willreadily recognize that the present disclosure can be practiced without one or more of thespecific details or with other methods etc. In other instances, well known structures or theoperations are not shown in detail to avoid obscuring the details of the present disclosure.BRIEF DESCRIPTION OF THE DRAWINGS
[0010] FIG.1 illustrates the process of synthesizing a multifunctional electrode material.
[0011] FIG.2 illustrates the process of preparation of activated carbon from white chickpeas.
[0012] FIG.3 illustrates the fabrication of Lithium-ion and sodium ion batteries with pictorialprocedures.
[0013] FIG.4 illustrates the (a) XRD and (b) Raman spectroscopy of ACH 1, ACH 2, and ACH3.
[0014] FIG.5 illustrates the (a) BET isotherms of N2 adsorption / desorption and (b) Porediameter of ACH 1, ACH 2, and ACH 3, and (c) TGA analysis of the ACH sample.
[0015] FIG.6 illustrates the (a-f) FESEM images and EDAX spectrum of ACH-1, ACH-2, andACH-3 samples.
[0016] FIG.7 illustrates the (a-c) low to high magnification of HRTEM images of ACH-2 andXPS results of (d) full survey, (e) C 1s spectrum, and (f) O 1s spectrum of the ACH-2 sample
[0017] FIG.8 illustrates the supercapacitor analysis (a) Cyclic voltammetry of all samples, (b)Cyclic voltammetry of ACH 2, (c) Galvanostatic charge-discharge of ACH 2, (d) Ratecapability of ACH 2, (e) EIS spectrum of ACH 2, and (f) Cyclic stability of ACH 2.
[0018] FIG.9 illustrates the Lithium-ion batteries analysis (a) Cyclic voltammetry of allsamples, (b) Cyclic voltammetry of ACH 2, (c) Galvano-static charge-discharge curves ofACH 2, (d) Rate capability of all the samples, (e) Cyclic stability of all samples, and (f) EIS ofthe ACH 2 sample.
[0019] FIG.10 illustrates the sodium-ion batteries analysis (a) Cyclic voltammetry of allsamples, (b) Cyclic voltammetry of ACH 2, (c) Galvano-static charge-discharge curves ofACH 2, (d) Rate capability of all the samples, (e) Cyclic stability of all samples, and (f) EIS ofthe ACH 2 sample.
[0020] FIG.11 illustrates the fast charging analysis (a-c) Comparative rate performance ofACH 2 at various current densities. (d-f) Galvanostatic charge-discharge (GCD) profiles ofACH 2 in Lithium-ion battery, Sodium-ion battery, and Supercapacitor devices at differentcurrent densities.DETAILED DESCRIPTION OF PREFERRED EXAMPLES
[0021] The present invention relates to a novel multifunctional electrode material, suitable forlithium-ion batteries, sodium-ion batteries, and supercapacitors. The material is derived froma sustainable carbon source through a simple, low-cost synthesis route without the need forexpensive inert atmospheres and high temperature.
[0022] A process of synthesizing a multifunctional electrode material has following steps;(101): Preparation of activated carbon from white chickpeas and (102): Preparation of electrodeusing prepared activated carbon. The process is shown in the FIG.1.
[0023] In the step (101), White chickpeas (Kabul channa), and potassium hydroxide (KOH)pellets (85% extra pure, Loba Chemie) are used for the synthesis. The activated carbon isprepared through a two-step process involving initial carbonization followed by chemicalactivation, represented in FIG.2.
[0024] First, the white chickpeas are soaked overnight in deionized water to promote poreactivation by inducing cellular swelling through water absorption. The following day, thesoaked white chickpeas (201) are subjected to preliminary carbonization in ambient air usinga muffle furnace at around 450 °C to 500 °C for 30 minutes (202). After carbonization, thematerial is allowed to cool naturally to room temperature. The resulting carbon is thenthoroughly mixed with KOH at a weight ratio of 1:3, using a few drops of double distilledwater to assist homogenization (203). The mixture is stirred while being heated at 80 °C untilcomplete evaporation of water. The obtained gel is subsequently dried overnight at 100 °C ina vacuum oven, yielding a fine powder. This powder is swiftly transferred into a crucible tominimize moisture absorption and tightly sealed with aluminum foil to restrict airflow duringthe subsequent activation step. The sealed crucible is introduced into a preheated mufflefurnace and heated at around 500 °C to 550 °C with a ramp rate of 2 °C per minute, maintainedat the target temperature for 1 hour (204).
[0025] The chemical activation is carried out in air without any inert atmosphere, emphasizinga cost-effective and scalable methodology suitable for industrial applications. After heating,the furnace is allowed to cool naturally to room temperature overnight, and the sample iscollected. The obtained activated carbon (205) is washed multiple times with 1 M hydrochloricacid, ethanol, acetone, and double-distilled water to remove residual impurities, followed bydrying at 80 °C overnight. Samples prepared at final activation temperatures of around 400 °Cto 450 °C, 500 °C to 550 °C, and 650 °C to 700 °C are designated as ACH-1, ACH-2, andACH-3, respectively.
[0026] Referring to FIG.1, in the step (102), at temperature around 20°C controlled by airconditioner, electrochemical analysis are performed using battery and super capacitorelectrode. To make the working electrode, a slurry of 10 wt% carbon black, 80 wt% activematerial, and 10 wt% polyvinylidene fluoride (PVDF) is mixed with a few drops of N-methyl-pyrrolidinone. The coating is done on copper foil for lithium and sodium-ion batteries using aDoctor Blade coater machine, whereas, for supercapacitor application, it is coated on titaniumfoil. The electrode is then dried for 12 hours at 120 °C in a vacuum to remove the solvent.
[0027] The supercapacitor study is done in three-electrode systems in 1M KOH electrolyte.For batteries, fabrication is performed inside an argon-filled glove box using CR2032 coincells. A lithium / sodium metal counter / reference electrode, a Whatman 50 filter paper (for LIB)and Whatman microglassy fibre GF / D (for SIB) used as separator, and a 1 M LiPF6 (for LIB) / 1 M NaPF6 (for SIB) electrolyte solution dissolved in a combination of ethylene carbonate(EC) and dimethyl carbonate (DMC) (EC / DMC, 1: 1 v / v) are used to assemble the cells in anargon-filled glove box. Using a Biologic SP-150 electrochemical workstation, measurementsof cyclic voltammograms (CV) and electrochemical impedance spectroscopy (EIS) are made.At scan rates of 0.1 mV s-1 , the CV curves are obtained over the potential range of 0.01-3.00 Vvs. Li+ / Li and 0.01-2.5 V vs. Na+ / Na. The frequency range used for the EIS measurements is100 mHz to 100 kHz. A NEWARE BTS4000 battery analyzer testing equipment evaluatedgalvanostatic charge-discharge cycles at varied current densities from 100 to 400 mA g-1 withcut-off voltages from 0.01 to 3 V (vs. Li+ / Li) and 0.01 to 2.5 V (vs. Na+ / Na). The fabricationof Lithium-ion and sodium-ion batteries with pictorial procedures displayed in FIG.3.
[0028] Characterization of the prepared electrode and Electrochemical Performance of thefabricated electrode are described in the following paragraphs.
[0029] X-ray diffraction (XRD) analysis is a non-destructive analytical technique used todetermine the atomic and molecular structure of crystalline materials. XRD analysis as in FIG.4(a) confirmed amorphous carbon with partially graphitic domains, showing improved structuralordering at higher carbonization temperatures.
[0030] Raman analysis is a non-destructive spectroscopic technique used for chemicalidentification and characterization by observing the vibrational, rotational, and other low-frequency modes of molecules. Raman analysis as shown in FIG.4 (b) showed an increasingID / IG ratio with temperature, indicating enhanced defect density and partial graphitic orderingin air-treated activated carbon, beneficial for electrochemical performance.
[0031] Nitrogen adsorption analysis (also known as N2 physisorption) is the standard analyticaltechnique in 2025 for determining the specific surface area, pore volume, and pore sizedistribution of porous materials. Nitrogen adsorption analysis FIG.5 (a) shows the highest BETsurface area (860 m² / g) for ACH 2 due to optimized KOH-carbon interaction under limitedair activation, while lower (ACH 1) and higher (ACH 3) temperatures yielded reduced surfaceareas.
[0032] Pore analysis is an analytical process used to quantify the void spaces within a solidmaterial. Pore analysis as in FIG.5 (b) shows that ACH 2 possessed a uniform hierarchicalmicro-meso-macroporous structure with stable morphology, offering optimal ion transportand charge storage for superior electrochemical performance.
[0033] Thermogravimetric Analysis (TGA) is a thermal analysis technique that measures thechange in weight (mass) of a sample as it is heated, cooled, or held at a constant temperaturein a controlled atmosphere. TGA confirmed (FIG.5 (c)) controlled activation under airconditions at around 500 °C to 550 °C, enabling potassium intercalation and gas evolution thatproduced a stable, hierarchically porous carbon framework consistent with BET results.
[0034] Field Emission Scanning Electron Microscopy (FESEM) is an advanced imagingtechnique used to observe ultrafine surface features of materials at the nanoscale. FESEMrevealed that ACH 2 possessed a well-interconnected and uniform porous framework, whereaslower (ACH 1) and higher (ACH 3) temperatures produced less defined or degraded structures.FIG.6 (a-f) represents the FESEM images and EDAX spectrum of ACH-1, ACH-2, and ACH3 samples.
[0035] High-Resolution Transmission Electron Microscopy (HRTEM) is an advanced imagingmode of Transmission Electron Microscopy (TEM) that allows for direct visualization ofmaterial structures at the atomic scale.
[0036] X-ray Photoelectron Spectroscopy (XPS), also known as Electron Spectroscopy forChemical Analysis (ESCA), is a highly surface-sensitive technique used to identify elementsand their chemical states. FIG.7 (a-c) depicts the low to high magnification of HRTEM imagesof ACH-2 and XPS results of (d) full survey, (e) C 1s spectrum, and (f) O 1s spectrum of theACH-2 sample. HRTEM of ACH 2 showed a porous carbon network with few-layeredgraphitic (002) domains, combining high conductivity and enhanced ion-accessible surface forenergy storage.
[0037] The electrochemical performance of a fabricated electrode is assessed through astandardized suite of tests focusing on charge storage capacity, kinetics, and long-termdurability. The fabricated electrode material may be used for multiple applications such as forsuper capacitors, Li-ion batteries and Sodium-ion batteries. The performance of the electrodein each of the application is described in the following paragraphs.
[0038] In the supercapacitors (SC), ACH-2 exhibits an initial specific capacitance of 436 F g⁻¹at 0.5 A g⁻¹ current density and retains 70 F g⁻¹ at high current density of 10 A g⁻¹ after 10,000cycles, demonstrating excellent long-term cyclic stability and rate capability. FIG.8 (a) Cyclicvoltammetry of all samples, (b) Cyclic voltammetry of ACH 2, (c) Galvano-static chargedis-charge curves of ACH 2, (d) Rate capability of all the samples, (e) Cyclic stability of allsamples, and (f) EIS of the ACH 2 sample.
[0039] In the lithium-ion batteries (LIB), ACH-2 delivers an initial specific capacity of 691mAh g⁻¹ at 100 mA g⁻¹ current density and retains 133 mAh g⁻¹ at 500 mA g⁻¹ current densityafter 1000 cycles, highlighting outstanding cyclic stability and fast-charging performance,while maintaining high capacity even at increased current densities. FIG.9 (a) Cyclicvoltammetry of all samples, (b) Cyclic voltammetry of ACH 2, (c) Galvano-static chargedis-charge curves of ACH 2, (d) Rate capability of all the samples, (e) Cyclic stability of allsamples, and (f) EIS of the ACH 2 sample.
[0040] In the sodium-ion batteries (SIB), ACH-2 achieves (FIG.10 (a-f)) an initial specificcapacity of 693 mAh g⁻¹ at 100 mA g⁻¹ and retains 90 mAh g⁻¹ at 500 mA g⁻¹ current densityafter 1000 cycles, demonstrating robust long-term electrochemical performance and excellentrate capability. FIG.10: (a) Cyclic voltammetry of all samples, (b) Cyclic voltammetry of ACH2, (c) Galvano-static charge-discharge curves of ACH 2, (d) Rate capability of all the samples,(e) Cyclic stability of all samples, and (f) EIS of the ACH 2 sample.
[0041] CV and EIS studies indicate high reversibility and low charge-transfer resistance,confirming superior conductivity and multifunctional energy storage capability of ACH-2.Ratecapability: ACH-2 (FIG.11 (a-f)) retains high specific capacitance / capacity even at increasedcurrent densities, demonstrating efficient ion / electron transport. FIG.11 (a-c) Comparative rateperformance of ACH 2 at various current densities. (d-f) Galvanostatic charge-discharge(GCD) profiles of ACH 2 in Lithium-ion battery, Sodium-ion battery, and Supercapacitordevices at different current densities.
[0042] In the fast charging test, the ACH-2 electrode demonstrates exceptional fast-chargingcapability, completing LIB charging at 600 mA g⁻¹ in ~11 min (discharge at 100 mA g⁻¹ for ~2h 28 min), SIB charging at 600 mA g⁻¹ in ~12.5 min (discharge at 100 mA g⁻¹ for ~1 h 14 min),and supercapacitor charging at 100 A g⁻¹ in just ~4.4 s (discharge at 1 A g⁻¹ for ~187 s),underscoring its superior rate capability and structural robustness.
[0043] The prepared material may be applicable as an advanced anode material in lithium-ionbatteries used in electric cars, scooters, buses, and hybrid vehicles due to its high specificcapacity and long cycle life. Ideal for lithium-ion batteries powering smartphones, tablets,laptops, cameras, and smartwatches, offering improved energy density and reduced chargingtime. It is also suitable for grid-scale and residential energy storage systems integrated withsolar and wind energy, owing to the material's stability over extended cycling.
[0044] While various embodiments of the present disclosure have been described above, itshould be understood that they have been presented by example only and not by limitation.Thus, the breadth and scope of the present disclosure should not be limited by any of the abovediscussed embodiments but should be defined only by the following claims and theirequivalents.
Claims
1. An electrode material for batteries and supercapacitors comprising an activated carbon derived from white chickpeas.
2. The electrode material for batteries and supercapacitors as claimed in claim 1, wherein the said activated carbon is formed by carbonisation at 450 °C to 500 °C temperature for 30 minutes of white chickpeas and activation by potassium hydroxide (KOH) at 500 °C to 550 °C temperature for 1 hour to form ACH-2 electrode.
3. The electrode material of claim 1 exhibits an initial specific capacitance of 436 F g⁻¹ at 0.5 A g⁻¹ current density and retains 70 F g⁻¹ at high current density of 10 A g⁻¹ after 10,000 cycles for a super capacitors.
4. The electrode material of claim 1 exhibits an initial specific capacity of 691 mAh g⁻¹ at 100 mA g⁻¹ current density and retains 133 mAh g⁻¹ at 500 mA g⁻¹ current density after 1000 cycles for Li-ion batteries.
5. The electrode material of claim 1 exhibits an initial specific capacity of 693 mAh g⁻¹ at 100 mA g⁻¹ and retains 90 mAh g⁻¹ at 500 mA g⁻¹ current density after 1000 cycles for sodium ion batteries.
6. A process of synthesizing a electrode material of claim 1 comprising; preparing activated carbon from white chickpeas (101) and preparing an electrode using prepared activated carbon (102).
7. The process as claimed in claim 6, wherein the preparing activated carbon from white chickpeas (101) further comprising: soaking the white chickpeas overnight in deionized water to promote pore activation by inducing cellular swelling through water absorption; subjecting the soaked white chickpeas to preliminary carbonization in ambient air using a muffle furnace at around 450 °C to 500 °C for 30 minutes; cooling the carbonised white chickpea at room temperature; mixing the resulting carbon with KOH at a weight ratio of 1:3, using a few drops of double distilled water to assist homogenization; stirring the mixture while being heated at 80 °C until complete evaporation of water and to form gel; drying the obtained gel overnight at 100 °C in a vacuum oven to obtain a fine powder; transferring the obtained fine powder into a crucible to minimize moisture absorption and tightly sealed with aluminum foil to restrict airflow during the subsequent activation step; introducing the crucible into a preheated muffle furnace and heated at around 500 °C to 550 °C with a ramp rate of 2 °C per minute, maintained at the target temperature for 1 hour; cooling and washing the obtained activated carbon multiple times with 1 M hydrochloric acid, ethanol, acetone, and double-distilled water to remove residual impurities; and drying the washed sample at 80 °C overnight.
8. The process as claimed in claim 6, wherein the preparing an electrode using prepared activated carbon (102) further comprising; preparing a slurry containing 10 wt% carbon black, 80 wt% active material of claim 1, and 10 wt% polyvinylidene fluoride (PVDF) with a few drops of N-methylpyrrolidinone; and coating the prepared slurry on copper foil for lithium and sodium-ion batteries to make a working electrode.
9. The process as claimed in claim 6, wherein the preparing an electrode using prepared activated carbon further comprising; preparing a slurry containing 10 wt% carbon black, 80 wt% active material of claim 1, and 10 wt% polyvinylidene fluoride (PVDF) with a few drops of N-methylpyrrolidinone; and coating the prepared slurry on titanium foil for supercapacitors to make a working electrode.