High-nickel electrode sheet having reduced reactivity with moisture and manufacturing method therefor
Patent Information
- Application Number
- IN202217004618
- Authority / Receiving Office
- IN · IN
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-07
- Filing Date
- 2022-01-27
- Publication Date
- 2026-10-07
- Estimated Expiration
- 2041-04-26
AI Technical Summary
High-nickel content positive electrode active materials in lithium secondary batteries are prone to moisture reaction, leading to reduced thermal stability and capacity, and existing solutions fail to adequately inhibit moisture reaction while maintaining high energy density.
An electrode sheet design with a first positive electrode mixture layer in the central portion and a second positive electrode mixture layer with higher particle strength at the edges, containing lithium nickel oxide, to minimize moisture reactivity and enhance energy density.
The electrode sheet effectively reduces moisture-induced reactivity and improves battery lifespan and capacity retention by using a second positive electrode mixture layer with increased particle strength at the edges, where moisture penetration is higher.
Smart Images

Figure 00000043_0000
Abstract
Description
Title of Invention: High-nickel electrode sheet with reduced reactivity with moisture and manufacturing method thereoftechnical field[One]This application claims the benefit of priority based on Korean Patent Application No. 10-2020-0054235 on May 7, 2020 and Korean Patent Application No. 10-2021-0049862 on April 16, 2021. All disclosures are incorporated herein by reference.[2]The present invention relates to a positive electrode comprising a positive electrode active material having a high nickel content, a positive electrode sheet, and a method for manufacturing the same. The present invention relates to an electrode sheet in which reactivity with moisture is suppressed by applying a slurry for a second positive electrode mixture containing a positive electrode active material having strong particle strength, and a method for manufacturing the same.background[3]In a lithium secondary battery, an organic electrolyte or a polymer electrolyte is charged between a positive electrode and a negative electrode made of an active material capable of intercalation and deintercalation of lithium ions, and lithium ions are intercalated / deintercalated from the positive electrode and the negative electrode. Electric energy is produced by a reduction reaction with[4]As a positive active material of a lithium secondary battery, lithium cobalt oxide (LiCoO 2), lithium nickel oxide (LiNiO 2), lithium manganese oxide (LiMnO 2 or LiMn 2O 4, etc.), lithium iron phosphate compound (LiFePO 4), etc. were used. In addition, as a method for improving low thermal stability while maintaining the excellent reversible capacity of LiNiO 2 , a lithium composite metal oxide in which a part of nickel (Ni) is substituted with cobalt (Co) and manganese (Mn) (hereinafter simply referred to as ‘NCM-based Lithium composite transition metal oxide') was developed. However, the conventionally developed NCM-based lithium composite transition metal oxide has insufficient capacity characteristics, so there is a limit to its application.[5]In order to improve this problem, recently, research to increase the content of nickel in the NCM-based lithium composite transition metal oxide is being made. As the content of nickel increases, the energy density per volume increases, but in the case of a high-concentration nickel positive electrode active material, there is a problem in that the structural stability and chemical stability of the active material are deteriorated, so that thermal stability is rapidly reduced. In addition, nickel ions are irreversibly converted to NiO by reacting with moisture and carbon dioxide present in the storage environment, and as lithium ions escape in this process, lithium by-products present in the form of LiOH and Li 2CO 3 increase, Due to this, there are problems in increasing the resistance of the active material surface, reducing the capacity of the battery, and increasing gas generation during high temperature storage.[6]In general, after applying the slurry for electrode mixture containing the electrode active material on the current collector sheet, the dried and rolled electrode sheet is wound around the core until the electrode is punched for assembling the battery in a wound state. are kept 1 shows the electrode sheet 10 in a wound state for storage. At this time, based on the width direction (arrow) of the electrode sheet, the moisture permeation is easier at both ends (A) than the central part (B) of the holding part, and the moisture content is high by that amount. Therefore, in the case of the positive electrode sheet including the positive electrode active material of the NCM-based lithium composite transition metal oxide, there is a high probability that nickel and moisture react at both end portions compared to the central portion.[7]Accordingly, in order to alleviate moisture content during the manufacture of a high-nickel positive electrode active material electrode having a high nickel content, Japanese Patent Application Laid-Open No. 2019-149269 discloses a first positive electrode active material having a nickel content of 50% to 80% in the central portion. A secondary battery including a positive electrode to which a second positive electrode active material having a nickel content of 20% to 40% is applied to both ends thereof. However, the conventional technique has an effect of suppressing the precipitation of lithium, but is not sufficient to improve the life performance of the battery, and the second positive active material applied to both ends contains only 20% to 40% of nickel, There have been difficulties in realizing the desired energy density.[8]Therefore, in a positive electrode having a high nickel content, it is necessary to develop a technology for a battery capable of realizing a high energy density and suppressing a reaction with moisture.DETAILED DESCRIPTION OF THE INVENTIONtechnical challenge[9]The present invention was devised to solve the above problems, and specifically, in an electrode sheet wound in a roll, the positive electrode active material having a high nickel content alleviates the reaction with moisture, and an electrode capable of realizing a high energy density An object of the present invention is to provide a sheet and a method for manufacturing the same.means of solving the problem
[10] The electrode sheet of the present invention for solving the above problems is an electrode sheet comprising a holding portion and an uncoated portion coated with a positive electrode mixture layer on at least one surface of a current collector, wherein the holding portion is formed in a central portion along the longitudinal direction of the electrode sheet and a first positive electrode mixture layer comprising a positive electrode active material of lithium nickel oxide; and a second positive electrode mixture layer formed on one or both edges of the first positive electrode mixture layer and including a positive electrode active material of lithium nickel oxide, wherein the positive electrode active material particle strength in the second positive electrode mixture layer is, It is characterized in that it is greater than the particle strength of the positive active material in the layer.
[11] In one specific example, the width length of the second positive electrode mixture layer is 1 to 15% of the width length of the first positive electrode mixture layer.
[12] In one specific example, each of the positive electrode active materials included in the first positive electrode mixture layer and the second positive electrode mixture layer each independently includes a compound represented by Formula 1 below.
[13] [Formula 1]
[14] Li aNi 1-x-yCo xM1 yM2 wO 2
[15] (In Formula 1, 1.0≤a≤1.5, 0≤x≤0.2, 0≤y≤0.2, 0≤w≤0.1 and 0≤x+y≤0.4,
[16] M1 includes any one or both selected from the group consisting of Mn and Al, and M2 is any one or two or more elements selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb, and Mo. including)
[17] In one specific example, the ratio (B / A) of the particle strength (B) of the positive electrode active material in the second positive electrode mixture layer to the particle strength (A) of the positive electrode active material in the first positive electrode mixture layer is 1.01 to 1.5.
[18] In one specific example, the second positive electrode mixture layer may include a first positive electrode active material having a relatively large average particle size (D 50 ) and a second positive electrode having a relatively small average particle size (D 50 ). mixtures of active materials.
[19] In one specific example, the first positive active material has an average particle size (D 50 ) of 9 μm to 30 μm, and the second positive active material has an average particle size (D 50 ) of less than 9 μm.
[20] In one specific example, in the second positive electrode mixture layer, a mixing ratio of the first positive active material and the second positive active material is 95:5 to 65:35 by weight.
[21] In one specific example, the positive electrode active material of the first positive electrode mixture layer may be composed of a positive electrode active material having the same average particle size (D 50 ).
[22] In this case, the positive electrode active material of the first positive electrode mixture layer has an average particle size (D 50) of 9 μm to 30 μm.
[23] In one specific example, the first positive electrode mixture layer includes a first positive electrode active material having a relatively large average particle size (D 50 ) and a second positive electrode having a relatively small average particle size (D 50 ). It may also contain mixtures of active materials.
[24] In this case, the first positive active material may have an average particle size (D 50) of 9 μm to 30 μm, and the second positive active material may have an average particle size (D 50) of less than 9 μm.
[25] In this case, the ratio (b / a) of the weight (b) of the second positive electrode active material to the weight (a) of the first positive electrode active material in the second positive electrode material mixture layer is: It is greater than the ratio (b' / a') of the weight (b') of the second positive electrode active material to the weight (a') of
[26] The lithium secondary battery of the present invention includes a positive electrode in which the holding part and the uncoated part of the electrode sheet are punched out according to the shape and size of the unit electrode.
[27] A method of manufacturing an electrode sheet according to the present invention includes: a slurry preparation process of preparing a slurry for a first positive electrode mixture and a slurry for a second positive electrode mixture, respectively; a coating process of forming a first positive electrode mixture layer and a second positive electrode mixture layer by applying the first positive electrode mixture slurry and the second positive electrode mixture slurry on the current collector sheet; drying process; and a rolling process, wherein in the coating process, the first positive electrode mixture slurry is at the center of the electrode sheet, and the second positive electrode mixture slurry is the first positive electrode mixture slurry based on the width direction of the electrode sheet. Having a predetermined width on one or both edges, applied in the longitudinal direction of the electrode sheet, the second positive electrode mixture slurry includes a first positive electrode active material having a relatively large average particle size (D 50) and a large particle diameter, and average particles The size (D 50 ) includes a mixture of the second positive electrode active material having a relatively small particle diameter.
[28] In one specific example, the width length of the second positive electrode mixture layer in the coating process is 1 to 15% of the width length of the first positive electrode mixture layer.Effects of the Invention
[29] In the electrode sheet according to the present invention, in the second positive electrode mixture layer at both edges of the electrode sheet holding part, which is easy to be exposed to moisture and where particle crumbling can occur relatively well due to the rolled roll having a worn structure, the first By including the positive electrode active material having a greater particle strength than the positive electrode mixture layer, the reaction of the nickel component of the second positive electrode mixture layer with moisture after rolling is minimized, thereby improving the lifespan characteristics of the battery.
[30] In addition, the electrode sheet according to the present invention is applied to a high-nickel positive electrode material having a high energy density, and there is also an advantage in that the capacity characteristics of the battery are improved.Brief description of the drawing
[31] 1 is a schematic diagram of an electrode sheet in a wound state.
[32] 2 is a graph showing the moisture content in the electrode according to the electrode manufacturing step.
[33] 3 is a schematic diagram showing a rolling roller with wear on both ends as the number of uses increases; am.
[34] 4 is a schematic plan view showing an example of an electrode sheet according to an embodiment of the present invention.
[35] 5 is a graph showing the results of measuring the capacity retention rate according to the charge / discharge cycle for the batteries of Examples and Comparative Examples of the present invention.Best mode for carrying out the invention
[36] Hereinafter, the present invention will be described in detail. Prior to this, the terms or words used in the present specification and claims should not be construed as being limited to conventional or dictionary meanings, and the inventor should properly understand the concept of the term in order to best describe his invention. It should be interpreted as meaning and concept consistent with the technical idea of the present invention based on the principle that it can be defined in
[37]
[38] An electrode sheet according to an embodiment of the present invention is an electrode sheet comprising a holding part and an uncoated part coated with a positive electrode mixture layer on at least one surface of a current collector, wherein the holding part is formed in a central part along a longitudinal direction of the electrode sheet, a first positive electrode mixture layer including a positive electrode active material of lithium nickel oxide; and a second positive electrode mixture layer formed on one or both edges of the first positive electrode mixture layer and including a positive electrode active material of lithium nickel oxide, wherein the positive electrode active material particle strength in the second positive electrode mixture layer is, It is characterized in that it is greater than the particle strength of the positive active material in the layer.
[39] 2 is a graph showing the moisture content in the electrode according to the electrode manufacturing step. Referring to this graph, it can be seen that the moisture content in the electrode is greatly increased immediately after the rolling process. This is because, as the electrode is rolled with a large force, the active material particles in the electrode layer are crushed, and the specific surface area of the active material is rapidly increased.
[40] In addition, the rolling roller for rolling the electrode sheet may have a high rolling ratio at both ends of the roller due to causes such as structure or wear. 3 shows the shape of the rolling roller 20 due to wear, the central portion 20a of the roller has a structure that is more worn compared to both ends 20b of the roller, and in the rolling roller of this structure, Both end portions may have a greater rolling rate than the central portion. Accordingly, the portion corresponding to both ends of the roller in the electrode sheet receives more force during rolling than the portion corresponding to the center portion of the roller, so the active material particles may be more brittle by that amount, and thus the specific surface area of the active material particles can become vulnerable to moisture. Moreover, in the electrode sheet in the form of being wound into a roll for storage of the electrode sheet, the corresponding portion is to both end portions in the width direction, since the penetration of moisture from the outside can be facilitated, thus further exacerbating the moisture vulnerability.
[41] In this way, both ends of the electrode sheet in the width direction are easier to contact with moisture due to their position compared to the central part, and there is a possibility that the rolling rate is relatively high due to the influence of the worn rolling rollers, and the reaction between the active material and moisture It is an environment of increasing area. Therefore, in manufacturing a positive electrode or positive electrode sheet having a high nickel content, which is vulnerable to moisture, by including a positive electrode active material having a particle strength relatively stronger to rolling than a central portion in both end portions in the width direction of the electrode sheet, At both ends, the reaction between nickel and moisture was minimized.
[42] Referring to FIG. 4 , the electrode sheet of the present invention includes a holding part 100 and an uncoated part 200 coated with a positive electrode mixture layer on at least one surface of a current collector, and the holding part 100 includes an electrode sheet. It consists of a first positive electrode mixture layer 110 formed in a central portion along the longitudinal direction (y-axis) of , and a second positive electrode mixture layer 120 formed on both edges of the first positive electrode mixture layer 110 . Here, both sides refer to both edges with respect to the width direction (x-axis) of the electrode sheet. 4 illustrates an embodiment in which the second positive electrode mixture layer is formed on both edges of the first positive electrode mixture layer, but is not limited thereto, and the second positive electrode mixture layer may be formed on one edge region of the first positive electrode mixture layer. there is.
[43] In the electrode sheet of the present invention, the particle strength of the positive electrode active material included in the second positive electrode mixture layer is greater than the particle strength of the positive electrode active material in the first positive electrode mixture layer. By including the positive electrode active material having a relatively large particle strength in the second positive electrode mixture layer as described above, the magnitude of the force applied to the second positive electrode mixture layer during rolling due to the abrasion of the rolling roller is increased by the amount of force applied to the first positive electrode mixture layer. Even if it is larger than the magnitude of the force, the degree of particle breakage of the second positive electrode mixture layer is similar to or smaller than that of the first positive electrode mixture layer, and the increase in the specific surface area of the active material particles is suppressed by that amount. This will minimize the reactivity with water.
[44] In the present invention, the particle strength may be defined as compressive fracture strength. A cathode active material for a secondary battery is subjected to a rolling process as one of the manufacturing processes. The rolling process means pressing the active material layer several times with a predetermined pressure in order to increase the density and increase the crystallinity. During the rolling process, some particles of the cathode active material may be broken without overcoming the compressive stress received during rolling, and thus the particles may be destroyed. When a force is applied to the cathode active material particles, the particle strength can be quantified by measuring the force at the point in time when the cracks occur in the particles. For example, the particle strength is measured by measuring the point at which the particles crack (crack) by applying pressure to the positive active material with a force of 0.5 to 10 mN using a micro compression tester (Equipment for Electronic Components Research Institute). It may be a value converted to .
[45] In one specific example, the range of the particle strength of the positive electrode active material of the second positive electrode mixture layer may be 30 to 300 MPa, more preferably 40 to 200 MPa, more preferably 50 to 150 MPa. can In addition, the particle strength of the positive electrode active material of the first positive electrode mixture layer, within a range smaller than the particle strength of the positive electrode active material of the second positive electrode mixture layer, may be 30 to 300 MPa, more preferably 40 to 200 MPa and more preferably 50 to 150 MPa.
[46] In one specific example, the ratio (B / A) of the positive electrode active material particle strength (B) in the second positive electrode mixture layer to the positive electrode active material particle strength (A) in the first positive electrode mixture layer may be greater than 1 and 2.0 or less and may preferably be 1.01 to 1.5, and more preferably 1.1 to 1.4.
[47] In one specific example, the second positive electrode mixture layer includes a first positive electrode active material having a relatively large average particle size (D 50 ) and a second positive electrode active material having a relatively small average particle size (D 50 ). contains a mixture of The second positive electrode mixture layer in which the positive electrode active material of large particle diameter and small particle diameter are mixed is filled with the second positive electrode active material of small particle diameter in the pores formed by particles of the first positive electrode active material of large particle diameter, so that the first positive electrode active material of large particle diameter It can be stronger for the same compressive stress as compared to the case composed only of particles. The present invention applies a blending system of a first positive electrode active material having a large particle diameter and a second positive electrode active material having a small particle diameter to the second positive electrode mixture layer, so that the particle strength of the active material of the second positive electrode mixture layer is determined by the particles of the first positive electrode mixture layer active material greater than the strength.
[48] In one specific example, the first positive active material may have an average particle size (D 50) of 9 μm to 30 μm, preferably 9 to 25 μm, more preferably 10 to 20 μm, and the second The positive active material may have an average particle size (D 50) of less than 9 μm, preferably 1 to 8 μm, and more preferably 2 to 7 μm.
[49] And, in the present invention, the average particle size D 50 may be defined as a particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. The average particle diameter D 50 may be measured using, for example, a laser diffraction method. For example, in the method of measuring the average particle size (D 50) of the positive active material, the particles of the positive active material are dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device (eg, Microtrac MT 3000). After irradiating ultrasonic waves of about 28 kHz with an output of 60 W, the average particle diameter D 50 corresponding to 50% of the volume accumulation amount in the measuring apparatus can be calculated.
[50] In one specific example, each of the positive electrode active materials included in the first positive electrode mixture layer and the second positive electrode mixture layer each independently includes a compound represented by Formula 1 below.
[51] [Formula 1]
[52] Li aNi 1-x-yCo xM1 yM2 wO 2
[53] (In Formula 1, 1.0≤a≤1.5, 0≤x≤0.2, 0≤y≤0.2, 0≤w≤0.1 and 0≤x+y≤0.4,
[54] M1 includes any one or both selected from the group consisting of Mn and Al, and M2 is any one or two or more elements selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb, and Mo. including)
[55] When it has the composition represented by the above formula (1), it can exhibit excellent capacity characteristics along with excellent structural stability.
[56] Specifically, in the lithium nickel oxide represented by Formula 1, Li may be included in an amount corresponding to a, that is, 1.0≤a≤1.5. If a is less than 1.0, there is a fear that the capacity may decrease, and if it exceeds 1.5, the particles are sintered in the firing process, which may make it difficult to manufacture the active material. Considering the remarkable effect of improving the capacity characteristics of the positive electrode active material according to the control of the Li content and the balance of sinterability during the production of the active material, Li is more specifically 1.0≤a≤1.2, and more specifically 1.0≤a≤1.15. may be included.
[57] In addition, in the lithium nickel oxide represented by Formula 1, Ni may be included in a content corresponding to 1-x-y, that is, a content of 0.6≤1-x-y≤1. If 1-x-y is less than 0.6, there is a risk that the capacity characteristics may be deteriorated, and if it exceeds 1, there is a risk of deterioration in high-temperature stability.There are concerns. Considering the remarkable effect of improving the capacity characteristics according to the inclusion of Ni, Ni may be included in a content of 0.8≤1-x-y<1, more specifically, 0.8≤1-x-y<0.95.
[58] In addition, in the lithium nickel oxide represented by Formula 1, M1 may be at least one selected from the group consisting of Al and Mn, and more specifically, may be Al or Mn. The M1 may be included in a content corresponding to y, that is, a content of 0≤y≤0.2. When y exceeds 0.2, there is a fear that the output characteristics and capacity characteristics of the battery are rather deteriorated. Considering the remarkable effect of improving battery characteristics due to the inclusion of element M1, M1 may be more specifically included in a content of 0<y≤0.2, and more specifically, 0.05≤y≤0.2.
[59] In addition, the elements of Ni, Co and M1 in the lithium nickel oxide represented by Formula 1 may be partially substituted or doped by another element, that is, M2, in order to improve battery characteristics through distribution control of metal elements in the active material. may be Specifically, M2 may be any one or two or more elements selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb, and Mo, and more specifically, may be Zr or Ti. The element of M2 may be included in an amount corresponding to w, that is, 0≤w≤0.1 within a range that does not deteriorate the characteristics of the cathode active material. More specifically, M2 may be included in a content of 0<w≤0.1, and more specifically, 0<w≤0.02.
[60] In one specific example, the width length of the second positive electrode mixture layer is 1 to 15%, preferably 2 to 13%, more preferably 3 to 10% of the width length of the first positive electrode mixture layer. Referring to FIG. 4 , the width and length W2 of the second positive electrode mixture layer may be defined as the sum of the width length W2a of the second positive electrode mixture layer at the left edge of the holding part and the width length W2b of the second positive electrode mixture layer at the right edge of the holding part. The sum of these lengths (W2a + W2b) may be 1 to 15% of the width and length W1 of the first positive electrode mixture layer. When the width and length of the second positive electrode mixture layer satisfies the above numerical range, it is preferable in terms of realizing a high energy density while suppressing a reaction between nickel and moisture in the positive electrode active material.
[61] In one specific example, in the second positive electrode mixture layer, a mixing ratio of the first positive active material and the second positive active material may be 95:5 to 65:35 by weight, preferably 90: It may be 10 to 70:30, and more preferably 85:15 to 75:25. If the amount of the first positive active material exceeds 95:5, it is not preferable because the second positive active material cannot sufficiently fill the pores formed by the first positive active material, and the second positive active material exceeds 65:35 and contains too much of the second positive active material. In this case, it is not preferable because the specific surface area may rather increase due to the surplus of the second positive electrode active material remaining even after filling the pores.
[62] first embodiment
[63] In the electrode sheet according to the first embodiment of the present invention, the second positive electrode mixture layer includes the first positive electrode active material and the second positive electrode active material, and the first positive electrode mixture layer has the same average particle size (D 50 ). It may be composed of a cathode active material.
[64] In this case, the positive electrode active material of the first positive electrode mixture layer may have an average particle size (D 50) of 9 μm to 30 μm, preferably 9 to 25 μm, and more preferably 10 to 20 μm. . Also, the average particle size of the first positive electrode active material of the second positive electrode mixture layer may be the same.
[65] second embodiment
[66] In the electrode sheet according to the second embodiment of the present invention, the second positive electrode mixture layer includes the first positive electrode active material and the second positive electrode active material, and the first positive electrode mixture layer also has a large particle size, similarly to the second positive electrode mixture layer. It may include a mixture of the first positive active material and the second positive active material having a small particle size.
[67] At this time, in order for the second positive electrode mixture layer to be relatively stronger in rolling than the first positive electrode mixture layer, the weight (b) of the second positive electrode active material relative to the weight (a) of the first positive electrode active material in the second positive electrode mixture layer ) is greater than the ratio (b' / a') of the weight (b') of the second positive electrode active material to the weight (a') of the first positive electrode active material in the first positive electrode mixture layer (b' / a') . According to this design, in the second positive electrode mixture layer, the ratio of filling the empty space in the pores formed by the first positive active materials having a relatively large average particle diameter of the second positive electrode active materials having a relatively small average particle diameter is, In the first positive electrode mixture layer, the empty space formed by the first positive electrode active materials is greater than the filling ratio of the second positive electrode active materials, so that the second positive electrode mixture layer is stronger in rolling than the first positive electrode mixture layer. will be.
[68] In this case, the mixing ratio of the first positive active material particles having a large particle diameter and the second positive electrode active material particles having a small particle diameter in the second positive electrode mixture layer may be 95:5 to 65:35 by weight, preferably 90:10 to 70:30, and more preferably 85:15 to 75:25.
[69] In addition, the first positive electrode active material included in the second positive electrode mixture layer may have an average particle size (D 50) of 9 μm to 30 μm, preferably 9 to 25 μm, more preferably 10 to 20 μm, The second positive active material may have an average particle size (D 50) of less than 9 μm, preferably 1 to 8 μm, and more preferably 2 to 7 μm.
[70]
[71] Hereinafter, the lithium secondary battery of the present invention will be described. The lithium secondary battery of the present invention includes a positive electrode in which the holding part and the uncoated part of the electrode sheet are punched out according to the shape and size of the unit electrode.
[72] The positive electrode includes a positive electrode current collector and a first positive electrode mixture layer and a second positive electrode mixture layer formed on the positive electrode current collector.
[73] The positive electrode current collector is not particularly limited as long as it has conductivity without causing chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, fired carbon, or carbon, nickel, titanium on the surface of aluminum or stainless steel. , silver or the like surface-treated may be used. In addition, the positive electrode current collector may typically have a thickness of 3 to 500 μm, and may increase the adhesion of the positive electrode active material by forming fine irregularities on the surface of the positive electrode current collector. For example, it may be used in various forms, such as a film, a sheet, a foil, a net, a porous body, a foam, a non-woven body.
[74] The first positive electrode mixture layer may include a conductive material and a binder together with the above-described positive electrode active material, and the second positive electrode mixture layer may also include a conductive material and a binder together with the above-described positive electrode active material.
[75] The conductive material is used to impart conductivity to the electrode, and in the configured battery, it can be used without any particular limitation as long as it does not cause chemical change and has electronic conductivity. Specific examples include graphite such as natural graphite and artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powders or metal fibers, such as copper, nickel, aluminum, and silver; conductive whiskeys such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like, and one or a mixture of two or more thereof may be used. The conductive material may be included in an amount of 1 to 30 wt % based on the total weight of the cathode material layer.
[76] The binder serves to improve adhesion between the positive electrode active material particles and the adhesive force between the positive electrode active material and the positive electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC) ), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and any one of them or a mixture of two or more thereof may be used. The binder may be included in an amount of 1 to 30% by weight based on the total weight of the cathode material layer.
[77] The positive electrode uses the above-described positive electrode active material, a dual slot-die coater, a first positive electrode mixture layer is applied to a central portion, and a second positive electrode mixture layer is applied to both edges of the central portion, and a first positive electrode mixture layer and a second positive electrode Except for the fact that the composition of the mixture layer is different, it may be manufactured according to a conventional positive electrode manufacturing method. Specifically, the positive electrode slurry for forming a positive electrode composite layer comprising the above positive electrode active material and, optionally, a binder and a conductive material, is supplied to a dual slot-die coater, and applied on the positive electrode current collector using a dual slot-die coater. Then, it can be prepared by drying and rolling. In this case, the types and contents of the positive electrode material, the binder, and the conductive material are as described above.
[78] The positive electrode slurry solvent may be a solvent generally used in the art, dimethyl sulfoxide (DMSO), isopropyl alcohol (isopropyl alcohol), N-methylpyrrolidone (NMP), acetone ( acetone) or water, and any one of them or a mixture of two or more thereof may be used. The amount of the solvent used is enough to dissolve or disperse the positive electrode active material, the conductive material and the binder in consideration of the application thickness of the slurry and the production yield, and to have a viscosity capable of exhibiting excellent thickness uniformity during application for the production of the positive electrode thereafter. Do.
[79] Specifically, the lithium secondary battery includes a positive electrode, a negative electrode positioned to face the positive electrode, and a separator interposed between the positive electrode and the negative electrode It includes a catalyst and an electrolyte, and the positive electrode is the same as described above. In addition, the lithium secondary battery may optionally further include a battery container for accommodating the electrode assembly of the positive electrode, the negative electrode, and the separator, and a sealing member for sealing the battery container.
[80] The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical change in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, fired carbon, copper or stainless steel surface. Carbon, nickel, titanium, silver, etc. surface-treated, aluminum-cadmium alloy, etc. may be used. In addition, the negative electrode current collector may have a thickness of typically 3 to 500 μm, and similarly to the positive electrode current collector, fine irregularities may be formed on the surface of the current collector to strengthen the bonding force of the negative electrode active material. For example, it may be used in various forms, such as a film, a sheet, a foil, a net, a porous body, a foam, a nonwoven body.
[81] The negative electrode mixture layer optionally includes a binder and a conductive material together with the negative electrode active material. As an example, the negative electrode mixture layer is formed by applying a negative electrode active material, and optionally, a negative electrode forming slurry including a binder and a conductive material on a negative electrode current collector and drying, or casting the negative electrode forming slurry on a separate support. , may be produced by laminating a film obtained by peeling from this support onto a negative electrode current collector.
[82] As the anode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metal compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; metal oxides capable of doping and dedoping lithium, such as SiO x (0 < x < 2), SnO 2 , vanadium oxide, and lithium vanadium oxide; Alternatively, a composite including the metallic compound and a carbonaceous material such as a Si-C composite or a Sn-C composite may be used, and any one or a mixture of two or more thereof may be used. In addition, a metal lithium thin film may be used as the negative electrode active material. In addition, as the carbon material, both low crystalline carbon and high crystalline carbon may be used. As low crystalline carbon, soft carbon and hard carbon are representative, and as high crystalline carbon, amorphous, plate-like, flaky, spherical or fibrous natural or artificial graphite, Kish graphite (Kish) graphite), pyrolytic carbon, mesophase pitch based carbon fiber, meso-carbon microbeads, liquid crystal pitches (Mesophase pitches), and petroleum and coal tar pitch (petroleum or coal tar pitch) High-temperature calcined carbon such as derived cokes) is a representative example.
[83] In addition, the binder and the conductive material may be the same as those described above for the positive electrode.
[84] On the other hand, in the lithium secondary battery, the separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move, and as long as it is used as a separator in a lithium secondary battery, it can be used without any particular limitation, especially for the movement of ions in the electrolyte It is preferable to have a low resistance to respect and an excellent electrolyte moisture content. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer and ethylene / methacrylate copolymer, or these A laminate structure of two or more layers of may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high melting point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material may be used to secure heat resistance or mechanical strength, and may optionally be used in a single-layer or multi-layer structure.
[85] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes, which can be used in the manufacture of lithium secondary batteries, and are limited to these. it is not going to be
[86] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[87] The organic solvent may be used without particular limitation as long as it can serve as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, as the organic solvent, ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), propylene carbonate, carbonate-based solvents such as PC); alcohol solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a C2 to C20 linear, branched or cyclic hydrocarbon group, which may include a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; Or sulfolane may be used. Among these, a carbonate-based solvent is preferable, and a cyclic carbonate (eg, ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant capable of increasing the charge / discharge performance of the battery, and a low-viscosity linear carbonate-based compound ( For example, a mixture of ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferable. In this case, when the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to about 1:9, the performance of the electrolyte may be excellent.
[88] The lithium salt may be used without particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt is, LiPF 6, LiClO 4, LiAsF 6, LiBF 4, LiSbF 6, LiAl0 4, LiAlCl 4, LiCF 3SO 3, LiC 4F 9SO 3, LiN(C 2F 5SO 3) 2, LiN(C 2F 5SO 2) 2, LiN(CF 3SO 2) 2. LiCl, LiI, or LiB(C 2O 4) 2 and the like may be used. The concentration of the lithium salt is preferably used within the range of 0.1 to 2.0M. When the concentration of the lithium salt is included in the above range, the electrolyte may exhibit excellent electrolyte performance because it has appropriate conductivity and viscosity, and lithium ions may move effectively.
[89] In addition to the electrolyte components, the electrolyte includes, for example, haloalkylene carbonate-based compounds such as difluoroethylene carbonate, pyridine, tri Ethyl phosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imida One or more additives such as jolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxy ethanol or aluminum trichloride may be further included. In this case, the additive may be included in an amount of 0.1 to 5% by weight based on the total weight of the electrolyte.
[90] As described above, since the lithium secondary battery including the positive electrode according to the present invention stably exhibits excellent discharge capacity, output characteristics and capacity retention rate, it is used in portable devices such as mobile phones, notebook computers, digital cameras, etc. It is useful in the automotive field, etc.
[91] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided. The battery module or battery pack is a power tool (Power Tool); electric vehicles, including electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); Alternatively, it may be used as a power source for any one or more medium-to-large devices in a system for power storage.
[92]
[93] Hereinafter, a method for manufacturing an electrode sheet according to the present invention will be described.
[94] A method of manufacturing an electrode sheet according to an embodiment of the present invention includes: a slurry preparation process of preparing a slurry for a first positive electrode mixture and a slurry for a second positive electrode mixture, respectively; a coating process of forming a first positive electrode mixture layer and a second positive electrode mixture layer by applying the first positive electrode mixture slurry and the second positive electrode mixture slurry on the current collector sheet; drying process; and a rolling process, wherein in the coating process, the first positive electrode mixture slurry is at the center of the electrode sheet, and the second positive electrode mixture slurry is the first positive electrode mixture slurry based on the width direction of the electrode sheet. It has a predetermined width on one or both edges, and is applied in the longitudinal direction of the electrode sheet.
[95] The second positive electrode mixture slurry includes a mixture of a first positive electrode active material having a relatively large average particle size (D 50) and a second positive electrode active material having a relatively small average particle size (D 50). characterized in that
[96] Specifically, the slurry for the second positive electrode mixture includes both the first positive active material having an average particle size (D 50) of 9 μm to 30 μm and the second positive active material having an average particle size (D 50) of less than 9 μm. In preparing the slurry for the second positive electrode mixture, the positive electrode active material particle strength in the second positive electrode mixture layer is determined by including the first positive electrode active material having a large particle diameter and the second positive electrode active material having a small particle diameter, and the positive electrode active material particle strength in the first positive electrode mixture layer you can make it bigger
[97] In one preferred embodiment, the mixing ratio of the first positive active material particles having a large particle diameter and the second positive electrode active material particles having a small particle diameter may be 95:5 to 65:35, more preferably 90:10 to 75:25 days and more preferably 85:15 to 70:30. When the mixing ratio of the first positive electrode active material particles and the second positive electrode active material particles is within the above numerical range, it is easy to control the particle strength of the positive electrode active material in the second positive electrode mixture layer to be greater than that of the first positive electrode mixture layer.
[98] At this time, the positive electrode active material included in the first positive electrode mixture slurry may be composed of a positive electrode active material having the same average particle size (D50), and unlike the first positive electrode active material having a relatively large average particle size (D50) of a large particle diameter. and a mixture of the second positive electrode active material having a relatively small average particle size (D50).
[99] In one specific example, in the coating process, the width of the second positive electrode mixture layer is preferably 1 to 15% of the width of the first positive electrode mixture layer.
[100]
[101] Hereinafter, embodiments of the present invention will be described in detail so that those of ordinary skill in the art can easily carry out the present invention. However, the present invention may be embodied in several different forms and is not limited to the embodiments described herein.
[102]
[103] Example 1
[104] (Preparation of the first positive electrode slurry for forming the first positive electrode mixture layer)
[105] As a transition metal oxide of lithium-nickel-cobalt-manganese, a first positive active material having a nickel content of 80 mol% based on the total transition metal (D 50 is 11 μm) was prepared, and a carbon black conductive material and a PVDF binder were prepared. A first positive electrode slurry (viscosity: 7000 Pa·s) was prepared by mixing in N-methylpyrrolidone solvent in a weight ratio of 96.5:1.5:2.
[106] (Preparation of the second positive electrode slurry for forming the second positive electrode mixture layer)
[107] As a transition metal oxide of lithium-nickel-cobalt-manganese, the first positive active material having a nickel content of 80 mol% based on the total transition metal (D 50 is 11 μm) and a transition metal oxide of lithium-nickel-cobalt-manganese As such, a positive electrode active material in which a second positive active material having a nickel content of 80 mol% based on the total transition metal (D 50 is 6 μm) is mixed in a ratio of 8:2 by weight, and carbon black conductive material and PVDF binder in N-methylpyrrolidone solvent in a weight ratio of 96.5:1.5:2 to prepare a first positive electrode slurry (viscosity: 7000 Pa·s).
[108] (Manufacturing and storage of anode sheet)
[109] The first positive electrode slurry and the second positive electrode slurry are supplied to a dual slot-die coater, and the first positive electrode slurry and the second positive electrode slurry are applied to one surface of an aluminum current collector sheet using the coater to form a first positive electrode mixture A layer and a second positive electrode mixture layer were formed. At this time, the first positive electrode slurry was applied to the central portion of the slurry application portion, and the second positive electrode slurry was applied to both edges of the first positive electrode slurry application portion, and the sum of the widths and lengths of the second positive electrode slurry application portion was 1 It was set to be 8% of the width and length of the positive electrode slurry application part.
[110] Thereafter, the positive electrode sheet including the first positive electrode mixture layer and the second positive electrode mixture layer was dried at 130° C. and rolled.
[111] After the thus-prepared positive electrode sheet was wound in the form of a roll and stored at room temperature of 25° C. for 7 days, the positive electrode tab was notched in the uncoated part of the positive electrode sheet, and the positive electrode sheet was slitted to complete the production of the positive electrode. .
[112] (Manufacture of battery)
[113] An electrode assembly was prepared by interposing a porous polyolefin separator between lithium metal as the positive electrode and the negative electrode, and the electrode assembly was placed inside the case, and then the electrolyte was injected into the case to prepare a lithium secondary battery. At this time, it was prepared by dissolving lithium hexafluorophosphate (LiPF 6) at a concentration of 1.0M in an organic solvent consisting of ethylene carbonate / dimethyl carbonate / ethylmethyl carbonate (mixed volume ratio of EC / DMC / EMC=3 / 4 / 3).
[114]
[115] Example 2
[116] A battery was manufactured in the same manner as in Example 1, except that in Example 1, a mixing ratio of the first positive active material and the second positive active material was mixed in a ratio of 85:15 when the second positive electrode slurry was prepared. did
[117]
[118] Example 3
[119] A battery was manufactured in the same manner as in Example 1, except that in Example 1, a mixing ratio of the first positive active material and the second positive active material was mixed in a ratio of 75:25 when the second positive electrode slurry was prepared. did
[120]
[121] Example 4
[122] In Example 1, a battery was manufactured in the same manner as in Example 1, except that the first positive electrode slurry was prepared as follows.
[123] (Preparation of the first positive electrode slurry for forming the first positive electrode mixture layer)
[124] As a transition metal oxide of lithium-nickel-cobalt-manganese, the first positive active material having a nickel content of 80 mol% based on the total transition metal (D 50 is 11 μm) and a transition metal oxide of lithium-nickel-cobalt-manganese As a result, a positive electrode active material in which a second positive electrode active material having a nickel content of 80 mol% based on the total transition metal (D 50 is 6 μm) was mixed in a ratio of 9:1 by weight, and carbon black conductive material and PVDF binder in N-methylpyrrolidone solvent in a weight ratio of 96.5:1.5:2 to prepare a first positive electrode slurry (viscosity: 7000 Pa·s).
[125]
[126] Comparative Example 1
[127] A slurry for forming a positive electrode was prepared by using the same raw material and manufacturing method of the first positive electrode slurry of Example 1. The slurry for forming the positive electrode was applied on an aluminum current collector using a single slot-die coater to form a positive electrode mixture layer.
[128] Thereafter, a battery was manufactured in the same manner as in Example 1.
[129]
[130] Comparative Example 2
[131] A battery was manufactured in the same manner as in Example 1, except that in Example 1, the first positive electrode slurry and the second positive electrode slurry were prepared as follows.
[132] (Preparation of the first positive electrode slurry for forming the first positive electrode mixture layer)
[133] As a transition metal oxide of lithium-nickel-cobalt-manganese, the first positive active material having a nickel content of 80 mol% based on the total transition metal (D 50 is 11 μm) and a transition metal oxide of lithium-nickel-cobalt-manganese Thus, a positive electrode active material in which a second positive electrode active material having a nickel content of 80 mol% based on the total transition metal (D 50 is 6 μm) was mixed in a ratio of 7:3 by weight, and carbon black conductive material and PVDF binder in N-methylpyrrolidone solvent in a weight ratio of 96.5:1.5:2 to prepare a first positive electrode slurry (viscosity: 7000 Pa·s).
[134] (Preparation of the second positive electrode slurry for forming the second positive electrode mixture layer)
[135] As a transition metal oxide of lithium-nickel-cobalt-manganese, the first positive active material having a nickel content of 80 mol% based on the total transition metal (D 50 is 11 μm) and a transition metal oxide of lithium-nickel-cobalt-manganese As such, a positive electrode active material in which a second positive active material having a nickel content of 80 mol% based on the total transition metal (D 50 is 6 μm) is mixed in a ratio of 8:2 by weight, and carbon black conductive material and PVDF binder in N-methylpyrrolidone solvent in a weight ratio of 96.5:1.5:2 to prepare a first positive electrode slurry (viscosity: 7000 Pa·s).
[136]
[137] Experimental Example 1: Measurement of particle strength
[138] For each of the positive electrode active material in the first positive electrode mixture layer and the positive electrode active material in the second positive electrode mixture layer in Examples 1 to 4 and Comparative Examples 1 to 2, the force when the particles are broken while applying a pressure of 100 mN for 1 minute Measured, the size of the particle strength was compared, and the results are shown in Table 1. When the particle strength of the positive electrode active material of the second positive electrode mixture layer was greater than that of the first positive electrode mixture layer, “O” was indicated, and conversely, when the particle strength was less than or equal to that of the first positive electrode mixture layer, “X” was indicated.
[139]
[140] Experimental Example 2: Capacity and lifetime characteristics evaluation
[141] The lithium secondary batteries of Examples 1 to 4 and Comparative Examples 1 and 2 were initially charged and discharged using an electrochemical charger / discharger. At this time, charging was performed by applying a current at a current density of 0.33 C-rate up to a voltage of 4.2V, and discharging was performed at the same current density up to 2.5V (temperature of 45°C). A total of 500 such charging and discharging was performed.
[142] In the charging and discharging process as described above, the capacity of each battery was measured.
[143] From this, the capacity retention ratio of each battery was calculated as follows, and the results are shown in Table 1, and the change in the capacity retention ratio according to the cycle is shown in FIG. 5 .
[144] Capacity retention rate (%) = (capacity in N cycles / initial capacity) X 100
[145] [Table 1]Particle strength of the active material of the second positive electrode mixture layer > Particle strength of the active material of the first positive electrode mixture layer? Capacity retention at 500 cycles(%)Example 1 0 91.9Example 2 0 90.6Example 3 O 91.2Example 4 0 89.0Comparative Example 1 X 87.5Comparative Example 2 X 87
[146] Referring to Table 1 and Figure 5, the secondary battery according to the embodiment of the present invention has an excellent capacity retention rate compared to the battery of the comparative example, which is a positive electrode to which a positive electrode active material of lithium nickel oxide is applied. It is judged that this is due to the effect of suppressing the reactivity of the nickel component with moisture by differently controlling the particle strengths of the second positive electrode mixture layer and each positive electrode active material included in the first positive electrode mixture layer.
[147]
[148] As seen through the above, drawings, examples, etc.The invention has been described in more detail. However, the configuration described in the drawings or embodiments described in the present specification is only one embodiment of the present invention and does not represent all the technical spirit of the present invention, so at the time of the present application, various equivalents and It should be understood that there may be variations.
Claims
Claims
1. An electrode sheet comprising a holding part and an uncoated part coated with a positive electrode mixture layer on at least one surface of a current collector, wherein the holding part is formed in a central part along the length direction of the electrode sheet, and comprising a positive electrode active material of lithium nickel oxide 1 positive electrode mixture layer; and a second positive electrode mixture layer formed on one or both edges of the first positive electrode mixture layer and including a positive electrode active material of lithium nickel oxide, wherein the positive electrode active material particle strength in the second positive electrode mixture layer is, An electrode sheet, characterized in that it is greater than the particle strength of the positive electrode active material in the layer.
2. The electrode sheet according to claim 1, wherein a width of the second positive electrode mixture layer is 1 to 15% of a width of the first positive electrode mixture layer.
3. The electrode sheet according to claim 1, wherein each of the positive electrode active materials included in the first positive electrode mixture layer and the second positive electrode mixture layer each independently includes a compound represented by the following Chemical Formula 1. [Formula 1] Li aNi 1-x-yCo xM1 yM2 wO 2 (In Formula 1, 1.0≤a≤1.5, 0≤x≤0.2, 0≤y≤0.2, 0≤w≤0.1 and 0≤x+y ≤0.4, M1 includes any one or both selected from the group consisting of Mn and Al, and M2 is any one selected from the group consisting of Ba, Ca, Zr, Ti, Mg, Ta, Nb, and Mo or contains two or more elements)
4. According to claim 1, wherein the ratio (B / A) of the positive electrode active material particle strength (B) in the second positive electrode mixture layer to the positive electrode active material particle strength (A) in the first positive electrode mixture layer is 1.01 to 1.5 Characterized in the electrode sheet.
5. The method of claim 1, wherein the second positive electrode mixture layer comprises a first positive electrode active material having a relatively large average particle size (D 50) and a second positive electrode having a relatively small average particle size (D 50). An electrode sheet comprising a mixture of active materials.
6. The method according to claim 5, wherein the first positive active material has an average particle size (D 50) of 9 μm to 30 μm, and the second positive active material has an average particle size (D 50) of less than 9 μm. electrode sheet.
7. The electrode sheet according to claim 5, wherein in the second positive electrode mixture layer, a mixing ratio of the first positive active material and the second positive active material is 95:5 to 65:35 by weight.
8. The electrode sheet according to claim 5, wherein the positive electrode active material of the first positive electrode mixture layer is composed of a positive electrode active material having the same average particle size (D 50).
9. The electrode sheet according to claim 8, wherein the positive electrode active material of the first positive electrode mixture layer has an average particle size (D 50) of 9 μm to 30 μm.
10. The method of claim 7, wherein the first positive electrode mixture layer comprises a first positive electrode active material having a relatively large average particle size (D 50) and a second positive electrode having a relatively small average particle size (D 50). An electrode sheet comprising a mixture of active materials.
11. The method of claim 10, wherein the ratio (b / a) of the weight (b) of the second positive electrode active material to the weight (a) of the first positive electrode active material in the second positive electrode mixture layer is: An electrode sheet, characterized in that the ratio (b′ / a′) of the weight (b′) of the second positive electrode active material to the weight (a′) of the first positive electrode active material is greater than (b′ / a′).
12. The method according to claim 10, wherein the first positive active material has an average particle size (D 50) of 9 μm to 30 μm, and the second positive active material has an average particle size (D 50) of less than 9 μm. electrode sheet.
13. A lithium secondary battery comprising a positive electrode in which the holding part and the uncoated part of the electrode sheet according to claim 1 are punched out according to the shape and size of a unit electrode.
14. A method of manufacturing the electrode sheet according to claim 1, comprising: a slurry preparation process of preparing a slurry for a first positive electrode mixture and a slurry for a second positive electrode mixture, respectively; a coating process of forming a first positive electrode mixture layer and a second positive electrode mixture layer by applying the first positive electrode mixture slurry and the second positive electrode mixture slurry on the current collector sheet; drying process; and a rolling process, wherein in the coating process, the first positive electrode mixture slurry is at the center of the electrode sheet, and the second positive electrode mixture slurry is the first positive electrode mixture slurry based on the width direction of the electrode sheet. The slurry for the second positive electrode mixture having a predetermined width on one or both edges of the electrode sheet and applied in the longitudinal direction includes a first positive electrode active material having a relatively large average particle size (D 50) and a large particle diameter, and average particles A method of manufacturing an electrode sheet comprising a mixture of a second positive electrode active material having a relatively small size (D 50 ).
15. 15. The method of claim 14, wherein the width of the second positive electrode mixture layer in the coating process is 1 to 15% of the width of the first positive electrode mixture layer.