linerless film stack
Patent Information
- Application Number
- JP2023522759
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-10-14
- Filing Date
- 2021-10-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-10-08
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Background Art
[0001] Film stacks are used in many applications. For example, an overlaminate film stack is used for printed or imaged graphics film, particularly for graphics film applications to protect and provide durability to ink. Liners are typically used to protect any pressure-sensitive adhesive prior to installation.
Summary of the Invention
[0002] In one aspect, the present specification relates to a film stack. The film stack sequentially includes a first base substrate, a first pressure-sensitive adhesive, a release layer, a second pressure-sensitive adhesive, and a second base substrate. The first base substrate, the first pressure-sensitive adhesive, the release layer, the second pressure-sensitive adhesive, and the second base substrate are coextrudable.
[0003] In another aspect, the present specification relates to a method of forming a film. The method includes coextruding a melt stream sequentially including a first base substrate, a first pressure-sensitive adhesive, a release layer, a second pressure-sensitive adhesive, and a second base substrate. The method includes expanding the melt stream and quenching the melt stream to form a film.
Brief Description of the Drawings
[0004] [Figure 1] It is a schematic side cross-sectional view of a film stack.
Modes for Carrying Out the Invention
[0005] Film stacks can be used in many different situations to supply users with film in the appropriate format. In some cases, the film contains adhesive, and the stack is designed to protect the adhesive during transport, storage, or conversion. Often, these film stacks include a paper or polymer liner attached to the adhesive surface, which would otherwise be exposed. Paper liners or polymer materials are conventionally formed in different steps. This typically requires additional manufacturing and attachment steps, which can further complicate the manufacturing process.
[0006] In some embodiments, these film stacks may be paint-protecting films or other surface-protecting films. In some cases, these film stacks may be graphics films or overlaminates, or may include graphics films or overlaminates. Overlaminates are used with graphics films to protect or enhance the durability of the printed base graphics film. Overlaminates may provide physical protection against abrasion or ambient conditions. Overlaminates may help extend the usable or optimal lifespan of printed graphics film products. Conventionally, overlaminates are laminated onto the printed base graphics film during or after printing.
[0007] Figure 1 is a schematic side cross-sectional view of a film stack. Figure 1 includes a film stack 100 comprising a first base substrate 110A, a second base substrate 110B, a first pressure-sensitive adhesive 120A, a second pressure-sensitive adhesive 120B, a release layer 130, an optional first bonding layer 112A, an optional second bonding layer 112B, an optional first protective layer 114A, and an optional second protective layer 114B.
[0008] The first base substrate 110A and the second base substrate 110B may be any suitable material and may be formed by any suitable process. In some embodiments, the first or second base substrate contains or is made from polyvinyl chloride. In some embodiments, the first or second base substrate contains polyurethane and cellulose acetate propionate or cellulose acetate butyrate. In some embodiments, the first or second base substrate layer contains or is made from polyester or copolyester. In some embodiments, the first or second base substrate contains or is made from an ionomer resin of an ethylene-methacrylic acid copolymer. In some embodiments, the first or second base substrate contains or is made from ethylene vinyl acetate (EVA). In some embodiments, the first or second base substrate comprises or is made from polycarbonate, polypropylene, polylactic acid, or polystyrene. In some embodiments, the first or second base substrate layer comprises or contains an elastomer component. Polyamides and polyamide-containing block copolymers may be preferred. Specific materials or combinations of materials may be selected for their physical, optical, and / or rheological properties. In some embodiments, the first or second base substrate may comprise two or more layers, the two or more layers comprising the same or different materials. In certain embodiments, the first base substrate 110A and the second base substrate 110B may be formed from the same or similar materials, or from the same or different materials. In some embodiments, the first base substrate and the second base substrate may have the same thickness and material.
[0009] The first and second base substrates may have any preferred thickness and may be formed by an extrusion process (e.g., melt extrusion, also called multilayer cast film extrusion or simply cast film extrusion, or blown film molding). In some embodiments, each or either of the first and second base substrates has a thickness of 25 to 100 micrometers. The first and second base substrates may have a smooth surface structure or a textured surface structure.
[0010] An optional first protective layer 114A and an optional second protective layer 114B may be any suitable material and may be formed from any suitable process. In some embodiments, the first or second protective layer is more rigid than the base substrate. In some embodiments, the protective layer may be a polyolefin such as polypropylene, or may contain a polyolefin. In some embodiments, the protective layer may be any other suitable polymer, copolymer, or blend thereof, or may contain any other suitable polymer, copolymer, or blend thereof. The optional protective layer may have any suitable thickness, including 10 to 150 micrometers. The thickness and material may be selected to impart sufficient rigidity to the film stack and maintain a suitable peel force for delamination. In some embodiments, the 90-degree peel force for delamination may be 50 to 100 grams / inch (about 20 to 40 grams per centimeter). The removable skin layer may be extruded (melt extrusion or blow film molding), solvent cast, or coated. In some embodiments, the optional first protective layer and the optional second protective layer may be made of the same material or different materials. In some embodiments, the optional first protective layer and the optional second protective layer may be made of the same material and thickness.
[0011] The first pressure-sensitive adhesive 120A and the second pressure-sensitive adhesive 120B are placed between the release layer 130 and the first base substrate 110A or the second base substrate 110B, respectively. The first and second pressure-sensitive adhesive layers may be any suitable adhesive, including an acrylic adhesive, epoxy, or an optically transparent adhesive. Particularly in the case of transparent or translucent base substrates, the optical properties of the adhesive (typically high transmittance, low haze, and high clarity) may be important for maintaining the overall appearance of the film in use.
[0012] In some embodiments, the first or second pressure-sensitive adhesive may have a structure sufficient to maintain its shape (i.e., not flow) over a wide range of exposure temperatures and humidity. In some embodiments, the adhesive may be fully or partially crosslinked (before or after extrusion, if extruded). The adhesive may contain pigments, dyes, or other colorants. In some embodiments, the thickness of the adhesive may be 10 to 100 micrometers. In some embodiments, the adhesive may contain partially embedded microbeads made from materials such as glass, ceramic, or polymer resin, or aggregates thereof held together with a suitable binder material. In some embodiments, the microbeads may be index-matched to the structured adhesive and / or transparent.
[0013] In some embodiments, the first pressure-sensitive adhesive and the second pressure-sensitive adhesive may be made of the same material or different materials. In some embodiments, the first pressure-sensitive adhesive and the second pressure-sensitive adhesive may have the same thickness and be made of the same material.
[0014] Since the base substrate layer may not bond well to the pressure-sensitive adhesive, some embodiments may include an optional first bonding layer 112A and an optional second bonding layer 112B. The bonding layer, often also called a primer layer, may be any suitable material or composition having any suitable thickness. The choice of bonding layer is to ensure sufficient adhesion between the base substrate layer and the pressure-sensitive adhesive (to prevent plybold breakage). In some embodiments, the bonding layer may include a polyamide or copolyamide. Certain materials may be useful as an alternative or additional barrier layer to prevent migration of plasticizers, water, solvents, or other contaminants from the front of the film stack to the adhesive. The bonding layer may be very thin, with a thickness of less than 10 micrometers, less than 6 micrometers, less than 5 micrometers, less than 4 micrometers, less than 3 micrometers, less than 2 micrometers, or even less than 1 micrometer. The bonding layer may be solvent-cast, coated, or even extruded or co-extruded (together with one or more of the other layers).
[0015] If the first and second pressure-sensitive adhesives are intended to separate near or during application, a release layer 130 may be provided as part of the film stack 100 to protect the first and second pressure-sensitive adhesives from unintended self-adhesion. The release layer 130 may be silicone, wax, block copolymer, or any other suitable material. In some embodiments, it may be advantageous to use a release layer instead of a conventional release liner. A release liner is conventionally a relatively thick paper or polymer material with a thin coating for release properties. Most release liners are intended to prevent damage during storage and to impart rigidity to the film structure. In the embodiments described herein, since the release layer is embedded within the film stack, it does not need to provide mechanical or physical protection and can be made very thin. In some embodiments, the release layer 130 may be 10 to 150 micrometers thick. Furthermore, as a single layer compared to a coated liner material, co-extrusion in a single step may be more feasible in the release layer structure compared to conventional coated release articles, which typically require lamination. In some embodiments, the entire stack is symmetrical on both sides of the release layer with respect to material composition and thickness.
[0016] The films described herein may enable simpler manufacturing steps. If the entire film stack is co-extrudeable (melt extrusion or blow film molding), multiple coating and / or lamination steps are not required during manufacturing. Furthermore, the release coating does not need to be supported by a liner substrate, and such structures may enable thinner film structures that can be manufactured at a faster rate. Such film stacks may result in improved economy (two functionally useful films for a given area) and reduced waste (a single release layer for two films, as opposed to a release liner for two separate films). Finally, if such films are converted to form similar parts (e.g., paint protective films where one or more vehicle surfaces can be molded identically or symmetrically), a single conversion step may result in two films instead of one.
[0017] The film stacks described herein can be formed using any preferred method. Certain embodiments described herein may be particularly suitable for co-extrusion and / or blow film processes. In some embodiments, this includes co-extruding a molten flow comprising a first base substrate, a first pressure-sensitive adhesive, a release layer, a second pressure-sensitive adhesive, and a second base substrate; expanding the molten flow (e.g., by air pressure in a blow film process, or by stretching); and quenching the molten flow by exposure to air, contact with a cooling roll, or by any other method to form a film. This film can be wound to form a roll. In some embodiments, the molten flow may include an optional bonding layer or an optional protective layer as described in relation to Figure 1.
[0018] The terms and expressions used are for illustrative purposes only, not limitation, and in using such terms and expressions, there is no intention to exclude any equivalent or part of the illustrated and described features, and it should be understood that various modifications are possible within the scope of the embodiments of the present invention. Accordingly, although the present invention is specifically disclosed by certain embodiments and optional features, it should be understood that modifications and variations of the concepts disclosed herein can be used by those skilled in the art, and such modifications and variations are considered to be within the scope of the embodiments of the present invention. [Examples]
[0019] A 7-layer gas-expanded co-extruded film structure was manufactured. The film was separated and its peel force was measured.
[0020] These examples are for illustrative purposes only and are not intended to limit the scope of the appended claims. All parts, percentages, ratios, etc., in the examples and elsewhere herein are based on weight unless otherwise indicated. The following abbreviations are used herein: um = micrometer, in = inch, mm = millimeter, cm = centimeter, °C = Celsius, min = minute, kg = kilogram, g = gram, %RH = percent relative humidity.
[0021] material: [Table 1]
[0022] Test method: Peel test After holding the test piece in a room at a constant temperature / humidity (23 °C and 50% RH) for 24 hours, it was tested. A 10-inch (25.4 cm) (machine direction) × 1-inch (2.54 cm) (transverse direction) test piece was cut from the center of the experimental sample. The bottom layer (7) was laminated onto a 1 mm × 55 mm × 350 mm aluminum panel that had been wiped clean twice with IPA using 3M Removable Repositionable Tape 9415PC (3M Company, St. Paul, MN). The film was rolled by passing a 2.05 kg hard rubber roller over it three times. The panel with the sample was conditioned at room temperature (approximately 23 °C) for approximately 15 minutes. The upper half (3 layers) was separated from the release layer (INFUSE 9507 layer) to expose the functional layer. The upper half (3 layers) was connected to the jaw of a peel tester (Model#80-91-00-001 of Testing Machines, Inc. (New Castle, DE 19720 USA)) and pulled at an angle of 90° at a speed of 30.5 cm / min (12 inches / min). The results were measured in grams. The values are the average of three tests for each sample.
[0023] Example: Examples were manufactured on a 7-layer pancake-type stack die (Type LF-400 Coex 7-layer of Labtech Engineering). The air flow to the die was manually adjusted to achieve an expansion ratio of approximately 2:1. Then, the air-expanded extrudate was collapsed on a die of approximately 10 feet (3 meters), passed through rollers in the transverse direction, and then wound around a 3-inch (7.6 cm) core and taken up. The feed materials were supplied by seven independent 20 mm diameter extruders (Labtech Scientific Single Screw Extruder Type LE20-30 / C HA). The functional layer materials (layers 3 and 5) were introduced as described in the examples of U.S. Patent No. 9,486,982 (Emslander et al.).
[0024] [Table 2]
[0025] Result: The peel strength between the functional layer and the release layer was 54 grams.
Claims
1. 1. A film stack comprising: A first base substrate; a first pressure sensitive adhesive; A release layer; a second pressure sensitive adhesive; and A second base substrate; In order, The film stack, wherein the first base substrate, the first pressure sensitive adhesive, the release layer, the second pressure sensitive adhesive, and the second base substrate are coextrudable.
2. 10. The film stack of claim 1, further comprising at least one of a first tie layer between the first base substrate and the first pressure sensitive adhesive and a second tie layer between the second base substrate and the second pressure sensitive adhesive.
3. The film stack of claim 2 , wherein at least one of the first tie layer and the second tie layer comprises a polyamide or a copolyamide.
4. 10. The film stack of claim 1, further comprising at least one of a first protective layer disposed on the first base substrate opposite the first pressure sensitive adhesive and a second protective layer disposed on the second base substrate opposite the second pressure sensitive adhesive.
5. The film stack of claim 4 , wherein at least one of the first protective layer and the second protective layer comprises a polyolefin.
6. The film stack of claim 1 , wherein the first base substrate and the second base substrate are the same material and thickness.
7. The film stack of claim 6 , wherein the first base substrate and the second base substrate comprise polylactic acid.
8. The film stack of claim 6 , wherein the first base substrate and the second base substrate comprise polyurethane.
9. The film stack of claim 6 , wherein the first base substrate and the second base substrate comprise an ionomer resin.
10. 10. The film stack of claim 8, wherein the first base substrate and the second base substrate comprise a copolymer of ethylene and methacrylic acid.
11. 7. The film stack of claim 6, wherein the first base substrate and the second base substrate comprise ethylene vinyl acetate.
12. 10. The film stack of claim 1, wherein the first pressure sensitive adhesive and the second pressure sensitive adhesive are the same material and thickness, and optionally, the first pressure sensitive adhesive and the second pressure sensitive adhesive are acrylic pressure sensitive adhesives.
13. The film stack of claim 1 , wherein the film stack is symmetrical on either side of the release layer in terms of material composition and thickness.
14. The film stack of claim 1 , wherein the release layer comprises an olefin block copolymer or a silicone resin.
15. 1. A method of forming a film, comprising: A first base substrate; a first pressure sensitive adhesive; A release layer; a second pressure sensitive adhesive; and A second base substrate; co-extruding a melt stream comprising, in order, expanding the melt stream; and quenching the melt stream to form a film; and A method comprising: