Carbon material for sintering, sintered ore, and production method for carbon material for sintering

IN607315BActive Publication Date: 2026-10-27JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202517025865
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-11-14
Filing Date
2025-03-21
Publication Date
2026-10-27
Estimated Expiration
2043-11-06

AI Technical Summary

Technical Problem

Biomass carbon, with its high combustion rate and tendency to produce tar, leads to incomplete combustion in sintering processes, reducing the yield of sintered ore and causing equipment trouble in sintering machines.

Method used

A carbon material for sintering composed of coal and biomass carbon, with a fixed carbon ratio of 0-30% and volatile content ≤5.0%, produced by carbonizing an agglomerate at ≥1000°C for ≥6 hours in a nitrogen atmosphere, to control combustion and tar production.

Benefits of technology

This approach reduces environmental impact, maintains sintered ore yield, and prevents equipment issues by optimizing biomass carbon usage and tar volatilization.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided are: a carbon material for sintering with which it is possible to reduce the environmental impact of the production of sintered ore while also suppressing equipment trouble and decreases in the yield of sintered ore; sintered ore; and a production method for the carbon material for sintering. The carbon material for sintering is used in an iron ore sintering process and contains coal and biochar as compounding materials. Therein, the ratio (mass%) of the fixed carbon of the biochar with respect to the coal and fixed carbon of the biomass carbon after carbonization is greater than 0 but not greater than 30 mass%, and the volatile content after carbonization is less than or equal to 5.0 mass%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a carbon material for sintering used in a sintering process of iron ore, a sintered ore, and a method for producing a carbon material for sintering.Background Art

[0002] A sintering process of iron ore is a process of firing a raw material for sintering, which is obtained by mixing iron ore as an iron source, an auxiliary raw material, such as flux and / or limestone, and a carbon material for sintering as a solid fuel, in a sintering machine using combustion heat of the carbon material for sintering. Although coke breeze is commonly used as the carbon material for sintering, anthracite or the like other than coke breeze may also be used in light of risks such as occurrences of price fluctuation of coking coal and trouble in coke production facility.

[0003] On the other hand, in response to growing awareness of environmental conservation in recent years, carbon materialsfor sintering have been increasingly diversified in light of reducing the environmental load, and use of carbon materials derived from biomass (hereinafter referred to as "biomass carbon") as carbon materials for sintering has begun to attract attention. Biomass carbon is made from a plant that has grown while absorbing carbon dioxide in the atmosphere. That is, in terms of carbon neutral, a fuel using biomass carbon is evaluated as having no emission of carbon dioxide gas due to combustion. For this reason, use of biomass carbon as an alternative to coke breeze, which has been used as a carbon material for sintering in the related art, has also begun to be studied.

[0004] Here, Patent Literature 1 discloses a method in which in a carbonizing chamber of a coke oven, subbituminous coal or lignite pulverized so that the content of the material of not more than 10 mm is 80 mass% is fed into an upper portion or a bottom portion of fed coal for producing coke and is carbonized. In addition, this literature also discloses that waste plastic and / or woody biomass can be mixed as part of subbituminous coal and / or lignite.Citation List Patent Literature

[0005] Patent Literature 1: JP 5532574 BSummary of Invention Technical Problem

[0006] Biomass carbon is characterized by a low combustion initiation temperature. Biomass carbon is porous and thus has a large surface area compared with coke breeze derived from fossil fuels, which is commonly used in sintering processes. Thus, even in a state of a low combustion initiation temperature, biomass carbon has a large contact area with the atmosphere and provides a high combustion rate.

[0007] The combustion reaction of the carbon material for sintering is a gas-solid reaction. In addition, the carbon material for sintering reacts with oxygen in the surrounding gas and burns. Furthermore, in a gas-solid reaction under conditions in which a gas flows as in a sintering process, a region called a gas laminar film, which is a thin layer, is generated on the surface of the carbon material for sintering. The gas laminar film is not affected by a turbulent flow of the outside gas, and a laminar flow is maintained. Oxygen enters from the outside of the gas laminar film into the gas laminar film, diffuses and reaches the surface of the carbon material for sintering, and thus burns the carbon material for sintering.

[0008] Here, when the combustion rate of the carbon material for sintering is high, even when the surrounding oxygen concentration is high, the oxygen consumption rate on the surface due to the combustion of the carbon material for sintering becomes higher than the oxygen supply rate due to the diffusion of oxygen in the gas laminar film, and the oxygen concentration in the gas laminar film decreases.This results in incomplete combustion of the carbon material for sintering and increase in the amount of generated carbon monoxide.

[0009] That is, when the combustion rate of the carbon material for sintering is high, part of the carbon material for sintering is discharged as carbon monoxide, which thus reduces the reaction heat to be supplied to the sintering process. That is, the combustion heat for firing the sintering raw material (an iron source and an auxiliary raw material) is insufficient and leads to a decrease in the yield in the production of sintered ore. Thus, in using biomass carbon with a high combustion rate as the carbon material for sintering, there is a problem in that the yield of sintered ore decreases due to the shortage of the combustion heat for firing the sintering raw material.

[0010] Furthermore, biomass carbon produces (volatilizes) a large amount of tar, which is a by-product, by a thermal reaction. The produced (volatilized) tar adheres to the inside of a pipe, a filter provided for dust removal, an impeller of a blower, and / or the like in a sintering machine. Thus, there is also a problem of causing equipment trouble.

[0011] The present invention has been made in view of such circumstances, and an object of the present invention is to provide a carbon material for sintering which is capable of reducing the environmental load as well as preventing a decrease in the yield of sintered ore and equipment trouble in production of sintered ore; a sintered ore; and a method for producing a carbon material for sintering.Solution to Problem

[0012] The gist configuration of the present invention for solving the above problems are as follows.[1] A carbon material for sintering used in a sintering process of iron ore, the carbon material containing coal and biomass carbon as blending materials, in which a proportion (mass%) of fixed carbon in the biomass carbon to fixed carbon in the coal and the biomass carbon after carbonization is more than 0 and not more than 30 mass%, anda volatile component content after carbonization is not more than 5.0 mass%.[2] A sintered ore produced using the carbon material for sintering described in [1].[3] A method for producing a carbon material for sintering used in a sintering process of iron ore, the method including: forming an agglomerate containing coal and biomass carbon as blending materials; and carbonizing the agglomerate by holding it at a temperature of not lower than 1000°C for not less than 6 hours in a nitrogen atmosphere.[4] The method for producing a carbon material for sintering according to [3], in which the carbonization is carried out in a coke oven.Advantageous Effects of Invention

[0013] According to the present invention, in the production of sintered ore, the environmental load can be reduced, and a decrease in the yield of sintered ore and equipment trouble can be prevented.Description of Embodiments

[0014] Hereinafter, the present invention will be described through embodiments of the present invention.

[0015] A carbon material for sintering used in a sintering process of iron ore contains coal and biomass carbon as blending materials. In contrast to blending only coal composed of coke breeze, anthracite, and the like in the related art, partial substitution (blending) of biomass carbon reduces the relative use of coal and can reduce the environmental load.

[0016] In addition, in the carbon material for sintering, a proportion (mass%) of fixed carbon in the biomass carbon to fixed carbon in the coal and the biomass carbon after carbonization is more than 0 and not more than 30 mass%. Here, "fixed carbon" means a carbon component contained in an agglomerate after carbonization of an agglomerate containing coal and biomass carbon as blending materials. Increasing the blending proportion of the biomass carbon reduces the relative blending proportion of the coal and can reduce the environmental load. However, this increases the biomass carbon with a high combustion rate and thus reduces the yield of sintered ore. Thus, adjusting the proportion (mass%) of fixed carbon in the biomass carbon to more than 0 and not more than 30 mass% can prevent a decrease in the yield of sintered ore. In addition, based on the prevention of the decrease in the yield of sintered ore, the proportion of fixed carbon in the biomass carbon can be maximized, theproportion of fixed carbon in the coal can be minimized, and the reduction in the emission amount of carbon dioxide can be maximized.

[0017] Here, in the biomass carbon, a large number of pores derived from the vascular bundle of a raw material plant remain, and moisture and / or the like in the air is adsorbed in the pores. In addition, due to the thermal reaction in the sintering process, a large amount of tar, which is a byproduct, also volatilizes along with the volatilization of moisture and / or the like remaining in the pores. Thus, after blending coal and biomass carbon to form an agglomerate as a carbon material for sintering, volatile components, such as moisture, contained in the biomass carbon need to be completely removed by carbonizing the agglomerate in advance. However, the pores inherent in the biomass carbon are complexly formed in large numbers, and thus it is difficult to completely remove volatile components by carbonization.

[0018] Thus, for the carbon material for sintering, an agglomerate with coal and biomass carbon blended is carbonized until the volatile component content (mass%) in the carbon material for sintering after carbonization becomes not more than 5.0 mass%. This can reduce, when thecarbon material for sintering is used in the sintering process, the volatilization of moisture and / or the like due to a thermal reaction and also reduce the volatilization of tar. As a result, equipment trouble caused by adhesion of tar and / or the like can be prevented.

[0019] In a method for producing a carbon material for sintering used in a sintering process of iron ore, first, an agglomerate containing coal and biomass carbon as blending materials is formed. Then, the agglomerate is carbonized by holding it at a temperature of not lower than 1000°C for not less than 6 hours in a nitrogen atmosphere. The carbonization may be carried out in a coke oven. Carbonization of the carbon material for sintering in a coke oven eliminates the need for providing special equipment for carrying out carbonization of the carbon material for sintering and provides an effect of reducing the equipment cost.

[0020] The iron ore sintering process is carried out using a sintering machine. In the sintering process, first, a raw material for sintering obtained by adding an auxiliary raw material, such as flux, and the carbon material for sintering to iron ore as an iron source is continuously fed onto a sintering machine to form a sintering bed. Then, thecarbon material for sintering at the upper end of the sintering bed is ignited, and then the exhaust gas is sucked from the lower end. This propagates the combustion of the carbon material for sintering from the upper end to the lower end of the sintering bed, the combustion heat causes a combustion reaction between the iron source and the auxiliary raw material, and the raw material for sintering is firing. The exhaust gas is sucked from the lower end of the sintering bed using a blower. The sucked exhaust gas flows through a duct via a blower, passes through a dust collector, desulfurization equipment, denitration equipment, and the like, and is discharged from a chimney.Examples

[0021] Hereinafter, examples performed using the carbon material for sintering and the method for producing a carbon material for sintering according to the present embodiment will be described.

[0022] Example 1: As biomass carbon, a biomass material of wood chips (hereinafter referred to as the "biomass A") and a biomass material of palm kernel shell (hereinafter referred to as the "biomass B") were prepared and were each blended with coal at a predetermined ratio, carbonization was carried out in a carbonization furnace (coke oven), anda carbon material for sintering was produced. The carbonization was carried out under conditions of holding at a temperature of not lower than 1000°C for not less than 6 hours in a nitrogen atmosphere. The proportion (mass%) of fixed carbon in the biomass carbon to fixed carbon in the coal and the biomass carbon after the carbonization and the volatile component content (mass%) in the carbon material for sintering after the carbonization were measured based on the JIS standard "Coal and coke-Methods for proximate analysis" (JIS M8812).

[0023] Next, as a sintering process, iron ore (iron source) and limestone (auxiliary raw material) were mixed with the produced carbon material for sintering and return fines, a certain amount of water was added, and the mixture was granulated. Then, the raw material for sintering obtained by granulation was fed into a sinter pot test apparatus and subjected to a sintering test. The sinter pot test apparatus has a sinter pot with a diameter of 300 mm and a height of 600 mm; an ignition oven; and exhaust gas equipment, such as a wind box and a blower. In the sinter pot test apparatus, a test simulating an actual sintering machine can be performed, in which a combustion reaction is allowed to proceed from an upper layer of a raw material layer of a raw material for sintering and the combustionreaction reaches a lower layer of the raw material layer to complete sintering. In addition, in the sintering test, the fed raw material for sintering was sintered to form sintered ore, and then a drop test was performed, in which the sintered ore was dropped four times from the height of 2 m. For the sintered ore after dropping, a sintered ore keeping a size of not less than 5 mm was regarded as a product, and a proportion of the product was evaluated as a product yield (%). Furthermore, for the evaluation of the product yield (%), a three-class evaluation (yield evaluation) was performed, in which a case with a product yield of not less than 70% was rated as "good (o)", not less than 65% and less than 70% as "average (A)", and less than 65% as "poor (x)". Many cases of not blending biomass carbon in the carbon material for sintering show a product yield (%) of around 80%.

[0024] In addition, the sinter pot test apparatus is provided with a blower similarly to an actual sintering machine.Thus, after completion of the sintering test, the adhesion state of tar in the blower was observed, and to evaluate exhaust gas equipment, a two-class evaluation was also performed, in which a state of requiring cleaning or causing equipment trouble was rated as "bad (x)" and other states were rated as "no problem (o)".

[0025] [Table 1]

[0026] [Table 2]

[0027] Comparative Examples 1 and 6 in Tables 1 and 2 show examples in which the sintering process was carried out using a carbon material for sintering without the biomass carbon. Comparative Examples 5 and 10 show examples in which the sintering process was carried out using only the biomass carbon as the carbon material for sintering. Thus, for Comparative Examples 5 and 10, the emission amount of carbon dioxide is indicated as "0". The blending proportion (mass%) of the biomass A or the biomass B in Tables 1 and 2 means a proportion (mass%) of the mass of the biomass carbon to the mass of the agglomerate in a state before the carbon material for sintering was carbonized, that is, a state in which the agglomerate containing coal and the biomass carbon as blending materials is formed.

[0028] As shown in Table 1, Inventive Examples 1 to 3, in which the biomass A (wood chips) was used as biomass carbon and the proportion of fixed carbon in the biomass A after the carbonization was more than 0 and not more than 30 mass%, were able to confirm that the yield was evaluated as "good (o)". This case (Inventive Examples 1 to 3) was able to confirm that the emission amount of carbon dioxide (kg-CCy / t-Sinter) was able to be reduced by up to about 20%. In addition, Inventive Examples 1 to 3 were able to confirmthat the volatile component content (mass%) after the carbonization was not more than 5.0 mass%. Thus, Inventive Examples 1 to 3 were all able to confirm that the exhaust gas equipment evaluation was "good (o)".

[0029] On the other hand, Comparative Examples 2 to 5, in which the proportion of fixed carbon in the biomass A after the carbonization was not less than 40 mass%, were able to confirm that the yield was evaluated as "poor (*)". In Comparative Examples 2 to 4, despite the state in which the yield was evaluated as "poor (*)", the production amount of sintered ore was maintained, and thus the emission amount of carbon dioxide increased. In addition, Comparative Examples 2 to 5 revealed a value of more than 5.0 mass% for the volatile component content (mass%) after the carbonization and were able to confirm that the exhaust gas equipment evaluation was "poor (*)".

[0030] In addition, as shown in Table 2, Inventive Examples 4 to 6, in which the biomass B (palm kernel shell) was used as biomass carbon and the proportion of fixed carbon in the biomass B after the carbonization was more than 0 and not more than 30 mass%, were able to confirm that the yield was evaluated as "good (o)" or "average (A)". This case (Inventive Examples 4 to 6) was able to confirm that theemission amount of carbon dioxide (kg-CO2 / t-Sinter) was able to be reduced by up to about 15%. In addition, Inventive Examples 4 to 6 were able to confirm that the volatile component content (mass%) after the carbonization was not more than 5.0 mass%. Thus, Inventive Examples 4 to 6 were all rated as "good (o)" for the exhaust gas equipment evaluation.

[0031] On the other hand, Comparative Examples 7 to 10, in which the proportion of fixed carbon in the biomass B after the carbonization was not less than 40 mass%, were able to confirm that the yield was evaluated as "poor (*)" although the emission amount of carbon dioxide decreased. In addition, Comparative Examples 7 to 10 revealed a value of more than 5.0 mass% for the volatile component content (mass%) after the carbonization and were all able to confirm that the exhaust gas equipment evaluation was "poor (*)".

[0032] The above results were able to confirm that a carbonmaterial for sintering used in a sintering process andcontaining coal and biomass carbon as blending materials with a proportion (mass%) of fixed carbon in the biomass carbon to fixed carbon in the coal and the biomass carbonafter carbonization of more than 0 and not more than 30mass% and a volatile component content (mass%) aftercarbonization of not more than 5.0 mass%, can reduce the environmental load and prevent a decrease in the yield of sintered ore and equipment trouble.

[0033] Example 2: A biomass material (biomass A) of wood chips was prepared as biomass carbon, and an agglomerate was formed with a blending proportion (mass%) of the biomass carbon (biomass A) of 54% and a blending proportion (mass%) of coal of 46%. Then, carbonization was carried out in a carbonization furnace (coke oven) in a nitrogen atmosphere under each condition with the temperature and carbonization time changed. During the carbonization, the rates of temperature increase and decrease were 10°C / min.

[0034] The proportion (mass%) of fixed carbon in the biomass carbon to fixed carbon in the coal and the biomass carbon after the carbonization and the volatile component content (mass%) in the carbon material for sintering after the carbonization were measured based on the JIS standard "Coal and coke-Methods for proximate analysis" (JIS M8812) as in the previous examples. In the carbon material for sintering after the carbonization, the proportion (mass%) of fixed carbon in the biomass carbon to fixed carbon in the coal and the biomass carbon was 30 mass%. For the evaluation of the volatile component content (mass%), a case with a volatilecomponent content of not more than 5.0 mass% was evaluatedas "good (o)" and more than 5.0 mass% as "poor (x)".

[0035] [Table 3]

[0036] As shown in Table 3, which is the implementation results with use of the biomass A, using the biomass A as the biomass carbon (Inventive Examples 7 and 8) was able to reduce the volatile component content (mass%) after thecarbonization to not more than 5.0 mass% by carrying out the carbonization under conditions of holding at a temperature of not lower than 1000°C for not less than 6 hours in both examples.

[0037] The results confirmed that setting the conditions of the carbonization to a temperature of lower than 1000°C or a holding time of the carbonization of less than 6 hours (Comparative Examples 11 to 14) failed to reduce the volatile component content (mass%) after the carbonization to not more than 5.0 mass%.

Claims

1. A carbon material for sintering used in a sintering process of iron ore, the carbon material comprising coal and biomass carbon as blending materials, wherein a proportion (mass%) of fixed carbon in the biomass carbon to fixed carbon in the coal and the biomass carbon after carbonization is more than 0 and not more than 30 mass%, and a volatile component content after carbonization is not more than 5.0 mass%.

2. A sintered ore produced using the carbon material for sintering according to Claim 1.

3. A method for producing a carbon material for sintering used in a sintering process of iron ore, the method comprising: forming an agglomerate containing coal and biomass carbon as blending materials; and carbonizing the agglomerate by holding the agglomerate at a temperature of not lower than 1000°C for not less than 6 hours in a nitrogen atmosphere.

4. The method for producing a carbon material for sintering according to Claim 3, wherein the carbonization is carried out in a coke oven.