Resin coating compositions, its process of preparation and applications thereof
Patent Information
- Application Number
- IN202611016580
- Authority / Receiving Office
- IN · IN
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2026-02-14
- Publication Date
- 2026-10-26
- Estimated Expiration
- 2046-02-14
AI Technical Summary
Existing antifog coatings for optical devices suffer from durability issues, vulnerability to environmental factors, water marks, and adhesion problems, limiting their effectiveness and applicability.
A resin coating composition with dual crosslinking via acyl hydrazone bonds and hydrogen bonds, prepared by oxidizing natural gum with an oxidizing agent and mixing it with cross-linking and film-forming agents under acidic conditions, resulting in a self-healing, hydrophilic coating.
The coating composition provides enhanced antifogging performance, improved mechanical properties, and self-healing capabilities, maintaining optical clarity and durability even under harsh conditions.
Abstract
Description
TECHNICAL FIELD OF THE DISCLOSURE:
[0001] The present disclosure relates generally to the field of chemical engineering. Specifically, the present disclosure relates to design and manufacturing of resin coating compositions which comprised of dual crosslinking of components contained therein, and a process of preparation thereof. The present disclosure also relates to a device comprising a substrate coated with said resin coating composition. BACKGROUND OF THE DISCLOSURE:
[0002] Fogging is defined as a natural phenomenon occurring when humid air condenses and separates into small and discrete liquid droplets on a solid surface with a temperature less than or equal to the dew point. The as-formed droplets create an uneven pattern that causes a blurred view due to the scattering of incident light in all directions, leading to a hazy view. Optical devices are prone to fogging, leading to significant performance loss in health and safety, for example drivers’ vision may be impaired by fog on the vehicle windscreen or rearview mirrors, which is one of the primary reasons for traffic accidents. Furthermore, fog on optical sensors often reduces the precision of spectrographs. Therefore, there is a great need for an efficient antifogging technique for optical system.
[0003] The problem of fogging has been addressed using two approaches: changing the environmental parameters by changing the temperature, airflow, and relative humidity of the surrounding air to promote the evaporation of the condensed water droplet, while the second approach is to modify the surface (physically or chemically) or to deposit a coating layer. Compared to the first approach, the modification of the material / substrate is more feasible because it is easier to manipulate, more cost-effective, and capable of producing long-lasting antifogging performance. This strategy is based on altering surface properties chemically and / or surface topography to meet the desired wettability (I. F. Wahab, et al., Journal of Materials Research and Technology, vol. 23, pp. 687–714, 2023).
[0004] Hydrophilic polymers like polyethylene glycol, polyvinyl alcohol (PVA), and natural polysaccharides are ideal for antifog coatings due to their high-water adsorption capacity. They effectively retain both freezable and non-freezable water, preventing fog formation by maintaining a clear, moisture-absorbing surface. Mansoor and co-workers synthesized an antifogging and antimicrobial coating using chitosan for optical devices (Carbohydrate Polymers, vol. 296, 2022). Li and colleagues developed a highly transparent antifogging and frost-resistant film using a PVA-Nafion complex (Chemistry of Materials, vol. 28, no. 19, pp. 6975–6984, 2016).
[0005] However, the abovementioned and other known antifog coating compositions suffer from limitations such as: i) Durability and Lifespan Issues: many anti-fog coatings are topical or non-covalently bonded to the substrate, making them prone to washing or wearing off over time, especially with frequent handling or cleaning; ii) Vulnerability to Environmental Factors: anti-fog layers can be delicate and wear down if exposed to rough cleaning methods or abrasive materials, exposure to alcohol-based, ammonia-based, or other harsh cleaners can degrade the coating's effectiveness, and some photoactive inorganic coatings, such as those made with titanium dioxide (TiO₂), depend on UV light for their superhydrophilicity and may not perform well in indoor applications without UV exposure; iii) Water Marks: the use of certain surfactants in hydrophilic coatings can sometimes result in unsightly water marks caused by condensation; iv) Adhesion Problems: poor adhesion to the underlying substrate can restrict the general applicability of some coatings for antifogging purposes.
[0006] Therefore, there is a need in the art to arrive at a new and effective coating composition which has better effects in terms of antifog effect along with other efficient mechanical and physical properties, thus can address the shortcomings of traditionally known compositions / materials including discussed above.OBJECTS OF THE PRESENT DISCLOSURE
[0007] Some of the objects of the present disclosure, which at least one embodiment herein satisfies are as listed herein below.
[0008] An object of the present disclosure is to provide a resin coating composition.
[0009] Another object of the present disclosure is to provide a device comprising a substrate coated with the resin coating composition.
[0010] Yet another object of the present disclosure is to provide a process of preparation of said resin coating composition.
[0011] Still another object of the present disclosure is to provide a process of preparation of said device containing the resin coating composition.SUMMARY OF THE DISCLOSURE
[0012] In general aspect, the present disclosure relates to design and manufacturing of resin coating compositions which comprised of dual crosslinking of components contained therein, and a process of preparation thereof. The present disclosure also relates to a device comprising a substrate coated with said resin coating composition.
[0013] In an aspect, the present disclosure relates to a resin coating composition, comprising: i) natural gum(s); ii) cross-linking agent(s); and iii) film forming agent; wherein the composition comprises dual crosslinking via acyl hydrazone bond(s) and hydrogen bond(s).
[0014] In another aspect, the present disclosure provides a process of preparation of the resin coating composition, comprising: a) preparing oxidized natural gum by treating natural gum with oxidizing agent; b) mixing the oxidized natural gum with cross-linking forming agent(s) in acidic conditions at pH in the range of 4 to 5 to obtain a crosslinked material; and c) adding and mixing the crosslinked material with film forming agent to obtain the resin coating composition.
[0015] In yet another aspect, the present disclosure provides a device comprising the resin coating composition and a substrate, wherein the resin coating composition is coated onto the substrate.
[0016] In yet another aspect, the present disclosure provides a process of preparation of the device comprising coating the resin coating composition onto a substrate followed by drying to obtain the device. BRIEF DESCRIPTION OF ACCOMPANYING DRAWINGS OF THE DISCLOSURE
[0017] FIG. 1 illustrates the synthetic protocol of resin coating composition synthesized, in accordance with embodiments of the present disclosure.
[0018] FIG. 2 illustrates the (A) oxidation of neem gum being natural gum (NG); (B) formation of acyl hydrazone bond; and (C) formation of hydrogen bond, in accordance with embodiments of the present disclosure.
[0019] FIG. 3a shows (A) combined FTIR Spectra of NGSHF-1.56, (B) spectra of NGSHF-2.94, (C) spectra of NGSHF-4.17, and (D) spectra of NGSHF-5.26, where the NGSHF is resin coating composition in the form of a film, and the values 1.56, 2.94, 4.17, and 5.26 are weight % of the natural gum contained in the composition.
[0020] FIG. 3b shows deconvoluted spectra of FTIR peaks from 3000-3700cm-1 of NGSHF or SHF, where (A) shows spectra of NGSHF-1.56, (B) shows spectra of NGSHF-2.94, (C) shows spectra of NGSHF-4.17, and (D) spectra of NGSHF-5.26, where the NGSHF / SHF is resin coating composition in the form of film, and the values 1.56, 2.94, 4.17, and 5.26 are weight % of the natural gum contained in the composition.
[0021] FIG. 4a shows 1H-NMR spectra of natural gum (NG).
[0022] FIG. 4b shows 1H-NMR spectra of oxidized natural gum (O-NG).
[0023] FIG. 4c shows 1H-NMR spectra of crosslinked natural gum (O-NG-AHx).
[0024] FIG. 5 shows (a) schematic representation of self-healing mechanism, and (b) optical microscope images of the cracked and self-healed films of the resin coating composition.
[0025] FIG. 6a shows amplitude sweep of NGSHFs at room temperature.
[0026] FIG. 6b shows storage modulus and loss modulus versus angular frequency plot of NGSHF at room temperature.
[0027] FIG. 6c shows step strain test of all NGSHFs prepared and disclosed in the present disclosure.
[0028] FIG. 7 shows stress-strain curve of all NGSHFs prepared and disclosed in the present disclosure.
[0029] FIG. 8 shows contact angle of control and RCG prepared and disclosed in the present disclosure.
[0030] FIG. 9 shows SEM images of control and all RCG prepared and disclosed in the present disclosure.
[0031] FIG. 10 shows UV data of all the coatings (as coated device disclosed herein) and the transparency of each coating. DETAILED DESCRIPTION OF THE DISCLOSURE
[0032] The following is a detailed description of embodiments of the disclosure. The embodiments are in such detail as to clearly communicate the disclosure. However, the amount of detail offered is not intended to limit the anticipated variations of embodiments; on the contrary, the intention is to cover all modifications, equivalents, and alternatives falling within the spirit and scope of the present disclosure.
[0033] All publications herein are incorporated by reference to the same extent as if each individual publication or patent application were specifically and individually indicated to be incorporated by reference. Where a definition or use of a term in an incorporated reference is inconsistent or contrary to the definition of that term provided herein, the definition of that term provided herein applies, and the definition of that term in the reference does not apply.
[0034] Reference throughout this specification to “one embodiment” or “an embodiment” means that a particular feature, structure or characteristic described in connection with the embodiment is included in at least one embodiment. Thus, the appearances of the phrases “in one embodiment” or “in an embodiment” in various places throughout this specification are not necessarily all referring to the same embodiment. Furthermore, the particular features, structures, or characteristics may be combined in any suitable manner in one or more embodiments.
[0035] In some embodiments, numbers have been used for quantifying weight percentages, ratios, and so forth, to describe and claim certain embodiments of the disclosure and are to be understood as being modified in some instances by the term “about.” Accordingly, in some embodiments, the numerical parameters set forth in the written description and attached claims are approximations that can vary depending upon the desired properties sought to be obtained by a particular embodiment. In some embodiments, the numerical parameters should be construed in light of the number of reported significant digits and by applying ordinary rounding techniques. Notwithstanding that the numerical ranges and parameters setting forth the broad scope of some embodiments of the disclosure are approximations, the numerical values set forth in the specific examples are reported as precisely as practicable. The numerical values presented in some embodiments of the disclosure may contain certain errors necessarily resulting from the standard deviation found in their respective testing measurements.
[0036] Various terms as used herein are shown below. To the extent a term used in a claim is not defined below, it should be given the broadest definition persons in the pertinent art have given that term as reflected in printed publications and issued patents at the time of filing.
[0037] As used in the description herein and throughout the claims that follow, the meaning of “a,” “an,” and “the” includes plural reference unless the context clearly dictates otherwise. Also, as used in the description herein, the meaning of “in” includes “in” and “on” unless the context clearly dictates otherwise.
[0038] Unless the context requires otherwise, throughout the specification which follow, the word “comprise” and variations thereof, such as “comprises” and “comprising” are to be construed in an open, inclusive sense that is as “including, but not limited to.”
[0039] The recitation of ranges of values herein is merely intended to serve as a shorthand method of referring individually to each separate value falling within the range. Unless otherwise indicated herein, each individual value is incorporated into the specification as if it were individually recited herein.
[0040] All methods described herein can be performed in any suitable order unless otherwise indicated herein or otherwise clearly contradicted by context. The use of any and all examples, or exemplary language (e.g. “such as”) provided with respect to certain embodiments herein is intended merely to better illuminate the disclosure and does not pose a limitation on the scope of the disclosure otherwise claimed. No language in the specification should be construed as indicating any non-claimed element essential to the practice of the disclosure.
[0041] Groupings of alternative elements or embodiments of the disclosure disclosed herein are not to be construed as limitations. Each group member can be referred to and claimed individually or in any combination with other members of the group or other elements found herein. One or more members of a group can be included in, or deleted from, a group for reasons of convenience and / or patentability. When any such inclusion or deletion occurs, the specification is herein deemed to contain the group as modified.
[0042] The description that follows, and the embodiments described therein, is provided by way of illustration of an example, or examples, of particular embodiments of the principles and aspects of the present disclosure. These examples are provided for the purposes of explanation, and not of limitation, of those principles and of the disclosure.
[0043] It should also be appreciated that the present disclosure can be implemented in numerous ways, including as a system, a method or a device. In this specification, these implementations, or any other form that the disclosure may take, may be referred to as processes. In general, the order of the steps of the disclosed processes may be altered within the scope of the disclosure.
[0044] The headings and abstract of the disclosure provided herein are for convenience only and do not interpret the scope or meaning of the embodiments.
[0045] The following discussion provides many example embodiments of the inventive subject matter. Although each embodiment represents a single combination of inventive elements, the inventive subject matter is considered to include all possible combinations of the disclosed elements. Thus, if one embodiment comprises elements a, b, and c, and a second embodiment comprises elements b and d, then the inventive subject matter is also considered to include other remaining combinations of a, b, c, or d, even if not explicitly disclosed.
[0046] The term “NGSHF” is used herein refer to the resin composition as tested in the form of film.
[0047] The term “RCG” is used herein refer to resin coated glass, where the resin in RCG is the resin coating composition of the present disclosure.
[0048] The “room temperature” indicated throughout the specification refer to a temperature in the range of 20 to 35 °C.
[0049] In an embodiment, the present disclosure relates to a resin coating composition, comprising: i) natural gum(s); ii) cross-linking agent(s); and iii) film-forming agent, wherein the composition comprises dual crosslinking via acyl hydrazone bond(s) and hydrogen bond(s).
[0050] In some embodiments, the natural gum(s) is / are selected from but not limited to Azadirachta indica gum (also termed as neem gum) (NG), cellulose, carboxymethyl cellulose (CMC), chitosan, starch, starch-based derivatives, shellac, hyaluronic acid (HA), and gelatin or any combination thereof.
[0051] In some embodiments, the cross-linking forming agent(s) is / are selected from but not limited to adipic acid dihydrazide (ADH), sebacic dihydrazide (SDH), isophthalic dihydrazide (IDH), adipic acid di(propylidene hydrazide), adipic acid di(2-propylidene hydrazide), silane-polyurethane hybrids, silyl-polyurethane, amino-functional siloxane resin, and genipin or any of combination thereof.
[0052] In some embodiments, the film forming agent(s) is / are selected from but not limited to polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), cellulose and derivatives thereof, pullulan (a biodegradable polysaccharide), chitosan, proteinoid polymer, poly(acrylic acid) (PAA), poly(2-hydroxyethyl acrylate), polyacrylamide, methyl acrylate copolymer, ethyl acrylate copolymer, methacrylic acid copolymer, Poly(ethylene glycol) (PEG), water soluble silicone, hydrophilic urethane polymer, modified polyvinyl alcohol, and modified polyvinyl acetate or any of combination thereof.
[0053] In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 1 to 6% w / v.
[0054] In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 1.56 to 5.26% w / v.
[0055] In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 2 to 5.26% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 2.26 to 5.26% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 2.56 to 5.26% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 2.94 to 5.26% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 3.15 to 5.26% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 3.5 to 5.26% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 4.17 to 5.26% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 1.56 to 5% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 1.56 to 4.75% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 1.56 to 4.5% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 1.56 to 4% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 1.56 to 3.5% w / v. In some embodiments, the amount / concentration of the natural gum(s) in the composition is in the range of 1.56 to 2.94% w / v.
[0056] In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 1 to 6% w / v.
[0057] In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 1.56 to 5.26% w / v.
[0058] In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 2 to 5.26% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 2.26 to 5.26% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 2.56 to 5.26% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 2.94 to 5.26% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 3.15 to 5.26% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 3.5 to 5.26% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 4.17 to 5.26% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 1.56 to 5% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 1.56 to 4.75% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 1.56 to 4.5% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 1.56 to 4% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 1.56 to 3.5% w / v. In some embodiments, the amount / concentration of the crosslinking agent(s) in the composition is in the range of 1.56 to 2.94% w / v.
[0059] In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 1 to 6% w / v.
[0060] In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 1.56 to 5.26% w / v.
[0061] In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 2 to 5.26% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 2.26 to 5.26% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 2.56 to 5.26% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 2.94 to 5.26% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 3.15 to 5.26% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 3.5 to 5.26% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 4.17 to 5.26% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 1.56 to 5% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 1.56 to 4.75% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 1.56 to 4.5% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 1.56 to 4% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 1.56 to 3.5% w / v. In some embodiments, the amount / concentration of the film forming agent(s) in the composition is in the range of 1.56 to 2.94% w / v.
[0062] In some embodiments, the rest of composition comprises water or demineralised water.
[0063] In some embodiments, the composition is in the form of film, sheet, liquid spray, cream, gel, wet wipe, aqueous dispersion, aqueous emulsion, and concentrated solution.
[0064] In some embodiments, the composition has a self-healing characteristic.
[0065] In some embodiments, the composition is hydrophilic in nature.
[0066] In some embodiments, the absorbance of the acyl hydrazone bond(s) in the composition is in the range of 0.286 to 0.479. This trend from 0.286 to 0.479 indicates that the aldehyde groups undergo condensation with the hydrazide group, forming a higher number of acylhydrazone bonds.
[0067] In some embodiments, the hydrogen bond content in the composition is in the range of 44.18 to 60.9%.
[0068] In some embodiments, the solid content contained in the composition is in the range of 6.56 to 22.11% w / v.
[0069] In another embodiment, the present disclosure provides a process of preparation of the resin coating composition, comprising: a) preparing oxidized natural gum by treating natural gum solution with oxidizing agent; b) mixing the oxidized natural gum with cross-linking forming agent(s) under stirring in acidic conditions at pH in the range of 4 to 5 to obtain a crosslinked material; and c) adding and mixing the crosslinked material with film forming agent to obtain the resin coating composition.
[0070] In some embodiments, the oxidizing agent used in step a) is selected from but not limited to hydrogen peroxide, sodium periodate (NaIO4), sodium hypochlorite (NaOCl), potassium persulfate, ammonium persulfate, peracetic acid, sodium percarbonate, and urea peroxide or any of combination thereof.
[0071] In some embodiments, the natural gum solution as used in step a) is prepared by mixing natural gum with water under stirring at temperature in the range of 25-35 °C for time period in the range of 1.5 to 3 hours.
[0072] In some embodiments, the step a) is done at temperature in the range of 60 to 70 °C for time period in the range of 45 to 75 minutes.
[0073] In some embodiments, the acidic conditions in step b) is attained by adding acid solution.
[0074] In some embodiments, the concentration of the acid solution is in the range of 0.5 to 1.5 M.
[0075] In some embodiments, the acid solution is made by mixing acid and water / demineralized water.
[0076] In some embodiments, the acid is selected from but not limited to hydrochloric acid, sulfuric acid and nitric acid.
[0077] In some embodiments, the step b) is done at temperature in the range of 20 to 35 °C for time period in the range of 90 to 150 minutes.
[0078] In some embodiments, step c) is done at a temperature in the range of 20 to 35 °C for a time period in the range of 22 to 26 hours.
[0079] In additional embodiments, the resin coating composition as obtained in step c) is additionally made into a form selected from but not limited to film, sheet, liquid spray, cream, gel, wet wipe, aqueous dispersion, aqueous emulsion, and concentrated solution.
[0080] In yet another embodiment, the present disclosure provides a device comprising the resin coating composition and a substrate, wherein the resin coating composition is coated onto the substrate.
[0081] In some embodiments, the substrate is selected from but not limited to glass slide, polycarbonate (PC), polyethylene terephthalate (PET), polymethyl methacrylate (PMMA / Acrylic), polydimethylsiloxane (PDMS), stainless steel, metal surface, silicon wafers, quartz, aluminium (Al) films, polymeric Membrane, textile material, fabric material and so on.
[0082] In some embodiments, the device is anti-fogging device where the resin coating composition acts as coating material which prevents fogging or humid droplet formation on the substrate.
[0083] In some embodiments, the device comprises a thickness of the coating composition onto the substrate is in the range of 0.064 to 0.152mm.
[0084] In some embodiments, the coating composition onto device is self-healing within at least 5 minutes. The self-healing as observed was attributed to the dynamic and reversible nature of acyl hydrazone bonds and hydrogen bonds present within the polymer network of the composition.
[0085] In some embodiments, the contact angle of the coating composition coated onto the device is in the range of 66.02 ± 10.36° to 38.52 ± 5.33°.
[0086] In some embodiments, the surface energy (ΔG) of the coating composition onto the device is in the range of -102.39 to -129.76 mN / m. This signifies a more thermodynamically favourable wetting state, and the negative ΔG indicates higher surface energy, facilitating droplet spreading and reducing the energy barriers to wetting. This trend confirms that introducing hydrophilic groups through coating significantly enhances surface hydrophilicity and antifogging performance.
[0087] In some embodiments, the surface of coating composition onto the device comprises: i) sparse, island-like resin domains, indicating incomplete coverage; ii) evenly dispersed resin clusters with partial merging, reflecting the onset of continuous film formation; iii) compact, continuous coating with minimal gaps; and / or iv) dense, smooth, and fully covered surface.
[0088] In yet another embodiment, the present disclosure provides a process of preparation of the device comprising coating the resin coating composition onto a substrate followed by drying to obtain the device.
[0089] In some embodiments, said coating step is done at temperature in the range of 20 to 35 °C.
[0090] In specific embodiments, the present disclosure provides formulations of oxidized-Azadirachta indica gum (O-NG), Adipic acid dihydrazide (ADH), and Polyvinyl alcohol (PVA)- based self-healing resin were prepared. The resin consists of dual crosslink, viz., chemical crosslink via acyl hydrazone bond and physical crosslink via hydrogen bond. Fourier transform infrared spectroscopy and proton nuclear magnetic resonance spectroscopy confirm the presence of dual crosslinking in the resin. The different formulations of resin were prepared by varying the concentration of neem gum from 1.56% w / v to 5.26 %w / v and poured on a petri plate, and films of thickness 0.064 to 0.152mm were formed by the solvent casting method. The films having neem gum concentration 1.56 %w / v showed the highest tensile strength of 18.56 MPa and excellent self-healing property. The self-healing properties of films were analysed qualitatively by an optical microscope and quantitatively by a rheometer. Contact angle analysis revealed that surface hydrophilicity increased with an increase in concentration of neem gum. The resin with the varying concentration of neem gum was coated on the glass slide and labelled as resin-coated glass (RCG). RCG-5.26 showed the lowest contact angle (38.52°), compared to the control (70.73°). Surface morphology observed by SEM showed discontinuous patches in RCG-1.56, which evolved into a homogeneous and compact structure in RCG-5.26. While RCG-5.26 demonstrated superior antifogging performance owing to its high hydrophilicity (contact angle: 38.52°), which promoted uniform water film formation, the control sample exhibited poor transparency due to discrete fog droplet formation. UV data revealed that all RCG samples maintained high optical transparency (>98.5%) in the visible range (400–800 nm), with RCG-5.26 showing only a slight reduction, indicating minimal light scattering.
[0091] While the foregoing description discloses various embodiments of the disclosure, other and further embodiments of the disclosure may be devised without departing from the basic scope of the disclosure. The disclosure is not limited to the described embodiments, versions or examples, which are included to enable a person having ordinary skill in the art to make and use the disclosure when combined with information and knowledge available to the person having ordinary skill in the art.EXAMPLES
[0092] Materials used: Azadirachta indica gum was purchased from Indian Jadibooti Pvt. Ltd., Tamil Nadu, India. Hydrogen peroxide 30% (w / v) was procured from Rankem, Adipic acid dihydrazide (ADH) 95% was obtained from BLD Pharm, HCl was purchased from CDH, and Polyvinyl alcohol (PVA)-hot (M.W: Average 60000-1250000, hydrolysis (mole%):87-89% bought from CDH. Borosil glass slides were used as it is. All the chemicals were used without further purification, and deionized water was used throughout the experiment.
[0093] Preparation of Coating Composition as Film:
[0094] Preparation of Oxidized NG: NG was oxidized using hydrogen peroxide. Briefly, a solution of a known amount of NG with deionized water was prepared at room temperature for 24 hours. Subsequently, a known amount of hydrogen peroxide was added to the solution, and the reaction mixture was stirred at 65 °C for 1 hour. After the oxidation, the sample was abbreviated as O-NGx (Where x is the concentration of NG).
[0095] Preparation of Self-healing Resin: The required concentration of ADH was added in a known concentration of O-NGx solution prepared in distilled water under 1M HCl to maintain a mild acidic condition, pH=4.5, which was later stirred at room temperature for 24 hours. This solution was named O-NG-AHx. The O-NG-AHx solution was mixed with a known amount of PVA solution and stirred at room temperature for 24 hours. This solution was named O-NG-AH-HBx. The O-NG-AH-HBx solution was poured into a petri plate, and films were formed using the solution casting method, and the films were named as NGSHF. Four different films were prepared by varying the composition of NG / ADH / PVA and named as NGSHF-1.56, NGSHF-2.94, NGSHF-4.17, and NGSHF-5.26. The chemical composition and condition of preparation, and the solid content are given in Table 1. Table 1: Chemical composition, conditions of preparation, and solid content
[0096] FIG. 1 describes the synthesis of aldehyde groups on neem gum utilizing hydrogen peroxide as an oxidant, which converts the hydroxyl groups of neem into aldehyde groups, the solution labelled as O-NGx. The aldehyde groups of oxidized neem gum can covalently establish crosslinks with the hydrazide group of ADH through an Acyl hydrazone bond, which was labelled as O-NG-AHx. This solution with an acyl hydrazone bond was later crosslinked with the hydroxyl group of PVA to form Hydrogen bonding, which was abbreviated as O-NG-AH-HBx. This solution was poured onto a petri plate to form a self-healing film, further characterized as below.
[0097] The macromolecular chain of Azadirachta indica contains mainly arabinose, galactose, and glucuronic acid. A represented sugar molecule has been taken as a standard for proposing the mechanism. The proposed reaction scheme is shown in FIG. 2. By using H2O2 as an oxidizing agent, which converts the hydroxyl group (-OH) of NG into an aldehyde group (-CHO), abbreviated as (O-NGx), as shown in FIG. 2a. The aldehyde group of O-NGx reacts with the hydrazide group (–CONHNH₂) of ADH to form an acyl hydrazone bond labelled as O-NG-AHx, as shown in FIG. 2b. The O-NG-AHx react with the hydroxyl group (-OH) of PVA to form a hydrogen bond, labelled as O-NG-AH-HBx, shown in FIG. 2c.
[0098] Preparation of Antifogging Coating (the device disclosed herein): The resin solution O-NG-AH-HBx of varying concentration of NG, ranging from 1.56 -5.26 % (w / v) was coated on a glass slide using another glass slide, followed by air drying. The coated samples were named as RCG-1.56, RCG-2.94, RCG-4.17, and RCG-5.26. Here, RCG-1.56 means that the resin contains 1.56% (w / v) of NG concentration. Characterization and Analysis of prepared compositions and devices:
[0099] A) FTIR analysis:
[00100] FTIR Spectrometer (Nicolet iS50) was used to determine the functional group present in NG, O-NG, O-NG-AH, and O-NG-AH-HB, analysed between 4000- 400 cm-1. FIG. 3 illustrates the FTIR Spectra of neem gum (NG), oxidized NG, oxidized NG and acyl hydrazone network (O-NG-AH), oxidized NG and acyl hydrazone and hydrogen-bonded network (O-NG-AH-HB). In neem gum (NG), the broad peak is at 3318 cm-1 due to OH stretching vibration, and 2918 cm-1 is due to CH stretching of the CH3 group. The strong band at 1602 cm-1 was due to the carbonyl stretching mode, and the peak at 1014 cm-1 was due to the CO stretching vibration of the alcoholic group. The O-NG peak at 1735 cm-1 was due to the carbonyl stretching of the aldehyde group. In O-NG-AH, the peak at 3207 cm-1 is due to NH stretching of the hydrazone group of ADH, 1683 cm-1 is CO stretching of ADH, and the peak at 1598 cm-1 is due to the imine bond (C=N) due to the reaction of NH2 of ADH with CHO of O-NG to form a (-CH=N-NH-) acyl hydrazone bond.
[00101] The FTIR spectra of O-NGx, O-NG-AHx (where x= 1.56, 2.94, 4.17, 5.26 % concentration of NG). The absorption peaks at 1735 and 1598 cm-1 were used to calculate the amount of aldehyde and acyl hydrazone content using the Beer-Lambert law.
[00102] As per Beer-Lambert law:(i) [Equation] (1)
[00103] Where A is absorption, ϵis the molar extinction coefficient, and c is concentration, l is the path length. The absorption can be calculated from the % T peak using the formula given below:(ii) [Equation] (2)
[00104] From the above formula, it was clear that the concentration of a particular group is directly proportional to absorbance. The absorbance values were calculated from transmittance using the Beer–Lambert law (A = εlc), which establishes a linear relationship between absorbance and concentration under controlled conditions.
[00105] The data on aldehyde and acylhydrazone content are shown in Table 2. It was observed that the absorption value shows a non-linear trend. FTIR analysis revealed a gradual decrease in the characteristic aldehyde absorption at 1735 cm⁻¹ across the samples NGSHF 1.56 to NGSHF 5.26. The %T values dropped from 90.27 to 83.31, while the corresponding absorbance increased from 0.045 to 0.080. This inverse relationship indicates that as the neem gum concentration increases, fewer free aldehyde groups remain in the system, suggesting their progressive consumption during the reaction. The diminishing aldehyde signal highlights the ongoing condensation reaction with hydrazide groups, which leads to acylhydrazone bond formation in the final material. The aldehyde groups in oxidized polysaccharides can convert into hemiacetal or hydrated forms, which exhibit weak FTIR signals, thereby justifying the non-linear absorbance trend.Table 2: Amount of acylhydrazone content in all samples / compositions
[00106] Similarly, the increase in acyl hydrazone bond absorption at 1598 cm⁻¹ from NGSHF 1.56 to NGSHF 5.26. The %T values decreased significantly from 51.77% to 33.28%, while the corresponding absorbance rose from 0.286 to 0.479. This trend indicates that as the NGSHF concentration increased, more aldehyde groups undergo condensation with the hydrazide group, forming a higher number of acylhydrazone bonds.
[00107] The amount of hydrogen bonding was analysed as per the protocol described by Dai and coworkers (ACS Omega, vol. 8, no. 19, pp. 17064–17076, 2023). Briefly, the FTIR peak from 3000-3700 cm-1 was considered to calculate the hydrogen bonding using Lorentz fitting. Hydrogen bonding (HB%) calculated using equation 3 given below in Table 3, by comparing the area of bonded and free OH in FTIR spectra.% Hydrogen bonding = ×100 (3)Table 3: Amount of hydrogen bonding content in all samples / compositions
[00108] HB% content decreases with an increase in concentration from NGSHF-1.56 to NGSHF-5.26, from 60.9% to 44.18% respectively. This is possibly due to increased viscosity, which limits the formation of hydrogen bonding.
[00109] B) NMR analysis:
[00110] 1HNMR Bruker advance III, 400MHz was used to analyse the NG, O-NG, O-NG-AH samples using (dimethyl sulfoxide-d6) as a solvent. FIG. 4 shows the 1H-NMR of NG, O-NG, and O-NG-AH samples. Specifically, FIG. 4 (a) illustrates that the peak at 2.5 ppm is of solvent DMSO-d6. The spectral band between 3.3- 5.2 ppm is due to the protons of different sugars present in neem gum. FIG. 4 (b) illustrates the new sharp peak at 10.224 ppm is due aldehyde (-CHO) proton. FIG. 4 (c) illustrates the peak at 2.5 ppm of solvent DMSO-d6. The peak at 8.934 ppm is due to H in (-CH=N-). The peak at 9.882 ppm is due to H in (-N-NH-). Together, they confirm the presence of an acyl hydrazone bond in O-NG-AHx.
[00111] C) Optical analysis:
[00112] Optical images of both control and self-healing films were studied using Motic SMZ-1613. The qualitative self-healing behavior was studied using the crack-healing observation method as proposed by Cash and co-worker (Macromolecules, vol. 48, no. 7, pp. 2098–2106, 2015). Surface cracks were introduced on synthesized films of (NGSHF-1.56), (NGSHF-2.94), (NGSHF-4.17), and (NGSHF-5.26), with thicknesses of 0.062, 0.115,0.134,0.160 mm, respectively. A scratch was manually introduced on each film using a scissor, and a few drops of deionized water were gently applied to the scratched region at room temperature. The self-healing process was monitored using an optical microscope, as shown in FIG. 5, and images were captured at two-time intervals: immediately after scratching (labelled as “Cracked Film”) and after 5 minutes of water treatment (labelled as “Healed Film”). The optical images clearly confirm that all four films exhibited self-healing within 5 minutes. The observed self-healing was attributed to the dynamic and reversible nature of acyl hydrazone bonds and hydrogen bonds present within the polymer network, which was earlier confirmed by FTIR and 1H NMR.
[00113] D) Analysis of viscoelasticity of the compositions:
[00114] The rotational rheometer MCR 302 of Anton Paar GmbH, Graz, Austria, with parallel plate fixtures of 25 mm diameter, was used for viscoelastic characterizations of the SHFs.
[00115] The oscillatory strain sweep was measured to determine a linear viscoelastic region (LVER) in shear strain ranges from 0.01 % to 100 % at 10 rad / s angular frequency.
[00116] The amplitude sweep was carried out to determine the viscoelastic behaviour of the films at room temperature under shear strain % of 0.01% to 100% at 10 rad / s steady frequency. As shown in FIG. 6 (a), the storage modulus (G′) and loss modulus (G′′) were plotted against shear strain to identify the crossover point, where G′ equals G′′. The corresponding strain value at this point, referred to as the crossover strain, represents the transition from solid-like (elastic) to liquid-like (viscous) behaviour and serves as an indicator of the structural integrity of the material. This crossover point represents the transition from solid (elastic-like) to liquid (viscous-like) behaviour and indicates the material's structural integrity. The crossover strain increases from 0.46 % in NGSHF-1.56 to 1.22 % in NGSHF-4.17, indicating progressive film strength. However, a sharp decrease in crossover strain to 0.179% in NGSHF-5.26 may be due to excessive crosslinking and restricted chain mobility, leading to brittleness and premature failure.
[00117] The frequency sweep analysis demonstrates the viscoelastic behaviour of NGSHF across different angular frequencies at a shear strain of 0.05%, angular frequencies (0.1- 100 rad / s) at room temperature. The frequency sweep analysis demonstrates the viscoelastic behaviour of NGSHF across different angular frequencies at a shear strain of 0.05%, angular frequencies (0.1- 100 rad / s) at room temperature. As given in FIG. 6 (b), for NGSHF-1.56, the storage modulus (G′ : 6116.8 Pa) exceeds the loss modulus (G″: 4186.1 Pa) at 0.1 rad / s, and this dominance of G′ persists across all frequencies, confirming an elastic-dominated response. NGSHF-2.94 displays a comparable trend (G′:6233.6 Pa, G″: 4083.8 Pa at 0.1 rad / s), with both moduli rising steadily with frequency, indicating progressive network stiffening. A stronger viscoelastic reinforcement is evident in NGSHF-4.17, where G′:28,169 Pa was substantially higher than G″:12,482 Pa. The highest rigidity was observed for NGSHF-5.26, showing G′: 41,584 Pa and G″:19,881 Pa at 0.1 rad / s. In all cases, G′ remains higher than G″ (tan δ < 1), confirming a gel-like, elastic-dominated behaviour, with stiffness systematically increasing from NGSHF-1.56 to NGSHF-5.26.
[00118] The mechanical properties of all control and their (NGSHFs) were studied through tensile testing, and the results are presented in FIG. 7 (A-D) and Table 4. At lower concentrations (1.56 % w / v), the NGSHF-1.56 film exhibited improved mechanical strength with an increase in Young’s modulus (234.92 to 296.68 MPa) and tensile strength (16.43 to 18.56 MPa) compared to Control-1.56, while maintaining comparable elongation. This suggests successful self-healing with minimal compromise on flexibility. In contrast, at 2.94% w / v, both Young’s modulus and tensile strength exhibited a slight reduction in the self-healed NGSHF-2.94 sample compared to its (Control-2.94), indicating a relatively less efficient healing response, potentially due to incomplete structural restoration at this concentration. A significant enhancement in stiffness was observed at 4.17%, where NGSHF-4.17 showed a remarkably high Young’s modulus (806.34 MPa) and tensile strength (27.44 MPa), closely approaching the control values. However, its extension at break dropped sharply (4.58 mm), implying a trade-off between rigidity and flexibility in the self-healed state. At the highest concentration (5.26%), the NGSHF-5.26 film maintained high tensile strength (26.79 MPa) and showed similar ductility to undamaged, indicating effective mechanical recovery and balanced performance. Table 4: Mechanical properties of NGSHFs / compositions prepared
[00119] F) Self-healing capacity analysis:
[00120] Oscillatory step-strain measurements were used to assess the self-healing capacity. At a low strain value of 0.5 % for 120 sec, the strain shifted to a high value of 100 % for 120 sec and back to a 0.5 % strain value for 120 sec. A quantitative self-healing test was carried out using a step-strain test and a rheometer, as described in the materials and methods section. The results are shown in FIG. 6(c), all samples exhibited a characteristic three-phase response: During the initial phase (120 s) at a low strain of 0.5%, both G´ and G´´ remained stable. In the second stage (120 s) at a high strain of 100%, a sharp decline in both G´ and G´´ was observed. Following the removal of applied strain (120s), at a low strain of 0.5%, the samples exhibited varying degrees of G´ and G´´ recovery. This trend correlates with the HB% determined by FTIR, as shown in FIG. 3(b) which decreased from 60.9% in NGSHF 1.56 to 44.18% in NGSHF 5.26. As hydrogen bonds serve as physical crosslinks, their reduction at higher concentrations, likely due to increased viscosity and steric hindrance, limits chain mobility and reversible interactions, thereby reducing the modulus and network recovery. This, in turn, decreases their self-healing ability of films.
[00121] G) Hydrophilic nature analysis:
[00122] Water contact angle of control and RCG was studied using KRUSS, Advance 1.6.2.0. Scanning electron microscope (SEM) of JEOL JSM-6610LV used to analyse surface morphology of control and RCG. FIG. 8 illustrates water contact angle of control, 70.73 ± 4.05°, which was hydrophilic in nature. On coating, noticeable decrease in contact angle was observed from 66.02 ± 10.36° in RCG-1.56, 59.19 ± 4.92° in RCG-2.94, 47.84 ± 9.9° in RCG-4.17, and 38.52 ± 5.33° in RCG-5.26. This progressive reduction in contact angle with higher neem gum content confirms significant enhancement in surface hydrophilicity. Decreasing contact angle indicates that coating introduces hydrophilic groups, which enhance surface wettability.
[00123] The surface roughness and uneven chemistry influence droplet behavior by creating energy barriers that hinder smooth spreading. These barriers make the contact angle higher or lower than expected, leading to hysteresis. To move the droplet or reach the real contact angle, Gibbs' free energy (ΔG) is needed to overcome these barriers.
[00124] Gibbs Free energy is calculated using the Young-Dupre equation: [Equation] Where γ is 72.8 mN / m (surface tension of water)θ = contact angle in degrees
[00125] This improved wettability is further supported by the corresponding (ΔG) values given below in Table 5, which became more negative, from −96.83 mN / m for the control to −129.76 mN / m for RCG-5.26, signifying a more thermodynamically favourable wetting state. The increased negative ΔG indicates higher surface energy, facilitating droplet spreading and reducing the energy barriers to wetting. This trend confirms that introducing hydrophilic groups through coating significantly enhances surface hydrophilicity and antifogging performance. Table 5: Contact Angle and Surface Energy Trends
[00126] H) Surface Analysis of the device prepared (SEM analysis):
[00127] The surface morphology of the control and the RCG with varying concentrations of neem gum (RCG-1.56, RCG-2.94, RCG-4.17, and RCG-5.26) was examined using SEM (FIG. 9). The smooth morphology of the control slide confirmed the absence of any surface coating. In contrast, the RCG samples exhibited concentration-dependent morphological changes with increasing concentration from (1.56 to 5.26% w / v). At the lowest concentration (RCG-1.56), the surface exhibited sparse, island-like resin domains, indicating incomplete coverage. This aligns with its relatively high WCA (66.02°) and less negative ΔG (−102.39 mN·m-1), which reflect poor wetting; the limited spreading and low solids content allowed surface-tension–driven dewetting during evaporation, leading to the formation of discontinuous patches. As the concentration increased to RCG-2.94, the WCA decreased (59.19°) and ΔG became more negative (−110.09 mN·m-1), indicating enhanced wetting. The SEM showed more evenly dispersed resin clusters with partial merging, reflecting the onset of continuous film formation. In RCG-4.17, the WCA dropped further (47.84 °) and ΔG became more negative (−121.66 mN·m-1), and the SEM revealed a compact, continuous coating with minimal gaps. In (RCG-5.26), the WCA reached (38.52 °) with the most negative ΔG (−129.76 mN·m-1), and SEM displayed a dense, smooth, and fully covered surface. This strong correlation indicates that enhanced wettability (lower WCA and more negative ΔG), together with higher solids content, gradually minimizes dewetting and promotes the formation of a uniform and continuous coating.
[00128] I) UV analysis:
[00129] UV-Visible Spectrophotometer (Solid State), Agilent Cary 5000, was used to evaluate the transparency of control and RCG at room temperature at a scan range of 400-800nm. The UV spectra (FIG. 10) show that all coatings, including the control and coated samples (RCG-1.56 to RCG-5.26), exhibit exceptionally high transparency across the visible wavelength range of 400–800 nm. The % transmittance measured at 550 nm indicates that the control film has the highest transparency (77.76%), reflecting minimal light scattering. Among the coated films, RCG-5.26 exhibits the highest transmittance (69.05%), followed by RCG-2.94 (51.00%), RCG-4.17 (46.52%), and RCG-1.56 (40.27%). The progressive reduction in %T with increasing modification level suggests enhanced light–matter interaction and slight scattering introduced by the dual crosslinked network. Nevertheless, even the most modified film (RCG-5.26) maintains appreciable transparency (>60%), confirming that the coating process does not significantly compromise visible clarity. This observation is further supported by the coated film photographs, where the underlying text “CHEMISTRY” remains clearly visible.
[00130] J) Antifogging testing of the device:
[00131] The antifogging testing of samples was performed as described by Hu et al., (refer, “Layer-by-layer assembly of polysaccharide films with self-healing and antifogging properties for food packaging applications,” ACS Applied Nano Materials, vol. 1, no. 7, pp. 3733–3740, 2018). The antifogging of the film was studied by transferring an uncoated glass and a coated glass slide from a −10 °C refrigerator (frozen for 4 hours) to laboratory conditions (25 °C). A backdrop covered with the words “DTU” was placed behind the two glass slides to check the fogging behaviour.
[00132] The antifogging results directly correlate with the contact angle and surface energy trends. The control, with a contact angle of 70.73° and ΔG of −96.83 mN / m, exhibited significant fog formation due to poor wettability, leading to discrete droplet formation and light scattering. In contrast, the RCG samples showed a progressive reduction in contact angle, reaching 38.52° with a ΔG of −129.76 mN / m for RCG 5.26. This highly hydrophilic surface facilitated the uniform spreading of condensed water into a continuous thin film, thereby preventing fogging and maintaining clear visibility of the background. These results confirm that enhanced hydrophilicity through coating is crucial in achieving effective antifogging performance. The coating functions by enhancing hydrophilicity, which allows water to spread uniformly over the surface instead of forming discrete droplets. ADVANTAGES OF THE PRESENT DISCLOSURE
[00133] The present disclosure provides a self-healing resin system (resin coating compositions) derived from natural gum along with adipic dihydrazide (ADH), and polyvinyl alcohol (PVA), forming a dual crosslinked network through acyl hydrazone bonding and hydrogen-bonding interactions. This unique dual-network structure imparts simultaneous self-healing capability, mechanical robustness, optical transparency, and durable antifogging properties.
[00134] The synergistic interplay of reversible acyl hydrazone linkages and hydrogen-bonded domains enables rapid, autonomous surface repair, thereby preserving surface clarity and functionality.
[00135] It provides a sustainable, bio-based, and multifunctional polymeric coating that demonstrates long-term antifogging performance, increased self-healing efficiency, and greater environmental compatibility.
[00136] It provides a dual-network configuration which enables simultaneous dynamic covalent exchange and reversible hydrogen bonding interactions, resulting in superior self-healing ability, transparency, antifogging stability, and mechanical durability.
Claims
1. A resin coating composition, comprising: i) natural gum(s); ii) cross-linking agent(s); and iii) film forming agent; wherein the composition comprises dual crosslinking via acyl hydrazone bond(s) and hydrogen bond(s).
2. The resin coating composition as claimed in claim 1, wherein the natural gum(s) is / are selected from Azadirachta indica gum (neem gum) (NG), cellulose, carboxymethyl cellulose (CMC), chitosan, starch, starch-based derivatives, shellac, hyaluronic acid (HA), and gelatin or any of combination thereof.
3. The resin coating composition as claimed in claim 1, wherein the cross-linking forming agent(s) is / are selected from adipic acid dihydrazide (ADH), sebacic dihydrazide (SDH), isophthalic dihydrazide (IDH), adipic acid di(propylidene hydrazide), adipic acid di(2-propylidene hydrazide), silane-polyurethane hybrids, silyl-polyurethane, amino-functional siloxane resin, and genipin or any of combination thereof; and the film forming agent(s) is / are selected from polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), cellulose and derivatives thereof, pullulan (a biodegradable polysaccharide), chitosan, proteinoid polymer, poly(acrylic acid) (PAA), poly(2-hydroxyethyl acrylate), polyacrylamide, methyl acrylate copolymer, ethyl acrylate copolymer, methacrylic acid copolymer, Poly(ethylene glycol) (PEG), water soluble silicone, hydrophilic urethane polymer, modified polyvinyl alcohol, and modified polyvinyl acetate or any of combination thereof.
4. The resin coating composition as claimed in claim 1, wherein the amount / concentration of the natural gum(s) in the composition is in the range of 1 to 6% w / v.
5. The resin coating composition as claimed in claim 1, wherein the rest of composition comprises water or demineralised water.
6. A process of preparation of the resin coating composition as claimed in claim 1, comprising: a) preparing oxidized natural gum by treating natural gum solution with oxidizing agent; b) mixing the oxidized natural gum with cross-linking forming agent(s) under stirring in acidic conditions at pH in the range of 4 to 5 to obtain a crosslinked material; and c) adding and mixing the crosslinked material with film forming agent to obtain the resin coating composition.
7. The process as claimed in claim 6, wherein the oxidizing agent used in step a) is selected from but not limited to hydrogen peroxide, sodium periodate (NaIO4), sodium hypochlorite (NaOCl), potassium persulfate, ammonium persulfate, peracetic acid, sodium percarbonate, and urea peroxide or any of combination thereof.
8. The process as claimed in claim 6, wherein the natural gum solution as used in step a) is prepared by mixing natural gum with water under stirring at temperature in the range of 25-35 °C for time period in the range of 1.5 to 3 hours; and the step a) is done at temperature in the range of 60 to 70 °C for time period in the range of 45 to 75 minutes.
9. The process as claimed in claim 6, wherein the acidic conditions in step b) is attained by adding acid solution; a concentration of the acid solution is in the range of 0.5 to 1.5 M; the step b) is done at temperature in the range of 20 to 35 °C for time period in the range of 90 to 150 minutes; and the step c) is done at temperature in the range of 20 to 35 °C for time period in the range of 22 to 26 hours.
10. A device comprising the resin coating composition as claimed in claim 1, and a substrate, wherein the resin coating composition is coated onto the substrate.