Laminate and method for using laminate

IN604659BActive Publication Date: 2026-09-30SEKISUI CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202317016722
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-09-29
Filing Date
2023-03-13
Publication Date
2026-09-30
Estimated Expiration
2041-09-24

AI Technical Summary

Technical Problem

Existing battery covers, particularly those made of metal materials, fail to adequately reduce heat and flame transmission from igniting batteries, potentially leading to vehicle fires during thermal runaway events.

Method used

A laminate comprising a fiber layer with a resin and a thermal insulation layer is developed, which includes a chlorinated polyvinyl chloride resin and inorganic fillers, enhancing mechanical strength and effectively impeding heat and flame transmission when used as a battery cover.

Benefits of technology

The laminate provides excellent flame-shielding and heat-shielding performance, significantly reducing the transmission of heat and flame from an igniting battery to the outside, thereby preventing rapid vehicle interior heating and potential fires.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a laminate having exceptional flame-shielding performance and heat-shielding performance, the laminate particularly being capable of suppressing transmission of flames or heat produced due to ignition from inside a battery to the outside when the laminate is used as a cover of a vehicle-mounted battery. The present invention is a laminate having a fiber layer that includes a resin and fibers, and a heat-insulating layer provided to at least one surface of the fiber layer.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to a laminate that hasexcellent flame-shielding performance and heat-shieldingperformance and can reduce the transmission of flame andheat generated by ignition inside a battery to the outside,especially when used as a cover for an in-vehicle battery.BACKGROUND ART

[0002] Various batteries, such as lithium-ion batteries, areat risk of thermal runaway and ignition due to events suchas internal short circuits. In particular, in-vehiclebatteries can undergo thermal runaway and ignite due to theimpact of a vehicular accident, for example, and may causea vehicle fire. Covers for batteries thus need to impedethe transmission of heat from the battery to thesurroundings when the battery has become abnormally hot dueto thermal runaway, or impede the transmission of flamegenerated by battery ignition to the outside.

[0003] As an example of such a cover for an in-vehiclebattery, Patent Literature 1 discloses a battery casingmade of a metal material such as iron or aluminum.Patent Literature 2 discloses a vehicle batterycasing including a metal material such as an aluminum alloyor stainless steel as a substrate.Patent Literature 3 discloses an in-vehicle batterycontaining body constituted by a laminate that includes alayer including a thermoplastic resin such as polyamide anda reinforcing fiber such as glass fiber.CITATION LIST- Patent Literature

[0004] Patent Literature 1: JP 2001-294048 APatent Literature 2: JP 2013-97883 APatent Literature 3: WO 2019 / 044801SUMMARY OF INVENTIONTechnical problem

[0005] However, covers including a metal material as asubstrate as disclosed in Patent Literatures 1 and 2 maynot sufficiently reduce the transmission of heat generatedby battery ignition and may fail to prevent the inside ofthe vehicle from rapidly becoming hot. The in-vehiclebattery containing body disclosed in Patent Literature 3may not sufficiently reduce the combustion of the resinitself.

[0006] The present invention aims to provide a laminate thathas excellent flame-shielding performance and heat-shielding performance and can reduce the transmission offlame and heat generated by ignition inside a battery tothe outside, especially when used as a cover for an in-vehicle battery.Solution to problem

[0007] The present invention relates to a laminateincluding: a fiber layer including a resin and a fiber; anda thermal insulation layer formed on at least one surfaceof the fiber layer.The present invention is described in detail below.

[0008] After extensive studies, the present inventors foundout that forming a thermal insulation layer on at least cnesurface of a fiber layer including a resin and a fiber canimpede the transmission of flame and heat generated insidea battery to the outside especially when the laminate isused as a cover for an in-vehicle battery. The inventorsthus completed the present invention.

[0009] The laminate of the present invention includes afiber layer including a resin and a fiber.The presence of the fiber layer enables the laminateto exhibit sufficient mechanical strength and preventdamage and the like due to collision accidents when thelaminate is used as a battery cover.

[0010] The fiber layer includes a resin.Examples of the resin include: synthetic resins suchas thermoplastic resins and thermosetting resins; andelastomers.

[0011] Examples of the thermoplastic resins includechlorinated polyvinyl chloride resins (CPVC), polyvinylchloride resins (PVC), polyolefins such as polyethylene andpolypropylene, polystyrene (PS), acrylonitrile-styrenecopolymers (AS resins), acrylonitrile-butadiene-styrenecopolymers (ABS resins), acrylic resins such as polymethylmethacrylate, polyamides, polycarbonates, polysulfone (PSUresin), polyphenylsulfone (PPSU), polyethersulfone (PESresin), polyetherimide (PEI resin), polyphenylene sulfide(PPS resin), polyester resins such as polyethyleneterephthalate and polybutylene terephthalate, polyacetals,polyimides, polyphenylene ether, polyether ether ketone,and liquid crystal polymers.

[0012] Examples of the thermosetting resins includepolyurethanes, phenolic resins, epoxy resins, urea resins,melamine resins, silicone resins, unsaturated polyesterresins, alkyd resins, and thermosetting polyimides.

[0013] Examples of the elastomers include thermoplasticelastomers such as olefin elastomers, styrene elastomers,ester elastomers, amide elastomers, and vinyl chlorideelastomers.

[0014] The above resins may be used alone or in combinationof two or more thereof.In particular, thermoplastic resins are preferred,and chlorinated polyvinyl chloride resins are morepreferred.The resin may be crosslinked or modified as long asthe effects of the present invention are not impaired.The method for crosslinking is not limited. Examplesthereof include crosslinking methods typically used for theabove resin components, such as crosslinking methodsinvolving the use of various crosslinking agents orperoxides and crosslinking methods involving electron rayirradiation.

[0015] When the resin includes a chlorinated polyvinylchloride resin, the chlorinated polyvinyl chloride resinpreferably has a chlorine content of 57% by mass or greaterand 72% by mass or less.A decrease in the chlorine content decreases heatresistance, while an increase in the chlorine contentdecreases moldability.The chlorine content of the chlorinated polyvinylchloride resin is more preferably 60% by mass or greaterand 71% by mass or less.The chlorine content can be measured by a method inconformity with JIS K 7229, for example.

[0016] The chlorinated polyvinyl chloride resin preferablyhas an average degree of polymerization of 400 to 3,000,more preferably 600 to 2,000.The average degree of polymerization within the rangeis advantageous in that thermally decomposed products ofthe resin are less likely to disperse in combustion,allowing the flame-shielding performance to be kept high.The average degree of polymerization can be measuredby a method in conformity with JIS K 6720-2:13999, forexample.

[0017] The chlorinated polyvinyl chloride resin is a resinobtained by chlorinating a polyvinyl chloride resin (PVC).Examples of the polyvinyl chloride resin include avinyl chloride homopolymer, a copolymer of a vinyl chloridemonomer and a monomer with unsaturated bond(s) that iscopolymerizable with the vinyl chloride monomer, and agraft copolymer obtained by grafting a vinyl chloridemonomer to a polymer. These polymers may be used alone orin combination of two or more thereof.

[0018] Examples of the monomer with unsaturated bond(s) thatis copolymerizable with the vinyl chloride monomer includea-olefins, vinyl esters, vinyl ethers, (meth)acrylates,aromatic vinyls, vinyl halides, and N-substitutedmaleimides. These monomers may be used alone or incombinations of two or more.Examples of the a-olefins include ethylene,propylene, and butylene.Examples of the vinyl esters include vinyl acetateand vinyl propionate.Examples of the vinyl ethers include butyl vinylether and cetyl vinyl ether.Examples of the (meth)acrylates include methyl(meth)acrylate, ethyl ({(meth)acrylate, butyl acrylate, andphenyl methacrylate.Examples of the aromatic vinyls include styrene andα-methyl styrene.Examples of the vinyl halides include vinylidenechloride and vinylidene fluoride.Examples of the N-substituted maleimides include N-phenyl maleimide and N-cyclohexyl maleimide.

[0019] The polymer to which vinyl chloride is graftcopolymerized is not limited as long as vinyl chloride canbe graft polymerized. Examples of such a polymer includeethylene copolymers, acrylonitrile-butadiene copeclymers,polyurethane, chlorinated polyethylene, and chlorinatedpolypropylene. These may be used alone or in combinationof two or more. Examples of the ethylene copolymersinclude ethylene-vinyl acetate copolymers, ethylene-vinylacetate-carbon monoxide copolymers, ethylene-ethyl acrylatecopolymers, ethylene-butyl acrylate-carbon monoxidecopolymers, ethylene-methyl methacrylate copolymers, andethylene-propylene copolymers.

[0020] The average degree of polymerization of the BVC isnot limited, and a typical average degree of polymerizationof 400 to 3,000 is preferred. The average degree ofpolymerization is more preferably 600 to 2,000. Theaverage degree of polymerization can be measured by amethod specified in JIS K 6720-2:1999.The method for polymerizing the PVC is not limited.A conventionally known method such as aqueous suspensionpolymerization, bulk polymerization, solutionpolymerization, or emulsion polymerization can be used.

[0021] The resin preferably has an oxygen index of 20 orgreater.When the oxygen index is 20 or greater, the resin canexhibit excellent flame-shielding performance.The oxygen index is more preferably 22 or greater andis preferably 90 or less, more preferably 70 or less.The oxygen index is the minimum concentration (% byvolume) of oxygen necessary to sustain combustion of amaterial. Tt is determined in conformity with JIS K7201-2:2007, for example.

[0022] The resin preferably has a weight average molecularweight of 1,000 to 1,000,000. Thermosetting resins arepreferably crosslinked to such an extent that they do notflow when heated, but the extent of crosslinking is notlimited to the extent.The weight average molecular weight can be measuredby a method in conformity with ASTM D 2503, for example.The weight average molecular weight also can bemeasured by gel permeation chromatography (GPC) usingappropriate standards (e.g., polymethyl methacrylatestandards). Examples of a column used for measuring theweight average molecular weight include TSKgel SuperAWM-H.

[0023] The resin has a glass transition temperature ofpreferably 0°C or higher, more preferably 20°C or higher,still more preferably 40°C or higher, and preferably 300°¢or lower, more preferably 250°C or lower, still morepreferably 200°C or lower.The glass transition temperature can be measured inconformity with JIS K 7121, for example.

[0024] The amount of the resin in the fiber layer ispreferably 10% by mass or greater, more preferably 20% bymass or greater and is preferably 80% by mass or less, morepreferably 70% by mass or less.

[0025] The fiber layer includes a fiber.Examples of the fiber include reinforcing fibers suchas carbon fibers, metal fibers, organic fibers, andinorganic fibers.Examples of the carbon fibers include PAN carbonfibers, pitch carbon fibers, cellulose carbon fibers, andvapor-grown carbon fibers.Examples of the metal fibers include fibers made ofmetals such as iron, gold, silver, copper, aluminum, brass,and stainless steel.Examples of the organic fibers include fibers made oforganic materials such as aramids, polybenzoxazole (PBO),polyphenylene sulfide, polyesters, polyamides, andpolyethylene.Examples of the inorganic fibers include fibers madeof inorganic materials such as glass, basalt, siliconcarbide, and silicon nitride. Examples of the glass fibersinclude E glass, C glass, S glass, and T glass.In particular, carbon fibers and inorganic fibers arepreferred. Carbon fibers and glass fibers are morepreferred.

[0026] The fiber has an average fiber size of preferably 2pm or greater, more preferably 3 pm or greater, andpreferably 30 pm or less, more preferably 26 um or less.The average fiber size can be calculated from theaverage of the fiber sizes at 10 random points in an imagecaptured with a scanning electron microscope (SEM), forexample.

[0027] The fiber may be a discontinuous fiber that isintermittently divided, or may be a continuous fiber thatis not divided.When the fiber is discontinuous fiber, the fiber hasan average fiber length of preferably 2 mm or greater, morepreferably 4 mm or greater, and preferably 100 mm or less,more preferably 80 mm or less.The average fiber length can be calculated from theaverage of the fiber lengths of 20 random samples eachmeasured with a caliper, for example.

[0028] The fiber has a specific gravity of preferably 1.5 orgreater, more preferably 1.7 or greater, still morepreferably 2.0 or greater, and preferably 3.0 or less, morepreferably 2.7 or less, still more preferably 2.6 or less.The specific gravity can be measured with anelectronic densimeter, for example.

[0029] The fiber may be in any form. Examples thereofinclude a fiber form and a form of a sheet of woven fabric,knitted fabric, or non-woven fabric.When the fiber is in a sheet form, the fiber has aweight per unit area of preferably 100 g / m2 or greater,more preferably 350 g / m2 or greater, and preferably 1,000g / m2 or less, more preferably 650 g / m2 or less.The weight per unit area can be measured by, forexample, cutting the sheet-form fiber to a size of 10 cm x10 cm, measuring the weight of the cut sheet-form fiber,and calculating the weight per unit area.

[0030] The amount of the fiber in the fiber layer ispreferably 10% by mass or greater, more preferably 20% bymass or greater and is preferably 80% by mass or less, morepreferably 70% by mass or less.When the amount of the fiber is within the range, thefiber can sufficiently increase the mechanical strength ofthe laminate.

[0031] The fiber layer may optionally include, in additionto the resin and the fiber, additives such as thermalstabilizers, lubricants, inorganic fillers, pigments, flameretardants, antioxidants, processing aids, ultravioletabsorbers, and light stabilizers.

[0032] The thickness of the fiber layer is preferably 0.2 mmor greater, more preferably 0.4 mm or greater and ispreferably 10 mm or less, more preferably 7 mm or less.When the laminate of the present invention includestwo or more fiber layers, the "thickness of the fiberlayer" means the total thickness of the fiber layers.

[0033] The proportion, by mass, of the fiber layer in thelaminate of the present invention is preferably 1 / 10 orgreater, more preferably 2 / 10 or greater and is preferably9 / 10 or less, more preferably 8 / 10 or less.

[0034] The proportion of the thickness of the fiber layer inthe thickness of the laminate of the present invention ispreferably 1 / 10 or greater, more preferably 2 / 10 or greaterand is preferably 9 / 10 or less, more preferably 8 / 10 orless.

[0035] The laminate of the present invention includes athermal insulation layer on at least one surface of thefiber layer.The presence of the thermal insulation layer enablesthe laminate to impede the transmission of flame and heatgenerated inside a battery to the outside when the laminateis used as a cover for an in-vehicle battery.

[0036] The thermal insulation layer preferably includes aresin.Examples of the resin include the same resin as theresin constituting the fiber layer.In particular, a chlorinated polyvinyl chloride resinis preferred.

[0037] The amount of the resin in the thermal insulationlayer is preferably 50% by mass or greater, more preferably70% by mass or greater and is preferably 99% by mass orless, more preferably 97% by mass or less.

[0038] The thermal insulation layer may include an inorganicfiller.Examples of the inorganic filler include silica,diatomite, alumina, zinc oxide, titanium oxide, calciumoxide, magnesium oxide, iron oxide, tin oxide, antimonyoxide, ferrites, calcium hydroxide, magnesium hydroxide,aluminum hydroxide, basic magnesium carbonate, calciumcarbonate, magnesium carbonate, zinc carbonate, bariumcarbonate, dawsonite, hydrotalcite, calcium sulfate, bariumsulfate, gypsum fiber, calcium silicate, talc, clay, mica,montmorillonite, bentonite, activated clay, sepiolite,imogolite, sericite, glass beads, silica balloons, aluminumnitride, boron nitride, silicon nitride, carbon black,graphite, carbon balloons, charcoal powder, various metalpowders, potassium titanate, magnesium sulfate, leadzirconium titanate, aluminum borate, molybdenum sulfide,silicon carbide, stainless steel fibers, zinc borate,various magnetic powders, fly ash, and dewatered sludge.

[0039] The amount of the inorganic filler in the thermalinsulation layer is preferably 0.1% by mass or greater,more preferably 1% by mass or greater and is preferably 50%by mass or less, more preferably 30% by mass or less.

[0040] The thermal insulation layer may further includeadditives such as thermal stabilizers, lubricants, andfoaming agents.The foaming agents are not limited and may bechemical foaming agents or physical foaming agents.Examples of the chemical foaming agents includethermally decomposable inorganic foaming agents, thermallydecomposable organic foaming agents, inorganic reactivefoaming agents based on sodium bicarbonate and acid, andorganic reactive foaming agents based on isocyanate andwater.Examples of the thermally decomposable inorganicfoaming agents include thermally expandable graphite, acidammonium, sodium carbonate, ammonium hydrogen carbonate,sodium hydrogen carbonate, ammonium nitrite, sodiumborohydride, and monosodium citrate anhydrous.Examples of the thermally decomposable organicfoaming agents include: azo compounds such asazodicarbonamide, azodicarboxylic acid metal salts {(e.g.,barium azodicarboxylate), and azobisiscbutyronitrile;nitroso compounds such as N,N'-dinitrosopentamethylenetetramine; hydrazine derivativessuch as hydrazodicarbonamide, 4,4'-oxybis(benzenesulfonylhydrazide), and toluenesulfonylhydrazide;and semicarbazide compounds such astoluenesul fonylsemicarbazide.Examples of physical foaming agents include:vermiculite; and thermally expandable particles havinghydrocarbon encapsulated therein.

[0041] The thermal insulation layer has a thickness beforeheating of preferably 0.2 mm or greater, more preferably0.3 mm or greater, and preferably 10 mm or less, morepreferably 7 mm or less.

[0042] The proportion, by mass, of the thermal insulationlayer in the laminate of the present invention ispreferably 1 / 10 or greater, more preferably 2 / 10 or greaterand is preferably 9 / 10 or less, more preferably 8 / 10 orless.

[0043] The proportion of the thickness of the thermalinsulation layer in the thickness of the laminate of thepresent invention is preferably 1 / 10 or greater, morepreferably 2 / 10 or greater and is preferably 9 / 10 or less,more preferably 8 / 10 or less.

[0044] The proportion of the thickness of the thermalinsulation layer to the thickness of the fiber layer(thickness of thermal insulation layer / thickness of fiberlayer) is preferably 1 / 10 or greater, more preferably 2 / 10or greater and is preferably 9 / 10 or less, more preferably8 / 10 or less.

[0045] The laminate of the present invention may furtherinclude, on a surface of the thermal insulation layeropposite to the surface facing the fiber layer, a fiberlayer including a resin and a fiber.In other words, the laminate of the present inventionmay have a laminated structure of fiber layer (A) / thermalinsulation layer (B) / fiber layer (C), where the fiber layer(a) is the fiber layer having the thermal insulation layeron at least one surface thereof, and the fiber layer (C) isthe fiber layer formed on a surface of the thermalinsulation layer opposite to the surface facing the fiberlayer (A).The structure of the fiber layer may be the same asthat of the fiber layer described above.

[0046] When the laminate of the present invention includesthe fiber layer (A) and the fiber layer (C), the ratio ofthe thickness of the fiber layer (A) to the thickness ofthe fiber layer (C) (thickness of fiber layer (A) / thicknessof fiber layer (C)) is preferably 10 / 1 or greater, morepreferably 10 / 2 or greater and is preferably 10 / 10 or less,more preferably 10 / 9 or less.

[0047] When the laminate of the present invention includesthe fiber layer (A) and the fiber layer (C), the ratio ofthe mass of the fiber layer (A) to the mass of the fiberlayer (C) (mass of fiber layer (A) / mass of fiber layer (C})is preferably 10 / 1 or greater, more preferably 10 / 2 orgreater and is preferably 10 / 10 or less, more preferably10 / 9 or less.

[0048] The laminate of the present invention may have anyshape. Examples thereof include a film shape, a plateshape, a sheet shape, a cylindrical shape, a ring shape, aframe shape, and a box shape.

[0049] The laminate of the present invention preferably hasa thermal conductivity before heating of 0.05 W / mK orgreater, more preferably 0.1 W / mK or greater, andpreferably 0.5 W / mK or less, more preferably 0.4 W / mK orless.The thermal conductivity can be measured inconformity with JIS R 2616, for example.

[0050] The laminate of the present invention preferably hasa thermal conductivity after heating at 800°C for oneminute of 0.01 W / mK or greater, more preferably 0.05 W / mKor greater, and preferably 0.15 W / mK or less, morepreferably 0.12 W / mK or less.When the thermal conductivity is within the range,the laminate can sufficiently reduce the transmission offlame and heat generated by ignition inside a battery tothe outside when used as a cover for an in-vehicle battery.

[0051] In the laminate of the present invention, the rate ofchange of thermal conductivity after heating at 800°C forone minute, represented by the following formula (1), ispreferably 0.5 or greater and 50 or less.(Rate of change of thermal conductivity) = [(Thermalconductivity before heating) - (Thermal conductivity afterheating) 1 / (Thermal conductivity after heating) (1)The rate of change within the range is advantageousin that the heat-shielding performance can be increasedwithout greatly increasing the thickness of the laminatebefore heating.The rate of change is more preferably 1 or greaterand is more preferably 30 or less, still more preferably 10or less.

[0052] In the laminate of the present invention, the rate ofdecrease in thermal conductivity after heating at 800°C forone minute, represented by the following formula (2), ispreferably 50% or greater, more preferably 55% or greaterand is preferably 95% or less, more preferably 90% or less.(Rate of decrease in thermal conductivity) = [(Thermalconductivity before heating) - (Thermal conductivity afterheating) ] / (Thermal conductivity before heating) x 100 (2)

[0053] In the laminate, the rate of volume expansion,represented by the following formula (3), after heating at800°C for one minute is preferably 2 times or greater.(Rate of volume expansion) = [(Maximum thickness afterheating) - (Thickness before heating)] / (Thickness beforeheating) (3)The rate of volume expansion of two times or greateris advantageous in that the heat-shielding performance canbe increased without greatly increasing the thickness ofthe laminate before heating.The rate of volume expansion is more preferably 2.2times or greater and is preferably 10 times or less, morepreferably 7 time or less.

[0054] The laminate of the present invention may be producedby, for example, preparing a composition containingmaterials to constitute the fiber layer such as the resinand the fiber and a composition containing materials toconstitute the thermal insulation layer such as the resin,and forming the fiber layer and the thermal insulationlayer. If necessary, the layers may be formed such thatthey form the structure of fiber layer (A) / thermalinsulation layer (B) / fiber layer (C).The fiber layer and the thermal insulation layer maybe formed by a method such as an extrusion molding methodor an injection molding method, for example,

[0055] The laminate of the present invention, havingexcellent flame-shielding performance and heat-shieldingperformance, can be suitably used as any of various moldedmembers such as a member of transportation machinery or amember of battery systems. Moreover, the laminate of thepresent invention can be suitably used as a member ofbattery systems used in transportation machinery.

[0056] Examples of the transportation machinery includeautomobiles such as gasoline-powered vehicles, hybridvehicles, electric vehicles, and fuel cell vehicles;motorcycles such as gasoline-powered motorcycles, hybridmotorcycles, and electric motorcycles; bicycles such aspower assisted bicycles; railway vehicles; vessels; andaircraft.Examples of the member of transportation machineryinclude mechanism members, interior members, exteriormembers, windowpanes, and light covers.Examples of the mechanism members include coolingpipes, air bag covers, air ducts, heater units, and coversfor in-vehicle batteries.Examples of the interior members include ceiling,instrument panels, console boxes, arm rests, seat beltbuckles, switches, and door trims.Examples of the exterior members include emblems,number plate housings, bumper cores, and under covers.

[0057] Examples of the battery systems include primarybatteries such as nickel manganese batteries, lithiumbatteries, and zinc-air batteries; secondary batteries suchas nickel hydrogen batteries, lithium-ion batteries, andlead storage batteries; solar cells such as silicon solarcells, dye-sensitized solar cells, and perovskite solarcells; and fuel cells such as solid polymer fuel cells,alkali fuel cells, phosphoric acid fuel cells, and solidoxide fuel cells.Examples of the member of battery systems includebattery covers, battery cooling water jackets, hydrogentank covers, connectors, and insulation sheets.Examples of the member of battery systems used intransportation machinery include covers for batteries fortransportation machinery and covers for in-vehiclebatteries.The laminate of the present invention can beparticularly suitably used as a cover for a lithium-ionbattery. Moreover, the laminate can be suitably used as acover for an in-vehicle battery because the laminate canreduce the transmission of flame and heat generated byignition inside a battery to the outside if the batteryundergoes thermal runaway.The laminate of the present invention is particularlypreferably used as a cover for a lithium-ion battery.- Advantageous Effects of Invention

[0058] The present invention can provide a laminate that hasexcellent flame-shielding performance and heat-shieldingperformance and can reduce the transmission of flame andheat generated by ignition inside a battery to the outside,especially when used as a cover for an in-vehicle battery.BRIEF DESCRIPTION OF DRAWINGS

[0059] FIG. 1 is a perspective view of a mold for molding abattery cover.FIG. 2 is a cross-sectional view illustrating moldingof a battery cover.FIG. 3 is a perspective view of a drawn sample usedfor measuring bending strength after drawing.FIG. 4 is a perspective view of a bending test samplecut out of the drawn sample.DESCRIPTION OF EMBODIMENTS

[0060] The present invention is hereinafter described inmore detail with reference to examples. The presentinvention should not be limited to these examples.

[0061] The following materials were used in the examples andthe comparative examples.

[0062] (Example 1)(Preparation of fiber layers (A) and (C)}One hundred parts by mass of a chlorinated polyvinylchloride resin (CPVC, produced by Tokuyama Sekisui Co.,Ltd., average degree of polymerization 1,000, chlorinecontent 72.0% by mass) and 10 parts by mass of a thermalstabilizer (produced by Nitto Kasei Co., Ltd., organotinthermal stabilizer "TVS#1380") were mixed with 400 parts bymass of tetrahydrofuran (THF, produced by FUJIFILM WakoPure Chemical Corporation) to prepare a resin solution.The chlorine content of the resin was measured by amethod in conformity with JIS K 7229. The average degreeof polymerization of the resin was measured by a method inconformity with JIS K 6720-2:1999.Subsequently, a sheet-form glass fiber ("MC450A"produced by Nitto Boseki Co., Ltd., average fiber size 7um, average fiber length 50 nm, specific gravity 2.6,weight per unit area 450 g / m2) was impregnated with theresin solution by a hand lay-up method. The process wasrepeated seven times to stack seven glass fiber layers.Then, the THF was evaporated by drying with a drier,whereby fiber layers (&) and (C) were obtained. Thethickness of the obtained fiber layers (A) and (C) was 1.7mm. The (fiber mass / resin mass) was 1.13. The averagefiber size of the glass fiber was calculated from theaverage of the fiber sizes at randomly selected 10 pointsin an image captured with a scanning electron microscope(SEM). The average fiber length was calculated from theaverage of the fiber lengths of randomly selected 20samples each measured with a caliper. The specific gravitywas calculated with an electronic densimeter (produced byAlfa Mirage, "ED120T"). The weight per unit area of theglass fiber was determined by cutting the sheet-form glassfiber to a size of 10 cm x 10 cm, measuring the weight ofthe cut sheet-form glass fiber, and calculating the weight(g) per m2.

[0063] (Preparation of thermal insulation layer (B))One hundred parts by mass of a chlorinated polyvinylchloride resin (produced by CPVC, Tokuyama Sekisui Co.,Ltd., average degree of polymerization 500, chlorinecontent 67.3% by mass), 10 parts by mass of a thermalstabilizer (produced by Nitto Kasei Co., Ltd., organotinthermal stabilizer "TVS#1380"), 2 parts by mass of alubricant ("WAX-OP" produced by Clariant), and 1 part bymass of an inorganic filler (carbon black, "BLACKPEARLS L"produced by Cabot Corporation) were mixed and roll-kneadedto prepare a thermal insulation layer (B) having athickness of 0.3 mm.

[0064] (Preparation of laminate)The fiber layer {A), the thermal insulation layer(B), and the fiber layer (C) were stacked (fiber layer (A)-thermal insulation layer (B)-fiber layer (C)) and pressedwith a press machine, whereby a laminate was obtained.

[0065] (Example 2)A laminate was obtained as in Example 1 except thatin (Preparation of fiber layers (A} and (C)), the (fibermass / resin mass) was 1.13, and that in (Preparation ofthermal insulation layer (B)), 10 parts by mass of titaniumoxide ("TIPAQUE CR-90" produced by Ishihara Sangyo Kaisha,Ltd.) was used instead of 1 part by mass of carbon black.

[0066] (Example 3)In (Preparation of fiber layers (A) and (C)), a glassfiber-reinforced thermoplastic prepreg containing apolyamide resin ("Tepexdynalite 102-FG290 (x) / 45%" producedby LANXESS) was used to prepare fiber layers (A) and (C)having a thickness of 1.7 mm. The (fiber mass / resin mass)was 1.12.A laminate was obtained as in Example 2 except thatthe obtained fiber layers (A) and (C) were used.

[0067] (Example 4)In (Preparation of fiber layers (A) and (C)), a glassfiber-reinforced thermoplastic prepreg containing apolycarbonate resin ("Tepexdynalite 102fr-FG290(x) / 45%"produced by LANXESS) was used to prepare fiber layers (A)and (C) having a thickness of 1.7 mm. The (fibermass / resin mass) was 1.13.A laminate was obtained as in Example 2 except thatthe obtained fiber layers (A) and (C) were used.

[0068] (Example 5)A laminate was obtained as in Example 2 except thatin (Preparation of fiber layers (A) and (C)), a polyvinylchloride resin (PVC, produced by Tokuyama Sekisui Co.,Ltd., average degree of polymerization 1,000, chlorinecontent 56.7% by mass) was used as the resin, and that the(fiber mass / resin mass) was 1.54.

[0069] (Example 6)A laminate was obtained as in Example Z except thatin (Preparation of fiber layers (A) and (C)), a chlorinatedpolyvinyl chloride resin (CPVC, produced by TokuyamaSekisui Co., Ltd., average degree of polymerization 500,chlorine content 67.3% by mass) was used as the resin, andthat the (fiber mass / resin mass) was 1.54.

[0070] (Example 7)A laminate was obtained as in Example 6 except thatin (Preparation of fiber layers (A) and (C)), a sheet-formcarbon fiber ("T-700" produced by Toray Industries Inc.,average fiber size 10 pm, specific gravity 2.1, weight perunit area 220 g / m2) as the fiber, and that the (fibermass / resin mass) was 1.09.

[0071] (Example 8)A laminate was obtained as in Example 6 except thatin (Preparation of thermal insulation layer (B))}, apolyvinyl chloride resin (PVC, produced by Tokuyama SekisuiCo., Ltd., average degree of polymerization 500, chlorinecontent 56.7% by mass) was used as the resin,

[0072] (Example 9)A laminate was obtained as in Example 6 except thatin (Preparation of thermal insulation layer (B)), apolycarbonate resin (produced by Mitsubishi Gas ChemicalCompany, Inc., PCZ-500) was used as the resin, and that thethermal insulation layer (B) was produced without theaddition of the thermal stabilizer and the lubricant.

[0073] (Example 10)A laminate was obtained as in Example 6 except thatin (Preparation of thermal insulation layer (B)), apolyamide resin (produced by Unitika Ltd., Al030BRT) wasused as the resin, and that the thermal insulation layer(B) was produced without the addition of the thermalstabilizer and the lubricant.

[00741] (Example 11)A laminate was obtained as in Example 6 except thatin (Preparation of thermal insulation layer (B)),expandable graphite ("EXP-508300" produced by FujikokuenCo., Ltd.) was used instead of titanium oxide.

[0075] (Example 12}A laminate was obtained as in Example 6 except thatin (Preparation of fiber layers (A) and (C)), a sheet-formglass fiber ("MC 380A" produced by Nitto Boseki Co., Ltd.,average fiber size 7 pm, average fiber length 50 nm,specific gravity 2.6, weight per unit area 380 g / m2) wasused as the fiber, and that the (fiber mass / resin mass) was1.35.

[0076] (Example 13)A laminate was obtained as in Example 6 except thatin (Preparation of fiber layers (A) and (C)), a sheet-formglass fiber ("MC 600A" produced by Nitto Boseki Co., Ltd.,average fiber size 7 um, average fiber length 30 nm,specific gravity 2.6, weight per unit area 600 g / m2) wasused as the fiber, and that the (fiber mass / resin mass) was2.10.

[0077] (Example 14)A laminate was obtained as in Example 3 except thatin (Preparation of thermal insulation layer (B)), apolyamide resin (produced by Unitika Ltd., Al030BRT) wasused as the resin, and that the thermal insulation layer(B) was produced without the addition of the thermalstabilizer and the lubricant.

[0078] (Example 15)A laminate was obtained as in Example 4 except thatin (Preparation of thermal insulation layer (B)), apolycarbonate resin (produced by Mitsubishi Gas ChemicalCompany, Inc., PCZ-500) was used as the resin, and that thethermal insulation layer (B) was produced without theaddition of the thermal stabilizer and the lubricant.

[0079] (Comparative Example 1)One hundred parts by mass of a chlorinated polyvinylchloride resin (CPVC, produced by Tokuyama Sekisui Co.,Ltd., average degree of polymerization 1,000, chlorinecontent 72.0% by mass), 10 parts by mass of a thermalstabilizer (produced by Nitto Kasei Co., Ltd., "TVS#1380"},and 2 parts by mass of a lubricant ("WAX-OP" produced byClariant) were mixed and roll-kneaded to prepare resinlayers each having a thickness of 0.3 mm.The obtained resin layers were stacked and press-molded, whereby a laminate having a thickness of 2.0 mm wasobtained.

[0080] (Comparative Example 2)One hundred parts by mass of a chlorinated polyvinylchloride resin (CPVC, produced by Tokuyama Sekisui Co.,Ltd., average degree of polymerization 1,000, chlorinecontent 72.0% by mass) and 10 parts by mass of a thermalstabilizer (produced by Nitto Kasei Co., Ltd., organotinthermal stabilizer ""TVS#1380") were mixed with 400 parts bymass of tetrahydrofuran (THF, produced by FUJIFILM WakoPure Chemical Corporation) to prepare a resin solution.Subsequently, a sheet-form glass fiber ("MC430A-1048s" produced by Nitto Boseki Co., Ltd., average fibersize 7 pm, weight per unit area 450 g / m2) was impregnatedwith the resin solution by a hand lay-up method. Theprocess was repeated to stack glass fiber layers. Then theTHF was evaporated by drying with a drier, whereby alaminate having a thickness of 2.0 mm was obtained. The(fiber mass / resin mass) was 0.98.

[00811] (Comparative Example 3)A glass fiber-reinforced thermoplastic prepregcontaining a polyamide resin ("Tepexdynalite 102-FG290 (x) / 45%" produced by LANXESS) was used to prepare afiber layer having a thickness of 2.5 mm. The (fibermass / resin mass) was 1.12.

[0082] (Comparative Example 4)A glass fiber-reinforced thermoplastic prepregcontaining a polycarbonate resin ("Tepexdynalite 102fr-FG290 (x) / 45%" produced by LANXESS) was used to prepare afiber layer having a thickness of 2.0 mm. The (fibermass / resin mass) was 1.13.

[0083] (Evaluation)The resins, laminates, and resin layers used in theexamples and the comparative examples were evaluated asfollows. Tables 1 to 4 show the results.

[0084] (1) Oxygen index, weight average molecular weight, andglass transition temperature (Tg) of resinThe oxygen index of the resins was measured by amethod in conformity with JIS X 7201-2:2007. The weightaverage molecular weight of the resins was measured by amethod in conformity with ASTM D 2503. The glasstransition temperature (Tg) of the resins was measured by amethod in conformity with the JIS K 7121.

[0085] The weight average molecular weight of thechlorinated polyvinyl chloride resins, polyvinyl chlorides,and polycarbonate resins was specifically measured by thefollowing method.First, a resin sample was dissolved in THF andfiltrated through a filter having a pore size of 0.2 um.Measurement was then performed using a GPC unit (pump unit:PU-4180, detector unit: RI-4030, column oven: CO-4065)produced by JASCO Corporation at a flow rate of 0.7 ml / minand an oven temperature of 40°C, whereby the sample waseluted and separated. The molecular weight was determinedbased on a calibration curve produced using standardpolystyrene. The columns used were SHODEX columns LF-804(two columns connected).

[0086] The weight average molecular weight of the polyamideresins was measured by the following method.Specifically, first, a laminate sample was weighed.A predetermined amount of eluent was added, and the samplewas allowed to stand at room temperature overnight fordissolution. Subsequently, the obtained solution wasshaken gently and then filtered through a 0.45pm PTFEcartridge filter to separate the polyamide resin as thefiltrate.Measurement was then performed under the followingconditions.<GPC device>HLC-8420GPC (produced by Tosoh Corporation)<Column>TSKgel SuperBWM-H (6.0 mm I.D. x 15 cm) x 2 (produced byTosoh Corporation)<Detector>Differential refractometer (RI detector), polarity = (+)<Eluent>HFIP (1,1,1,3,3,3-hexafluoro-2-propanol) (produced byFUJIFILM Wako Pure Chemical Corporation)+ 10 mM-CF3CO0Na (produced by FUJIFILM Wako Pure ChemicalCorporation, 1st grade)<Measurement conditions>Flow rate: 0.3 ml / minColumn temperature: 40°CSample concentration: 1 mg / ml (polyamide-basedconcentration)Sample injection volume: 20 μlCalibration curve: cubic approximation curve produced usingstandard. PMMA - (produced by Agilent Technologies, Inc.)

[0087] (2) Thermal conductivity and rate of volume expansionThe laminates obtained in Examples 1 to 15 andComparative Examples 1 and 2 and the fiber layers obtainedin Comparative Examples 3 and 4 were each cut into ameasurement sample having a size of 100 mm x 100 mm. Thethermal conductivity of the measurement sample was measuredin conformity with JIS R 2616.Further, the obtained measurement sample was fixed toa fixture such that the thickness direction corresponded tothe vertical direction. The sample was heated from belowwith the distance between the sample and a burner being 20mm. The heating was continued at 800°C for one minute, andthen the thermal conductivity was measured in the samemanner as above. The rate of change of thermalconductivity and the rate of decrease in thermalconductivity were calculated by the following formulas (1)and (2).(Rate of change of thermal conductivity) = [ (Thermalconductivity before heating) - (Thermal conductivity afterheating) 1 / (Thermal conductivity after heating) (1)(Rate of decrease in thermal conductivity) = [ (Thermalconductivity before heating) - (Thermal conductivity afterheating) ] / (Thermal conductivity before heating} x 100 (2)The thickness of the measurement sample after heatingat 800°C for one minute was measured, and the rate ofvolume expansion was measured by the following formula (3).(Rate of volume expansion) = [ (Maximum thickness afterheating) - (Thickness before heating) l / (Thickness beforeheating) (3)For the laminate obtained in Comparative Example 1,the thermal conductivity after heating, the rate of changeof thermal conductivity, the rate of decrease in thermalconductivity, and the rate of volume expansion were unableto be measured because the resin was burned off before800°C was reached.

[0088] (3) Flame escape and back surface temperatureThe laminates obtained in Examples 1 to 15 andComparative Example 1 and 2 and the fiber layers obtainedin Comparative Examples 3 and 4 were each cut into ameasurement sample having a size of 150 mm x 150 mm. Theobtained measurement sample was fixed to a fixture suchthat the thickness direction corresponded to the verticaldirection. The sample was heated for five minutes frombelow with the distance between the sample and a burnerbeing 20 mm. The state during heating was observed andevaluated in accordance with the following criteria.o (Good): No flame escape above the measurement sample wasobserved.x (Poor): A flame escape above the measurement sample wasobserved.The temperature of the back surface opposite to theheated surface was monitored with a thermography, and thetime required for the back surface temperature to reach300°C was measured.

[0089] (4) Appearance of battery cover(Preparation of cover for lithium-ion battery)The laminates obtained in Examples 1 to 15 were eachpress-molded as shown in FIG. 2 (temperature 200°C,preheating for four minutes, compression for four minutes,cooling for four minutes) using molds shown in FIG. 1 toprepare a molded article simulating a cover for a lithium-ion battery. The obtained molded articles had goodappearance free of cracks or fractures.

[0090] (3) Bending strength after drawingThe laminates obtained in Examples 1 to 15 andComparative Examples 1 and 2 and the fiber layers obtainedin Comparative Example 3 and 4 were each heated with aninfrared heater to a surface temperature of 210°C (230°Cfor a resin including a polycarbonate resin, 240°C for aresin including a polyamide resin).The laminate after heating was placed in a press moldat a mold temperature of 170°C. The laminate was pressedat a clamping force of 30 t and held for 10 seconds. Themold was then cooled to 50°C over 20 minutes, whereby adrawn sample as shown in FIG. 3 was obtained.From a flat portion (portion indicated by dashedlines in FIG. 3) of the drawn sample, a bending test sample(65 mm x 10 mm) was cut out as shown in FIG. 4 using acomposite material cutter AC-300CF (produced by MarutoTesting Machine Company).The bending strength wasmeasured using "TENSILON" produced by Orientec Corporationin conformity with JIS K7171.

[0091] [Table 1]

[0092] [Table 2}

[0093] [Table 3]

[0094] [Table 4]INDUSTRIAL APPLICABILITY

[0095] The present invention can provide a laminate that hasexcellent flame-shielding performance and heat-shieldingperformance and can reduce the transmission of flame andheat generated by ignition inside a battery to the outside,especially when used as a cover for an in-vehicle battery.REFERENCE SIGNS LIST

[0096] 1 mold2 laminate

Claims

1. A laminate comprising: a fiber layer including a resin and a fiber; and a thermal insulation layer formed on at least one surface of the fiber layer.

2. The laminate according to claim 1, having a thermal conductivity after heating at 800°C for one minute of 0.01 to 0.15 W / mK.

3. The laminate according to claim 1 or 2, wherein a rate of change of thermal conductivity after heating at 800°C for one minute, represented by the following formula (1), is 1 to 10: (Rate of change of thermal conductivity) = [ (Thermal conductivity before heating) - (Thermal conductivity after heating) 1 / (Thermal conductivity after heating) (1).

4. The laminate according to any one of claims 1 to 3, wherein a rate of volume expansion, represented by the following formula {3), after heating at 800°C for one minute is 2 times or greater: (Rate of volume expansion) = [ (Maximum thickness after heating) - (Thickness before heating)] / (Thickness before heating} (3).

5. The laminate according to any one of claims 1 to 4, further comprising, on a surface of the thermal insulation layer opposite to the surface facing the fiber layer, a fiber layer including a resin and a fiber.

6. The laminate according to any one of claims 1 to 5, wherein the resin constituting the fiber layer has an oxygen index of 20 or greater.

7. The laminate according to any one of claims 1 to 6, wherein the resin constituting the fiber layer is a chlorinated polyvinyl chloride resin having an average degree of polymerization of 400 to 3,000 and a chlorine content of 57 to 72% by mass.

8. The laminate according to any one of claims 1to7, wherein the fiber constituting the fiber layer is at least one selected from the group consisting of a glass fiber and a carbon fiber.

9. The laminate according to any one of claims 1 to 8, wherein an amount. of the fiber in the fiber layer is 10 to 80% by mass.

10. The laminate according to any one of claims 1 to 9, which. is a cover for a lithium-ion battery.

11. A method for using the laminate according to any one of claims 1 to 9 as a cover for a lithium-ion battery. .