High melt strength polypropylene with improved processability
Patent Information
- Application Number
- JP2019542421
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2017-03-13
- Filing Date
- 2018-01-03
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2038-01-03
AI Technical Summary
The applicability of polypropylene in industrial extrusion processes is limited due to its low melt strength and lack of work hardening, leading to high shear viscosities that complicate processing, particularly in applications like foam molding and thermoforming.
A process involving the combination of branched polypropylene with a low molecular weight polyolefin to create a polypropylene composition with enhanced melt strength and reduced shear viscosity, maintaining work hardening through specific molecular weight ratios and the use of organic peroxides to achieve branched polypropylene.
The resulting polypropylene composition exhibits improved processability with high melt strength and work hardening, suitable for applications involving both shear and extensional flow, such as thermoforming and foam molding, while maintaining a broad processing window.
Abstract
Description
Technical Field
[0001] (Claim of Priority) This application claims the benefit of Provisional Application No. 62 / 455,707, filed Feb. 7, 2017, and European Application No. 17160477.0, filed Mar. 13, 2017, the disclosures of which are incorporated herein by reference. This disclosure relates to improved processing of branched polypropylene, and more particularly, to mixing of branched polypropylene and low molecular weight polyolefins.
Background Art
[0002] The applicability of polypropylene in industrial extrusion processes involving both shear flow and extensional flow has been limited. This is due in part to its low melt strength and lack of work hardening. Multiple efforts have been attempted in the industry to improve the melt strength and work hardening of polypropylene, including increasing molecular weight, broadening the molecular weight distribution (Mw / Mn), adding ultra-high molecular weight tails, and / or adding long chain branches (LCB). Polypropylenes with improved melt strength and work hardening have been made, but these polypropylenes tend to have very high shear viscosities, making them difficult to process. It would be beneficial to discover polypropylenes that have high melt strength and work hardening but have a wide process operating window for applications such as foam molding and thermoforming. One way to achieve this is to lower the process temperature and reduce the viscosity by adding low molecular weight additives. However, the challenge with this approach is that at higher concentrations of low molecular weight additives, work hardening decreases. A better approach is needed. Related publications include U.S. Patent Application Publication No. 2015 / 0018463; U.S. Patent Application Publication No. 2010 / 222470; U.S. Patent Application Publication No. 2003 / 0119996; U.S. Patent No. 4,897,452; U.S. Patent No. 6,103,833; U.S. Patent No. 9,410,034; European Patent No. 1159,309B1; European Patent Application Publication No. 2325248; European Patent Application Publication No. 2386601; European Patent Application Publication No. 2433982; International Publication No. 2010 / 049371; International Publication No. 2014 / 070384; International Publication No. 2015 / 200586; International Publication No. 2016 / 053468; and Japanese Patent Publication No. 2010-043162; and ME Shivokhin, This includes L. Urbanczyk, J. Michel, and C. Bailly, in "The influence of molecular weight distribution of industrial polystyrene on its melt extensional and ultimate properties", 56(9) POLYMER ENGINEERING & SCIENCE, 1012-1020 (September 2016). [Overview of the Initiative]
[0003] A process for producing a polypropylene composition is described herein, comprising (or consisting of or essentially consisting of) the step of combining branched polypropylene with a low molecular weight polyolefin having a melt flow rate of at least 50 g / 10 min (ASTM D1238, 230°C / 2.16 kg) to obtain a polypropylene composition. A polypropylene composition comprising (or consisting of, or essentially consisting of) these steps, wherein the polypropylene composition has a melt flow rate in the range of 0.5 to 40 g / 10 min, a melt strength in the range of 20 to 80 cN (at 190°C), and is obtained by combining linear polypropylene having a melt strength in the range of 10 to 40 cN (at 190°C) with an organic peroxide, wherein the melt strength of the branched polypropylene exceeds the melt strength of the linear polypropylene; and a polypropylene homopolymer having a melt flow rate in the range of 0.1 to 20 g / 10 min and an Mw / Mn of at least 5, in the range of 5 to 40% by mass relative to the mass of the branched polypropylene and the polypropylene homopolymer.
[0004] Polypropylene compositions comprising (or essentially comprising) branched polypropylene and low molecular weight polyolefins having a melt flow rate of at least 50 g / 10 min are also described. In particular, foamed molded articles, thermoformed articles, and / or extruded articles comprising (or essentially comprising) a polypropylene composition comprising (or essentially comprising) a polypropylene composition comprising (or essentially comprising) a branched polypropylene having a melt strength (190°C) in the range of 20 to 80 cN and a melt flow rate (190°C) in the range of 0.1 to 20 g / 10 min, in the range of 95 to 60% by mass relative to the mass of branched polypropylene and polypropylene homopolymers; and a polypropylene homopolymer having a melt flow rate (190°C) in the range of 5 to 40% by mass relative to the mass of branched polypropylene and polypropylene homopolymers, in the range of at least 50 g / 10 min, wherein the polypropylene composition has a melt flow rate (190°C) in the range of 0.5 to 40 g / 10 min and a melt strength (190°C) in the range of 20 to 80 cN and exhibits at least 90% of the work hardening shown by branched polypropylene. [Brief explanation of the drawing]
[0005] [Figure 1] 1 -1 These are extensional rheological traces of a comparative mixture and two of the present invention's mixtures, showing viscosity as a function of time at a rate of seconds. [Figure 2] 5 -1 These are extensional rheological traces of a comparative mixture and two of the present invention's mixtures, showing viscosity as a function of time at a rate of seconds. [Figure 3] 10 -1 These are extensional rheological traces of a comparative mixture and two of the present invention's mixtures, showing viscosity as a function of time at a rate of seconds. [Figure 4] These are traces of SAOS for a comparative mixture and two of the present invention's mixtures, showing angular frequency as a function of shear viscosity. [Modes for carrying out the invention]
[0006] It has been found that by a wise selection of the molecular weight and concentration of the low molecular weight polyolefins used herein, which are low molecular weight additives, it is possible to simultaneously maintain a high melt strength and a reduced shear viscosity of work-hardened polypropylene while simultaneously maintaining a level of work hardening (extensional thickening). This behavior is unique and had not been previously demonstrated in polypropylene. Work hardening is important for industrial applications involving extensional flow, such as thermoforming, fiber drawing / spinning, inflated films, and foam molding, as well as other industrial applications involving both shear and extensional flow deformation. The present invention is described in more detail below and is ordered based on the description of the starting materials and processes that yield the desired end polypropylene compositions. (Linear polypropylene) Throughout this specification, the term “linear polypropylene” refers to reactor-grade polypropylene homopolymers or copolymers useful for forming “branched polypropylene” having a branching index g’(vis) greater than 0.98. The most preferred linear polypropylene in any embodiment of the present invention has the properties described herein and can also be produced by any means known to those skilled in the art, but most preferably it is produced using the Ziegler-Natta succinate-containing catalyst. The properties referred to herein are those of the reactor-grade material before or after melt mixing with non-peroxide “additives,” such as antioxidants, alkyl radical scavengers, etc. In any embodiment, the desired linear polypropylene is a homopolymer of propylene-derived units, or ethylene or C4-C in amounts ranging from 0.20, 0.40, or 0.80% by mass to 1.0, 2.0, 4.0, or 6.0% by mass relative to the mass of the linear polypropylene. 12 The copolymer comprises α-olefin-derived units, most preferably ethylene, 1-butene, or 1-hexene-derived units, with the remainder being propylene-derived units.
[0007] Ziegler-Natta catalysts suitable for producing useful linear polypropylene include the solid titanium-supported catalyst systems described in U.S. Patent No. 4,990,479, U.S. Patent No. 5,159,021, International Publication No. 00 / 63261, and the like. Briefly, the Ziegler-Natta catalyst can be obtained by: (1) suspending a dialkoxymagnesium compound in an aromatic hydrocarbon that is liquid at 20-25 °C; (2) contacting the dialkoxymagnesium hydrocarbon composition with a titanium halide and a diester of an aromatic dicarboxylic acid; and (3) contacting the resulting functional dialkoxymagnesium hydrocarbon composition from step (2) with additional titanium halide. The "catalyst system" typically includes a solid titanium catalyst component containing titanium, as well as magnesium, halogen, at least one non-aromatic "internal" electron donor, and at least one, preferably two or more "external" electron donors. The solid titanium catalyst component, also referred to as a Ziegler-Natta catalyst, can be prepared by contacting a magnesium compound, a titanium compound, and at least an internal electron donor. Examples of titanium compounds used in the preparation of the solid titanium catalyst component include those of formula (I): Ti(OR n )X 4-n (I) including tetravalent titanium compounds having, wherein R is a hydrocarbyl radical, X is a halogen atom, and n is from 0 to 4.
[0008] The terms "hydrocarbyl radical", "hydrocarbyl", and "hydrocarbyl group" are used interchangeably throughout this specification unless otherwise specified. For the purposes of this disclosure, a hydrocarbyl radical can be, where appropriate, linear, branched, or cyclic (aromatic or non-aromatic), a C1-C 20 radical, or a C1-C 10 radical, or a C6-C 20 radical, or a C7-C 20It is defined as a radical and includes hydrocarbyl radicals that are substituted with one or more functional groups containing other hydrocarbyl radicals and / or elements from groups 13–17 of the periodic table. In addition, two or more such hydrocarbyl radicals may together form a condensed ring system, which may include a partially or completely hydrogenated condensed ring system and may include a heterocyclic radical.
[0009] Preferably, the halogen-containing titanium compound is titanium tetrahalide or titanium tetrachloride. The titanium compounds may be used alone or in combination with each other. The titanium compounds may be diluted with hydrocarbon compounds or halogenated hydrocarbon compounds. Non-limiting examples include titanium tetrahalides such as TiCl4, TiBr4, and / or TiI4; trihaloxytitanium trihalides including Ti(OCH3)Cl3, Ti(OC2H5)Cl3, Ti(On-C4H9)Cl3, Ti(OC2H5)Br3, and / or Ti(O-iso-C4H9)Br3; dialkoxytitanium dihalides including Ti(OCH3)2Cl2, Ti(OC2H5)2Cl2, Ti(On-C4H9)2Cl2, and / or Ti(OC2H5)2Br2; monohaloxytitanium monohalides including Ti(OCH3)3Cl, Ti(OC2H5)3Cl, Ti(On-C4H9)3Cl, and / or Ti(OC2H5)3Br; and tetraalkoxytitaniums including Ti(OCH3)4, Ti(OC2H5)4, and / or Ti(On-C4H9)4. Preferably, the magnesium compounds used in the preparation of the solid titanium catalyst component include reducible magnesium compounds and / or non-reducible magnesium compounds. Suitable reducible magnesium compounds may be, for example, magnesium compounds having magnesium-carbon bonds or magnesium-hydrogen bonds. Suitable examples of such reducible magnesium compounds include dimethylmagnesium, diethylmagnesium, dipropylmagnesium, dibutylmagnesium, diamylmagnesium, dihexylmagnesium, didecylmagnesium, ethylmagnesium chloride, propylmagnesium chloride, butylmagnesium chloride, hexylmagnesium chloride, amylmagnesium chloride, butylethoxymagnesium, ethylbutylmagnesium, and / or butylmagnesium halides. These magnesium compounds may be used alone or may form complexes with organoaluminum cocatalysts as described herein. These magnesium compounds may be liquid or solid.
[0010] Suitable examples of non-reducible magnesium compounds include magnesium halides such as magnesium chloride, magnesium bromide, magnesium iodide, and magnesium fluoride; alkoxymagnesium halides such as magnesium methoxychloride, magnesium ethoxychloride, magnesium isopropoxychloride, magnesium phenoxychloride, and magnesium methylphenoxychloride; alkoxymagnesiums such as magnesium ethoxychloride, magnesium isopropoxychloride, magnesium butoxychloride, n-octaoxymagnesium, and 2-ethylhexaoxymagnesium; aryloxymagnesiums such as magnesium phenoxymagnesium and magnesium dimethylphenoxymagnesium; and / or magnesium carboxylates such as magnesium laurate and magnesium stearate. The non-reducible magnesium compound may be a compound derived from a reducible magnesium compound, or a compound derived at the time of preparing the catalyst component. The non-reducible magnesium compound may be derived from a reducible compound, for example, by contacting the reducible magnesium compound with a polysiloxane compound, a halogen-containing silane compound, a halogen-containing aluminum compound, an ester, an alcohol, etc.
[0011] Reducible magnesium compounds and / or non-reducible magnesium compounds may be complexes of the above magnesium compounds with other metals, or mixtures of such compounds with other metal compounds. They may also be mixtures of two or more types of the above compounds. Furthermore, halogen-containing magnesium compounds, including magnesium chloride, magnesium alkoxychloride, and magnesium aryloxychloride, may be used. The supported Ziegler-Natta catalyst may be used in combination with a co-catalyst, and is referred to herein as a Ziegler-Natta co-catalyst. A compound containing at least one aluminum-carbon bond in its molecule may be used as a co-catalyst, and is referred to herein as an organoaluminum co-catalyst. A suitable organoaluminum compound is given by general formula (II): R 1 m Al(OR 2 ) n H p X q (II) It contains an organoaluminum compound, in which R 1 and R 2 However, they are either the same or different, and each represents a hydrocarbyl radical containing 1 to 15 carbon atoms, or 1 to 4 carbon atoms; X represents a halogen atom; m is 1, 2, or 3; n is 0, 1, or 2; p is 0, 1, 2, or 3; and q is 0, 1, or 2; and where m + n + p + q = 3.
[0012] Other suitable organoaluminum compounds include general formula (III): M 1 AlR 1 4(III) This includes complex alkylated compounds of Group I metals (periodic table, lithium, etc.) and aluminum, represented by the formula, where M 1 These are Group I metals such as Li, Na, or K, and R 1 This is as defined in equation (II). Suitable examples of organoaluminum compounds include trialkylaluminum such as trimethylaluminum, triethylaluminum, and tributylaluminum; trialkenylaluminum such as triisophenylaluminum; dialkylaluminum alkoxides such as diethylaluminum ethoxide and dibutylaluminum ethoxide; alkylaluminum sesquialkoxides such as ethylaluminum sesquiethoxide and butylaluminum sesquibutoxide; and compounds with the general formula R 1 2.5 Al(OR 2 ) 0.5 This includes partially alkoxylated alkylaluminum having an average composition represented by; partially halogenated alkylaluminum dihalides, such as ethylaluminum dichloride, propylaluminum dichloride, and butylaluminum dibromide; partially hydrogenated alkylaluminum dihydrogenates, such as ethylaluminum dihydrogenate and propylaluminum dihydrogenate; and partially alkoxylated and halogenated alkylaluminum, such as ethylaluminum ethoxycyclolide, butylaluminum butoxycyclolide, and ethylaluminum ethoxybromide.
[0013] Electron donors are present with the metal components in forming catalysts suitable for producing the linear polypropylene described herein. Both “internal” and “external” electron donors are desirable for forming catalysts suitable for producing the linear polypropylene described herein. More specifically, internal electron donors may be used in catalyst formation reactions such as those in which a transition metal halide is reacted with a metal hydride or metal alkyl. Examples of suitable internal electron donors include amines, amides, ethers, esters, ketones, nitriles, phosphines, stilbenes, arsines, phosphoramides, thioethers, thioesters, aldehydes, alkoxides, and salts of organic acids.
[0014] More preferably, one or more internal donors are non-aromatic. Non-aromatic internal electron donors may include aliphatic amines, amides, esters, ethers, ketones, nitriles, phosphines, phosphoramides, thioethers, thioesters, aldehydes, alkoxides, carboxylic acids, or combinations thereof. More preferably, the non-aromatic internal electron donor is a substituted or unsubstituted C2-C 10 C1-C dicarboxylic acid 20 Diesters are included. The non-aromatic internal electron donor is given by formula (IV): [Formula 1] (IV) It may be one or more succinate compounds, where R 1 and R 2 However, independently, C1-C 20 It is a linear or branched alkyl, alkenyl, or cycloalkylhydrocarbyl radical; and R 3 ~R 6 However, independently, hydrogen, halogen, or C1-C 20 A linear or branched alkyl, alkenyl, or cycloalkylhydrocarbyl radical, where R 3 ~R 6 The radicals are not bonded together, and here, R 3 ~R 6At least two of the radicals are bonded together to form a cyclic divalent radical, or a combination thereof.
[0015] R in equation (IV) 3 ~R 5 The group may be hydrogen, R 6 This may be a radical selected from the group consisting of primary branched, secondary, or tertiary alkyl groups, or cycloalkyl radicals having 3 to 20 carbon atoms.
[0016] The internal donor may be a monosubstituted non-aromatic succinate compound. Suitable examples include diethyl-sec-butyl succinate, diethylhexyl succinate, diethyl-cyclopropyl succinate, diethyl-trimethylsilyl succinate, diethyl-methoxy succinate, diethyl-cyclohexyl succinate, diethyl-(cyclohexylmethyl) succinate, diethyl-t-butyl succinate, diethyl-isobutyl succinate, diethyl-isopropyl succinate, and diethyl-(cyclohexylmethyl) succinate. Diethyl-neopentyl succinate, diethyl-isopentyl succinate, diethyl-(1,1,1-trifluoro-2-propyl) succinate, diisobutyl-sec-butyl succinate, diisobutylhexyl succinate, diisobutyl-cyclopropyl succinate, diisobutyl-trimethylsilyl succinate, diisobutyl-methoxysuccinate, diisobutyl-cyclohexyl succinate, diisobutyl-(cyclohexylmethyl) succinate, Diisobutyl-t-butyl succinate, diisobutyl-isobutyl succinate, diisobutyl-isopropyl succinate, diisobutyl-neopentyl succinate, diisobutyl-isopentyl succinate, diisobutyl-(1,1,1-trifluoro-2-propyl) succinate, dineopentyl-sec-butyl succinate, dineopentylhexyl succinate, dineopentylcyclopropyl succinate, dineopentyltrimethylsilyl succinate This includes dineopentyl methoxysuccinate, dineopentyl cyclohexyl succinate, dineopentyl (cyclohexylmethyl) succinate, dineopentyl t-butyl succinate, dineopentyl isobutyl succinate, dineopentyl isopropyl succinate, dineopentyl neopentyl succinate, dineopentyl isopentyl succinate, and / or dineopentyl (1,1,1-trifluoro-2-propyl) succinate.
[0017] An internal electron donor having a structure consistent with equation (IV) is R 3 From R 6It may contain at least two radicals up to C1-C, and these radicals are different from hydrogen and C1-C 20 The group is selected from linear or branched alkyl, alkenyl, and / or cycloalkylhydrocarbyl groups, and may contain heteroatoms. Two radicals other than hydrogen may be linked to the same carbon atom. Appropriate examples include diethyl-2,2-dimethyl succinate, diethyl-2-ethyl-2-methyl succinate, diethyl-2-(cyclohexylmethyl)-2-isobutyl succinate, diethyl-2-cyclopentyl-2-n-propyl succinate, diethyl-2,2-diisobutyl succinate, diethyl-2-cyclohexyl-2-ethyl succinate, diethyl-2-isopropyl-2-methyl succinate, diethyl-2,2-diisopropyl-diethyl-2-isobutyl-2-ethyl succinate, diethyl-2-(1,1,1-trifluoro-2-propyl)-2-methyl succinate, diethyl-2-isopentyl-2-isobutyl succinate, diisobutyl-2,2-dimethyl succinate,
[0018] Diisobutyl-2-ethyl-2-methyl succinate, diisobutyl-2-(cyclohexylmethyl)-2-isobutyl succinate, diisobutyl-2-cyclopentyl-2-n-propyl succinate, diisobutyl-2,2-diisobutyl succinate, diisobutyl-2-cyclohexyl-2-ethyl succinate, diisobutyl-2-isopropyl-2-methyl succinate, diisobutyl-2-isobutyl-2-ethyl succinate, diisobutyl-2-(1,1,1-trifluoro-2-propyl)-2-methyl succinate, diisobutyl-2-isopentyl-2-isobutyl succinate, diisobutyl-2,2-diisopropyl succinate, dineopentyl-2,2-dimethyl succinate, dineopentyl The collection includes 2,2-disubstituted succinates, including -2-ethyl-2-methyl succinate, dineopentyl-2-(cyclohexylmethyl)-2-isobutyl succinate, dineopentyl-2-cyclopentyl-2-n-propyl succinate, dineopentyl-2,2-diisobutyl succinate, dineopentyl-2-cyclohexyl-2-ethyl succinate, dineopentyl-2-isopropyl-2-methyl succinate, dineopentyl-2-isobutyl-2-ethyl succinate, dineopentyl-2-(1,1,1-trifluoro-2-propyl)-2-methyl succinate, dineopentyl 2,2-diisopropyl succinate, and / or dineopentyl 2-isopentyl-2-isobutyl succinate.
[0019] At least two radicals other than hydrogen are R in equation (IV). 3 From R 6 It may be linked to different carbon atoms up to R. For example, R 3 and R 5 , or R 4 and R 6These include: Diethyl-2,3-bis(trimethylsilyl)succinate, Diethyl-2,2-sec-butyl-3-methylsuccinate, Diethyl-2-(3,3,3-trifluoropropyl)-3-methylsuccinate, Diethyl-2,3-bis(2-ethylbutyl)succinate, Diethyl-2,3-diethyl-2-isopropylsuccinate, Diethyl-2,3-diisopropyl-2-methylsuccinate, Diethyl-2,3-dicyclohexyl-2-methylsuccinate Diethyl-2,3-diisopropyl succinate, diethyl-2,3-bis(cyclohexylmethyl) succinate, diethyl-2,3-di-t-butyl succinate, diethyl-2,3-diisobutyl succinate, diethyl-2,3-dineopentyl succinate, diethyl-2,3-diisopentyl succinate, diethyl-2,3-(1-trifluoromethyl-ethyl) succinate, diethyl-2-isopropyl-3-isobutyl succinate, diethyl-2-t-butyl-3-isopropyl succinate,
[0020] Diethyl-2-isopropyl-3-cyclohexyl succinate, diethyl-2-isopentyl-3-cyclohexyl succinate, diethyl-2-cyclohexyl-3-cyclopentyl succinate, diethyl-2,2,3,3-tetramethyl succinate, diethyl-2,2,3,3-tetraethyl succinate, diethyl-2,2,3,3-tetrapropyl succinate, diethyl-2,3-diethyl-2,3-diisopropyl succinate, diisobutyl-2,3-bis(trimethylsilyl) succinate, diisobutyl-2,2-sec-butyl-3-methyl succinate, diisobutyl- 2,3-Bis(2-ethylbutyl) succinate, diisobutyl-2,3-diethyl-2-isopropyl succinate, diisobutyl-2,3-diisopropyl-2-methyl succinate, diisobutyl-2,3-dicyclohexyl-2-methyl succinate, diisobutyl-2,3-diisopropyl succinate, diisobutyl-2,3-bis(cyclohexylmethyl) succinate, diisobutyl-2,3-di-t-butyl succinate, diisobutyl-2,3-diisobutyl succinate, diisobutyl-2,3-dineopentyl succinate, diisobutyl-2,3-diisopentyl succinate, diisobutyl-2,3-(1,1,1-trifluoro-2-propyl) succinate,
[0021] Diisobutyl-2,3-n-propyl succinate, diisobutyl-2-isopropyl-3-isobutyl succinate, diisobutyl-2-terbutyl-3-isopropyl succinate, diisobutyl-2-isopropyl-3-cyclohexyl succinate, diisobutyl-2-isopentyl-3-cyclohexyl succinate, diisobutyl-2-n-propyl-3-(cyclohexylmethyl) succinate, diisobutyl-2- Cyclohexyl-3-cyclopentyl succinate, diisobutyl-2,2,3,3-tetramethyl succinate, diisobutyl-2,2,3,3-tetraethyl succinate, diisobutyl-2,2,3,3-tetrapropyl succinate, diisobutyl-2,3-diethyl-2,3-diisopropyl succinate, dineopentyl-2,3-bis(trimethylsilyl) succinate, dineopentyl-2,2-di-sec-butyl -3-methylsuccinate, Dineopentyl 2-(3,3,3-trifluoropropyl)-3-methylsuccinate, Dineopentyl-2,3-bis(2-ethylbutyl)succinate, Dineopentyl 2,3-diethyl-2-isopropylsuccinate, Dineopentyl-2,3-diisopropyl-2-methylsuccinate, Dineopentyl-2,3-dicyclohexyl-2-methylsuccinate, Dineopentyl-2,3-diiso Propyl succinate, Dineopentyl-2,3-bis(cyclohexylmethyl) succinate, Dineopentyl-2,3-di-t-butyl succinate, Dineopentyl-2,3-diisobutyl succinate, Dineopentyl-2,3-Dineopentyl succinate, Dineopentyl-2,3-diisopentyl succinate, Dineopentyl 2,3-(1,1,1-trifluoro-2propyl) succinate, Dineopentyl-2,This includes 3-n-propyl succinate, dineopentyl-2-isopropyl-3-isobutyl succinate, dineopentyl-2-t-butyl-3-isopropyl succinate, dineopentyl-2-isopropyl-3-cyclohexyl succinate, dineopentyl-2-isopentyl-3-cyclohexyl succinate, dineopentyl-2-n-propyl-3-(cyclohexylmethyl) succinate, dineopentyl-2-cyclohexyl-3-cyclopentyl succinate, dineopentyl-2,2,3,3-tetramethyl succinate, dineopentyl-2,2,3,3-tetraethyl succinate, dineopentyl-2,2,3,3-tetrapropyl succinate, and / or dineopentyl-2,3-diethyl-2,3-diisopropyl succinate.
[0022] The electron donor in formula (IV) is a cyclic polyvalent radical, and consists of two or four R atoms bonded to the same carbon atom. 3 ~R 6 The compounds may contain radicals. Examples of suitable compounds include 1-(ethoxycarbonyl)-1-(ethoxyacetyl)-2,6-dimethylcyclohexane, 1-(ethoxycarbonyl)-1-(ethoxyacetyl)-2,5-dimethylcyclopentane, 1-(ethoxycarbonyl)-1-(ethoxyacetylmethyl)-2-methylcyclohexane, and / or 1-(ethoxycarbonyl)-1-(ethoxy(cyclohexyl)acetyl)cyclohexane.
[0023] Preferably, the internal electron donor may be selected from the group consisting of diethyl-2,3-diisopropyl succinate, diisobutyl-2,3-diisopropyl succinate, di-n-butyl-2,3-diisopropyl succinate, diethyl-2,3-dicyclohexyl-2-methyl succinate, diisobutyl-2,3-dicyclohexyl-2-methyl succinate, diisobutyl-2,2-dimethyl succinate, diethyl-2,2-dimethyl succinate, diethyl-2-ethyl-2-methyl succinate, diisobutyl-2-ethyl-2-methyl succinate, diethyl-2-(cyclohexylmethyl)-3-ethyl-3-methyl succinate, diisobutyl-2-(cyclohexylmethyl)-3-ethyl-3-methyl succinate, and combinations thereof.
[0024] In addition to the internal donor, two or more external electron donors may also be used in combination with the catalyst. The external electron donor has a general formula (V): R 1 n Si(OR 2 ) 4-n (V) It may also contain organosilicon compounds, where R 1 and R 2 However, independently, it represents a hydrocarbyl radical, and n is 1, 2, or 3. Examples of suitable organosilicon compounds include trimethylmethoxysilane, trimethylethoxysilane, dimethyldimethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, diisopropyldiethoxysilane, t-butylmethyl-n-diethoxysilane, t-butylmethyldiethoxysilane, t-amylmethyldiethoxysilane, diphenyldimethoxysilane, phenylmethyldimethoxysilane, diphenyldiethoxysilane, bis-o-tolyldimethoxysilane, bis-m-tolyldimethoxysilane, bis-p-tolyldimethoxysilane, bis-p-tolyldimethoxysilane, bisethylphenyldimethoxysilane, dicyclohexyldiethoxysilane, cyclohexylmethyl-dimethoxysilane, cyclohexylmethyldiethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, vinyl-trimethoxysilane, methyltrimethoxysilane, n-propyl- This includes riethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, phenyltrimethoxysilane, [γ]-chloropropyltrimethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, t-butyltriethoxysilane, n-butyltriethoxysilane, iso-butyltriethoxysilane, phenyltriethoxysilane, γ-aminopropyltriethoxysilane, chlorotriethoxysilane, vinyltributoxysilane, cyclohexyltrimethoxysilane, cyclohexyltriethoxysilane, 2-norbornanetriethoxysilane, 2-norbornanemethyldimethoxysilane, ethyl silicate, butyl silicate, trimethylphenoxysilane, methylallyloxysilane, vinyltris(β-methoxyethoxysilane), vinyltriacetoxysilane, and / or dimethyltetraethoxydisiloxane.
[0025] Suitable examples of organosilicon compounds where n is 0, 1, or 3 include trimethylmethoxysilane, trimethylethoxysilane, methylphenyldimethoxysilane, methyltrimethoxysilane, t-butylmethyldimethoxysilane, t-butylmethyldiethoxysilane, t-amylmethyldimethoxysilane, phenylmethyldimethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexylmethyldiethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, propyltrimethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, phenyltrimethoxysilane, propyltriethoxysilane, butyltriethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, vinyltributoxysilane, cyclohexyltrimethoxysilane, 2-norbornanetrimethoxysilane, and / or 2-norbornanetriethoxysilane.
[0026] Preferably, the external electron donor is selected from one or more of the following: methyltrimethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, vinyltriethoxysilane, propyltrimethoxysilane, decyltrimethoxysilane, decyltriethoxysilane, propyltriethoxysilane, butyltriethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, vinyltributoxysilane, and / or cyclohexyltrimethoxysilane. External electron donors act to control stereoregularity, thereby influencing the ratio of isotactic polymer to atactic polymer produced in a given system. More stereoregular isotactic polymers are more crystalline, resulting in materials with higher flexural modulus. Highly crystalline isotactic polymers also exhibit lower melt flow rates (MFRs) as a result of reduced hydrogen responsiveness during polymerization. The stereoregularity and hydrogen responsiveness of a given external electron donor are typically directly related and inversely proportional.
[0027] The organosilicon compounds disclosed above can be used by adding a compound convertible to such an organosilicon compound at the time of polymerization or prepolymerization of the olefin, so that the organosilicon compound may be formed in situ during the polymerization or prepolymerization of the olefin. In any embodiment, the production of linear polypropylene may involve the use of two external electron donors. The two external electron donors may be selected from any of the external electron donors described herein. However, in certain embodiments, the first external electron donor is of formula R 1 2Si(OR 2 ) has 2, in the formula, each R 1 However, independently, each R is a hydrocarbyl radical containing 1 to 10 carbon atoms, where the carbon adjacent to Si is a secondary or tertiary carbon atom, and in the formula, 2 However, independently, it is a hydrocarbyl radical containing 1 to 10 carbon atoms; and the second external electron donor is of formula R 3 n Si(OR 4 ) 4-n It has, in the formula, each R 3 and R 4 However, independently, each is a hydrocarbyl radical containing 1 to 10 carbon atoms, and n is 1, 2, or 3; where the second external electron donor is different from the first external electron donor.
[0028] In any embodiment, the first and second external electron donors may be selected from the group consisting of tetraethoxysilane, methylcyclohexyldimethoxysilane, propyltriethoxysilane, dicyclopentydimethoxysilane, and combinations thereof. The Ziegler-Natta catalyst system may include a first external electron donor in a total mol% of 2.5 mol% to less than 50 mol%, and a second external electron donor in a total mol% of more than 50 mol%, based on the total mol% of the external electron donors. In any embodiment, a method for producing linear polypropylene comprises the steps of contacting a propylene monomer (and possibly a comonomer) with a catalyst system under propylene polymerization conditions as described herein to produce linear polypropylene having at least 94.0, 96.0, 98.0, 99.0, 99.2, 99.6, 99.8, or 100% by mass of propylene-derived units, a Mw / Mn greater than 5 (or as described herein) and a melt strength of at least 10 cN as determined using an extensional rheometer at 190°C (further described below), wherein the comonomer may be selected from ethylene, butene, hexene, octene, and combinations thereof.
[0029] The polymerization process may include a prepolymerization step. The prepolymerization may include a step utilizing a Ziegler-Natta catalyst system comprising a non-aromatic internal electron donor combined with at least a portion of an organoaluminum cocatalyst, wherein at least a portion of an external electron donor is present, and the catalyst system is utilized at a higher concentration than that used in the subsequent "main" polymerization process. The concentration of the catalyst system in the main polymerization step and / or prepolymerization step may be 0.01 to 200 mM, or more preferably 0.05 to 100 mM, and is calculated as titanium atoms per liter of inert hydrocarbon medium. The organoaluminum cocatalyst may be present in an amount sufficient to produce 0.1 to 500 g of polymer, or more preferably 0.3 to 300 g of polymer, per gram of titanium catalyst present, and may be present in an amount of 0.1 to 100 mol, or more preferably 0.5 to 50 mol, per mole of titanium atoms present in the catalyst component.
[0030] Prepolymerization, if performed, may be carried out under mild conditions in an inert hydrocarbon medium in which the olefin and catalyst components are present. Examples of inert hydrocarbon mediums that can be used include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene; alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane; aromatic hydrocarbons such as benzene, toluene, and xylene; halogenated hydrocarbons such as ethylene chloride and chlorobenzene; and mixtures thereof. Such inert hydrocarbons can also be used in the main polymerization process. The olefin used in prepolymerization may also be the same as the olefin intended to be used in the main polymerization. The reaction temperature for prepolymerization may be such that the resulting prepolymer is not substantially soluble in the inert hydrocarbon medium, and may be between -20 and +100°C, or between -20 and +80°C, or between 0 and 40°C. During prepolymerization, a molecular weight control agent such as hydrogen may be used. The molecular weight control agent may be used in an amount such that the polymer obtained by prepolymerization has properties consistent with the intended product. Prepolymerization is carried out so that 0.1 to 1000 g of polymer, or more preferably 0.3 to 300 g of polymer, is formed per gram of titanium catalyst. The polymerization of propylene and any selected comonomer may be carried out in the gas phase, liquid phase, bulk phase, slurry phase, or any combination thereof. In particular, polymerization may be carried out by slurry polymerization, using an inert hydrocarbon as the reaction solvent or using an olefin liquid as the solvent under its reaction conditions. The polymerization process includes a step of contacting a titanium catalyst component, one or more internal electron donors, an organoaluminum cocatalyst, and two external electron donors with each other at the time of the main polymerization, before the main polymerization, for example, at the time of prepolymerization, or at the time of a combination thereof. When contacting them before the main polymerization, any two or more of these components may be freely selected and brought into contact. Any two or more of these components may be brought into contact individually or partially and then brought into contact with each other together to form a catalyst system. In any case, hydrogen may be used during polymerization to control the molecular weight and other properties of the resulting polymer.
[0031] In any embodiment, polymerization conditions include polymerization temperatures ranging from 20, 40, or 60°C to 120, 140, 160, 180, or 200°C, and atmospheric pressure from atmospheric pressure up to 100 kg / cm³. 2 Up to a pressure of 2 or 6 kg / cm², more preferably 6 kg / cm². 2 From 20, or 50, or 100 kg / cm³ 2 The pressure range includes up to . The polymerization process may be carried out in batches, semi-continuously, or continuously, and / or sequentially in two or more reactors. If carried out in more than one reactor, the conditions in each reactor may be the same or different. The reaction slurry (homopolymer granules in bulk propylene) may then be removed from the reactor, and the polymer granules are continuously separated from the liquid propylene. The polymer granules may then be separated from the unreacted monomer to produce granular products for compounding and / or mechanical properties.
[0032] In any case, the linear polypropylene has the desirable properties described herein. In any embodiment, the melt flow rate (MFR) of the linear polypropylene is in the range of 0.1, 0.2, or 0.5 g / 10 min to 4, 8, 10, or 20 g / 10 min. In any embodiment, the weight-average molecular weight (Mw) of the linear polypropylene, as determined by GPC-3D analysis, is in the range of 100,000, 150,000, 200,000, or 250,000 g / mol to 500,000, 550,000, 600,000, or 800,000 g / mol. In any embodiment, the linear polypropylene has a molecular weight distribution (Mw / Mn) of at least 5, 6, or 8, or in the range of 5, 6, or 8 to 9, 10, 12, or 16. In any embodiment, the z-average molecular weight (Mz) of a desirable linear polypropylene, as determined by GPC-3D analysis and beneficial in the present invention, is in the range of 800,000, or 1,000,000, or 1,100,000 g / mol to 1,300,000, or 1,400,000, or 1,500,000, or 1,800,000, or 2,000,000 g / mol, and the ratio of z-average molecular weight to weight-average molecular weight (Mz / Mw) is greater than 2.8, or 2.9, or 3.0, or in the range of 2.8, or 2.9, or 3.0, or 3.5 to 4.0, or 4.5, or 5.0, where values greater than 2.8 indicate a high molecular weight portion relative to linear polyethylene.
[0033] Beneficial linear polypropylene may also possess other desirable properties. In any embodiment, the linear polypropylene has a yield strength of 20, 25, or 30 MPa, or a yield strength of 25 MPa to 40, 45, 50, 55, or 80 MPa (using an Instron Machine with a crosshead speed of 50.8 mm / min (2.0 in / min) and a gauge length of 50.8 mm (2.0 in), ASTM D638). In any embodiment, the linear polypropylene has a 1% secant flexural modulus in the range of 1800, 1900, or 2000 MPa to 2100, 2200, 2400, or 2600 MPa (using an Instron Machine with a crosshead speed of 1.27 mm / min (0.05 in / min) and a support span of 50.8 mm (2.0 in), ASTM D790A). In any embodiment, the linear polypropylene has a melt strength of at least 10, 15, or 20 cN at 190°C, or a melt strength in the range of 10, 15, 20, or 30 cN to 35, or 40 cN (determined by the extensional rheology described below). In any embodiment, the melt strength of the branched polypropylene described below exceeds the melt strength of the linear polypropylene, and preferably is at least 5, 10, 15, or 20 cN higher than the melt strength of the linear polypropylene.
[0034] (branched polypropylene) Here, and throughout this specification, the term “branched polypropylene” means a homopolymer or copolymer of polypropylene having a branching index g'(vis) less than 0.98, 0.97, or 0.96. Branched polypropylene can be formed by any means, including catalyst production for reactor-grade branched polypropylene, or reactive extrusion, among other means. Preferred branched polypropylene may also have other characteristics, as further described below.
[0035] In any embodiment, branched polypropylene is formed by combining linear polypropylene and an organic peroxide under suitable conditions, where “organic peroxide” is any organic compound containing at least one -(O)COO- group and / or -OO- group, and preferably has a half-life temperature of less than 100°C determined in an aromatic and / or halogenated aromatic hydrocarbon solvent. 1 T 1 / 2 Preferably, within the range of 25, 35, or 45°C to 65, 75, 85, or 100°C. 1 T 1 / 2 ) has.
[0036] In any embodiment, the organic peroxide is selected from one or more compounds having structures selected from (a) and (b): [Case 2] In the formula, each "R" group is independently selected from the group consisting of hydrogen, C1 or C5-C24 or C30 linear alkyl, C1 or C5-C24 or C30 secondary alkyl, C1 or C5-C24 or C30 tertiary alkyl, C7-C34 alkylaryl, C7-C34 arylalkyl, and substituted forms thereof. Most preferably, the organic peroxide is selected from the structure represented by formula (a). "Substituted" means a hydrocarbon "R" group having substituents such as halogens, carboxylates, hydroxyl groups, amines, mercaptans, and phosphorus-containing groups. In certain embodiments, each "R" group is independently selected from the group consisting of octyl, decyl, lauryl, mythrityl, cetyl, arachidyl, behenyl, erucyl, and ceryl groups, as well as C8-C24 alkylaryl, tertiary, and tertiary forms thereof. 20Alternatively, a C24 linear, secondary, or tertiary alkyl group may be selected. Detailed, non-limiting examples of suitable organic peroxides include di-sec-butyl peroxydicarbonate, diisopropyl peroxydicarbonate, dicyclohexyl peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, dicetyl peroxydicarbonate, dibutyl peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, didodecyl peroxydicarbonate, diicosyl peroxydicarbonate, and ditetracosyl peroxydicarbonate. The formation of branched polypropylene as described herein is achieved in any embodiment by melt-mixing linear polypropylene with an organic peroxide, particularly by applying shear force during mixing / extrusion and radiant heating up to at least the melting point of the linear polypropylene, for example, up to at least 140, or 150, or 160°C, or from 140, or 150, or 160°C to 180, or 200, or 220, or 240, or 260, or 280, or 300°C. Suitable means include a single-screw or twin-screw extruder or a Brabender-type apparatus. Most preferably, the organic peroxide is combined with the linear polypropylene in an amount ranging from 0.1, or 0.5, or 1 to 2, or 3, or 4, or 5% by mass relative to the mass of the organic peroxide and the linear polypropylene.
[0037] In any embodiment, branched polypropylene is formed directly from the extrusion process into reactor flakes and / or granules or extruded pellets without treatment and / or solvent washing under vacuum. In any embodiment, it is preferable that the peroxide melts before reacting with the linear polypropylene so that the granules are uniformly coated and a high specific surface area is utilized before the branching and / or crosslinking reactions. In any embodiment, the reactor granules of linear polypropylene used herein are preferable to extruded pellets. Such linear polypropylene granules are preferably dry-mixed with an organic peroxide before "combining" so that they melt-mix in, for example, a uniscrew or twin-screw extruder ("melt extrusion").
[0038] In any embodiment, the reaction products between the organic peroxide and linear polypropylene may include carbon dioxide, as well as decomposition products consisting of an alcohol, preferably a C8-C24 alcohol, and most preferably an organic peroxide of hydroxyl equivalent used in the reaction. The alcohol is typically present, if at all, only in amounts of 2, 1, or 0.5% by mass relative to the mass of the branched polypropylene. As described herein, the branched polypropylene may have any of the properties described herein with respect to the composition. Having thus been formed, the branched polypropylene described herein can be transported, shipped, and / or stored without further processing and used in mixing with low molecular weight polyolefins to produce any number of articles, both foamed and non-foamed. In any embodiment, a blowing agent may be added during the heating / extrusion process described above so that it does not become activated after transport and can be used to produce foamed articles. Preferably, the low molecular weight polyolefin is also mixed with the branched polypropylene before foaming. As mentioned, the composition may be heated / extruded again later to form articles and achieve foaming, if desired.
[0039] Branched polypropylene will have the same levels of propylene and comonomer-derived units as its linear polypropylene precursor. In any embodiment, diene monomers such as butadiene, isoprene, norbornene, and 1,9-decadien (linear, branched, or cyclic C4-C20 alkenes having at least two conjugated or unconjugated carbon-carbon double bonds) are not present in the branched polypropylene and / or are not present in any of the process steps in the formation of the branched polypropylene. The polypropylene useful in the compositions of the present invention is characterized by any number of parameters, distinct from its linear polypropylene precursor. In any embodiment, the branched polypropylene has a melt strength of at least 20, or 30, or 40 cN, or a melt strength in the range of 20, or 30, or 40, or 45 cN to 60, or 65, or 80 cN. In any embodiment, the branched polypropylene has an MFR ranging from 0.1, 0.2, or 0.5 g / 10 min to 4, 8, 10, or 20 g / 10 min.
[0040] In any embodiment, the branched polypropylene has a number-average molecular weight (Mn) determined by GPC-3D analysis, ranging from 18,000, 20,000, 24,000, or 28,000 g / mol to 40,000, 44,000, 48,000, or 50,000 g / mol. In any embodiment, the polypropylene also has a weight-average molecular weight (Mw) determined by GPC-4D analysis, ranging from 250,000, 300,000, or 350,000 g / mol to 450,000, 500,000, 550,000, or 600,000 g / mol. In any embodiment, the branched polypropylene has a z-average molecular weight (Mz) determined by GPC-4D analysis, ranging from 1,000,000, or 1,100,000, or 1,200,000 g / mol to 1,500,000, or 1,600,000, or 1,700,000, or 1,800,000 g / mol. As an indicator of its high molecular weight component or "tail," the branched polypropylene has, in any embodiment, an Mz / Mw value greater than 3.0, or 3.2, or 3.6, or an Mz / Mw value ranging from 3.0, or 3.2, or 3.6 to 4.0, or 4.5, or 5.0, or 6.0. Furthermore, branched polypropylene has an Mz / Mn greater than 30, 35, or 40, or an Mz / Mn in the range of 30, 35, or 40 to 44, 48, 50, 55, or 60. In any embodiment, branched polypropylene also has an Mz / Mn of at least 5, 6, 8, or 10, or an Mz / Mn in the range of 5, 6, 8, or 10 to 16, 18, or 20.
[0041] Branched polypropylene exhibits improved work hardening (compared to linear polypropylene), as evidenced by an increase in peak extension viscosity. In any embodiment, branched polypropylene has a peak extension viscosity (annealed) greater than 50, 55, or 60 kPa·s at a strain rate of 0.01 / sec (190°C), or a peak extension viscosity (annealed) in the range of 50, 55, or 60 kPa·s to 500, 550, or 600 kPa·s. In any embodiment, branched polypropylene has a peak extension viscosity (annealed) greater than 500, 550, or 600 kPa·s at a strain rate of 0.01 / sec (190°C), or a peak extension viscosity (annealed) in the range of 500, 550, or 600 kPa·s to 2000, 2500, or 3000 kPa·s.
[0042] (Polypropylene composition) In any embodiment, a polypropylene composition comprising (or essentially comprising) branched polypropylene and low molecular weight polyolefins as described above is disclosed. In any embodiment, the composition comprises low molecular weight polyolefins in an amount ranging from 5 or 10% by mass to 15, 20, 25, 30, 35, or 40% by mass relative to the mass of the low molecular weight polyolefins and branched polypropylene. Most preferably, the remainder of the composition is branched polypropylene and additives. In any embodiment, the polypropylene composition exhibits at least 90% or 95% of the work hardening shown by branched polypropylene alone, as measured by extensional rheology at 190°C at the same strain rate. Also in any embodiment, the polypropylene composition exhibits at least 10% or 5% lower complex viscosity at 500 rad / s compared to branched polypropylene alone, as determined by small-amplitude oscillatory spectroscopy at 190°C. In any embodiment, the composition may be formed into foamed articles, thermoformed articles, and / or extruded articles. Desired articles include cups, plates, food containers, and insulating containers. "Low molecular weight polyolefin" is a polyolefin polymer having a weight-average molecular weight of 80,000 or 100,000 g / mol or less, preferably containing ethylene and C4-C10 derived units, most preferably containing propylene derived units, and may also contain ethylene derived units. In any embodiment, the low molecular weight polyolefin has a melt flow rate (230°C / 2.16 kg) of at least 50, or 100, or 200, or 500 g / 10 min, or a melt flow rate (230°C / 2.16 kg) in the range of 50, or 100, or 200, or 500 g / 10 min to 1500, or 2000, or 5000 g / 10 min.
[0043] In any embodiment, the low molecular weight polyolefin is selected from the group consisting of polypropylene homopolymers, polypropylene copolymers, polyethylene homopolymers, polyethylene copolymers, and mixtures thereof. Most preferably, the low molecular weight polyolefin is a polypropylene homopolymer, meaning it contains less than 1 or 2% by mass of ethylene or C4-C10 derived units. In any embodiment, the low molecular weight polyolefin has a Mw / Mn of 5, or 4, or less than 3. The composition is more processable than branched polypropylene alone, but maintains a desirable level of work hardening for forming a closed-cell structure, making it suitable for thermoformed articles, and especially foamed articles. Accordingly, in any embodiment, the foamed articles, thermoformed articles, and / or extruded articles include a polypropylene composition comprising branched polypropylene and a small amount of additives, having a melt strength (190°C) in the range of 20 to 80 cN and a melt flow rate in the range of 0.1 to 20 g / 10 min, in the range of 95 to 60% by mass relative to the mass of branched polypropylene and polypropylene homopolymer; and a polypropylene homopolymer having a melt flow rate of at least 50 g / 10 min, in the range of 5 to 40% by mass relative to the mass of branched polypropylene and polypropylene homopolymer, wherein the polypropylene composition has a melt flow rate in the range of 0.5 to 40 g / 10 min, a melt strength (190°C) in the range of 20 to 80 cN and exhibits at least 90% of the work hardening shown by branched polypropylene.
[0044] Almost any mixing technique can be used to combine the components and produce a polypropylene composition. Preferably, the process of the present invention comprises the steps of: combining linear polypropylene with an organic peroxide to obtain branched polypropylene; and combining branched polypropylene with a low molecular weight polyolefin to obtain a polypropylene composition. Preferably, the low molecular weight polyolefin is combined in an amount ranging from 5 or 10% by mass to 15, 20, 25, 30, 35, or 40% by mass relative to the mass of the low molecular weight polyolefin and the branched polypropylene. The remainder is branched polypropylene with or without additives such as antioxidants, fillers, and other additives known in the art. The components are most preferably melt-mixed using a single-screw or twin-screw extruder operating at a temperature that melts the polymer raw materials but is below the decomposition temperature, preferably in the range of 190 to 260°C.
[0045] In any embodiment, the low molecular weight polyolefin is combined with other raw materials by directly supplying it to an extruder, preferably in its solid form, or by first forming a master blend of the low molecular weight polyolefin containing a higher molecular weight polyolefin. In any embodiment, a process for producing a polypropylene composition comprises the steps of: combining linear polypropylene having a melt strength (190°C) in the range of 10 to 40 cN with an organic peroxide to obtain branched polypropylene having a melt strength (190°C) in the range of 20 to 80 cN, wherein the melt strength of the branched polypropylene exceeds that of the linear polypropylene; and combining branched polypropylene having a melt flow rate in the range of 0.1 to 20 g / 10 min and at least 5 Mw / Mn with a polypropylene homopolymer having a melt flow rate of at least 50 g / 10 min and less than 5 Mw / Mn, in the range of 5 to 40% by mass relative to the mass of the branched polypropylene and the polypropylene homopolymer, wherein the polypropylene composition has a melt flow rate in the range of 0.5 to 40 g / 10 min, a melt strength (190°C) in the range of 20 to 80 cN, and exhibits at least 90% of the work hardening shown by the branched polypropylene.
[0046] The various descriptive elements and numerical ranges disclosed herein relating to the polypropylene compositions and processes of the present invention for obtaining them can be combined with other descriptive elements and numerical ranges to describe the present invention, and furthermore, with respect to a given element, any numerical upper limit can be combined with any numerical lower limit described herein, including examples in jurisdiction that enable such combinations. [Examples]
[0047] The features of the present invention will be demonstrated in the following non-limiting examples. First, the test method and experimental procedure are described. MFR (Measuring Factor). ASTM D1238, using a load of 2.16 kg at 230°C.
[0048] Molecular weight determination using DRI (GPC-3D). This method describes the first of two different methods used to determine the molecular weight moment of the polymers described herein, the so-called "GPC-3D" method and the "GPC-4D" method, as shown, each based on gel permeation chromatography (GPC) but using different detection methods. In the GPC-3D method, the number-average molecular weight (Mn) value was determined by using high-temperature gel permeation chromatography (Agilent PL-220) equipped with three in-line detectors: a differential refractive index detector (DRI), a light scattering (LS) detector, and a viscometer. Three Agilent PLgel 10 μm Mixed-B LS columns were used. The nominal flow rate was 0.5 mL / min and the nominal injection volume was 300 μL. Various transfer lines, columns, viscometers, and differential refractometers (DRI detectors) were housed in an oven maintained at 145°C. The experimental solvent was prepared by dissolving 6 grams of butylated hydroxytoluene (BHT) as an antioxidant in 4 liters of Aldrich reagent-grade 1,2,4-trichlorobenzene (TCB). The TCB mixture was then filtered through a 0.1 μm Teflon® filter. The TCB was then degassed using an online degasser before being introduced into the GPC-3D. Polymer solutions were prepared by placing the dry polymer in a glass container, adding the desired amount of TCB, and then heating the mixture at 160°C with continuous shaking for approximately 2 hours. All volumes were measured by mass spectrometry. The TCB densities, used to express polymer concentration in mass / volume units, were 1.463 g / ml at 23°C and 1.284 g / ml at 145°C. Injection concentrations ranged from 0.5 to 2.0 mg / ml, with lower concentrations used for samples with higher molecular weights. The DRI detector and viscometer were purged before running each sample. Subsequently, increase the flow rate in the instrument to 0.5 ml / min and allow the DRI to stabilize for 8 hours before injecting the first sample. Turn on the LS laser at least 1 to 1.5 hours before running the sample. The concentration "c" of each point in the chromatogram is given by the formula: c=(K DRI / I DRI ) / (dn / dc) Using the DRI signal with the baseline subtracted, I DRI Calculated from, in the formula, K DRI λ is a constant determined by the calibration of the DRI, and (dn / dc) is the refractive index increment of the system. The refractive index of TCB at 145°C is n=1.500 and λ=690nm. The units of the parameters throughout this description of the GPC-3D method are, in terms of concentration, g / cm³. 3 It is expressed such that its molecular weight is expressed in g / mol and its intrinsic viscosity is expressed in dL / g. Unless otherwise specified, all concentrations are expressed in g / cm³. 3 All molecular weights are expressed in g / mol, and all intrinsic viscosities are expressed in dL / g. For GPC-3D or GPC-4D data processing, the Mark-Houwink constants used were K=0.000229 and a=0.705, and dn / dc=0.1048 mL / mg. A2 (input value)=0.0006.
[0049] Molecular weight determination using an Ir detector (GPC-4D). The distribution and moments of weight-average and z-average molecular weights (Mw, Mz) were determined using GPC-4D or a very similar method as performed by GPC-3D, using a high-temperature GPC (Polymer Char GPC-IR) equipped with a multi-channel band filter-based infrared detector IR5, an 18-angle light scattering detector, and a viscometer. Three Agilent PLgel 10 μm Mixed-B LS columns were used to separate the polymers. Aldrich reagent-grade TCB containing 300 ppm of the antioxidant BHT was used as the mobile phase. The TCB mixture was filtered through a 0.1 μm Teflon® filter and degassed with an online degasser before entering the GPC instrument. The nominal flow rate was 1.0 mL / min and the nominal injection volume was 200 μL. The entire system, including the transfer line, column, and detector, was placed in an oven maintained at 145°C. A predetermined volume of polymer sample was weighed and sealed in a standard vial containing 80 μL of added flow marker (heptane). After loading the vial into the autosampler, the polymer was automatically dissolved in the instrument with 8 mL of added TCB solvent. The polymer was then dissolved at 160°C with continuous shaking for approximately 2 hours. The TCB densities used for concentration calculations were 1.463 g / ml at 23°C and 1.284 g / ml at 145°C. Sample solution concentrations ranged from 0.2 to 2.0 mg / ml, with lower concentrations used for samples with higher molecular weights.
[0050] The intensity "c" of each point in a chromatogram is given by the following formula: c=βI The mass recovery rate is calculated from the IR5 broadband signal intensity "I" with the baseline subtracted, where β is the mass constant determined using the polypropylene standard. The mass recovery rate is calculated from the ratio of the integral area of concentration chromatography to the elution volume, and from the injection mass equal to the predetermined concentration multiplied by the injection loop volume. Conventional molecular weight (IR MW) is determined by combining a universal calibration relationship with column calibration performed using a series of monodisperse polystyrene (PS) standards ranging from 700 g / mol to 10,000,000 g / mol. The MW for each elution volume is given by the following formula: [Math 1] The calculation is performed using the formula, where variables with the subscript "PS" represent polystyrene, and those without a subscript represent the test sample. In this method, a PS = 0.67, K PS While "K" and "a" are 0.000229 and 0.705, respectively, with respect to polypropylene as used herein. In all cases, the values of Mn, Mw, and Mz for both GPC-3D and GPC-4D have an accuracy of ±10%.
[0051] (branching index) The specific viscosity of the polymer eluting from the above GPC was determined using a high-temperature Viscotek viscometer equipped with four capillaries arranged in a Wheatstone bridge configuration with two pressure transducers. One transducer measures the total pressure drop across the detector, while the other transducer, located between the two sides of the bridge, measures the differential pressure. The specific viscosity ηs of the solution flowing through the viscometer is calculated from their outputs. The intrinsic viscosity [η] at each point in the chromatogram is given by the following formula: η s =c[η]+0.3(c[η]) 2 The formula was calculated from the following, where c is the concentration, and was determined from the DRI output.
[0052] Branching index (g' vis The following is calculated using the output of the GPC-DRI-LS-VIS method: Average intrinsic viscosity of the sample [η] avg of, [Math 2] The calculation is performed by the formula, where the sum spans chromatographic slice i between the integration limits. Then, the branching index g'(vis) [Math 3] is defined as, where M v is the viscosity average molecular weight based on the molecular weight determined by LS laser analysis. The Z-average branching index (g’Z ave ) is calculated using Ci = the polymer concentration in slice i in the polymer peak times the square of the mass of slice Mi 2 . A value of g’(vis) close to 1 indicates a linear polymer, and lower values indicate a certain level of branching that increases as the g’(vis) value decreases.
[0053] SAOS. Small Angle Oscillatory Spectroscopy was used to determine the viscosity at low shear rates. The polymer sample was prepared using a heating press (either a Carver Press or a Wabash Press) to make a disk with a diameter of 25 mm and a thickness of 2.5 mm. To characterize the shear thinning behavior, small angle oscillatory shear measurements were performed using a rheometer ARES-G2 (TA Instruments) at a temperature of 190 °C and a fixed strain of 10% at angular frequencies ranging from 0.01 to 500 rad / s. Then, the data was converted to viscosity as a function of shear rate. Strain sweep measurements were performed (at an angular frequency of 100 Hz) to ensure that measurements within the linear change range were provided by the selected strain. The data was processed using Trios software.
[0054] Elongational rheology. To characterize the work hardening behavior of polypropylene, annealed samples were tested using a DHR-3 rheometer (TA Instruments) with a mounted SER fixture to measure the stress in elongation. The samples were prepared using the above procedure (SAOS) and then cut into a rectangular shape with approximate dimensions of 18 mm in length and 12.7 mm in width. The measurements were made at 1, 5, and 10 seconds -1The process was carried out at the Hencky strain rate and a temperature of 190°C. Data was processed using Trios software. The sample was annealed by heating to approximately 200°C for 3 minutes to melt the polypropylene pellets without the use of pressure. Subsequently, a pressure of 1500 psi was applied while the sample was continued to heat between two plates for a further 3 minutes. After that, the pressure applied to the sample was removed while the sample was continued to heat at 200°C for a further 20 minutes. After 20 minutes, the sample was cooled by water circulation for a further 20 minutes without the application of any pressure. The melt strength values reported herein have an accuracy of ±10%. Procedure for mixing components. The components listed in Table 1 were melt-mixed using a ZSK 30mm extruder to produce the mixtures for each example, where 15–50% by mass (based on the mass of all components in the mixture) of low molecular weight polyolefin, in this case 1550 MFR polypropylene homopolymer, was pre-mixed with 50–85% by mass of branched polypropylene in a Patterson Double Cone Blender. The dry mixture was fed into a Coperion Werner and Pfleiderer ZSK 30mm extruder (twin-screw co-rotating screw, L / D=36) with an output of approximately 10 kg / hour and nitrogen applied to the hopper. The extruder torque was approximately 50%, the die pressure was approximately 400 psi, and the screw rotation speed was approximately 200 rpm. The melting temperature was approximately 435°F (222°C). Finally, pellets of each of the example mixtures were produced using an underwater pelletizer.
[0055] Branched polypropylene (b-PP) was produced by melt extrusion of the Ziegler-Natta-produced linear polypropylene homopolymer, prepared as described above using 1.5 mass% Perkadox (Akzo Nobel), at temperatures ranging from 190 to 220°C. In all exemplary mixtures, b-PP had a g'(vis) of less than 0.98, a melt strength of 40 ± 5 cN, an MFR of 2.09 g / 10 min, a Mw / Mn of 15, and a Mz / Mw of 6. In all mixtures, the low molecular weight polyolefin (LMW-PO) was a polypropylene homopolymer (100% by mass of propylene-derived units) having an MFR of 1550 g / 10 min and a Mw / Mn ratio of 2.5 (GPC-3D).
[0056] Summary of the polypropylene compositions of the present invention shown in Table 1: Example 1 is an 85:15 mixture of branched polypropylene (polypropylene homopolymer, 100% by mass of propylene-derived units) and LMW-PO, and the hybrid had a melt strength of 17.5 cN and a draw ratio close to 5. Example 2 is a 50:50 mixture of branched polypropylene (100% by mass of propylene-derived units) and PolyOne mixed by a third-party compounder; the hybrid had a melt strength of 2.5 cN and a draw ratio close to 12. Example 3 is a 50:50 mixture, but the branched polypropylene has ethylene-derived units of about 0.55% by mass or less relative to the mass of the polymer. Example 4 is a 50:50 mixture, but the branched polypropylene is a polypropylene homopolymer having 100% by mass of propylene-derived units. Table 1. Polypropylene compositions [Table 1]
[0057] The SAOS data in Figure 4 demonstrates that the viscosity, and therefore the processability, of the polypropylene composition is improved compared to branched polypropylene alone, while the data in Figures 1-3 demonstrate that the composition still exhibits a desirable level of work hardening compared to branched polypropylene. Thus, the polypropylene composition exhibits a complex viscosity at least 10% lower at 500 rad / s compared to branched polypropylene, as determined by micro-amplitude vibrational spectroscopy at 190°C, while preferably exhibiting at least 90% of the work hardening shown by branched polypropylene at the same strain rate.
[0058] As used herein, “essentially consisting of” means that the claimed polymer or polymer mixture consists only of the specified components and does not contain any additional components that alter its measured properties by 10 or 20% or more; most preferably, additional components or “additives” are present at a level of less than 5, 4, 3, or 2% by mass relative to the mass of the composition. Such additives include, for example, fillers, colorants, antioxidants, alkyl radical scavengers, anti-UV additives, acid scavengers, slip agents, curing agents and crosslinking agents, oligomers or polymers containing aliphatic compounds and / or cyclic compounds (also known as “hydrocarbon resins”), and other additives known in the art.
[0059] In the case of a process, the phrase “essentially from” means that there are no other process features that would alter the claimed properties of the polymer, polymer mixture, or article produced from that process by 10 or 20 percent or more. For all jurisdictions to which the theory of “incorporation by reference” applies, all test methods, patent publications, patents, and referenced papers are incorporated herein by reference, either in whole or in the relevant parts thereof.
Claims
1. 1. A polypropylene composition comprising: A composition comprising a branched polypropylene and a low molecular weight polyolefin in an amount ranging from 5% to 40% by weight based on the weight of the composition. fruit , a polypropylene composition, wherein the low molecular weight polyolefin has a melt flow rate of at least 50 g / 10 min.
2. Claim 10 comprising branched polypropylene in the range of 95% to 60% by weight based on the weight of the composition. 1 The polypropylene composition according to claim 1.
3. Claim 10. The branched polypropylene has a melt flow rate (230°C / 2.16 kg) in the range of 0.1 g / 10 min to 20 g / 10 min; and a melt strength (190°C) of at least 20 cN. 1 or 2 The polypropylene composition according to claim 1.
4. 10. The branched polypropylene of claim 9, wherein the branched polypropylene has a Mw / Mn of at least 5. 1 from 3 The polypropylene composition according to any one of claims 1 to 10.
5. Claim 10: The low molecular weight polyolefin has a melt flow rate (230°C / 2.16 kg) in the range of 50 g / 10 min to 5,000 g / 10 min. 1 from 4 The polypropylene composition according to any one of claims 1 to 10.
6. Claim 10. The low molecular weight polyolefin is selected from the group consisting of polypropylene homopolymer, polypropylene copolymer, polyethylene homopolymer, polyethylene copolymer, and mixtures thereof. 1 from 5 The polypropylene composition according to any one of claims 1 to 10.
7. Claims wherein the low molecular weight polyolefin has a Mw / Mn of less than 5. 1 from 6 The polypropylene composition according to any one of claims 1 to 10.
8. minutes Branch polypropylene only when measured by extensional rheology at 190°C at the same strain rate. to show At least 90% of work hardening Processing hardness Claim showing Any one of items 1 to 7 The polypropylene composition according to claim 1.
9. 1 Claim 10: Exhibiting at least a 10% lower complex viscosity at 500 rad / s compared to the branched polypropylene alone as determined by small amplitude vibrational spectroscopy at 90°C. Any one of items 1 to 8 The polypropylene composition according to claim 1.
10. Claim 1 from 9 10. A foam-molded, thermoformed, or extruded article comprising the polypropylene composition according to any one of claims 1 to 9.
11. 1. A process for producing a polypropylene composition, comprising: combining a linear polypropylene having a melt strength (190°C) in the range of 10 to 40 cN with an organic peroxide to obtain a branched polypropylene having a melt strength (190°C) in the range of 20 to 80 cN, wherein the melt strength of the branched polypropylene exceeds the melt strength of the linear polypropylene; combining a branched polypropylene having a melt flow rate in the range of 0.1 to 20 g / 10 min and a Mw / Mn of at least 5 with a low molecular weight polyolefin in the range of 5% to 40% by weight based on the weight of the branched polypropylene and the polypropylene homopolymer, wherein the polypropylene homopolymer has a melt flow rate of at least 50 g / 10 min and a Mw / Mn of less than 5 to obtain a polypropylene composition; Including, The process wherein the polypropylene composition has a melt flow rate in the range of 0.5 to 40 g / 10 min, a melt strength (190°C) in the range of 20 to 80 cN, and exhibits at least 90% of the work hardening exhibited by branched polypropylene.