Polyolefin resin composition
Patent Information
- Application Number
- JP2021212960
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-12-25
- Filing Date
- 2021-12-27
- Publication Date
- 2024-12-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Polyolefin resin compositions derived from recycled materials face challenges in maintaining toughness, environmental stress crack resistance (ESCR), and heat stability during molding, which are crucial for achieving high sustainability goals set by regulatory bodies like the EU.
A polyolefin resin composition is formulated by blending recycled polyolefin with virgin polyolefin in specific proportions and adding antioxidants, with controlled molecular structures and properties, including long-chain branches and optimized molecular weights, to enhance toughness, ESCR, and heat stability.
The composition achieves excellent sustainability, toughness, and heat stability during molding, meeting regulatory requirements and improving the recyclability of polyolefin materials.
Smart Images

Figure 00000020_0000
Abstract
Description
Technical Field
[0001] The present invention relates to a polyolefin resin composition.
Background Art
[0002] The problem of plastic waste, typified by the problem of marine plastics, is recognized as an urgent global issue, and innovative solutions are sought. Among them, polyolefin, which is a strong and flexible plastic, is used in applications such as containers and packaging based on its ease of processing and excellent chemical resistance, and is an important plastic with a very high production volume. Recycling and reusing such polyolefins can be said to be one means of solving the plastic waste problem. Patent Document 1 discloses a technique for recycling waste materials (scrap resins) generated when extruding polyolefin-based resins to produce extruded products of various shapes. Further, Patent Document 2 discloses a polyolefin-based resin composition containing a recycled resin obtained from waste materials of an extruded product made of a polyolefin-based resin, a virgin material of a polyolefin-based resin, a hindered phenol-based antioxidant, and a phosphorus-based heat stabilizer. Since it can be used as a resin composition for manufacturing extruded products without deteriorating the waste materials, it is said that the recycling rate of the waste materials can be increased.
Prior Art Documents
Patent Documents
[0003]
Patent Document 1
Patent Document 2
Summary of the Invention
Problems to be Solved by the Invention
[0004] When polyolefins obtained from recycled plastic waste (hereinafter referred to as "recycled polyolefins") are reused for applications such as containers and packaging, it has been found that they exhibit low toughness, environmental stress crack resistance (hereinafter referred to as "ESCR"), and thermal stability during molding. Therefore, there is a need for polyolefin resin compositions containing recycled polyolefins that exhibit excellent toughness, ESCR, and thermal stability during molding. Furthermore, the EU, which is addressing the plastic waste problem, has set targets to increase the recycled material content of plastic bottles to 25% by 2025 and 30% by 2030 ("Directive on Reducing the Environmental Impact of Certain Plastic Products" https: / / www.jetro.go.jp / biznews / 2019 / 05 / 53834b4b467aaafb.html). In light of these targets, there is a demand for polyolefin resin compositions that are highly sustainable, that is, those with a high recycled polyolefin content.
[0005] In view of the above problems, the present invention aims to provide a polyolefin resin composition that is excellent in sustainability and also excellent in toughness, ESCR, and thermal stability during molding. [Means for solving the problem]
[0006] As a result of diligent research to solve the above problems, the present inventors have discovered that a polyolefin resin composition that can solve the above problems can be obtained by mixing recycled polyolefin and virgin polyolefin in a specific ratio, and further mixing in a specific amount of antioxidant, and have completed the present invention.
[0007] In other words, the present invention is as follows. [1] A polyolefin resin composition comprising recycled polyolefin, virgin polyolefin, and an antioxidant, The content of the recycled polyolefin is 30% by mass or more and 99% by mass or less relative to the total of the recycled polyolefin and virgin polyolefin. The virgin polyolefin content is 1% by mass or more and 70% by mass or less relative to the total of recycled polyolefin and virgin polyolefin. A polyolefin resin composition in which the content of the antioxidant is 100 ppm or more and 5000 ppm or less relative to the total polyolefin resin composition. [2] The polyolefin resin composition according to [1] above, wherein the recycled polyolefin is a polyolefin derived from recycled material recovered from the market. [3] The polyolefin resin composition according to [1] or [2] above, wherein the polyethylene content in the recycled polyolefin is 50% by mass or more relative to the recycled polyolefin. [4] The polyolefin resin composition according to any one of [1] to [3] above, wherein the virgin polyolefin has a long-chain branched structure. [5] The polyolefin resin composition according to any one of [1] to [4] above, wherein the virgin polyolefin comprises a polyolefin obtained by polymerization using a chromium-based catalyst or by radical polymerization. [6] The polyolefin resin composition according to any one of [1] to [5] above, wherein the MMI of the virgin polyolefin is 0.10 g / 10 min or more and 20 g / 10 min or less. [7] The density of the aforementioned virgin polyolefin is 945 kg / m³ 3 More than 965kg / m 3 The polyolefin resin composition described in any of the above [1] to [6], which is as follows: [8] The polyolefin resin composition according to any one of the above [1] to [7], wherein the virgin polyolefin is polyethylene. [9] The polyolefin resin composition according to any one of [1] to [8] above, wherein the content of the antioxidant is 2000 ppm or more and 5000 ppm or less relative to the total polyolefin resin composition.
[10] A polyolefin resin composition according to any one of the above [1] to [9], wherein the MI is 0.1 g / 10 min or more and 10 g / 10 min or less.
[11] A polyolefin resin composition according to any of the above [1] to
[10] , for use in blow molding. [Effects of the Invention]
[0008] According to the present invention, a polyolefin resin composition is available that is excellent in sustainability, toughness, ESCR, and thermal stability during molding. [Brief explanation of the drawing]
[0009] [Figure 1] The Mark-Houwink-Sakurada plot of polyethylene (A) obtained in the examples is shown. [Modes for carrying out the invention]
[0010] The following describes in detail embodiments for carrying out the present invention (hereinafter also referred to as "this embodiment"). Note that this embodiment is illustrative for explaining the present invention and is not intended to limit the present invention to the following content. The present invention can be implemented in various modified forms within the scope of its gist.
[0011] [Polyolefin resin composition] The polyolefin resin composition of this embodiment comprises recycled polyolefin, virgin polyolefin, and an antioxidant, wherein the recycled polyolefin content is 30% by mass or more and 99% by mass or less relative to the total of recycled polyolefin and virgin polyolefin, the virgin polyolefin content is 1% by mass or more and 70% by mass or less relative to the total of recycled polyolefin and virgin polyolefin, and the antioxidant content is 100 ppm or more and 5000 ppm or less relative to the total of the polyolefin resin composition.
[0012] The composition of the polyolefin resin composition of this embodiment will be described below.
[0013] The polyolefin resin composition of this embodiment contains recycled polyolefins and virgin polyolefins, wherein the recycled polyolefin content is 30% to 99% by mass, preferably 45% to 99% by mass, and more preferably 60% to 99% by mass, relative to the total of recycled polyolefins and virgin polyolefins, and the virgin polyolefin content is 1% to 70% by mass, preferably 1% to 55% by mass, and more preferably 1% to 40% by mass, relative to the total of recycled polyolefins and virgin polyolefins. By having the content of recycled polyolefins and virgin polyolefins within the above range, a polyolefin resin composition with excellent sustainability, toughness, and ESCR can be obtained.
[0014] The melt index (hereinafter referred to as "MI") of the polyolefin resin composition of this embodiment is preferably 0.1 g / 10 min to 10 g / 10 min, more preferably 0.14 g / 10 min to 5 g / 10 min, and even more preferably 0.18 g / 10 min to 1 g / 10 min. When the MI is within the above range, it tends to be possible to obtain a polyolefin resin composition with superior toughness and moldability. There are no particular limitations on the method for adjusting the MI to the above range, but examples include melt-kneading virgin polyolefins (e.g., polyethylene or polypropylene) or polystyrene, etc., to match the MI of recycled polyolefins to the above range. MI can be measured according to the method described in the examples below.
[0015] [Recycled polyolefins] The recycled polyolefin contained in the polyolefin resin composition of this embodiment is preferably derived from recycled materials recovered from the market, such as plastic waste like containers and packaging discharged from households (hereinafter also referred to as "PCR" (Post-Consumer Recycled material)), and is obtained by selecting polyolefin from the PCR and then undergoing processes such as washing. The recycled polyolefin consists of polyolefin and other resins, with polyolefin being the main component.
[0016] Examples of polyolefins included in recycled polyolefins are ethylene homopolymers and copolymers of ethylene with other comonomers copolymerizable with ethylene (e.g., binary or ternary copolymers). The bonding configuration of the copolymer may be random or blocky.
[0017] Other comonomers copolymerizable with ethylene are not particularly limited, but examples include α-olefins and vinyl compounds. These other comonomers may be used individually or in combination of two or more.
[0018] The α-olefin is not particularly limited, but examples include α-olefins having 3 to 20 carbon atoms, specifically propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, etc. The vinyl compound is not particularly limited, but examples include vinylcyclohexane, styrene, and their derivatives.
[0019] Other comonomers may be used, if necessary, including non-conjugated polyenes such as 1,5-hexadiene and 1,7-octadiene.
[0020] Other resins included in recycled polyolefins are not limited to polystyrene, but include polystyrene, etc.
[0021] The polyethylene content in the recycled polyolefin is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, relative to the recycled polyolefin. There is no particular upper limit to the content, but it is preferably 99% by mass or less, and more preferably less than 100% by mass. When the polyethylene content in recycled polyolefin is within the above range, it tends to be possible to obtain a polyolefin resin composition with superior toughness and ESCR.
[0022] [Virgin polyolefin] The virgin polyolefin contained in the polyolefin resin composition of this embodiment is not particularly limited, and examples include polyethylene such as high-density polyethylene, high-pressure low-density polyethylene, and linear low-density polyethylene, as well as polypropylene. From the viewpoint of toughness and ESCR, polyethylene is preferred. Examples of polyethylene include ethylene homopolymers and copolymers of ethylene and other comonomers copolymerizable with ethylene (e.g., binary or ternary copolymers). One type may be used alone, or two or more types may be used in combination. The bonding configuration of the copolymer may be random or blocky, but from the viewpoint of processability, a non-star configuration is preferred.
[0023] Other comonomers copolymerizable with ethylene are not particularly limited, but examples include α-olefins and vinyl compounds. These other comonomers may be used individually or in combination of two or more.
[0024] The α-olefin is not particularly limited, but examples include α-olefins having 3 to 20 carbon atoms, specifically propylene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, etc. The vinyl compound is not particularly limited, but examples include vinylcyclohexane, styrene, and their derivatives.
[0025] Other comonomers may be used, if necessary, including non-conjugated polyenes such as 1,5-hexadiene and 1,7-octadiene.
[0026] Furthermore, the virgin polyolefin included in the polyolefin resin composition of this embodiment is preferably a polyolefin having a long-chain branched structure, from the viewpoint of ESCR and moldability.
[0027] Here, a long-chain branched structure preferably refers to a structure in which the main chain has side chains with 6 or more carbon atoms. A known method for analyzing whether a polyolefin has a long-chain branched structure is an analytical method combining a viscosity detector and GPC. The specific analytical method is as follows. An Agilent Technologies PL-GPC200 GPC system equipped with a differential refractometer (RI) and a viscometer is used. The RI and viscometer are connected in parallel. The mobile phase solvent is 1,2,4-trichlorobenzene (with 4,4'-thiobis(2-t-butyl-5-methylphenol) added at a concentration of 0.05 wt%) manufactured by Wako Pure Chemical Industries. The flow rate is 1 mL / min, and two Agilent Technologies PLgel MIXED-A columns (13 μm, 7.5 mm I.D × 30 cm) are connected together. The temperature of the column, sample injection section, and each detector is 160°C. The sample concentration is 0.4 mg / mL, and the injection volume (sample loop volume) is 500 μL. A universal calibration curve is prepared using polystyrene as the standard substance. The logarithm of the weight-average molecular weight Mw obtained by measuring the target sample using the above apparatus is plotted on the x-axis, and the logarithm of the intrinsic viscosity η is plotted on the y-axis. On the other hand, the same measurement is performed on linear polymers, and the same plot is produced. In this case, if the graph of the target sample lies below the graph of the linear polymer, it indicates that the target sample is a long-chain branched polymer. Thus, a graph plotting the intrinsic viscosity and molecular weight obtained by a viscosity detector and GPC is known as a Mark-Houwink-Sakurada plot, and it is well known that this analytical method can indicate that a polymer has long-chain branching.
[0028] Furthermore, the degree of long-chain branching in polymers having such long-chain branched structures can be quantified by the branching index (g'). For example, the branching index (g') at a weight-average molecular weight of 1 million can be calculated in the above Mark-Houwink-Sakurada plot as the ratio (g' = ηbr / ηlin) of the viscosity ηlin of the linear polymer at a weight-average molecular weight of 1 million to the viscosity ηbr of the target sample at a weight-average molecular weight of 1 million. The virgin polyolefin contained in the polyolefin resin composition of this embodiment preferably has a branching index (g') of 0.30 or more and 0.94 or less at a weight-average molecular weight of 1 million, more preferably 0.40 or more and 0.90 or less, and even more preferably 0.50 or more and 0.85 or less, from the viewpoint of moldability and ESCR. When the branching index (g') of a polymer with long-chain branching is within the above range, appropriate molecular chain entanglement is formed in resin compositions containing recycled polyolefins, which tends to improve moldability and ESCR.
[0029] The method for obtaining polyolefins having such long-chain branched structures is not particularly limited and includes methods such as polymerization using a chromium-based catalyst or polymerization by radical polymerization.
[0030] The middle melt index (MFR) (hereinafter referred to as "MMI") of the virgin polyolefin contained in the polyolefin resin composition of the present embodiment, measured at a measurement temperature of 190 °C and a load of 5.0 kg in accordance with JIS K7210, is preferably 0.10 g / 10 min or more and 20 g / 10 min or less, more preferably 0.14 g / 10 min or more and 10 g / 10 min or less, still more preferably 0.18 g / 10 min or more and 5 g / 10 min or less, and even more preferably 0.18 g / 10 min or more and 1 g / 10 min or less. When the MMI of the virgin polyolefin is within the above range, the toughness, moldability, and ESCR tend to be further improved.
[0031] The method for adjusting the MMI of the virgin polyolefin to the above range is not particularly limited, and examples thereof include changing various polymerization conditions such as temperature and pressure. The MMI of the virgin polyolefin can be measured according to the method described in the examples below.
[0032] The density of the virgin polyolefin contained in the polyolefin resin composition of the present embodiment is preferably 915 kg / m 3 or more and 968 kg / m 3 or less, more preferably 945 kg / m 3 or more and 965 kg / m 3 or less, still more preferably 947 kg / m 3 or more and 960 kg / m 3 or less, and particularly preferably 949 kg / m 3 or more and 956 kg / m 3 or less. When the density of the virgin polyolefin is within the above range, the toughness tends to be further improved.
[0033] The molecular weight distribution of the virgin polyolefin used in this embodiment is the ratio (Mw / Mn) of the weight-average molecular weight (Mw) to the number-average molecular weight (Mn) determined by gel permeation chromatography. The molecular weight distribution is preferably 19 or more and less than 150, more preferably 21 or more and less than 80, and even more preferably 23 or more and less than 30. By using virgin polyolefins within this range, it is possible to obtain polyolefin resin compositions with superior toughness and ESCR.
[0034] The method for adjusting the density of virgin polyolefin to the above range is not particularly limited and includes changing various polymerization conditions such as temperature and pressure. The density of virgin polyolefin can be measured according to the method described in the examples below.
[0035] The catalyst used in the production of virgin polyolefins is not particularly limited, but metallocene catalysts, Ziegra-Natta catalysts, Phillips catalysts, etc., can be used individually or in combination of two or more. Among these, Ziegra-Natta catalysts and chromium-based catalysts are preferred from the viewpoint of toughness and ESCR.
[0036] Examples of Ziegler-Natta catalysts include known catalysts such as catalysts in which a titanium compound is supported on a support made of porous polymer material (where the matrix includes, for example, polyolefins and their modified products such as polyethylene, polypropylene, polystyrene, ethylene-propylene copolymer, ethylene-vinyl ester copolymer, styrene-divinylbenzene copolymer, and partial or complete saponified ethylene-vinyl ester copolymers; thermoplastic resins such as polyamide, polycarbonate, and polyester; thermosetting resins such as phenolic resin, epoxy resin, urea resin, and melamine resin); inorganic solid oxides of elements belonging to groups 2-4, 13, or 14 of the periodic table (for example, silica, alumina, magnesia, magnesium chloride, zirconia, titania, boron oxide, calcium oxide, zinc oxide, barium oxide, vanadium pentoxide, chromium oxide, thorium oxide, or mixtures thereof or composite oxides thereof).
[0037] A preferred catalyst in this embodiment is, for example, (a) Organomagnesium compounds represented by the following general formula (1) MαMgβR 1 p R 2 q X r Y s (1) (In the formula, α is 0 or a number greater than 0, p, q, r, and s are 0 or a number greater than 0, and the relationship p+q+r+s=mα+2β exists, M is a metallic element belonging to group I to group III of the periodic table, m is the valence of M, and R 1 , R 2 X and Y are hydrocarbon groups with the same or different number of carbon atoms, X and Y are the same or different groups, and are halogens, OR 3 OSiR 4 R 5 R 6 , NR 7 R 8 , SR 9 It represents a base, R 3 , R 4 , R 5 , R 6 , R 7 , R 8R is a hydrogen atom or a hydrocarbon group. 9 (represents a hydrocarbon group), (b) Titanium compounds containing at least one halogen atom, and (c) Halide compounds of Al, B, Si, Ge, Sn, Te, and Sb. The present invention comprises a solid catalyst component [A] obtained by reacting (a) and (b) or (a), (b), and (c), and an organometallic compound [B].
[0038] As for the organometallic compound [B], compounds from groups I to III of the periodic table are preferred, with organoaluminum compounds or organomagnesium compound complexes containing organoaluminum compounds being particularly preferred.
[0039] The reaction between catalyst component [A] and organometallic compound component [B] can be carried out by adding both components to the polymerization system and proceeding under polymerization conditions as polymerization progresses, or it may be carried out in advance prior to polymerization.
[0040] Furthermore, it is preferable that the reaction ratio of the catalyst components be in the range of 1 to 3000 mmol of component [B] per 1 g of component [A].
[0041] Examples of chromium-based catalysts include known catalysts such as solid catalysts in which a chromium compound is supported on an inorganic oxide support, or catalysts that combine the solid catalyst with an organometallic compound.
[0042] Preferred catalysts in this embodiment include those produced by combining a chromium compound-supported catalyst treated with an organometallic compound and a co-catalyst. For example, a polymerization catalyst comprising a solid catalyst component obtained by mixing a chromium oxide catalyst supported on a refractory compound and activated by heat treatment in a non-reducing atmosphere with an organoaluminum compound containing both an alkoxy group and a hydrosiloxy group represented by the following general formula (2), and an organoaluminum compound containing an alkoxy group represented by the following general formula (3). AlR 1 p H q (OR 2) x (OSiHR 3 R 4 ) y (2) (In the equation, p≧1, 0≦q≦1, x≧0.25, y≧0.15, 0.5≦x+y≦1.5 and p+q+x+y=3, R 1 , R 2 , R 3 , R 4 (This represents identical or different hydrocarbon groups with 1 to 20 carbon atoms.) AlR 5 3-n (OR 6 ) n (3) (In the formula, 0 <n≦1、R 5 , R 6 (This represents identical or different hydrocarbon groups with 1 to 20 carbon atoms.)
[0043] The method for producing the virgin polyolefin contained in the polyolefin resin composition of this embodiment is not particularly limited, but known methods such as the solution method, high-pressure method, high-pressure bulk method, gas method, and slurry method can be used.
[0044] The virgin polyolefin contained in the polyolefin resin composition of this embodiment preferably includes at least two types of polyethylene (A) and (B). The polyethylene (A) is preferably an ethylene homopolymer produced using a chromium-based catalyst or a copolymer of ethylene and an α-olefin having 3 to 20 carbon atoms. The MMI of polyethylene (A) is preferably 0.01 g / 10 min to 10 g / 10 min, and the density is 940 kg / m³. 3 It is preferable that the above conditions are met. As polyethylene (B), a resin produced using a Ziegler-Natta catalyst is preferred, and a resin produced by two-stage polymerization is even more preferred. In the two-stage polymerization, it is preferable to first produce a low molecular weight polymer component by homopolymerizing ethylene or copolymerizing ethylene with an α-olefin having 3 to 20 carbon atoms, and then copolymerizing ethylene with an α-olefin having 3 to 20 carbon atoms to produce a high molecular weight polymer component in a weight ratio of 0.95 to 1.1 times the amount of the low molecular weight polymer component. The low molecular weight polymer component preferably has an MI of 10 g / 10 min to 300 g / 10 min or less. The MMI of polyethylene (B) is preferably 0.03 g / 10 min to 1 g / 10 min or less, and the density is 958 kg / m³ 3 The following is preferable: The ratio of polyethylene (A) to (B) is preferably (A) / (B) = 20 / 80 to 80 / 20 by weight, more preferably 30 / 70 to 70 / 30, and even more preferably 40 / 60 to 60 / 40.
[0045] The high-pressure low-density polyethylene in this embodiment can be obtained by radical polymerization of ethylene in an autoclave-type or tubular-type reactor. When using an autoclave-type reactor, the polymerization conditions can be set to, for example, a polymerization temperature of 200-300°C and a polymerization pressure of 100-250 MPa in the presence of a peroxide acting as an initiator. On the other hand, when using a tubular-type reactor, the polymerization conditions can be set to, for example, a polymerization temperature of 180-400°C and a polymerization pressure of 100-400 MPa, preferably 200-350°C and 150-350 MPa in the presence of a peroxide and a chain transfer agent.
[0046] The above peroxides are not particularly limited, but include, for example, methyl ethyl ketone peroxide, peroxyketals (specifically 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 2,2-bis(t-butylperoxy)octane, n-butyl 4,4-bis(t-butylperoxy)barate, 2,2-bis(t-butylperoxy)butane, etc.), and hydroperoxides (specifically t-butyl hydroperoxide, cumulonimbus). Dialkyl peroxides (specifically, di-t-butyl peroxide, dicumyl peroxide, bis(t-butylperoxyisopropyl)benzene, t-butylcumyl peroxide, 2,5-di(t-butylperoxy)hexane, 2,5-dimethyldi(t-butylperoxy)hexane, diacyl peroxides) (Specifically, acetyl peroxide, isobutyryl peroxide, octanoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, benzoyl peroxide, etc.), peroxydicarbonates (specifically, diisopropyl peroxydicarbonate, di-2-ethylhexyl peroxycarbonate, di-n-propyl peroxydicarbonate, di-2-ethoxyethyl peroxycarbonate, dimethoxyisopropyl peroxydicarbonate, dimethoxyisopropyl peroxy Dicarbonates, di(3-methyl-3-methoxybutyl peroxydicarbonate, diallyl peroxydicarbonate, etc.), peroxyesters (specifically, t-butyl peroxyacetate, t-butyl peroxyisobutyrate, t-butyl peroxypivalate, t-butyl peroxyoctate, t-butyl peroxyneodecanoate, t-butyl peroxyneodecanoate, cumyl peroxyneodecanoate, t-butyl peroxy-2-ethylhexanoate, t-butyl peroxy-3,5,Examples include 6-trimethylhexanoate, t-butyl peroxylaurate, t-butyl peroxybenzoate, t-butyl peroxyisopropyl carbonate, cumyl peroxyoctoate, t-hexyl peroxyneodecanoate, t-hexyl peroxypivalate, t-butyl peroxyneohexanoate, t-hexyl peroxyneohexanoate, cumyl peroxyneohexanoate, etc., acetylcyclohexylsulfonyl peroxide, t-butyl peroxyallyl carbonate, etc. The peroxide may be fed into the polymerization reactor after being diluted with an isoparaffinic solvent.
[0047] Furthermore, a chain transfer agent may be added as needed to adjust the molecular weight. The chain transfer agent is not particularly limited, but examples include alcohols such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, and isobutyl alcohol; alkanes or alkenes such as ethane, propane, propylene, butane, 1-butene, and 2-butene; and ketones or aldehydes such as acetone, methyl ethyl ketone, 2-pentanone, 3-pentanone, 2-hexanone, 3-hexanone, diisobutyl ketone, methyl isopropyl ketone, formaldehyde, acetaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, and isovaleraldehyde.
[0048] The reactor may have multiple locations for feeding ethylene and polymerization initiators. As described above, the polymerized polyethylene is separated from the unreacted raw materials and polyethylene resin using a high-pressure separator and a low-pressure separator while reducing the pressure, and the molten polyethylene is granulated into pellets using an extruder.
[0049] [Antioxidant] The antioxidant content in the polyolefin resin composition of this embodiment is 100 ppm to 5000 ppm relative to the total polyolefin resin composition, preferably 1000 ppm to 5000 ppm, and more preferably 2000 ppm to 5000 ppm. By having the antioxidant content within the above range, a polyolefin resin composition with excellent thermal stability during molding can be obtained.
[0050] The antioxidant included in the polyolefin resin composition of this embodiment is not particularly limited, but for example, phenolic compounds or phenolic phosphate compounds are preferred. Specifically, examples include phenolic antioxidants such as 2,6-di-t-butyl-4-methylphenol (dibutylhydroxytoluene), n-octadecyl-3-(4-hydrox-3,5-di-t-butylphenyl)propionate, and tetrakis(methylene(3,5-di-t-butyl-4-hydroxyhydrocinnamate))methane; phenol-phosphorus antioxidants such as 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenzo[d,f][1,3,2]dioxaphosfepin; and phosphorus antioxidants such as tetrakis(2,4-di-t-butylphenyl)-4,4'-biphenylene-diphosphonite, tris(2,4-di-t-butylphenyl)phosphite, and cyclic neopentanetetraylbis(2,4-t-butylphenyl phosphite).
[0051] [Additives] The polyolefin resin composition of this embodiment may optionally contain known additives such as slip agents, neutralizing agents, light stabilizers, antistatic agents, and pigments, to the extent that they do not impair the effects of the present invention.
[0052] The slip agent or neutralizing agent is not particularly limited, but examples include aliphatic hydrocarbons, higher fatty acids, higher fatty acid metal salts, fatty acid esters of alcohols, waxes, higher fatty acid amides, silicone oils, rosin, etc. Specifically, stearates such as calcium stearate, magnesium stearate, and zinc stearate can be listed as suitable additives.
[0053] Examples of light stabilizers are not particularly limited, but include benzotriazole-based light stabilizers such as 2-(5-methyl-2-hydroxyphenyl)benzotriazole and 2-(3-t-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole; and hindered amine-based light stabilizers such as bis(2,2,6,6-tetramethyl-4-piperidine) sebacate and poly[{6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl}{(2,2,6,6-tetramethyl-4-piperidyl)imino}hexamethylene{(2,2,6,6-tetramethyl-4-piperidyl)imino}].
[0054] Antistatic agents are not particularly limited, but examples include aluminosilicates, kaolin, clay, natural silica, synthetic silica, silicates, talc, diatomaceous earth, and glycerin fatty acid esters.
[0055] Pigments are not particularly limited, but examples include titanium dioxide, carbon black, titanium yellow, iron oxide pigments, ultramarine, cobalt blue, chromium oxide, spinel green, lead chromate pigments, and cadmium pigments. Organic pigments include, for example, azo pigments such as azo lake pigments, benzimidazolone pigments, diarylide pigments, and condensed azo pigments; phthalocyanine pigments such as phthalocyanine blue and phthalocyanine green; condensed polycyclic pigments such as isoindolinone pigments, quinophthalone pigments, quinacridone pigments, perylene pigments, anthraquinone pigments, perinone pigments, and dioxazine violet; and azine dyes, etc.
[0056] [Method for producing polyolefin resin composition] The polyolefin resin composition of this embodiment can be manufactured by conventionally known melt-kneading methods using the recycled polyolefin, virgin polyolefin, antioxidant, and other additives as needed. For example, melt-kneading methods using a single-screw extruder, twin-screw extruder, rolls, kneader, Brabender plastograph, Banbury mixer, etc. are possible, but the method using a twin-screw extruder is preferred. The melt-kneading temperature is preferably in the range of 180 to 260°C.
[0057] [Application] The polyolefin resin composition of this embodiment can be used as a raw material for applications such as containers and packaging, and is particularly suitable as a raw material for blow molding, and especially suitable as a raw material for blow-molded bottles. When used as a raw material for blow molding, the MI of the polyolefin resin composition is preferably 0.18 g / 10 min or more and 1 g / 10 min or less. [Examples]
[0058] The embodiment will be described in more detail below with reference to specific examples and comparative examples, but the embodiment is not limited in any way to the following examples and comparative examples.
[0059] The methods for measuring various characteristics and physical properties are shown below. [Physical properties of polyolefin resin compositions and virgin polyolefins] First, we will explain the methods for evaluating the physical properties of polyolefin resin compositions and virgin polyolefins.
[0060] (MI and MMI) The MI and MMI of the polyolefin resin composition and virgin polyolefin were measured in accordance with JIS K7210. MI is a value measured under conditions of 190°C and a load of 2.16 kg, with units of g / 10 min. MMI is a value measured under conditions of 190°C and a load of 5 kg, with units of g / 10 min.
[0061] (density) The density of virgin polyolefins was measured in accordance with JIS K7112:1999 (Method D).
[0062] (Polyethylene content in recycled polyolefins) (Soxhlet extraction procedure) Recycled polyolefin pellets were powdered using a freeze-mill. 1 g of the recycled polyolefin powder was placed in a cylindrical filter paper and solvent extraction was performed with chloroform solvent for 5 hours using a Soxhlet extractor. The Soxhlet extraction residue in the cylindrical filter paper was vacuum-dried (40°C, 2 hours) to completely remove the solvent. At this time, the Soxhlet extraction residue ratio r was calculated using the following formula. r = (weight of Soxhlet extraction residue after complete removal of solvent) / (weight of recycled polyolefin powder used in Soxhlet extraction) (Weight measurement of o-dichlorobenzene soluble content) For the high-temperature filtration operation in the measurement of the weight percentage of o-dichlorobenzene soluble matter, a high-temperature filtration device SSC-9300 manufactured by Senshu Scientific was used. The weight of a PTFE membrane filter (1.0 μm) was measured (this was defined as the weight of the filter before filtration), and it was placed inside a stainless steel test tube for high-temperature dissolution. 20 mg of the Soxhlet extraction residue (referred to as sample weight (2)), from which the solvent had been completely removed using the previously described procedure, was placed in a stainless steel test tube for high-temperature dissolution, and 5 mL of o-dichlorobenzene was added. The test tube was placed on a 160°C heating block and allowed to stand for 1 hour, then shaken for 3 hours. While still heating at 160°C, the soluble components were filtered by pressurizing the top of the test tube with a syringe. Subsequently, 5 mL of o-dichlorobenzene was added to wash the residue on the filter in the stainless steel test tube, and the test tube was placed on a 160°C heating block and shaken for 30 minutes. While still heating at 160°C, the soluble components were filtered by pressurizing the top of the test tube with a syringe. To wash out any remaining residue, 5 mL of o-dichlorobenzene was added, the sample was placed on a 160°C heating block, shaken for 30 minutes, and then, while still heated at 160°C, the soluble matter was filtered by pressurizing the top of the test tube with a syringe. After cooling, the filter with the residual residue attached was removed from the stainless steel test tube and vacuum-dried to remove the solvent (80°C, 4 hours). After the solvent was completely removed, the weight of the filter with the residual residue attached was measured. (This is referred to as the weight of the filter after filtration.) (Weight measurement of the blank) The weight of the PTFE membrane filter was measured (this was referred to as the weight of the blank filter before filtration) and placed inside a stainless steel test tube for high-temperature dissolution. 5 mL of o-dichlorobenzene was added to an empty stainless steel test tube for high-temperature dissolution. The test tube was placed on a heating block at 160°C, allowed to stand for 1 hour, and then shaken for 3 hours. While maintaining the 160°C temperature, the soluble matter was filtered by pressurizing the top of the test tube with a syringe. Subsequently, 5 mL of o-dichlorobenzene was added to a stainless steel test tube, which was then placed on a heating block at 160°C and shaken for 30 minutes. While maintaining the 160°C temperature, the soluble components were filtered by pressurizing the top of the test tube with a syringe. 5 mL of o-dichlorobenzene was added again, the mixture was placed on a heating block at 160°C, shaken for 30 minutes, and while still heated at 160°C, the soluble matter was filtered by pressurizing the top of the test tube with a syringe. After cooling, the filter was removed from the stainless steel test tube and vacuum-dried to remove the solvent (80°C, 4 hours). After the solvent was completely removed, the weight of the filter with the residual residue attached was measured. (This is the weight of the filter after blank filtration.) (Calculation of o-dichlorobenzene soluble fraction) The solubility fraction r' of recycled polyolefin in o-dichlorobenzene was calculated as follows. (6) Residue weight (mg) = (((3) Weight of filter after filtration) - ((1) Weight of filter before filtration) - (((5) Weight of blank filter after filtration) - ((4) Weight of blank filter before filtration)) r'(wt%) = 100 × (1 - ((6) Residue weight) / ((2) Sample weight)) (Recycled polyolefins) 1 (HNMR measurement) Recycled polyolefins 1 1HNMR measurements were performed using a JEOL RESONANCE ECS400 under the following conditions, with deuterated orthodichlorobenzene as the solvent and a sample concentration of 50 mg / mL. Observation frequency: 400MHz Chemical shift reference: Orthodichlorobenzene (7.05 ppm) Pulse delay: 3 seconds Number of scans: 256 Pulse width: 45° Measurement temperature: 140℃ (Calculation of polyethylene content) In the obtained NMR spectrum, the weight fraction Rpe (wt%) of polyethylene in recycled polyolefin was calculated using the following formula, with the peak integral around 6.7 ppm defined as Ips (corresponding to the two protons at the ortho position on the benzene ring in one repeating unit of the polystyrene chain (―CHC5H6―CH2―)), the peak integral around 1.7 ppm defined as Ipp (corresponding to one proton on the tertiary carbon in one repeating unit of the polypropylene chain (―CHCH3―CH2―)), and the integral around 1.4 ppm defined as Ipe (corresponding to the sum of the four protons in one repeating unit of the polyethylene chain (―CH2―CH2―), the two protons on the secondary carbon in one repeating unit of the polypropylene chain, and the two protons on the secondary carbon in one repeating unit of the polystyrene chain). The baseline was created horizontally in the region where no peaks were detected. For Ipp and Ipe, we used the integral values obtained by splitting the valley between the peak around 1.7 ppm and the peak around 1.4 ppm perpendicular to the baseline. Rpe(weight%) = ((Ipe-Ipp×2-Ips) / 4×28.05) / (((Ipe-Ipp×2-Ips) / 4×28.05)+(Ipp×42.08)+(Ips / 2×104.15))×r×r'
[0063] (Long-chain branched structure of virgin polyethylene) An Agilent Technologies PL-GPC200 GPC system equipped with a differential refractometer (RI) and a viscometer was used. The RI and viscometer were connected in parallel. The mobile phase solvent was 1,2,4-trichlorobenzene (with 4,4'-thiobis(2-t-butyl-5-methylphenol) added at a concentration of 0.05 wt%) manufactured by Wako Pure Chemical Industries. The flow rate was 1 mL / min, and two Agilent Technologies PLgel MIXED-A columns (13 μm, 7.5 mm I.D × 30 cm) were connected together. The temperature of the column, sample injection section, and each detector was set to 160°C. The sample concentration was 0.4 mg / mL, and the injection volume (sample loop volume) was 500 μL. A universal calibration curve was prepared using polystyrene as the standard substance. The logarithmic values of the molecular weight M obtained by measuring the target sample using the above apparatus were plotted on the x-axis, and the logarithmic values of the intrinsic viscosity η were plotted on the y-axis. On the other hand, the above measurements were performed using 1475a (supplied from the National Institute of Standards and Technology (NIST)) as a linear polymer, and the plot was performed similarly. In this case, if the graph of the target sample lies below the graph of the linear polymer, it indicates that the target sample contains a branched polymer. The branching index (g') at a weight-average molecular weight of 1 million was calculated as the ratio (g' = ηbr / ηlin) of the viscosity ηlin of the linear polymer at a weight-average molecular weight of 1 million to the viscosity ηbr of the target sample at a weight-average molecular weight of 1 million in the Mark-Houwink-Sakurada plot shown above. The calculated value was rounded to two significant figures, with the third digit rounded off.
[0064] (molecular weight distribution) Polyethylene resin compositions were measured by high-temperature gel permeation chromatography (GPC), and the molecular weight distribution chart obtained was used to determine the ratio of weight-average molecular weight (Mw) to number-average molecular weight (Mn). For the high-temperature GPC measurements, a PolymerChar GPC-IR5 was used, with one Showa Denko AT-807S column and two Tosoh Corporation GMHHR-H(S)HT columns connected in series. Orthodichlorobenzene (ODCB) was used as the mobile phase, and the measurements were performed under the following conditions: column temperature 140°C, flow rate 1.0 mL / min, sample concentration 20 mg / 10 mL of solvent (ODCB), sample dissolution temperature 140°C, and sample dissolution time 1 hour.
[0065] [Evaluation of characteristics] (Evaluation of toughness (Charpy impact strength)) The toughness (Charpy impact strength) of the polyolefin resin composition was measured in accordance with JIS K7111. The unit is kJ / m 2 The test specimen was type B3, and the measurement was taken at 23°C. Based on the results obtained, the evaluation was conducted according to the following evaluation criteria. <Evaluation Criteria> ◎(Good): 4.5kJ / m 2 That's all. ○ (normal): 3.5kJ / m 2 More than 4.5kJ / m 2 less than × (Bad): 3.5 kJ / m 2 less than
[0066] (ESCR evaluation) The ESCR of the polyolefin resin composition was measured in accordance with JIS K6922. A 10% aqueous solution of IGEPAL CO-630 manufactured by SIGMA-ALDRICH was used as the test solution. The time at which the probability of cracking due to environmental stress reached 50% (hereinafter referred to as the F50 value) was measured and defined as the ESCR value. The unit is hr. Based on the results obtained, the evaluation was conducted according to the following evaluation criteria. <Evaluation Criteria> ◎(Good): 60 hours or more ○(Normal): 30 hours or more but less than 60 hours × (Bad): Less than 30 hours
[0067] (Evaluation of moldability) Moldability was assessed using the melt tension of the resin composition as an indicator. The melt tension was measured using a Toyo Seiki Capillograph 1D, with an orifice having a barrel diameter of 9.55 mm, an orifice diameter of 2.10 mm, a length of 7.98 mm, and an inlet angle of 90 degrees, at a resin temperature of 190°C. The piston descended at 6 mm / min, and the take-up speed was set to 2 mm / min. Based on the results obtained, the moldability was evaluated according to the following evaluation criteria. <Evaluation Criteria> ◎(Good): 120mN or more ○ (Normal): 80mN or more and less than 120mN × (Bad): Less than 80mN
[0068] (Evaluation of thermal stability during molding) The thermal stability during molding was measured using the oxidation induction time (OIT) with a Shimadzu DSC60. 8.5 mg of the sample was heated to 200°C at a rate of 25°C / min under a nitrogen atmosphere, and then switched to an oxygen atmosphere while maintaining the temperature at 200°C. The time from switching to the oxygen atmosphere until the exothermic peak rose was defined as the OIT. Based on the obtained results, evaluation was performed according to the following criteria. ◎(Good): 30 minutes or more ○ (Normal): 10 minutes or more but less than 30 minutes × (Bad): Less than 10 minutes
[0069] (Sustainability assessment) Sustainability refers to a high recycling rate (especially material recycling) relative to the amount of polyolefin produced, and was evaluated according to the following criteria. The content criteria were based on the total amount of recycled polyolefin and virgin polyolefin. <Evaluation Criteria> ◎(Good): Contains 50% or more recycled polyolefin by mass. ○(Normal): Recycled polyolefin content is 30% by mass or more and less than 50% by mass. × (Bad): Recycled polyolefin content is less than 30% by mass.
[0070] [Catalyst synthesis for virgin polyethylene production] (1) Synthesis of chromium oxide catalyst (I) Four moles of chromium trioxide were dissolved in 80 liters of distilled water. 20 kg of silica (Grade 952, WR Grace & Company) was immersed in this solution and stirred at room temperature for 1 hour. The slurry was then heated to remove the water, followed by vacuum drying at 120°C for 10 hours. Finally, the slurry was calcined at 600°C for 5 hours with dry air flowing through it to obtain chromium oxide catalyst (I) containing 1.0 wt% chromium.
[0071] (2) Synthesis of organoaluminum compounds (II) 100 moles of triethylaluminum, 50 moles of methylhydropolysiloxane (viscosity at 30°C: 30 centistokes) (based on Si), and 150 liters of n-hexane were weighed into a pressure-resistant vessel under a nitrogen atmosphere and reacted at 50°C for 24 hours with stirring to produce Al(C2H5). 2.5 (OSi·H·CH3·C2H5) 0.5 A hexane solution was prepared. Next, 100 moles (based on Al) of this solution was transferred to a 600-liter reactor under a nitrogen atmosphere. A mixed solution of 50 liters of ethanol and 50 liters of n-hexane was added at -10°C with stirring. After the addition, the temperature was raised to 50°C and the reaction was carried out at this temperature for 1 hour to produce Al(C2H5). 2.0 (OC2H5) 0.5 (OSi·H·CH3·C2H5) 0.5 A hexane solution was prepared.
[0072] (3) Synthesis of titanium catalyst (III) In a 15-liter reactor that has been thoroughly purged with nitrogen, 3 liters of trichlorosilane as a 2 mol / liter n-heptane solution are charged, and the reactor is kept at 65°C while stirring, with the chemical formula AlM g6(C2H5)3(n-C4H9) 6.4 (On-C4H9) 5.6Seven liters of an n-heptane solution of the organomagnesium component shown (equivalent to 5 moles of magnesium) were added over one hour, and the reaction was continued at 65°C for another hour with stirring. After the reaction was complete, the supernatant was removed, and the mixture was washed four times with seven liters of n-hexane to obtain a solid slurry. This solid was separated, dried, and analyzed, and it was found to contain 7.45 mmol of Mg per gram of solid. A slurry containing 500 g of solid was reacted with 0.93 liters of n-hexane solution containing 1 mol / liter of n-butyl alcohol under stirring at 50°C for 1 hour. After the reaction, the supernatant was removed and washed once with 7 liters of n-hexane. This slurry was kept at 50°C and 1.3 liters of n-hexane solution containing 1 mol / liter of diethylaluminum chloride were added under stirring and reacted for 1 hour. After the reaction, the supernatant was removed and washed twice with 7 liters of n-hexane. This slurry was kept at 50°C and 0.2 liters of n-hexane solution containing 1 mol / liter of diethylaluminum chloride and 0.2 liters of n-hexane solution containing 1 mol / liter of titanium tetrachloride were added and reacted for 2 hours. After the reaction, the supernatant was removed and the solid catalyst was isolated and washed with hexane until no free halogens were detected. This solid catalyst contained 2.3 wt% titanium.
[0073] [Manufacturing of Virgin Polyethylene 1] (1) Manufacturing of polyethylene (A) In a single-stage polymerization process, polymerization was carried out in a 230 L polymerizer. The polymerization temperature was 80°C and the polymerization pressure was 0.98 MPa. Purified hexane was supplied at a rate of 60 L / hr, and as a co-catalyst, an organoaluminum compound obtained by reacting methanol and aluminum trihexyl in a molar ratio of 0.92:1 was supplied to the polymerizer at a concentration of 0.08 mmol / L. 50 g of the chromium oxide catalyst (I) synthesized in (1) was added to this polymerizer, along with 0.03 moles (Al basis) of the organoaluminum compound (II) prepared in (2), and the solid catalyst obtained by reacting at room temperature for 1 hour was supplied at a rate of 2 g / hr. Ethylene was also supplied at a rate of 12 kg / hr, and hydrogen was supplied as a molecular weight modifier to maintain a gas phase concentration of approximately 1 mol%. Polymerization was carried out, resulting in an MMI of 0.6 g / 10 min and a density of 964 kg / m³. 3 Polyethylene (A) was manufactured. The intrinsic viscosity and molecular weight of this polyethylene (A) were measured using the aforementioned analytical method combining a viscosity detector and GPC, and a Mark-Houwink-Sakurada plot was created (Figure 1). From Figure 1, since the plot of polyethylene (A) lies below the plot of linear polyethylene, it was shown that polyethylene (A) has long-chain branching. At this time, the branching index (g') value was 0.45.
[0074] (2) Manufacturing of polyethylene (B) To produce the low molecular weight polymer component in the first stage of polymerization, a stainless steel polymerizer 1 with a reaction volume of 300 liters was used, under conditions of polymerization temperature of 81°C and polymerization pressure of 1 MPa. The catalysts used were the above-mentioned solid catalyst (III) at a rate of 1.3 mmol (Ti atom basis) / hr, triisobutylaluminum at a rate of 20 mmol (metal atom basis) / hr, and hexane at a rate of 40 liters / hr. Hydrogen was used as a molecular weight modifier, and polymerization was carried out by supplying hydrogen to achieve a hydrogen concentration of 65 mol% relative to ethylene. The polymer slurry solution in polymerizer 1 was introduced into a flash drum at a pressure of 0.1 MPa and a temperature of 75°C, and after separating unreacted ethylene and hydrogen, the slurry was pressurized and introduced into polymerizer 2 with a reaction volume of 250 liters using a slurry pump. In polymerizer 2, under conditions of temperature of 65°C and pressure of 0.5 MPa, triisobutylaluminum was introduced at a rate of 7.5 mmol / hr and hexane at a rate of 40 liters / hr. Ethylene, hydrogen, and butene-1 are introduced to this mixture so that the hydrogen gas phase concentration is approximately 1 mol% and the butene gas phase concentration is approximately 10 mol%. Polymerization is carried out so that the weight ratio of the high molecular weight polymer component produced in polymerizer 2 is 1.05 times the amount of the low molecular weight polymer component produced in polymerizer 1. The resulting mixture has an MMI of 0.2 g / 10 min and a density of 941 kg / m³. 3 Polyethylene (B) was manufactured. The MI of the low molecular weight polymer component produced in polymerizer 1 was 50 g / 10 min, and the density was 971 kg / m³. 3 That was the case.
[0075] (3) Production of virgin polyethylene 1 The polyethylene (A) and (B) powders produced as described above were mixed by weight in a ratio of 40 to 60 and stirred in a mixer. This mixture was extruded using a twin-screw extruder with a cylinder diameter of 44 mm (TEX44HCT-49PW-7V manufactured by Japan Steel Works Co., Ltd.) while kneading at a cylinder temperature of 200°C and an extrusion rate of 35 kg / hour to obtain virgin polyethylene 1. The resulting virgin polyethylene 1 had an MMI of 0.20 g / 10 min and a density of 950 kg / m³. 3 The molecular weight distribution was 25.1. For virgin polyethylene 1, the intrinsic viscosity and molecular weight were measured using the aforementioned analytical method combining a viscosity detector and GPC, and a Mark-Houwink-Sakurada plot was created. Since the plot for virgin polyethylene 1 lies below the plot for linear polyethylene, it was shown that virgin polyethylene 1 has long-chain branching. At this time, the branching index (g') value was 0.77.
[0076] [Virgin polyethylene 2 manufacturing] (1) Manufacturing of polyethylene (C) To produce the low molecular weight polymer component in the first polymerization stage, a stainless steel polymerizer 1 with a reaction volume of 300 liters was used, under conditions of polymerization temperature of 83°C and polymerization pressure of 1 MPa. The catalysts used were the above-mentioned solid catalyst (III) at a rate of 1.4 mmol (Ti atom basis) / hr, triisobutylaluminum at a rate of 20 mmol (metal atom basis) / hr, and hexane at a rate of 40 liters / hr. Hydrogen was used as a molecular weight modifier, and polymerization was carried out by supplying hydrogen to achieve a hydrogen concentration of 70 mol% relative to ethylene. The polymer slurry solution in polymerizer 1 was introduced into a flash drum at a pressure of 0.1 MPa and a temperature of 75°C, and after separating unreacted ethylene and hydrogen, the slurry was pressurized and introduced into polymerizer 2 with a reaction volume of 250 liters using a slurry pump. In polymerizer 2, under conditions of temperature of 77°C and pressure of 0.5 MPa, triisobutylaluminum was introduced at a rate of 7.5 mmol / hr and hexane at a rate of 40 liters / hr. Ethylene, hydrogen, and butene-1 are introduced to this mixture so that the gas phase concentration of hydrogen is approximately 5 mol% and the gas phase concentration of butene is approximately 5 mol%. Polymerization is carried out so that the weight ratio of the high molecular weight polymer component produced in polymerizer 2 is 1.0 times the amount of the low molecular weight polymer component produced in polymerizer 1. The resulting polymer has an MI of 0.2 g / 10 min and a density of 953 kg / m³. 3 Polyethylene (C) was produced. The low molecular weight polymer component produced in polymerizer 1 had a molecular weight (MI) of 70 g / 10 min and a density of 972 kg / m³. 3 That was the case.
[0077] (2) Production of virgin polyethylene 2 The polyethylene (A) and (C) powders produced as described above were mixed by weight in a ratio of 65 to 35 and stirred in a mixer. This mixture was extruded using a twin-screw extruder with a cylinder diameter of 44 mm (TEX44HCT-49PW-7V manufactured by Japan Steel Works Co., Ltd.) while kneading at a cylinder temperature of 200°C and an extrusion rate of 35 kg / hour to obtain virgin polyethylene 2. The resulting virgin polyethylene 2 had an MMI of 0.20 g / 10 min and a density of 959 kg / m³. 3 The molecular weight distribution was 21.4. For virgin polyethylene 2, the intrinsic viscosity and molecular weight were measured using the aforementioned analytical method combining a viscosity detector and GPC, and a Mark-Houwink-Sakurada plot was created. Since the plot for virgin polyethylene 2 lies below the plot for linear polyethylene, it was shown that virgin polyethylene 2 has long-chain branching. At this time, the branching index (g') value was 0.65.
[0078] [Virgin polyethylene 3 manufacturing] (1) Synthesis of raw material (a-1) 2,000 mL of hexane solution of 1 mol / L Mg6(C4H9)12AL(C2H5)3 (equivalent to 2,000 mmol of magnesium and aluminum) was charged into an 8 L stainless steel autoclave that had been thoroughly purged with nitrogen. 146 mL of 5.47 mol / L n-butanol hexane solution was added dropwise over 3 hours while stirring at 50°C, and after completion, the line was washed with 300 mL of hexane. Stirring was then continued at 50°C for 2 hours. After the reaction was complete, the mixture was cooled to room temperature and used as the starting material (a-1). The magnesium concentration of starting material (a-1) was 0.704 mol / L.
[0079] (2)(A-1) Synthesis of the support 1,000 mL of a hexane solution of 1 mol / L hydroxytrichlorosilane was charged into an 8 L stainless steel autoclave that had been thoroughly purged with nitrogen. 1,340 mL of a hexane solution of the organomagnesium compound (a-1) (equivalent to 943 mmol of magnesium) was added dropwise over 3 hours at 50°C, and the reaction was continued for another hour at 50°C with stirring. After the reaction was complete, the supernatant was removed and washed four times with 1,800 mL of hexane to obtain the (A-1) support.
[0080] (3) Preparation of solid catalyst [A] A slurry containing 500 g of the above solid (A-1) was heated to 50°C while stirring, and 1078 mL of a 1 mol / L n-butyl alcohol solution in n-hexane was added. The mixture was then stirred and reacted at 50°C for 1 hour to obtain solid slurry (A-1b). The solid slurry (A-1b) was kept at 50°C, and 431 mL of a 1 mol / L n-hexane solution of diethylaluminum chloride was added under stirring and allowed to react for 1 hour. After the reaction was complete, the supernatant was removed and washed twice with 2,000 mL of n-hexane to obtain solid slurry (A-1c). This solid slurry (A-1c) was kept at 50°C, and 67 mL of a 1 mol / L n-hexane solution of diethylaluminum chloride and 67 mL of a 1 mol / L n-hexane solution of titanium tetrachloride were added and the mixture was reacted for 1 hour. Subsequently, 202 mL of a 1 mol / L n-hexane solution of diethylaluminum chloride and 202 mL of a 1 mol / L n-hexane solution of titanium tetrachloride were added, and the reaction was continued for another hour. After the reaction was complete, the supernatant was removed, and the mixture was washed four times with 2,000 mL of n-hexane while maintaining the internal temperature at 50°C to obtain solid catalyst component [A] as a hexane slurry solution.
[0081] (4) Polymerization A two-stage polymerization was performed using a continuous slurry polymerization method with two polymerization tanks connected in series, utilizing a polymerization catalyst containing the solid catalyst component [A] obtained above and a mixture of triisobutylaluminum and diisobutylaluminum hydride (9:1) (component [B]). The comonomer used was 1-butene. In the first stage polymerization tank, only ethylene was supplied as the monomer, at a temperature of 85°C and a pressure of 9.5 kg / cm². 3 G. Polymerization was carried out at a hydrogen concentration of 72%, and in the second stage, ethylene and 1-butene were supplied at 70°C and 2.8 kg / cm³. 3 Polymerization was carried out at a hydrogen concentration of 1.7% and a 1-butene concentration of 11.5%. The production ratio of the low molecular weight polyethylene resin component (D) consisting of ethylene homopolymer obtained in the first polymerization tank was set to 52 wt%, and the production ratio of the high molecular weight polyethylene resin component (E) consisting of copolymer obtained in the second polymerization tank was set to 48 wt%, resulting in an MMI of 0.48 g / 10 min and a density of 950 kg / m³. 3 I obtained the powder.
[0082] (5) Production of virgin polyethylene 3 The powder obtained by the above polymerization was dried and extruded into pellets using a Japan Steel Works TEX-44 extruder (screw diameter 44 mm, L / D = 42) at a set temperature of 200°C and a resin extrusion rate of 40 kg / hr. The pellets had an MMI of 0.22 g / 10 min and a density of 950 kg / m³. 3 The obtained virgin polyethylene 3 was analyzed using the aforementioned viscosity detector and GPC method to measure its intrinsic viscosity and molecular weight, and a Mark-Houwink-Sakurada plot was created, revealing that it did not possess a long-chain branched structure. At this time, the branching index (g') value was 1.0.
[0083] [Manufacturing of Virgin Polyethylene 4] Low-density polyethylene resin was polymerized in a tube reactor using a high-pressure method with an average polymerization temperature of 249°C, a polymerization pressure of 240 MPa, 0.3 mol% propylene relative to ethylene as a chain transfer agent, and t-butyl peroctoate and di-t-butyl peroxide as peroxide initiators. The molten resin obtained by the above polymerization was extruded and granulated in a Japan Steel Works TEX-44 extruder (screw diameter 44 mm, L / D = 42) at a set temperature of 200°C and a resin extrusion rate of 40 kg / hr to obtain pellets. The resulting virgin polyethylene 4 had an MMI of 1.30 g / 10 min and a density of 918 kg / m³. 3 The molecular weight distribution was 66.3. For virgin polyethylene 4, the intrinsic viscosity and molecular weight were measured using the aforementioned analytical method combining a viscosity detector and GPC, and a Mark-Houwink-Sakurada plot was created. Since the plot of virgin polyethylene 4 lies below the plot of linear polyethylene, it was shown that virgin polyethylene 1 has long-chain branching. At this time, the branching index (g') value was 0.40.
[0084] [Recycled polyolefins] RBP-PE(K) manufactured by Toyama Environmental Services Co., Ltd. was used. The polyethylene content in the recycled polyolefin was 90% by mass.
[0085] [Antioxidant] We used the AO-50F manufactured by ADEKA Corporation.
[0086] [Examples 1-7, Comparative Examples 1-2] [Manufacturing of polyolefin resin compositions] A twin-screw extruder (Toshiba Machine Co., Ltd. TEM26SS) was used in the direction of the raw material flow. The cylinder temperature was set to 200°C, the screw rotation speed to 200 rpm, and the discharge rate to 20 kg / h. In addition, openings were provided in the cylinder block located in the center of the extruder and in the cylinder block immediately before the die, and residual volatile components and oligomers were removed by vacuum suction. The raw materials (units in the table are "mass%" for polyolefins and "ppm" for antioxidants) were supplied according to the composition listed in Table 1 below and melt-kneaded. The strands extruded from the tip of the extruder die were cooled in a stainless steel strand bath filled with cooling water. Afterward, they were cut with a strand cutter to obtain resin composition pellets. Table 1 shows the MI and evaluation results of various properties of the obtained polyolefin resin composition.
[0087] [Table 1] *In the table, "Recycled" refers to recycled polyolefin, "Virgin 1" refers to virgin polyolefin 1, "Virgin 2" refers to virgin polyolefin 2, "Virgin 3" refers to virgin polyolefin 3, and "Virgin 4" refers to virgin polyolefin 4. [Industrial applicability]
[0088] The polyolefin resin composition of the present invention has industrial applicability as a raw material for various molded articles, containers, and packaging applications.
Claims
1. A polyolefin resin composition comprising a recycled polyolefin, a virgin polyolefin, and an antioxidant, The content of the recycled polyolefin is 30% by mass or more and 99% by mass or less based on the total amount of the recycled polyolefin and the virgin polyolefin, The content of the virgin polyolefin is 1% by mass or more and 70% by mass or less based on the total amount of the recycled polyolefin and the virgin polyolefin, The content of the antioxidant is 100 ppm or more and 5000 ppm or less based on the entire polyolefin resin composition, A polyolefin resin composition, wherein the virgin polyolefin has a long chain branched structure.
2. The polyolefin resin composition according to claim 1, wherein the recycled polyolefin is a polyolefin derived from recycled materials collected from the market.
3. The polyolefin resin composition according to claim 1 or 2, wherein the content of polyethylene contained in the recycled polyolefin is 50 mass% or more based on the recycled polyolefin.
4. The polyolefin resin composition according to any one of claims 1 to 3, wherein the virgin polyolefin comprises a polyolefin obtained by polymerization using a chromium-based catalyst or polymerization by radicals.
5. The polyolefin resin composition according to any one of claims 1 to 4, wherein the virgin polyolefin has an MMI of 0.10 g / 10 min or more and 20 g / 10 min or less.
6. The density of the virgin polyolefin is 945 kg / m 3 More than 965kg / m 3 The polyolefin resin composition according to any one of claims 1 to 5, wherein:
7. The polyolefin resin composition according to any one of claims 1 to 6, wherein the virgin polyolefin is polyethylene.
8. The polyolefin resin composition according to any one of claims 1 to 7, wherein the content of the antioxidant is 2000 ppm or more and 5000 ppm or less based on the entire polyolefin resin composition.
9. The polyolefin resin composition according to any one of claims 1 to 8, having an MI of 0.1 g / 10 min or more and 10 g / 10 min or less.
10. The polyolefin resin composition according to any one of claims 1 to 9, which is for blow molding.