Pig iron production method and ore raw material

IN598323BActive Publication Date: 2026-08-07KOBE STEEL LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202347078907
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-08
Filing Date
2023-11-21
Publication Date
2026-08-07
Estimated Expiration
2041-06-21

AI Technical Summary

Technical Problem

Conventional methods for operating blast furnaces face challenges in maintaining gas permeability due to segregation of reduced iron, which affects the stability and efficiency of the furnace operation, despite efforts to balance strength and segregation inhibition.

Method used

The use of reduced iron molded products with a specific rectangular shape and limited grain size distribution, which are compression molded and have a length ratio of longer to shorter side less than or equal to 1.5, to prevent segregation and improve gas flow and permeability in the blast furnace.

Benefits of technology

This approach enhances gas permeability and reduces segregation, leading to improved charging yield and reduced coke usage, thereby stabilizing furnace operation and increasing efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The pig iron production method according to an embodiment of the present invention is for producing pig iron using a blast furnace having a tuyere, and comprises: a step for alternately layering, in the blast furnace, first layers containing an ore raw material and second layers containing coke; and a step for reducing and melting the ore raw material of the layered first layers while blowing an auxiliary fuel into the blast furnace by means of hot air blown from the tuyere. The ore raw material contains a plurality of reduced iron molded products obtained by compression-molding reduced iron. The shapes of the reduced iron molded products each have, on both surfaces, bulges that are thicker at the center portion than at a peripheral portion thereof, and are each a chamfered rectangle in a plan view. The length ratio of the longer sides to the shorter sides of the reduced iron molded products in a plan view is at most 1.5.
Need to check novelty before this filing date? Find Prior Art

Description

[TECHNICAL FIELD]

[0001] The present invention relates to a method for producing pig iron, and an iron orematerial.[BACKGROUND ART]

[0002] A method for producing pig iron by alternately charging a first layer containing aniron ore material and a second layer containing coke alternately in a blast furnace, andreducing and melting the iron ore material while injecting an auxiliary reductant into the blastfurnace by hot air blown from a tuyere is known. During this, the coke serves as a heatsource for melting the iron ore material, a reducing agent for the iron ore material, arecarburizing agent for carburizing the molten iron to lower the melting point, and a spacerfor ensuring gas permeability in the blast furnace. Due to the coke maintaining gaspermeability, descent of the burden is stabilized, and in turn, stable operation of the blastfurnace is enabled.

[0003] In operation of a blast furnace, it is preferred that a proportion of the coke is low inlight of cost reduction. However, decreasing the proportion of the coke decreases the roleplayed by the coke. For example, as a method of decreasing the proportion of the coke, inother words increasing the proportion of the iron ore material, a method for operating a blastfurnace using reduced iron has been proposed (see Japanese Unexamined Patent ApplicationPublication No. 2015-199978). In the method for operating a blast furnace described above,operation of the blast furnace without increasing the high temperature gas permeabilityresistance is made possible by blending the reduced iron and the acidic lump ore beforehandand charging to the blast furnace.[PRIOR ART DOCUMENTS][PATENT DOCUMENTS]

[0004] Patent Document 1: Japanese Unexamined Patent Application Publication No.2015-199978[SUMMARY OF THE INVENTION][PROBLEMS TO BE SOLVED BY THE INVENTION]

[0005] The conventional method for operating a blast furnace described above takesadvantage of the reduced iron which is a material hard to pulverize, to maintain a gas flow ina shaft portion in such a manner that the reduced iron maintains its shape and serves as anaggregate even when other iron ore materials are pulverized. Therefore, in the conventionalmethod for operating a blast furnace described above, strength of the reduced iron is requiredand it is essential that the reduced iron is in a briquette form with a great apparent density.However, increasing the apparent density causes the reduced iron to accumulate in a lowerlayer, generally referred to as segregation, and the effect of improving gas permeability due tothe reduced iron is not attained. Since such an influence is remarkable when the size of thereduced iron is great, in the conventional method for operating a blast furnace describedabove, a balance between the strength of the reduced iron and inhibition of segregation isachieved by increasing the grain size of the reduced iron in accordance with to the apparentdensity. However, the above-described balanced point does not provide a sufficient effect ofimproving gas permeability, and further improvement of the gas permeability in the blastfurnace is required.

[0006] The present invention was made in view of the foregoing circumstances, and anobjective thereof is to provide a method for producing pig iron and an iron ore materialenabling improvement of gas permeability in the blast furnace.[MEANS FOR SOLVING THE PROBLEMS]

[0007] The present inventors thoroughly investigated the segregation of the reduced iron tofind that using reduced iron having a particular shape inhibits segregation, whereby thepresent invention was accomplished.

[0008] A method for producing pig iron according to an aspect of the present invention is amethod for producing pig iron using a blast furnace comprising a tuyere, the methodincluding: charging a first layer containing an iron ore material and a second layer containingcoke alternately in the blast furnace; and reducing and melting the iron ore material in thecharged first layer while injecting an auxiliary reductant into the blast furnace by hot airblown from the tuyere, in which: the iron ore material contains a plurality of reduced ironmolded products obtained by compression molding reduced iron; the reduced iron moldedproduct is in a rectangular shape chamfered in a plan view, having on both faces a bulgeresulting from a center portion being thicker than a peripheral portion; and a length ratio of alonger side to a shorter side of the reduced iron molded product in the plan view is less thanor equal to 1.5.

[0009] In the method for producing pig iron, the iron ore material in the first layer containsthe reduced iron molded product, of which a length ratio of a longer side to a shorter side inthe plan view is less than or equal to the upper limit. The reduced iron molded product is notlikely to cause segregation during charging of the first layer, whereby gas flow in the blastfurnace is made uniform and gas permeability in the blast furnace can be improved.

[0010] A proportion of the reduced iron molded product having a grain size of greater thanor equal to 50 mm in the plurality of reduced iron molded products is preferably less than orequal to 10% by mass. The reduced iron molded product contained in the iron ore materialis not likely to cause segregation during charging of the first layer, and can therefore inhibitsegregation without depending on the reduced iron molded product having a large grain size.In addition, the reduced iron molded product having a large grain size has great drop impactenergy during charging of the first layer, and is likely to be pulverized by the impact.Therefore, due to the proportion of the reduced iron molded product having a grain size ofgreater than or equal to 50 mm being less than or equal to the upper limit, the drop impactenergy is decreased, pulverization or volume breakage is inhibited, and a charging yield of thereduced iron molded product is improved, whereby the gas permeability in the blast furnacecan further be improved.

[0011] An iron ore material according to another aspect of the present invention is an ironore material used for producing pig iron including a plurality of reduced iron molded productsobtained by compression molding reduced iron, wherein: the reduced iron molded product isin a rectangular shape chamfered in a plan view, having on both faces a bulge resulting from acenter portion being thicker than a peripheral portion; and a length ratio of a longer side to ashorter side of the reduced iron molded product in the plan view is less than or equal to 1.5.

[0012] The iron ore material includes the reduced iron molded product, of which a lengthratio of a longer side to a shorter side in the plan view is less than or equal to the upper limit.The reduced iron molded product is not likely to cause segregation during charging of the ironore material; thus, when the reduced iron molded product is used for production of pig iron,gas flow in the blast furnace is made uniform and gas permeability in the blast furnace can beimproved.

[0013] As used herein, the "reduced iron molded product having a grain size of greater thanor equal to 50 mm" as referred to means a reduced iron molded product remaining on a sievehaving a 50 mm mesh after sifting.[EFFECTS OF THE INVENTION]

[0014] As described above, the method for producing pig iron and the iron ore materialaccording to the present invention can be utilized to achieve improvement of the gaspermeability in the blast furnace.[BRIEF DESCRIPTION OF THE DRAWINGS]

[0015] FIG. 1 is a flow diagram illustrating the method for producing pig iron according toan embodiment of the present invention.FIG. 2 is a schematic view illustrating the inside of the blast furnace used in themethod for producing pig iron in FIG. 1.FIG. 3 is a schematic perspective view illustrating a shape of a reduced iron moldedproduct.FIG. 4 is a schematic partial enlarged view of the vicinity of an area from a cohesivezone to a dripping zone in FIG. 2.FIG. 5 is a schematic view illustrating a configuration of a blast furnace burdendistribution experiment device used in EXAMPLES.FIG. 6 is a graph showing proportions of the material in five radial directions inEXAMPLES in a case in which a dimension of an iron plate is 20 mm x 7 mm x 4 mm.FIG. 7 is a graph showing proportions of the material in five radial directions inEXAMPLES in a case in which a dimension of an iron plate is 10 mm x 7 mm x 4 mm.FIG. 8 is a graph showing a relationship between the number of tumbler rotationsand a gas permeability resistance index during a tumbler rotation test in EXAMPLES.FIG. 9 is a graph showing a relationship between a proportion of HBI having a grainsize of greater than or equal to 50 mm and the gas permeability resistance index inEXAMPLES.[DESCRIPTION OF EMBODIMENTS]

[0016] Hereinafter, the method for producing pig iron according to each embodiment of thepresent invention will be described.

[0017] The method for producing pig iron illustrated in FIG. 1 uses a blast furnace 1illustrated in FIG. 2, and includes a charging step S1 and a reduction / melting step S2.

[0018] <Blast Furnace>A blast furnace 1 includes, as shown in FIG. 2, a tuyere 1a and a taphole 1b providedin a lower portion of a furnace. In general, a plurality of tuyeres 1a are provided. The blastfurnace 1 is a solid-gas countercurrent type shaft furnace that enables: hot air, which ishigh-temperature air with high-temperature or normal-temperature oxygen being added asneeded, to be blown from the tuyere 1a into the furnace; a series of reactions such asreduction and melting of an iron ore material 11 described later to take place; and pig iron tobe tapped from the taphole 1b. In addition, the blast furnace 1 is equipped with a bell-armortype raw material charging device 2. The raw material charging device 2 will be describedlater.

[0019] <Charging Step>In a charging step S1, as shown in FIG. 2, a first layer 10 and a second layer 20 arealternately charged in the blast furnace 1. In other words, the first layer 10 and the secondlayer 20 each have two or more layers.

[0020] (First Layer)The first layer 10 includes an iron ore material 11 which is itself an embodiment ofthe present invention. The iron ore material 11 is used for production of pig iron, and isheated and reduced into molten iron F by the hot air blown from the tuyere 1a in thereduction / melting step S2.

[0021] [Iron Ore Material]The "iron ore material" refers to mineral ore serving as an iron material, and containsprincipally iron ore. The iron ore material 11 contains a plurality of reduced iron moldedproducts 11a obtained by compression molding reduced iron. The iron ore material 11 maycontain, as other iron ore materials 11b, calcined iron ore (iron ore pellets, sinter), lump ironore, carbon composite agglomerated iron ore, metal, and the like.

[0022] The reduced iron molded product 11a (Hot Briquette Iron, HBI) improves gaspermeability in a cohesive zone D described later, and serves as an aggregate for causing thehot air to permeate to the central portion of the blast furnace 1.

[0023] The reduced iron molded product 11a is obtained by molding direct reduced iron(DRI) in a hot state. While the DRI has disadvantages of high porosity and exothermicoxidization during marine transportation and outdoor storage, the HBI has low porosity and isless likely to be reoxidized. After serving to ensure gas permeability in the first layer 10, thereduced iron molded product 11a functions as a metal and becomes molten iron. Since thereduced iron molded product 11a is high in metallization rate and requires no reduction, at thetime of becoming the molten iron, the reduction agent is not required in a large amount. TheCO2 emission can thus be decreased. Note that the "metallization rate" as referred to meansa proportion [% by mass] of the metallic iron with respect to the total iron content.

[0024] The reduced iron molded product 11a is generally produced by a twin roll moldingdevice. At this time, as shown in FIG. 3, the reduced iron molded product 11a is in arectangular shape chamfered in a plan view, having on both faces a bulge resulting from acenter portion being thicker than a peripheral portion. Specifically, a contour of a crosssection in a direction perpendicular to the longer side of the reduced iron molded product 11abulges upward and downward in an arcuate shape with respect to a rectangular face. On theother hand, a contour of a cross section in a direction parallel to the longer side is in anarcuate shape upward and downward in the vicinity of each of shorter sides, and substantiallyparallel to the rectangular face in a center portion. Note that the contour of the cross sectionin the direction perpendicular to the longer side may also include a portion substantiallyparallel to the rectangular face in a center portion. Endpoints of the arcs extending upwardand downward at the positions of the longer sides of the contour of the cross section in thedirection perpendicular to the longer side, and the positions of the shorter sides of the contourin the direction parallel to the longer side may coincide or, as shown in FIG. 3, have a certaindistance, between which the contour may have a linear portion extending upward anddownward. In addition, a shape in a plan view is the chamfered rectangular shape asdescribed above, in other words a rectangle with rounded corners. At least sidescorresponding to the longer side are composed of rounded corners and straight lines, whilesides corresponding to the shorter side may be composed of either rounded corners andstraight lines, or only rounded corners as shown in FIG. 3. Note that the reduced ironmolded product 11a may have a so-called burr particularly in a circumferential edge portion.In addition, the reduced iron molded product may be partially cracked due to a molding defect,or broken due to impact and / or the like during transportation or charging to the blast furnace,and such an incomplete reduced iron molded product may be contained in a part of the ironore material; however, the "shape of the reduced iron molded product" as used to herein refersto a complete product, which does not include the incomplete reduced iron molded product,and means a shape of a main part of the reduced iron molded product without the burr.

[0025] A proportion of the reduced iron molded product 11a in which a length of the longerside of the reduced iron molded product 11a in a plan view (L in FIG. 3) is greater than orequal to 40 mm and less than or equal to 140 mm, a length of the shorter side of the reducediron molded product 11a in a plan view (B in FIG. 3) is greater than or equal to 20 mm andless than or equal to 70 mm, and a thickness of the reduced iron molded product 11a (heightof a thick part of the central portion, H in FIG. 3) is greater than or equal to 20 mm and lessthan or equal to 50 mm is preferably greater than or equal to 50% by mass, more preferablygreater than or equal to 70% by mass, and still more preferably greater than or equal to 80%by mass.

[0026] In addition, the upper limit of a ratio of the longer side L to the shorter side B (L / B)of the reduced iron molded product 11a in a plan view is 1.5, and more preferably 1.4.When L / B is greater than the upper limit, the reduced iron molded product 11a may be morelikely to segregate when the iron ore material 11 is charged in the first layer 10. On the otherhand, the lower limit of L / B is 1.0, since the longer side ≥ the shorter side.

[0027] The upper limit of the proportion of the reduced iron molded product 11a having agrain size of greater than or equal to 50 mm in the plurality of reduced iron molded products11a is preferably 10% by mass, and more preferably 8% by mass. The reduced iron moldedproduct 11a contained in the iron ore material 11 is not likely to cause segregation duringcharging of the first layer 10, and can therefore inhibit segregation without depending on thereduced iron molded product 11a having a large grain size. In addition, the reduced ironmolded product 11a having a large grain size has great drop impact energy during charging ofthe first layer 10, and is likely to be pulverized by the impact. Therefore, when theproportion of the reduced iron molded product 11a having a grain size of greater than or equalto 50 mm is less than or equal to the upper limit, the drop impact energy is decreased,pulverization or volume breakage is inhibited, and a charging yield of the reduced ironmolded product 11a is improved, whereby the gas permeability in the blast furnace can furtherbe improved.

[0028] The upper limit of a content of the reduced iron molded product 11a in the iron orematerial 11 is preferably 30% by mass, and more preferably 25% by mass. When thecontent of the reduced iron molded product 11a is less than or equal to the upper limit, thesegregation can be inhibited, whereby the ore inclined angle is stabilized at a low level. As aresult, the reduced iron molded product 11a can be present in the first layer 10 relativelyhomogeneously, whereby the hot air can be ensured to permeate to the central portion of theblast furnace 1. Therefore, the amount of coke 21 used can be decreased. In addition,instability of the first layer 10 due to the segregation of the reduced iron molded product 11acan be avoided, whereby layer collapse can be inhibited when melting occurs from a lowerside and an upper layer descends in the reduction / melting step S2. Note that the ore inclinedangle refers to an angle of an inclined face of an iron ore deposition layer (such as the firstlayer 10) from the horizon.

[0029] The lower limit of a charged rate of the reduced iron molded product 11a ispreferably 100 kg and more preferably 150 kg per 1 ton of the pig iron. When the chargedrate of the reduced iron molded product 11a is less than the lower limit, the function of thereduced iron molded product 11a ensuring gas permeability in the cohesive zone D in thereduction / melting step S2 may not be sufficiently exerted. On the other hand, the upper limitof the charged rate of the reduced iron molded product 11a is defined as appropriate in such arange that the aggregate is not excessive and does not decrease the effect of the aggregate, andis, for example, 700 kg per 1 ton of the pig iron.

[0030] The lower limit of a ratio of an average grain size of the reduced iron molded product11a to an average grain size of the other iron ore materials 11b is preferably 1.3, and morepreferably 1.4. As illustrated in FIG. 4, even when a part of the other iron ore materials 11bin the first layer 10 is melted and moves to the lower side of the blast furnace 1 as drippingslag 12 and the other iron ore materials 11b having moved are softened and shrunk, thereduced iron molded product, having a high melting point, is not softened. Blending thereduced iron molded product 11a, which is larger than the other iron ore materials 11b to atleast a certain degree, as the aggregate facilitates the aggregate effect of the reduced ironmolded product 11a to be exerted and enables suppression of layer shrinkage of the entire firstlayer 10. Consequently, when the ratio of the average grain sizes is greater than or equal tothe lower limit, a channel of the hot air shown by an arrow in FIG. 4 can be secured, wherebygas permeability in the reduction / melting step S2 can be improved. Meanwhile, the upperlimit of the ratio of the average grain sizes is preferably 10 and more preferably 5. When theratio of the average grain sizes is greater than the upper limit, it may be difficult to blend thereduced iron molded product 11a uniformly into the first layer 10, leading to an increase insegregation. Note that the "average grain size" as referred to means such a grain size that anaccumulated mass is 50% in a grain size distribution.

[0031] In addition, when the reduced iron molded product 11a contains aluminum oxide, theupper limit of the content of the aluminum oxide in the reduced iron molded product 11a ispreferably 1.5% by mass and more preferably 1.3% by mass. When the content of thealuminum oxide is greater than the upper limit, ensuring of the gas permeability in a lowerposition of the furnace may be difficult due to a higher melting point of the slag and increasedviscosity. Consequently, by configuring the content of aluminum oxide in the reduced ironmolded product 11a to be less than or equal to the upper limit, an increase in the amount ofthe coke 21 used in the second layer 20 described later can be inhibited. Note that thecontent of the aluminum oxide may be 0% by mass, in other words the reduced iron moldedproduct 11a may not contain the aluminum oxide, but the lower limit of the content of thealuminum oxide is preferably 0.5% by mass. When the content of the aluminum oxide isless than the lower limit, the reduced iron molded product 11a may become expensive and theproduction cost of the pig iron may increase.

[0032] In addition to the iron ore material 11, auxiliary materials such as limestone,dolomite, and silica may also be charged into the first layer 10. Furthermore, in the firstlayer 10, undersize small-grain coke obtained by sifting the coke is generally used in mixture,in addition to the iron ore material 11.

[0033] (Second Layer)The second layer 20 contains the coke 21.

[0034] The coke 21 serves: as a heat source for melting the iron ore material 11; to generateCO gas as a reducing agent necessary for reduction of the iron ore material 11; as arecarburizing agent for carburizing the molten iron to lower the melting point; and as a spacerfor ensuring gas permeability in the blast furnace 1.

[0035] (Charging Method)Various methods can be used as a method for alternately charging the first layer 10and the second layer 20. The method is described herein with reference to the blast furnace1 equipped with the bell-armor type raw material charging device 2 as shown in Fig. 2(hereinafter, may be also merely referred to as "raw material charging device 2").

[0036] The raw material charging device 2 is provided in a furnace top portion. In otherwords, the first layer 10 and the second layer 20 are charged from the furnace top. The rawmaterial charging device 2 includes a bell cup 2a, a lower bell 2b, and an armor 2c as shownin FIG. 2.

[0037] In the bell cup 2a, the raw material to be charged is loaded. When the first layer 10is charged, a raw material constituting the first layer 10 is loaded into the bell cup 2a, andwhen the second layer 20 is charged, a raw material constituting the second layer 20 is loaded.

[0038] The lower bell 2b is in a cone shape expanding downward, and is provided in the bellcup 2a. The lower bell 2b is vertically movable (in FIG. 2, a solid line shows a state inwhich the lower bell has moved upward and a dotted line shows a state in which the lowerbell has moved downward). The lower bell 2b moves upward to hermetically seal a lowerportion of the bell cup 2a, and moves downward to leave a gap on an extended line of a lateralwall of the bell cup 2a.

[0039] The armor 2c is provided on a furnace wall portion of the blast furnace 1, below thelower bell 2b. When the lower bell 2b is moved downward, the raw material falls throughthe gap. The armor 2c serves as a rebound plate for rebounding the fallen raw material. Inaddition, the armor 2c is configured to be protrudable and retractable with respect to a centerof the blast furnace 1.

[0040] By using the raw material charging device 2, the first layer 10 can be charged asfollows. Note that the same applies to the second layer 20. In addition, the first layer 10and the second layer 20 are alternately charged.

[0041] First, the lower bell 2b is positioned upward and the raw material of the first layer 10is charged into the bell cup 2a. When the lower bell 2b is positioned upward, the lowerportion of the bell cup 2a is hermetically sealed and the raw material is loaded into the bellcup 2a. Note that the loading amount thereof is a charging amount of each layer. In a casein which a capacity of the bell cup 2a is smaller than a charging amount of each layer, the firstlayer 10 can be charged in a plurality of installments. The charging with a single load maybe also referred to as a "batch".

[0042] Next, the lower bell 2b is moved downward. As a result, a gap is formed withrespect to the bell cup 2a, and the raw material falls through the gap to hit the armor 2c. Theraw material having hit and been rebounded by the armor 2c is charged into the furnace.The raw material falls while moving in an inward direction of the furnace due to reboundingat the armor 2c, and accumulates while flowing from the fallen position toward a central sideof the furnace interior. Since the armor 2c is configured to be protrudable and retractablewith respect to the inside of the blast furnace, the fallen position of the raw material can beadjusted by protruding and retracting the armor 2c. Due to this adjustment, the first layer 10can be accumulated in a desired shape.

[0043] <Reduction / Melting Step>In the reduction / melting step S2, the iron ore material 11 in the charged first layer 10is reduced and melted while an auxiliary reductant is injected into the blast furnace 1 by hotair blown from the tuyere 1a. Note that the operation of the blast furnace is continuous, andthus the reduction / melting step S2 is carried out continuously. On the other hand, thecharging step S1 is carried out intermittently, and the first layer 10 and the second layer 20 tobe processed in the reduction / melting step S2 are added according to the circumstances of thereduction and melting process of the first layer 10 and the second layer 20 in thereduction / melting step S2.

[0044] FIG. 2 illustrates a state in the reduction / melting step S2. As shown in FIG. 2, araceway A, which is a hollow portion in which the coke 21 swivels and is present in asignificantly sparse state, is formed in the vicinity of the tuyere 1a, due to the hot air from thetuyere 1a. In the blast furnace 1, the temperature of the raceway A is the highest, beingabout 2,000 °C. A deadman B, which is an aggregation-stagnation zone of the coke insidethe blast furnace 1, is present adjacent to the raceway A. In addition, the dripping zone C,the cohesive zone D, and the lumpy zone E are present in an upward direction in this orderfrom the deadman B.

[0045] The temperature in the blast furnace 1 increases from the top portion toward theraceway A. In other words, the temperature increases in the order of the lumpy zone E, thecohesive zone D, and the dripping zone C. For example, the temperature of the lumpy zoneE is about greater than or equal to 20 °C and less than or equal to 1,200 °C, while thetemperature of the deadman B is about greater than or equal to 1,200 °C and less than or equalto 1,600 °C. Note that the temperature of the deadman B varies in the radial direction, andthe temperature of a central portion of the deadman B may be lower than the temperature ofthe dripping zone C. In addition, by stably circulating the hot air in the central portion in thefurnace, the cohesive zone D having an inverted V-shaped cross section is formed, wherebygas permeability and reducibility are ensured in the furnace.

[0046] In the blast furnace 1, the iron ore material 11 is first heated and reduced in thelumpy zone E. In the cohesive zone D, the iron ore reduced in the lumpy zone E is softenedand shrunk. The softened and shrunk iron ore falls as the dripping slag, and moves to thedripping zone C. In the reduction / melting step S2, reduction of the iron ore material 11proceeds principally in the lumpy zone E, while melting of the iron ore material 11 proceedsprincipally in the dripping zone C. Note that in the dripping zone C and the deadman B,direct reduction proceeds, which is a direct reaction between the fallen liquid iron oxide FeOand carbon in the coke 21.

[0047] The reduced iron molded product 11a exerts the aggregate effect in the cohesive zoneD. In other words, even in a state in which the iron ore is softened and shrunk, the reducediron molded product 11a having a high melting point is not softened, and secures a gaspermeation channel ensuring permeation of the hot air to the central portion of the blastfurnace 1.

[0048] In addition, the molten iron F obtained by melting the reduced iron is accumulated ona hearth, and molten slag G is accumulated on the molten iron F. The molten iron F and themolten slag G can be tapped from the taphole 1b.

[0049] <Advantages>The iron ore material 11 includes the reduced iron molded product 11a, of which alength ratio of a longer side to a shorter side in the plan view is less than or equal to 1.5. Thereduced iron molded product 11a is not likely to cause segregation during charging of the ironore material 11; thus, when the reduced iron molded product is used for production of pig iron,gas flow in the blast furnace 1 is made uniform and gas permeability in the blast furnace 1 canbe improved.

[0050] In addition, in the method for producing pig iron, the iron ore material 11 accordingto the present invention is charged in the first layer 10, whereby a gas flow in the blast furnace1 is made uniform and the gas permeability in the blast furnace 1 can be improved.

[0051] [Other Embodiments]It is to be noted that the present invention is not limited to the above-describedembodiments.

[0052] In the above-described embodiment, regarding the iron ore material of the presentinvention, a case of containing the reduced iron molded product and the other iron orematerials has been described; however, the iron ore material of the present invention maycontain only the reduced iron molded product. Such an iron ore material can be blendedwith other types of iron ore materials as needed, and included in the first layer charged in theblast furnace.

[0053] In the above-described embodiment, the method for producing pig iron of the presentinvention including only the charging step and the reduction / melting step has been described;however, the method for producing pig iron may include other steps.

[0054] For example, the method for producing pig iron may include a step of charging amixture of the coke and the reduced iron molded product to the central portion of the blastfurnace. In this case, it is preferred that the proportion of the reduced iron molded product11a having a grain size of greater than or equal to 5 mm is greater than or equal to 90% bymass in the reduced iron molded products in the mixture, and the content of the reduced ironmolded product in the mixture is less than or equal to 70% by mass. The hot air that hasreached the central portion of the blast furnace goes up in the central portion. Due to thereduced iron molded product having a large grain size included in the central portion in acontent less than or equal to the upper limit, the sensible heat can be effectively used withoutencumbering the flow of the hot air. Therefore, the amount of coke used can further bedecreased. As used herein, the "central portion" of the blast furnace refers to a region at adistance of no greater than 0.2Z from the center, Z being a radius of a furnace throat portion.

[0055] In addition, the method for producing pig iron may include a step of finelypulverizing powder derived from the reduced iron molded product and coal. In this case, itis preferred that the fine powder obtained by the fine pulverizing step is included as theauxiliary reductant. A part of the reduced iron molded product is pulverized into powderduring a transportation process and / or the like. Such powder lowers the gas permeability inthe blast furnace, and is inappropriate for use as the first layer. In addition, this powder has agreat specific surface area, and is reoxidized into iron oxide. Injecting the auxiliaryreductant containing the iron oxide from the tuyere enables improvement of gas permeability.Consequently, by finely pulverizing powder derived from the reduced iron molded producttogether with coal and using fine powder obtained by finely pulverizing the powder and thecoal as the auxiliary reductant to be injected from the tuyere, the reduced iron molded productcan be effectively used and gas permeability in the blast furnace can be improved.

[0056] Although the case of employing the bell-armor type as the charging step according tothe above-described embodiment has been described, other types may also be employed.Examples of the other types include a bell-less type. With the bell-less type, charging can becarried out by using a swivel chute and adjusting the angle thereof.[EXAMPLES]

[0057] Hereinafter, the present invention is explained in further detail by way of Examples,but the present invention is not in any way limited to these Examples.

[0058] <Shape of reduced iron molded product>First, an experiment was conducted regarding an influence of the shape of thereduced iron molded product on segregation.

[0059] FIG. 5 illustrates a blast furnace burden distribution experiment device 8 used in thisexperiment. The blast furnace burden distribution experiment device 8 illustrated in FIG. 5is a two-dimensional slice cold model simulating the bell-armor type raw material chargingdevice on a scale of 1 / 10.7. The size of the blast furnace burden distribution experimentdevice 8 is 1,450 mm in height (length L1 in FIG. 5), 580 mm in width (length L2 in FIG. 5),and 100 mm in depth (length in a direction perpendicular to a sheet surface of FIG. 5).

[0060] Each constitutive element of the blast furnace burden distribution experiment device8 is denoted by the same reference numeral as the corresponding constitutive element havingthe same function of the bell-armor type raw material charging device 2 in FIG. 2. Since thefunction is the same, detailed description thereof is omitted. In addition, the blast furnaceburden distribution experiment device 8 includes a center charging chute 8a for charging thecoke, simulating central charging, as shown in FIG. 5.

[0061] A coke layer 81 as a base, a center charged coke layer 82, a first iron ore layer 83,and a second iron ore layer 84 were charged in this order to the blast furnace burdendistribution experiment device 8.

[0062] Raw materials used for charging the first iron ore layer 83 and the second iron orelayer 84 were: sinter simulating sinter and lump iron ore (2.8 to 4.0 mm in grain size);alumina balls simulating the iron ore pellets (2 mm in diameter); coke simulating lump coke(8.0 to 9.5 mm in grain size), and an iron plate simulating the reduced iron molded product(HBI). The raw materials were on a scale of 2 / 11.2. Meanwhile, a mass ratio of theHBI / sinter / alumina balls was 18.5% by mass / 32.6% by mass / 48.9% by mass.

[0063] Under the above-specified conditions, with the iron plates simulating the HBI havingthe sizes of 20 mm x 7 mm x 4 mm (length ratio L / B of a longer side to a shorter side = 2.86)and 10 mm x 7 mm x 4 mm (L / B = 1.43), iron ore samples were obtained after charging infive positions (A to E) in a radial direction, and proportions of each raw material weredetermined. The results in the case of L / B = 2.86 are shown in FIG. 6, and the results in thecase of L / B = 1.43 are shown in FIG. 7.

[0064] As shown in FIG. 5, the first iron ore layer 83 and the second iron ore layer 84accumulated in a downward inclined manner toward the vicinity of the center. In this case,the HBI having a great individual weight tends to segregate in the vicinity of the center, whichis on a lower side. FIG. 6 shows that in the case of L / B = 2.86, the proportion of the HBI inthe vicinity of the center increased and segregation occurred. Note that the small proportionof the HBI in A and B, being close to the periphery, was intentional. In other words, this isdue to control such that the proportion of the HBI is decreased during charging of the rawmaterial, since the gas permeability is easily ensured in the periphery.

[0065] In contrast, although the individual weight was sufficiently greater than that of thesinter and the alumina ball in the case of L / B = 1.43 as well, the proportion of the HBI wasrelatively stable in C to E, being close to an intermediate position to the vicinity of the center,as shown in FIG. 7, and the segregation was inhibited as compared to the case of L / B = 2.86in FIG. 6.

[0066] The foregoing shows that the length ratio of the longer side to the shorter side of thereduced iron molded product being less than or equal to 1.5 can inhibit segregation duringcharging of the iron ore material.

[0067] <Grain size of reduced iron molded product>Next, an experiment was conducted regarding an influence of the grain size of thereduced iron molded product on the gas permeability resistance index.

[0068] First, an influence of a difference in the drop impact energy due to difference in grainsize on the gas permeability resistance index was investigated. Specifically, a tumblerrotation test was conducted in order to subject the HBI to an impact simulating atransportation state.

[0069] The tumbler rotation test of the HBI was conducted pursuant to JIS-M8712:2000"Iron ores (pellets, sinter) -- Determination of tumble strength". The rotary drum was madeof a steel plate having a thickness of 6 mm, an inner diameter of 1,000 mm, and a length of500 mm. On an inner face, two blades made of equal-angle steel of 50 mm x 50 mm x 6mm were attached in an axial direction in symmetrical positions. An attachment face thereofwas opposite to a rotational direction, whereby the sample was easily lifted by rotation.

[0070] The sample used was dried HBI of 15 ± 0.15 kg. The test was conducted whilechanging details of the size of the sample (changing proportions of large-sized HBI andsmall-sized HBI). Note that the large-sized HBI refers to HBI having a grain size of greaterthan or equal to 40 mm and less than or equal to 100 mm, and the small-sized HBI refers toHBI having a grain size of greater than or equal to 20 mm and less than 40 mm.

[0071] After rotating the rotary drum a predetermined number of times at a rotation speed of25 ± 1 rpm, a gas permeability resistance index K was calculated as follows. Specifically,the following procedure was followed. After conducting the tumbler rotation test, a grainsize distribution of the reduced iron molded product was obtained by sieving. The grain sizedistribution is expressed with di [cm] as a representative grain size (median value) betweenmeshes used for the sieving, and wi as a weight fraction of the reduced iron molded productfalling into the representative grain size di. Using this grain size distribution, a harmonicmean diameter Dp [cm] and a granularity composition index Isp were calculated by thefollowing equation 1. Furthermore, by using the gravitational conversion factor gc [9.807(g·cm) / (G·sec2)], the gas permeability resistance index K was obtained by the followingequation 1. The results are shown in FIG. 8.[Math. 1]Equation

[0072] The results in FIG. 8 show that when the number of tumbler rotations increased andaccumulated rotation drop impact increased, the HBI was destroyed and the gas permeabilityresistance index K increased. On the other hand, with the same number of rotations,comparison shows that when the proportion of the large-sized HBI increased and theproportion of the small-sized HBI decreased, the gas permeability resistance index Kincreased. The reason therefor is inferred to be an increase in drop impact due to an increasein the individual weight.

[0073] Given this, the proportion of the HBI having a grain size of greater than or equal to50 mm was changed, and the above-described tumbler rotation test was conducted with 400and 800 rotations to calculate the gas permeability resistance index K. The results are shownin FIG. 9.

[0074] The results in FIG. 9 show that the proportion of the HBI having a grain size ofgreater than or equal to 50 mm being less than or equal to 10% by mass enabled inhibition ofpulverization and volume breakage during transportation and charging to the blast furnace.As a result, a charging yield of the HBI and the gas permeability in the blast furnace can beimproved.[INDUSTRIAL APPLICABILITY]

[0075] The method for producing pig iron and the iron ore material according to the presentinvention can be utilized to achieve improvement of the gas permeability in the blast furnace.[Explanation of the Reference Symbols]

[0076] 1 Blast furnace1a Tuyere1b Taphole2 Raw material charging device2a Bell cup2b Lower bell2c Armor10 First layer11 Iron ore material11a Reduced iron molded product11b Other iron ore materials12 Dripping slag20 Second layer21 Coke8 Blast furnace burden distribution experiment device8a Center charging chute81 Coke layer82 Center charged coke layer83 First iron ore layer84 Second iron ore layerA RacewayB DeadmanC Dripping zoneD Cohesive zoneE Lumpy zoneF Molten ironG Molten slag

Claims

1. A method for producing pig iron using a blast furnace comprising a tuyere, the method comprising: charging a first layer comprising an iron ore material and a second layer comprising coke alternately in the blast furnace; and reducing and melting the iron ore material in the charged first layer while injecting an auxiliary reductant into the blast furnace by hot air blown from the tuyere, wherein: the iron ore material comprises a plurality of reduced iron molded products obtained by compression molding reduced iron; the reduced iron molded product is in a rectangular shape chamfered in a plan view, having on both faces a bulge resulting from a center portion being thicker than a peripheral portion; and a length ratio of a longer side to a shorter side of the reduced iron molded product in the plan view is less than or equal to 1.5.

2. The method for producing pig iron according to claim 1, wherein a proportion of the reduced iron molded product having a grain size of greater than or equal to 50 mm in the plurality of reduced iron molded products is less than or equal to 10% by mass.

3. An iron ore material used for producing pig iron comprising a plurality of reduced iron molded products obtained by compression molding reduced iron, wherein: the reduced iron molded product is in a rectangular shape chamfered in a plan view, having on both faces a bulge resulting from a center portion being thicker than a peripheral portion; and a length ratio of a longer side to a shorter side of the reduced iron molded product in the plan view is less than or equal to 1.5.