White cement based water resistant putty and process of preparation thereof

IN607217BActive Publication Date: 2026-10-27HIL LIMITED
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202341033938
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2026-10-27
Estimated Expiration
2043-05-15
Patent Text Reader

Abstract

The present invention discloses white cement based water resistant putty and process of preparation thereof. The white cement based wall putty composition of the subject invention has good water resistance along with better compatibility, adhesion, workability, coverage and mechanical properties. The water resistant white cement based wall putty composition comprises 15 – 30 parts by weight of white cement, 25 – 55 parts by weight of inorganic filler material, 0.2 – 0.5 parts by weight of cellulose ether, 1 – 5 parts by weight of redispersible polymer powder, 15 – 50 parts by weight of coated mineral powder and 3 – 5 parts by weight of mineral clay. The selected raw materials of the white cement based water resistant wall putty composition shows synergistic effect on the performance including water resistance and cost effectiveness.
Need to check novelty before this filing date? Find Prior Art

Description

Field of the Invention:

[0001] The present invention relates to a white cement based waterresistant putty and process of preparation thereof. More particularly thepresent invention relates to a wall putty with higher water resistance alongwith improved physico-mechanical properties.Background of the invention:

[0002] White cement based wall putty is a fine powder which is mixed withwater and applied in the form of a thin layer mortar of less than 3 mmthickness to obtain a smooth skim coat on the internal and externalplaster surfaces.

[0003] The composition of white cement based wall putty comprises ofinorganic binders, inorganic fillers and additives such as thickeningagents, re-dispersible polymer powder, etc. to modify and improve theproperties of putty.

[0004] The conventional white cement based wall putty provides a smoothaesthetic finish with levelled surface, helps in removing undulation andfills the minor cracks, imperfections, gaps on the plaster wall. But it hasthe limitation of water resistance that allows the passage of water throughpores and capillaries as a result it reduces the life of decorative paints.

[0005] The Chinese publication CN104250466A discloses a waterresistant inner wall putty powder. The water resistant putty compositioncontains white cement 15 - 25 part, sierozem powder 20 - 30 part,redispersible glue powder 1 - 2 part, ether of cellulose 0.2 - 0.4 part,lignocellulose 0.3 - 0.5 part, thixotropic lubricant 0.1 - 3 part, talcumpowder 5 - 10 part and calcium carbonate 45 - 60 parts. The waterresistance of putty is achieved by selecting re-dispersible glue powder, highstrength white cement for excellent cohesive strength of putty andsierozem powder of suitable particle diameter in composition. Here,Sierozem powder is a type soil used as active filler material for good waterphysiological property.

[0006] The Chinese publication CN108084770A deals with a kind ofwaterproof putty powder and preparation method. The waterproof puttycomposition includes 40 - 55 parts by weight of white cement, 35 - 50parts by weight of talcum powder, 30 - 40 parts by weight of grey calcium,1 - 3 parts by weight of cellulose ether, 2 - 5 parts by weight of water-fastrubber powder, 10 - 15 parts by weight of bentonite, 1 - 3 parts by weightof cellulose, 1 - 2 parts by weight of hydroxyethyl cellulose and 0.1 - 0.4parts by weight of antifoaming agents such as silicone oil, dibutyl esterand tributyl phosphate. In this publication, the combination of water fastrubber powder and bentonite powder showed the effect of thewaterproofing property of wall putty.

[0007] Chinese publication CN107974124A discloses method ofpreparation of a kind of putty powder for exterior wall, resistant againstwater, corrosion, temperature, free from cracking and weatherability. Thecomposition of putty powder contains Paris white of 180 - 250 parts byweight, white cement of 60 - 100 parts by weight, hydroxyethyl celluloseof 2 - 8 parts by weight, nano aluminium oxide of 8 - 12 parts by weight,nano-titanium dioxide of 8 - 12 parts by weight, polymethyl methacrylateof 10 - 15 parts by weight, zirconic acid tungsten of 5 - 8 parts by weight,diatomite of 15 - 20 parts by weight and 5 - 8 parts by weight of EVAplastic materials. In this document, the materials such as Paris white fillerand ethylene vinyl acetate plastic materials contribute the waterresistance, corrosion and temperature resistance.

[0008] Various water repellents or hydrophobic materials can beincorporated into the composition of white cement based wall putty toimprove the water resistance. However, most of the materials are veryexpensive, and sporadically shows incompatibility with raw materials usedin white cement based wall putty composition. As a result, mixturebecomes non-homogenous and impedes the workability, adhesion andcoverage.

[0009] Therefore, there is a need for an improved white cement basedwater resistant wall putty composition which is economical, betteradhesion and improves the physico-mechanical properties and easyworkability.Objectives

[0010] The principal object of the present invention is to provide a whitecement based water resistant wall putty with improved physicomechanical properties.

[0011] Another object of the present invention is to provide an improvedwater resistant wall putty which has good adhesion properties, easyworkability, maximum whiteness, high plasticity, better coverage andcohesive mechanical strength.

[0012] Yet another object of the present invention is to provide animproved water resistant wall putty which is cost effective.Summary of the invention:

[0013] Accordingly, the present invention discloses a white cement basedwater resistant wall putty with improved physico-mechanical propertiesand method of preparation thereof. It has improved adhesion properties,workability and coverage and is cost effective.

[0014] In one aspect of the present invention, the white cement basedwater resistant wall putty composition comprises 15 - 30 parts by weightof white cement, 25 - 55 parts by weight of inorganic filler material, 0.2 -0.5 parts by weight of cellulose ether, 1 - 5 parts by weight of redispersiblepolymer powder, 15 - 50 parts by weight of coated mineral powder and 3- 5 parts by weight of mineral clay.

[0015] In another aspect, the inorganic filler material is selected from thegroup consisting of calcite, dolomite powder and marble powder, preferablymarble powder. The average particle size of said marble powder is in therange of 20 to 30 μm.

[0016] In another aspect, cellulose ether is selected from the groupconsisting of methyl hydroxyl ethyl cellulose, hydroxyl propyl methylcellulose and hydroxyl ethyl cellulose, preferably methyl hydroxyl ethylcellulose having preferable viscosity in the range of 70000 to 80000 cps.

[0017] In yet another aspect, the re-dispersible polymer powder is selectedfrom the group consisting of vinyl acetate methacrylate copolymer, vinylacetate ethylene copolymers, vinyl acetate vinyl ester of versatic acidcopolymers, styrene butadiene copolymer and acrylic polymers, preferablyvinyl acetate ethylene copolymers.

[0018] In yet another aspect, the coated mineral powder is selected fromthe group consisting of ground dolomite powder, ground calciumcarbonate powder, ground talcum powder and ground limestone powder,preferably ground calcium carbonate. The average particle size of groundcalcium carbonate is in the range of 1-5 μm. The calcium carbonate forsurface coating is selected from the group consisting of organo-silanes,siloxanes, salts of fatty acids, organo-titanates, metal stearates and zircon-aluminates. The calcium carbonate used for surface coating is preferablysalts of fatty acids and the amount of coating is in the range of 0.7 to 1.3% by weight of ground calcium carbonate.

[0019] Another aspect of the present invention discloses a process ofpreparation of the white cement based water resistant wall puttycomprising the steps of:- sequentially adding an inorganic filler material, white cement, a coatedmineral powder, a mineral clay, a redispersible polymer powder andcellulose ether into a plough shear mixer (150rpm) with chopper;- maintaining the capacity of dry powder to about 50-70% volume; and- mixing the powders up to 5 minutes at temperature of 27o ± 2oC andrelative humidity 50% ± 5% to obtain a homogenous powder.Detailed description of the invention:

[0020] Accordingly, the present invention provides a white cement basedwall putty application which has some of the critical properties such aseasy workability, maximum whiteness, high plasticity, good homogeneouspaste, lumps free, better coverage, good adhesion to plaster wall and strongcohesive mechanical strength.

[0021] Hydrophobic or water repellent materials can be incorporated tothe conventional white cement based putty composition to alleviate thewater related issues.

[0022] The present invention of water resistant white cement based wallputty composition contains 15 - 30 parts by weight of white cement, 25 -55 parts by weight of inorganic filler material, 0.2 - 0.5 parts by weight ofcellulose ether, 1 - 5 parts by weight of redispersible polymer powder, 15- 50 parts by weight of coated mineral powder and 3 - 5 parts by weight ofmineral clay.

[0023] The white cement is used as hydraulic binder in putty compositionwhich is available commercially. The preferred white cement of the presentinvention is a setting material as similar like ordinary Portland cement andused in the range of about 15 to 30 parts by weight.

[0024] Inorganic filler materials such as marble powder, calcite or dolomitepowder with average particle size of 10 - 40 μm, preferably 20 - 30 μm isused as whitening filler in the range of about 25 to 55 parts by weight. Itimproves the properties such as hardness, alkali resistance anddimensional stability of water resistant white cement based wall putty.

[0025] Cellulose ether is a non-ionic semi-synthetic cellulose polymer withtwo types, water soluble and solvent soluble available commercially. Theseare selected from the group consisting of methyl hydroxyl ethyl cellulose,hydroxyl propyl methyl cellulose and hydroxyl ethyl cellulose with viscosityrange of 60000 to 100000 cps, preferably 70000 to 80000 cps. They areused to improve the water retention, adhesion, levelling, consistency andsag resistance depending on the viscosity range of cellulose ether. About0.2 to 0.5 parts by weight of cellulose ether of medium viscosity range isused in the present invention which makes the paste workable.

[0026] Re-dispersible polymer powder is available as a free-flowing powderand obtained by spray drying of a special emulsion such as aqueousdispersions of vinyl acetate ethylene copolymers, vinyl acetate vinyl esterof versatic acid copolymers, vinyl acetate methacrylate copolymer, styrenebutadiene copolymer and acrylic polymers. It can be dispersed into anemulsion quickly after contact with water and has the same properties ofemulsion film of high flexibility, weather resistance and improved adhesionafter evaporation of water. The redispersible polymer powder is used inthe range of 1 to 5 parts by weight for improving the adhesion, flexibility,film formation, workability, water resistance, impact resistance, durabilityand mechanical properties of the putty.

[0027] The surface coated mineral powder used in the present inventionhas a very fine particle size of 1 - 10 μm preferably 1- 5 μm. It is a powderof minerals such as ground dolomite, ground calcium carbonate, andground talcum powder. It is a white powder having more than 95%whiteness (IS 8042: 2020), used as water repellent agent or hydrophobicin the range of 15 to 50 parts by weight. The surface coating of mineralpowder is a chemical modification of mineral surface to improve thecompatibility and adhesion by using various chemicals such as organosilanes, siloxanes, salts of fatty acids, organo-titanates, metal stearatesand zircon-aluminates. The most preferred chemicals used are salts ofhigh molecular weight saturated fatty acids with carbon content of at leastC >12 including lauric acid, stearic acid, myristic acid, palmitic acid usedalone or in combination to balance the desired adhesion and waterrepellent properties and are in the range of 0.5 to 1.5 % preferably 0.7 to1.3 % by weight of mineral powder.

[0028] The mineral clay of high water swelling and good bonding incementitious material such as ball clay, bentonite, sepiloite, zeolite,attapulgite and kaolin are used in the range of 3 to 5 parts by weight.

[0029] The disclosure will now be illustrated with working examples, whichis intended to illustrate the working of disclosure and not intended to takerestrictively to imply any limitations on the scope of the present disclosure.Unless defined otherwise, all technical and scientific terms used hereinhave the same meaning as commonly understood to one of ordinary skillin the art to which this disclosure belongs. It is to be understood that thisdisclosure is not limited to particular methods, and experimentalconditions described, as such methods and conditions may vary.Hereinafter, the present invention will be described in detail with specificexamples. However, this is not limited to the following examples.EXAMPLESTable 1: Composition of white cement based conventional and waterresistant putty

[0030] Table 1 shows the composition of white cement based conventionalwall putty devoid of water resistant properties and three different examplesof white cement based water resistant wall putty of the present invention.

[0031] The preparation of white cement based water resistant wall puttycomprised the following steps of sequentially adding inorganic fillermaterial, white cement, coated mineral powder, mineral clay, redispersiblepolymer powder and cellulose ether into a plough shear mixer (150 rpm)with chopper to maintain the capacity of dry powder about 50 - 70%volume and mixing time of up to 5 minutes at ambient condition(temperature 27o ± 2oC and relative humidity 50% ± 5%) to obtain ahomogenous powder. The white cement based water resistant wall puttypowder mixed with an appropriate quantity of water (up to 45%) anduniformly mixed to get the proper consistency for the application by usingputty knife / putty blade.

[0032] Bulk Density of the putty powder was calculated using calibrateddensity cup. The empty calibrated density cup was weighed. Then thedensity cup was completely filled with putty powder and without tapping,excess powder from the edge was removed using putty blade. The densitycup filled with putty powder was weighed and bulk density is calculatedusing the formulaEquationWherein, weight of filled putty powder = weight of density cup filled withputty - weight of empty density cup.

[0033] Residue 45 μm (%) was calculated using a 45 micron standardsieve. 100 gm of putty powder was weighed and put in 45 micron sieve. The 45micron sieve obtained was placed in sieve shaker. The sieve shaker wasstarted for 10 minutes, took out the sieve from the shaker and weighed theputty powder remains on the sieve. The residue is calculated using theformulaResidue (45 micron) = Weight of powder remains on sieveWeight of sample taken (100 gm) X 100 (%)

[0034] Water absorption was measured by using Karsten tube. Fourteendays cured putty surface was taken on a concrete substrate. The Karstentube was placed on putty surface with the help of silicon grease. TheKarsten tube was filled with water up to the mark and noted the time. Thewater absorption reading was noted in 30 minutes, 2 hrs, 24 hrs and 48hrs. Thereafter the water absorption was reported in mL respectively.

[0035] Degree of whiteness (%) was calculated by using reflectometer. Thereflectometer was calibrated using standard MgO block with knownwhiteness. After the calibration of MgO block, palate of putty powder wasplaced and checked the whiteness of the palate, reported the whiteness ofputty powder in %.

[0036] Compressive strength (N / mm2) was calculated using a calibratedCTM machine. The paste of the putty powder was prepared with desiredamount of water. Then poured the paste in 50mm mold and kept it for 28days at 27-30oC under controlled condition. After 28 days of curing in CTMmachine, broken down the putty cube and took the average of three cubesbreakage and reported in N / mm2.

[0037] Tensile adhesion (N / mm2) was calculated using a calibrated TensileAdhesion Testing Machine (TATM). Fourteen days cured putty surface wastaken on concrete surface and pasted 50mm dolly on the putty surfacewith the help of resin. On fourteenth day, the dolly was pulled out with thehelp of Tensile Adhesion Testing Machine and took the average pull outstrength of three dollies, and reported in N / mm2.

[0038] For calculating the water absorption coefficient, putty paste wasmade using the desired amount of water and poured into 40 x 40 x 160mmmould and kept 21 days for curing. After the 21 days of curing, put thespecimen in a vertical tray filled with water and took the weight in 10minutes (M1) and after 90 minutes (M2). Then calculated the waterabsorption coefficient using the formulaEquationTable 2: Properties of white cement based conventional and waterresistant putty

[0039] The physico-mechanical property comparison of conventional whitecement based wall putty devoid of water resistance, commercially availablewater resistant white cement based wall putty and three different examplesof white cement based water resistant wall putty of the present inventionare shown in Table 2.

[0040] It can be seen that there is a decrease in bulk density (IS 4669:2018) of the present invention of white cement based water resistant wallputty as compared to conventional wall putty devoid of water resistance.

[0041] Due to the usage of finer particle size of coated mineral powderalong with conventional inorganic filler material of the present inventionshowed less retention of residue at 45 μm (IS 4031: Part 1: 2021) ascompared to the conventional wall putty and commercial water resistantwall putty as known in the art. However, due to the finer particle size ofcoated mineral powder of the present invention exhibits less waterabsorption by Karsten tube method as shown in Table 2. This can beattributed to the high packing of the finer particle size of the coatedmineral powder and also better hydrophobicity of the coating materials onthe surface of the coated mineral powder.

[0042] From Table 2, as compared to the conventional white cement basedwall putty, the present invention of the white cement based water resistantwall putty shows the improved whiteness degree, compressive strength (IS4031: Part 6: 2019) and tensile adhesion strength (IS 17545: 2021).

[0043] Further, the commercial white cement based water resistant wallputty shows decrease in compressive strength and tensile adhesionstrength. This can be due to the incompatibility between the hydrophobicor water repellent agent and binder material used in the commercial waterresistant white cement based wall putty. However, due to the usage offiner particle size and better compatibility of the coated mineral powder ofthe present invention shows increase in both compressive strength andtensile adhesion strength.

[0044] It can be observed from Table 2 that wall putty of the presentinvention displays very low water absorption coefficient (EN 1015: Part 18:2002) than that of conventional white cement based wall putty. It alsoconfirms the water resistance of the present invention is much greater andthis result is corroborated with capillary water absorption of the presentinvention.

[0045] In contrast to the commercially available white cement based waterresistant wall putty, the present invention with fine particle size of coatedmineral powder shows better water resistance. Also, due to thecompatibility, coated mineral powder showed better adhesion andimproved the physico-mechanical properties and easy workability. It alsohas higher whiteness, good compressive strength, better tensile adhesionstrength, maximum coverage and low paint absorption. By the usage ofcoated mineral powder, the present invention is the cost-effective.

[0046] The putty composition of the present invention can be applied onany suitable surface of the substrate materials such as, concrete, plasterwall, brick wall, AAC block, gypsum board and cement board.

Claims

1. A white cement based water resistant wall putty composition comprising, a) 15-30 parts by weight of total mix of white cement; b) 25-55 parts by weight of total mix of an inorganic filler material; c) 0.2-0.5 parts by weight of total mix of a cellulose ether; d) 1-5 parts by weight of total mix of a re-dispersible polymer powder; e) 15-50 parts by weight of total mix of a coated mineral powder; and f) 3-5 parts by weight of total mix of a mineral clay.

2. The white cement based water resistant wall putty composition as claimed in claim 1 wherein said inorganic filler material is selected from the group consisting of calcite, dolomite powder and marble powder.

3. The white cement based water resistant wall putty composition as claimed in claim 2 wherein said inorganic filler material is marble powder.

4. The white cement based water resistant wall putty composition as claimed in claim 3 wherein said marble powder is having average particle size in the range of 20 to 30 μm.

5. The white cement based water resistant wall putty composition as claimed in claim 1 wherein said cellulose ether is selected from the group consisting of methyl hydroxyl ethyl cellulose, hydroxyl propyl methyl cellulose and hydroxyl ethyl cellulose.

6. The white cement based water resistant wall putty composition as claimed in claim 5 wherein said cellulose ether is methyl hydroxyl ethyl cellulose.

7. The white cement based water resistant wall putty composition as claimed in claim 6 wherein said methyl hydroxyl ethyl cellulose is having viscosity in the range of 70000 to 80000 cps.

8. The white cement based water resistant wall putty composition as claimed in claim 1 wherein said re-dispersible polymer powder is selected from the group consisting of vinyl acetate methacrylate copolymer, vinyl acetate ethylene copolymers, vinyl acetate vinyl ester of versatic acid copolymers, styrene butadiene copolymer and acrylic polymers.

9. The white cement based water resistant wall putty composition as claimed in claim 8 wherein said re-dispersible polymer powder is vinyl acetate ethylene copolymers.

10. The white cement based water resistant wall putty composition as claimed in claim 1 wherein said coated mineral powder is selected from the group consisting of ground dolomite powder, ground calcium carbonate powder, ground talcum powder and ground limestone powder.

11. The white cement based water resistant wall putty composition as claimed in claim 10 wherein said coated mineral powder is ground calcium carbonate.

12. The white cement based water resistant wall putty composition as claimed in claim 11 wherein said ground calcium carbonate is having average particle size in the range of 1-5 μm.

13. The white cement based water resistant wall putty composition as claimed in claim 11 wherein said calcium carbonate for surface coating is selected from the group consisting of organo-silanes, siloxanes, salts of fatty acids, organo-titanates, metal stearates and zircon-aluminates.

14. The white cement based water resistant wall putty composition as claimed in claim 13 wherein said calcium carbonate used for surface coating is salts of fatty acids.

15. The white cement based water resistant wall putty composition as claimed in claim 13 wherein said coating has an amount in the range of 0.7 to 1.3 % by weight of ground calcium carbonate.

16. A process of preparation of the white cement based water resistant wall putty comprising the steps of: - sequentially adding an inorganic filler material, white cement, a coated mineral powder, a mineral clay, a redispersible polymer powder and a cellulose ether into a plough shear mixer (150rpm) with chopper; - maintaining the capacity of dry powder to 50-70% volume; and - mixing the powders up to 5 minutes at ambient conditions to obtain a homogenous powder of white cement based water resistant wall putty composition.

17. The process as claimed in claim 16 wherein the ambient conditions for mixing powder is temperature in the range of 27o - 30oC and relative humidity in the range of 50% - 55%.