Photodetector, modulator, semiconductor device and semiconductor device

JP2023517900A5Active Publication Date: 2024-11-19BLACK SEMICON GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2022554184
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-03-09
Filing Date
2021-02-23
Publication Date
2024-11-19
Estimated Expiration
2041-02-23
Patent Text Reader

Abstract

The present invention relates to a photodetector 3, comprising a longitudinal cross section 12 of a waveguide 11, which includes or is formed by at least two longitudinally extending waveguide segments 12a, 12b that are substantially parallel to one another, and an active element 13 that overlaps the longitudinal cross section 12 of the waveguide 11 and includes or consists of at least one material that absorbs electromagnetic radiation of at least one wavelength and generates an electrical optical signal as a result of said absorption. The waveguide segments 12a, 12b are preferably laterally spaced apart from one another so as to form a gap 14 extending between them. The two waveguide segments 12a, 12b are each at least partially in contact on at least one side, in particular the side facing the active element 13, with a gate electrode 15a, 15b, preferably including or consisting of silicon.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to photodetectors and modulators. Further, the present invention relates to a semiconductor device having a chip and at least one photodetector and / or modulator, and a semiconductor device having a wafer and at least one photodetector and / or modulator.

Background Art

[0002] Electro-optic elements, such as photodetectors or modulators (electro-optic modulators), are known from the prior art. The electro-optic element includes a waveguide having several waveguide segments that extend in the longitudinal direction and at least substantially parallel to each other, or a longitudinal cross-section thereof. In the case of a photodetector, it includes one graphene film as an active element, and in the case of a modulator, it includes two graphene films as active elements. Such are disclosed, for example, in U.S. Patent No. 9,893,219.

Summary of the Invention

Problems to be Solved by the Invention

[0003] Known photodetectors and modulators have their own proven principles. However, there is a desire for further, alternatively designed photodetectors and modulators that can be manufactured with reasonable effort and are characterized by an optimal operating mode.

[0004] Therefore, an object of the present invention is to provide alternatively designed photodetectors and modulators that meet these requirements.

[0005] This object is solved for the photodetector by the means according to claims 1 and 6, and for the modulator by the means according to claims 9, 10 and 11.

[0006] According to a first aspect of the present invention, the photodetector comprises a longitudinal cross-section of a waveguide including or formed by two longitudinally extending waveguide segments that are at least substantially parallel to each other, and an active element including or made of at least one material that overlaps the longitudinal cross-section of the waveguide and absorbs electromagnetic radiation of at least one wavelength and generates an electro-optical signal as a result of the absorption, wherein the two waveguide segments are preferably spaced apart from each other in the transverse direction to form a gap extending between them, and each of the two waveguide segments is at least partially in contact with a gate electrode, preferably containing or made of silicon, on at least one side, particularly the side facing the active element.

[0007] A method for manufacturing such a photodetector of the present invention includes, for example, the steps of: fabricating a waveguide material by preferably depositing it on a film provided in contact or non-contact on a wafer; fabricating a gate electrode material, preferably silicon, by particularly depositing it; performing structuring to obtain two waveguide segments having a gap and a gate electrode; and providing an active element.

[0008] The gate electrode enables the realization of a pn junction in the active element during operation. By positioning the pn junction in the optical mode region, optimal overlap between the absorbing material and the active region of the photodetector is achieved.

[0009] In an advantageous embodiment, each gate electrode contacts the upper surface of the waveguide segment on its underside and the lower surface of a dielectric film provided between the active element and the waveguide segment on its upper side. The dielectric film comprises or is composed of at least one dielectric material. Suitable dielectric materials have been proven to be, for example, silicon dioxide (SiO2) and aluminum oxide (Al2O3). The term “dielectric” may also be used instead of “dielectric material.” The dielectric film may also be called a gate dielectric.

[0010] The active element may be placed on top of the dielectric film beforehand or afterward, and it may be manufactured on top of it beforehand or afterward.

[0011] In a preferred embodiment, the dielectric coating can be characterized by a roughness on its upper surface in the range of 1.0 nm RMS to 0.1 nm RMS, particularly 0.6 nm RMS to 0.1 nm RMS, preferably 0.4 nm RMS to 0.1 nm RMS. RMS represents the root mean square. An upper surface having this range of roughness has proven particularly suitable when the active element is provided on the upper surface of the dielectric coating, especially in the form of deposition.

[0012] The thickness of the dielectric coating may be, for example, in the range of 10 to 20 nm.

[0013] Preferably, the gate electrode comprises or is composed of a material that is transparent to and / or conductive to electromagnetic radiation of at least one wavelength, preferably at least one wavelength range.

[0014] More preferably, the gate electrode comprises or is composed of at least one material that is transparent to electromagnetic radiation at wavelengths of 850 nm and / or 1310 nm and / or 1550 nm. In particular, it is preferable that it be transparent to electromagnetic radiation in the wavelength range of 800 nm to 900 nm and / or 1260 nm to 1360 nm (the so-called original band or abbreviated as the O band) and / or 1360 nm to 1460 nm (the so-called extended band or abbreviated as the E band) and / or 1460 nm to 1530 nm (the so-called short band or abbreviated as the S band) and / or 1530 nm to 1565 nm (the so-called conventional band or abbreviated as the C band) and / or 1565 nm to 1625 nm (the so-called long band or abbreviated as the L band). These bands are known in the field of communications engineering.

[0015] Such materials are preferentially applied to gate electrode materials used in manufacturing processes.

[0016] Silicon has proven to be a particularly suitable material for gate electrodes. Polysilicon can also be used. Indium tin oxide (ITO) may also be considered. The materials constituting the gate electrode can also be doped.

[0017] Each gate electrode is preferably a coating provided on each waveguide segment of the longitudinal cross-section of the waveguide facing the active element, and more preferably a coating fabricated on or on each waveguide segment.

[0018] Furthermore, the gate electrode is either fabricated beforehand or afterward by depositing a coating material, particularly by chemical vapor deposition (CVD), preferably low-pressure chemical vapor deposition (LPCVD) and / or plasma-enhanced chemical vapor deposition (PECVD) and / or physical vapor deposition (PVD).

[0019] There are various prior art chemical vapor deposition processes, all of which can be used in the context of the present invention. What they all have in common is that they typically involve a chemical reaction of an introduced gas, resulting in the deposition of the desired material.

[0020] Furthermore, with regard to physical vapor deposition, all types known in the prior art may be used. Purely as examples, electron beam deposition, which melts and vaporizes a material using an electron beam; thermal deposition, which heats to its melting point and vaporizes it onto a target substrate; and sputter deposition, which knocks out atoms from a material support using plasma and deposits them onto a target substrate.

[0021] Alternatively, or in addition to the above deposition processes, atomic layer deposition (ALD) can be used to obtain the gate electrode. In this method, an insulating or conductive material (dielectric, semiconductor, or metal) is continuously deposited in atomic layers. A transfer process can also be used.

[0022] Furthermore, each of the two gate electrodes is associated with a connecting element that contacts them, and one of the connecting elements may extend through one of the waveguide segments. Following deposition, an appropriate structuring process may be performed, for example, lithography and / or etching. The connecting elements are preferably Vertical Interconnect Accesses, abbreviated as VIAs. VIAs are typically defined by lithography and etched by dry chemical etching, particularly reactive ion etching (abbreviated as RIE). They are then preferably metallized, and the metallized surface is structured by CMP (Damascene process) or lithography and RIE.

[0023] Reactive ion etching is a dry etching process, according to which selective and directional etching of the substrate surface is typically achieved by a special gaseous chemical substance excited to form a plasma. A resist mask can be used to protect the parts that are not to be etched. The etching chemistry and process parameters usually determine the selectivity of the process, i.e., the etching rates of different materials. This property is important for limiting the etching process in depth and for defining the coatings separately from each other.

[0024] For the sake of convenience, the connecting element comprises or is composed of at least one conductive material, especially a metal such as copper and / or aluminum and / or tungsten.

[0025] In another advantageous embodiment, further, the active element is provided to at least partially, especially laterally, overlap with respect to the two waveguide segments and the gap located at least in part therebetween. The lateral direction should be understood, for the sake of convenience, as the direction orthogonal to the longitudinal direction of the cross-section of the waveguide.

[0026] According to a second aspect of the present invention, there is provided an optical detector comprising a longitudinal cross-section of a waveguide and an active element comprising or consisting of at least one material that absorbs electromagnetic radiation of at least one wavelength and generates an electro-optical signal as a result of the absorption, wherein two carrier elements are arranged spaced apart on both sides of the longitudinal cross-section of the waveguide so as to form two gaps, the two gaps contain no material, and the active element preferably laterally overlaps at least a part of the longitudinal cross-section of the waveguide, the two gaps and the two carrier elements. Preferably, the two carrier elements are laterally spaced apart from the longitudinal cross-section.

[0027] The method according to the invention for manufacturing such a photodetector comprises, for example, the step of preferably depositing a waveguide material on a wafer or on a coating provided on the wafer, the step of structuring to obtain two gaps as well as longitudinal cross-sections of the waveguide and the carrier element, and the step of providing an active element on top of the longitudinal cross-sections of the waveguide and the carrier element.

[0028] The gaps that do not contain material are provided, in particular, by regions where material is removed by an etching process and then not provided, for example, by depositing new material. They can be filled with air or another gas or can be made into a vacuum. However, there is no solid substance in them. The vacuum should preferably be understood as a vacuum space obtained, for example, by pumping.

[0029] In a preferred embodiment, the active element is located on top of the longitudinal cross-section of the waveguide facing the active element and / or on top of the carrier element facing the active element.

[0030] The carrier element may be of the same material as the longitudinal cross-section of the waveguide, which is to be understood as exemplary. For example, TiO2 and / or Si have proven to be materials suitable for the carrier element. Any other material suitable for the waveguide can also be considered.

[0031] The active element may include, or be composed of, at least one material capable of absorbing electromagnetic radiation at wavelengths of 850 nm and / or 1310 nm and / or 1550 nm, and generating an optical signal as a result of the absorption. Preferably, the material of the active element is capable of absorbing electromagnetic radiation in the wavelength range of 800 nm to 900 nm and / or 1260 nm to 1360 nm (the so-called original band or abbreviated as the O band) and / or 1360 nm to 1460 nm (the so-called extended band or abbreviated as the E band) and / or 1460 nm to 1530 nm (the so-called short band or abbreviated as the S band) and / or 1530 nm to 1565 nm (the so-called conventional band or abbreviated as the C band) and / or 1565 nm to 1625 nm (the so-called long band or short band), and generating an optical signal as a result of the absorption.

[0032] It has been proven that at least one material of the active element, which absorbs electromagnetic radiation of at least one wavelength and generates an electrical optical signal as a result of the absorption, is particularly preferable to be graphene and / or at least one dichalcogenide, in particular two-dimensional transition metal dichalcogenides and / or heterostructures of two-dimensional materials and / or germanium and / or at least one electro-optic polymer and / or silicon and / or at least one compound semiconductor, in particular at least one III-V semiconductor and / or at least one II-VI semiconductor.

[0033] In particular, photodetectors can be useful for converting signals from light to the electronic world.

[0034] A modulator, in particular an electro-optic modulator, is provided, comprising a longitudinal section of a waveguide including or formed by at least four longitudinally extending waveguide segments substantially parallel to each other, and two active elements or one such active element and one electrode comprising or made of at least one material whose refractive index changes as a function of voltage and / or in the presence of charge and / or an electric field, wherein one of the lower waveguide segments is positioned between the two active elements or between the one active element and the one electrode, one of the upper and lower middle waveguide segments is positioned above the two active elements or above the one active element and the one electrode, the remaining upper two waveguide segments are positioned above the upper and lower middle waveguide segment, and the remaining upper two waveguide segments are preferably spaced apart from each other laterally so as to form a gap extending between them.

[0035] In particular, there may be a sandwich-like structure that includes an active element or electrode, followed by the lower waveguide segment in the longitudinal cross-section of the waveguide, then a second active element or electrode, followed by the middle waveguide segment in the longitudinal cross-section of the waveguide, and then the two upper waveguide segments in the longitudinal cross-section of the waveguide, extending from the bottom to the top.

[0036] A method for manufacturing such a modulator according to the present invention includes, for example, the steps of: providing an active element or electrode in contact with a wafer, or in contact with or without contact with a coating provided on a wafer; obtaining a lower waveguide segment by preferably depositing a waveguide material; further providing an active element or electrode above the lower waveguide segment; obtaining an intermediate waveguide segment by preferably depositing a waveguide material; and obtaining an upper waveguide segment and the gap therebetween by preferably depositing a waveguide material and subsequently structuring it.

[0037] An element, segment, or coating is positioned above or below another element, segment, or coating. Here, the element, segment, or coating may be directly above or below the other element, segment, or coating, for example, in contact with the other element, segment, or coating above or below, or at least one other element, segment, or coating may be positioned between them. This applies to photodetectors and modulators according to all aspects of the present invention.

[0038] According to a fourth aspect of the present invention, a longitudinal cross-section of a waveguide comprising or formed by at least five longitudinally extending waveguide segments substantially parallel to each other, and two active elements or one such active element and one electrode comprising or made of at least one material whose refractive index changes as a function of voltage and / or in the presence of charge and / or an electric field, wherein the two lower waveguide segments are positioned below the two active elements or below the one active element and the one electrode, and these A modulator, in particular an electro-optic modulator, is provided, characterized in that the waveguide segments are preferably spaced apart from each other laterally to form a gap extending between them, with one upper and lower intermediate (12c) of the waveguide segments positioned between the two active elements or between one active element and one electrode, the other upper and lower intermediate of the waveguide segments positioned above the two active elements or above one active element and one electrode, and the upper one of the waveguide segments positioned above the other upper and lower intermediate of the waveguide segments.

[0039] The upper waveguide segment preferably has a lateral distance smaller than the lateral distance between the other waveguide segments. The lateral distances between the two lower segments and the two intermediate segments may be multiples of the lateral distance between the upper segments.

[0040] A method for manufacturing such a modulator according to the present invention includes, for example, the steps of: fabricating by depositing waveguide material particularly in contact with a wafer or in contact with a coating provided on or without a wafer; structuring to obtain two lower waveguide segments and the gap between them; providing active elements or electrodes above them; fabricating by preferably depositing waveguide material to obtain a first intermediate waveguide segment; providing further active elements or electrodes above the first intermediate waveguide segment; fabricating by preferably depositing waveguide material to obtain a second intermediate waveguide segment; and fabricating by preferably depositing waveguide material to obtain an upper waveguide segment, preferably performing subsequent structuring.

[0041] According to a fifth aspect of the present invention, a longitudinal cross-section of a waveguide includes or is formed by at least six longitudinally extending waveguide segments substantially parallel to each other, and two active elements or one such active element and one electrode, which include or are made of at least one material whose refractive index changes as a function of voltage and / or in the presence of charge and / or an electric field, wherein the two lower waveguide segments are positioned below the two active elements or below the one active element and one electrode, forming a gap extending between them. A modulator, in particular an electro-optic modulator, is provided, which is preferably spaced apart from each other laterally, such that one upper and lower intermediate waveguide segment is positioned between two active elements or between one active element and one electrode, another upper and lower intermediate waveguide segment is positioned above two active elements or above one active element and one electrode, and the remaining two upper waveguide segments are positioned above the other upper and lower intermediate waveguide segment, thereby forming a gap extending between them.

[0042] A method of the present invention for fabricating such a modulator includes, for example, the steps of: fabricating by depositing waveguide material particularly in contact with a wafer or in contact with a coating provided on or without a wafer; structuring to obtain two lower waveguide segments and the gap between them; providing active elements or electrodes above them; fabricating by preferably depositing waveguide material to obtain a first intermediate waveguide segment; providing further active elements or electrodes above the first intermediate waveguide segment; fabricating by preferably depositing waveguide material to obtain a second intermediate waveguide segment; and fabricating by preferably depositing waveguide material to obtain two upper waveguide segments and the gap between them, preferably performing subsequent structuring.

[0043] Modulators (electro-optic modulators) can be used, in particular, for optical signal coding. Modulators can also be designed as ring modulators.

[0044] In the case of a modulator comprising two active elements, it is preferable that the two active elements are spaced apart from each other and offset from each other such that one of the two active elements is partially located above the other, forming an overlapping region. In a preferred embodiment, when the modulator comprises only one active element and one (conventional) electrode, it is also preferable that the active element and the electrode are spaced apart from each other and offset from each other such that one of the active elements is partially located above the other, forming an overlapping region.

[0045] In other words, it is preferable that portions of one active element and portions of the other active element or electrode are aligned or overlap without contacting each other. Preferably, in at least the overlapping region, the two active elements or one active element and one electrode (or at least portions thereof) extend at least substantially parallel to each other.

[0046] The overlapping region is particularly preferably located above or below the gap, or provided therein, in alignment with the gap. Thus, optical modes (slot modes) can be guided into the slot (gap) between two waveguide segments having high electric field strength. At the upper and lower edges of the slot, a portion of the optical modes lies outside the slot. In these regions, the optical modes can interact efficiently with particularly effective optical materials.

[0047] When two gaps are present, the overlapping region is positioned above one gap and below the other gap. The two gaps and the overlapping region or parts thereof can be aligned, which has proven particularly favorable. With two gaps, one positioned above the other, the proportion of optical modes in the region between the gaps is particularly high, especially compared to an arrangement with only one gap, which allows for particularly efficient interaction with electro-optic materials.

[0048] Furthermore, the exact gap formed between two spaced waveguide segments may be provided either before or after the two active elements or above one active element and one electrode. Alternatively or additionally, the exact gap formed between two spaced waveguide segments may be provided below the two active elements or below one active element and one electrode.

[0049] In a particularly advantageous embodiment, the lateral distance of the overlapping region corresponds to a range of 0.8 to 1.8 times, preferably 1.0 to 1.5 times, the lateral distance of the gap (at least one of the gaps).

[0050] It should be understood that a material changing its refractive index is, in particular, changing its dispersion (especially its refractive index) and / or its absorption. Dispersion or refractive index is usually given by the real part of the complex refractive index, and absorption is given by the imaginary part of the complex refractive index. Materials whose refractive index changes as a function of voltage and / or charge and / or electric field are understood herein, in particular, to be materials characterized by the Pockels effect and / or the Franz-Keldysh effect and / or the Kerr effect. Furthermore, materials characterized by plasma dispersion effects are also considered to be such materials.

[0051] As at least one material for at least one active element in which the refractive index changes as a function of voltage and / or charge and / or electric field, graphene, preferably chemically modified graphene and / or at least one dichalcogenide, in particular two-dimensional transition metal dichalcogenides and / or heterostructures of two-dimensional materials and / or germanium and / or lithium niobate and / or at least one electro-optic polymer and / or silicon and / or at least one compound semiconductor, in particular at least one III-V semiconductor and / or at least one II-VI semiconductor has proven to be particularly suitable.

[0052] Graphene has proven to be a particularly suitable material for active elements in all five aspects of the present invention.

[0053] Electro-optic polymers are polymers characterized in particular by having a strong linear electro-optic coefficient (Pockels effect). A strong linear electro-optic coefficient is understood to be preferably at least 150 pm / V, and preferably at least 250 pm / V. This is at least about five times that of lithium niobate.

[0054] There are different types of chalcogenides. In the context of this invention, transition metal dichalcogenides as two-dimensional materials such as MoS2 or WSe2 have proven particularly suitable.

[0055] Lithium niobate and electro-optic polymers are based on electro-optics, and it should be noted that they exhibit the Pockels effect, i.e., the change in refractive index caused by an electric field (for example, as the Pockels effect is used in Pockels cells). In germanium, it is the Franz-Keldisch effect, i.e., the change in optical properties caused by an electric field shifting the valence electrons and conduction band edges relative to each other. These effects are electric field-based effects. In the case of silicon or graphene, there is a charge carrier-based plasma dispersion effect, i.e., charge carriers (electrons or holes) are brought into the optical mode region (there are charged capacitors in an array or diodes with depleted and enriched junctions). The refractive index (real part of the refractive index) and absorption (imaginary part of the refractive index, leading to free carrier absorption) change with the charge carrier concentration.

[0056] III-V semiconductors are compound semiconductors composed of elements from Group III and Group V, while II-VI semiconductors are compound semiconductors composed of elements from Group II or Group XII and Group VI.

[0057] Many materials are characterized by both the fact that their refractive index changes as a function of voltage and / or the presence of charge and / or the electric field, and the fact that they absorb electromagnetic radiation of at least one wavelength, producing an electrical optical signal as a result of the absorption. Graphene, for example, is one such material. Therefore, graphene is suitable for active elements in both photodetectors and modulators. This also applies to dichalcogenides such as two-dimensional transition metal dichalcogenides, heterostructures of two-dimensional materials, germanium, silicon, and compound semiconductors, particularly III-V and / or II-VI semiconductors. For example, lithium niobate is generally only suitable for modulators because, being transparent, it does not match the absorption characteristics and is therefore unsuitable for photodetectors.

[0058] A material that absorbs electromagnetic radiation of at least one wavelength and generates an electrical optical signal as a result of the absorption, and / or a material whose refractive index changes as a function of voltage and / or charge and / or electric field, may also be called an electro-optical active material. In other words, an active element may be said to contain or consist of at least one electro-optical active material.

[0059] At least one active element may be provided in the form of a film. The film is preferably characterized by a transverse elongation that is significantly greater than its thickness, in a manner known by itself. At least one active element may be further characterized by a square or rectangular cross-section.

[0060] At least one active element may further include, or consist of, one or more layers or coatings of at least one material that changes and / or absorbs refractive indices. In particular, at least one active element may be formed as a film comprising several layers or coatings of one or other materials.

[0061] Graphene, preferably a chemically modified graphene film, or a dichalcogenide-graphene heterostructure comprising or consisting of at least one layer of graphene and at least one layer of dichalcogenide, or a combination of at least one layer of boron nitride and at least one layer of graphene, has proven to be particularly preferable.

[0062] The active element may, for example, include one or more silicon films, or be provided by one or more silicon films. In this case, in particular, one or more active elements or portions thereof can form a waveguide (cross-section).

[0063] The active element may be further doped, or may have doped portions or regions, for example, it may be p-doped and / or n-doped, or it may include portions or regions corresponding to p-doping and / or n-doping. In addition to the p-doped and n-doped regions, preferably an intermediate undoped region may be present or provided. This is also called a pin junction, where i (intrinsic) represents intrinsic, i.e., undoped.

[0064] In relation to the manufacturing of active elements, the same process described above as in relation to gate electrodes can be used.

[0065] This also includes a transfer process. In other words, each active element may not be manufactured monolithically on a film, for example, but may be manufactured separately and transferred, or in other words, transferred. The graphene transfer process is described in Li et al.'s paper "Large-Area Synthesis of High-Quality and Uniform Graphene Films on Copper Foils" Science 324, 1312, (2009) and Bae et al.'s paper "Roll-to-roll production of 30-inch graphene films for transparent electrodes" Nature Nanotech 5, 574-578 (2010), or in the paper on lithium niobate "Integrated lithium niobate electro-optic modulators operating at CMOS-compatible voltages", Nature volume 562, pages 101104 (2018), or in the paper on GaAs "Transfer print techniques for heterogeneous integration of photonic components", Progress in Quantum Electronics, Volume 52, March 2017, Pages 1-17. One of these processes can also be used in the context of the present invention to obtain coatings or films of one or more graphene or LiNbO or GaAs. Following the transcription process, structuring can be performed.

[0066] A passivation coating and / or cladding may be further provided on the upper side, preferably in contact with at least one active element. The cladding is particularly suitable or designed to reduce refractive index contrast somewhat, so that the roughness on the sidewalls does not usually have a very strong effect, allowing losses to return into the waveguide. The passivation coating preferably serves the purpose of protecting the device or circuit from environmental influences, particularly water. The passivation coating may consist of dielectric materials, for example, aluminum oxide (Al2O3) and silicon dioxide (SiO2) have proven particularly suitable.

[0067] The upper final passivation film advantageously has openings or relays to the lower contacts to enable electrical connection. These openings or relays in the passivation film can be obtained, for example, by lithography and / or etching, particularly reactive ion etching.

[0068] Each active element may, in each case, be connected to a contact or contact element on one or the other side. The contact or contact element may contact a connecting element, in particular a via. Through the connecting element, for example, a connection can be achieved from the FEOL of a chip or wafer to one or more integrated electronic components. The term "connected" is intended to mean an electrical connection.

[0069] In particular, in the case of a photodetector having only one active element, it should be noted that this active element is preferably in contact with two contacts or contact elements located on opposite sides, and in the case of a modulator having two active elements or one active element and one electrode, these are each made to be in contact with a contact or contact element. This contact is preferably made in an edge region or end away from the region where they at least partially overlap.

[0070] An active element or at least one of a group of active elements is conveniently positioned so as to be at least partially exposed to the evanescent field of electromagnetic radiation guided within the waveguide, with respect to the longitudinal cross-section of the waveguide. Preferably, at least one of the active elements positioned at a distance of, for example, 10 nm from the longitudinal cross-section of the waveguide is positioned at a distance of 50 nm or less, more preferably 30 nm or less.

[0071] The active element or at least one active element is more preferably characterized by a longitudinal distance in the range of 5 to 500 micrometers (μm).

[0072] Furthermore, the active element or at least one of the active elements may extend over and / or into the longitudinal cross-section of the waveguide, or in the latter case, for example, between those two segments, at least in portion.

[0073] In a further advantageous embodiment, an active element or at least one active element is positioned in contact with or without contact with the upper side of the waveguide, preferably following a trapezoidal shape, in a region of the longitudinal cross-section of the waveguide where the cross-section is at least substantially trapezoidal. Alternatively or additionally, an active element or at least one active element is positioned in contact with or without contact with the upper side of the planarizing coating, preferably following a trapezoidal shape, in a region of the planarizing coating where the cross-section is at least substantially trapezoidal as viewed from the cross-section.

[0074] In a waveguide, some electromagnetic radiation, particularly light, is guided outside the waveguide as evanescent light. The waveguide interface is dielectric, and therefore the intensity distribution is described by boundary conditions according to Maxwell, with exponential decay. If an electro-optically active material, such as graphene, is placed on or near the waveguide of the evanescent field, photons can interact with the material, especially graphene.

[0075] Graphene exhibits four effects that result in photocurrents. One is the bolometric effect, where absorbed energy increases the resistance of graphene and decreases the applied DC current. This change in DC current is a light signal. Another effect is photoconductivity. Absorbed photons increase the charge carrier concentration, and the additional charge carriers, due to the proportionality of resistance to charge carrier concentration, decrease the resistance of graphene. The applied DC current increases, and this change is a light signal. Another effect is the thermoelectric effect, where, due to the different Seebeck coefficients in the p and n regions, a thermoelectric voltage arises from the pn junction and the temperature gradient at this junction. The temperature gradient arises from the energy of the absorbed light signal. This thermoelectric voltage is a signal. The fourth effect is due to the separation of electron-hole pairs excited at the pn junction. The resulting photocurrent is a signal.

[0076] In the case of a modulator, as described above, appropriately insulated electrical control electrodes and active elements for this purpose may include or be constructed from at least one material, particularly graphene, whose refractive index changes as a function of voltage, charge, or electric field, and the electrodes may also be made of the corresponding material, particularly graphene, so that when in operation, the two active elements come together in an evanescent field to perform electro-optical functions, for example, graphene can change its optical properties with a control voltage. In the particularly advantageous case of a graphene-dielectric-graphene array, capacitance is generated and the two graphene films influence each other. The voltage charges the capacitance consisting of the graphene electrodes forming the two active elements, and electrons occupy states in the graphene. As a result, the Fermi energy (the energy of the last occupied state in the crystal) shifts to a higher energy (or a lower energy due to symmetry). When the Fermi energy reaches half the energy of the photon, absorption no longer occurs because the free states necessary for the absorption process are already occupied at the correct energy. Therefore, in this state, absorption is prohibited, and the graphene is transparent. By changing the voltage, graphene is switched between absorbing and transparent states. The continuously shining laser beam is modulated in intensity and can therefore be used for information transmission. Similarly, the real part of the refractive index changes with the control voltage. By changing the voltage, the phase position of the laser can be modulated through the changing refractive index, and thus phase modulation can be achieved. Preferably, the phase modulation operates in a range where all states are occupied until they exceed half the photon energy, so that graphene is transparent, the real part of the refractive index shifts significantly, and the change in absorption plays a small role.

[0077] Furthermore, the following can be applied in relation to both the photodetectors according to the first and second aspects of the present invention and the modulators according to the third, fourth, and fifth aspects.

[0078] Waveguides or their longitudinal sections are elements or configurations that guide electromagnetic waves, particularly light. For guiding electromagnetic waves, wavelength-dependent sections of a material that are optically transparent at least to this wavelength and distinguishable from adjacent materials that are also transparent to this wavelength are conveniently provided by refractive index contrast. If the refractive index of the surrounding material is low, light is guided to a region of higher refractive index. In the specific case of slit modes, two regions of high refractive index are separated from a region of low refractive index that is narrow with respect to wavelength, and light is guided to the region of low refractive index. Low sidewall roughness is advantageous to achieve low loss due to scattering.

[0079] Generally, one or more waveguides are provided, for example, on a chip or wafer. Part of the photodetector or modulator according to the present invention is usually only the longitudinal portion of the photodetector or modulator, which is the longitudinal portion extending beneath the active element of the latter. Of course, it is not excluded that the waveguide along its entire length may be considered part of the photodetector or modulator according to the present invention. In other words, in addition to the longitudinal cross-section of the waveguide, particularly the portion extending beneath the active element, such a waveguide may also include the rest of the latter.

[0080] Regarding the dimensions of the waveguide, for example, the following may apply: The thickness is preferably in the range of 150 nanometers (nm) to 10 micrometers (μm). In particular, the width and length of the waveguide may be in the range of 100 nanometers and 10 micrometers, respectively.

[0081] The waveguide may be characterized, for example, by a rectangular or square cross-section and formed as a strip waveguide applied to the longitudinal cross-section of such a waveguide. Alternatively or additionally, the waveguide may be formed as a ridge waveguide having a T-shaped cross-section. Furthermore, alternatively or additionally, the waveguide may be provided by a slot waveguide.

[0082] The waveguide or longitudinal section of such a waveguide may include several parts or segments within the section, for example, a first segment, e.g., lower or left side, and a second segment, e.g., upper or right side, or composed of these segments. One or more waveguide segments may be characterized by a rectangular or square section. It is also possible that one or more segments of the waveguide may be characterized in part by a tapered section and / or in part by an enlarged section.

[0083] If a waveguide comprises or is composed of two or more segments, these segments may be adjacent to each other, interlocked, or spaced apart from each other, for example, to form at least one gap or slot.

[0084] The longitudinal cross-section of the waveguide includes, or comprises, at least one material transparent to electromagnetic radiation at wavelengths of 850 nm and / or 1310 nm and / or 1550 nm, in particularly useful embodiments in both the photodetector described above according to the first and second aspects of the present invention and the modulator described above according to the third, fourth and fifth aspects of the present invention. Such a material is particularly preferably transparent to electromagnetic radiation in the wavelength range of 800 nm to 900 nm and / or 1260 nm to 1360 nm (the so-called original band or abbreviated as the O-band) and / or 1360 nm to 1460 nm (the so-called extended band or abbreviated as the E-band) and / or 1460 nm to 1530 nm (the so-called short band or abbreviated as the S-band) and / or 1530 nm to 1565 nm (the so-called conventional band or abbreviated as the C-band) and / or 1565 nm to 1625 nm (the so-called long band or abbreviated as the L-band). These bands are known in the field of communications engineering.

[0085] As materials for the longitudinal cross-section of the waveguide, for example, titanium dioxide and / or aluminum nitride and / or tantalum pentoxide and / or silicon nitride and / or aluminum oxide and / or silicon oxynitride and / or lithium niobate and / or silicon, particularly polysilicon and / or indium phosphate and / or gallium arsenide and / or indium gallium arsenide and / or aluminum gallium arsenide and / or at least one dichalcogenide, particularly two-dimensional transition metal dichalcogenides and / or chalcogenized glasses and / or heterostructures of two-dimensional materials and / or resins or resin-containing materials, particularly SU8 and / or polymers or polymer-containing materials, particularly OrmoClad and / or OrmoCore have been proven to be particularly suitable. In this regard, the longitudinal cross-section of the waveguide may contain one or more of these materials, one or more of these materials, or a combination of two or more of these materials. This can apply to one or more or possibly all waveguide segments in each case.

[0086] If the longitudinal cross-section of a waveguide comprises multiple waveguide segments, these may all contain or be composed of the same material. However, of course, it is also possible for two or more segments to differ with respect to their materials. For example, at least one waveguide segment may feature a refractive index higher than that of at least one other waveguide segment. For example, if several waveguide segments are sandwiched or stacked, the outer segments may have a lower refractive index. In this case, light is focused towards the center of the waveguide array. Purely exemplary materials are the upper and lower segments of aluminum oxide with an intermediate segment of titanium oxide.

[0087] A higher refractive index compared to the remaining segments has proven advantageous even for waveguide segments placed between two active elements, because it allows light to be focused within the region of the active elements.

[0088] Different materials for waveguide segments (or at least parts thereof) can be advantageous because they are characterized by different etching rates. This translates to manufacturing advantages, such as providing the required structuring.

[0089] With regard to the fabrication of the longitudinal section of the waveguide, the fabrication of the waveguide material may be carried out by deposition, spin-on, or transfer, and then, preferably, the structuring of the applied waveguide material is carried out by lithography and / or reactive ion etching (RIE). For example, the same deposition process described above in relation to the gate electrode can be used.

[0090] Waveguides or longitudinal sections can be formed in one or more parts. They may be formed from several waveguide segments, or may include several waveguide segments, especially when viewed in cross-section. These may be spaced apart from each other, or they may face each other and be in contact with each other, for example, by one segment being directly fabricated on top of another segment by applying a manufacturing method such as material deposition.

[0091] The longitudinal cross-section of the waveguide may, more preferably, consist of or include at least one material whose refractive index differs from that of the surrounding material.

[0092] In an advantageous embodiment, if a waveguide or the longitudinal section of a waveguide comprises two or more segments, at least two of which are spaced apart from each other to form a gap, the gap may be filled with at least one dielectric material having a refractive index lower than the refractive index of the materials of the waveguide segments defining the gap.

[0093] The longitudinal cross-section of the waveguide may be surrounded on one or more sides by, for example, a planar coating. In such cases, the pairs of pure refractive indices are 3.4 (Si) for the longitudinal cross-section of the waveguide and 1.5 (SiO2) for the planar coating, or, if a dielectric material is used, 2.4 (TiO2) for the longitudinal cross-section of the waveguide and 1.5 (SiO2) for the planar coating, or 2.0 (Sin) for the longitudinal cross-section of the waveguide and 1.47 for the planar coating.

[0094] It is particularly preferable that the refractive index of the longitudinal cross-section of the waveguide is at least 20%, preferably at least 30%, greater than the refractive index of the surrounding material.

[0095] The longitudinal section of the waveguide may be positioned either in contact with or without contact with the upper side of the planarization coating.

[0096] Preferably, the planarization film is characterized at least partially by a roughness in the range of 1.0 nm RMS to 0.1 nm RMS, particularly 0.6 nm RMS to 0.1 nm RMS, preferably 0.4 nm RMS to 0.1 nm RMS, on the side on which the longitudinal cross-section of the waveguide is positioned. (Note that nm stands for nanometer (10)) -9 This is an abbreviation of ).

[0097] Alternatively or additionally, the longitudinal cross-section of the waveguide can be embedded in at least a portion of the planarization film, and the active elements (in the case of a modulator having two such elements, one active element) are positioned on the upper side of the planarization film. In this case, the planarization film is preferably characterized at least partially by a roughness in the range of 1.0 nm RMS to 0.1 nm RMS, particularly 0.6 nm RMS to 0.1 nm RMS, preferably 0.4 nm RMS to 0.1 nm RMS, on the side on which the active elements are arranged on its upper side.

[0098] When the longitudinal cross-section of the waveguide is positioned above the planarization coating and embedded in the planarization coating, two planarization coatings exist.

[0099] To achieve the appropriate roughness, for example, chemical mechanical polishing and / or resist planarization can be performed.

[0100] In chemical mechanical polishing, the object being polished is typically polished by rotational motion between polishing pads. Polishing is performed chemically on the one hand and physically by polishing paste on the other. By combining chemical and physical actions, a smooth surface with a roughness of less than nanometers can be obtained.

[0101] In particular, resist planarization involves the formation of single or repeated spin-on-glass coatings and subsequent etching, preferably reactive ion etching (RIE). When planarizing surfaces such as SiO2 surfaces with height differences, this can be done by forming and etching spin-on-glass coatings. The spin-on-glass coating partially compensates for the height differences; that is, depressions formed on the surface have a higher coating thickness than adjacent areas after the formation of the spin-on-glass coating. The etching rates of spin-on-glass and, for example, SiO2, are similar or identical in the adapted RIE process. Here, adaptation means that pressure, gas flow rate, gas mixture composition, and power are selected accordingly. It has been shown that etching the entire spin-on-glass coating by RIE after its formation reduces the height difference due to the planarization effect of the spin-on-glass coating. The height difference can be further reduced by repetition. When depositing the SiO2 coating, the consumed SiO2 coating thickness must be taken into consideration, and the desired SiO2 coating thickness is achieved after the final etching step is completed. It should be emphasized that resist planarization is not limited to SiO2, and other materials can also be considered. It is advantageous if the etching rate of the material can be similar to, or at least substantially the same as, the etching rate of spin-on glass. This condition is met in the case of SiO2 and spin-on glass. For example, materials with etching rates twice as different as spin-on glass are also possible, in which case several passes are generally required. Hydrogen silsesquioxanes and / or polymers can be coated, for example, as liquid materials, particularly in a spin-on manner. They are called spin-on glass because they vitrify during subsequent annealing. Hydrogen silsesquioxane (HSQ) is given by the formula [HSiO2]. 1.5 It is a type of inorganic compound that contains ]n.

[0102] Chemical mechanical polishing and / or resist planarization can be carried out in a manner that yields a roughness in the range of 1.0 nm RMS to 0.1 nm RMS, particularly 0.6 nm RMS to 0.1 nm RMS, preferably 0.4 nm RMS to 0.1 nm RMS.

[0103] The roughness within the above range has proven particularly suitable. They are especially advantageous for avoiding stress and strain in the upper layer. For more information, see the paper “Identifying suitable substrates for high-quality graphene-based heterostructures” by L. Banszerus et al, 2D Mater. vol. 4, no. 2, 025030, 2017.

[0104] It should be noted that in a photodetector according to the first aspect of the present invention, a dielectric layer that may be provided particularly between the gate electrode and the active element may be obtained in the same manner, for example by CMP and / or resist planarization, if its upper surface is characterized by the roughness within the range described above.

[0105] Atomic force microscopy (AFM) can be used as a measurement method for determining roughness, particularly as described in the EN ISO 25178 standard. Atomic force microscopy is discussed in particular in Part 6 of this standard (EN ISO 25178-6:2010-01), which deals with methods for measuring roughness.

[0106] Furthermore, the planarization film and / or any additional planarization film provided as needed are preferably provided on the planarized surface and may include one or more cover layers, which may be, for example, a dichalcogenide layer or a dichalcogenide heterostructure, or a boron nitride layer. These materials are preferably deposited or transferred without requiring further chemical mechanical polishing or further resist planarization, although the possibility of chemical mechanical polishing and resist planarization being performed is not ruled out.

[0107] Furthermore, each planarization film may be obtained by coating, or it may be obtained as a film beforehand. In principle, the same processes (CVD, PVD, atomic layer deposition, transfer) used for the planarization coatings described above in relation to the gate electrode can be used. The above and the following descriptions for planarization coatings can also be applied to dielectric layers, if present.

[0108] A coating can consist of just one or more layers. It may be composed of only one material, or it may contain multiple materials. For example, a coating can consist of two or more layers of two or more different materials. Of course, a coating can have multiple layers, but all of them may be made of the same material. More than one layer can be obtained by providing layers, such as several atomic layers, through deposition or other means for its manufacture.

[0109] The planarization coating may further contain, or be composed of, spin-on glass and / or at least one polymer and / or at least one oxide, particularly silicon dioxide and / or at least one nitride. Spin-on glass is generally a liquid substance that can coat a wafer by spin-on deposition. After spin-on deposition, a film is formed on the wafer, and its thickness depends on the surface irregularities. Thus, the depth is partially smoothed, and the formation of a spin-on glass film has a planarization effect. Spin-on glass is usually heated after deposition, and therefore becomes a glass-like film.

[0110] In particular, the modulator may further include a diode or a capacitor. For example, the present invention may be an integrated III-V semiconductor modulator as described in the paper “Heterogeneously integrated III-V / Si MOS capacitor Mach-Zehnder modulator” from Hiaki, Nature Photonics volume 11, pages 482-485 (2017).

[0111] If a diode is provided, it may include multiple coatings consisting of multiple compositions of, for example, InGaAsP, in particular, to generate a pn junction and two contact regions.

[0112] The subject of the present invention is also a semiconductor device comprising a chip and at least one, preferably a plurality of, photodetectors and / or modulators according to the present invention, wherein one or more photodetectors are preferably disposed on the chip or on a coating disposed on or in contact with the chip or not.

[0113] Finally, the present invention relates to a semiconductor device comprising a wafer and at least one, preferably a plurality of, photodetectors and / or modulators according to the present invention, wherein one or more photodetectors and / or modulators are preferably disposed on the wafer or on a coating disposed in contact with or without contact on the wafer.

[0114] The photodetector and / or modulator may be part of a photonics platform, for example, manufactured on a chip or wafer, or bonded to a chip or wafer.

[0115] Bonding, in particular, means that the photodetector and / or modulator are not manufactured on the chip or wafer, but are manufactured separately from the chip or wafer and then bonded to the chip or wafer, perhaps as part of a larger unit, for example, by using a suitable intercoat.

[0116] When viewing a chip or wafer in cross-section, its vertical structure can be divided into different sub-regions. The lowest side is the front end of line, or FEOL, which typically contains one or more integrated electronic components. These integrated electronic components may be, for example, transistors and / or capacitors and / or resistors. Above the front end of line is the back end of line, or BEOL, which typically contains various metal surfaces that serve as means for interconnecting the integrated electronic components of the FEOL.

[0117] A wafer contains multiple regions, each of which forms a chip or die, following dicing / fragmentation. These regions are also called chip or die regions. Each chip region of a wafer preferably includes a cross-section or partial cross-section of a particular single piece semiconductor substrate of the wafer. Preferably, each chip region further includes one or more integrated electronic components extending within and / or above the corresponding region of the semiconductor substrate within the FEOL, particularly when viewed in cross-section. It should be emphasized that a chip region does not represent an individual chip; i.e., a wafer does not contain individual chips.

[0118] For both the semiconductor device and the semiconductor device according to the present invention, it is effective to provide a plurality of identically designed photodetectors and / or a plurality of identically designed modulators according to the present invention, or a plurality of differently designed photodetectors and / or modulators according to the present invention. Furthermore, there may be several identical photodetectors and / or modulators, as well as one or more differently designed photodetectors and / or modulators.

[0119] Embodiments of the present invention are to be seen with reference to the accompanying drawings, the dependent claims of the claims, and the following description of some examples of embodiments. [Brief explanation of the drawing]

[0120] [Figure 1] This is a partial cross-sectional view through a semiconductor device equipped with one embodiment of a photodetector according to a first aspect of the present invention. [Figure 2] Figure 1 is a top view of the photodetector. [Figure 3] This is a partial cross-section through a semiconductor device comprising a further embodiment of a photodetector according to a first aspect of the present invention. [Figure 4] This is a partial cross-sectional view through a semiconductor device equipped with one embodiment of a photodetector according to a second aspect of the present invention. [Figure 5] This is a partial cross-sectional view through a semiconductor device equipped with one embodiment of a modulator (electro-optical modulator) according to a third aspect of the present invention. [Figure 6] This is a partial cross-sectional view through a semiconductor device equipped with one embodiment of a modulator (electro-optical modulator) according to a fourth aspect of the present invention. [Figure 7] This is a partial cross-sectional view through a semiconductor device equipped with one embodiment of a modulator (electro-optical modulator) according to a fifth aspect of the present invention. [Figure 8] This figure shows the steps for the manufacturing method of the device described in Figure 1. [Modes for carrying out the invention]

[0121] All diagrams are purely schematic. In the diagrams, identical components or elements are denoted by the same reference numeral.

[0122] Figure 1 shows a partial cross-sectional view through one embodiment of a semiconductor device according to the present invention.

[0123] It includes a wafer (1), a planarization film (2) fabricated on the wafer (1), and a plurality of photodetectors (3) fabricated on the planarization film (2). In the partial cross-sectional view shown in Figure 1, only one of the plurality of photodetectors (3) is shown as an example.

[0124] The wafer (1) comprises a single semiconductor substrate (4) and, in the illustrated example, a plurality of integrated electronic components (5) extending within the semiconductor substrate (4). The integrated electronic components (5) may be transistors and / or resistors and / or capacitors, and are shown in schematic Figure 1 in simplified form only by hatched lines labeled reference numeral 5. At corresponding locations within the substrate (4), a plurality of integrated electronic components (5) are shown in known manner. These may also be components of a processor such as a CPU and / or GPU, and may form components of such a processor in known manner.

[0125] A wafer (1) has a front-end of line (FEOL(6)) on which multiple integrated electronic components (5) are arranged, and a back-end of line (BEOL(7)) above the FEOL where the integrated electronic components (5) of the FEOL are interconnected by different metal surfaces. The integrated electronic components (5) in the FEOL(6) and the associated interconnections in the BEOL(7) form an integrated circuit on the wafer (1) in a well-known manner. The FEOL(6) is sometimes called the transistor front-end, and the BEOL(7) is sometimes called the metal back-end. The metal surface comprises multiple connection elements (8), which in this example are provided by vertical interconnection accesses (VIA). The VIA(8) are made of a metal, such as copper, aluminum, or tungsten.

[0126] The planarization film is fabricated on the upper surface (9) of the wafer (1) facing away from the FEOL(6) and consists of a dielectric material. In this example, the planarization film (2) consists of silicon dioxide (SiO2), but this should be understood as illustrative, and other materials can be used.

[0127] In the illustrated embodiment, the planarized coating (2) is a coating obtained by depositing a corresponding coating material (in this case, SiO2) onto the upper surface (9) of the wafer (1) facing away from the FEOL (6), followed by a planarization treatment of the deposited material on the upper side (10) facing away from the wafer. As a result of the planarization treatment of the deposited material on the upper side (10) facing away from the wafer, the planarized coating (2) is now characterized by a roughness of 0.2 nm RMS, which should be understood as illustrative.

[0128] In the illustrated example, the planarization film (2) extends across the entire upper surface (9) of the wafer (1). The material of the planarization film (2) is deposited across the entire upper surface (9) of the wafer (1). Thus, the planarization film (2) is characterized by having a diameter that is at least substantially corresponding to the diameter of the wafer (1).

[0129] The photodetector (3) fabricated on the planarized coating (2) is an embodiment of the photodetector (3) according to a first aspect of the present invention. In this embodiment, all of these photodetectors (3) are identical in structure, but this should not be understood as restrictive.

[0130] The design and manufacture of photodetectors (3) are described below as an example based on one photodetector (3) shown in Figure 1. Furthermore, the designs of the further embodiments of photodetectors and modulators described below (see Figures 3 to 6) are described based on an example shown in a partial cross-section.

[0131] Each photodetector (3) includes one longitudinal section (12) of the waveguide (11), i.e., the longitudinal section overlapped by the active element (13) of the photodetector (3). In Figure 2, the active element (13) and the waveguide (11) below it are shown in a purely schematic top view, where the longitudinal section (12) of the waveguide covered by the active element (13) is shown as a dashed line.

[0132] Dielectric materials, preferably titanium dioxide, as used in the illustrated embodiments, are particularly suitable as waveguide materials. Alternatively or additionally, one or more waveguides are possible, consisting of aluminum nitride and / or tantalum pentoxide and / or silicon nitride and / or aluminum oxide and / or silicon oxynitride and / or lithium niobate, or semiconductors such as silicon, indium phosphate, gallium arsenide, indium gallium arsenide, aluminum gallium arsenide, dichalcogenides or chalcogenized glasses, or polymers such as SU8, OrmoClad, or OrmoCore.

[0133] The longitudinal section (12) of the waveguide is formed here by two waveguide segments (12a) and (12b), which extend longitudinally, are at least substantially parallel to each other, and are spaced apart from each other laterally (from left to right or vice versa in the figure), forming a gap (14) between them. Thus, it is a slot waveguide. Through such a waveguide (11), optical modes are guided into the gap (14) during operation. In the illustrated example, the two waveguide segments are characterized by rectangular cross-sections. The gap (14) can be filled with, for example, SiO2.

[0134] Each of the two waveguide segments (12a) and (12b) has at least one side, in this case the side facing the active element (13), in contact with a silicon gate electrode (15a) and (15b). The gate electrodes (15a) and (15b) are formed by a silicon coating fabricated on each of the waveguide segments (12a) and (12b).

[0135] The active element (13) comprises or comprises at least one material that absorbs electromagnetic radiation of at least one wavelength and generates an electrical optical signal as a result of the absorption. In the illustrated example, it is given by a graphene film (13). Graphene may also have its refractive index (refractive and / or absorptive) varied as a function of voltage and / or charge and / or electric field. It should be emphasized that the active element (13) may also be given by at least one other or further electro-optically active material, for example, a dichalcogenide-graphene heterostructure comprising or comprising at least one layer of graphene and at least one layer of dichalcogenide, or a film comprising at least one layer of boron nitride and at least one layer of graphene.

[0136] As can be seen from Figure 1, the graphene film (13) is positioned above (16) a further planarization coating (17) into which the waveguide (11) and thus its longitudinal cross-section (12) are embedded. This further planarization coating (17) is made of the same material as the planarization coating (2) and is characterized by having the same roughness above (16) as above (10) the planarization coating (2). However, this should be understood only illustratively and not limitingly.

[0137] Gate electrodes (15a) and (15b) provided on waveguide segments (12a) and (12b) allow a pn junction to be realized within the region of the graphene film (13) extending above the gap (14), and therefore within the region of the optical mode guided during operation within the gap (14) of the waveguide (11). The pn junction can be used to separate electron-hole pairs generated by absorption in order to generate a photocurrent. Similarly, the thermoelectric effect can be utilized in graphene, where oppositely signified Seebeck coefficients are generated in the p and n regions, and a thermoelectric voltage is generated when heated by absorbed energy (photons).

[0138] Note that the connections for power gate electrodes (15a) and (15b), which are not shown, can be arranged laterally adjacent to VIA(8), for example.

[0139] The photodetector (3), in particular its graphene film (13), is electrically connected to at least one of the integrated electronic components (5) at the FEOL (6) of the wafer (1). As can be seen in the schematic cross-sectional view in Figure 1, the connection is achieved not only by a via (8) at the BEOL (7) of the wafer (1), but also by a further via (8) extending through the planarization coating (2) and any further coatings or elements present above it (in this case, a further planarization coating (17)).

[0140] Specifically, the graphene film (13) is electrically connected at the opposite end region either directly or via a connecting element (18) to a further planarization film (17) and the upper end of a VIA (8) that extends to the planarization film (2) on the BEOL (7) of the wafer (1). In the top view of Figure 2, the VIA (8) located below the connecting element (18) and connected to the connecting element (18) is shown as a thin line.

[0141] In the illustrated embodiment, a passivation coating (19) containing or composed of aluminum oxide (Al2O3) and / or silicon dioxide (SiO2) is provided on the upper side of the graphene film (13).

[0142] The photodetector (3) shown in Figures 1, 3, and 4 and described below can be used by itself, in particular, in known ways for signal conversion from the light world to the electronic world.

[0143] To obtain the semiconductor device shown in Figure 1, in the first step S1 (see Figure 8), an integrated circuit including an integrated electronic component (5) and a metallization including a VIA (8) is provided on the wafer (1). The wafer (1) may be any conventional wafer (1) obtained by a known processing process.

[0144] In the second step S2, the planarization film (2) is fabricated on the BEOL (7) upper side of the wafer (1). For this purpose, in this case, silicon dioxide (SiO2) is deposited as the coating material, and chemical deposition such as low-pressure chemical deposition or plasma-enhanced chemical deposition, or physical deposition, or spin-on glass is used. In this embodiment, PECVD is used. After depositing the coating material, the upper side of the obtained coating is planarized (step S3), in this case resist planarization is performed to obtain an upper side (10) having a roughness of 0.2 nm RMS.

[0145] Resist planarization involves single or repeated spin-on glass spinning and subsequent etching (the etching in practice is reactive ion etching (RIE)). The spin-on glass film partially compensates for height differences; i.e., recesses formed on the surface have a higher film thickness than adjacent areas after the formation of the spin-on glass film. Etching the entire spin-on glass film after its formation, for example by RIE, reduces the height difference due to the planarization effect of the spin-on glass film. By repeating the process, the height difference can be further reduced to obtain the desired roughness. Note that the upper (10) of the planarized film (2) corresponding to low roughness can alternatively be obtained by, for example, chemical mechanical polishing (CMP).

[0146] In the next step S4, which represents the first step in the fabrication of the photodetector (3), waveguides (11) (each) equipped with gate electrodes (15a) and (15b) are fabricated. For this purpose, waveguide material, currently titanium dioxide (TiO2), is deposited over the entire upper side (10) of the obtained planarization film (2). Deposition can be carried out by PVD or CVD, particularly PECVD or LPCVD, or by atomic layer deposition (ALD) which can be performed by spin-on, as with the planarization film, or by performing a transfer print process. LPCVD is also used in the same manner as in the formation of the planarization film (2).

[0147] Next, a gate electrode material, in this case silicon, is deposited as a coating material for the gate electrodes (15a) and (15b) by a PVD or CVD process, preferably two-dimensionally.

[0148] To obtain individual waveguides (11) having individual waveguide segments (12a) (12b) having gaps (14), and individual gate electrodes (15a) (15b), structuring is performed by lithography and in particular by reactive ion etching (RIE).

[0149] In the next step S5, a further planarization film (17) is formed on the waveguide (11) with the gate electrodes (15a) and (15b) located above it, and on the upper side (10) of the planarization film (2). This is obtained by deposition by PECVD and resist planarization, a method completely similar to that of the planarization film (2). During or for the purpose of material deposition, the gap (14) is also filled with SiO2. As a result of resist planarization, the cross-section of the further planarization coating (17) above the waveguide (11) becomes trapezoidal (see Figure 1).

[0150] Furthermore, for the further planarized coating (17), other processes can be used instead of LPCVD and CMP, and other planarization treatments such as CMP and / or further planarization are possible for the planarized coating (2).

[0151] The planarization film (2) and the further planarization coating (17) are preferably provided on the surface to be planarized and may include one or more coating layers, for example, a dichalcogenide layer or dichalcogenide heterostructure, or a boron nitride layer. These materials are preferably deposited or transferred without requiring further chemical mechanical polishing or further resist planarization, but are not limited thereto.

[0152] For integrity, it should be noted that in areas of the semiconductor device of the present invention that do not have further planarization coatings (17), for example, in areas where the structure corresponds to those in Figures 3 to 6, the further planarization coatings (17) (and any coatings placed above them) are subsequently partially removed, particularly by lithography and etching.

[0153] In step S6, the VIA(8) is manufactured by penetrating the planarization film (2) and the further planarization film (17). In principle, this can be done by any method known from the prior art. In particular, the areas to which they are extended are first defined, preferably by lithography, and dry etched by RIE. Then, metallization is performed, and the metallized surface is structured, for example, by CMP (damassene process) or by lithography and RIE. The VIA(8) can be manufactured after the further planarization film (17) is formed through both planarization films (2)(17), or after a portion of the first planarization film (2) is formed through the first planarization film (2) and a portion of the second planarization film (17) is formed through the second planarization film (17).

[0154] In step S7, the active elements of the (each) photodetector (3) provided by the graphene film (13) are provided on the upper side (16) of the further planarization film (17), and are deposited on the upper side (16), for example.

[0155] The graphene film (13) of each photodetector can be deposited, for example, by the transfer process described above. Then, in each case, the graphene film manufactured on a separate substrate, a separate metal foil, or a separate germanium wafer is transferred to a further planarization film (17). Alternatively, the graphene film (13) can be manufactured directly on the further planarization film (17). This may include, for example, material deposition.

[0156] When a transfer process is used, the passivation film may already be present on the upper side of each graphene film (13), or it may be transferred, for example, after being deposited on the graphene film (13). Alternatively, the passivation film may be deposited after the graphene film (13) has been transferred or manufactured.

[0157] First, it is also possible to fabricate a full-area graphene film and / or a full-area passivation film extending over the entire surface of the further planarization film (17) above the further planarization film (17). In this case, the individual graphene films (13) are structured in particular by lithography and RIE to be obtained as active elements for several photodetectors (3).

[0158] Next, the connecting elements (18) are preferably manufactured by depositing metal on the entire surface to obtain individual connecting elements (18), and then structuring them by lithography and RIE (step S8).

[0159] In step S9, prior to the final step, an upper passivation coating (19) of Al2O3 and / or SiO2 is preferably deposited. In this coating, openings are conveniently fabricated by lithography and RIE, particularly for connecting elements (step S10). Preferably, the openings are formed in contact elements that serve to connect photonics and / or electronics to the outside.

[0160] Figure 3 shows a further embodiment of the photodetector (3) according to the first aspect of the present invention.

[0161] This embodiment differs in essence from that shown in Figure 1, in that the two waveguide segments (12a) and (12b) of the longitudinal cross-section (12) of the waveguide (11) do not have a rectangular cross-section, and there is no further planarization film (17). Instead, the active element, exemplified by the graphene film (13), is placed on a dielectric film not shown in the figure, which is provided above the gate electrodes (15a) and (15b). The dielectric film represents the gate dielectric. It is characterized by a roughness of 0.2 nm RMS on its upper side. Its thickness is 15 nm, and these two values ​​should be understood purely as examples.

[0162] As can be seen in the figure, each of the two waveguide segments (12a) and (12b) has an end region facing the gap (14) extending between the two segments (12a) and (12b), and its cross-section partially widens in the direction of the gap (14). As can be seen in the figure, the two end regions and the gap (14) form a central trapezoidal region. The portions or regions of segments (12a) and (12b) adjacent to this trapezoidal region on both sides are characterized by a constant thickness, as can be seen.

[0163] The two gate electrodes (15a) and (15b) extend laterally only across the upper cross-section of their respective segments (12a) and (12b).

[0164] In Figure 3, vias (8) are visible in relation to the gate electrodes (15a) and (15b), contacting each gate electrode (15a) and (15b). These are connected from the FEOL (6) to at least one integrated electronic component (5), although these connections are not shown in the figure for the sake of simplified representation. As can be seen from the figure, these vias (8) extend through the planarization film (2) and waveguide segments (12a) and (12b) on which each gate electrode (15a) and (15b) is positioned in each case. Voltage supply to the gate electrodes (15a) and (15b) is ensured through the vias (8). In the example shown in Figure 3, a pn junction can be obtained in the graphene film (13) via the gate electrodes (15a) and (15b) during operation, and a pn junction can be obtained in the region extending above the gap (14) through which the optical mode is guided during operation.

[0165] To obtain the sequence shown in Figure 3, steps S1 to S3 may be the same as those for producing the sequence shown in Figure 1.

[0166] In step S4, an etching process adapted for the fabrication of the waveguide (11) and gate electrodes (15a)(15b), particularly a RIE process, is performed after the waveguide material has been deposited on this region to obtain a trapezoidal region with beveled edges, for example, as described above in relation to Figure 1. The isotropic etching behavior of the RIE process can be obtained, for example, by increasing the process pressure and mixing adaptive gases compared to an anisotropic etching process. An increased process pressure of, for example, 20 mTorr compared to 10 mTorr gives the etching process an undirected component, which results in a higher removal rate at the upper edge for a longer etching time. Subsequently, first, a VIA(8) for the gate electrodes (15a)(15b) is fabricated, and then again, a material for the gate electrodes (15a)(15b), such as silicon, is deposited.

[0167] Next, the gaps (14) and gate electrodes (15a)(15b) are etched. As a result, the gate electrode coating, which was initially the entire surface, is "divided".

[0168] Here, since there is no need to fabricate a further planarization coating (17), step S5 for the configuration shown in Figure 1 is omitted. Therefore, the VIA (8) of the graphene film (13) is fabricated in step S5 here.

[0169] In step S6, the dielectric coating is first formed on the upper side of the gate electrodes (15a) and (15b), preferably planarized on the upper side to achieve the roughness described above, and then the graphene film (13) is provided on the upper side thereof.

[0170] The trapezoidal shape ensures that the active element, in this case the graphene film (13), follows the gate electrodes (15a)(15b) or the particularly inclined edge of the dielectric coating. As a result, the graphene is always located on the dielectric coating on the electrodes (15a)(15b) and can be controlled particularly well electrostatically. Furthermore, a particularly uniform electric field can be achieved.

[0171] The steps following the provision of each graphene film (13) may correspond to the steps of the arrangement shown in Figure 1 (in particular, the fabrication of the connecting element (18), the fabrication of the passivation coating (19), and the provision of openings therein).

[0172] Figure 4 shows an embodiment of a photodetector according to a second aspect of the present invention.

[0173] This embodiment also comprises a longitudinal section (12) of a waveguide (11) and an active element (13) comprising or composed of at least one material that absorbs electromagnetic radiation of at least one wavelength and generates an electrical optical signal as a result of the absorption. In the photodetector shown in Figure 3, the active element is exemplified by a graphene film (13).

[0174] Unlike the embodiments shown in Figures 1 and 3, in this embodiment, the waveguide (11) belonging to the photodetector (3) and its longitudinal cross-section (12) are integrally formed. Specifically, it is a strip waveguide having a rectangular cross-section.

[0175] Furthermore, a further difference is given by the fact that the two carrier elements (20) are positioned on opposite sides of the longitudinal portion of the waveguide (11), spaced apart from it to form two gaps (21). Thus, the carrier elements (20) are positioned laterally away from the longitudinal cross-section (12) of the waveguide (11). The two gaps (21) contain no material and are a vacuum.

[0176] The carrier element (20) can be made of the same material as the longitudinal cross-section (12) of the waveguide (11), but this should be understood as illustrative.

[0177] As can be seen from the figure, the active element (13) overlaps in the lateral direction with the longitudinal cross-section (12) of the waveguide (11), the two gaps (21), and a portion of the two carrier elements (20).

[0178] Furthermore, the graphene film (13) is entirely flat, in contrast to the embodiments in Figures 1 and 3, which include a trapezoidal cross-section.

[0179] As far as the wafer (1), planarization coating (2), and passivation coating (19) are concerned, the arrangement in Figure 4 is identical to the arrangement in Figure 2. As can be seen from the figure, it also lacks an additional planarization coating (17). Furthermore, this photodetector (3) does not include a gate electrode.

[0180] To create the sequence shown in Figure 4, steps S1 to S3 may be the same as those described in relation to Figure 1.

[0181] Next, in step S4, the waveguide (11) and carrier element (20) are manufactured. For this purpose, the waveguide material is deposited on a surface, for example, as in the embodiments described above, and then the gap (21) is obtained by lithography and etching.

[0182] Next, the VIA(8) is manufactured to extend through one planarized film (2) and one of the carrier elements (20) (step S5).

[0183] In step S6, an active element in the form of, for example, a graphene film (13) is provided, which is easily carried out by a transfer process as described in more detail above.

[0184] The remaining steps may be similar to those in the above-described embodiments for providing the active element (13) (in particular, for manufacturing the connecting element (18), manufacturing the passivation coating (19), and providing the opening therein).

[0185] Figure 5 shows one embodiment of a modulator (electro-optic modulator) (22) according to a third aspect of the present invention.

[0186] This embodiment also includes, as the longitudinal section (12) of the waveguide (11), four waveguide segments (12a)(12b)(12c)(12d) that extend longitudinally and extend at least substantially parallel to one another.

[0187] Since it is a modulator (22), it further includes two active elements (13a)(13b) comprising or consisting of at least one material whose refractive index changes as a function of voltage and / or the presence of charge and / or the electric field. In the illustrated example, the two active elements are given by two graphene films (13a)(13b).

[0188] Of the two active elements (13a) and (13b), the lower element (13a) is positioned on the upper side (10) of the planarization film (2).

[0189] It should be noted that instead of providing and arranging two active elements (13a) and (13b), one active element and one conventional electrode, such as one made of metal, may be provided and arranging in correspondence with each other.

[0190] Furthermore, for the four waveguide segments (12a) to (12d), the lower waveguide segment (12a) is positioned between the two active elements (13a) and (13b), and the middle waveguide segment (12b) is positioned above the two active elements (13a) and (13b), particularly above the upper active element (13b). In other words, there is a sandwich configuration (from bottom to top in Figure 5) consisting of the first active element (13a), the lower waveguide segment (12a), the second active element (13b), and the middle waveguide segment (12b). The upper active element (13b) extends within the longitudinal cross-section (12) of the waveguide. Waveguide segments (12a) to (12d) may all be made of the same material.

[0191] The lower and intermediate waveguide segments (12a) and (12b) simultaneously function as passivation and etching protection. In particular, the lower waveguide segment (12a) is part of the waveguide and protects the lower active element (13a) when the upper active element (13b) is etched. The lower waveguide segment (12a) also functions as an etch stop coat and a passivation coat to protect the graphene (13a). In particular, the intermediate waveguide segment (12b) is also an etch stop coat to structure the upper waveguide segments (12c) and (12d) during the fabrication of the gap (14).

[0192] The remaining two upper waveguide segments (12c)(12d) are positioned above the intermediate waveguide segment (12b). The two upper waveguide segments (12c)(12d) are spaced apart laterally from each other, forming a gap (14) extending between them. Thus, the two upper waveguide segments (12c)(12d) are located adjacent to the upper side of the intermediate waveguide segment (12b), and the gap (14) is located between the two upper waveguide segments (12c)(12d). This means that exactly one gap (14) is provided above the two active elements (13a)(13b). The gap (14) is filled with the material of the passivation coating (19).

[0193] The lateral distance between the lower and intermediate waveguide segments (12a) and (12b) is, as can be seen, greater than a multiple of the distance between the two upper waveguide segments (12c) and (12d) in this direction. The cross-section of segments (12a) to (12d) is rectangular.

[0194] The two active elements (13a) and (13b) are separated from each other by the lower waveguide segment (12a) and are further offset laterally from each other so that they are located above and below each other in the overlapping region (23). A portion of one active element (13a) is aligned with or overlaps with a portion of the other active element (13b). Specifically, the opposing end regions are located above and below each other or aligned to form the overlapping region (23). As can be seen in Figure 5, the overlapping region (23) is located below and aligned with the gap (14) formed between the two segments (12c) and (12d).

[0195] The distance of the overlap region (23) and the distance of the lateral gap (14) are related to each other. Specifically, the distance of the lateral overlap region (23) is approximately 1.3 times the distance of the gap (14) in this direction. For example, it can correspond to 1.0 times or 0.8 times, meaning that the distance in this direction can be the same or smaller. In particular, a smaller overlap results in lower capacitance and a faster modulator.

[0196] In the case of a modulator (22) having two active elements (13a) and (13b), specifically the active elements (13a) and (13b) of the modulator are connected to at least one integrated electronic component (5) from the FEOL (6) of the wafer (1). Each active element (13a) and (13b) is associated with a VIA (8) and connected to the VIA (8) by a contact element (18) that contacts it, and the VIA (8) (VIA (8) for the active element (13a) on the left side of Figure 5) penetrates the planarization film (2), and the VIA (8) (VIA (8) for the active element (13b) on the right side of Figure 5) extends through the planarization film (2) and the waveguide segment (12a), together with further VIA (8) on the BEOL (7) to ensure connection.

[0197] As shown in Figures 5, 6, and 7, the modulator (22), which will be described in more detail, can itself be used in known ways, particularly for optical signal coding.

[0198] Steps S1 to S3 can be identical in order to obtain the arrangement shown in Figure 5.

[0199] Next, in step S4, the first lower graphene film (13a) can be provided as the lower active element. This can be done in the same manner as described above for one active element (13) of the photodetector (3). Thus, this can include, for example, whole-region deposition of the material and subsequent structuring.

[0200] Next, the connecting element (18) belonging to this active element (13a) can be manufactured again in exactly the same way as the connecting element (18) in Figures 1, 3, and 4.

[0201] Next, in step S6, the lower waveguide segment (12a) is manufactured, which preferably includes material deposition and subsequent structuring, similar to segments (12a) and (12b) from the figure above. As the waveguide material, the same material as in the above embodiments can be used.

[0202] In step S7, the second upper graphene film (13b) is preferably provided on the upper side of the segment (12a) in the same manner as the first lower graphene film (13a).

[0203] In step S8, the connecting element (18) is manufactured.

[0204] In step S9, the intermediate segment (12b) is preferably manufactured in the same manner as the lower segment (12a), and in step S10, the two upper segments (12c)(12d) are manufactured above the intermediate segment (12c). Here again, the waveguide material may be deposited in the manner described above, and then configured to obtain two adjacent segments (12c)(12d) surrounding the gap (14) between them. Note that, for example, if different waveguide materials are used, the material deposition of the intermediate segment (12b) and the two upper segments (12c)(12d) may be interrupted or separated. However, it is not excluded that the material required for the intermediate segment (12b) and the material required for the upper segments (12c)(12d) are applied in a single deposition process without interruption, and that the segments (12b)(12c)(12d) are obtained by subsequent structuring.

[0205] Step S10 preferably follows the steps of obtaining a passivation coating (19) (S11) and obtaining an opening therein (S12), as described above in relation to the aforementioned drawings. The gap (14) is filled with material for the passivation coating (19) during or for the purpose of material deposition for the passivation coating (19).

[0206] Figure 6 shows one embodiment of a modulator (22) according to a fourth aspect of the present invention.

[0207] This embodiment differs in particular from that shown in Figure 5 in that the gap (14) is located below rather than above the active elements (13a)(13b), which is also shown here by graphene film (13a)(13b) as an example. The longitudinal section (12) of the waveguide (11) contains five segments (12a)(12b)(12c)(12d)(12e) instead of four.

[0208] Specifically, the two lower waveguide segments (12a) and (12b) are placed below the lower active element (13a), and they are spaced apart laterally from each other so that a gap (14) is formed between them. The first intermediate waveguide segment (12c) is placed between the two active elements (13a) and (13b), the second intermediate waveguide segment (12d) is placed above the upper one (13b) of the two active elements (13a) and (13b), and the upper waveguide segment (12e) is placed above the second intermediate waveguide segment (12d), particularly in contact with its upper surface. In this example, a sandwich-like structure is formed from the bottom to the top, namely, a sandwich-like structure consisting of two lower waveguide segments (12a) and (12b), a lower active element (13a), a first intermediate waveguide segment (12c), an upper active element (13b), a second intermediate waveguide segment (12d), and an upper waveguide segment (12e) above it. Here, the two active elements (13a) and (13b) extend within the longitudinal cross-section (12) of the waveguide (11).

[0209] Here, the two lower waveguide segments (12a)(12b) and the first intermediate waveguide segment (12c) also function as passivation and etching protection.

[0210] The lateral extension of the gap (14) in the overlapping region (23) is the same as in Figure 5.

[0211] To obtain the arrangement shown in Figure 6, steps S1 to S3 can again be the same.

[0212] In step S4, two waveguide segments (12a) and (12b) are first fabricated on the upper side (10) of the planarized film (2), and then the waveguide material is deposited, preferably in exactly the same manner as in the previously described embodiments, thereby first obtaining a continuous coating, and then the gap (14) is preferably subjected to structuring, including lithography and etching, particularly RIE, and filled with a dielectric material, such as SiO2. The surface is preferably planarized by CMP and / or resist planarization.

[0213] Next, a VIA(8) associated with the left graphene film (13a) in Figure 5 can be fabricated (step S5), which can be done by extending the VIA(8) through the planarized coating (2) in Figure 5 and one of the left segments (12a) of the lower segment (12a), as described above.

[0214] Next, the lower graphene film (13a) is provided (step S6). This can be done in the same manner as in the embodiments described above. Preferably, the lower graphene film (13a) is positioned to completely overlap the gap (14) in the lateral direction, as shown in Figure 5.

[0215] Next, the associated connecting element (18) is manufactured as described above (step S6), and then the VIA (8) for the first intermediate waveguide segment (12c) and the upper graphene film (13b) (step S7), the upper graphene film (13b) (S8), the first waveguide segment (12d) (S9), and the upper segment (12e) (S10) can be manufactured. The manufacturing of these waveguide segments (12c) (12d) (12e) is similar to, for example, the manufacturing of segments (12a) to (12d) in Figure 5, except that the segment (12e) does not have a gap and is etched only as a strip-shaped segment having a rectangular cross-section.

[0216] Finally, the above steps for obtaining the passivation coating (19) (S11) and the opening (S12) within it can also be carried out here.

[0217] Figure 7 shows one embodiment of a modulator (22) according to a fifth aspect of the present invention.

[0218] This embodiment differs from the example in Figure 6 only in that a second gap (14) is additionally provided above the two active elements (13a) and (13b) formed by the graphene film, again as an example. Instead of the strip-shaped waveguide segment (12e) as in Figure 6, two adjacent segments (12e) and (12f) spaced apart from each other to form the second gap (upper gap) (14) are provided above the upper graphene film (13b) in contact with the upper side of the second intermediate segment (12d). It should be noted that the upper gap (14) is also filled with the material of the passivation coating (19) during or for the deposition of the material of the passivation coating (19) in this case.

[0219] In this embodiment, the structure is sandwich-like, including two lower waveguide segments (12a) and (12b) extending from the bottom to the top, a lower active element (13a), a first intermediate waveguide segment (12c), an upper active element (13b), a second intermediate waveguide segment (12d), and two upper waveguide segments (12e) and (12f) above it. Here again, the two active elements (13a) and (13b) extend within the longitudinal cross-section (12) of the waveguide (11).

[0220] The two lower waveguide segments (12a)(12b) and the first intermediate waveguide segment (12c) also function simultaneously here as passivation and etching protection.

[0221] As can be seen in Figure 6, the overlap region (23) formed by the two active elements (13a) and (13b) due to the offset is located above the lower gap (14) between the lower segments (12a) and (12b), and also above the upper gap (14) between the upper segments (12e) and (12f).

[0222] The lower gap (14), overlapping region (23), and upper gap (14) are aligned.

[0223] Furthermore, here, the distance of the overlapping region (23) and the distances of both gaps (14) are related to each other laterally. Specifically, the lateral distance of the overlapping region (23) is approximately 1.3 times the distance between the upper gap (14) and the lower gap (14). This ratio may be, for example, 1.0 or 0.8.

[0224] To obtain the configuration shown in Figure 7, the procedure can be the same as in Figure 6, with the only difference being that the upper gap (14) must also be etched. As a result, instead of one upper segment (12e), two upper segments (12e)(12f) with a gap (14) are obtained above the second mid-waveguide segment (12d).

[0225] As described above, each example of a semiconductor device according to the present invention includes a plurality of photodetectors (3) or modulators (22), of which only one is shown as a partial cross-section as an example. In the illustrated embodiments of the semiconductor device according to the present invention, all photodetectors (3) or modulators (22) may be identical in design. This compatibility allows for particularly simple and rapid manufacturing. However, it should be emphasized that, of course, the semiconductor device according to the present invention may also include different embodiments of the photodetectors (3) and / or modulators (22) shown in Figures 1 and 3 to 6, for example, the photodetector (3) according to Figure 1 and the modulator according to Figure 5. Furthermore, there may be two or more different embodiments, for example, one or more of each of the shown photodetectors (3) and / or modulators (22).

[0226] It should be noted that each component, including the planarization film (2) (which may include the films shown in (17) and (19)) and the photodetector (3) and / or modulator (22), provided on the wafer (1), can be designed as a photonics platform. Furthermore, it should be noted that, in principle, it is also possible to bond separately manufactured components to the wafer (1) instead of manufacturing the photonics platform on the BEOL (7) of the wafer (1), as in the embodiments described above.

[0227] After the semiconductor device according to the present invention is completed, a plurality of semiconductor devices, each formed by a chip equipped with an integrated photonic having one or more photodetectors (3) and / or modulators (22) according to the present invention, can be easily and quickly obtained by simply dicing, i.e., dividing.

[0228] The “bare chip” obtained by dicing, which includes the photodetector (3) and / or modulator (22), is inserted into a package and supplied for further use, as is known from conventional bare chips.

[0229] A chip obtained by dicing a semiconductor device having a wafer (1) and one or more photodetectors (3) and / or modulators (22) is one embodiment of the semiconductor device according to the present invention.

[0230] It should be noted that in the figures shown in the embodiments, all partial cross-sectional views show only relatively small cross-sections, specifically, cross-sections showing only small portions of the wafer (1), or chips obtained after dicing. Therefore, all parts represent both parts through embodiments of the semiconductor device according to the present invention and through embodiments of the semiconductor device according to the present invention. Furthermore, it should be noted that multiple photodetectors (3) and / or modulators (22), for example tens, hundreds, or thousands, can already be provided on a single chip, depending on the application.

Claims

1. a longitudinal cross-section (12) of a waveguide (11) including or formed by at least two longitudinally extending waveguide segments (12a) and (12b) that are substantially parallel to one another; an active element (13) overlapping a longitudinal section (12) of said waveguide (11) and including or consisting of at least one material adapted to absorb electromagnetic radiation of at least one wavelength and to generate an electrical optical signal as a result of said absorption; The two waveguide segments (12a) and (12b) are spaced apart from one another to define a gap (14) extending therebetween; A photodetector (3), characterized in that the two waveguide segments (12a)(12b) are in at least partial contact, on at least one side, with two gate electrodes (15a)(15b), respectively.

2. An optical detector (3) as described in claim 1, characterized in that the two waveguide segments (12a) (12b) are laterally spaced apart from each other.

3. A photodetector (3) as described in claim 1 or 2, characterized in that the two waveguide segments (12a) (12b) are in at least partial contact with the two gate electrodes (15a) (15b), respectively, on the sides facing the active element (13).

4. A photodetector (3) as claimed in any one of claims 1 to 3, characterized in that the two gate electrodes (15a) (15b) contain or consist of silicon.

5. 5. The photodetector (3) according to claim 1, wherein the two gate electrodes (15a), (15b) are in contact with upper surfaces of the two waveguide segments (12a), (12b) on their lower sides and in contact with lower surfaces of a dielectric coating provided between the active element (13) and the two waveguide segments (12a), (12b) on their upper sides.

6. 6. The photodetector (3) according to any one of claims 1 to 5, characterized in that the two gate electrodes (15a) (15b) comprise or consist of a material that is transparent to electromagnetic radiation of at least one wavelength and / or a material that is electrically conductive.

7. 7. A photodetector (3) according to any one of the preceding claims, characterized in that each of the two gate electrodes (15a)(15b) is associated with a connection element (8) in contact therewith, one of the connection elements (8) extending through one of the two waveguide segments (12a)(12b).

8. 8. A photodetector (3) according to any one of claims 1 to 7, characterized in that the active element (13) overlaps the two waveguide segments (12a)(12b) and at least a portion of the gap (14) located between them.

9. a longitudinal section (12) of a waveguide (11) and an active element (13) including or consisting of at least one material that absorbs electromagnetic radiation of at least one wavelength and generates an electrical optical signal as a result of said absorption, Two support elements (20) are spaced apart on either side of a longitudinal cross section (12) of the waveguide (11) so as to form two gaps (21); The two gaps (21) are free of material; The active element (13) overlaps at least a portion of the longitudinal section (12) of the waveguide (11), the two gaps (21) and the two support elements (20).

10. 10. The photodetector (3) of claim 9, characterized in that the active element (13) is located on the upper side of a longitudinal cross section (12) of the waveguide (11) facing the active element (13) and / or on the upper side of the support element (20) facing the active element (13).

11. A photodetector as described in any one of claims 1 to 10, characterized in that at least one material of the active element (13) is graphene and / or at least one dichalcogenide and / or a heterostructure of two-dimensional materials and / or germanium and / or at least one electro-optical polymer and / or silicon and / or at least one compound semiconductor.

12. a longitudinal cross-section (12) of a waveguide (11) including or formed by at least four longitudinally extending waveguide segments (12a), (12b), (12c), (12d) that are substantially parallel to one another; It comprises two active elements (13a)(13b) containing or consisting of at least one material whose refractive index changes as a function of voltage and / or in the presence of an electric charge and / or an electric field, or one such active element and one electrode, a lower one (12a) of the waveguide segments is disposed between the two active elements (13a)(13b) or between the active element and the electrode, a middle one (12b) of the waveguide segments is disposed above the two active elements (13a)(13b) or above the active element and the electrode, and the remaining upper two (12c)(12d) of the waveguide segments are disposed above the middle one (12b) of the waveguide segments, the remaining upper two (12c)(12d) of the waveguide segments being spaced apart from one another to define a gap (14) extending therebetween.

13. a longitudinal cross-section (12) of a waveguide (11) including or formed by at least five longitudinally extending waveguide segments (12a), (12b), (12c), (12d), and (12e) that are substantially parallel to one another; It comprises two active elements (13a)(13b) containing or consisting of at least one material whose refractive index changes as a function of voltage and / or in the presence of an electric charge and / or an electric field, or one such active element and one electrode, a modulator (22) in which two lower waveguide segments (12a) and (12b) are disposed below the two active elements (13a) and (13b) or below the one active element and the one electrode and are spaced apart from each other to form a gap (14) extending therebetween, one intermediate waveguide segment (12c) between the two active elements (13a) and (13b) or between the one active element and the one electrode, another intermediate waveguide segment (12d) between the two active elements (13a) and (13b) or above the one active element and the one electrode, and one upper waveguide segment (12e) is disposed above the other intermediate waveguide segment (12d) between the two active elements (13a) and (13b).

14. a longitudinal cross-section (12) of a waveguide (11) including or formed by at least six longitudinally extending waveguide segments (12a), (12b), (12c), (12d), (12e), (12f) that are substantially parallel to one another; It comprises two active elements (13a)(13b) containing or consisting of at least one material whose refractive index changes as a function of voltage and / or in the presence of an electric charge and / or an electric field, or one such active element and one electrode, a second intermediate waveguide segment (12c) disposed between the first active element (13a) and the second active element (13b) or between the first active element and the first electrode, the second intermediate waveguide segment (12d) disposed above the first active element (13a) and the second active element (13b) or above the first active element and the first electrode, and the second intermediate waveguide segment (12e) disposed above the first intermediate waveguide segment (12d) or above the first active element and the first electrode, and the second intermediate waveguide segment (12e) disposed above the second intermediate waveguide segment (12d) and above the first active element and the first electrode, the second intermediate waveguide segment (12c) disposed between the first active element (13a) and the second active element (13b) or between the first active element and the first electrode, and the second intermediate waveguide segment (12d) disposed between the first active element (13a) and the second active element (13b) or

15. 15. A modulator (22) according to any one of claims 12 to 14, characterized in that the two active elements (13a)(13b) are spaced apart from each other and arranged offset from each other such that one of the two active elements (13a)(13b) is partially located above the other to form an overlap region (23).

16. 16. The modulator (22) of claim 15, wherein the overlap region (23) is located above or below the gap (14).

17. 17. The modulator (22) according to claim 15 or 16, characterized in that the overlap region (23) is located above one gap (14) and below the other gap (14).

18. A modulator (22) according to any one of claims 15 to 17, characterized in that the lateral distance of the overlap region (23) is in the range of 0.8 to 1.8 times the lateral distance of at least one of the gaps (14).

19. 19. The modulator (22) according to any one of claims 12 to 18, characterized in that exactly one gap (14) formed between two of the waveguide segments (12a-12f) spaced apart from each other is provided above and / or below the two active elements (13a)(13b) or the one active element and the one electrode.

20. A modulator (22) as described in any of claims 12 to 19, characterized in that at least one material of the active elements (13a) (13b) is graphene and / or at least one dichalcogenide and / or a heterostructure of two-dimensional materials and / or germanium and / or at least one electro-optical polymer and / or silicon and / or at least one compound semiconductor.

21. the longitudinal section (12) of the waveguide (11) is placed in contact or without contact on a planarization coating (2)(17), the planarization coating (2)(17) being characterized, at least in part, by a roughness in the range of 1.0 nm RMS to 0.1 nm RMS on the side on which the longitudinal section (12) of the waveguide (11) is placed, and / or 21. The photodetector (3) or modulator (22) according to any of the preceding claims, characterized in that the longitudinal section (12) of the waveguide (11) is at least partially embedded in the planarization coating (2) (17) on which one or both of the active elements (13) (13a) (13b) are arranged, and that the planarization coating (2) (17) on the side on which the active element (13) (13a) (13b) is arranged is at least partially characterized by a roughness in the range of 1.0 nm RMS to 0.1 nm RMS.

22. 22. The photodetector (3) or modulator (22) according to any of the preceding claims, characterized in that the longitudinal section (12) of the waveguide (11) comprises or consists of titanium dioxide and / or aluminium nitride and / or tantalum pentoxide and / or silicon nitride and / or aluminium oxide and / or silicon oxynitride and / or lithium niobate and / or silicon and / or indium phosphate and / or gallium arsenide and / or indium gallium arsenide and / or aluminium gallium arsenide and / or at least one dichalcogenide and / or chalcogenide glass and / or a heterostructure of two-dimensional materials and / or a resin or resin-containing material and / or a polymer or polymer-containing material.

23. A semiconductor device comprising a chip and at least one photodetector (3) and / or modulator (22) according to any of the claims 1 to 22.

24. 24. The semiconductor device according to claim 23, characterized in that the photodetector (3) and / or the modulator (22) are part of a photonics platform fabricated on or bonded onto the chip.

25. A semiconductor device comprising a wafer (1) and at least one photodetector (3) and / or modulator (22) according to any one of the claims 1 to 22.

26. 26. The semiconductor device of claim 25, wherein the photodetector (3) and / or the modulator (22) are part of a photonics platform fabricated on or bonded to the wafer (1).