Aqueous coating agent.

IT202600041278T2Active Publication Date: 2026-08-19BRILLUX GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IT502026000041278
Authority / Receiving Office
IT · IT
Patent Type
Patents
Current Assignee / Owner
Priority Date
2016-07-21
Filing Date
2017-07-18
Publication Date
2026-08-19
Estimated Expiration
2037-07-18

AI Technical Summary

Technical Problem

Existing aqueous coating agents for interior and exterior use lack adhesion to common surfaces, are prone to the 'writing effect' under mechanical stress, and do not provide a soft-feel effect suitable for both feel and visual appeal, while also being difficult to apply with standard painting tools.

Method used

An aqueous coating agent comprising 5-30% polymer with an average particle size of 60-300 nm, 2-30% organic filler, 0.5-8% matting agent with an average size of 0.5-9 µm, and 30-70% water, which can be easily applied and provides good adhesion and mechanical resistance, while maintaining a soft-feel and matte appearance.

Benefits of technology

The coating agent achieves excellent adhesion to surfaces like concrete, stone, and plaster, is easy to apply with standard tools, and exhibits high resistance to mechanical influences with minimal 'writing effect', while maintaining a pleasant soft-feel and matte appearance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

An aqueous coating composition is presented and described, containing, based on total weight, a. 5 to 30 wt.% polymer with an average particle size of 60 to 300 nm, b. 2 to 30 wt.% organic filler, c. 0.5 to 8 wt.% matting agent with an average particle size of 0.5 to 9 µm, d. 30 to 70 wt.% water. Furthermore, a process for producing the aqueous coating composition according to the invention and the use of the aqueous coating composition as a dispersion paint for interior and / or exterior applications are described.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to an aqueous coating agent, a method for producing the aqueous coating agent, and the use of the aqueous coating agent as a dispersion paint for indoor and / or outdoor use.

[0002] Particularly in the automotive sector, a trend towards so-called soft-feel coatings has been observed for some time. These coatings create a unique tactile sensation (haptic quality) that can be described as velvety, soft, rubbery, or warm, and is perceived as pleasant. Furthermore, these soft-feel coatings give the surface a matte appearance that is considered appealing.

[0003] In the automotive sector, such coatings can be applied using specialized machines and processes, such as in special coating systems that operate at elevated temperatures and / or reduced pressure. Therefore, many materials and material combinations can be used that, for example, cannot be used in interior and / or exterior dispersion paints because they are difficult to apply or dry poorly.

[0004] Matte emulsion paints, especially matte wall paints, often suffer from an effect commonly referred to as "writing effect." This describes the phenomenon where even slight mechanical stress, such as scratching with a fingernail, leaves marks on a matte surface. This effect is usually undesirable, as it disrupts the desired visual appearance.

[0005] WO 2006 / 032373 A1 describes coating compositions containing hydroxyl-group-free polyurethanes and / or polyurethane ureas based on polycarbonate polyols and polytetramethylene glycol polyols, ionically modified polyurethanes and / or polyurethane ureas containing hydroxyl and / or amino groups, a crosslinker, and optionally other film-forming resins. These coatings are described as hydrolysis-stable and produce a soft-feel effect. However, WO 2006 / 032373 A1 does not specify the size of the components contained in the coating composition.

[0006] Similarly, US Patent 2007 / 0049683 A1 describes an aqueous coating composition for plastic automotive interior parts. This composition contains an aqueous polyurethane or acrylic resin or mixtures thereof, an aqueous polyurethane resin with hydroxyl groups, micronized silica with an average particle size of 10 to 30 µm, a polyethylene paraffin wax with an average particle size of 30 to 100 nm, a polysiloxane, a polyoxyethylene sorbitan monooleate stabilizer, optionally encapsulated aromatic particles for deodorization, and a trifunctional hexamethylene diisocyanate crosslinker. However, this composition does not contain a specific matting agent. Furthermore, the composition is specifically designed for plastic components in automotive interiors; its suitability as an interior and / or exterior dispersion paint is not mentioned.

[0007] The object of the invention is to provide an aqueous coating agent that can be used as a dispersion paint, particularly indoors and / or outdoors.

[0008] Another object of the invention is to provide an aqueous coating agent that exhibits good adhesion to surfaces on which dispersion paints are usually applied, for example concrete, stone, wallpaper, in particular paper, glass fabric, plastic, canvas, plaster.

[0009] Another object of the invention is to provide an aqueous coating agent that can be easily applied with frequently used painting tools such as brushes and / or paint rollers.

[0010] Another object of the invention is to provide an aqueous coating agent that exhibits a soft-feel effect, particularly with regard to the tactile sensation and / or the optical impression.

[0011] Another object of the invention is to provide an aqueous coating agent that has good resistance to mechanical impacts and, in particular, exhibits only a low "writing effect".

[0012] All or some of these problems are solved by the aqueous coating agents specified in claims 1 and 19, the method specified in claim 16, and the use specified in claim 20.

[0013] Advantageous configurations are specified in the dependent claims and are explained in detail below.

[0014] The aqueous coating agent according to the invention contains, based on the total weight of the coating agent, a. 5 to 30 wt.% polymer with a mean particle size of 60 to 300 nm, b. 2 to 30 wt.% organic filler, c. 0.5 to 8 wt.% matting agent with a mean particle size of 0.5 to 9 µm, d. 30 to 70 wt.% water.

[0015] Surprisingly, it was found that the combination of 5 to 30 wt.% of a polymer with a mean particle size of 60 to 300 nm with 2 to 30 wt.% of an organic filler and 0.5 to 8 wt.% matting agent with a mean particle size of 0.5 to 9 µm in 30 to 70 wt.% water results in an aqueous coating that exhibits a pleasant soft-feel effect both in terms of tactile sensation and visual appearance and / or can be used as a dispersion paint indoors and / or outdoors and / or shows good adhesion to concrete, stone, wallpaper and / or plaster and / or can be applied well, especially evenly, with common painting tools such as brushes and / or paint rollers and / or has good resistance to mechanical stress.This was particularly surprising because coating materials with a pleasing optical appearance, especially a matte optical appearance, usually exhibit low resistance to mechanical stress.

[0016] The mean particle size can, in particular, be defined as the Dso value. The Dso value can, in particular, define the size at which 50%, e.g., 50 wt.%, of the particles are smaller than the specified size. For example, 50%, e.g., 50 wt.%, of the particles would then pass through a theoretical sieve size. Methods for determining the mean particle size, in particular the Dso value, are known to those skilled in the art. The mean particle size, in particular the Dso value, can, for example, be determined by generating a particle size distribution. The measurement can be carried out, for example, by light scattering, in particular by laser diffractometry or photon correlation spectroscopy. In particular, the mean particle size, in particular the Dso value, can be measured in a liquid medium, for example, an aqueous medium.The measurement can be carried out in accordance with ISO 13321, in particular ISO 13321:1996, and / or ISO 22412, in particular ISO 22412:2008. For example, a Malvern Mastersizer 2000 or 3000 can be used to determine the mean particle size, in particular the Dso value. Other methods for determining the mean particle size, in particular the Dso value, include light and / or laser diffraction. Furthermore, the mean particle size, in particular the Dso value, can be determined using an ultracentrifuge or chromatographic methods, for example, capillary hydrodynamic fractionation (CHDF).

[0017] Mattifying agents are additives for coating materials that affect the surface of the coating in such a way that its gloss level, especially the reflectometer value, decreases.

[0018] The aqueous coating composition contains 5 to 30 wt.%, preferably 8 to 17 wt.%, more preferably 10 to 15 wt.%, and particularly preferably 11 to 13 wt.% polymer, in each case based on the total weight of the coating composition. The information regarding the polymer content in the aqueous coating composition refers to the polymer as a solid fraction. However, the polymer is preferably added in the form of a dispersion, particularly an aqueous dispersion, when producing an aqueous coating composition. Advantageously, these polymer dispersions, particularly the aqueous polymer dispersions, contain 40 to 70 wt.%, preferably 45 to 60 wt.%, more preferably 45 to 55 wt.%, and particularly preferably 50 wt.% polymer as a solid fraction. If the polymer is added as an aqueous polymer dispersion, the water of the polymer dispersion is considered part of the total water content of the aqueous coating composition.If the polymer is present, for example, as a 50% dispersion in water, the aqueous coating material contains 10 to 60 wt.%, preferably 16 to 34 wt.%, more preferably 20 to 30 wt.%, and particularly preferably 22 to 26 wt.%, of the polymer dispersion and 25 to 50 wt.% water, in each case based on the total weight of the aqueous coating material. Aqueous coating materials containing polymer in these amounts have shown good processing properties, in particular good applicability.

[0019] Various polymers are suitable for use as the aqueous coating agent. The polymer can be a homopolymer or a copolymer, with different architectures being conceivable for copolymers, such as statistical copolymers, gradient copolymers, alternating copolymers, block or segment copolymers, and graft copolymers.

[0020] Suitable monomers for the polymer of the coating material according to the invention, or from which it is constructed or on which it is based, are in particular monomers with a carbon-carbon double bond. Examples of monomers with a carbon-carbon double bond are acrylic acid and its esters or amides such as methyl acrylate, ethyl acrylate, propyl acrylate and butyl acrylate, acrylamide, methyl acrylamide, methacrylic acid and its esters and amides such as methyl methacrylate, ethyl methacrylate, propyl methacrylate and butyl methacrylate, methacrylamide, methyl methacrylamide, carboxylic acid vinyl esters such as vinyl acetate, vinyl propionate, N-vinylpyrrolidone and derivatives thereof, unsaturated carboxylic acids, their esters, amides and anhydrides, as well as ethylene-unsaturated compounds such as acrylonitrile, vinyl chloride and styrene.Homopolymers and copolymers, wherein the copolymers may have the aforementioned architectures, based on the aforementioned monomers yield polymers suitable for the aqueous coating material according to the invention.

[0021] Other polymers suitable for the aqueous coating material according to the invention are polyurethanes and polyester polyurethanes.

[0022] Furthermore, mixtures of the aforementioned polymers can also be used as polymers in the aqueous coating material according to the invention.

[0023] Preferably, the polymer is selected from the group consisting of polymers based on carboxylic acid vinyl esters, in particular vinyl acetate, vinyl propionate, N-vinylpyrrolidone and derivatives thereof, unsaturated carboxylic acids, their esters, amides and anhydrides, in particular acrylic acid and methacrylic acid as well as their esters and amides, and ethylene-unsaturated compounds such as acrylonitrile, vinyl chloride, styrene, and copolymers of the aforementioned monomers, polyurethanes, polyester polyurethanes and mixtures thereof.

[0024] Advantageously, the polymer is in the form of an aqueous dispersion with a solids content of 40 to 70 wt.%, preferably 45 to 60 wt.%, more preferably 45 to 55 wt.%, and particularly preferably 50 wt.%. This aqueous dispersion can, in particular, have a Brookfield viscosity at 25°C of 1000 to 10000 mPas, especially of 1500 to 8000 mPas, and / or a pH value of 7 to 11.4, especially of 8 to 9.

[0025] The polymer also advantageously has a glass transition temperature Tg, measured according to ISO 16805, in particular ISO 16805:2003, of -20 to 20°C, preferably of -10 to 10°C, more preferably of -5 to 5°C, and particularly preferably of 0 to 5°C.

[0026] Preferably, the polymer in the aqueous coating composition according to the invention has an average particle size of 70 to 200 nm, more preferably of 80 to 170 nm, more preferably of 100 to 150 nm, and particularly preferably of 120 nm. The above applies to the average particle size and its determination.

[0027] Advantageously, the polymer in the aqueous coating composition according to the invention is a copolymer. It is particularly advantageous if the copolymer contains or consists of at least acrylic acid or acrylic acid derivatives such as acrylic acid esters and at least one ethylene-unsaturated monomer such as, for example, styrene or acrylonitrile. Optimal results are obtained if the polymer in the aqueous coating composition according to the invention is a styrene-acrylate copolymer, in particular containing one or more acrylic acid esters and styrene, and especially with an average particle size of 120 nm. The above applies to the average particle size and its determination.

[0028] Furthermore, the polymer in the aqueous coating material according to the invention can also contain a crosslinker, in particular an ionic crosslinker.

[0029] It has been found that water-based coatings containing such polymers exhibit good adhesion to various surfaces, particularly concrete, stone, wallpaper, paper, fiberglass, plastic, canvas, and plaster. Furthermore, these water-based coatings can be easily applied with standard painting tools. They also demonstrate good resistance to mechanical stress.

[0030] The aqueous coating material further contains 2 to 30 wt.%, preferably 5 to 25 wt.%, more preferably 10 to 20 wt.%, particularly preferably 13 to 18 wt.%, organic filler, in each case based on the total weight of the coating material. Such quantities of organic filler result in a surface with a pleasant feel.

[0031] Various substances are suitable as organic fillers. Preferably, the organic filler is selected from the group consisting of polyurethane particles, polymethyl methacrylate particles, polymeric microspheres, cellulose fibers, textile fibers, cork flour, and mixtures thereof. Polyurethane particles, especially cross-linked polyurethane particles, are preferred as organic fillers. Such organic fillers integrate well into the aqueous coating material and exhibit minimal segregation effects even in the dry film.

[0032] Advantageously, the organic filler has an average particle size of 1 to 50 µm, preferably 5 to 40 µm, more preferably 20 to 40 µm, even more preferably 25 to 35 µm, particularly preferably 28 to 33 µm, and especially 30 µm. Organic fillers with such particle sizes result in surfaces with a pleasant feel. Surprisingly, it has also been found that organic fillers with such particle sizes impart good resistance to mechanical stress to the resulting surface. The above applies to the average particle size and its determination.

[0033] Furthermore, the aqueous coating agent contains 0.5 to 8 wt.%, preferably 1 to 6 wt.%, more preferably 2 to 4 wt.%, in each case based on the total weight of the coating agent, matting agent with an average particle size of 0.5 to 9 µm. The inclusion of a matting agent helps to create, in particular, the desired visual appearance, but also the desired tactile feel. The above statements regarding the average particle size and its determination apply.

[0034] Various substances can be used as matting agents. Preferably, the matting agent is selected from the group consisting of pyrogenic silica, polymethyl urea, ceramic microspheres, diatomaceous earth, quartz flour, talc, and wax additives such as polyethylene waxes. Polymethyl urea is preferably used as the matting agent. These matting agents have proven suitable for producing the effects described above.

[0035] Advantageously, the matting agent has a mean particle size of 1 to 8 µm, preferably 2 to 6 µm, and more preferably 4 µm. This allows for precise adjustment of both the desired visual appearance and the tactile feel. The above description applies to the mean particle size and its determination.

[0036] Aqueous coating compositions according to the invention, containing a combination of the aforementioned components, possess advantageous properties. In particular, coatings produced with the aqueous coating composition according to the invention have a pleasant feel. Furthermore, the coatings produced with the aqueous coating composition according to the invention have a matte appearance and can exhibit a gloss level, particularly a reflectometer value, according to DIN EN 13300, especially according to DIN EN 13300:2002-11, and measured according to DIN EN ISO 2813, especially according to DIN EN ISO 2813:2015-02, of less than 10, particularly less than 5, at a measuring angle of 85°. Moreover, aqueous coating compositions according to the invention adhere very well to various substrates such as concrete, stone, wallpaper, and / or plaster. They are also very suitable for use as dispersion paints in interior and / or exterior applications.They exhibit particularly good application properties, for example with typical painting tools such as brushes and / or paint rollers. Furthermore, they have high resistance to mechanical stress, and in particular, they show only a minimal writing effect. Such effects have been achieved especially with aqueous coating agents containing a polymer with a mean particle size of 100 to 150 nm, preferably 120 nm, in particular a styrene acrylate, an organic filler, in particular cross-linked polyurethane particles, with a mean particle size of 28 to 33 µm, preferably 30 µm, and a matting agent, in particular polymethyl urea, with a mean particle size of 2 to 6 µm, preferably 4 µm.

[0037] Furthermore, the aqueous coating composition preferably contains at least one inorganic filler and / or pigment. In particular, the aqueous coating composition can contain 1 to 20 wt.%, preferably 3 to 17 wt.%, more preferably 5 to 15 wt.%, and particularly preferably 8 to 12 wt.%, at least one inorganic filler and / or pigment, in each case based on the total weight of the coating composition. Inorganic fillers can, in particular, help to reduce the abrasion and / or wear of the coatings produced with the coating composition according to the invention.

[0038] Various substances are suitable as at least one inorganic filler. Advantageously, the at least one inorganic filler is selected from the group consisting of diatomaceous earth, dolomite, barium sulfate, feldspar, quartz, calcium carbonate, mica, kaolin, calcined kaolin, talc, aluminum silicates, and mixtures thereof. It is also advantageous if the average particle size of the at least one inorganic filler is smaller than the average particle size of the organic filler.

[0039] Various substances can also be used as pigments. For example, only inorganic or only organic pigments, or mixtures of inorganic and organic pigments, can be used.

[0040] Preferably, the pigment is selected from the group consisting of titanium dioxide, iron oxide yellow, arylide (monoazo), bismuth vanadate, perinone, rutile tin zinc, quinacridone, diketo-pyrrolo-pyrrole, iron oxide red, phthalocyanine blue, dioxazine, cobalt blue, ultramarine blue, phthalocyanine green, chromium oxide green, cobalt green, carbon black, iron oxide black, pyrazolo-quinazolone, naphthol-AS monoazo pigment and mixtures thereof.

[0041] Examples of inorganic pigments that can be used include oxides such as titanium dioxide, iron oxides (e.g., PY 42, PR 101, P.Bk. 11), chromium oxide green (e.g., PG 17), mixed-phase pigments (e.g., cobalt oxides blue PB 28 and green PG 50), bismuth vanadate PY 184, rutile tin-zinc PO 216), silicates (e.g., ultramarine blue PB 29), and carbon (e.g., carbon black P.Bk. 7).

[0042] Examples of organic pigments that can be used include azo pigments, e.g., arylide yellow (monoazo) PY 74, polycyclic pigments, e.g., quinacridone PR 122, perinone PO 43, pyrazolo-quinazolone PO 67, diketo-pyrrolo-pyrrole (DPP) PR 254, dioxazines PV 23, and metal complex pigments, e.g., copper phthalocyanines blue PB 15:3 and green PG 7.

[0043] The names of the inorganic and organic pigments used for the examples correspond to the Generic Names of the Colour Index of the British Society of Dyers and Colourists.

[0044] The use of pigments allows for the production of colored waterborne coatings that essentially cover the entire color spectrum. The use of fillers is particularly helpful in the production of white waterborne coatings.

[0045] In addition, the aqueous coating composition according to the invention may also contain further conventional additives. In particular, the aqueous coating composition may additionally contain one or more further additives selected from the group consisting of defoamers, dispersants, wetting agents, preservatives, stabilizers, surface protectants, water repellents, solvents and thickeners.

[0046] Additives and / or other additives may be present in a total amount of 0.1 to 30 wt.%, preferably 0.5 to 20 wt.%, more preferably 1 to 10 wt.%, particularly preferably 1.5 to 5 wt.%, in each case based on the total weight of the aqueous coating material.

[0047] Examples of thickening agents include alcohol alkoxylates, ethylene oxide-propylene oxide copolymers, maleic anhydride-diisobutylene copolymers, polyacrylic and polymethacrylic acid and their salts, methylcelluloses, carboxymethylcelluloses, hydroxymethylcelluloses, polyurethanes, alkali metal phosphates and salts of modified phosphoric acids, as well as mixtures thereof.

[0048] Examples of defoamers include polyglycols, triglycerides, polysiloxane polyether copolymers, and silicone oils.

[0049] Examples of hydrophobic agents include oligomeric and polymeric siloxanes and silicone resins.

[0050] Examples of preservatives include isothiazolines.

[0051] The invention further provides a method for producing the aqueous coating agent according to the invention, which comprises the following steps: a. Providing a composition containing, based on the total weight of the composition, i. 5 to 30 wt.% polymer with a mean particle size of 60 to 300 nm, ii. 2 to 30 wt.% organic filler, iii. 0.5 to 8 wt.% matting agent with a mean particle size of 0.5 to 9 µm, iv. 30 to 70 wt.% water, b. Dispersing the components mentioned in a.

[0052] The steps listed can be carried out in any order, but preferably they are carried out in the order given.

[0053] Devices known to those skilled in the art can be used to disperse the components. For example, turbomills or dissolvers, preferably dissolvers, can be used for this purpose.

[0054] What has been said in connection with the aqueous coating agent according to the invention regarding the polymer also applies equally to the polymer of the process according to the invention.

[0055] What has been said in connection with the aqueous coating agent according to the invention regarding the organic filler also applies equally to the organic filler of the process according to the invention.

[0056] What has been said in connection with the aqueous coating agent according to the invention as a matting agent also applies equally to the matting agent of the method according to the invention.

[0057] In particular, the composition of the process according to the invention can contain 8 to 17 wt.%, preferably 10 to 15 wt.%, more preferably 11 to 13 wt.%, polymer and / or 5 to 25 wt.%, preferably 10 to 20 wt.%, more preferably 13 to 18 wt.%, organic filler and / or 1 to 6 wt.%, preferably 2 to 4 wt.%, matting agent and / or additionally at least one inorganic filler and / or pigment, preferably 1 to 20 wt.%, more preferably 3 to 17 wt.%, even more preferably 5 to 15 wt.%, particularly preferably 8 to 12 wt.%, at least one inorganic filler and / or pigment, in each case based on the total weight of the composition.

[0058] The foregoing applies to the at least one inorganic filler and / or pigment of the composition of the process according to the invention.

[0059] Furthermore, the composition of the process according to the invention can also contain 0.1 to 30 wt.%, preferably 0.5 to 20 wt.%, more preferably 1 to 10 wt.%, particularly preferably 1.5 to 5 wt.%, in each case based on the total weight of the aqueous coating material, additives and / or additives such as, for example, defoamers, dispersants, wetting agents, preservatives, stabilizers, surface protectants, hydrophobizing agents, solvents and thickeners.

[0060] The invention further relates to an aqueous coating agent obtainable by the inventive method.

[0061] The aqueous coating agent is suitable for various uses. In particular, it is suitable as a dispersion paint. Accordingly, the use of the aqueous coating agent according to the invention as a dispersion paint for interior and / or exterior use is also part of the invention.

[0062] The invention is explained in more detail below by means of examples, which, however, serve only for illustration and are not limiting. EXAMPLE

[0063] An aqueous coating agent with the following formulation, as shown in Table 1, was produced by mixing the components listed in Table 1, with dosages given in wt.%. Table 1: Formulation of the aqueous coating agent ingredient Recipe Styrene acrylate, 120 nm mean particle size, as a 50% aqueous dispersion 25 Cross-linked polyurethane particles, 30 µm average particle size 15 Defoamer 0,34 Dispersing agent 0,23 preservatives 0,16 Thickener 1,9 Matting agent, 4 µm average particle size 3 Filler, average particle size less than 30 µm 5,5 Pigment, average particle size less than 30 µm 4,13 Water 44,74

[0064] A composition with the formulation specified in Table 1 was dispersed using a dissolver. The resulting aqueous coating was used as a dispersion paint for interior applications on plaster and wallpaper. The aqueous coating and the resulting coating exhibited good adhesion to both plaster and wallpaper. Furthermore, it could be applied easily and, in particular, evenly with a brush and / or paint roller. After drying, the coating showed a gloss level, specifically a reflectometer value, of less than 5 at a measuring angle of 85°, according to DIN EN 13300, specifically DIN EN 13300:2002-11, measured according to DIN EN ISO 2813, specifically DIN EN ISO 2813:2015-02. In addition, the coating had a pleasant feel to the touch. Furthermore, it was highly resistant to mechanical stress.

[0065] The invention further relates to the embodiments of the invention described in the following sentences: 1. Aqueous coating material containing, based on the total weight of the coating material, a. 5 to 30 wt.% polymer with a mean particle size of 60 to 300 nm, b. 2 to 30 wt.% organic filler, c. 0.5 to 8 wt.% matting agent with a mean particle size of 0.5 to 9 µm, d. 30 to 70 wt.% water. 2. Aqueous coating material according to sentence 1, characterized by the fact that The coating material contains 8 to 17 wt.%, in particular 10 to 15 wt.% or 11 to 13 wt.%, polymer, in each case based on the total weight of the coating material. 3. Aqueous coating material according to one of sentences 1 or 2, characterized by the fact thatThe polymer is selected from the group consisting of polymers based on carboxylic acid vinyl esters, in particular vinyl acetate, vinyl propionate, N-vinylpyrrolidone and derivatives thereof, unsaturated carboxylic acids, their esters, amides and anhydrides, in particular acrylic acid and methacrylic acid as well as their esters and amides, and ethylene-unsaturated compounds such as acrylonitrile, vinyl chloride, styrene, and copolymers of the aforementioned monomers, polyurethanes, polyester polyurethanes and mixtures thereof. 4. Aqueous coating agent according to any of the preceding sentences, characterized by the fact thatthe polymer is in the form of an aqueous dispersion with a solids content of 40 to 70 wt.%, in particular 45 to 60 wt.% or 45 to 55 wt.% or 50 wt.%, in particular with a Brookfield viscosity at 25°C of 1000 to 10000 mPas, in particular of 1500 to 8000 mPas, and / or a pH value of 7 to 11.4, in particular of 8 to 9, and / or a glass transition temperature Tg, measured according to DIN EN ISO 16805:2005-07, of -20 to 20°C, in particular of -10 to 10°C or of -5 to 5°C or of 0 to 5°C, and / or is a styrene acrylate copolymer. 5. Aqueous coating material according to one of the preceding sentences, characterized by the fact that The polymer has a mean particle size of 70 to 200 nm, in particular 80 to 170 nm or 100 to 150 nm or 120 nm. 6. Aqueous coating material according to one of the preceding sentences, characterized by the fact thatThe aqueous coating material contains 5 to 25 wt.%, in particular 10 to 20 wt.% or 13 to 18 wt.%, organic filler, in each case based on the total weight of the coating material. 7. Aqueous coating material according to one of the preceding sentences, characterized by the fact that The organic filler is selected from the group consisting of polyurethane particles, polymethyl methacrylate particles, polymeric microspheres, cellulose fibers, textile fibers, cork flour, and mixtures thereof. 8. Aqueous coating agent according to any of the preceding sentences, characterized by the fact that The organic filler has a mean particle size of 1 to 50 µm, in particular 5 to 40 µm, or 20 to 40 µm, or 25 to 35 µm, or 28 to 33 µm, or 30 µm. 9. Aqueous coating material according to one of the preceding sentences, characterized by the fact thatThe coating material contains 1 to 6 wt.%, in particular 2 to 4 wt.% matting agent, in each case based on the total weight of the coating material. 10. Aqueous coating material according to one of the preceding sentences, characterized by the fact that The matting agent is selected from the group consisting of pyrogenic silica, polymethyl urea, ceramic microspheres, diatomaceous earth, quartz flour, talc, and wax additives such as polyethylene waxes. 11. Aqueous coating agent according to any of the preceding sentences, characterized by the fact that The matting agent has a mean particle size of 1 to 8 µm, in particular 2 to 6 µm or 4 µm. 12. Aqueous coating agent according to one of the preceding sentences, characterized by the fact that The coating material additionally contains at least one inorganic filler and / or pigment. 13. Aqueous coating material according to sentence 12, characterized by the fact thatThe coating material contains 1 to 20 wt.%, in particular 3 to 17 wt.% or 5 to 15 wt.% or 8 to 12 wt.%, at least one inorganic filler and / or pigment, in each case based on the total weight of the coating material. 14. Aqueous coating material according to one of sentences 12 or 13, characterized by the fact that which contains at least one inorganic filler selected from the group consisting of diatomaceous earth, dolomite, barium sulfate, feldspar, quartz, calcium carbonate, mica, kaolin, calcined kaolin, talc, aluminum silicates and mixtures thereof. 15. Aqueous coating material according to any of the preceding sentences, characterized by the fact thatThe coating composition additionally contains one or more further additives and / or admixtures selected from the group consisting of defoamers, dispersants, wetting agents, preservatives, stabilizers, surface protectants, water repellents, solvents, and thickeners. 16. A process for producing an aqueous coating composition according to any one of sentences 1 to 15, comprising the steps: a. Providing a composition containing, in each case based on the total weight of the composition, i. 5 to 30 wt.% polymer with a mean particle size of 60 to 300 nm, ii. 2 to 30 wt.% organic filler, iii. 0.5 to 8 wt.% matting agent with a mean particle size of 0.5 to 9 µm, iv. 30 to 70 wt.% water; b. Dispersing the components mentioned in a. 17. A process according to sentence 16. characterized by the fact thatthe composition contains 8 to 17 wt.%, in particular 10 to 15 wt.% or 11 to 13 wt.%, polymer and / or 5 to 25 wt.%, in particular 10 to 20 wt.% or 13 to 18 wt.%, organic filler and / or 1 to 6 wt.%, in particular 2 to 4 wt.%, matting agent and / or additionally at least one inorganic filler and / or pigment, in particular 1 to 20 wt.%, in particular 3 to 17 wt.% or 5 to 15 wt.% or 8 to 12 wt.%, at least one inorganic filler and / or pigment, in each case based on the total weight of the composition. 18. Method according to one of sentences 16 or 17, characterized by the fact thatThe polymer according to one of claims 3, 4, or 5, and / or the organic filler according to one of claims 7 or 8, and / or the matting agent according to one of claims 10 or 11, and / or the inorganic filler according to claim 14, is defined, and / or the composition contains one or more additives selected from the group consisting of defoamers, dispersants, wetting agents, preservatives, stabilizers, surface protectants, water repellents, solvents, and thickeners. 19. Aqueous coating material obtainable by a method according to one of sentences 16 to 18. 20. Use of an aqueous coating material according to one of sentences 1 to 15 or 19 as a dispersion paint for interior and / or exterior use.

Claims

1. Aqueous coating compound containing, based on the total weight of the coating compound, a. 5 to 30 wt.% polymer with a mean particle size of 60 to 300 nm, b. 2 to 30 wt.% organic filler, c. 0.5 to 8 wt.% matting agent with a mean particle size of 0.5 to 9 µm, d. 30 to 70 wt.% water.

2. Aqueous coating agent according to claim 1, characterized by the fact that The coating material contains 8 to 17 wt.%, in particular 10 to 15 wt.% or 11 to 13 wt.%, polymer, in each case based on the total weight of the coating material.

3. Aqueous coating material according to one of claims 1 or 2, characterized by the fact thatthe polymer is selected from the group consisting of polymers based on carboxylic acid vinyl esters, in particular vinyl acetate, vinyl propionate, N-vinylpyrrolidone and derivatives thereof, unsaturated carboxylic acids, their esters, amides and anhydrides, in particular acrylic acid and methacrylic acid as well as their esters and amides, and ethylene-unsaturated compounds such as acrylonitrile, vinyl chloride, styrene, and copolymers of the aforementioned monomers, polyurethanes, polyester polyurethanes and mixtures thereof.

4. Aqueous coating material according to any one of the preceding claims, characterized by the fact that the polymer is in the form of an aqueous dispersion with a solids content of 40 to 70 wt.%, in particular 45 to 60 wt.% or 45 to 55 wt.% or 50 wt.%, in particular with a Brookfield viscosity at 25°C of 1000 to 10000 mPas, in particular of 1500 to 8000 mPas, and / or a pH value of 7 to 11.4, in particular of 8 to 9, and / or a glass transition temperature Tg , measured according to DIN EN ISO 16805:2005-07, from -20 to 20°C, in particular from -10 to 10°C or from -5 to 5°C or from 0 to 5°C, and / or is a styrene acrylate copolymer.

5. Aqueous coating material according to any one of the preceding claims, characterized by the fact that the polymer has a mean particle size of 70 to 200 nm, in particular 80 to 170 nm or 100 to 150 nm or 120 nm, and / or that the aqueous coating material contains 5 to 25 wt.%, in particular 10 to 20 wt.% or 13 to 18 wt.%, organic filler, in each case based on the total weight of the coating material.

6. Aqueous coating material according to any one of the preceding claims, characterized by the fact that The organic filler is selected from the group consisting of polyurethane particles, polymethyl methacrylate particles, polymeric micro-hollow spheres, cellulose fibers, textile fibers, cork flour and mixtures thereof.

7. Aqueous coating material according to any one of the preceding claims, characterized by the fact that The organic filler has a mean particle size of 1 to 50 µm, in particular 5 to 40 µm or 20 to 40 µm or 25 to 35 µm or 28 to 33 µm or 30 µm.

8. Aqueous coating material according to any one of the preceding claims, characterized by the fact that the coating material contains 1 to 6 wt.%, in particular 2 to 4 wt.% matting agent, in each case based on the total weight of the coating material and / or that the matting agent is selected from the group consisting of pyrogenic silica, polymethyl urea, ceramic microspheres, diatomaceous earth, quartz flours, talc and wax additives such as polyethylene waxes and / or that the matting agent has a mean particle size of 1 to 8 µm, in particular of 2 to 6 µm or of 4 µm.

9. Aqueous coating material according to any one of the preceding claims, characterized by the fact thatthe coating material additionally contains at least one inorganic filler and / or pigment and / or that the coating material contains 1 to 20 wt.%, in particular 3 to 17 wt.% or 5 to 15 wt.% or 8 to 12 wt.%, at least one inorganic filler and / or pigment, in each case based on the total weight of the coating material and / or that the at least one inorganic filler is selected from the group consisting of diatomaceous earth, dolomite, barium sulfate, feldspar, quartz, calcium carbonate, mica, kaolin, calcined kaolin, talc, aluminum silicates and mixtures thereof.

10. Aqueous coating composition according to any one of the preceding claims, characterized by the fact that The coating compound additionally contains one or more further additives and / or additives selected from the group consisting of defoamers, dispersants, wetting agents, preservatives, stabilizers, surface protectants, hydrophobic agents, solvents and thickeners.

11. A method for producing an aqueous coating composition according to any one of claims 1 to 10, comprising the steps of: a. Providing a composition containing, based on the total weight of the composition, i. 5 to 30 wt.% polymer with a mean particle size of 60 to 300 nm, ii. 2 to 30 wt.% organic filler, iii. 0.5 to 8 wt.% matting agent with a mean particle size of 0.5 to 9 µm, iv. 30 to 70 wt.% water, b. Dispersing the components mentioned in a.

12. Method according to claim 11, characterized by the fact thatThe composition contains 8 to 17 wt.%, in particular 10 to 15 wt.% or 11 to 13 wt.%, polymer and / or 5 to 25 wt.%, in particular 10 to 20 wt.% or 13 to 18 wt.%, organic filler and / or 1 to 6 wt.%, in particular 2 to 4 wt.%, matting agent and / or additionally at least one inorganic filler and / or pigment, in particular 1 to 20 wt.%, in particular 3 to 17 wt.% or 5 to 15 wt.% or 8 to 12 wt.%, at least one inorganic filler and / or pigment, in each case based on the total weight of the composition.

13. Method according to one of claims 11 or 12, characterized by the fact thatthe polymer according to one of claims 3, 4 or 5 and / or the organic filler according to one of claims 7 or 8 and / or the matting agent according to one of claims 10 or 11 and / or the inorganic filler according to claim 14 is defined and / or the composition contains one or more additives selected from the group consisting of defoamers, dispersants, wetting agents, preservatives, stabilizers, surface protectants, hydrophobizing agents, solvents and thickeners.

14. Aqueous coating material obtainable by a method according to any one of claims 11 to 13.

15. Use of an aqueous coating agent according to one of claims 1 to 10 or 14 as a dispersion paint for interior and / or exterior use.