AI Technical Summary
Existing polyamide resin compositions fail to provide excellent mechanical properties, appearance, and self-tapping screw fastening performance, especially when exposed to vibrations, due to inadequate mold processability and dimensional stability.
A polyamide resin composition comprising 75-89% crystalline aliphatic polyamide and 11-25% semi-aromatic polyamide, with fibrous reinforcing materials, carbon black, and a crystallization retarder, optimized for improved mechanical strength, mold processability, and self-tapping properties.
The composition achieves excellent flexural modulus, tensile strain, and appearance, ensuring reliable self-tapping screw fastening without damaging the female thread, even under high tightening torque conditions.
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a polyamide resin composition and a molded article.BACKGROUND
[0002] Since polyamide resins represented by polyamide 6 (hereinafter referred to as "PA6") and polyamide 66 (hereinafter referred to as "PA66") possess excellent mechanical characteristics as well as excellent heat resistance, impact resistance, and chemical resistance, they are widely used in a wide variety of applications, such as automotive parts, electrical parts, electronic parts, and household goods.
[0003] In recent years, in view of economic efficiency and productivity, there has been a strong demand for polyamide resins that demonstrate superior mold processability and secondary processability. Particularly, polyamide resin materials that have both good tap processability for tightening screws and the appearance of a molded article are especially sought after in the market. Moreover, screw tightening used in automobiles is constantly subjected to vibrations, and very high reliability in fastening is demanded. Therefore, a challenge lies in controlling fastening with stable axial force by reducing the influence of variations of the tightening torque.
[0004] PTL 1 discloses a composition containing a crystalline polyamide resin and an amorphous polyamide resin compounded with glass fibers and an acid-modified elastomer, aiming to improve the self-tapping property and appearance while maintaining mechanical strength and heat resistance. However, in view of appearance and screw fastening with high torque, this composition was found to be inadequate for parts exposed to vibrations such as automotive interior and exterior parts.
[0005] PTL 2 discloses a composition containing a fibrous reinforcing material compounded with a crystalline semi-aromatic polyamide as the main component. However, when molded under high-cycle molding conditions that are achieved by elevating the molding temperature and lowering the mold temperature to enhance productivity, the appearance and dimensional stability of a molded article was found to be unsatisfactory.CITATION LISTPatent Literature
[0006] PTL 1: JP 2000-248172 A PTL 2: JP 2015-55538 A SUMMARY(Technical Problem)
[0007] Therefore, in view of the aforementioned problem with the prior art, the present invention is to provide a resin composition and a resin molded article that are excellent in mechanical properties and the appearance of a molded article, and with which a female thread (boss) is not damaged even when a self-tapping screw is tightened with high tightening torque when parts are fastened using the screws.(Solution to Problem)
[0008] Specifically, the present invention is as follows.[1]A polyamide resin composition comprising:75 to 89 parts by mass of (A) a crystalline aliphatic polyamide containing (A-a) at least one selected from the group consisting of a lactam unit having a carbon number of 4 or more and 14 or less and (A-a') an aminocarboxylic acid unit having a carbon number of 4 or more and 14 or less, or (A-b) an aliphatic dicarboxylic acid unit and (A-c) an aliphatic diamine unit; and11 to 25 parts by mass of (B) a semi-aromatic polyamide containing (B-a) a dicarboxylic acid unit containing at least 50 mol% of isophthalic acid and (B-b) a diamine unit, andfurther comprising, with respect to 100 parts by mass of a total of the (A) crystalline aliphatic polyamide and the (B) semi-aromatic polyamide:100 to 200 parts by mass of (C) a fibrous reinforcing material; 0 to 2.5 parts by mass of (D) carbon black; and0.05 to 0.5 parts by mass of (E) a crystallization retarder.[2]The polyamide according to [1], wherein a cold crystallization peak of a molded article, which is obtained by molding a specimen having a thicknessof 0.75 mm at a cylinder temperature of 280 °C and a mold temperature of 90 °C, when a temperature is kept at 30 °C for 3 minutes by differential scanning calorimetry (DSC) and is then increased to 280 °C at 20 °C / min is 2.0 J / g or less.[3] The polyamide resin composition according to [1] or [2], wherein the (A) aliphatic polyamide resin is polyamide 6.[4]The polyamide resin composition according to any one of [1] to [3], wherein the (B) semi-aromatic polyamide contains 75 mol% or more of the isophthalic acid unit in total (B-a) dicarboxylic acid unit constituting the (B) semi-aromatic polyamide.[5]The polyamide resin composition according to any one of [1] to [4], wherein the (B) semi-aromatic polyamide contains 100 mol% of the isophthalic acid unit in the total (B-a) dicarboxylic acid unit constituting the (B) semi-aromatic polyamide.[6]The polyamide resin composition according to any one of [1] to [5], wherein a weight average molecular weight Mw is 10000 ≤ Mw ≤ 40000. [7]The polyamide resin composition according to any one of [1] to [6], wherein a mass ratio Dw / Ew of the (D) carbon black and the (E) crystallization retarder in the polyamide composition is 5 or more and 20 or less. [8]A molded article having an insertion portion for tightening a self-tapping screw, the molded article being produced by molding the polyamide resin composition according to any one of [1] to [7].(Advantageous Effect)
[0009] According to the present invention, a polyamide resin composition is provided which is excellent in flexural modulus, tensile strain, appearance, and provides an excellent self-tapping property of screw fastening when molded into a molded article.DETAILED DESCRIPTION
[0010] Hereinafter, an embodiment for embodying the present invention (hereinafter referred to merely as "the present embodiment") will be described in detail. Note that the present embodiment set forth below is an illustrative embodiment for describing the present invention and is not intended to limit the present invention to the following matter. The present invention can be implemented with appropriate modifications that do not deviate from the gist thereof. In this specification, the term "polyamide" refers to a polymer having amide (-NHCO-) bonds in the main chain.
[0011] <<Polyamide resin composition>> A polyamide resin composition of the present invention includes 75 to 89 parts by mass of (A) a crystalline aliphatic polyamide containing (A-a) at least one selected from the group consisting of a lactam unit having a carbon number of 4 or more and 14 or less and (A-a') an aminocarboxylic acid unit having a carbon number of 4 or more and 14 or less, or (A-b) an aliphatic dicarboxylic acid unit and (A-c) an aliphatic diamine unit; and 11 to 25 parts by mass of (B) a semi-aromatic polyamide containing (B-a) a dicarboxylic acid unit and (B-b) a diamine unit, and further including, with respect to 100 parts by mass of a total of the (A) crystalline aliphatic polyamide and the (B) semi-aromatic polyamide: 100 to 200 parts by mass of (C) a fibrous reinforcing material; 0 to 2.5 parts by mass of (D) carbon black; and 0.05 to 0.5 parts by mass of (E) a crystallization retarder.
[0012] The details of each component of the polyamide resin composition of the present embodiment will be described.
[0013] <(A) Crystalline aliphatic polyamide> Preferably, the (A) crystalline aliphatic polyamide contained in the polyamide resin composition of the present invention contains (A-a) a lactam unit and / or (A-a') an aminocarboxylic acid unit, or (A-b) an aliphatic dicarboxylic acid unit and (A-c) an aliphatic diamine unit.
[0014] ((A-a) Lactam unit and / or (A-a') aminocarboxylic acid unit) The (A) crystalline aliphatic polyamide can contain (A-a) a lactam unit and / or (A-a') an aminocarboxylic acid unit. The inclusion of such units tends to provide polyamides with excellent toughness. The lactam constituting the (A-a) lactam unit and the aminocarboxylic acid constituting the (A-a') aminocarboxylic acid unit are a lactam and an aminocarboxylic acid capableof being polymerized (condensation polymerized), respectively.
[0015] The lactam constituting the (A-a) lactam unit and the aminocarboxylic acid constituting the (A-a') aminocarboxylic acid unit are a lactam and an aminocarboxylic acid having a carbon number of 4 to 14, respectively, and lactams and aminocarboxylic acids having a carbon number of 6 to 12 are preferred.
[0016] Examples of the lactam constituting the (A-a) lactam unit are not limited to the following but include: butyrolactam, pivalolactam, ε-caprolactam, capryrolactam, enanthrolactam, undecanolactam, and laurolactam (dodecanolactam), for example. Of these, ε-caprolactam and laurolactam are preferred, and ε-caprolactam is more preferred. When the (A) crystalline aliphatic polyamide contains (A-a) a lactam unit derived from such a lactam, a polyamide resin composition with excellent toughness tends to be obtained.
[0017] Examples of the aminocarboxylic acid constituting the (A-a') aminocarboxylic acid unit are not limited to the following but include: ω-aminocarboxylic acids and α,ω-amino acids that are a compound in which a lactam is ring-opened.The aminocarboxylic acid is preferably a linear or branched saturated aliphatic carboxylic acid having a carbon number of 4 to 14 in which the ω-position is substituted with an amino group. Examples of such aminocarboxylic acids are not limited to the following but include: 6-aminocaproic acid, 11-aminoundecanoic acid, and 12-aminododecanoic acid, for example. Examples of the aminocarboxylic acid also include para-aminomethylbenzoic acid.
[0018] One lactam may be used or two or more lactams may be used in combination to constitute the (A-a) lactam unit, and one aminocarboxylic acid may be used or two or more aminocarboxylic acids may be used in combination to constitute the (A-a') aminocarboxylic acid.
[0019] ((A-b) Aliphatic dicarboxylic acid unit) Examples of the aliphatic dicarboxylic acid constituting the (A-b) aliphatic dicarboxylic acid unit are not limited to the following but include: linear or branched saturated aliphatic dicarboxylic acids having a carbon number of 3 to 20, such as malonic acid, dimethylmalonic acid, succinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid,2,3-diethylglutaric acid, glutaric acid, 2,2-dimethylglutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, suberinic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosanedioic acid, and diglycolic acid, for example.
[0020] The (A-b) aliphatic dicarboxylic acid unit containing an aliphatic dicarboxylic acid having a carbon number of 6 or more is preferred because the polyamide resin composition tends to have even better heat resistance, flowability, toughness, low water absorption, and stiffness. Examples of the aliphatic dicarboxylic acid constituting the (A-b) aliphatic dicarboxylic acid unit having a carbon number of 6 or more include, but are not particularly limited to, adipic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, and eicosanedioic acid, for example. Of these, adipic acid, sebacic acid, and dodecanedioic acid are preferred in view of the heat resistance, etc. of the polyamide resin composition.One aliphatic dicarboxylic acid may be used alone, or two or more aliphatic dicarboxylic acids may be used in combination to constitute the aliphatic dicarboxylic acid unit.
[0021] Note that the (A) crystalline aliphatic polyamide may further contain a unit derived from a trivalent or higher polyvalent carboxylic acid such as trimellitic acid, trimethynic acid, and pyromellitic acid, as needed, to the extent that the purpose of the present invention is not compromised. One of trivalent or higher polyvalent carboxylic acids may be used alone, or two or more of these may be used in combination.
[0022] ((A-c) Aliphatic diamine unit)The (A-c) aliphatic diamine constituting the aliphatic diamine unit may be linear or branched.Examples of the linear aliphatic diamine constituting the (A-C) aliphatic diamine unit are not limited to the following but include: linear saturated aliphatic diamine having a carbon number of 2 to 20, such as ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, andtridecamethylenediamine, for example.
[0023] Example of the branched aliphatic diamine constituting the (A-c) aliphatic diamine unit having a substituent branched from the main chain are not limited to the following but include: branched saturated aliphatic diamines having a carbon number of 3 to 20, such as 2-methylpentamethylenediamine (also referred to as 2-methyl-1,5-diaminopentane) 2,2,4-trimethyl hexamethylenediamine, 2,4,4-trimethyl hexamethylenediamine, 2-methyl-1,8-octanediamine (also referred to as 2-methyl-octamethylenediamine), and 2,4-dimethyl-octamethylenediamine, for example. Of these, 2-methylpentamethylenediamine and 2-methyl-1,8-octanediamine are preferred, and 2-methylpentamethylenediamine is more preferred. When such an (A-c) aliphatic diamine unit is included, the polyamide resin composition tend to have excellent heat resistance, stiffness, etc.
[0024] The carbon number of the (A-c) aliphatic diamine unit is preferably 6 or more and 12 or less. A carbon number of 6 or more is desirable because excellent heat resistance is achieved, and a carbon number of 12 or less is desirable because excellent crystallinity and release properties are achieved. The carbon number of the (A-c) diamine unit is more preferably 6 or more and 10 or less.One of the (A-c) aliphatic diamine unit may be used alone, or two or more of these may be used in combination.
[0025] Note that the (A) crystalline aliphatic polyamide may further contain a unit derived from a trivalent or higher polyvalent aliphatic amine such as bishexamethylenetriamine, as needed, to the extent that the purpose of the present invention is not compromised.
[0026] A specific example of the (A) crystalline aliphatic polyamide used in the polyamide resin composition of the present invention is polyamide 6 (PA6). PA6 is considered to be a suitable material for automotive parts because of its superiority in terms of mechanical characteristics, appearance, formability, and toughness.
[0027] In the present invention, the content of the (A) crystalline aliphatic polyamide is 75.0 parts by mass or more and 89.0 parts by mass or less, preferably 78.0 parts by mass or more and 85.0 parts by mass or less, morepreferably 80.0 parts by mass or more and 82.0 parts by mass or less, and even more preferably 80.0 parts by mass. When the content of the (A) crystalline aliphatic polyamide is set within the above range, a polyamide resin composition with excellent mechanical characteristics, mold processability, and self-tapping characteristic can be obtained.
[0028] <(B) Semi-aromatic polyamide>The (B) semi-aromatic polyamide is a polyamide containing (B-a) a dicarboxylic acid unit and (B-b) a diamine unit.The (B) semi-aromatic polyamide preferably contains 20 mol% or more and 80 mol% or less of aromatic constituting units, more preferably contains 30 mol% or more and 70 mol% or less of aromatic constituting units, and even more preferably contains 40 mol% or more and 60 mol% or less of aromatic constituting units, with respect to all constituting units of the (B) semi-aromatic polyamide. The term "aromatic constituting unit" as used herein refers to aromatic diamine units and aromatic dicarboxylic acid units.
[0029] ((B-a) Dicarboxylic acid unit)The (B-a) dicarboxylic acid unit may contain, but is not particularly limited to, an aromatic dicarboxylic acid unit, an aliphatic dicarboxylic acid unit, and an alicyclic dicarboxylic acid unit. In particular, the (B-a) dicarboxylic acid unit preferably contains 50 mol% or more and 100 mol% or less, more preferably 65 mol% or more and 100 mol% or less, even more preferably 70 mol% or more and 100 mol% or less, further preferably 75 mol% or more and 100 mol% or less, even further preferably contains 80 mol% or more and 100 mol% or less, most preferably contains 100 mol% of an isophthalic acid unit, which is an aromatic dicarboxylic acid unit, on the basis of total mols of dicarboxylic acids.When the ratio of the isophthalic acid unit in the (B-a) dicarboxylic acid unit is equal to or more than the above lower limit, it tends to be possible to obtain a polyamide resin composition that simultaneously satisfies mechanical characteristics, particularly stiffness upon water absorption, stiffness upon heating, flowability, surface appearance, and the like.The ratio of the above-described isophthalic acid unit can be measured by nuclear magnetic resonance spectroscopy (NMR) or the like.
[0030] -Aromatic dicarboxylic acid unit-Examples of the aromatic dicarboxylic acid constituting the aromaticdicarboxylic acid unit other than the isophthalic acid unit are not limited to the following but include: dicarboxylic acid with aromatic rings such as benzene and naphthalene rings, for example. The aromatic group of the aromatic dicarboxylic acid may be unsubstituted or may have a substituent.Examples of the substituent include, but are not particularly limited to, alkyl groups having a carbon number of 1 to 4, aryl groups having a carbon number of 6 to 10, arylalkyl groups having a carbon number of 7 to 10, halogen groups such as chloro and bromo groups, silyl groups having a carbon number of 1 to 6, and sulfonic acid groups and salts (such as sodium salt) thereof, for example. Specifically, examples are not limited to the following but include: aromatic dicarboxylic acids having carbon numbers of 8 to 20, either unsubstituted or substituted with certain substituents, such as terephthalic acid, naphthalene dicarboxylic acid, 2-chloroterephthalic acid, 2-methyl terephthalic acid, 5-methylisophthalic acid, and sodium 5-sulfoisophthalic acid, for example.One aromatic dicarboxylic acid may be used alone, or two or more aromatic dicarboxylic acids may be used in combination to constitute the aromatic dicarboxylic acid unit.
[0031] -Aliphatic dicarboxylic acid unit- Examples of the aliphatic dicarboxylic acid constituting the aliphatic dicarboxylic acid unit are not limited to the following but include: linear or branched saturated aliphatic dicarboxylic acids having a carbon number of 3 to 20, such as malonic acid, dimethyl malonic acid, succinic acid, 2,2-dimethyl succinic acid, 2,3-dimethyl glutaric acid, 2,2-diethyl succinic acid, 2,3-diethyl glutaric acid, glutaric acid, 2,2-dimethyl glutaric acid, adipic acid, 2-methyl adipic acid, trimethyl adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosanedioic acid, and diglycolic acid, for example.
[0032] -Alicyclic dicarboxylic acid unit-Examples of the alicyclic dicarboxylic acid constituting the alicyclic dicarboxylic acid unit (hereinafter referred to as the "alicyclic dicarboxylic acid unit") are not limited to the following but include: alicyclic dicarboxylic acids having an alicyclic structure with a carbon number of 3 to 10, andalicyclic dicarboxylic acids having an alicyclic structure with a carbon number of 5 to 10 are preferred.Examples of such an alicyclic dicarboxylic acid are not limited to the following but include: 1,4-cyclohexane dicarboxylic acid, 1,3-cyclohexane dicarboxylic acid, and 1,3-cyclopentane dicarboxylic acid. Of these, 1,4-cyclohexane dicarboxylic acid is preferred.One alicyclic dicarboxylic acid may be used alone, or two or more alicyclic dicarboxylic acids may be used in combination to constitute the alicyclic dicarboxylic acid unit.
[0033] Examples of the alicyclic structure of the alicyclic dicarboxylic acid are not limited to the following but include: cycloalkane structures, cycloalkene structures, bicyclic alkane structures, bicyclic alkene structures, polycyclic compound structures, and spiro compound structures, having carbon numbers of 3 to 10. The alicyclic structure in the alicyclic dicarboxylic acid may be unsubstituted or may have a substituent. Examples of the substituent are not limited to the following but include: alkyl groups having a carbon number of 1 to 4, such as methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, and tert-butyl group.
[0034] The (B-a) dicarboxylic acid unit other than the isophthalic acid unit preferably contains an aromatic dicarboxylic acid unit, and more preferably an aromatic dicarboxylic acid having a carbon number of 6 or more.The use of such a dicarboxylic acid tends to improve the mechanical characteristics of the polyamide resin composition, particularly stiffness upon water absorption, stiffness upon heating, flowability, and surface appearance.
[0035] In the present invention, the dicarboxylic acid constituting the (B-a) dicarboxylic acid unit is not limited to the compounds listed as dicarboxylic acids above, but may be any compound equivalent to the above dicarboxylic acids.The term "compound equivalent to a dicarboxylic acid" as used herein refers to a compound that can have a dicarboxylic acid structure similar to the dicarboxylic acid structure derived from the above dicarboxylic acids. Such compounds are not limited to the following but include: anhydrides and halides of dicarboxylic acids.
[0036] In addition, the (B) semi-aromatic polyamide may further contain a unit derived from trivalent or higher polyvalent carboxylic acids such astrimellitic acid, trimethylic acid, and pyromellitic acid, as needed.One of trivalent or higher polyvalent carboxylic acids may be used alone, or two or more of these may be used in combination.
[0037] ((B-b) Diamine unit)The (B-b) diamine unit constituting the (B) semi-aromatic polyamide may contain, but are not particularly limited to, an aromatic diamine acid unit, an aliphatic diamine unit, and an alicyclic diamine unit. Of these, it is preferred that a diamine unit having a carbon number of 4 or more and 10 or less is contained.The total amount of diamine units having a carbon number of 4 to 10 or more is preferably 50 mol% or more and 100 mol% or less, more preferably 80 mol% or more and 100 mol% or less, even more preferably 90 mol% or more and 100 mol% or less, and particularly preferably 100 mol%, per 100 mol% of the total (B-b) diamine units constituting the (B) semi-aromatic polyamide. When the ratio of diamine units having a carbon number of 4 or more and 10 or less in the total diamine units (B-b) is equal to or greater than the above lower limit, the polyamide resin composition tends to simultaneously satisfy mechanical characteristics, particularly stiffness upon water absorption, stiffness under high-temperature use (stiffness upon heating), flowability, surface appearance, and the like.The total amount of the above diamine units having a carbon number of 4 or more and 10 or less can be measured by nuclear magnetic resonance spectroscopy (NMR) or the like.
[0038] - Aliphatic diamine unit - Examples of the aliphatic diamine constituting the aliphatic diamine unit are not limited to the following but include: linear saturated aliphatic diamine having a carbon number of 4 to 20, such as ethylene diamine, propylene diamine, tetramethylene diamine, pentamethylene diamine, hexamethylene diamine, heptamethylene diamine, octamethylene diamine, nonamethylene diamine, decamethylene diamine, undecamethylene diamine, dodecamethylene diamine, and tridecamethylene diamine, for example.
[0039] -Alicyclic diamine unit-Examples of the alicyclic dicarboxylic acid constituting the aliphatic diamine unit (hereinafter, referred to as "aliphatic diamine") are not limited tothe following but include: 1,4-cyclohexane diamine, 1,3-cyclohexane diamine, and 1,3-cyclopentane diamine, for example.
[0040] -Aromatic diamine unit-The aromatic diamine constituting the aromatic diamine unit is not limited as long as it is a diamine containing an aromatic ring, and is exemplified by, for example, meta-xylene diamine.
[0041] Among (B-b) diamine units, aliphatic diamine units are preferred, diamine units having a linear saturated aliphatic group having a carbon number of 4 or more and 10 or less are more preferred, diamine units having a linear saturated aliphatic group having a carbon number of 6 or more and 10 or less are even more preferred, and hexamethylene diamine is still even more preferred.The use of such diamines tends to result in a polyamide resin composition with excellent mechanical characteristics, particularly stiffness upon water absorption, stiffness under high-temperature use (stiffness upon heating), flowability, surface appearance, and the like.Note that one diamine may be used alone, or two or more diamines may be used in combination.
[0042] Note that the (B) semi-aromatic polyamide may further contain trivalent or higher polyvalent aliphatic amines such as bishexamethylene triamine, if necessary.Note that one trivalent or higher polyvalent aliphatic amine may be used alone, or two or more of these may be used in combination.
[0043] As the (B) semi-aromatic polyamide used in the polyamide resin composition, polyamide 6I (polyhexamethyleneisophthalamide), polyamide 9I, and polyamide 10I are preferred, and polyamide 6I is most preferred. Polyamide 6I tends to be compatible with crystalline aliphatic polyamides, resulting in a polyamide resin composition with excellent mechanical characteristics, mold processability, and self-tapping characteristic.
[0044] In the present invention, the content of the (B) semi-aromatic polyamide is preferably 11.0 mass% or more and 25.0 mass% or less, more preferably 15.0 mass% or more and 22.0 mass% or less, even more preferably 18.0 mass% or more and 20.0 mass% or less, and still even more preferably 20.0 mass%. When the content of the (B) semi-aromatic polyamide is set to equal to or more than the above lower limit, it is possible to tighten a tapscrew with high tightening force because the toughness of the (A) crystalline aliphatic polyamide is not compromised, in addition to having good dimensional stability of a self-tap and an increased contact area with the screw. On the other hand, when the content of the (B) semi-aromatic polyamide is set to equal to or less than the above upper limit, reduction in the crystallinity and toughness of the polyamide resin composition can be suppressed and crack destruction before the screw being tightened slips can be prevented.
[0045] <End-capping agent>The ends of the polyamide used in the present invention may capped with a known end-capping agent.Such an end-capping agent can also be added as a molecular weight modifier when the polyamide is produced from the dicarboxylic acid and the diamine mentioned above, and a lactam and / or an aminocarboxylic acid are used as needed.
[0046] Examples of the end-capping agent are not limited to the following but include: monocarboxylic acids, monoamines, acid anhydrides such as phthalic anhydride, monoisocyanates, monoacid halides, monoesters, and monoalcohols, for examples.Of these, monocarboxylic acids and monoamines are preferred. When the ends of the polyamide are capped with an end-capping agent, the polyamide resin composition tends to have better thermal stability.One end-capping agent may be used alone, or two or more end-capping agents may be used in combination
[0047] The monocarboxylic acid that can be used as the end-capping agent is not particularly limited to as long as it has reactivity with an amino group that can exist at the end of a polyamide, and examples are not limited to the following but include: aliphatic monocarboxylic acids such as formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexanecarboxylic acid; and aromatic monocarboxylic acids such as benzoic acid, toluylic acid, α-naphthalene carboxylic acid, β-naphthalene carboxylic acid, methyl naphthalene carboxylic acid, and phenylacetic acid, for example.In particular, an end of the (B) aromatic polyamide is preferably capped by acetic acid from the viewpoint of flowability, dimensional stability of a molded article, and mechanical strength.One of monocarboxylic acids may be used alone, or two or more of these may be used in combination.
[0048] The monoamine that can be used as the end-capping agent is not particularly limited to as long as it has reactivity with a carboxyl group that can exist at the end of a polyamide, and examples are not limited to the following but include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; and aromatic monoamines such as aniline, toluidine, diphenylamine, and naphthylamine, for example.One of monoamines may be used alone, or two or more of these may be used in combination.A polyamide resin composition containing a polyamide of which end is capped by an end-capping agent tends to have excellent flowability, dimensional stability of a molded article, and mechanical strength.
[0049] <Production method of polyamide> Upon production of the polyamides (the (A) crystalline aliphatic polyamide and the (B) semi-aromatic polyamide) of the resin composition of the present embodiment, the amount of the dicarboxylic acid added and the amount of the diamine added is preferably near the same molar amount. Taking into account the escape of diamines from the reaction system during polymerization, the molar amount of the total diamines in terms of molar ratio is preferably 0.9 or more and 1.2 or less, more preferably 0.95 or more and 1.1 or less, and even more preferably 0.98 or more and 1.05 or less, per 1 mol of the total dicarboxylic acids.
[0050] The method of producing a polyamide is not limited to the following but includes, for example, the polymerization step of (1) or (2) below.(1) The step of polymerizing one or more selected from the group consisting of a lactam constituting the lactam unit (e.g., (A-a) a lactam unit having a carbon number of 4 or more and 14 or less) and an aminocarboxylic acid constituting the aminocarboxylic acid unit (e.g., (A-a') anaminocarboxylic acid unit having a carbon number of 4 or more and 14 or less) to obtain a polymer.(2) The step of polymerizing a combination of a dicarboxylic acid constituting the dicarboxylic acid unit and a diamine constituting the diamine unit (e.g., a combination of (A-b) an aliphatic dicarboxylic acid unit and (A-c) an aliphatic diamine unit, or a combination of (B-a) a dicarboxylic acid unit and (B-b) a diamine unit) to obtain a polymer.
[0051] It is also preferred that the method of producing a polyamide further includes, after the polymerization step, a raising step to raise the degree of polymerization of the polyamide. If necessary, the polymerization step and the rising step may be followed by a capping step in which the ends of the resulting polymer are capped with an end-capping agent.
[0052] Specific methods of producing a polyamide include various methods as exemplified in 1) to 4) below.1) A method in which an aqueous solution or suspension of a lactam and one or more selected from the group consisting of an aminocarboxylic acid, a dicarboxylic acid-diamine salt, and a mixture of a dicarboxylic acid and a diamine is heated and polymerized while the molten state is maintained (hereinafter sometimes referred to as "thermal melt polymerization method").2) A method in which a polyamide obtained through the thermal melt polymerization method is maintained in the solid state at a temperature equal to or lower than the melting point to increase the degree of polymerization of the polyamide (hereinafter sometimes referred to as "thermal melt polymerization-solid phase polymerization method").3) A method in which one or more selected from the group consisting of a dicarboxylic acid-diamine salt, a mixture of a dicarboxylic acid and a diamine, a lactam, and / or an aminocarboxylic acid are polymerized while the solid state is maintained (hereinafter sometimes referred to as "solid phase polymerization method").(4) A method in which a dicarboxylic acid halide component equivalent to a dicarboxylic acid and a diamine component is used for polymerization (hereinafter sometimes referred to as the "solution method").
[0053] Of these, production methods involving the thermal melt polymerization method are preferred as the specific method of producing a polyamide. In addition, when a polyamide is produced by the thermal meltpolymerization method, it is preferable to maintain the molten state until polymerization is completed. In order to maintain the molten state, production must be carried out under polymerization conditions suitable for a polyamide resin composition. The polymerization conditions include, for example, the following conditions. First, the polymerization pressure in the thermal melt polymerization method is controlled to 14 kg / cm2 or more and 25 kg / cm2 or less (gauge pressure), and heating is continued. The pressure in the tank is then lowered over 30 minutes or longer until it reaches atmospheric pressure (the gauge pressure indicates 0 kg / cm2).
[0054] In the method of producing a polyamide, the mode of polymerization is not limited and can be batch or continuous.The polymerization apparatus used for the production of the polyamide is not particularly limited, and any known apparatus can be used. Specific examples of the polymerization apparatus include autoclave-type reactors, tumbler-type reactors, and extruder-type reactors (kneaders, etc.), for example.
[0055] A method of producing a polyamide by batch thermal melt polymerization method will be specifically described, but the method of producing a polyamide is not limited to this method.First, an aqueous solution containing about 40 mass% or more and 60 mass% or less of the raw material components of a polyamide (a lactam and / or an aminocarboxylic acid, a dicarboxylic acid, a diamine) is prepared. Then, the aqueous solution is heated in a concentration tank operated at a temperature 110°C or higher and 180°C or lower under a pressure of about 0.035 MPa or more and 0.6 MPa or less (gauge pressure) and concentrated to about 65 mass% or more and 90 mass% or less to obtain a concentrated solution.The resulting concentrated solution is then transferred to an autoclave, and heating is continued until the pressure in the autoclave reaches about 1.2 MPa or more and 2.2 MPa or less (gauge pressure). Then, in the autoclave, the pressure is maintained at about 1.2 MPa or more and 2.2 MPa or less (gauge pressure) while at least one of water and gas component are vented. Then, when the temperature reaches about 220°C or more and 260°C or less, the pressure is lowered to atmospheric pressure (gauge pressure is 0 MPa). After the pressure in the autoclave is reduced toatmospheric pressure, by-produced water can be effectively removed by depressurizing as necessary.The autoclave is then pressurized with inert gas such as nitrogen, and the polyamide melt is extruded from the autoclave into strands. The extruded strands are cooled and cut to obtain pellets of a polyamide.
[0056] (Polymer ends of polyamide)The polymer ends of polyamides used in the present invention can be, but are note limited to, classified and defined as follows.Specifically, they include 1) an amino end, 2) a carboxyl end, 3) an end by an end-capping agent, and 4) other ends.
[0057] (1) An amino end is a polymer end having an amino group (-NH2 group) and is derived from the raw material diamine unit.(2) A carboxyl end is a polymer end having a carboxyl group (-COOH group) and is derived from the raw material dicarboxylic acid.(3) An end by an end-capping agent is an end formed when an end-capping agent is added during polymerization. End-capping agents include the end-capping agents described above.(4) Other ends are polymer ends that are not classified as 1) to 3) above, such as an end formed by deammonia reaction of an amino end and an end formed by decarboxylation reaction of a carboxyl end.
[0058] <(A) Characteristics of aliphatic polyamide>The molecular weight of the crystalline aliphatic polyamide can be specifically measured with the method described in Examples below.
[0059] The Mw(A) (weight average molecular weight) can be used as a measure of the molecular weight of the (A) aliphatic polyamide. The Mw(A) (weight average molecular weight) of the (A) crystalline aliphatic polyamide is preferably 10000 or more, more preferably 15000 or more, even more preferably 17000 or more, even more preferably 20000 or more, and is preferably 50000 or less, even more preferably 40000 or less, even more preferably 34000 or less, and even more preferably 30000 or less. When the Mw(A) (weight average molecular weight) is within the above range, a polyamide resin composition with excellent flowability, appearance of a molded article, dimensional stability of a tap part, mechanical characteristics, and the like can be obtained. In addition, the polyamide resin composition containing a component typified by an inorganic filler will have an excellentsurface appearance. Note that the Mw(A) (weight average molecular weight) can be measured using gel permeation chromatography (GPC).
[0060] The molecular weight distribution of the (A) crystalline aliphatic polyamide is expressed by Mw(A) (weight average molecular weight) / Mn(A) (number average molecular weight). Mw(A) (weight average molecular weight) / Mn(A) (number average molecular weight) of the (A) crystalline aliphatic polyamide is preferably 1.8 or more, more preferably 1.9 or more, and is preferably 2.2 or less, more preferably 2.1 or less. The lower limit of the molecular weight distribution is 1.0. When Mw(A) (weight average molecular weight) / Mn(A) (number average molecular weight) is within the above range, a polyamide resin composition with excellent flowability, etc. can be obtained.
[0061] In addition, a polyamide resin composition containing a component typified by an inorganic filler will have an excellent surface appearance.
[0062] The method of controlling Mw(A) (weight average molecular weight) / Mn(A) (number average molecular weight) of the (A) crystalline aliphatic polyamide within the above range includes, for example, a method by adding a known polycondensation catalyst such as phosphoric acid or sodium hypophosphite as an additive during thermal melt polymerization of a polyamide, and a method by controlling polymerization conditions such as the heating condition and the reduced pressure condition. In the present invention, Mw(A) (weight average molecular weight) / Mn(A) (number average molecular weight) of the (A) crystalline aliphatic polyamide can be calculated using the Mw(A) (weight average molecular weight) and the Mn(A) (number average molecular weight) obtained using GPC (gel permeation chromatography).
[0063] <Characteristics of (B) semi-aromatic polyamide>The molecular weights, the melting point Tm2, the crystallization enthalpy ΔH, and peak temperature of tanδ of the (B) semi-aromatic polyamide can be specifically measured by the methods described below.
[0064] The Mw(B) (weight average molecular weight) can be used as a measure of the molecular weight of (B) the semi-aromatic polyamide. The Mw(B) (weight average molecular weight) of the (B) polyamide is preferably 10000 or more, more preferably 13000 or more, even more preferably 15000 or more, even more preferably 18000 or more, particularly preferably 19000or more, and is preferably 50000 or less, more preferably 40000 or less, even more preferably 25000 or less, still even more preferably 22000 or less, and particularly preferably 21000 or less.
[0065] When the Mw(B) (weight average molecular weight) is within the above range, a polyamide resin composition with excellent flowability, dimensional stability of a molded article, mechanical strength, and the like can be obtained. In addition, a polyamide resin composition containing a component typified by an inorganic filler will have an excellent surface appearance. Note that the Mw(B) (weight average molecular weight) can be measured using gel permeation chromatography (GPC).
[0066] The molecular weight distribution of (B) the semi-aromatic polyamides is expressed by the Mw(B) (weight average molecular weight) / the Mn(B) (number average molecular weight).Mw(B) (weight average molecular weight) / Mn(B) (number average molecular weight) of the (B) semi-aromatic polyamide is preferably 2.4 or less, more preferably 1.7 or more and 2.4 or less, even more preferably 1.8 or more and 2.3 or less, still even more preferably 1.9 or more and 2.2 or less, and most preferably 1.9 or more and 2.1 or less. The lower limit of Mw(B) (weight average molecular weight) / Mn(B) (number average molecular weight) is 1.0. When Mw(B) (weight average molecular weight) / Mn(B) (number average molecular weight) is within the above range, a polyamide resin composition with excellent flowability, etc. can be obtained. In addition, a polyamide resin composition containing a component typified by an inorganic filler will have an excellent surface appearance.
[0067] A method to control Mw(B) (weight average molecular weight) / Mn(B) (number average molecular weight) of the (B) semi-aromatic polyamide within the above range is, for example, a method by adding a known polycondensation catalyst such as phosphoric acid or sodium hypophosphite as an additive during thermal melt polymerization of the polyamide. It is also important to control the polymerization conditions, such as the heating condition and depressurization condition, to complete the polycondensation reaction at the lowest possible temperature and in the shortest possible time. In particular, it is desirable that the (B) semi-aromatic polyamide is an amorphous polyamide because this polyamide does not have a melting point and thus the reaction temperature can be lowered.When an aromatic compound unit is included in the molecular structure of a polyamide, the molecular weight distribution (Mw / Mn) tends to increase as the molecular weight increases. A high molecular weight distribution indicates a higher proportion of polyamide molecules with three-dimensional molecular structures. This makes the three-dimensional structuring of the molecules more likely to progress during high-temperature processing, resulting in reduced flowability, and a deterioration in surface appearance of a polyamide resin composition containing a component typified by an inorganic filler.
[0068] In the present invention, Mw(B) (weight average molecular weight) / Mn(B) (number average molecular weight) of the (B) semi-aromatic polyamide can be calculated using the Mw(B) (weight average molecular weight) and the Mn(B) (number average molecular weight) obtained using GPC (gel permeation chromatography).
[0069] The crystallization enthalpy ΔH of the (B) semi-aromatic polyamide is preferably 15 J / g or less, more preferably 10 J / g or less, more preferably 5 J / g or less, even more preferably 2 J / g or less, and particularly preferably 0 J / g.A method to control the crystallization enthalpy ΔH of the (B) semi-aromatic polyamide within the above range is to increase the ratio of aromatic monomers to the (B-a) dicarboxylic acid unit. It is important that 75 mol%, more preferably 100% of the dicarboxylic acid unit is included in the (B-a) isophthalic acid.An apparatus for measuring the crystallization enthalpy ΔH of the (B) semi-aromatic polyamide may be, for example, Diamond-DSC manufactured by PERKIN-ELMER.
[0070] The amount of amino ends of the (B) semi-aromatic polyamide is preferably 5 to 100 μ eq. / g, more preferably 10 to 90 μ eq. / g, even more preferably 20 to 80 μeq. / g, still even more preferably 30 to 70 μ eq. / g, and further even more preferably 40 to 60 μeq. / g per 1 g of the polyamide. When the amount of amino ends is within the above range, the composition can be made to be excellently resistant to heat and discoloration by light. The amount of amino ends can be measured by neutralization titration.
[0071] The amount of carboxyl ends of the (B) semi-aromatic polyamide is preferably 50 to 300 μ eq. / g, more preferably 100 to 280 μ eq. / g, even more preferably 150 to 260 μ eq. / g, still even more preferably 180 to 250 μ eq. / g,and further even more preferably 200 to 240 μeq. / g per 1 g of the polyamide. When the amount of carboxyl ends is within the above range, a polyamide resin composition with excellent flowability, etc. can be obtained. In addition, a polyamide resin composition containing a component typified by an inorganic filler will have an excellent surface appearance. The amount of carboxyl ends can be measured by neutralization titration.
[0072] The total amount of amino ends and carboxyl ends is preferably 150 to 350 μ eq. / g, more preferably 160 to 300 μ eq. / g, even more preferably 170 to 280 μ eq. / g, still even more preferably 180 to 270 μ eq. / g, and further even more preferably from 190 to 260 μeq. / g per 1 g of the polyamide. When the total amount of amino ends and carboxyl ends are in the above range, a polyamide resin composition with excellent flowability, etc. can be obtained. In addition, the polyamide resin composition containing a component typified by an inorganic filler will have an excellent surface appearance.
[0073] <(C) Fibrous reinforcing material> In addition to the above (A) to (B) components, the polyamide resin composition of the present embodiment further contains (C) a fibrous reinforcing material. The (C) fibrous reinforcing material can be used to improve the mechanical strength of the polyamide resin composition and the durability of a molded article.
[0074] Examples of the (C) fibrous reinforcing material are not limited to the following but include: glass fibers, carbon fibers, calcium silicate fibers, potassium titanate fibers, aluminum borate fibers, aramid fibers, and cellulose nanofibers, for example. Of these, glass fibers, carbon fibers, or potassium titanate fibers with circular and non-circular cross-sections are preferred from the viewpoint of increasing the strength and stiffness of the resulting molded article. Glass or carbon fibers with circular and non-circular cross sections are more preferred. One of these (C) fibrous reinforcing materials may be used alone or two or more of these may be used in combination.
[0075] As glass fibers and carbon fibers, from the viewpoint of imparting excellent mechanical characteristics to the polyamide resin composition, preferred are those having a number average fiber diameter of 3 μm or more and 30 μm or less, a weight average fiber length of 100 μm or more and 750 μm or less, and an aspect ratio of the weight average fiber length to the number average fiber diameter (the value obtained by dividing the weightaverage fiber length by the number average fiber diameter) of 10 or more and 100 or less.
[0076] As calcium silicate fibers, from the viewpoint of imparting excellent mechanical characteristics to the polyamide resin composition, preferred are those with a number average fiber diameter of 3 μm or more and 30 μm or less, a weight average fiber length of 10 μm or more and 500 μm or less, and an aspect ratio of 3 or more and 100 or less.
[0077] Here, the number average fiber diameter and weight average fiber length can be obtained as follows.
[0078] Specifically, the polyamide resin composition is placed in an electric furnace to incinerate the organic matter contained therein, and arbitrarily 100 or more fibers of the (C) fibrous reinforcing materials, for example, are selected from the residue and observed under SEM, and their fiber diameters are measured and the average value is calculated to be used as the number average fiber diameter.
[0079] Furthermore, the fiber lengths are measured using an SEM photograph with a magnification of 1000∑ and the weight average fiber length can be obtained using a predetermined formula (when fiber lengths of n fibers are measured, the weight average fiber length = ∑(I = 1 ->n)(fiber length of the nth fiber)2 / ∑(I = 1->n)(fiber length of the nth fiber)).
[0080] The content of the (C) fibrous reinforcing material in the polyamide resin composition of the present invention is 100.0 parts by mass or more and 200.0 parts by mass or less, preferably 110.0 parts by mass or more and 175.0 parts by mass or less, more preferably 120.0 parts by mass or more and 150.0 parts by mass or less, when the total of the (A) crystalline aliphatic polyamide and the (B) semi-aromatic polyamide is taken as 100 parts by mass. If the content of the (C) fibrous reinforcing material exceeds the above upper limit, the toughness of the polyamide resin composition tends to decrease and the self-tapping characteristic tends to decrease. If the content of the (C) fibrous reinforcing material is below the above range, the polyamide resin composition tends not to exhibit strength. Therefore, by setting the content of the (C) fibrous reinforcing material within the above range, a polyamide resin composition with excellent mechanical characteristics, mold processability, and self-tapping characteristic can be obtained.
[0081] <(D) Carbon black>The polyamide resin composition of the present invention may further contain (D) carbon black. The carbon black is not particularly limited, but the average primary particle size is preferably in the range of 10 nm to 40 nm, more preferably 10 nm to 30 nm, and particularly preferably 10 nm to 20 nm. It is preferably 10 nm or more from the viewpoint of dispersibility into the composition, and is 40 nm or less from the viewpoint of strength, stiffness, and expression of the thin portions of a molded piece. In addition, one having a specific surface area in the range of 50 to 300 m2 / g (BET adsorption method) and an oil absorption (measured using dibutyl phthalate) in the range of 50 mL / 100 g to 150 mL / 100 g is preferably used.
[0082] In the case where (D) carbon black is used, it is sufficient that the amount of the carbon black added is 0 parts by mass or more when the total of the (A) crystalline aliphatic polyamide resin, the (B) semi-aromatic polyamide, and the (C) fibrous reinforcing material is taken as 100 parts by mass. The amount is preferably 0.04 parts by mass or more, more preferably 0.1 parts by mass or more, even more preferably 0.4 parts by mass or more, and is 1.00 parts by mass or less, more preferably 0.8 parts by mass or less, and even more preferably 0.7 parts by mass or less. In addition, the amount of the (D) carbon black added is 0 part by mass or more, preferably 0.1 part by mass or more, more preferably 0.25 part by mass or more, and even more preferably 1 part by mass or more, and is preferably 2.5 parts by mass or less, more preferably 2.0 parts by mass or less, even more preferably 1.75 parts by mass or less, when the total of the (A) crystalline aliphatic polyamide resin and the (B) semi-aromatic polyamide is taken as 100 parts by mass. When the content of the (D) carbon black is within the above range, the (D) carbon black tends to efficiently function as a crystal nucleating agent and the degree of crystallinity of a boss section tends to be increased. Therefore, a polyamide resin composition with excellent mechanical characteristics, mold processability, and self-tapping characteristic can be obtained.
[0083] <(E) Crystallization retarder> The polyamide resin composition of the present invention further contains (E) a crystallization retarder from the viewpoint of further improving the appearance and mechanical strength of a molded article. A crystallization retarder is a substance that has the effect of lowering the crystallization starting point of a polyamide resin when blended with a polyamide resin.Examples of the (E) crystallization retarder are not particularly limited, but include azine-based dyes, phthalocyanine-based dyes and lithium chloride. Azine-based dyes or phthalocyanine-based dyes are particularly preferred. Nigrosine is preferred as an azine-based dye, and copper phthalocyanine dyes are preferred as a phthalocyanine-based dye.
[0084] The content of the (E) crystallization retarder is preferably 0.02 parts by mass or more, more preferably 0.03 parts by mass or more, even more preferably 0.04 parts by mass or more, and is 0.2 parts by mass or less, more preferably 0.08 parts by mass or less, and even more preferably 0.06 parts by mass or less, when the total of the (A) crystalline aliphatic polyamide resin, the (B) semi-aromatic polyamide, and the (C) glass fiber is taken as 100 parts by mass. Furthermore, the content of the (E) crystallization retarder is preferably 0.05 parts by mass or more, more preferably 0.075 parts by mass or more, even more preferably 0.1 parts by mass, and is preferably 0.5 parts by mass or less, more preferably 0.2 parts by mass or less, and even more preferably 0.15 parts by mass or less, when the total of the (A) crystalline aliphatic polyamide resin and the (B) semi-aromatic polyamide is taken as 100 parts by mass. If the content of the (E) crystallization retarder exceeds the above range, crystallinity and toughness tend to decrease, cracking tends to occur readily, and uniformity in crystallization tends to decrease, leading to a decrease in appearance of a molded article and strength of a tapping portion. When the content of the (E) crystallization retarder is within the above range, uniform crystallization is induced and dimensions tend to be stabilized. As a result, a polyamide resin composition with excellent mechanical characteristics, mold processability, and self-tapping characteristic can be obtained.
[0085] <Other additives>The polyamide resin composition may also contain other additives that are commonly used for polyamides to the extent that the purpose of the present embodiment is not impeded. Examples of other additives include, for example, antioxidants, fibrillating agents, lubricants, fluorescent bleaches, plasticizers, UV absorbers, antistatic agents, flow modifiers, reinforcing agents, spreading agents, nucleating agents, rubber, strengthening agents, flame retardants, and other polymers. The content of other additives in the polyamide resin composition of the present embodiment can be set by a personskilled in the art according to the purpose thereof.
[0086] <Method of producing polyamide resin composition>The method of producing the polyamide resin composition is not particularly limited as long as the method involves mixing the (A) crystalline aliphatic polyamide, the (B) semi-aromatic polyamide, the (C) fibrous reinforcing material, the (D) carbon black, and the (E) crystallization retarder.
[0087] Methods for mixing the above components (A), (B), (D), and (E) include, for example, the method (1) or (2) below.(1) A method in which the above components (A), (B), (D), and (E) are mixed using a Henschel mixer or the like and fed to a melt-kneader for kneading.(2) A method in which the above components (A), (B), (D), and (E) are mixed in advance using a Henschel mixer or the like and mixed in a single or twin screw extruder to prepare a mixture containing the components (A) to (D). After the mixture is then fed to a melt-kneader and kneaded, the (C) component is optionally blended from a side feeder.
[0088] The method for feeding the components of the polyamide resin composition to the melt-kneader may be accomplished by feeding all the components at once to the same feed port, or by feeding the components from different feed ports.
[0089] The temperature of the melt kneading is preferably a temperature higher than the melting point of the (A) crystalline aliphatic polyamide by about 1°C or higher and 100°C or lower, and is more preferably a temperature higher than the melting point of the (A) crystalline aliphatic polyamide by about 20°C or higher and 70°C or lower. The shear rate in the kneader is preferably about 100 sec-1 or higher. The average residence time of kneading is preferably 0.5 minutes or longer and 5 minutes or shorter.Any apparatus for performing melt-kneading may be used, and single or twin screw extruders, Banbury mixers, melt kneaders (mixing rolls, etc.), and like are preferably used, for example.The amounts of the respective components in the polyamide resin composition of the present embodiment are the same as the amounts of the respective components in the polyamide resin composition described above.
[0090] <Characteristics of the polyamide resin composition >The Mw (weight average molecular weight) can be used as a measure of the molecular weight of the polyamide resin composition. The Mw (weight average molecular weight) of the polyamide resin composition is preferably 10000 or more, preferably 17000 or more, more preferably 20000 or more, even more preferably 25000 or more, still even more preferably 27000 or more, most preferably 29000, and is preferably 40000 or less, preferably 37000 or less, more preferably 35000 or less, even more preferably 34000 or less, still even more preferably 33000 or less, and most preferably 32000 or less. When the Mw (weight average molecular weight) is within the above range, a polyamide resin composition with excellent mechanical characteristics, mold processability, and self-tapping characteristic can be obtained.Methods of controlling the Mw of the polyamide composition within the above range include the use of the (A) crystalline aliphatic polyamide and the (B) semi-aromatic polyamide with Mw within the respective ranges mentioned above.Note that the Mw (weight average molecular weight) can be measured using gel permeation chromatography (GPC), as will be described in EXAMPLES below.
[0091] The total content of the (A) crystalline aliphatic polyamide and the (B) semi-aromatic polyamide having a number average molecular weight Mn of 500 or more and 2000 or less is preferably 0.5 mass% or more and less than 2.5 mass%, more preferably 0.8 mass% or more and less than 2.5 mass%, even more preferably 1.0 mass% or more and less than 2.5 mass%, still even more preferably 1.2 mass% or more and less than 2.5 mass%, and most preferably 1.4 mass% or more and less than 2.5 mass%, with respect to the total polyamide content in the polyamide resin composition. When the content of those having a number average molecular weight Mn is 500 or more and 2000 or less is 0.5 mass% or more, excellent flowability tends to be achieved and a polyamide composition containing a component typified by an inorganic filler tends to have an excellent surface appearance. The content of less than 2.5 mass% tends to suppress gas generation during molding.
[0092] A method to control the total content of polyamides with a number average molecular weight Mn of 500 or more and 2000 or less within the above range is a method by adjusting the molecular weight of the (B)semi-aromatic polyamide, and the Mw (weight average molecular weight) is preferably 10000 to 25000.The total content of the (A) aliphatic polyamide and the (B) semi-aromatic polyamide with a number average molecular weight Mn of 500 or more and 2000 or less with respect to the total polyamide content is determined using GPC from an elution curve under the measurement conditions described in Examples below.In the case where other components that are soluble in a solvent for dissolving the polyamides are contained in the composition containing the (A) crystalline aliphatic polyamide and the (B) semi-aromatic polyamide upon a GPC measurement, the other components are removed by extracting them using a solvent in which the polyamides are insoluble but the other components are soluble before the GPC measurement. Inorganic fillers and other materials that are insoluble in the solvent for dissolving the polyamide resins are dissolved in the solvent for dissolving the polyamide resin composition, which is then filtered to remove the insoluble materials before the GPC measurement.
[0093] The molecular weight distribution of the polyamide resin composition of the present invention is expressed by Mw (weight average molecular weight) / Mn (number average molecular weight). Mw (weight average molecular weight) / Mn (number average molecular weight) of the polyamide resin composition of the present invention is preferably 2.4 or less, more preferably 1.7 to 2.3, more preferably 1.8 to 2.2, and even more preferably 1.9 to 2.1. The lower limit of the molecular weight distribution is 1.0. When Mw (weight average molecular weight) / Mn (number average molecular weight) is within the above range, a polyamide resin composition with excellent flowability, etc. tends to be obtained. In addition, a polyamide resin composition containing a component typified by an inorganic filler tend to have excellent self-tapping characteristic, surface appearance, and the like.
[0094] As a method to control Mw (weight average molecular weight) / Mn (number average molecular weight) of the polyamide resin composition within the above range, it is important to keep Mw (weight average molecular weight) / Mn (number average molecular weight) of the (B) semi-aromatic polyamide within the above-mentioned range.When aromatic compound units are included in the molecular structure of the polyamide resin composition, the molecular weight distribution (Mw / Mn) tends to increase as the molecular weight increases. A high molecular weight distribution indicates a high percentage of polyamide molecules with a three-dimensional molecular structure, and the three-dimensional structuring of molecules tends to progress further during high-temperature processing, resulting in reduced flowability and a deteriorated surface appearance of the polyamide resin composition containing a component typified by an inorganic filler.
[0095] In the present invention, a calculation of Mw (weight average molecular weight) / Mn (number average molecular weight) of the polyamide resin composition can be achieved using the Mw (weight average molecular weight) and the Mn (number average molecular weight) obtained using GPC (gel permeation chromatography), as will be described in Examples below.
[0096] The cold crystallization peak of a molded article of the polyamide resin composition of the present invention, which is obtained by molding a specimen having a thickness of 0.75 mm at a cylinder temperature of 280 °C and a mold temperature of 90 °C, when the temperature is kept at 30°C for 3 minutes by differential scanning calorimetry (DSC) and is then increased to 280 °C at 20.0 °C / min is preferably 2.0 J / g or less, more preferably 1.0 J / g or less, even more preferably 0.5 J / g or less, and still even more preferably 0.2 J / g or less. If the above range is exceeded for the polyamide resin composition of the present invention, a boss tends to break by cracking before a screw slips during self-tapping due to poor crystallization in the mold during injection molding. Therefore, when the above range is satisfied, a polyamide resin composition with excellent mechanical characteristics, mold processability, and self-tapping characteristic can be obtained.
[0097] In the polyamide resin composition of the present invention, the mass ratio Dw / Ew of the (D) carbon black and the (E) crystallization retarder is preferably 5 or more and 25 or less, more preferably 10 or more and 20 or less, even more preferably 11 or more and 18 or less, still even more preferably 12 or more and 16 or less, further even more preferably 13 or more and 15 or less. When the mass ratio Dw / Ew is equal to or more than the above lower limit, the polyamide resin composition can be made to have excellent appearance and self-tapping property of screw tightening. When the massratio Dw / Ew is equal to or lower than the above upper limit, a polyamide composition can be made to have excellent self-tapping property for screw tightening.
[0098] <Molded article>A molded article of the present embodiment is produced by molding the above polyamide resin composition.In addition, the molded article of the present embodiment has a high surface gloss value. The surface gloss value of the molded article of the present embodiment is 60 or more, preferably 70 or more, and more preferably 80 or more. When the surface gloss value of the molded article is set to equal to or more than the above lower limit, the resulting molded article can be suitably used for various parts for automobile applications, electrical and electronic applications, industrial material applications, manufacturing industrial material applications, daily product and household product applications, and the like. It is also suitable for molded articles with a self-tapping screw insertion portion because of its excellent self-tapping property for screw tightening.
[0099] The method of producing the molded article is not specifically limited and commonly known methods may be used. Commonly known molding methods are not limited to the following but include: generally known plastic molding methods, such as press molding, injection molding, gas-assisted injection molding, fusion molding, extrusion molding, blow molding, film molding, hollow molding, multilayer molding, and melt spinning, for example.
[0100] <Applications> A molded article obtained by molding the polyamide resin composition by the production method of the present embodiment is excellent in mechanical properties, the appearance of the molded article, and self-tapping property of screw-tightening because it is made from the polyamide resin composition described above. Therefore, this molded article can be suitably used as various parts, such as automotive parts, electric and electronic parts, home appliance parts, parts for OA (Office Automation) apparatuses, mobile device parts, parts for industrial apparatuses, and daily good and household product parts, and used for extrusion applications. The molded articles are particularly suitable for automotive parts, electrical andelectronic parts, home appliance parts, parts for OA apparatuses, or mobile device parts. Of these, it is further suitable for a molded article with a self-tapping screw insertion portion.
[0101] Automotive parts are not particularly limited, but include, for example, intake system parts, cooling system parts, fuel system parts, interior parts, exterior parts, and electrical parts.EXAMPLES
[0102] The following provides a more detailed description of the present invention through specific examples and comparative examples. However, the present invention is not limited to the following examples.
[0103] Each component of polyamide resin compositions used in the present examples and comparative examples will be described.
[0104] <Components>[(A) Crystalline aliphatic polyamide] A-1: Polyamide 6 (trade name: "SF1013A", manufactured by UBE Corporation, Mw(A) = 31500, Mw(A) / Mn(A) = 2.2)
[0105] [(B) Semi-aromatic polyamide]B-1: Polyamide 6IB-2: Polyamide 6I / 6T (trade name: "G21", manufactured by EMS, Mw(B) = 27000, Mw(B) / Mn(B) = 2.4)B-3: Polyamide MXD6 (TOYOBO Nylon trade name "T-600" manufactured by TOYOBO CO., LTD., the Mw(B): 45000, the Mw(B) / the Mw(B): 2.2)
[0106] [(C) Fibrous reinforcing material]C-1: Glass fiber (GF) (trade name: "ECS03T275H", manufactured by Nippon Electric Glass Co., Ltd., average fiber diameter: 10 μm φ, cut length: 3 mm)C-2: Wollastonite (trade name "400WC" (manufactured by NYCO, number average particle diameter: 8.0 μm, number average particle length: 35 μm)
[0107] [(D) Carbon black]D-1: Carbon black (CB) (trade name: "#52B", manufactured by Mitsubishi Chemical Corporation)
[0108] [(E) Crystallization retarder]E-1: Nigrosine dye (TH807, manufactured by ORIENT CHEMICAL INDUSTRIES CO., LTD)
[0109] <Production of polyamide>The details of each production method of the semi-aromatic polyamide B-1 will be described below. Note that the semi-aromatic polyamide B-1 obtained by the following production method was dried in a nitrogen stream to adjust the moisture content to about 0.2 mass%, and then was used as a raw material for polyamide resin compositions in the examples and comparative examples described below.
[0110] [Synthesis Example 1] Synthesis of semi-aromatic polyamide B-1 (Polyamide 6I)A polymerization reaction of the polyamide was carried out by the "thermal melting polymerization method" as follows. First, a 50-mass% homogeneous water solution of raw monomers was prepared by dissolving, in 1500 g of distilled water, 1500 g of an equimolar salt of isophthalic acid and hexamethylenediamine, adipic acid at 1.5 mol% excess relative to the total equimolar salt components, and 0.5 mol% of acetic acid. Next, the solution was concentrated by gradually venting water vapor until the concentration of the solution reached 70 mass% while stirring at a temperature of about 110°C or higher and 150°C or lower. The internal temperature was then raised to 220°C. At this time, the pressure of the autoclave was increased to 1.8 MPa. A reaction was caused to take place for 1 hour while the pressure was maintained to 1.8 MPa until the internal temperature reached 245°C by gradually venting water vapor for 1 hour. The pressure was then lowered over 30 minutes. The interior of the autoclave was then maintained to a reduced pressure of 650 torr (86.66 kPa) for 10 minutes using a vacuum apparatus. At this time, the final internal temperature of the polymerization was 265°C. The resultant was then extruded by pressurization with nitrogen through a lower spinneret (nozzle) into strands, which were water-cooled, cut, and discharged in the form of pellets The pellets were then dried at 100°C for 12 hours under a nitrogen atmosphere to obtain a semi-aromatic polyamide B-1 (polyamide 6I).The content of the isophthalic acid unit in the dicarboxylic acid unit in the resulting semi-aromatic polyamide B-1 (polyamide 6I) was 100 mol%. Mw(B) was 20000.
[0111] <Measurement methods of physical properties>First, pellets of the polyamide resin composition obtained in the Examples and Comparative Examples were dried in a nitrogen stream toreduce the moisture content in the polyamide resin composition to 500 ppm or less. Then, using pellets of each polyamide resin composition of which moisture content was adjusted, various physical properties were measured and evaluations were made using the following methods.
[0112] [Physical property 1] Molecular weight of polyamide resin composition(Molecular weight (Mn, Mw / Mn) of polyamide resin composition)The Mw (weight average molecular weight) / Mn (number average molecular weight) of each obtained polyamide resin composition in the examples and comparative examples was calculated using Mw and Mn measured by GPC (gel permeation chromatography, HLC-8020, manufactured by Tosoh Corporation, in hexafluoroisopropanol solvent, in terms of PMMA (polymethyl methacrylate) standard sample (manufactured by Polymer Laboratories, Inc.)). GPC columns used were TSK-GEL GMHHR-M and G1000HHR columns.
[0113] [Physical property 2] Degree of cold crystallization of polyamide resin compositionA strip molded piece (12.7 cm x 1.27 cm, 0.75 mm in thick) was produced using an injection molding machine [NEX50III-5EG, manufactured by NISSEI PLASTIC INDUSTRIAL CO., LTD.] by setting the cooling time to 25 seconds, the screw rotation speed to 200 rpm, the mold temperature to 90 °C, and the cylinder temperature to 280 °C, and adjusting the injection pressure and injection speed as appropriate so that a filling time was within the range of 1.6 ± 0.1 seconds. The center of the strip molded piece was cut with nippers to obtain a sample of 8 g, and a calculation was made from the endothermic peak obtained when the temperature was kept at 30 °C for 3 minutes by differential scanning calorimetry (DSC) and was then increased at 20 °C / min.
[0114] <Evaluation methods>[Evaluation 1] Appearance of molded article A flat plate molded piece (6 cm ± 9 cm, 3 mm in thickness) was produced using an injection molding machine [NEX50III-5EG, manufactured by NISSEI PLASTIC INDUSTRIAL CO., LTD.] by setting the cooling time to 25 seconds, the screw rotation speed to 200 rpm, the mold temperature to 90 °C, and the cylinder temperature to 280 °C, and adjusting the injectionpressure and injection speed as appropriate so that a filling time was within the range of 1.6 ± 0.1 seconds. The 60° gloss of the center part of the flat plate molded piece prepared in this way was measured according to JIS-K7150 using a gloss meter (IG320 manufactured by HORIBA, Ltd.). The surface appearance was determined to be better as the value was higher.
[0115] [Evaluation 2] Tensile strainAn ISO type A multipurpose test specimen was produced using an injection molding machine [NEX50III-5EG, manufactured by NISSEI PLASTIC INDUSTRIAL CO., LTD.] under the conditions of a resin temperature of 290°C, a mold temperature of 80°C, an injection and pressuring holding time of 25 seconds, and a cooling time of 15 seconds. The obtained multipurpose specimen was used to measure tensile fracture strain at a tensile speed of 5 mm / min according to ISO 527. The obtained fracture strain was taken as the tensile strain. A higher evaluation was given as the tensile strain was higher.
[0116] (3) Flexural modulusAn ISO type A multipurpose test specimen was produced using an injection molding machine [NEX50III-5EG, manufactured by NISSEI PLASTIC INDUSTRIAL CO., LTD.] under the conditions of a resin temperature of 290°C, a mold temperature of 80°C, an injection and pressuring holding time of 25 seconds, and a cooling time of 15 seconds. The obtained multipurpose specimen was used to measure the flexural modulus according to ISO 178. A higher evaluation was given as the flexural modulus was higher.
[0117] [Evaluation 4] Change in inner diameter of self-tapping molded article A molded article that had a boss with a thickness of 5.6 mm and an inner diameter of 3.4 mm φ was injection molded on a circular flat plate having a diameter Φ of 140 mm and a thickness of 3 mm. The actual inner diameter of the molded piece was measured with a precision of 0.1 mm using a pin gauge. A higher evaluation was given when the difference between the inside diameter and the actual inside diameter, i.e., shrinkage ratio, was in the range of 0.06 to 0.15 mm, preferably 0.07 to 0.13 mm, more preferably 0.08 to 0.10 mm.
[0118] [Evaluation 5] Fracture torque strength and mode of fracture by self-tapping screwA molded article that had a boss with a thickness of 5.6 mm and an internal diameter of 3.4 mm φ was injection molded on a circular flat plate having a diameter Φ of 140 and a thickness of 3 mm. A self-tapping screw (manufactured by Osaka Damashii, pan head tapping screw, M4x10, thread diameter: 4 mm, thread length: 10 mm, cross-shaped hole) was inserted into the boss hole. The maximum torque until the inside of the resin was fractured and the screw slipped was measured as the tightening torque using a digital torque meter HDP-50 (manufactured by HIOS Inc.), and an evaluation was made. A higher evaluation was given as the tightening torque was high. Moreover, the behavior upon tightening was evaluated according to the following criteria.
[0119] (Evaluation criteria)OK: Screw was slippedNG: Boss was fractured by cracking before the screw slipped
[0120] <Method of producing polyamide resin composition> [Example 1] Production of resin compositionsTEM 35 mm twin-screw extruder, manufactured by Toshiba Machine Co., Ltd. (set temperature: 280°C, screw speed: 300 rpm) was used. The polyamide (A-1), and a mixture of (B-1), (D-1), and (E-1) that were blended in advance was fed from the top feed port provided at the most upstream of the extruder, and (C-1) was fed from a side feed port on the downstream of the extruder (in the state where the resins fed from the top feed port were fully molten), and the molten mixture extruded from the die head was cooled in strands and pelletized to obtain pellets of a polyamide resin composition. The blended amounts are summarized in Table 1. The resulting pellets of the polyamide resin composition were used to produce molded articles by the method described above, and various physical properties were measured and evaluations were made. The evaluation results are summarized in Table 1.
[0121] [Examples 2 to 8 and Comparative Examples 1 to 6] Production of resin compositionPellets of resin compositions were obtained using the method similar to that of Example 1, except that the blended components and amounts were set as summarized in Table 1. Molded articles were produced from the obtained pellets of resin compositions by the methods described above, andvarious physical properties were measured and evaluations were made. The evaluation results are listed in Table 1.
[0122] [Table 1]
[0123] Table 1 indicates that polyamide resin compositions containing the (A) crystalline aliphatic polyamide, the (B) semi-aromatic polyamide, the (C) fibrous filler, the (D) carbon black, and the (E) crystallization retarder within the specified numerical ranges had good appearance, mechanical characteristics, boss dimensional stability, and tapping properties of molded articles, and molded articles with no crack fracture of the bosses upon tapping were obtained.
[0124] In a comparison of PA-a1 to PA-a3 with different content of the (B) aromatic polyamide relative to the total polyamide content in the polyamide resin composition, it was observed that the appearance and flexural modulus of the molded bodies tended to be more excellent as the content of the (B) crystalline aliphatic polyamide increased. On the other hand, as the content of the (B) aromatic polyamide decreased (as the content of polyamide A-1 increased), tensile strain and change in inner diameter of self-tap tended to be more excellent. Furthermore, tapping strength tended to increase when the content of the (B) aromatic polyamide was set in the range of 18.0 to 20.0 parts by mass.
[0125] In a comparison of the polyamide resin composition PA-a2 and PA-a6 with different amounts of the (E) crystallization retarder component, the appearance of the molded article tended to improve as the amount of the (E) crystallization retarder component increased. On the other hand, as the content of the (E) crystallization retarder component decreased, the change in inner diameter of self-tap tended to be more excellent.
[0126] In a comparison of PA-a2 and PA-a4 where the (B) aromatic polyamide were different, those containing polyamide 6I tended to be more excellent in flexural modulus, change in inner diameter of self-tap, and tapping strength.
[0127] In a comparison of PA-a2 and PA-b4 where the (B) aromatic polyamides are different, those containing polyamide 6I tented to be more excellent in appearance, tensile strain, change in inner diameter of self-tap, fracture behavior of self-tap, and tapping strength of the molded articles.
[0128] In a comparison of PA-a2 and PA-a5 with different content of the (C) fibrous reinforcing material, the flexural modulus, change in inner diameter of self-tap, fracture behavior of self-tap, and tapping strength tended to more excellent as the content of the (C) fibrous reinforcing material increased.INDUSTRIAL APPLICABILITY
[0129] The polyamide resin composition of the present invention is excellent in mechanical properties, appearance of a molded article, and self-tapping property of screw-tightening, and it has industrial applicability. For example, it is suitably used as molded materials for various parts for automobile applications, electrical and electronic applications, industrial material applications, manufacturing industrial material applications, daily product and household product applications, and the like; of these, it is particularly suitably used as molded materials with a self-tapping screw insertion portion.
Claims
1. A polyamide resin composition comprising: 75 to 89 parts by mass of (A) a crystalline aliphatic polyamide containing (A-a) at least one selected from the group consisting of a lactam unit having a carbon number of 4 or more and 14 or less and (A-a') an aminocarboxylic acid unit having a carbon number of 4 or more and 14 or less, or (A-b) an aliphatic dicarboxylic acid unit and (A-c) an aliphatic diamine unit; and 11 to 25 parts by mass of (B) a semi-aromatic polyamide containing (B-a) a dicarboxylic acid unit containing at least 50 mol% of isophthalic acid and (B-b) a diamine unit, and further comprising, with respect to 100 parts by mass of a total of the (A) crystalline aliphatic polyamide and the (B) semi-aromatic polyamide: 100 to 200 parts by mass of (C) a fibrous reinforcing material; 0 to 2.5 parts by mass of (D) carbon black; and 0.05 to 0.5 parts by mass of (E) a crystallization retarder.
2. The polyamide according to claim 1, wherein a cold crystallization peak of a molded article, which is obtained by molding a specimen having a thickness of 0.75 mm at a cylinder temperature of 280 °C and a mold temperature of 90 °C, when a temperature is kept at 30 °C for 3 minutes by differential scanning calorimetry (DSC) and is then increased to 280 °C at 20 °C / min is 2.0 J / g or less.
3. The polyamide resin composition according to claim 1 or 2, wherein the (A) aliphatic polyamide resin is polyamide 6.
4. The polyamide resin composition according to claim 1 or 2, wherein the (B) semi-aromatic polyamide contains 75 mol% or more of the isophthalic acid unit in total (B-a) dicarboxylic acid unit constituting the (B) semi-aromatic polyamide.
5. The polyamide resin composition according to claim 1 or 2, wherein the (B) semi-aromatic polyamide contains 100 mol% of the isophthalic acid unit in the total (B-a) dicarboxylic acid unit constituting the (B) semi-aromatic polyamide.
6. The polyamide resin composition according to claim 1 or 2, wherein a weight average molecular weight Mw is 10000 ≤ Mw ≤ 40000.
7. The polyamide resin composition according to claim 1 or 2, wherein a mass ratio Dw / Ew of the (D) carbon black and the (E) crystallization retarder in the polyamide composition is 5 or more and 20 or less.
8. A molded article having an insertion portion for tightening a self-tapping screw, the molded article being produced by molding the polyamide resin composition according to claim 1 or 2.