Biodegradable nanofiber and a method of fabrication thereof
Patent Information
- Application Number
- IN202521091072
- Authority / Receiving Office
- IN · IN
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2025-09-23
- Publication Date
- 2026-10-09
- Estimated Expiration
- 2045-09-23
AI Technical Summary
Existing air filtration technologies face challenges such as high initial capital and operational costs, limited particle capture efficiency, noise generation, significant energy consumption, and environmental impact due to non-biodegradable materials that contribute to waste and carbon emissions.
A method for fabricating biodegradable nanofibers from waste banana peels using a reducing agent solution, followed by electrospinning with a biopolymer to create a filter medium that can be reused and eventually biodegraded, utilizing a sustainable electrospinning process.
The biodegradable nanofibers achieve high particulate matter removal efficiency, reduce environmental burden, and support sustainable development goals by being regenerable and eco-friendly, with the residual biomass used as a soil ameliorant to enhance soil moisture retention.
Abstract
Description
FIELD OF INVENTION
[0001] The present invention relates to air filtration and, more particularlyto a biodegradable nanofiber and a method of fabrication thereof from food wastematerials.BACKGROUND OF THE INVENTION
[0002] Air pollution poses a substantial risk to human health and theenvironment. According to the World Health Organization (WHO), more than 99%of the global population resides in areas where air quality levels exceed thepermissible limits established by the WHO guidelines. Prolonged exposure topolluted air is associated with an elevated risk of various health conditions,including cardiovascular disease, respiratory disorders such as asthma,cerebrovascular events, and lung cancer. Indoor air pollution is also recognized asa major contributor to adverse health outcomes, particularly in regions whereinefficient combustion technologies and low-quality fuels are used for domesticpurposes. Women and children bear a disproportionate share of the health burdendue to extended exposure during household activities.
[0003] Therefore, effective air filtration is critical for maintaining healthyindoor environments. However, existing air filtration technologies present severaltechnical and environmental challenges. These include high initial capitalrequirements, ongoing maintenance and operational costs, limited particle captureefficiency, noise generation during operation, and significant energy consumption.Additionally, most commercially available air filters are fabricated from non-biodegradable materials. Once spent, these filters contribute to the solid wastestream, creating end-of-life disposal issues and adding to the environmental burdenby occupying landfill space and increasing carbon emissions. These limitationsunderscore the need for improved air filtration solutions that are efficient,sustainable, and environmentally responsible.
[0004] In accordance with one of the prior art document, a complex multi-step method for extraction of multi-scale cellulose nanofibers via mechanical (e.g.,steam explosion) and chemical (alkali and organic solvent) has been disclosed.Further incorporates antibacterial fiber integration using polychitosin and ramiefibers. However, the prior art has not addressed the durability and reusability of thenasal plug filter.
[0005] Therefore, there remains a need for low-cost, regenerable, andbiodegradable filter media that can be used multiple times after exhaustion and arecapable of undergoing eventual biodegradation.OBJECT OF THE INVENTION
[0006] It is the primary object of the present disclosure to provide a methodfor fabricating a biodegradable nanofiber.
[0007] It is yet another object of the present disclosure to provide abiodegradable nanofiber.
[0008] It is yet another object of the present disclosure to provide abiodegradable air filter.SUMMARY OF THE INVENTION
[0009] In an aspect of the present disclosure, a method for fabricating abiodegradable nanofiber is disclosed. The method comprises the steps of grindingwaste banana peels with a reducing agent solution to obtain a fibrous slurry,followed by filtering the resulting slurry with a double-layered muslin cloth andsieving the filtrate through a 120 to 80 mesh screen to obtain a slurry filtrate, thensedimenting the filtrate at a temperature ranging from 15°C to 20°C for a timeperiod ranging from 6 hours to 8 hours and removing the settled semi-solid filtrateresidue by decanting the supernatant, followed by washing the semi-solid filtrateresidue 2 to 3 times with deionized water, and centrifuging the washed filtrateresidue for 500 to 1000 rpm thereby generating an extract, then dissolving theextract in a biopolymer solution with constant stirring for a time period rangingfrom 6 to7 hours at 200 rpm to 500 rpm to form a polymeric solution, followed byelectrospinning the polymeric solution at a temperature ranging from 20 to 25 °Cwith the polymeric solution being pumped at a flow rate ranging from 1 to 2mL / hour using a syringe pump through a needle at an applied electric potentialranging from 18 to 23 kV and finally collecting the fabricated electrospunnanofibers on a rotating drum collector wrapped in aluminium sheet, rotating at aspeed in the range of 200 to 300 rpm, along with a translational movement rangingfrom 0.5 to 0.82 m / min.
[0010] In yet another aspect of the present disclosure, a biodegradablenanofiber, comprising an electrospun polymeric solution comprising an extractderived from waste banana peels dissolved in biopolymer solution such that theweight / weight ratio of extract derived from banana peel to the biopolymer is in therange of 0.5 / 1 to 1 / 1.
[0011] These and other object, features and advantages will becomeapparent to those of ordinary skill in the art from a reading of the following detaileddescription.BRIEF DESCRIPTION OF DRAWINGS
[0012] The exemplary embodiments of the present invention have beendescribed with reference to the accompanying figures.
[0013] Figure 1 illustrates a flow chart depicting the method for fabricatinga biodegradable nanofiber in accordance with an embodiment of the presentdisclosure.
[0014] Figure 2 illustrates a schematic representation of a custom-madecontinuous flow air filtration setup for testing nanofibrous air filters pressure dropand filtration efficiency, in accordance with an embodiment of the presentinvention.
[0015] Figure 3 illustrates a tabular representation of the fiber diameter,maximum load, contact angle, effective surface area, pressure drop, filtrationefficiency, quality factor and food waste incorporation percentage in thebiodegradable nanofibers, in accordance with an embodiment of the presentdisclosure.
[0016] Figure 4 (a) illustrates SEM images of PVA (10%), BPE / PVA (1:2),and BPE / PVA (2:2) electrospun nanofibers, in accordance with an embodiment ofthe present disclosure.
[0017] Figure 4 (b) illustrates diameter distribution of PVA (10%),BPE / PVA (1:2), and BPE / PVA (2:2) electrospun nanofibers, in accordance with anembodiment of the present disclosure.
[0018] Figure 4 (c) illustrates water contact angle of PVA (10%), BPE / PVA(1:2), and BPE / PVA (2:2) electrospun nanofibers, in accordance with anembodiment of the present disclosure.
[0019] Figure 4 (d) illustrates Three Dimensional (3D) images of AtomicForce Microscopy (AFM) of PVA (10%), BPE / PVA (1:2), and BPE / PVA (2:2)electrospun nanofibers, in accordance with an embodiment of the presentdisclosure.
[0020] Figure 4 (e) illustrates tensile strength profiles of PVA (10%),BPE / PVA (1:2), and BPE / PVA (2:2) electrospun nanofibers, in accordance with anembodiment of the present disclosure.
[0021] Figure 4 (f) illustrates FTIR image of PVA (10%), BPE / PVA (1:2),BPE / PVA (2:2) electrospun nanofibers and BPE waste, in accordance with anembodiment of the present disclosure.
[0022] Figure 5 (a) illustrates SEM image of BPE / PVA nanofiber beforeand after filtration and after regeneration and schematic understanding ofregeneration and reuse upto 3 cycles, in accordance with an embodiment of thepresent disclosure.
[0023] Figure 5 (b) illustrates pressure drop profile of regenerated nanofiberwith smoke particles, in accordance with an embodiment of the present disclosure.
[0024] Figure 6 (a) illustrates the banana peel extract waste (BPEW) andsoil particles at a 177 to 500 μm size range, in accordance with an embodiment ofthe present disclosure.
[0025] Figure 6 (b) illustrates the soil water holding capacity test at equalvolume and equal weight, in accordance with an embodiment of the presentdisclosure.
[0026] Figure 6 (c) illustrate a graphic representation of comparison of soilwater retention (SWR) with only soil and soil-BPEW mix, in accordance with anembodiment of the present disclosure.DETAILED DESCRIPTION OF THE INVENTION
[0027] The invention will be described in detail below with reference to thedrawings and specific embodiments. This embodiment is implemented on thepremise of the technical solution of the present invention, and detailedimplementation manners and specific operation procedures are given, but the scopeof the protection of the present invention is not limited to the followingembodiments.
[0028] In an embodiment of the present disclosure, a sustainable fabricationof a biodegradable electrospun nanofibers (ENs) derived from food waste,specifically waste raw banana peel is disclosed. The present disclosure addressesthe solid waste challenge by converting food waste into valuable filter mediaprecursors and replacing conventional non-biodegradable filters, thereby reducingcarbon footprint and enhancing eco-friendliness and cost-effectiveness.
[0029] Referring to Figure 1, illustrates a flow chart depicting the methodfor fabricating a biodegradable nanofiber, in accordance with the present disclosure.The method comprises the step of grinding waste banana peels with a reducingagent solution to obtain a fibrous slurry, followed by filtering the resulting slurrywith a double-layered muslin cloth and sieving the filtrate through a 120 to 80 meshscreen to obtain a slurry filtrate, then sedimenting the filtrate at a temperatureranging from 15°C to 20°C for a time period ranging from 6 hours to 8 hours andremoving the settled semi-solid filtrate residue by decanting the supernatant,followed by washing the semi-solid filtrate residue 2 to 3 times with deionizedwater, and centrifuging the washed filtrate residue for 500 to 1000 rpm therebygenerating an extract, then dissolving the extract in a biopolymer solution withconstant stirring for a time period ranging from 6 to7 hours at 200 rpm to 500 rpmto form a polymeric solution, followed by electrospinning the polymeric solution ata temperature ranging from 20 to 25 °C with the polymeric solution being pumpedat a flow rate ranging from 1 to 2 mL / hour using a syringe pump through a needleat an applied electric potential ranging from 18 to 23 kV and finally collecting thefabricated electrospun nanofibers on a rotating drum collector wrapped inaluminium sheet, rotating at a speed in the range of 200 to 300 rpm, along with atranslational movement ranging from 0.5 to 0.82 m / min.
[0030] In an embodiment of the present disclosure, the weight / weight ratioof the extract derived from banana peel to the biopolymer is in the range of 0.5 / 1 to1 / 1.
[0031] In an embodiment of the present disclosure, during the step ofcollecting the fabricated electrospun nanofiber, the distance between the spinneretand the collector is fixed in the range of 8 to 12 cm.
[0032] In an embodiment of the present disclosure, the biopolymer solutioncomprises a biopolymer selected from polyvinyl alcohol, polylactic acid,polysaccharides.
[0033] In an embodiment of the present disclosure, the biopolymer solutionis a polyvinyl alcohol solution at a concentration ranging from 8% w / v to 10% w / v.
[0034] In an embodiment of the present disclosure, the reducing agentsolution is selected from sodium bisulfite, sodium sulphite.
[0035] In an embodiment of the present disclosure, the reducing agentsolution is sodium bisulfite solution with a concentration in a range of 0.025% to0.05% w / v.
[0036] In an embodiment of the present disclosure, the biodegradablenanofibers have a fiber diameter in the range of 100 to 150 nm.
[0037] In an embodiment of the present disclosure, the biodegradablenanofibers have a particulate matter (PM) removal efficiency in the range of 98%to 99%.
[0038] In an embodiment of the present disclosure, a biodegradablenanofiber comprising an electrospun polymeric solution comprising an extractderived from waste banana peels dissolved in a biopolymer solution. Theweight / weight ratio of the extract derived from banana peel to the biopolymer is inthe range of 0.5 / 1 to 1 / 1.
[0039] In yet another embodiment of the present disclosure, a biodegradableair filter comprises a membrane composed of a biodegradable nanofiber comprisingan electrospun polymeric solution comprising an extract derived from waste bananapeels dissolved in a biopolymer solution is disclosed.Working Examples
[0040] Extraction and polymeric solution formation: Raw bananas werepurchased from the local IIT Bombay market. The peels were manually removed,cut into small pieces, and ground in sodium bisulfite (0.05%, w / v) using a mixergrinder. The resultant slurry was filtered through two layers of muslin cloth, andthe residue fibrous waste was collected. The filtrate was sieved using an 80-meshsize screen and allowed to settle for 24 hours at 4°C. The settled semisolid wasseparated by removing the supernatant, washed 2-3 times, and then subjected tocentrifugation. The recovered extract was added based on weight / weight ratio to a10% poly vinyl alcohol (PVA) solution and dissolved by constant stirring for 6 to7 hours at 200 rpm. The polymeric solution was electrospun using anelectrospinning technique. The solution was filled into a 5 ml syringe with a needlesize of 15G and pumped using a syringe pump at a flow rate of 1 ml / hour with astable electric potential of 23.5 kV. Nanofibers were collected on a rotating drumwrapped with aluminum foil, rotating at 200 rpm with translational movement of0.82 m / min. The distance between the spinneret and collector was fixed at 10 cm.The electrospun nanofiber was formed at room temperature.
[0041] Pressure drop and filtration efficiency tests of the nanofibers:Referring to figure 2, illustrates a schematic representation of a custom-madecontinuous flow air filtration setup for testing nanofibrous air filters pressure dropand filtration efficiency, in accordance with an embodiment of the presentinvention. The pressure drop and filtration efficiency of each nanofiber sample wereevaluated using the custom-made continuous flow air filtration setup. A 0.6 N NaClsolution was used for aerosol generation via an aerosol generator, producing 106particles / cm3 at a flow rate of 5 LPM, with particle sizes ranging from 0.01 to 2 μm.Electrospun nanofibers of specified diameters were inserted between the flange andsecured tightly. The suction flow was maintained at 7.5 LPM. The pressure dropacross the nanofibers was monitored using a differential manometer. Filtrationefficiency (η) was calculated according to Equation (1):Equation (1)where Cinlet and Coutlet are the NaCl aerosol concentrations at the inlet andoutlet of the filters, respectively. Aerosol concentrations were determined bybubbling inlet and outlet air in 100 ml of distilled water for a fixed duration,followed by analysis using ion chromatography. The quality factor (Qf) of eachnanofiber was evaluated using Equation (2):Equation (2) Where ΔP is pressure drop.
[0042] Nanofiber characterization: The morphology of the preparednanofibrous mat was examined by scanning electron microscope (SEM) (JSM7600F, JEOL Ltd.) accelerated with a voltage range of 5-10 kV. A small piece ofthe nanofiber sample was attached to the SEM stub, fixed with carbon tape, andcoated with platinum using a sputter (JFC-1600, JEOL Ltd.) at the conditions of100 V and 10 mA for 120 s. The average diameter of the fabricated nanofibrousmat was evaluated using ImageJ analytical software developed by the NationalInstitute of Health (NIH) by taking 50 readings of the length of the nano-fiber crosssection from each SEM image. Chemical characteristics, composition, andfunctional group interaction between PVA and BPE nanofibers were examined byFourier-transform infrared (FTIR) spectrometer (Vertex 80, Bruker, Germany),single point detector operated at wavenumber range of 4000-450 cm-1. Thedegree of hydrophilicity or surface wettability of various nanofibers wasinvestigated with a water contact angle (WCA) analyser using the drop method(Digidrop, GBX). 1.6 μL of water sample was dropped on the sample, and imageswere automatically captured at different time intervals. Subsequently, the contactangle was evaluated using image analysis software. The tensile strength of the ENwas estimated by a table top universal tensile testing machine (3345, Single columnmodel, Instron) with maximum capacity of 5kN. The nanofiber sample cross-section for tensile testing was 10 cm long and 1.5 cm wide with a stress-strainstretching rate of 0.2 cm / min with a gauge length of 2.5cm. Vernier caliper wasused to measure the thickness of the nanofiber. The sample was inserted into thegripping part of the instrument in the vertical direction, and during the test, thenanofiber sample was stretched up to the breaking point. Atomic force microscopy(AFM) (MFP3D Origin, Asylum / Oxford Instruments, contact and tapping(noncontact) mode, frequency 180 kHz) was used to measure external surfaceroughness, morphology, and effective surface area with topographical features.
[0043] Regeneration of the exhausted nanofiber: For regenerationstudies, the nanofiber were first loaded with the aerosols by exposing them to thesmoke of incense sticks. The setup was equipped with a suction pump of 7.5 LPM.The exhausted filter was meticulously placed into a nanofiber holder, soaked in99.9% ethanol solution for 8-10 h, and then dried at room temperature. The batchprocess of regeneration, recycling, and reuse was continued for three runs, and theairflow resistance was evaluated by measuring the initial pressure drop across theregenerated nanofiber. SEM imaging was also done before and after the filtrationto confirm the regeneration process at the nanoscale.
[0044] Processing of the leftover material after BPE extraction frombanana peels: The fibrous waste material (termed as BPEW (banana peelextractwaste)) obtained after BPE extraction from the banana peel was dried at 35°C for 12 h in a hot air oven (AI-7981, i-therm) and ground into small particles bymixer grinder for soil water retention studies. To ensure uniformity in particle size,both the BPEW and soil particles were sieved within a specific size range of > 30and < 80 mesh sizes. Two different sets of centrifuge tubes were prepared: onecontaining 10 g of soil and 5g of BPEW in 40 ml of water and another with 15 g ofsoil in 40 ml of water. After allowing 24 h for soaking in water, the centrifuge tubeswere centrifugated at 5000 rpm to evaluate water holding capacity. The resultingsupernatant water was collected, and its volume was measured to assess the mediawater retention capacity using Eqs. (3) and (4).Waterretained = Watertotal - Waterremoved (3)Equation (4) Where Water retained is volume of water retained (mL), Water total istotal volume of water added (mL), Water removed is volume of water as supernatantand SWR is soil water retention.Results:
[0045] Banana peel nanofibers exhibited increasing water-repellentcharacteristics with increasing concentration of banana peel extract (BPE),contributing to a lower pressure drop. As the concentration of BPE increased, thepressure drop over time decreased, corresponding to a reduction in nanofiberthickness from 0.14 mm to 0.11 mm. It was observed that banana peel nanofibersachieved a maximum particulate matter (PM) removal efficiency exceeding 98%.Increasing the BPE concentration in the solution enhanced filtration efficiency,attributed to a decrease in average fiber diameter from 130 nm to 112 nm, whichimproved the removal efficiency via diffusion mechanisms for particles smallerthan 0.1 μm.
[0046] Referring to figure 3, illustrating a tabular representation of the fiberdiameter, maximum load, contact angle, effective surface area, pressure drop,filtration efficiency, quality factor and food waste incorporation percentage in thebiodegradable nanofibers, in accordance with an embodiment of the presentdisclosure. In the fabricated biodegradable nanofibers (BPE / PVA), there is areduction in hydrophilic behavior in comparison with neat PVA (10%) nanofiberswith observed water contact angle (WCA) of 44.53° and 48.50° for BPE / PVA (1:2)and BPE / PVA (2:2) respectively. Upon increasing the BPE (2:1 BPE: PVA ratio)dosing in the electrospinning solution, a higher WCA for BPE / PVA nanofibers hasbeen observed, up to 94.76°. The increase in WCA could be attributed to BPE'swater-repellent characteristics due to silica, polyphenols, cellulose, wax, and lipidcontent.
[0047] Further, BPE / PVA nanofibers shows a minimum initial pressuredrop (PD) in the range of 156-160 Pa. Increasing the molar ratio of BPE extract intothe PVA solution decreases the pressure drop of the filters due to the decrease infiber diameter which consequentially increases the effective surface area andsurface roughness. The pressure drop over 60 min filtration time profile withcharacteristics of various nanofiber compositions were also investigated. BPE / PVA(1:2) and BPE / PVA (2:2) nanofiber shows a gradual increment in PD over timefrom 305 to 610 Pa and 190 to 458 Pa, respectively till 30-35 min. However, a slightsteady phase was achieved after 35-40 min with an approximate increment of 100Pa.
[0048] Referring to figures 4(a) to 4 (f) illustrating the materialcharacterization of the nanofibers, in accordance to an embodiment of the presentdisclosure.
[0049] Referring to figure 4(a) illustrates SEM images of PVA (10%),BPE / PVA (1:2), and BPE / PVA (2:2) electrospun nanofibers, in accordance with anembodiment of the present disclosure. With the addition of BPE to PVA (10%)solution, a significant decrease in the average nanofiber diameter for BPE / PVAnanofibers was observed It was observed that increasing the BPE weight from33.33% to 50% gradually decreases the average nanofiber diameter from 130nm to112nm with more beading. The increased conductivity of the polymeric solutioncontributed to the decrease in the average nanofiber diameter of fabricatedelectrospun nanofibers. The increasing conductivity of the solution increases thesurface charge of the solution, which parallelly increases the force due to the electricfield on the jet, and it can effectively stretch and draw the fibres out. This leads tothinner nanofibers during jet stretching. However, it is essential to note that therelationship between solution conductivity and nanofiber diameter is not alwaysstraightforward and can be influenced by other factors, such as the viscosity of thepolymeric solution, surface tension, etc. The viscosity of a polymeric solutiondetermines the ability to flow and controls the stretching and thinning of the jetduring electrospinning. However, if the viscosity is too high, it can offer moreresistance to stretching and thinning, reducing the elongation and resulting in largerdiameter and leading to clogging of the spinneret or other related problems.
[0050] Further it was observed that in the case of BPE / PVA nanofiber,despite the lower despite the lower conductivity of its polymeric solution (0.59 to0.598 mS / cm), the average diameter is between 110 to 130 nm. It is because theviscosity of BPE / PVA solution is lower 842 to 1050 mPa-s which offers lowerresistance to jet thinning and forms thinner nanofibers. Referring to figure 4 (b)illustrates diameter distribution of PVA (10%), BPE / PVA (1:2), and BPE / PVA(2:2) electrospun nanofibers, in accordance with an embodiment of the presentdisclosure.
[0051] Referring to figure 4 (c) illustrates water contact angle of PVA(10%), BPE / PVA (1:2), and BPE / PVA (2:2) electrospun nanofibers, in accordancewith an embodiment of the present disclosure. PVA (10%) nanofibers have goodhydrophilic behavior with a water contact angle (WCA) of 29.34°, which was alsoconfirmed from the broad peak of the hydroxyl group. For BPE / PVA nanofibers,there is a reduction in hydrophilic behavior in comparison with neat PVA (10%)nanofibers with observed WCA of 44.50° and 48.50° for BPE / PVA (1:2) andBPE / PVA (2:2) respectively. The increase in WCA could be attributed to BPE'swater-repellent characteristics due to silica, polyphenols, cellulose, wax, and lipidcontent
[0052] Referring to figure 4 (d) illustrates Three Dimensional (3D) imagesof AFM of PVA (10%), BPE / PVA (1:2), and BPE / PVA (2:2) electrospunnanofibers, in accordance with an embodiment of the present disclosure.
[0053] Referring to figure 4 (e) illustrates tensile strength profiles of PVA(10%), BPE / PVA (1:2), and BPE / PVA (2:2) electrospun nanofibers, in accordancewith an embodiment of the present disclosure. Tensile strength has been determinedfor the nanofibers to assess their applicability in air filter applications and theirability to withstand air pressure. It was observed that the maximum load of PVA(10%) nanofiber is 26 N. The molecular interaction within pure PVA nanofiber ismore robust due to the higher hydrogen bonding between PVA chains. When PVAis mixed with BPE, the interaction between PVA chains is disrupted by the presenceof BPE molecules, creating a heterogeneous structure, leading to a reduction of theoverall tensile strength of electrospun nanofibers. The tensile strength and max loadof BPE / PVA (1:2) and BPE / PVA (2:2) are 4.32 to 1.36 MPa (mega Pascal) and 9.7N to 3.6N, respectively, while BPE / PVA (2:2) experiences over a 50% loadreduction due to an average diameter decrease from 130 nm to 112 nm.
[0054] Figure 4 (f) illustrates FTIR image of PVA (10%), BPE / PVA (1:2),BPE / PVA (2:2) electrospun nanofibers and BPE waste, in accordance with anembodiment of the present disclosure. There is abundant availability of -OH groupsin the fabricated electrospun nanofibers, which make the nanofibers hydrophilic innature. In the range between 1000 to 1500 cm-1 wavenumber for PVA nanofibers,only five peaks are observed. Whereas, in BPE / PVA, there is shift in these peaksand formation of new peaks, confirming the cross-linking between PVA and BPE.In the case of BPE / PVA nanofibers, the hydroxyl group peak range was narrowedcompared to neat PVA ENs, between 3232 to 3398 cm-1 due to the interaction withthe organic compound and changes in the chemical environment of the hydroxylgroup. Also, there are two peaks (at 513 cm-1 and 578 cm-1) observed in BPE / PVA(1:2) and BPE / PVA (2:2) nanofibers in the range of 500 to 600 cm-1, which are dueto the stretching vibrations of silicon oxygen (Si-O) bonds found in BPE.Additionally, Si-O-Si stretching vibrations offer sharp and weak peak at 1010 cm-1observed in BPE and BPE / PVA nanofiber, respectively
[0055] Regeneration of nanofibers: Referring to figure 5 (a) illustratesSEM image of BPE / PVA nanofiber before and after filtration and after regenerationand schematic understanding of regeneration and reuse upto 3 cycles, in accordancewith an embodiment of the present disclosure. The present study focused onchemical cleaning utilizing ethanol for regeneration process, due to ethanol'scompatibility with various nanofiber materials and its ability to dissolvecontaminants without harming the nanofiber structure. Figure 5 (a) illustrates SEMimage of BPE / PVA(1:2) before filtration, after filtration, and after regeneration,and it is evident that appreciable regeneration has been achieved. It is furthercorroborated by the regenerated filter performance in the subsequent cycles as theregenerated nanofiber filter was reused for more than 3 cycles, and airflowresistance was evaluated by measuring initial pressure drop.
[0056] Figure 5 (b) illustrates pressure drop profile of regenerated nanofiberwith smoke particles, in accordance with an embodiment of the present disclosure.It has been observed that the initial pressure drop of the nanofiber increases afterevery run from 280 to 340 Pa. Additionally, the nanofiber color has also changedafter the subsequent cycles, which estimates that a few smoke particles areadhesively attached to the nanofibers. Removal of PMs from incense smoking ismore complicated than test NaCl aerosols because it is considered soft due to watercontent and is carbonaceous, making it more adhesive than inorganic rigid PMs onthe filter media.
[0057] Leftover material utilization: To achieve a materially closed-loopsustainable nanofiber fabrication process, a by-product, i.e., BPEW generated afterthe BPE extraction process, has been utilized as a soil ameliorant. Referring tofigure 6 (a) illustrates the banana peel extract waste (BPEW) and soil particles at a177 to 500 μm size range, in accordance with an embodiment of the presentdisclosure.
[0058] Referring to figure 6 (b) illustrates the soil water holding capacitytest at equal volume and equal weight, in accordance with an embodiment of thepresent disclosure. The SWR of the soil sample containing soil and BPEW shownin Fig. 6 (b) in the ratio of 2:1 (w / w) was 55%, whereas the sample containing onlysoil and no BPEW illustrates a SWR of 22.5% as illustrated in figure 6 (c).Referring to figure 6 (c) illustrate a graphic representation of comparison of soilwater retention (SWR) with only soil and soil-BPEW mix, in accordance with anembodiment of the present disclosure.
[0059] Therefore, adding BPEW into the soil increased its water holdingcapacity by 32.5% at similar granular size and equal weight comparison. An equalvolume of soil mix and only soil samples were compared to make the results morerobust. The soil + BPEW mixture showed 35% SWR while only soil had acorresponding SWR of 15% as illustrated in Fig. 6 (c). The BPEW are rich inorganic matter such as lignin, cellulose, and hemicellulose. Incorporating these intothe soil increases the soil structure and porosity and enhances its water retentioncapacity. These organic matter act as a sponge for holding water over time. Theratio of main biopolymer (BPE) to BPEW is 1:3. Given this significant ratio, theBPEW residue holds potential for utilization as a soil fertilizer as it is rich inphosphorus. Moreover, BPEW in the soil can be helpful in enhancing soil water-holding capacity, particularly under arid conditions and for plants requiring morewater, such as rice, cranberries, willow trees, etc. This approach not only mitigatesthe need for additional processing of the waste material but also presents directapplication to improve soil quality. The reuse of BPEW to increase soil waterholding capacity can be a sustainable and environmentally friendly practice, and itwill close the material loop in nanofiber fabrication from banana peels.
[0060] The present disclosure utilizes a simple and efficient electrospinningtechnique to fabricate an eco-friendly, low-cost, biodegradable electrospunnanofibers characterized by high surface area-to-volume ratio, small pore size,tunable properties, higher uptake capacity and are densely packed, and haveinterconnected pores. These features enable effective air exchange at low pressuredrop and improved particulate matter removal. Significantly, this is the firstdemonstration of regenerating and reusing exhausted banana peel based nanofiberfilter media over multiple cycles, contributing to sustainable production andsupporting sustainable development goals (SDGs). Additionally, residual biomassfrom banana peel extraction is repurposed as a soil ameliorant, which has shownenhanced soil moisture retention, thus promoting a closed-loop, sustainablematerial lifecycle.
[0061] The biodegradable air filters of the present disclosure have beenregenerated and reused in multiple cycles, thereby enhancing the air filter'ssustainable production, reducing the net carbon emission, and contributing tosustainable development goals (SDGs). During biomass extraction from the bananapeel waste, the left-over material was used as soil ameliorant and has beensuccessfully tested for soil moisture retention capabilities. This has led to thedevelopment of a materially closed-loop and sustainable process for BPE / PVAnanofibers fabrication.
[0062] While the present invention has been described above in terms ofspecific embodiments, it is to be understood that the invention is not intended to beconfined or limited to the embodiment disclosed herein.
Claims
1. A method for fabricating a biodegradable nanofiber, comprising the steps of: grinding waste banana peels with a reducing agent solution to obtain a fibrous slurry; filtering the resulting slurry with a double-layered muslin cloth and sieving the filtrate through a 120 to 80 mesh screen to obtain a slurry filtrate; sedimenting the filtrate at a temperature ranging from 15°C to 20°C for a time period ranging from 6 hours to 8 hours and removing the settled semi-solid filtrate residue by decanting the supernatant; washing the semi-solid filtrate residue 2 to 3 times with deionized water, and centrifuging the washed filtrate residue for 500 to 1000 rpm thereby generating an extract; dissolving the extract in a biopolymer solution with constant stirring for a time period ranging from 6 to7 hours at 200 rpm to 500 rpm to form a polymeric solution; electrospinning the polymeric solution at a temperature ranging from 20 to 25 °C with the polymeric solution being pumped at a flow rate ranging from 1 to 2 mL / hour using a syringe pump through a needle at an applied electric potential ranging from 18 to 23 kV; and collecting the fabricated electrospun nanofibers on a rotating drum collector wrapped in aluminium sheet, rotating at a speed in the range of 200 to 300 rpm, along with a translational movement ranging from 0.5 to 0.82 m / min.
2. The method as clamed in claim 1, wherein the weight / weight ratio of the extract derived from banana peel to the biopolymer is in the range of 0.5 / 1 to 1 / 1.
3. The method as claimed in claim 1, wherein during the step of collecting the fabricated electrospun nanofiber, the distance between the spinneret and the collector is fixed in the range of 8 to 12 cm.
4. The method as claimed in claim 1, wherein the biopolymer solution comprises a biopolymer selected from polyvinyl alcohol, polylactic acid, polysaccharides.
5. The method as claimed in claim 1, wherein the biopolymer solution is a polyvinyl alcohol solution at a concentration ranging from 8% w / v to 10% w / v.
6. The method as claimed in claim 1, wherein the reducing agent solution is selected from sodium bisulfite, sodium sulphite.
7. The method as claimed in claim 1, wherein the reducing agent solution is sodium bisulfite solution with a concentration in a range of 0.025% to 0.05% w / v.
8. The method as claimed in claim 1, wherein the biodegradable nanofibers have a fiber diameter in the range of 100 to 150 nm.
9. The method as claimed in claim 1, wherein the biodegradable nanofibers have a particulate matter (PM) removal efficiency in the range of 98% to 99%.
10. A biodegradable nanofiber, comprising: a electrospun polymeric solution comprising an extract derived from waste banana peels dissolved in a biopolymer solution, wherein the weight / weight ratio of extract derived from banana peel to the biopolymer is in the range of 0.5 / 1to 1 / 1.
11. The nanofiber as claimed in claim 10, wherein the biodegradable nanofibers have a fiber diameter in the range of 100 to 150 nm.
12. The nanofiber as claimed in claim 10, wherein the biopolymer solution comprises a biopolymer selected from polyvinyl alcohol, polylactic acid, polysaccharides.
13. The nanofiber as claimed in claim 10, wherein the biopolymer solution is a polyvinyl alcohol solution at a concentration ranging from 8% w / v to 10% w / v.
14. The nanofiber as claimed in claim 10, wherein the biodegradable nanofibers have a particulate matter removal efficiency in the range of 98% to 99%.
15. A biodegradable air filter comprising a membrane composed of a biodegradable nanofiber as claimed in claim 10.