Hemostatic polymer material kit
Patent Information
- Application Number
- IN202217062485
- Authority / Receiving Office
- IN · IN
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-08
- Filing Date
- 2022-11-02
- Publication Date
- 2026-10-28
- Estimated Expiration
- 2041-05-06
AI Technical Summary
Conventional hemostatic methods face challenges such as infection risks from biologically derived materials, difficulty in applying to complex structures, and ineffective blood coagulation in patients on anticoagulants, due to reliance on blood coagulability.
A polymer material kit comprising two hydrophilic polymer solutions that form a hydrogel in situ at a bleeding site or blood vessel, using polymers with specific molecular weights, functional groups, and pH/ionic strength conditions to create a gel-blood complex for efficient coagulation and hemostasis.
The polymer material kit provides a safe, efficient, and effective hemostatic effect by forming a gel-blood complex that promotes blood coagulation and physical hemostasis, applicable to complex structures and patients on anticoagulants, without relying on blood coagulability.
Abstract
Description
Technical Field
[0001] The present invention relates to a polymer materialkit for hemostasis, vascular occlusion, tissue covering, orbody fluid coagulation, and further relates to a hemostaticmethod, a vascular occlusion method, a tissue coveringmethod, and a body fluid coagulation method in which thepolymer material kit is used.Background Art
[0002] Conventional methods used for blood coagulationmainly include a method of accelerating a hemostaticreaction by using a pharmacological action of abiologically derived blood coagulation factor representedby a fibrin glue (for example, Patent Literature 1) and amethod of physically blocking a blood flow and coagulatingthe blood by the coagulability of the blood itself.
[0003] However, the former method in which a biologicallyderived material is used has an infection risk becauseinfection control is not easy in an animal as a rawmaterial or in a donor. In fact, problems have occurredsuch as HIV infection through unheated blood products andiatrogenic Creutzfeldt-Jakob disease. Meanwhile, thelatter method in which physical blocking is used isdifficult to apply to an affected part having a complicatedstructure because a sheet-like material is to be used dueto the characteristics of the hemostasis principle.Furthermore, both the methods have a common problem that ablood coagulation effect is difficult to obtain for apatient to whom an agent such as an anticoagulant isadministered because the final hemostatic state depends onthe blood coagulability of the patient.Citation ListPatent Literature
[0004] Patent Literature 1: JP 2017-66150 ASummary of InventionTechnical Problem
[0005] Therefore, an object of the present invention is toprovide a hemostatic method, a vascular occlusion method, atissue covering method, and a body fluid coagulation methodthat are safe and efficient using a polymer material thatis a non-biologically derived synthetic product.Solution to Problem
[0006] As a result of intensive studies to solve the abovedescribedproblems, the present inventors have found thatan excellent blood coagulation effect and an excellenthemostatic effect can be obtained by preparing a solution(pre-gel solution) that contains, under a specificconcentration condition, a hydrophilic polymer capable offorming a hydrogel by intermolecular crosslinking and has aspecific pH condition and specific ionic strength, followedby forming the solution into a gel in situ in anenvironment, such as a bleeding site or the interior of ablood vessel, where blood is present, and thus the presentinvention has been completed.
[0007] That is, in one aspect, the present inventionrelates to a kit for formation of a hydrogel in anenvironment where blood is present, and specificallyprovides:<1> A polymer material kit including a polymersolution A containing a first polymer and a second polymersolution B containing a second polymer, the first polymerand the second polymer being a hydrophilic polymer having apolyalkylene glycol skeleton or a polyvinyl skeleton,wherein a combination of the first polymer and the secondpolymer is capable of forming a hydrogel when the firstpolymer and the second polymer are crosslinked with eachother, the first polymer and the second polymer have aweight average molecular weight (Mw) in a range of 1 x 103to 1 x 105, the polymer solution A and the second polymersolution B have a concentration of the first polymer and aconcentration of the second polymer in a range of 10 to 300g / L, respectively, and a mixed solution obtained by mixingthe polymer solution A and the second polymer solution Bhas a pH of 3 to less than 7 and an ionic strength in arange of 10 to 100 mM;<2> The polymer material kit according to the item<1>, wherein the first polymer and the second polymer are atwo-, three-, or four-armed polyethylene glycol;<3> The polymer material kit according to the item<1> or <2>, wherein the first polymer has one or morenucleophilic functional groups in a side chain or at aterminal, and the second polymer has one or moreelectrophilic functional groups in a side chain or at aterminal;<4> The polymer material kit according to any one ofthe items <1> to <3>, wherein the one or more nucleophilicfunctional groups are selected from the group consisting ofa thiol group and an amino group, and the one or moreelectrophilic functional groups are selected from the groupconsisting of a maleimidyl group, an N-hydroxy-succinimidyl(NHS) group, a sulfosuccinimidyl group, a phthalimidylgroup, an imidazoyl group, an acryloyl group, a nitrophenylgroup, and -CO2PhNO2;<5> The polymer material kit according to any one ofthe items <1> to <4>, wherein the polymer solution A andthe second polymer solution B have a pH in a range of 3 toless than 7;<6> The polymer material kit according to any one ofthe items <1> to <5>, wherein a hydrogel in which the firstpolymer and the second polymer are crosslinked with eachother is formed when the polymer solution A and the secondpolymer solution B are mixed in an environment where aliquid having a pH of 6.5 to 8.0 is present;<7> The polymer material kit according to the item<6>, wherein the hydrogel formed using the first polymerand the second polymer has a gelation time in a range of 1to 30 seconds;<8> The polymer material kit according to the item<6> or <7>, wherein the hydrogel formed using the firstpolymer and the second polymer has an equilibrium swellingdegree in a range of 0.9 to 3.5;<9> The polymer material kit according to any one ofthe items <6> to <8>, wherein the hydrogel formed using thefirst polymer and the second polymer has a Young's modulusin a range of 0.1 x 104 to 4 x 104 Pa;<10> The polymer material kit according to any oneof the items <1> to <9>, to be used for hemostasis,vascular occlusion, tissue covering, or body fluidcoagulation;<11> A hemostatic agent including the polymermaterial kit according to any one of the items <1> to <10>;<12> A vascular occlusion agent including thepolymer material kit according to any one of the items <1>to <10>;<13> A tissue covering agent including the polymermaterial kit according to any one of the items <1> to <10>;and<14> A body fluid coagulant including the polymermaterial kit according to any one of the items <1> to <10>.
[0008] In another aspect, the present invention relates toa method for producing a hemostatic agent or the likecontaining a hydrogel using the kit, and specificallyprovides:<15> A method for producing a hemostatic agent, avascular occlusion agent, a tissue covering agent, or abody fluid coagulant containing a hydrogel, the methodincluding a step of applying a mixed solution of a polymersolution A containing a first polymer and a second polymersolution B containing a second polymer to an environmentwhere a liquid having a pH of 6.5 to 8.0 is present,wherein the first polymer and the second polymer are ahydrophilic polymer having a polyalkylene glycol skeletonor a polyvinyl skeleton, a combination of the first polymerand the second polymer is capable of forming a hydrogelwhen the first polymer and the second polymer arecrosslinked with each other, the first polymer and thesecond polymer have a weight average molecular weight (Mw)in a range of 1 x 103 to 1 x 105, the polymer solution Aand the second polymer solution B have a concentration ofthe first polymer and a concentration of the second polymerin a range of 10 to 300 g / L, respectively, and the mixedsolution obtained by mixing the polymer solution A and thesecond polymer solution B has a pH of 3 to less than 7 andan ionic strength in a range of 10 to 100 mM;<16> The method according to the item <15>,including mixing the polymer solution A and the secondpolymer solution B in an environment where a liquid havinga pH of 6.5 to 8.0 is present;<17> The method according to the item <15>,including dripping the polymer solution A and the secondpolymer solution B on a carrier and then bringing thecarrier into contact with an environment where a liquidhaving a pH of 6.5 to 8.0 is present; and<18> The method according to any one of the items<15> to <17>, wherein the polymer solution A and the secondpolymer solution B have a pH in a range of 3 to less than7.
[0009] In another aspect, the present invention alsorelates to a hemostatic method and the like in which thekit is used, and specifically provides:<19> A hemostatic method including using the polymermaterial kit according to any one of the items <1> to <10>;<20> A vascular occlusion method including using thepolymer material kit according to any one of the items <1>to <10>;<21> A tissue covering method including using thepolymer material kit according to any one of the items <1>to <10>;<22> A body fluid coagulation method including usingthe polymer material kit according to any one of the items<1> to <10>;<23> A medical device including the polymer materialkit according to any one of the items <1> to <10>; and<24> The medical device according to the item <23>,wherein at least one of the polymer solution A or thesecond polymer solution B is stored in a sprayer.Advantageous Effects of Invention
[0010] According to the polymer material kit of the presentinvention, by applying two polymer solutions to anenvironment where blood is present such as a bleeding siteor the interior of a blood vessel, a change in pH is causedin the polymer solutions to promote a gelation reaction insitu, and thus a gel-blood complex incorporating blood canbe formed in a short time. As a result, it is possible toprovide an excellent blood coagulation effect by takingblood into the gel, and a physical hemostatic effect bycovering the bleeding site or the like with the gel.
[0011] Unlike in the prior art, the polymer material usedin the present invention is not an animal-derived materialand therefore can avoid a risk of infection or the like.Furthermore, there is an advantage that the presentinvention can be applied to a tissue having a complicatedstructure because after mixing two polymer solutions, theresulting mixture can maintain the liquid state for acertain period of time. In addition, there is also anadvantage that the present invention can be applied to apatient to whom an anticoagulant or the like isadministered because unlike a conventional method, thepresent invention can provide excellent blood coagulabilitynot depending on the coagulability of the blood itself.
[0012] The present invention can be also applied tovascular occlusion by applying the in-situ gel formation ofthe present invention to a blood vessel such as a vein oran artery. Furthermore, the gel formation mechanism canexhibit a coagulation effect not only on blood but also ona body fluid having a pH near neutral because the gelformation mechanism utilizes a pH change due to applicationto a biological environment.Brief Description of Drawings
[0013] Fig. 1 is a graph showing an influence ofconcentration and pH on gelation time.Fig. 2 is a graph showing a change in gelation timedepending on ionic strength.Fig. 3 is a graph showing a change in pH dependingon ionic strength.Fig. 4 is a graph showing a relation betweengelation time and pH.Fig. 5 is a graph showing a change in the Young'smodulus caused by mixing with cow milk.Fig. 6 is a graph showing a time-course change inswelling degree in cow milk.Fig. 7 is a graph showing the equilibrium swellingdegree at each prepolymer concentration in water.Fig. 8 is an image in which a gel is applied to avenous blood vessel of a rat thigh.Fig. 9 is an image in which a gel is applied to anarterial blood vessel of a rat abdomen.Description of Embodiments
[0014] Hereinafter, embodiments of the present inventionwill be described. The scope of the present invention isnot limited by these descriptions and can be appropriatelychanged, and embodiments other than the following examplescan be implemented without impairing the gist of thepresent invention.
[0015] 1. Polymer Material Kit of the Present InventionThe polymer material kit of the present inventionincludes a polymer solution A containing a first polymerand a second polymer solution B containing a secondpolymer, and each polymer solution contains, under aspecific concentration condition, a hydrophilic polymercapable of forming a hydrogel by intermolecularcrosslinking and has a specific pH condition and specificionic strength.
[0016] Under such solution conditions, the gelationreaction does not proceed in a short time even if thesepolymer solutions A and B are mixed as they are, but if thetwo solutions are mixed in a solution having a pH nearneutral such as blood, gelation is promoted and caused insitu in a relatively short time and thus a hydrogelincorporating the blood into the gel (also referred to as a"gel-blood complex" or a "gel-body fluid complex") can beformed. It can be said that the polymer material kit ofthe present invention is a novel technique that has beenunavailable heretofore because by forming such a gel-bloodcomplex in situ, it is possible to provide both the bloodcoagulation effect by taking the blood itself into the geland the physical hemostatic effect by covering the bleedingsite or the like with the gel.
[0017] Hereinafter, polymer materials and solutionconditions used in the polymer material kit of the presentinvention will be described in detail.
[0018] (1-1) Polymer MaterialsThe first polymer and the second polymer used in thepolymer solutions A and B of the present invention arehydrophilic polymers having a polyalkylene glycol skeletonor a polyvinyl skeleton that are capable of forming ahydrogel when crosslinked with each other. As thehydrophilic polymers, those known in the art can be used aslong as a hydrogel can be formed by a gelation reaction(crosslinking reaction or the like) in an aqueous solution,and more specifically, polymers are preferable that arecapable of forming a network structure, particularly athree-dimensional network structure when the polymers arecrosslinked with each other in the final gel.
[0019] Typical examples of the polymer having apolyethylene glycol skeleton include polymer species havinga plurality of branches having a polyethylene glycolskeleton, and a two-, three-, or four-armed polyethyleneglycol is particularly preferable. In particular, a gelincluding a four-armed polyethylene glycol skeleton isgenerally known as a Tetra-PEG gel, and a network structureis constructed by an AB cross-end coupling reaction betweentwo four-armed polymers having an electrophilic functionalgroup such as an active ester structure and a nucleophilicfunctional group such as an amino group at the terminalrespectively (Matsunaga et al., Macromolecules, Vol. 42,No. 4, pp. 1344-1351, 2009). The Tetra-PEG gel can beeasily prepared in situ by simple two-liquid mixing of thepolymer solutions, and the gelation time can also becontrolled by adjusting the pH and the ionic strength atthe time of gel preparation. This gel contains PEG as amain component, and therefore is also excellent inbiocompatibility.
[0020] Examples of the hydrophilic polymer having apolyvinyl skeleton include polyalkyl methacrylates such aspolymethyl methacrylate, polyacrylates, polyvinyl alcohols,poly N-alkyl acrylamides, and polyacrylamide.
[0021] The first polymer and the second polymer have aweight average molecular weight (Mw) in the range of 1 x103 to 1 x 105, preferably in the range of 0.5 x 104 to 5 x104, and more preferably in the range of 1 x 104 to 2 x 104.
[0022] The first polymer and the second polymer arepreferably a combination of a polymer having one or morenucleophilic functional groups in the side chain or at theterminal and a polymer having one or more electrophilicfunctional groups in the side chain or at the terminal.For example, the first polymer preferably has one or morenucleophilic functional groups in the side chain or at theterminal, and the second polymer preferably has one or moreelectrophilic functional groups in the side chain or at theterminal. The nucleophilic functional group and theelectrophilic functional group are crosslinked to form agel. Here, the total number of the nucleophilic functionalgroups and the electrophilic functional groups ispreferably 5 or more. These functional groups are morepreferably present at the terminal.
[0023] Examples of the nucleophilic functional grouppresent in the first and the second polymers include athiol group (-SH) and an amino group, and those skilled inthe art can appropriately use a known nucleophilicfunctional group. The nucleophilic functional group ispreferably a -SH group. The nucleophilic functional groupsmay be the same or different, but are preferably the same.If the functional groups are the same, the reactivity withan electrophilic functional group to be crosslinked becomesuniform and a gel having a uniform three-dimensionalstructure is easily obtained.
[0024] As the electrophilic functional group present in thefirst and the second polymers, an active ester group can beused. Examples of such an active ester group include amaleimidyl group, an N-hydroxy-succinimidyl (NHS) group, asulfosuccinimidyl group, a phthalimidyl group, an imidazoylgroup, an acryloyl group, a nitrophenyl group, and -CO2PhNO2 (Ph represents an o-, m-, or p-phenylene group),and those skilled in the art can appropriately use anotherknown active ester group. The electrophilic functionalgroup is preferably a maleimidyl group. The electrophilicfunctional groups may be the same or different, but arepreferably the same. If the functional groups are thesame, the reactivity with a nucleophilic functional groupto be crosslinked becomes uniform and a gel having auniform three-dimensional structure is easily obtained.
[0025] Preferred non-limiting specific examples of thepolymer having a nucleophilic functional group at theterminal include a compound that has four branches having apolyethylene glycol skeleton and has a thiol group at theterminal and is represented by the following formula (I).[Chem. 1]
[0026] In the formula (I), R11 to R14 are the same ordifferent and each represent a C1 to C7 alkylene group, a C2to C7 alkenylene group, -NH-R15-, -CO-R15-, -R16-O-R17-, -R16-NH-R17-, -R16-CO2-R17-, -R16-CO2-NH-R17-, -R16-CO-R17-, or -R16-CO-NH-R17-, wherein R15 represents a C1 to C7 alkylene group,R16 represents a C1 to C3 alkylene group, and R17 representsa C1 to C5 alkylene group.
[0027] n11 to n14 may be the same or different. The closerthe values of n11 to n14 are, the more uniform the threedimensionalstructure can be, and the higher the strengthbecomes. Therefore, in order to obtain a gel having highstrength, n11 to n14 are preferably the same. If the valuesof n11 to n14 are too high, the gel has low strength, and ifthe values of n11 to n14 are too low, the gel is less likelyto be formed due to the steric hindrance of the compound.Therefore, the values of n11 to n14 are, for example, aninteger value of 5 to 600, preferably 25 to 250, morepreferably 50 to 120, and still more preferably 110 to 120.
[0028] In the formula (I), R11 to R14 are linker moietieseach connecting a functional group and a core moiety. R11to R14 may be the same or different, but are preferably thesame in order to produce a gel having a uniform threedimensionalstructure and high strength. R11 to R14 eachrepresent a C1 to C7 alkylene group, a C2 to C7 alkenylenegroup, -NH-R15-, -CO-R15-, -R16-O-R17-, -R16-NH-R17-, -R16-CO2-R17-, -R16-CO2-NH-R17-, -R16-CO-R17-, or -R16-CO-NH-R17-. Here,R15 represents a C1 to C7 alkylene group. R16 represents aC1 to C3 alkylene group. R17 represents a C1 to C5 alkylenegroup.
[0029] Here, the term "C1 to C7 alkylene group" means analkylene group that has 1 or more and 7 or less carbonatoms and may have a branch, and means a linear C1 to C7alkylene group or a C2 to C7 alkylene group having one ormore branches (having 2 or more and 7 or less carbon atomsincluding carbon atoms in the branches). Examples of theC1 to C7 alkylene group include a methylene group, anethylene group, a propylene group, and a butylene group.Examples of the C1 to C7 alkylene group include -CH2-, -(CH2)2-, -(CH2)3-, -CH(CH3)-, -(CH2)3-, -(CH(CH3))2-, -(CH2)2-CH(CH3)-, -(CH2)3-CH(CH3)-, -(CH2)2-CH(C2H5)-, -(CH2)6-, -(CH2)2-C(C2H5)2-, and -(CH2)3C(CH3)2CH2-.
[0030] The term "C2 to C7 alkenylene group" refers to alinear or branched alkenylene group having 2 to 7 carbonatoms and having 1 or more double bonds in the chain, andexamples of the C2 to C7 alkenylene group include divalentgroups having 1 or more double bonds formed by excluding 2to 5 hydrogen atoms of adjacent carbon atoms from thealkylene groups.
[0031] Meanwhile, preferred non-limiting specific examplesof the polymer having an electrophilic functional group atthe terminal include a compound that has four brancheshaving a polyethylene glycol skeleton and has an N-hydroxysuccinimidyl(NHS) group at the terminal and is representedby the following formula (II).[Chem. 2]
[0032] In the formula (II), n21 to n24 may be the same ordifferent. The closer the values of n21 to n24 are, themore uniform three-dimensional structure and the higherstrength the gel can have, and therefore the values arepreferably close, and more preferably the same. If thevalues of n21 to n24 are too high, the gel has low strength,and if the values of n21 to n24 are too low, the gel is lesslikely to be formed due to the steric hindrance of thecompound. Therefore, the values of n21 to n24 are, forexample, an integer value of 5 to 600, preferably 25 to250, more preferably 50 to 120, and still more preferably110 to 120.
[0033] In the formula (II), R21 to R24 are linker moietieseach connecting a functional group and a core moiety. R21to R24 may be the same or different, but are preferably thesame in order to produce a gel having a uniform threedimensionalstructure and high strength. In the formula(II), R21 to R24 are the same or different, and eachrepresent a C1 to C7 alkylene group, a C2 to C7 alkenylenegroup, -NH-R25-, -CO-R25-, -R26-O-R27-, -R26-NH-R27-, -R26-CO2-R27-, -R26-CO2-NH-R17-, -R26-CO-R27-, or -R26-CO-NH-R27-. Here,R25 represents a C1 to C7 alkylene group. R26 represents aC1 to C3 alkylene group. R27 represents a C1 to C5 alkylenegroup.
[0034] In the present description, the alkylene group andthe alkenylene group may have one or more arbitrarysubstituents. Examples of the substituent include, but arenot limited to, alkoxy groups, halogen atoms (any of afluorine atom, a chlorine atom, a bromine atom, and aniodine atom), an amino group, mono- or disubstituted aminogroups, substituted silyl groups, acyl groups, and arylgroups. In the case of an alkyl group having two or moresubstituents, they may be the same or different. The sameapplies to alkyl moieties in other substituents havingalkyl moieties (such as alkyloxy groups and aralkylgroups).
[0035] In the present description, in a case where acertain functional group is defined as a functional groupthat may have a substituent, the kind of the substituent,the substitution position, and the number of substituentsare not particularly limited, and in the case of afunctional group having two or more substituents, they maybe the same or different. Examples of the substituentinclude, but are not limited to, alkyl groups, alkoxygroups, a hydroxyl group, a carboxyl group, halogen atoms,a sulfo group, an amino group, alkoxycarbonyl groups, andan oxo group. These substituents may further have asubstituent.
[0036] As another aspect, one of the first polymer or thesecond polymer can be replaced with a low molecular weightcompound. In this case, the low molecular weight compoundhas one or more nucleophilic functional groups orelectrophilic functional groups in the molecule. Thus, forexample, a low molecular weight compound having anucleophilic functional group in the molecule is used inplace of the first polymer and reacted with the secondpolymer having one or more electrophilic functional groupsin the side chain or at the terminal, and as a result, thesecond polymer can gel. Examples of the "low molecularweight compound having a nucleophilic functional group inthe molecule" include compounds having a thiol group in themolecule, and for example, dithiothreitol can be used.
[0037] (1-2) Conditions of Polymer SolutionsThe polymer solution A and the polymer solution Bincluded in the polymer material kit of the presentinvention satisfy the following conditions of the polymerconcentration, the pH, the ionic strength, and the like.
[0038] The concentration of the first polymer in thepolymer solution A and the concentration of the secondpolymer in the polymer solution B are each in the range of10 to 300 g / L, preferably in the range of 30 to 200 g / L,and more preferably in the range of 50 to 150 g / L. Byadjusting the polymer concentrations, the gelation time canbe set within a desired range. The concentrations of thefirst and the second polymers may be the same or differentas long as the above-described range is satisfied, but arepreferably the same.
[0039] The polymer solutions A and B are adjusted so that amixed solution obtained by mixing these solutions is in anacidic region (pH: less than 7), and are preferablyadjusted so that the pH is in the range of 3 to less than7, and more preferably in the range of 3.2 to 5.0. Any oneof the polymer solutions A and B preferably has a pH in therange of 3 to less than 7, and preferably in the range of3.2 to 5.0. However, as long as the mixed solution of thepolymer solutions A and B satisfies the above-describedacidic pH range, the other solution can have a pH of morethan 8. In a typical aspect, both the polymer solutions Aand B preferably have a pH in these ranges. With such a pHin an acidic side, no gelation reaction is caused(preferably, a gelation reaction does not proceed) in ashort time by only mixing the polymer solutions A and B asthey are, but in a case where the two solutions are mixedin an environment where blood or the like is present andthe pH is near neutral (including a case where the mixedsolution is applied to an environment having a pH nearneutral), the pH of the polymer solution increases, and agelation reaction can proceed. Thus, a gel can be formedin situ in a relatively short time in an environment whereblood or the like is present and the pH is near neutral.The pH of the polymer solution A and the pH of the polymersolution B may be the same or different as long as theabove-described range is satisfied, but are preferably thesame.
[0040] The pH of the polymer solutions A and B can be setusing a pH buffer known in the art. For example, acitrate-phosphate buffer (CPB) is used and the mixing ratioof citric acid and disodium hydrogen phosphate is changed,and thus the pH can be adjusted to the above-describedrange.
[0041] The polymer solutions A and B are adjusted so that amixed solution obtained by mixing the polymer solutions Aand B has an ionic strength in the range of 10 to 100 mM,and preferably in the range of 10 to 40 mM. By adjustingthe ionic strength, the gelation time can be set within adesired range. The ionic strength of the polymer solutionA and the ionic strength of the polymer solution B may bethe same or different as long as the above-described rangeis satisfied, but are preferably the same.
[0042] If the conditions of the polymer concentration, thepH, and the ionic strength are set within the abovedescribedrange in each of the polymer solutions A and B, ahydrogel in which the first polymer and the second polymerare crosslinked with each other can be formed in situ bymixing these solutions in an environment where a liquid ispresent that has a pH of 6.5 to 8.0, which corresponds tothe pH of a body fluid such as blood.
[0043] The gelation time at this time is preferably in therange of 1 to 30 seconds, and more preferably in the rangeof 1 to 10 seconds. Again, the gelation time can beadjusted mainly by appropriately setting the polymerconcentration, the pH, and the ionic strength in thepolymer solution. Here, the term "gelation time" refers toa time required until the storage elastic modulus G' andthe loss elastic modulus G" satisfy G' = G".
[0044] The solvents in the polymer solutions A and B arewater, but in some cases, may be a mixed solvent containingan alcohol such as ethanol or another organic solvent. Thepolymer solutions A and B are preferably an aqueoussolution in which water is used as a single solvent.
[0045] The volumes of the polymer solutions A and B in thepolymer material kit of the present invention can beappropriately adjusted according to, for example, the areaand the structure complexity of the bleeding site, theblood vessel, or the like to which the polymer solutions Aand B are applied, and are typically in the range of 0.1 to20 ml, and preferably 1 to 10 ml.
[0046] (1-3) HydrogelAs described above, the first polymer and the secondpolymer can be crosslinked with each other to form ahydrogel. In the present description, the term "gel"generally refers to a dispersion system of a polymer havingno fluidity, and refers to a state in which storage elasticmodulus G' and the loss elastic modulus G" have a relation. The term "hydrogel" refers to a gel containingwater.
[0047] The hydrogel formed using the first polymer and thesecond polymer preferably has an equilibrium swellingdegree in the range of 0.9 to 3.5, and more preferably inthe range of 0.9 to 2.5. As a result, after the hydrogelis formed in a bleeding site, a blood vessel, or the like,the gel does not excessively expand, and when the gelremains in the affected part for a certain period of time,an undesirable influence can be suppressed. Here, the term"equilibrium swelling degree" refers to a value of theswelling degree when a change in the swelling degree withtime after gel formation reaches an equilibrium state. Theswelling degree can be measured with a method commonly usedin the art. As the swelling degree, a value measured at25°C can be used.
[0048] The hydrogel formed using the first polymer and thesecond polymer preferably has a Young's modulus in therange of 0.1 x 104 to 4 x 104 Pa, and more preferably inthe range of 0.5 x 104 to 2 x 104 Pa. As a result, thehydrogel formed in a bleeding site, a blood vessel, or thelike can have an appropriate strength to remain in theaffected part for a certain period of time.
[0049] 2. Hemostatic Agent and the Like, and HemostaticMethod and the Like of the Present InventionIn another aspect, the present invention alsorelates to a hemostatic agent, a vascular occlusion agent,a tissue covering agent, or a body fluid coagulantincluding the polymer material kit.
[0050] As described above, a gel-blood complexincorporating blood can be formed using the polymermaterial kit of the present invention by applying thepolymer solutions A and B to an environment where blood ispresent such as a bleeding site or the interior of a bloodvessel to form a gel in situ. As a result, it is possibleto provide an excellent blood coagulation effect by takingblood into the gel, and a physical hemostatic effect bycovering the bleeding site or the like with the gel.Applying such in-situ gel formation to a blood vessel suchas a vein or an artery enables use for vascular occlusion,and enables use for coagulation of not only blood but alsoa body fluid having a pH near neutral.
[0051] Here, the term "tissue" showing a target of thepresent invention can broadly mean a living tissue and aliving organ where a liquid having a pH near neutral ispresent, and examples of the tissue include organs, nerves,muscles, and a part thereof. However, even a site having asurface that is generally considered to be acidicoriginally can be included in examples of the tissue as atarget of the present invention when the pH is temporarilyor permanently modified to a pH near neutral by a priortreatment. Examples of such a site include, but are notlimited to, a gastric mucosa.
[0052] From another viewpoint, the present invention alsorelates to a method for producing such a hemostatic agent,vascular occlusion agent, tissue covering agent, or bodyfluid coagulant. The method is characterized by includinga step of applying a polymer solution A containing a firstpolymer and a second polymer solution B containing a secondpolymer to an environment where a liquid having a pH nearneutral, that is, a pH of 6.5 to 8.0 is present. Inaddition, the kinds of the first and second polymers andthe conditions of the polymer solutions A and B are asdescribed above.
[0053] Here, the "environment where a liquid having a pH of6.5 to 8.0 is present" is preferably a place where blood ora body fluid is present, and can be, for example, a bloodvessel such as an artery or a vein, or a tissue where bloodor a body fluid is present. The range of the pH can bepreferably 6.5 to 7.5.
[0054] The step of "applying" a mixed solution of thepolymer solution A and the second polymer solution B to anenvironment where a liquid having a pH of 6.5 to 8.0 ispresent is typically exemplified by mixing the polymersolution A and the second polymer solution B in such a pHenvironment. Examples of the step include directlydripping or spraying the polymer solutions A and B in orderon an affected part where blood is present. In some cases,the polymer solutions A and B may be dripped or sprayedsimultaneously. As described above, the polymer solutionsA and B are set to solution conditions under which nogelation reaction is caused (preferably, a gelationreaction does not proceed) in a short time by only mixingthe polymer solutions A and B as they are, and therefore itis also possible to mix the polymer solutions A and B inadvance to obtain one solution and then apply the solutionto an environment where a liquid having a pH of 6.5 to 8.0is present.
[0055] Another aspect of the step of "applying" can beexemplified by dripping the polymer solution A and thepolymer solution B on a carrier and then bringing thecarrier into contact with an environment where a liquidhaving a pH of 6.5 to 8.0 is present. This case includesonce holding the polymer solutions in the carrier and thencovering or protecting an affected part where blood ispresent (such as an affected part after suture) with thecarrier. The carrier is not particularly limited as longas it includes a material capable of holding the polymersolutions, and examples of the carrier include clothmembers such as gauze and members having absorbability suchas sponge. Further modification example is also possiblein which the carrier in a state of holding any one of thepolymer solutions A and B is brought into contact with anaffected part or the like and then the other polymersolution is dripped or sprayed on the carrier.
[0056] In a method of mixing the polymer solutions A and Bby dripping, for example, a two-liquid mixing syringe asdisclosed in WO 2007 / 083522 A can be used. Thetemperatures of the two liquids at the time of mixing isnot particularly limited as long as the precursor units aredissolved and the liquids have fluidity. For example, thetemperatures of the two liquids may be different, but arepreferably the same because two liquids having the sametemperature are easily mixed.
[0057] In a method of spraying the polymer solution Aand / or the polymer solution B, a sprayer storing thesolution can be used. As the sprayer, a known sprayer inthe art can be appropriately used, and a medical sprayer ispreferable. Therefore, such a sprayer can be used as acontainer in the kit of the present invention, and in thiscase, one aspect of the present invention can be a medicaldevice and preferably a sprayer in which the polymersolutions A and B are stored.
[0058] It can also be said that performing the method forproducing of the present invention corresponds to ahemostatic method, a vascular occlusion method, a tissuecovering method, and a body fluid coagulation method inwhich the polymer material kit is used. Note that atissue, a blood vessel, or the like that can be a target isnot necessarily in a living body, and this method includesapplication to a tissue or the like taken out from the bodyby surgery or the like.Examples
[0059] Hereinafter, the present invention will be describedin more detail with reference to Examples, but the presentinvention is not limited thereto.
[0060] 1. Preparation of Polymer SolutionsAs raw material polymers, tetrathiol-polyethyleneglycol (Tetra-PEG-SH) having a -SH group at the terminaland tetramaleimidyl-polyethylene glycol (Tetra-PEG-MA)having a maleimidyl group at the terminal were used. Asthese raw material polymers, raw material polymerscommercially available from NOF CORPORATION were used.Both the raw material polymers had a weight averagemolecular weight (Mw) of 20000.
[0061] As a buffer for polymer solutions, a citratephosphatebuffer (CPB) was used. The mixing ratio ofcitric acid and disodium hydrogen phosphate was changed toadjust the pH. The molar concentrations (referred to asionic strength) of citric acid and disodium hydrogenphosphate were changed to adjust the buffer capacity.
[0062] In the case of preparing a CPB having a pH of 3.8and an ionic strength of 200 mM, each polymer solution wasprepared with the following procedure.1. A 200 mM aqueous citric acid solution and a 200mM aqueous disodium hydrogen phosphate solution areprepared.2. The aqueous citric acid solution and the aqueousdisodium hydrogen phosphate solution are mixed at a ratioof aqueous citric acid solution : aqueous disodium hydrogenphosphate solution = 32.3 : 35.4.
[0063] In the case of a pH of 5.8, the solutions are mixedat a ratio of 19.7 : 60.6, and in the case of a pH of 3.0,the solutions are mixed at a ratio of 39.8 : 20.4.
[0064] The pH was finely adjusted by mixing these CPBs at acertain ratio. Each pH was measured using a pH meter(manufactured by HORIBA, Ltd.).
[0065] 2. Gelation ExperimentThe gelation behavior of the Tetra-PEG polymer wasevaluated using cow milk having a pH equivalent to that ofblood (pH = 7.4).
[0066] Two kinds of prepolymer solutions were each preparedin an amount of 1 mL, and the time from mixing of thesolutions to gelation of the resulting mixture wasmeasured, and thus the gelation time was examined. Here,the gelation time was simply defined as the time until thesolution did not fall from the inverted containercontaining the solution. The concentration of the polymerand the pH and the ionic strength of the buffer werevaried.
[0067] Fig. 1 shows the results of the dependence of thepolymer concentration and the pH on the gelation time, andFig. 2 shows the results of the dependence of the ionicstrength on the gelation time. It has been found that thegelation time depends on the concentration of theprepolymer and the pH of the buffer. The gelation timealso changes when the ionic strength of the buffer (whichis an index of the strength of the ability to maintain thepH) is changed, but this is simply because the pH cannot bemaintained as the ionic strength decreases. In fact, whenthe relation between the pH and the gelation time obtainedfrom Figs. 2 and 3 is plotted on the graph of the relationbetween the pH and the gelation time at the sameconcentration, the same relation is obtained (Fig. 4).
[0068] Next, cow milk was subjected to a gelation test.First, a prepolymer solution was prepared for the presentcow milk gelation test (prepolymer concentration: 150 g / L,solvent: pH 3.4, 200 mM). This prepolymer solution wasadded to cow milk (cow milk 10 : prepolymer solution 1;volume ratio), and the fluidity of the cow milk wasevaluated macroscopically. The gelation time at this timewas 3 minutes. In order to further adjust the gelationtime, another prepolymer solution was prepared (prepolymerconcentration: 200 g / L, solvent: pH 3.4, 40 mM). When theabove test was performed using this prepolymer solution,the gelation time was shortened to 10 seconds.
[0069] Rat whole blood was subjected to a gelation test.First, a prepolymer solution was prepared for the presentgelation test (prepolymer concentration: 200 g / L, solvent:pH 3.4, 40 mM). Whole blood collected from a rat washeparinized. The heparinized whole blood was divided intotwo parts, and to one part, the previously preparedprepolymer solution was added (whole blood 10 : prepolymersolution 1; volume ratio). To the other part, noprepolymer solution was added. At this time, gelation wasobserved only in the group to which the prepolymer solutionwas added.
[0070] The Tetra-PEG-SH was replaced with dithiothreitol,which has two SH groups (molecular weight: 154.253 g / mol),and a gelation test was performed. First, a prepolymersolution of Tetra-PEG-MA was prepared (prepolymerconcentration: 200 g / L, solvent: pH 3.4, 40 mM). Adithiothreitol solution was newly prepared so that theterminal MA group of the prepolymer solution and the SHgroup of dithiothreitol were at the same molarconcentration. When these two liquids having the samevolume were mixed, the fluidity was lost, and gelation wasconfirmed.
[0071] The Tetra-PEG-SH was replaced with Linear-PEG-SHhaving two branches and having an SH group at the terminal,and a gelation test was performed. First, a prepolymersolution of Tetra-PEG-MA was prepared (prepolymerconcentration: 200 g / L, solvent: pH 3.4, 40 mM). A Linear-PEG-SH solution was newly prepared so that the terminal MAgroup of the prepolymer solution and the SH group ofLinear-PEG-SH were at the same molar concentration. Whenthese two liquids having the same volume were mixed, thefluidity was lost, and gelation was confirmed.
[0072] The Tetra-PEG-MA was replaced with Linear-PEG-MAhaving two branches and having an MA group at the terminal,and a gelation test was performed. First, a prepolymersolution of Tetra-PEG-SH was prepared (prepolymerconcentration: 200 g / L, solvent: pH 3.4, 40 mM). A LinearPEG-MA solution was newly prepared so that the terminal SHgroup of the prepolymer solution and the MA group ofLinear-PEG-MA were at the same molar concentration. Whenthese two liquids having the same volume were mixed, thefluidity was lost, and gelation was confirmed.
[0073] 3. Measurement of Young's ModulusThe prepolymer solution after mixing the two liquidsis injected into the body and then mixed with blood, andthus gels. The change in the hardness (Young's modulus)depending on the content of blood at this time wasexamined. A prepolymer solution was prepared with theabove-described procedure (prepolymer concentration: 50g / L, solvent: pH 3.8, 200 mM). Two kinds of prepolymerswere mixed, then cow milk was further mixed at variousratios, and after gelation and completion of the reaction,the Young's modulus was determined in a compression test(Fig. 5). For example, when cow milk having the samevolume as the prepolymer solution is added to theprepolymer solution, the fraction of milk is expressed as50%. The larger the volume of the added cow milk was, thelower the final Young's modulus was. This is because theaddition of cow milk caused dilution of the prepolymersolution and reduction in the crosslinking point density ofthe gel.
[0074] 4. Measurement of Equilibrium Swelling DegreeExperimental procedureSolvent: CPB (pH 3.0, 20 mM)Prepolymer concentration: 60, 120 g / L (6, 12 wt%)
[0075] The gel preparation procedure is the same asdescribed above. The two liquids were mixed, then aftergelation and completion of the reaction, the mixture wasput into cow milk, and the degree of swelling was examined.The gels at both concentrations reached an equilibriumswelling state in about 4 hours (Fig. 6). The equilibriumswelling degree was 1.7 at 60 g / L and 2.3 at 120 g / L, andthese values were the same as those in the case of swellingin water (Fig. 7), suggesting that the results of theswelling experiment in water may be used.
[0076] 5. Application to Rat Blood VesselExperimental procedureSolvent: CPB (pH 4.6, 20 mM) (mixed at CPB (pH 3.8,20 mM) : CP (pH 5.8, 20 mM) = 1 : 2)Prepolymer concentration: 50 g / L (5 wt%)
[0077] The gel preparation procedure is the same asdescribed above. The two liquids were mixed, and thenblood vessel of a rat thigh within about 3 minutes becausethe gelation time of the mixture in a state of being leftto stand was about 3 minutes (this gelation time can bechanged depending on the pH). At this time, the upstreampart of the blood vessel was compressed to stop the bloodflow, and thus the gel was prevented from flowingimmediately after the injection. The ionic strength of thebuffer was as low as 20 mM, and therefore the pH was easilyincreased when the solution was mixed with blood after theinjection, and gelation occurred immediately. The state ofcompressing the upstream part of the blood vessel wasmaintained for about 30 seconds, then the hand wasreleased, and it was confirmed that the gel was solidifiedand not flowing. After a lapse of a certain period oftime, the affected part was opened again, and it wasconfirmed that the gel did not flow out. Fig. 8 shows theimage at this time. It was confirmed that the effect ofvascular occlusion by the gel lasted for at least 2 to 3weeks.
[0078] In the case of using the conditions of the solvent:CPB (pH 3.0, 20 mM) and the prepolymer concentration: 100g / L (10 wt%), a gelation time of 10 minutes or more wasrequired after mixing the two liquids in a state of beingleft to stand, but the ionic strength was so low that thepH increased after mixing with rat blood, and gelationoccurred immediately.
[0079] 6. Experimental Procedure for Application toAbdominal Aorta of RatSolvent: CPB (pH 3.4, 40 mM)Prepolymer concentration: 200 g / L (20 wt%)An abdominal aorta of a rat was punctured with aninjection needle having an outer diameter of 0.2 mm topromote bleeding. A prepolymer solution after mixing thetwo liquids was added to the bleeding point (Fig. 9). Inthis state, pressure hemostasis was performed for 1 minute,and hemostasis was confirmed. At this time, as acomparative control group, pressure hemostasis wasperformed in the same manner for 1 minute without addingthe prepolymer solution, and as a result, hemostasis wasnot observed.
Claims
1. A polymer material kit comprising: a polymer solution A containing a first polymer; and a second polymer solution B containing a second polymer, the first polymer and the second polymer being a hydrophilic polymer having a polyalkylene glycol skeleton or a polyvinyl skeleton, wherein a combination of the first polymer and the second polymer is capable of forming a hydrogel when the first polymer and the second polymer are crosslinked with each other, the first polymer and the second polymer have a weight average molecular weight (Mw) in a range of 1 x 103 to 1 x 105, the polymer solution A and the second polymer solution B have a concentration of the first polymer and a concentration of the second polymer in a range of 10 to 300 g / L, respectively, and a mixed solution obtained by mixing the polymer solution A and the second polymer solution B has a pH in a range of 3 to less than 7 and an ionic strength in a range of 10 to 100 mM.
2. The polymer material kit according to claim 1, wherein the first polymer and the second polymer are a two-, three-, or four-armed polyethylene glycol.
3. The polymer material kit according to claim 1 or 2, wherein the first polymer has one or more nucleophilic functional groups in a side chain or at a terminal, and the second polymer has one or more electrophilic functional groups in a side chain or at a terminal.
4. The polymer material kit according to any one of claims 1 to 3, wherein the one or more nucleophilic functional groups are selected from the group consisting of a thiol group and an amino group, and the one or more electrophilic functional groups are selected from the group consisting of a maleimidyl group, an N-hydroxy-succinimidyl (NHS) group, a sulfosuccinimidyl group, a phthalimidyl group, an imidazoyl group, an acryloyl group, a nitrophenyl group, and -CO2PhNO2.
5. The polymer material kit according to any one of claims 1 to 4, wherein the polymer solution A and the second polymer solution B have a pH in a range of 3 to less than 7.
6. The polymer material kit according to any one of claims 1 to 5, wherein a hydrogel in which the first polymer and the second polymer are crosslinked with each other is formed when the polymer solution A and the second polymer solution B are mixed in an environment where a liquid having a pH of 6.5 to 8.0 is present.
7. The polymer material kit according to claim 6, wherein the hydrogel formed using the first polymer and the second polymer has a gelation time in a range of 1 to 30 seconds.
8. The polymer material kit according to claim 6 or 7, wherein the hydrogel formed using the first polymer and the second polymer has an equilibrium swelling degree in a range of 0.9 to 3.5.
9. The polymer material kit according to any one of claims 6 to 8, wherein the hydrogel formed using the first polymer and the second polymer has a Young's modulus in a range of 0.1 x 104 to 4 x 104 Pa.
10. The polymer material kit according to any one of claims 1 to 9, to be used for hemostasis, vascular occlusion, tissue covering, or body fluid coagulation.
11. A hemostatic agent comprising the polymer material kit according to any one of claims 1 to 10.
12. A vascular occlusion agent comprising the polymer material kit according to any one of claims 1 to 10.
13. A tissue covering agent comprising the polymer material kit according to any one of claims 1 to 10.
14. A body fluid coagulant comprising the polymer material kit according to any one of claims 1 to 10.
15. A method for producing a hemostatic agent, a vascular occlusion agent, a tissue covering agent, or a body fluid coagulant containing a hydrogel, the method comprising a step of applying a mixed solution of a polymer solution A containing a first polymer and a second polymer solution B containing a second polymer to an environment where a liquid having a pH of 6.5 to 8.0 is present, wherein the first polymer and the second polymer are a hydrophilic polymer having a polyalkylene glycol skeleton or a polyvinyl skeleton, a combination of the first polymer and the second polymer is capable of forming a hydrogel when the first polymer and the second polymer are crosslinked with each other, the first polymer and the second polymer have a weight average molecular weight (Mw) in a range of 1 x 103 to 1 x 105, the polymer solution A and the second polymer solution B have a concentration of the first polymer and a concentration of the second polymer in a range of 10 to 300 g / L, respectively, and the mixed solution obtained by mixing the polymer solution A and the second polymer solution B has a pH of 3 to less than 7 and an ionic strength in a range of 10 to 100 mM.
16. The method according to claim 15, comprising mixing the polymer solution A and the second polymer solution B in an environment where a liquid having a pH of 6.5 to 8.0 is present.
17. The method according to claim 15, comprising dripping the polymer solution A and the second polymer solution B on a carrier and then bringing the carrier into contact with an environment where a liquid having a pH of 6.5 to 8.0 is present.
18. The method according to any one of claims 15 to 17, wherein the polymer solution A and the second polymer solution B have a pH in a range of 3 to less than 7.
19. A hemostatic method comprising using the polymer material kit according to any one of claims 1 to 10.
20. A vascular occlusion method comprising using the polymer material kit according to any one of claims 1 to 10.
21. A tissue covering method comprising using the polymer material kit according to any one of claims 1 to 10.
22. A body fluid coagulation method comprising using the polymer material kit according to any one of claims 1 to 10.
23. A medical device comprising the polymer material kit according to any one of claims 1 to 10.
24. The medical device according to claim 23, wherein at least one of the polymer solution A or the second polymer solution B is stored in a sprayer.