Can steel sheet and method for producing same
Patent Information
- Application Number
- IN202417047106
- Authority / Receiving Office
- IN · IN
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-12-28
- Filing Date
- 2024-06-19
- Publication Date
- 2026-10-07
- Estimated Expiration
- 2042-10-18
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a steel sheet for cans(tin mill black plate) and a method for manufacturing the same.BACKGROUND ART
[0002] Patent Literature 1 discloses a steel sheet for cansincluding, "on a surface of a steel sheet, a chromium metallayer and a hydrated chromium oxide layer stacked in this orderfrom the steel sheet side" and further including "granularprotrusions" in the chromium metal layer.CITATION LISTPATENT LITERATURE
[0003] Patent Literature 1: WO 2017 / 098991 ASUMMARY OF INVENTIONTECHNICAL PROBLEMS
[0004] The steel sheet for cans having granular protrusions isexpected to exhibit favorable weldability. This is because whensteel sheets for cans are welded to each other, the hydratedchromium oxide layer is broken by the granular protrusions, andthe contact resistance is reduced. However, when granular protrusions are formed on a steelsheet for cans, a favorable surface appearance may not beobtained. This is presumed to be because the granularprotrusions diffusely reflect visible light. Therefore, an object of the present invention is to providea steel sheet for cans having not only excellent weldability butalso excellent surface appearance, and a method formanufacturing the same.SOLUTION TO PROBLEMS
[0005] The present inventors have conducted intensive studies, andas a result, have found that the object is achieved by adoptingthe following configuration, thereby completing the presentinvention.
[0006] That is, the present invention provides the following [1] to [6].[1] A steel sheet for cans comprising, on a surface of asteel sheet, a chromium metal layer and a hydrated chromiumoxide layer stacked in this order from a side closer to thesteel sheet, wherein a coating weight of the chromium metallayer is 50 to 200 mg / m2, a coating weight of the hydratedchromium oxide layer in terms of chromium is 3 to 50 mg / m2, thechromium metal layer includes a flat plate portion andprotrusion portions provided on the flat plate portion, a heightH of each of the protrusion portions is 10 nm or more and lessthan 500 nm, a bottom diameter D of each of the protrusionportions is 50 nm or more and 1000 nm or less, a ratio H / D ofthe height H and the bottom diameter D is less than 0.50, and anarea fraction of the protrusion portions is 5% or more.[2] A method for manufacturing the steel sheet for cansaccording to [1], the manufacturing method comprising subjectinga steel sheet to an immersion treatment with use of an aqueoussolution 1 and then to a cathodic electrolysis treatment withuse of an aqueous solution 2, wherein the aqueous solution 1contains a water-soluble organic compound, and the aqueoussolution 2 contains a hexavalent chromium compound, a fluorinecontaining compound, and sulfuric acid.[3] The method according to [2] for manufacturing thesteel sheet for cans, wherein a content of the water-solubleorganic compound in the aqueous solution 1 is 0.1 g / L or moreand less than 10 g / L.[4] The method according to [2] or [3] for manufacturingthe steel sheet for cans, wherein the water-soluble organiccompound is a water-soluble polymer having a weight averagemolecular weight of 300 to 100,000.[5] The method according to [4] for manufacturing thesteel sheet for cans, wherein the water-soluble polymer ispolyacrylic acid.[6] The method according to any one of [2] to [5] formanufacturing the steel sheet for cans, wherein a currentdensity of the cathodic electrolysis treatment is 10 to 200A / dm2.ADVANTAGEOUS EFFECTS OF INVENTION
[0007] According to the present invention, it is possible toprovide a steel sheet for cans having not only excellentweldability but also excellent surface appearance, and a methodfor manufacturing the same.BRIEF DESCRIPTION OF DRAWINGS
[0008] [FIG. 1] FIG. 1 is a cross-sectional view schematicallyillustrating a steel sheet for cans of the present embodiment.DESCRIPTION OF EMBODIMENTS
[0009] [Steel Sheet for Cans] FIG. 1 is a cross-sectional view schematically illustratinga steel sheet 1 for cans of the present embodiment. As illustrated in FIG. 1, the steel sheet 1 for cansincludes a steel sheet 2. The steel sheet 1 for cans furtherincludes, on a surface of the steel sheet 2, a chromium metallayer 3 and a hydrated chromium oxide layer 4 in this order fromthe steel sheet 2 side. The chromium metal layer 3 includes a flat plate portion 3ahaving a flat plate shape and covering the steel sheet 2, andprotrusion portions 3b provided on the flat plate portion 3a.The hydrated chromium oxide layer 4 is disposed on the chromiummetal layer 3 so as to follow the shape of the protrusionportions 3b. A height H and a bottom diameter D of the protrusionportion 3b will be described below.
[0010] Hereinafter, each constituent of the steel sheet for cansof the present embodiment will be described in more detail.
[0011] <Steel Sheet> The type of the steel sheet is not particularly limited.In general, steel sheets used as materials for containers (forexample, a low carbon steel sheet and an ultra low carbon steelsheet) can be used. A manufacturing method, material, and thelike of the steel sheet are also not particularly limited. Thesteel sheet is manufactured through a process starting with atypical billet manufacturing process, followed by such processesas hot rolling, pickling, cold rolling, annealing and temperrolling.
[0012] <Chromium Metal Layer> The chromium metal layer is disposed on the surface of thesteel sheet described above. The chromium metal layer suppressessurface exposure of the steel sheet and improves corrosionresistance.
[0013] <<Coating Weight>> For the reason that the corrosion resistance of the steelsheet for cans is excellent, the coating weight of the chromiummetal layer is 50 mg / m2 or more, preferably 70 mg / m2 or more, andmore preferably 80 mg / m2 or more. The coating weight is acoating weight per one surface of the steel sheet (the sameapplies hereinafter).
[0014] Meanwhile, when the coating weight of the chromium metallayer is too large, high-melting-point chromium metal covers theentire surface of the steel sheet, and this induces significantdecrease in weld strength in welding and significant generationof dust, which may lead to insufficient weldability. For the reason that the weldability of the steel sheet forcans is excellent, the coating weight of the chromium metallayer is 200 mg / m2 or less, preferably 180 mg / m2 or less, andmore preferably 160 mg / m2 or less.
[0015] (Method for Measuring Coating Weight) The coating weight of the chromium metal layer and thecoating weight of the hydrated chromium oxide layer describedbelow in terms of chromium are measured as follows. First, for the steel sheet for cans having the chromiummetal layer and the hydrated chromium oxide layer formedtherein, the amount of chromium (total amount of chromium) ismeasured using an X-ray fluorescence device. Next, the steelsheet for cans is subjected to alkaline treatment, i.e., isimmersed in a 6.5 N aqueous sodium hydroxide solution (liquidtemperature: 90°C) for 10 minutes, and then the amount ofchromium (the amount of chromium after alkaline treatment) ismeasured again using an X-ray fluorescence device. The amount ofchromium after alkaline treatment is taken as the coating weightof the chromium metal layer. Thereafter, the equation (amount of alkali-solublechromium) = (total amount of chromium) - (amount of chromiumafter alkaline treatment) is calculated, and the amount ofalkali-soluble chromium is taken as the coating weight of thehydrated chromium oxide layer in terms of chromium.
[0016] Such a chromium metal layer includes a flat plate portionand protrusion portions provided on the flat plate portion.Next, those portions included in the chromium metal layer willbe described in detail.
[0017] <<Flat Plate Portion>> The flat plate portion of the chromium metal layer mainlyserves to improve corrosion resistance by covering a surface ofthe steel sheet. It is preferable that the flat plate portion of thechromium metal layer has a thickness sufficient to prevent theflat plate portion from being destroyed by the protrusionportions provided in the surface layer and thus prevent thesteel sheet from being exposed, when the steel sheet for cansinevitably comes into contact with another steel sheet for cansat handling. For the reason that the corrosion resistance of the steelsheet for cans is excellent, the coating weight of the flatplate portion of the chromium metal layer is preferably 10 mg / m2or more, more preferably 30 mg / m2 or more, and even morepreferably 40 mg / m2 or more.
[0018] <<Protrusion Portion>> The protrusion portions of the chromium metal layer areformed on the surface of the flat plate portion described above,and reduce contact resistance between the steel sheets for cansto improve weldability. An estimated mechanism by which the contact resistance isreduced is described below. The hydrated chromium oxide layer covering the chromiummetal layer is a non-conductive coating and therefore has higherelectrical resistance than chromium metal, so that the hydratedchromium oxide layer works as a factor hindering welding. Byforming the protrusion portions on a surface of the flat plateportion of the chromium metal layer, the protrusion portions actto destroy the hydrated chromium oxide layer using the surfacepressure applied when to-be-welded portions of the steel sheetfor cans come into contact with each other in welding, and theprotrusion portions become current-carrying points of weldingcurrent, whereby the contact resistance greatly decreases.
[0019] (Height H) As the height H of the protrusion portion is increased, thesurface pressure applied when to-be-welded portions of the steelsheet for cans come into contact with each other is increased,whereby weldability becomes favorable. Therefore, the height H of the protrusion portion is 10 nmor more, preferably 50 nm or more, more preferably 100 nm ormore, and even more preferably 200 nm or more.
[0020] On the other hand, as the height H of the protrusionportion is too large, the surface appearance may be poor. The possible reasons of the above are for example asfollows: the protrusion portions absorb short-wavelength (blue)light, and accordingly, reflected light thereof is attenuated,so that a reddish brown color appears; and the protrusionportions diffuse reflected light, so that the overallreflectance decreases and the color tone becomes darker. Therefore, for the reason that the surface appearance ofthe steel sheet for cans is excellent, the height H of theprotrusion portion is less than 500 nm, preferably 450 nm orless, more preferably 400 nm or less, and even more preferablyless than 400 nm.
[0021] (Bottom Diameter D) As the bottom diameter D of the protrusion portion isincreased, the surface pressure applied when to-be-weldedportions of the steel sheet for cans come into contact with eachother is increased, whereby weldability becomes favorable. Therefore, the bottom diameter D of the protrusion portionis 50 nm or more, preferably 100 nm or more, more preferably 200nm or more, even more preferably 500 nm or more, andparticularly preferably 720 nm or more.
[0022] Meanwhile, as the bottom diameter D of the protrusionportion is too large, the surface appearance may be poor for thesame reason as when the height H of the protrusion portion istoo large. Therefore, for the reason that the surface appearance ofthe steel sheet for cans is excellent, the bottom diameter D ofthe protrusion portion is 1000 nm or less, preferably 900 nm orless, and more preferably 800 nm or less.
[0023] (H / D) When the height H is significantly larger than the bottomdiameter D, the surface appearance may be poor. Therefore, a ratio (H / D) of the height H and the bottomdiameter D of the protrusion portion is less than 0.50 andpreferably 0.49 or less. Meanwhile, the lower limit of the ratio (H / D) is notparticularly limited as long as the height H and the bottomdiameter D are within the foregoing ranges.
[0024] ((Method for Measuring Height H and Bottom Diameter D)) The height H and the bottom diameter D of the protrusionportion are determined as follows. First, a cross-sectional sample of a steel sheet for canshaving a chromium metal layer and a hydrated chromium oxidelayer formed therein is produced using a focused ion beam (FIB)and observed at a magnification of 20,000X with a transmissionelectron microscope (TEM). The vertical distance from the flatplate portion of the chromium metal layer to the apex of theprotrusion portion is measured for all the protrusion portionsin the observation field of view. This measurement is performedin five fields of view for each steel sheet for cans, and themaximum value in the measurement result is taken as the height Hof the protrusion portion of the steel sheet for cans (see FIG.1).
[0025] Similarly, a cross-sectional sample of a steel sheet forcans is observed with TEM, and the distance of the portion(bottom portion) where the protrusion portion is in contact withthe flat plate portion in the chromium metal layer is measuredfor all the protrusion portions in the observation field ofview. This measurement is performed in five fields of view foreach steel sheet for cans, and the maximum value in themeasurement result is taken as the bottom diameter D of theprotrusion portion of the steel sheet for cans (see FIG. 1).
[0026] (Area Fraction) When the area fraction of the protrusion portions is high,the current-carrying points increase in number, resulting inexcellent weldability. Therefore, the area fraction of the protrusion portions is5% or more, preferably 10% or more, and more preferably 20% ormore. The upper limit of the area fraction of the protrusionportions is not particularly limited, and may be 100%.
[0027] ((Method for Measuring Area Fraction)) The area fraction of the protrusion portions is determinedas follows. First, a surface of the steel sheet for cans having achromium metal layer and a hydrated chromium oxide layer formedtherein is subjected to carbon deposition to obtain anobservation sample. Next, the observation sample is observedusing a scanning electron microscope (SEM) to obtain an SEMimage at a magnification of 20,000X. For the obtained SEM image, the protrusion portion isbinarized and subjected to image analysis using software (tradename: ImageJ), and the area fraction (unit: %) of the protrusionportions is determined. The area fraction is an average of fivefields of view.
[0028] <Hydrated Chromium Oxide Layer> A hydrated chromium oxide is deposited along with chromiummetal on a surface of the steel sheet and improves corrosionresistance. The hydrated chromium oxide includes, for example,chromium oxide and chromium hydroxide.
[0029] <<Coating Weight>> For the reason that the corrosion resistance of the steelsheet for cans is secured, the coating weight of the hydratedchromium oxide layer in terms of chromium is 3 mg / m2 or more andpreferably 4 mg / m2 or more.
[0030] Meanwhile, the hydrated chromium oxide is inferior tochromium metal in conductivity, and accordingly, too much amountthereof leads to excessive resistance in welding, which maycause generation of dust, occurrence of splash, and a variety ofweld defects such as blowhole formation associated withoverwelding, thus resulting in poor weldability of the steelsheet for cans. For the reason that the weldability of the steel sheet forcans is excellent, the coating weight of the hydrated chromiumoxide layer in terms of chromium is 50 mg / m2 or less, preferably40 mg / m2 or less, and more preferably 30 mg / m2 or less.
[0031] The method for measuring the coating weight of the hydratedchromium oxide layer in terms of chromium is as described above.
[0032] [Method for Manufacturing Steel Sheet for Cans] Next, a method for manufacturing the steel sheet for cansof the present embodiment (hereinafter, also referred to as"present manufacturing method" for convenience) will bedescribed. In the present manufacturing method, generally, a steelsheet is subjected to an immersion treatment with use of anaqueous solution 1 containing a water-soluble organic compound,and then subjected to a cathodic electrolysis treatment with useof an aqueous solution 2 containing a hexavalent chromiumcompound, a fluorine-containing compound, and sulfuric acid. Asa result, a chromium metal layer and a hydrated chromium oxidelayer are formed on the surface of the steel sheet, and,further, protrusion portions are formed on the chromium metallayer.
[0033] The reason for this is presumed as follows. In the immersion treatment, the steel sheet is immersed inthe aqueous solution 1. At this time, the water-soluble organiccompound is randomly adsorbed on the surface of the steel sheet.As a result, deposition (electrodeposition) of chromium metal isinhibited in the cathodic electrolysis treatment to besubsequently performed. Then, chromium metal is preferentiallydeposited at a portion where the water-soluble organic compoundis not adsorbed, whereby protrusion portions are formed on thechromium metal layer.
[0034] In this way, a steel sheet for cans having protrusionportions can be manufactured by a simple method of onlyperforming an immersion treatment and a cathodic electrolysistreatment without adopting a method of performing an anodicelectrolysis treatment in the middle of a cathodic electrolysistreatment (see Patent Literature 1).
[0035] <Aqueous Solution 1> The aqueous solution 1 used in the immersion treatmentcontains a water-soluble organic compound.
[0036] <<Water-Soluble Organic Compound>> Examples of the water-soluble organic compound includesaccharin, 2-butine-1,4-diol, oxalic acid, imidazole, sodiumdodecyl sulfate, thiouric acid, and methanesulfonic acid.
[0037] Aside from these, as the water-soluble organic compound, awater-soluble polymer is suitable for the reason that depositionof chromium metal can be effectively inhibited because thewater-soluble polymer has many adsorption starting points to thesteel sheet and is bulky. Examples of the water-soluble polymerinclude polyethylene glycol, poly(meth)acrylic acid, polyvinylalcohol, polyethyleneimine, and polyvinylpyrrolidone. Among them, for the reason that stability in the aqueoussolution 1 is excellent and an adsorption force to a steel sheetis high due to a carboxy group, poly(meth)acrylic acid ispreferable and polyacrylic acid is more preferable.
[0038] (Content) When the content of the water-soluble organic compound istoo small, the amount of the water-soluble organic compoundadsorbed to the steel sheet is insufficient, so that theprotrusion portions may be hardly formed. Therefore, the content of the water-soluble organiccompound in the aqueous solution 1 is preferably 0.1 g / L ormore, more preferably 0.3 g / L or more, and even more preferably0.5 g / L or more.
[0039] On the other hand, when the content of the water-solubleorganic compound is too large, an excessive amount of the watersoluble organic compound is adsorbed to the steel sheet, so thatthe height H of the protrusion portion to be formed may becomeexcessively large. Therefore, the content of the water-soluble organiccompound in the aqueous solution 1 is preferably less than 10g / L, more preferably 8 g / L or less, even more preferably lessthan 8 g / L, and particularly preferably 5 g / L or less.
[0040] (Weight Average Molecular Weight of Water-Soluble Polymer) When the water-soluble organic compound is a water-solublepolymer, and when the weight average molecular weight (Mw) ofthe water-soluble polymer is too small, the number of adsorptionstarting points per one molecule of the water-soluble polymerdecreases. Hence, the steel sheet may not be sufficientlyadsorbed, and the protrusion portions may be hardly formed. Therefore, the Mw of the water-soluble polymer ispreferably 300 or more, more preferably 500 or more, and evenmore preferably 1,000 or more.
[0041] On the other hand, when the Mw of the water-soluble polymeris too large, the water-soluble polymer itself may be entangled,and the starting points at which the water-soluble polymer canbe adsorbed to the steel sheet may decrease. Also in this case,the water-soluble polymer may not be sufficiently adsorbed tothe steel sheet, and hence the protrusion portions may be hardlyformed. Therefore, the Mw of the water-soluble polymer ispreferably 100,000 or less, more preferably 50,000 or less, andeven more preferably 20,000 or less.
[0042] The weight average molecular weight (Mw) is a weightaverage molecular weight in terms of polystyrene as measured bygel permeation chromatography (GPC) performed under thefollowing conditions. - Device: HLC8020 (manufactured by Tosoh Corporation) - Column: three columns of TSKgelGMHXL connected in series - Medium: tetrahydrofuran- Flow rate: 1 mL / min - Concentration: 4 mg / 10 mL - Injection volume: 0.1 mL - Column temperature: 40°C
[0043] The liquid temperature of the aqueous solution 1 ispreferably 20°C or higher and more preferably 40°C or higher. Meanwhile, the liquid temperature of the aqueous solution 1is preferably 80°C or lower and more preferably 60°C or lower.
[0044] <Immersion Treatment> In the immersion treatment, the steel sheet is immersed inthe aqueous solution 1. As a result, the water-soluble organiccompound is adsorbed to the surface of the steel sheet. When the time for immersing the steel sheet in the aqueoussolution 1 (immersion time) is too short, the water-solubleorganic compound may not be sufficiently adsorbed to the surfaceof the steel sheet, and the protrusion portions may be hardlyformed. Therefore, the immersion time is preferably 1 second orlonger, more preferably 5 seconds or longer, and even morepreferably 10 seconds or longer. The upper limit of the immersion time is not particularlylimited. In the meantime, when the immersion time is too long,the surface state of the steel sheet may be altered. Therefore,the immersion time is preferably 300 seconds or shorter, morepreferably 180 seconds or shorter, and even more preferably 60seconds or shorter.
[0045] <Aqueous Solution 2> The aqueous solution 2 used in the cathodic electrolysistreatment contains a hexavalent chromium compound, a fluorinecontaining compound, and sulfuric acid. In the aqueous solution 2, the fluorine-containing compoundand sulfuric acid are present in a dissociated state (that is,as fluoride ions, sulfate ions, and hydrogen sulfate ions).These serve as catalysts involved in a reduction reaction ofhexavalent chromium ions present in the aqueous solution 2,which reduction reaction proceeds in the cathodic electrolysistreatment. When the aqueous solution 2 used in the cathodicelectrolysis treatment contains a fluorine-containing compoundand sulfuric acid, the coating weight of the hydrated chromiumoxide layer in terms of chromium on the steel sheet for cans tobe obtained can be reduced. The reason for this is not clear,but it is conceivable that the amount of hydrated chromium oxideproduced decreases as the amount of anions during theelectrolysis treatment increases.
[0046] <<Hexavalent Chromium Compound>> Examples of the hexavalent chromium compound includechromium trioxide (CrO3); dichromates such as potassiumdichromate (K2Cr2O7); and chromates such as potassium chromate(K2CrO4). The content of the hexavalent chromium compound, as theamount of Cr, in the aqueous solution 2 is preferably 0.14 mol / Lor more and more preferably 0.30 mol / L or more. Meanwhile, the content of the hexavalent chromium compound,as the amount of Cr, in the aqueous solution 2 is preferably3.00 mol / L or less and more preferably 2.50 mol / L or less.
[0047] <<Fluorine-Containing Compound>> Examples of the fluorine-containing compound includehydrofluoric acid (HF), potassium fluoride (KF), sodium fluoride(NaF), hydrosilicofluoric acid (H2SiF6), and a salt ofhydrosilicofluoric acid. Examples of the salt of hydrosilicofluoric acid includesodium silicofluoride (Na2SiF6), potassium silicofluoride(K2SiF6), and ammonium silicofluoride ((NH4)2SiF6). The content of the fluorine-containing compound, as theamount of F, in the aqueous solution 2 is preferably 0.02 mol / Lor more and more preferably 0.08 mol / L or more. Meanwhile, the content of the fluorine-containing compound,as the amount of F, in the aqueous solution 2 is preferably 0.48mol / L or less and more preferably 0.40 mol / L or less.
[0048] <<Sulfuric Acid>> A part or all of sulfuric acid (H2SO4) may be a sulfatesuch as sodium sulfate, calcium sulfate, or ammonium sulfate. The content of sulfuric acid, as the amount of SO42-, in the aqueous solution 2 is preferably 0.0001 mol / L or more, morepreferably 0.0003 mol / L or more, and even more preferably 0.0010mol / L or more. Meanwhile, the content of sulfuric acid, as the amount ofSO4 2-, in the aqueous solution 2 is preferably 0.1000 mol / L orless and more preferably 0.0500 mol / L or less.
[0049] The liquid temperature of the aqueous solution 2 ispreferably 20°C or higher and more preferably 40°C or higher. Meanwhile, the liquid temperature of the aqueous solution 2is preferably 80°C or lower and more preferably 60°C or lower.
[0050] <Cathodic Electrolysis Treatment> The cathodic electrolysis treatment deposits chromium metaland hydrated chromium oxide. When the current density of the cathodic electrolysistreatment is too low, the deposition efficiency of chromiummetal is reduced, and the proportion of the hydrated chromiumoxide layer tends to be high. Therefore, the current density of the cathodic electrolysistreatment is preferably 10 A / dm2 or more, more preferably 15A / dm2 or more, and even more preferably 20 A / dm2 or more.
[0051] On the other hand, when the current density of the cathodicelectrolysis treatment is too high, the protrusion portions aredeposited rapidly, and the height H and / or the bottom diameter Dof the protrusion portion may become excessively large. Therefore, the current density of the cathodic electrolysistreatment is preferably 200 A / dm2 or less and more preferably 150A / dm2 or less.
[0052] The current application time and the electric quantitydensity (product of the current density and the currentapplication time) of the cathodic electrolysis treatment areappropriately set in order to obtain a target coating weight.[EXAMPLES]
[0053] Hereinafter, the present invention will be specificallydescribed with reference to Examples. However, the presentinvention is not limited to the following Examples.
[0054] <Production of Steel Sheet for Cans> A steel sheet (tempered grade: T4CA) produced to have asheet thickness of 0.22 mm was subjected to normal degreasingand pickling. This steel sheet was subjected to the immersion treatmentwith use of the aqueous solution 1, and then subjected to thecathodic electrolysis treatment with use of the aqueous solution2. Details of the aqueous solution 1 and the aqueous solution 2used, and conditions of the immersion treatment and the cathodicelectrolysis treatment performed are shown in Table 1 below. Meanwhile, as to Comparative Example 1, since the immersiontreatment was not performed, "-" was described in the columns of"Aqueous solution 1" and "Immersion treatment" in Table 1 below.
[0055] In the aqueous solution 1, the water-soluble organiccompound shown in Table 1 was contained. When the water-solubleorganic compound was not a water-soluble polymer, "-" wasdescribed in the column of "Mw" in Table 1 below. In the aqueous solution 2, chromium trioxide (CrO3), sodiumfluorosilicate (Na2SiF6), and sulfuric acid (H2SO4) werecontained.
[0056] The aqueous solution was circulated by a pump at a rateequivalent to 100 mpm in a fluid cell. A lead electrode was usedin the cathodic electrolysis treatment. In this way, a steel sheet for cans was produced. Theproduced steel sheet for cans was rinsed with water and dried atroom temperature using a blower.
[0057] <Coating Weight and others> For the produced steel sheet for cans, the coating weightof the chromium metal layer and the coating weight of thehydrated chromium oxide layer in terms of chromium (simplyreferred to as "coating weight" in Table 1 below) were measured. For the protrusion portions of the chromium metal layer ofthe produced steel sheet for cans, the height H, the bottomdiameter D, the ratio (H / D), and the area fraction weremeasured. The measurement methods are as described above. Theresults are shown in Table 1 below.
[0058] <Evaluation> For the produced steel sheet for cans, the following testswere performed, and weldability and surface appearance wereevaluated. The results are shown in Table 1 below.
[0059] <<Weldability>> The produced steel sheet for cans was subjected to a heattreatment of 210°C x 10 minutes (held at a target sheettemperature of 210°C for 10 minutes) once, and then the contactresistance was measured. More specifically, first, two samples were collected fromthe steel sheet for cans, subjected to the heat treatment in abatch furnace, and then superposed after the heat treatment. Subsequently, the two superposed samples were sandwiched byusing 1 mass% Cr-Cu electrodes of DR type (electrodes processedto have a tip diameter of 6 mm and a curvature of R40 mm) andretained at a pressure of 1 kgf / cm2 for 15 seconds. Thereafter, the samples were energized at a current valueof 10 A, and the resistance value (unit: μΩ) between the twosamples was measured. The resistance value was measured at 10points, the average value was taken as the contact resistancevalue, and the weldability was evaluated according to thefollowing criteria. The case of "Superior", "Excellent", or"Good" was evaluated to be excellent in weldability. Superior: Contact resistance value of 100 μΩ or less Excellent: Contact resistance value of more than 100 μΩ and300 μΩ or less Good: Contact resistance value of more than 300 μΩ and 500μΩ or less Fair: Contact resistance value of more than 500 μΩ and 1000μΩ or less Poor: Contact resistance value of more than 1000 μΩ
[0060] <<Surface Appearance>> For the produced steel sheet for cans, the b value wasmeasured according to the Hunter-type color differencemeasurement defined in JIS Z 8730 of old version (1980) and thesurface appearance was evaluated according to the followingcriteria. The case of "Excellent" or "Good" was evaluated to beexcellent in surface appearance. Excellent: b value ≤ 0 Good: 0 < b value ≤ 2.0 Fair: 2.0 < b value ≤ 3.0 Poor: 3.0 < b value
[0061] [Table 1]Table 1 (1 / 2)Table 1 (2 / 2)CE: Comparative ExampleIE: Inventive Example
[0062] <Summary of Evaluation Results> As shown in Table 1 above, it was found that InventiveExamples 1 to 25 were excellent in weldability and surfaceappearance. On the other hand, in Comparative Examples 1 to 8,at least one of weldability or surface appearance wasinsufficient. More specifically, the evaluation results were as follows.
[0063] <<Comparative Example 1>> In Comparative Example 1 in which the immersion treatmentwas not performed, the protrusion portions of the chromium metallayer were not formed, and the weldability was insufficient.
[0064] <<Comparative Example 2 and Inventive Examples 1 to 3>> Comparative Example 2 and Inventive Examples 1 to 3 aredifferent from each other only in the content of the watersoluble organic compound (polyacrylic acid) in the aqueoussolution 1. In Comparative Example 2 in which the content of the watersoluble organic compound was 0.05 g / L, the height H of theprotrusion portion was not 10 nm or more, and the weldabilitywas insufficient. Comparing Inventive Examples 1 to 3, Inventive Examples 2and 3 in which the height H of the protrusion portion was 50 nmor more had more favorable weldability than Inventive Example 1not satisfying that range.
[0065] <<Comparative Example 3, Inventive Examples 4 to 10, andComparative Example 4>> Comparative Example 3, Inventive Examples 4 to 10, andComparative Example 4 are different from each other only in theweight average molecular weight (Mw) of the water-solubleorganic compound (polyacrylic acid) in the aqueous solution 1. In Comparative Example 3 in which the Mw was 200, thebottom diameter D of the protrusion portion was not 50 nm ormore, and the weldability was insufficient. In Comparative Example 4 in which the Mw was 120,000, thearea fraction of the protrusion portions was not 5% or more, andthe weldability was insufficient.
[0066] Comparing Inventive Examples 4 to 10, Inventive Examples 5to 9 in which the height H of the protrusion portion was 50 nmor more and the area fraction of the protrusion portions was 10%or more had more favorable weldability than Inventive Examples 4and 10 not satisfying those ranges.
[0067] Among Inventive Examples 5 to 9, Inventive Example 7 inwhich the height H of the protrusion portion was 200 nm or more,the bottom diameter D of the protrusion portion was 720 nm ormore, and the area fraction of the protrusion portions was 20%or more had more favorable weldability than Inventive Examples5, 6, 8, and 9 not satisfying at least one of those ranges.
[0068] <<Inventive Example 11 and Comparative Example 5>> Similarly to Comparative Example 2 and Inventive Examples 1to 3 described above, Inventive Example 11 and ComparativeExample 5 are different from each other only in the content ofthe water-soluble organic compound in the aqueous solution 1. In Comparative Example 5 in which the content of the watersoluble organic compound was 12 g / L, the height H of theprotrusion portion was not less than 500 nm, the ratio (H / D) wasnot less than 0.50, and the surface appearance was insufficient.
[0069] Comparing Inventive Example 11 and Inventive Examples 1 to3 described above, Inventive Examples 1 to 3 in which the bottomdiameter D of the protrusion portion was 800 nm or less had morefavorable surface appearance than Inventive Example 11 notsatisfying that range.
[0070] <<Comparative Example 6, Inventive Examples 12 to 16, andComparative Examples 7 and 8>> Comparative Example 6, Inventive Examples 12 to 16, andComparative Examples 7 and 8 are different from each other onlyin the conditions (such as current density) of the cathodicelectrolysis treatment. In Comparative Example 6 in which the current density was 5A / dm2, the coating weight of the hydrated chromium oxide layer interms of chromium was not 50 mg / m2 or less, and the weldabilitywas insufficient. In Comparative Example 7 in which the current density was220 A / dm2, the bottom diameter D of the protrusion portion wasnot 1000 nm or less, and the surface appearance wasinsufficient. In Comparative Example 8 in which the current density was250 A / dm2, the ratio (H / D) was not less than 0.50, and thesurface appearance was insufficient.
[0071] Comparing Inventive Examples 12 to 16, Inventive Examples13 to 16 in which the coating weight of the hydrated chromiumoxide layer in terms of chromium was 40 mg / m2 or less had morefavorable weldability than Inventive Example 12 not satisfyingthat range. Among Inventive Examples 13 to 16, Inventive Examples 14 to16 in which the coating weight of the hydrated chromium oxidelayer in terms of chromium was 30 mg / m2 or less had morefavorable weldability than Inventive Example 13 not satisfyingthat range.
[0072] Comparing Inventive Examples 12 to 16 again, InventiveExamples 12 and 13 in which the bottom diameter D of theprotrusion portion was 800 nm or less had more favorable surfaceappearance than Inventive Examples 14 to 16 not satisfying thatrange.
[0073] <<Inventive Examples 17 to 19>> Inventive Examples 17 to 19 use polyethylene glycol as thewater-soluble organic compound and are different from each otheronly in the Mw thereof. Inventive Example 18 in which the height H of theprotrusion portion was 200 nm or more, the bottom diameter D ofthe protrusion portion was 720 nm or more, and the area fractionof the protrusion portions was 20% or more had more favorableweldability than Inventive Examples 17 and 19 not satisfying atleast one of those ranges.
[0074] <<Inventive Examples 20 to 25>> Inventive Examples 20 to 25 use other water-soluble organiccompounds. Inventive Example 20 in which the height H of theprotrusion portion was 200 nm or more, the bottom diameter D ofthe protrusion portion was 720 nm or more, and the area fractionof the protrusion portions was 20% or more had more favorableweldability than Inventive Examples 21 to 25 not satisfying atleast one of those ranges.[REFERENCE SIGNS LIST]
[0075] 1: steel sheet for cans 2: steel sheet 3: chromium metal layer 3a: flat plate portion 3b: protrusion portion 4: hydrated chromium oxide layer D: bottom diameter of protrusion portion H: height of protrusion portion
Claims
1. A steel sheet for cans comprising, on a surface of a steel sheet, a chromium metal layer and a hydrated chromium oxide layer stacked in this order from a side closer to the steel sheet, wherein a coating weight of the chromium metal layer is 50 to 200 mg / m2, a coating weight of the hydrated chromium oxide layer in terms of chromium is 3 to 50 mg / m2, the chromium metal layer includes a flat plate portion and protrusion portions provided on the flat plate portion, a height H of each of the protrusion portions is 10 nm or more and less than 500 nm, a bottom diameter D of each of the protrusion portions is 50 nm or more and 1000 nm or less, a ratio H / D of the height H and the bottom diameter D is less than 0.50, and an area fraction of the protrusion portions is 5% or more.
2. A method for manufacturing the steel sheet for cans according to claim 1, the manufacturing method comprising subjecting a steel sheet to an immersion treatment with use of an aqueous solution 1 and then to a cathodic electrolysis treatment with use of an aqueous solution 2, wherein the aqueous solution 1 contains a water-soluble organic compound, and the aqueous solution 2 contains a hexavalent chromium compound, a fluorine-containing compound, and sulfuric acid.
3. The method according to claim 2 for manufacturing the steel sheet for cans, wherein a content of the water-soluble organic compound in the aqueous solution 1 is 0.1 g / L or more and less than 10 g / L.
4. The method according to claim 2 or 3 for manufacturing the steel sheet for cans, wherein the water-soluble organic compound is a water-soluble polymer having a weight average molecular weight of 300 to 100,000.
5. The method according to claim 4 for manufacturing the steel sheet for cans, wherein the water-soluble polymer is polyacrylic acid.
6. The method according to claim 2 or 3 for manufacturing the steel sheet for cans, wherein a current density of the cathodic electrolysis treatment is 10 to 200 A / dm2.
7. The method according to claim 4 for manufacturing the steel sheet for cans, wherein a current density of the cathodic electrolysis treatment is 10 to 200 A / dm2.
8. The method according to claim 5 for manufacturing the steel sheet for cans, wherein a current density of the cathodic electrolysis treatment is 10 to 200 A / dm2.