Method and single screw extrusion system for processing long fiber thermoplastic materials
Patent Information
- Application Number
- JP2023544615
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-09-28
- Filing Date
- 2021-09-28
- Publication Date
- 2024-10-07
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Current methods for producing long fiber thermoplastic (LFT) pellets face challenges in achieving economical and improved properties, particularly in maintaining long fiber lengths during the extrusion process, which is crucial for mechanical properties of injection molded parts.
A method involving a single screw extrusion system with separate inlet openings for feeding thermoplastic and thermoplastic composite (TPC) materials, allowing for controlled mixing and reduced fiber wear through localized heating and gentle conveying, which includes recycling waste materials like CFRT flakes and chips to produce high-quality LFT pellets.
The method achieves high fiber retention and long fiber lengths in LFT pellets, enhancing mechanical properties while being economically viable and environmentally friendly by utilizing waste materials.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for producing long fiber thermoplastic (LFT) extruded material, long fiber thermoplastic (LFT) material, and a single-screw extruder. [Background technology]
[0002] In one aspect, the present invention relates to a method for producing long fiber thermoplastic (LFT) materials, and more particularly, a method for producing LFT extruded materials (extruded products). LFT materials may also be referred to as long fiber reinforced thermoplastic materials. LFT extruded materials can be used to produce a variety of products containing LFT materials, such as parts in automobiles, such as vehicle door panels, instrument carriers, or front ends, and parts in other fields, such as electronic equipment. LFT extruded materials are used, for example, as raw materials for injection molding to form LFT products. LFT extruded materials are cut, for example, into pellets, and the pellets are used for injection molding. Injection molding of LFT materials is known as such, and often LFT pellets are used as feed material. Such LFT pellets are, for example, 5 mm to 15 mm in length, preferably about 11 mm in length, and have a diameter of, for example, 1 to 5 mm. Individual LFT pellets contain fibers (e.g., carbon fibers, glass fibers, or natural fibers) and a thermoplastic polymer. The method of the present invention can be used to produce such pellets in an improved and / or more economical manner.
[0003] Current exemplary methods for producing LFT pellets are based on wire coating or thermoplastic pultrusion using dry, continuous fibers. Here, "dry" indicates, for example, that the fibers are not yet embedded in the thermoplastic material. For example, in some prior art methods for producing LFT pellets, the dry fibers are wire-coated with a thermoplastic polymer. Wire coating and pultrusion give strands of coated or impregnated fibers, respectively, which are dimensioned (e.g., cut) into pellets of, for example, 11 mm in length. Longer pellets are difficult to process by injection molding. The fibers are continuous and aligned within the strands obtained by wire coating and pultrusion. In individual pellets produced by cutting such strands, the fibers are aligned parallel to each other and extend in a parallel arrangement along the length of the pellet. In typical production methods currently available for producing LFT pellets, the fiber length is equal to the pellet length. Longer fibers are desirable because they contribute to the mechanical properties of the injection-molded LFT parts. Extrusion, which differs from pultrusion, is not commonly used to produce LFT strands or pellets.
[0004] It is desirable to provide a method for producing LFT material (e.g., LFT pellets) such that the produced LFT material is suitable for further manufacturing steps (e.g., LFT injection molding or further extrusion processes) for producing LFT articles, and the method provides an LFT material that is more economical and / or has improved properties.
[0005] Patent Document 1 describes a method for producing fiber-reinforced plastic compositions, in which an apparatus equipped with a double-screw plasticizing extruder is used, and molten plastic and fiber material are combined at the entry opening of the plasticizing extruder.
[0006] Patent Document 2 describes a method for producing fiber-reinforced plastic ingots by using a plasticizing extruder, in which fibers and thermoplastic granules and / or long fiber-reinforced recycled chips are plasticized and extruded as a plasticized material that can be further processed. Large-sized long fiber-reinforced recycled chips having a circular area of approximately 50 mm in diameter and a length of up to 200 mm are weighed and introduced into a heated tube worm conveyor device, where they are preheated and dried to the point just before they become sticky. The chips are then introduced into a plasticizing extruder. [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] U.S. Patent Application Publication No. 2002 / 0089082 [Patent Document 2] European Patent No. 1008435 [Overview of the project] [Means for solving the problem]
[0008] In a first embodiment, the present invention relates to a method for producing long-fiber thermoplastic (LFT) extruded material, A) Providing a first feedstream containing a thermoplastic material; B) A step of providing a second feedstream comprising a thermoplastic composite (TPC) feed material (e.g., flakes or chips), wherein the TPC feed material comprises pieces, preferably, the pieces separately comprising both fibers and thermoplastic material, Includes, The method includes an extrusion step performed in an extrusion system, the extrusion system includes an extruder, The extruder includes a barrel, a single screw, and an outlet opening, and has an extrusion direction, the screw providing a channel within the extruder. The barrel comprises a first inlet opening and a second inlet opening, the first and second inlet openings being separate and spaced apart from each other, with the second inlet opening located downstream of the first inlet opening in the extrusion direction. The push step is, C) The steps of supplying the first feedstream into the channel in the extruder through the first inlet opening, and transporting the first feedstream from the first inlet opening to the second inlet opening by the screw; D) The steps of supplying the second feedstream through the second inlet opening into the channel in the extruder, thereby combining and mixing the first and second feedstreams inside the channel in the first mixing zone of the extruder to give a first mixed material; F) A step of conveying the stream containing the first mixed material through the outlet opening to provide LFT extruded material, This includes methods.
[0009] In a further embodiment, the present invention relates to long-fiber thermoplastic (LFT) materials obtainable by this method.
[0010] In a further embodiment, the present invention relates to pellets comprising fibers and a thermoplastic material, wherein the pellets have a length and a diameter, the fibers are preferably oriented in the longitudinal direction of the pellet, preferably at least partially curved, preferably at least some of the fibers in the pellet have a length greater than the length of the pellet, and at least some of the fibers in each individual pellet have a length less than the length of the pellet.
[0011] In a further aspect, the present invention relates to a single screw extrusion system for producing a long fiber reinforced thermoplastic material, the single screw extrusion system comprising an extruder barrel, an axially rotatable extruder screw within the extruder barrel, and a die including an exit opening, the screw including a shaft and one or more helical flights, the barrel including a first inlet and a second inlet, the first inlet, the second inlet, and the exit being spaced apart from each other, the first inlet being provided with a first feeder, and the second inlet being provided with a second feeder. The extrusion system is preferably suitable for the method. The method is preferably carried out by the extrusion system.
Brief Description of the Drawings
[0012] [Figure 1] FIG. schematically shows an exemplary extrusion system according to the present invention. [Figure 2A] FIG. schematically shows an exemplary method according to the present invention, showing in particular exemplary extrusion steps and some other steps. [Figure 2B] FIG. schematically shows an exemplary method according to the present invention, showing some exemplary steps for providing a second feed stream. [Figure 3] FIG. schematically illustrates a comparative method. [Figure 4] FIG. schematically shows an exemplary extrusion system according to the present invention. [Figure 5] FIG. schematically shows a suitable die head of an extrusion system according to the present invention. Panel A illustrates a suitable tapered die head and Panel B illustrates a straight die head. [Figure 6] FIG. schematically shows an exemplary extruder setup. [Figure 7] FIG. shows a histogram.
Embodiments for Carrying out the Invention
[0013] The figures are for illustrative purposes only and do not limit the present invention.
[0014] The present invention is based broadly on the insightful observation that suitable LFT material (e.g., LFT pellets) for manufacturing LFT articles (e.g., by LFT injection molding and / or extrusion molding) can be produced in an advantageous manner by using an extrusion step carried out in an extruder including a screw (preferably in a single-screw extruder), wherein the thermoplastic material is supplied into the extruder as a first feedstream at a first inlet opening, and the TPC feed material (e.g., TPC chips and / or flakes) is supplied into the extruder as a second feedstream at a downstream second opening, so that the TPC feed material is compounded with the thermoplastic material. Surprisingly, this has been found to allow for low fiber wear during the extrusion process.
[0015] The first and second feedstreams are different from each other.
[0016] The abbreviation "TPC" as used herein stands for "thermoplastic composite."
[0017] The second feedstream includes TPC feed material. The TPC feed material includes, for example, TPC chips and / or TPC flakes, and / or, for example, TPC pellets. Other TPC feed materials are also possible. The TPC feed material includes, for example, discrete solid pieces of TPC material. The TPC feed material is provided, for example, as a stream of solid pieces of TPC material. The pieces include, for example, TPC chips and / or TPC flakes.
[0018] The abbreviation "LFT" stands for "long fiber thermoplastic." As used herein, a long fiber thermoplastic material refers to a material comprising, substantially, or essentially comprising a thermoplastic polymer and long fibers, where the polymer can be, for example, a raw polymer or a polymer compounded with additives. The long fibers have a typical length of 0.5 mm to 50 mm, more preferably 1 mm to 20 mm, and most preferably 2 mm to 10 mm, and optionally have a typical diameter of 1.0 to 100 μm, 2 to 50 μm, and most preferably 5 to 30 μm. In LFT materials, the long fibers are embedded in a thermoplastic polymer, for example, as in the case of fibers impregnated with a thermoplastic polymer. In exemplary embodiments, the TPC feed material comprises an LFT material, and the fibers are embedded in a thermoplastic polymer. Preferably, the TPC feed material, in particular solid pieces, especially preferred chips or flakes, contains fibers, these fibers having lengths of, for example, 0.5 mm to 50 mm, more preferably 1 mm to 20 mm, and most preferably 2 mm to 10 mm, and optionally having typical diameters of 1.0 to 100 μm, 2 to 50 μm, and most preferably 5 to 30 μm.
[0019] As used herein, thermoplastic composite (TPC) materials refer to materials comprising, substantially from, or essentially from, thermoplastic polymers and (dried, impregnated, short, long, and continuous) fibers (or mixtures thereof), where the polymer can be, for example, a raw polymer or a polymer compounded with additives, and the fibers are, for example, dried or impregnated, and are, for example, short or long or continuous, or a mixture of any of such fibers. A TPC feed material as used herein is, for example, an LFT feed material. In some embodiments of TPC feed materials, the fibers are embedded in the thermoplastic polymer, for example, in the case of fibers impregnated with the thermoplastic polymer.
[0020] The TPC feed material is provided, for example, as a stream of solid pieces (i.e., discrete solid pieces) of the TPC material.
[0021] The discrete solid pieces typically have at least one dimension of at least 1.0 mm and at least two vertical dimensions of at least 1.0 mm. The discrete solid pieces preferably comprise fibers and thermoplastic material separately. These fibers preferably have a fiber length of at least 1.0 mm.
[0022] The second feedstream may include additional components, such as dried fiber fragments or particles of pure thermoplastic resin.
[0023] In exemplary embodiments, the TPC feed material may include flakes of TPC material having a thickness of at least 100 μm, typically less than 50 mm, and having a minimum size in the direction perpendicular to the thickness direction of at least 1 mm, at least 10 mm, or at least 100 mm. Discrete pieces of the TPC feed material typically have a size of less than 10 cm in at least one dimension.
[0024] The TPC feed material includes, for example, TPC flakes and / or TPC chips. Such TPC flakes more specifically have, for example, a length from 2 mm to 40 mm, a width from 2 mm to 40 mm, and a thickness less than the length and / or less than 5.0 mm, for example, a thickness from 0.1 mm to 4.0 mm. The TPC chips have, for example, a length (L) from 2 mm to 50 mm, a width (W) from 2 mm to 50 mm, and a thickness (H) of, for example, 0.1L < H < L. The TPC flakes have, for example, an aspect ratio L / H of at least 10, for example, at least 20. The TPC flakes have edges and two sides and, for example, have a surface area of at least 5 mm 2 or at least 10 mm 2 per each such side. TPC flakes having such dimensions are, for example, LFT flakes.
[0025] The TPC flakes can be obtained, for example, by cutting or shredding the material from a tape. The TPC chips can be obtained, for example, by crushing a CFRT (Continuous Fibre Reinforced Thermoplastic) material (such as by crushing a laminate or by crushing used parts of a TPC material). The TPC chips can also be obtained as production waste from a process for making a CFRT sheet. The TPC feed material (such as flakes and chips) is typically abrasive due to the fibre content.
[0026] In some embodiments, the TPC feed material includes, for example, size-reduced (such as crushed) waste material that contains or is composed of a TPC material. The TPC feed material is not limited to any particular thermoplastic polymer and is also not limited to any particular fibrous material.
[0027] Figure 1 schematically illustrates an example of a preferred method and apparatus according to the present invention. The apparatus includes an extrusion system (1), which includes an extruder (2). The extruder (2) includes a barrel (3) and a single screw (4). The screw (4) is axially rotatable. The barrel is a hollow container, typically a cylindrical container having length and diameter. The screw is located inside the barrel, typically within the length of the barrel, and includes a cylindrical shaft (11) and flights (12) (typically one or more helical flights). The flight pitch is shown only schematically. The screw provides a channel (8) in the extruder adapted to receive the material to be extruded. During operation, the material to be extruded is received into the channel through an inlet and transported in the extrusion direction (ED) to an outlet opening (5) by rotating the screw. The material, due to the shearing action of the screw and barrel, melts at least partially within the channel, forming a molten mass, which is then extruded into the extruded material at an exit opening typically provided into the die.
[0028] In the method of the present invention, a first feed thermoplastic material (A) is supplied into the channel through a first inlet opening (6) and received into the channel (8). The first feed material is transported through an extruder over a distance (S1) to a downstream second inlet opening (7). The thermoplastic material is already at least partially melted when it arrives at the second inlet opening (7) (where the TPC feed material (B) is introduced into the extruder), and is combined and mixed with the at least partially melted first feed thermoplastic material in the mixing zone (9) of the extruder (2) to give a first mixed material (C).
[0029] As an independent preferred feature, the extruder includes a heating element (10), which is located inside the screw (for example, inside the shaft). The heating element is, for example, a resistance heater. The heating element is adapted to selectively heat the first compounding material (C) in the mixing zone (9) of the channel (8). This localized heating locally reduces friction in the extruder, thereby providing good mixing of the TPC feed material (B) of the second feedstream and the molten first feed material (A) with an advantageously lower fiber breakage rate. The resulting compounding material (C) is transported to the die (15), and the extruded material (D) is received from the exit opening (5). As an independent preferred feature, the die (15) is tapered in the extrusion direction as shown in Figure 1. The extrusion system (1) further includes a first feeder (16) for a first inlet opening (6) and a second feeder (17) for a second inlet opening (7). The second feeder is, for example, a cramma feeder. The second feeder is equipped with, for example, a heating element (not shown) for heating the TPC feed material before it enters the extruder.
[0030] Particularly advantageous is that the TPC feed material used in this invention can be waste material. This provides the advantage that this method is an environmentally friendly way to process materials and that TPC raw materials are economical. This invention provides a method for recycling certain materials that have previously been considered waste materials.
[0031] Furthermore, the process of the present invention provides a highly sophisticated method for converting waste material into high-quality recyclable LFT material (for example, high-quality LFT pellets that can be used for LFT injection molding).
[0032] In a very preferred embodiment (but not limiting the invention), the TPC feed material includes separated side edges (e.g., trims) of an impregnated fiber layer (e.g., an impregnated fiber tape or sheet). Such a tape is an intermediate step in a particular production method for continuous fiber-reinforced material. The material can also be, for example, chips resulting from the crushing of CFRT material (e.g., CFRT sheets or CFRT articles, e.g., CFRT automotive parts).
[0033] In some embodiments, the method for producing LFT extruded material according to the present invention provides continuous recycling of fiber-reinforced thermoplastic (CFRT) waste material. In some embodiments, the present invention relates to a method for producing LFT extruded material, the method comprising the step of providing such separated side edges as at least a portion of a second feedstream.
[0034] Furthermore, in some embodiments, the second feedstream is provided at least partially by a recycling stream from the processes for manufacturing CFRT materials and CFRT parts, components, and articles, and / or a recycling stream from used CFRT articles.
[0035] In a preferred embodiment (which does not limit the present invention), step B, which provides a second feed material, B1) A step of providing dry, continuous fibers, B2) The step of impregnating the fibers with a thermoplastic resin to provide a continuous sheet of impregnated fibers having edges, B3) A step of separating at least a portion of the edges from the continuous sheet of impregnated fibers to give a flake and trimmed continuous sheet, wherein the flake is the separated edge piece, and the flake contains fibers and thermoplastic material separately. B4) The step of using the flakes as at least a portion of the second feed, B5) Optionally, a step of sizing a trimmed continuous sheet into a sheet or tape, and optionally, a step of creating a laminate from the sheet or tape, This includes the following: Sheets, tapes, or laminates are, for example, placed in a mold and subjected to molding (for example, by heat) to become molded CFRT articles.
[0036] Figure 2 schematically illustrates an example of a preferred method according to the present invention. In this preferred embodiment (it is not limited to the present invention), a method for producing LFT extruded material includes an extrusion step (205) using thermoplastic resin (TP) and TPC material, for example, LFT material (for example, streams A1, A2, A3, A4 as shown in Figure 2B, and combinations thereof with each other and / or other streams), as illustrated in Figure 2A, to give LFT extruded material strands, the LFT extruded material strands being sized (206) (i.e., dimensioned, pelletized) to become LFT pellets. The LFT pellets are then optionally injection molded or extruded (207) to give LFT parts, which are, for example, LFT articles or LFT components.
[0037] In this preferred embodiment, the step of providing a second feed material includes a process for producing a CFRT material (Figure 2B). The process includes impregnating continuous dry fibers (e.g., glass fibers, natural fibers, or carbon fibers) with a thermoplastic polymer resin (201) to give an impregnated continuous sheet or tape (single-layer sheet). The fibers are supplied, for example, as a woven or nonwoven fabric, or as a unidirectional tape. The sheet (having lower-quality edges) is typically processed to remove these edges (202) (e.g., trimmed). The removed edges are cut or shredded to reduce their size (202A) and collected as LFT flakes (A1). In an exemplary embodiment, the TPC feed material is supplied by feeding such LFT flakes into an extrusion step. The sheet, with the edges removed, is still a continuous sheet and is laminated to a CFRT material (e.g., a CFRT laminate) (203). The CFRT laminate is, for example, trimmed (204), giving the trimmed laminate ("blank") and trimming waste. The trimming waste is, for example, sized (e.g., crushed) to become LFT chips (A2) which are used as at least part of the TPC feed material.
[0038] CFRT material may be used for processing (208) to give CFRT articles. For example, processing (208) involves shaping the material by placing solid CFRT material (e.g., CFRT blanks, etc.) in a mold and closing the mold, as well as shaping the material using heat and / or pressure to give a shaped CFRT article. The shaping step is typically carried out separately from the manufacture of CFRT sheets (e.g., after storage and transport of CFRT material). Off-spec articles from processing (208) may optionally be sized to become chips (A3) to be used as at least part of TPC feed material (e.g., crushed). Furthermore, used CFRT articles (e.g., consumed articles) may optionally be sized to become chips (A4) to be used as at least part of TPC feed material (209) (e.g., crushed, etc.). The illustrated TPC feed materials (A1, A2, A3, and A4) are merely examples and in no way limit the invention.
[0039] LFT flakes resulting from the edge removal step (202) (for example, from the edge trimming step) are considered waste in the prior art and are burned in an incinerator, for example, or ground into dust in a grinding step in the prior art method. In the present invention, LFT flakes (and other types of TPC material as well as LFT flakes) are used as TPC feed material for the extrusion step (205) according to the present invention and as a second feed stream together with a separate first feed stream containing thermoplastic material to produce LFT extruded material (extruded product). The method of the present invention generally, and more preferably, includes the step of pelletizing (206) the LFT extruded material from the extrusion step (205) to give LFT pellets. These pellets may optionally be stored and / or transported and may optionally be further used for LFT injection molding, for example.
[0040] Each LFT pellet contains fibers and thermoplastic material. LFT pellets can be used, for example, for LFT injection molding (207). A comparative preparation method for producing LFT pellets is based on the steps of: combining (208) continuous fibers and thermoplastic resin to give a continuous strand, where the combining step is, for example, wire coating or pultrusion; and a further step of sizing (209) the strand into LFT pellets.
[0041] The LFT pellets according to the present invention are very suitable for LFT injection molding. In such an LFT injection molding process (207) (which is an optional further step of the method of the present invention), the LFT pellets are heated so that the thermoplastic fraction melts and the molten material containing fibers is injected into a mold. The mold is closed and the material inside the mold solidifies, giving an injection-molded LFT part, which is a molded article containing a thermoplastic polymer and fibers. The fibers preferably have a relatively long length within the molded article. The injection-molded LFT part is, for example, an automotive part.
[0042] In this preferred embodiment of the present invention, TPC flakes and TPC chips, which are obtained as essentially waste materials in a normal CFRT manufacturing process, are surprisingly and very advantageously recycled into high-value products. This embodiment of the present invention is very advantageous compared to currently used methods, such as incinerating the flakes or chips, or grinding the flakes or chips into dust (which can be used as a low-cost filler).
[0043] Figure 3 schematically illustrates a comparative method for producing LFT articles that is not according to the present invention. Here, a thermoplastic resin and continuous dried fibers are combined in a process (305) (e.g., pultrusion or wire coating) to give LFT strands, which are then sized (e.g., cut) (306) into pellets. The pellets can be used for LFT injection molding and / or LFT extrusion (307).
[0044] In a preferred embodiment, the TPC feed material of the second and / or optional third feedstream comprises flakes, chips, crushed material from a CFRT waste stream, or a combination thereof, more preferably comprising at least 90% by weight or at least 95% by weight of each of the second and third feedstreams. The flakes or chips are preferably composed of TPC material and can be obtained from any suitable source.
[0045] Accordingly, the present invention relates, in one aspect, to a method for producing long-fiber thermoplastic (LFT) extruded materials (e.g., extruded strands or pellets). The method includes the step of providing a first feedstream containing thermoplastic material and a separate second feedstream containing TPC feed material. The first and second feedstreams are different from each other, and in particular, the feedstreams have different chemical compositions.
[0046] The first feedstream generally, preferably, does not contain fibers, and more preferably, does not contain thermosetting polymer fibers or nonpolymer fibers, or preferably contains less than 5.0% by weight or less than 1.0% by weight of such fibers in total relative to the total of the first feedstream. Preferably, the first feedstream contains less than 5.0% by weight of carbon fibers, less than 5.0% by weight of glass fibers, and / or less than 5.0% by weight of natural fibers.
[0047] The first feedstream is preferably a solid material and is introduced into the extruder in the form of pellets. The first feedstream preferably contains at least 80% by weight or at least 90% by weight of a thermoplastic polymer in total, relative to the total weight of the first feedstream. The first feedstream may contain one or more thermoplastic polymers. The first feedstream preferably contains at least 80% by weight of an unreinforced thermoplastic polymer, which can be, for example, a virgin polymer, a recycled polymer, or a combination thereof.
[0048] The TPC feed material for the second feedstream and preferably a third feedstream generally includes, for example, flakes or chips of TPC material (preferably LFT material). The TPC feed material includes pieces of TPC material (e.g., flakes or chips), and preferably, the individual pieces include fibers and thermoplastic material. In a preferred embodiment, at least the second or third feedstream, or both, include LFT material to supply long fibers for LFT products. As discussed herein, the TPC feed material may be obtained from the production process of CFRT material or CFRT articles or parts, or from used CFRT articles or parts. CFRT articles are, for example, woven, nonwoven, or unidirectional CFRT articles. The TPC feed material may be obtained from, for example, common LFT parts and articles (e.g., from LFT injection-molded parts and articles and / or LFT extruded parts and articles, etc.), for example, by crushing used LFT parts and articles. TPC feed material can also be obtained as production waste from the methods used to manufacture LFT parts and articles.
[0049] The TPC feed material, preferably as an LFT feed material, comprises segments, each segment consisting of, for example, at least partially impregnated fibers, which are partially or entirely impregnated with a thermoplastic polymer. The TPC feed material may also contain other components (e.g., dried fibers).
[0050] The TPC feed material comprises, for example, substantially only one thermoplastic polymer, and for example, at least 90% by weight of the thermoplastic fraction of the TPC feed material is a single polymer. Preferably, the polymer or polymer blend of the TPC material is the same polymer as the polymer or polymer blend used in the first feed material.
[0051] Thermoplastic polymers are polymers selected from the group consisting of, for example, polyolefins, polyamides, polycarbonates, polyphenylene sulfides, polyaryl ether ketones, and polyethyleneimines.
[0052] The term “thermoplastic polymer” as used herein includes at least plastic polymers, which become flexible or moldable at certain elevated temperatures and solidify upon cooling.
[0053] In some embodiments (without limiting the present invention), the thermoplastic polymer is not crosslinked and is not cured.
[0054] Preferably, the first feed material comprises at least 80% by weight of the total first feed material, which is the same polymer or polymer blend used for at least 80% by weight of the TPC feed material.
[0055] The TPC feed material of the second feedstream includes fibers, which are selected from the group consisting of, for example, glass fibers, carbon fibers, and natural fibers. Preferably, the natural fibers are selected from the group consisting of, for example, hemp fibers, flax fibers, jute fibers, and cellulose fibers.
[0056] The TPC feed material may contain additional fibers. For example, the TPC feed material may contain at least 20% by weight of fibers or at least 30% by weight of fibers, and typically less than 80% by weight of fibers. The TPC feed material may contain, for example, 30% to 70% by weight of fibers, or, for example, 50% to 70% by weight of fibers. The TPC feed materials for the second and third feeds may have different fiber content, such as differing by at least 5 absolute percentage points or at least 10 absolute percentage points. Thus, variations in the fiber content of the first, second, and / or third feed streams can be offset by adjusting the feed rates of the first, second, and / or third feeds.
[0057] This method includes an extrusion step carried out in an extrusion system. The extrusion system includes an extruder, which includes a barrel, the barrel having a screw and an outlet opening. The outlet opening is provided in a die at the downstream end of the extruder. The extruder has an extrusion direction that is in the longitudinal direction of the screw toward the outlet opening. The extruder is a single-screw extruder, as opposed to a twin-screw extruder. Thus, the barrel contains at most one screw at each position along the length of the barrel.
[0058] The screw provides a channel within the extruder. The channel is an open space provided between the screw shaft, flights, and the inner wall of the barrel. The barrel is, for example, a cylindrical container. During operation, the material is conveyed in the extrusion direction through the channel by the rotational action of the screw.
[0059] The extruder includes a first inlet for a first feedstream and a separate second inlet for a second feedstream. The first and second inlets are spaced apart from each other in the extrusion direction. The second inlet opening is located downstream of the first inlet opening in the extrusion direction. The second inlet opening is spaced apart from the first inlet opening by, for example, only 10% or 20% of the screw length, and typically less than 90% or 80% of the screw length. This provides good mixing of the second feedstream (in particular, TPC feed material) and the first feedstream, and good extrusion in the die.
[0060] The first inlet includes a first opening in the barrel for supplying a first feed material to the screw. The second inlet includes a second opening in the barrel for supplying a second feed material to the screw. The method of the present invention includes the steps of supplying a first feed material into the extruder through the first inlet and supplying a second feed material into the extruder through the second inlet.
[0061] In this method, the first feedstream is introduced into the extruder through an inlet located upstream of the inlet for the second feedstream. Thus, the first feed material is conveyed by the screw over at least some distance from the first inlet to the second inlet. Furthermore, the screw channel is already partially filled with material in the section of the extruder into which the second feedstream is supplied, but not completely filled. Thus, the second inlet provides a mixing zone within the extruder, in which the initially separate first and second feed materials are combined and compounded by the action of the screw present in the zone. The compounded material is then further conveyed by the screw through the channel toward the die of the extruder, preferably, a third feedstream is added through a third inlet opening, which is located downstream of the second inlet opening and spaced apart from it. In the die, the compound material passes through the die or nozzle to give extruded LFT material, in particular extruded strands. The conveying step, as discussed, includes rotating the screw (preferably with low shear) to reduce fiber wear.
[0062] This offers the advantage that, preferably, high fiber fractionation can be achieved in LFT extruded materials, and similarly, large fiber lengths can also be achieved.
[0063] In the present invention, the first, second, and optional third inlet openings are each provided as openings within the barrel at predetermined positions in the extrusion direction (and at predetermined positions in the barrel length), where a screw is also provided. The barrel is typically a cylindrical container having a length and diameter. The first, second, and optional third inlet openings are each individually provided at such positions in the barrel length, perpendicular to the barrel length, such that the cross section of the barrel passing through the inlet opening also passes through the screw.
[0064] In the present invention, an extruder including first, second, and an optional third inlet opening also includes a die. Therefore, the die is typically positioned parallel to the screw and in the projection direction of the screw into the extrusion direction. The die is typically mounted or attached to a barrel containing these inlets.
[0065] In a preferred embodiment, the method includes the step of selectively heating a portion of the screw by at least one heating element, which is positioned in the screw at a predetermined location in the extrusion direction downstream of a second inlet opening. The heating element is, for example, a tracing. The localized heat supply advantageously provides relatively lower friction of the material in the channel where the heating element is positioned (compared to the case where such heating is omitted), which provides reduced shear and therefore a gentler mixing of the introduced material and the material already present in the channel (e.g., material from the first inlet). Thus, fiber wear and breakage are reduced and the length of long fibers is maintained.
[0066] In a preferred embodiment, the method further includes the step of providing a third feed stream containing TPC feed material, wherein the extruder includes a third inlet opening for the third feed stream. The third inlet opening is located downstream of the second inlet opening at a distance from it. The extrusion step more preferably includes the step of transporting the first compound material from the first mixing zone to the third inlet opening by a screw; and the step of supplying the third feed stream through the third inlet opening into a channel inside the extruder. Thus, the method preferably includes the step of mixing the first compound material with the third feed stream inside the channel in the second mixing zone of the extruder (2) to provide a second compound material. The method more preferably includes the step of transporting the stream containing the second compound material to a die, particularly through an outlet opening (e.g., through a nozzle), to provide LFT extrude material.
[0067] Figure 4 schematically illustrates a preferred method and apparatus according to the present invention. Reference numerals are the same as those in Figure 1 unless otherwise specified. The pitch of the flights (12) is schematically illustrated. The extruder includes a third inlet (13) for a third feedstream (E) containing TPC feed material. This TPC feed material may have the same or a different composition as the second feedstream (B). The third inlet opening (13) is configured to supply the third feedstream (E) into a channel (8) in the extruder (2). Thus, the first compounding material (C) is compounded in combination with the third feedstream (E) inside the channel (8) in the second mixing zone (14) of the extruder (2). This provides a second compounding material (F), which is then transported to a die (15) and, optionally, after the addition of further components through an optional further inlet opening, is transported through the die's exit opening (5) to provide LFT extruded material (D). A third inlet opening (13) is provided with a feeder (18). Preferably, the first, second, and third feeders (16, 17, 18) are each provided with drivers for providing feed into the inlet opening at a variable feed rate. Preferably, the second and third feeders (17, 18) are each provided with gravimetric sensors for measuring the gravimetric density of the feed material. This density can be used to determine the fiber content of the feed material. The extrusion system (1) further includes a controller (19) for adjusting the feed rates of first, second, and third feeders (16, 17, 18) using information from a gravimetric sensor to compensate for changes in the fiber content of the feedstream, thereby obtaining a controlled fiber content in the extruded material. This advantageously provides, among other things, homogenization of the fiber weight fraction of the output material when the second and / or third feeds are waste material that will be recycled by the method of the present invention, at least in part.
[0068] The third inlet opening (13) is arranged at a distance (ΔS2) from the second inlet opening (7), which enables effective mixing. The third inlet opening (13) is arranged at a distance (ΔS3) from the die (15), which enables good extrusion.
[0069] In a preferred embodiment of the method and the pellets of the present invention, the long fiber reinforced thermoplastic material obtained by the method and / or the pellets contains 20 to 75% by weight (preferably 30 to 60% by weight) of fibers based on the total weight of the long fiber reinforced thermoplastic material. Such a high fiber fraction contributes to good mechanical properties of the articles and parts prepared from the material.
[0070] In a preferred embodiment (which does not limit the present invention), the thermoplastic material contained in the second feed stream has a glass transition temperature T g and a melting temperature T m and comprises a thermoplastic polymer, and step B comprises, for example, heating the second feed stream material to a predetermined temperature, the predetermined temperature being i) above the temperature T g and ii) equal to or lower than the temperature T m , preferably lower than T m by less than 10.0 °C, or most preferably by less than 5.0 °C. The heating is preferably carried out in the feeder of the second inlet opening.
[0071] A preferred method further comprises the step of supplying the heated second feed stream through the second inlet opening. The advantage of this preheating is that less heating is required in the extruder, and thus it compensates for the reduction in heating due to less frictional heating.
[0072] In a further preferred embodiment in which a third feed stream is used, the third feed stream preferably has a glass transition temperature T g and a melting temperature T mThe thermoplastic polymer comprises, and step E preferably comprises heating the third feedstream material to a predetermined temperature, i) the temperature T g ii) The temperature T m Equal to or lower than, preferably T m The temperature is less than 10.0°C lower than, or most preferably less than 5.0°C lower. Heating is preferably carried out in the feeder of the third inlet opening. The advantage of this preheating is that less heating is required in the extruder (for example, in the mixing zone of the third inlet). Preheating of the third feedstream is preferably combined with suitable preheating of the second feedstream.
[0073] The method optionally further includes the step of pelletizing the LFT extruded material (particularly strands) into LFT pellets. Preferably, the LFT pellets are suitable for LFT injection molding and / or LFT extrusion, and / or compression molding.
[0074] Preferably, the pellets have a length in the range of 2 to 25 mm (preferably 6 to 15 mm). Pellets having such lengths are particularly suitable for LFT injection molding.
[0075] In a further embodiment, the present invention relates to an extrusion system. The extrusion system is suitable for producing long fiber-reinforced thermoplastic materials. Preferred features for an extrusion system, such as those discussed in relation to this method, apply equally to the extrusion system. The extrusion step of the present invention's method for producing LFT extruded material is preferably performed in an extrusion system such as those described herein.
[0076] However, the extrusion system is not limited to such use. The extrusion system includes an extruder, the extruder includes an extruder barrel, an extruder screw axially rotatable within the extruder barrel, and a die including an outlet opening, the screw including a shaft and one or more helical flights, the flights being, for example, mounted on the shaft or integrated with the shaft. The flights provide channels within the extruder for receiving and conveying the material to be extruded. The barrel includes a first inlet and a second inlet, the first inlet, the second inlet, and the outlet being spaced apart from each other. The first inlet preferably includes a first feeder. The second inlet preferably includes a second feeder, the second feeder being, for example, a packing feeder or a side feeder, or, for example, a further extruder. The second feeder preferably includes a heating element for heating the second feed material. Such heating elements for preheating the feed are advantageous in avoiding the need for high shear in the extruder.
[0077] The system is configured to supply a first feedstream into the extruder (particularly into the channel) through a first opening and a second feedstream into the extruder through a second inlet, wherein the first and second feedstreams are distinct from each other, and the feedstreams are preferably as discussed in relation to this method. The system includes, for example, separate supply lines for the first and second feeds to their respective inlets. An exemplary extruder system according to the present invention is schematically illustrated in Figure 1.
[0078] Preferably, the second feeder includes a gravimetric sensor for measuring the density of the second feedstream, and the extrusion system preferably includes a controller, which is connected to the first and / or second feeders and controls the first and / or second feeders using signals from the gravimetric sensor. In one embodiment, the controller is connected to both the first and second feeders. In this embodiment, the first and second inlets are therefore communicating with each other. In this embodiment, the system provides controlled addition, which allows for a stable and precise fiber content of the extruded material, even in the case of second and / or third feedstreams having fluctuating fiber content. The density measured indicates the fiber content. This is because, typically, fibers have a different (e.g., higher) density than thermoplastic components. The method preferably includes a step of measuring the density (e.g., continuously) while performing the extrusion step. This preferred embodiment is illustrated in Figure 4.
[0079] Preferably, the extrusion system further includes a third inlet opening for a third feedstream, as discussed. Preferably, the third inlet opening comprises a third feeder, which is, for example, a packing feeder or a side feeder. Preferably, the third feeder includes an additional gravimetric sensor for measuring the density of the third feedstream. This sensor is also coupled to a preferred controller of the extrusion system. Preferably, the controller is able to control the first, second, and third feeders using signals from the gravimetric sensors of the second and third feeders. A gravimetric sensor may also be provided in the first feeder. Other sensors may also be provided in the extrusion system and coupled to the controller. Such preferred embodiments are illustrated in Figure 4.
[0080] The extrusion system may further include a cooler downstream of the outlet to cool the continuous extruded strands received from the outlet, and optionally also include a pelletizer downstream of the cooler to convert the strands into pellets.
[0081] In a preferred embodiment, the screw includes a heating element. The heating element is, for example, an electric heater and / or tracing. The heating element is located, for example, within the shaft. The heating element is adapted to selectively heat only a portion of the screw, in particular to heat only a section of the screw in the longitudinal direction. This can be advantageously used to reduce or avoid any temperature drop, or at least avoid or prevent a significant temperature drop caused by the introduction of material into the extruder through second and optionally third inlet openings. One or more heating elements may be provided within the screw. In some embodiments, the screw includes a plurality of heating elements, which are located within the shaft and spaced apart along the longitudinal axis of the screw.
[0082] The production method of the present invention may include heating of the barrel. Preferred localized heating by a preferred heating element positioned within the screw may be applied in addition to heating the barrel, for example. The heating element provides selective heating of only a portion of the screw in the longitudinal direction, for example, heating a portion of the screw in the longitudinal direction that is less than 80%, less than 50%, or even less than 20% of the total screw length.
[0083] In one embodiment, the present invention also relates to such a screw equipped with such a heating element.
[0084] The screw (preferably equipped with such a heating element) preferably has a pitch length of 10 to 40 mm, preferably 15 to 30 mm, and / or a channel depth of 5 to 30 mm, preferably 15 to 25 mm. The screw preferably has a length-to-diameter ratio of 10 to 30, preferably 15 to 25. The screw preferably has a compression ratio of 4:1 to 1:4, preferably 3:1 to 1:1. Such a screw is preferably included in the extrusion system of the present invention as a single screw and is preferably used in the method of the present invention.
[0085] Preferably, the die includes a tapered die head, which is optionally configured to be heated by a heating means. The advantage of a tapered die head is that the fiber breakage rate is reduced, in particular, the fiber breakage rate in the transfer of the mixed material from the barrel (and channel) into the die. The die head is, for example, tapered, with a wide opening on the upstream side adjacent to the barrel and a narrow opening on the downstream side with a nozzle. The die head is, for example, a cone-shaped tapered vessel. Advantageously, discontinuity between the barrel and the die is avoided. A tapered die head is also used in preferred embodiments of the method of the present invention.
[0086] Figure 5 schematically illustrates die heads for an extrusion system and a method according to the present invention. Panel A illustrates a preferred tapered die head. Panel B illustrates a less preferred straight die head. Reference numerals are the same as those in Figure 1. The extruder (2) includes a die head (20) between a barrel (3) and a nozzle or outlet opening (5), the die head being tapered in Panel A and straight in Panel B. Fibers (21) are schematically shown, as are their movement (arrows) between the extrusion steps. In Panel A, the fibers are gradually fed into the nozzle through the tapered die head with lower fiber abrasion than that of the die head in Panel B.
[0087] Figure 6 schematically illustrates an exemplary extruder configuration comprising a granule inlet (1), a flake / chip inlet (2), a die (4), a cooling section (4), and a pelletizer (5).
[0088] Figure 7 illustrates a fiber length distribution histogram highlighting the length at 50% (D50) and the length at 90% (D90), which are, for example, those used in Example 1.
[0089] In a further embodiment, the present invention relates to LFT materials obtainable by the present method. The present method makes it possible to produce LFT materials having relatively long fibers and relatively high fiber fractionation using discontinuous long fibers.
[0090] For example, the material is in the form of pellets, and for example, the material has a ratio of D90 fiber length to initial fiber length (I) of at least 50%, at least 60%, at least 70%, or at least 80%, and / or a ratio of D50 fiber length to initial fiber length (I) of at least 20%, by glass fiber or carbon fiber. Here, D90 represents a point in the fiber length distribution (histogram) up to (and including) 90% of the total fibers, by frequency. For example, if D90 is 11 mm, this means that 90% of the fibers are 11 mm or less in size, and 10% of the fibers are longer than 11 mm, as illustrated in Figure 7. The D50 fiber length is calculated accordingly, with 50% of the fibers being shorter than the indicated value, and 50% being longer.
[0091] D90 (D50) indicates the fiber length up to (and including) 90% (50%) of the total counted fibers.
[0092] The D90 value of a material is important for the (mechanical) properties of LFT articles manufactured from LFT material (for example, by LFT injection molding).
[0093] The fiber length of individual fibers can be determined, for example, using optical image analysis.
[0094] The initial fiber length is the fiber length of the TCP material fed into the extruder (input fiber length), preferably the D50 fiber length value of the TCP material fed into the extruder.
[0095] In a preferred embodiment, the initial fiber length is considered to be equal to the length (maximum dimension) (i.e., input length, particularly with respect to flakes) of the TPC portion (e.g., chips or flakes, or TPC pellets) fed into the extruder. The TPC pellets comprise thermoplastic pellets having fibers having the maximum length within the size of the pellet.
[0096] In exemplary embodiments, the initial fiber length is considered to be equal to the length of the produced LFT pellet. Thus, in some embodiments, the LFT pellet has a ratio of D90 to pellet length of at least 50%, at least 60%, at least 70%, or at least 80%.
[0097] In a further embodiment, the present invention relates to pellets comprising fibers and thermoplastic materials, wherein the pellets have, for example, lengths and diameters obtainable by the method of the present invention. The pellets are, for example, (substantially) cylindrical body portions.
[0098] The present invention also provides LFT pellets having lengths obtainable by the method of the present invention, the LFT pellets having a D90 ratio to pellet length of at least 50%, at least 60%, at least 70%, or at least 80%, and the pellet length is in the range of, for example, 10 to 20 mm, for example, 12 to 16 mm. The pellets preferably contain thermoplastic material and fibers, as described in relation to the present method. Preferably, the pellets have a fiber content of at least 20% by weight.
[0099] In one embodiment, the pellet contains fibers, which are oriented in the longitudinal direction of the pellet and are preferably at least partially curved. For example, in a cross-section of the pellet perpendicular to the diameter of the pellet, the visible fiber fragments are preferentially oriented in the longitudinal direction of the pellet rather than exhibiting an anisotropic distribution. For example, in a cross-section of the pellet perpendicular to the diameter of the pellet, fiber fragments rather than whole fibers are visible due to the curvature (bending) of the fibers. This curvature provides a difference from pellets made by continuous dry fiber drawing or wire coating. In a preferred embodiment, the fibers in the pellet are discontinuous. Preferably, the pellet is the LFT material obtainable by the present method and more preferably has a D50 / I ratio of at least 20% and / or a D90 / I ratio of at least 50% or at least 80% as discussed above.
[0100] In one embodiment, at least some of the fibers in an individual pellet have a length greater than the length of the pellet, for example, at least 1% of the fibers (depending on the number of fibers) have a length that is at least 110% or at least 120% of the pellet length. More specifically, preferably, at least some of the fibers (e.g., at least 1% of the fibers (depending on the number of fibers)) have a length that is at least 50% of the length of the pellet, and / or, preferably, at least some of the fibers (e.g., at least 1% of the fibers (depending on the number of fibers)) are not oriented in the longitudinal direction of the pellet. In a preferred embodiment, at least some of the fibers in the pellet are not oriented in the longitudinal direction of the pellet and have a length that is at least 50% of the length of the pellet.
[0101] Optionally, in these embodiments as well, some of the fibers are oriented along the length of the pellet, and at least some of the fibers are curved.
[0102] In one embodiment, at least some of the fibers in an individual pellet have a length shorter than the length of the pellet (e.g., less than 90% of the pellet length). For example, in a pellet, at least 1% of the fibers (depending on the number of fibers) can have a length less than 90% of the pellet length. Both smaller and larger fibers provide a difference from pellets made using continuous dry fiber drawing or wire coating.
[0103] The fiber length distribution can be determined, for example, after matrix removal, by ashing the pellet, and / or by melting and / or dissolving the thermoplastic component of the pellet, and by optical measurement of the fibers, and / or by, for example, X-ray imaging without matrix removal. Preferably, the average fiber length (average by number) is at least 1.0 mm, or at least 2.0 mm, or at least 5.0 mm, and / or at least 30% or at least 50% of the pellet length.
[0104] The fibers and thermoplastic polymers are preferably those discussed in relation to this method. The pellets are preferably obtainable by the method according to the present invention. In a preferred embodiment, the fibers in the pellets are selected from the group consisting of glass fibers, natural fibers, and carbon fibers. The dimensions of the pellets are preferably those discussed in relation to this method.
[0105] In a preferred embodiment, the pellets of the present invention have a homogeneous fiber fraction. In an exemplary embodiment, the pellets of the present invention are typically 100 mm in size of the extruded material (pellets). 3 , more typically 50mm 3 , and most typically 25mm 3Based on the sample and based on fiber content in weight % fiber, the standard deviation of the fiber content is less than 20% or even less than 10% of the average fiber content, with the standard deviation being the percentage of the average fiber content value. For example, if the average fiber content is, for example, 50% by weight, the standard deviation is less than 10% by weight (20% of 50% by weight).
[0106] Preferably, the pellets are LFT material obtainable by the present method, and more preferably, as discussed above, have a D50 / I ratio of at least 20% and / or a D90 / I ratio of at least 50% or at least 80%.
[0107] In conclusion, the present invention relates to a method for producing long fiber thermoplastic (LFT) extruded material using an extruder comprising a first inlet for thermoplastic material and a second separate downstream inlet opening for TPC feed material.
[0108] Preferences regarding extrusion systems also apply to the extrusion systems used in this method. Preferences regarding materials used in this method also apply to the pellets of the present invention. Preferences regarding pellets of the present invention also apply to the products obtained by this method. The verb "comprising," as used herein, indicates that other elements (components, steps, features) not described may also exist.
[0109] (Examples) Herein, the present invention will be illustrated by the following embodiments, which are for illustrative purposes only and do not limit the scope of the present invention or the claims.
[0110] (Example 1) The extrusion method was tested for various samples to produce pellets as shown in Table 1, using glass fiber (GF) or carbon fiber-containing tape and other thermoplastic composite (TPC) feed materials, as well as an extruder setup MF as illustrated in Figure 6. For sample #1, heated material was used.
[0111] The feed thermoplastic granules were made of the same type of thermoplastic polymer (PP or PA6) used in tape / TPC materials.
[0112] The fiber length in a product is expressed as the maximum length of 50% (D50) and 90% (D90) of the fibers, respectively, as a percentage of frequency (see fiber shape length distribution histogram; for example, Figure 7 for the histogram). That is, 90% and 50% of the fibers, respectively, have a smaller length as a percentage of the total number of fibers counted. With respect to D90, 10% of the fibers have a fiber length longer than the D90 value. These longer fibers are important for the (mechanical) properties of the product (e.g., pellets and articles manufactured from pellets).
[0113] Table 2 shows the fiber length retention rate based on the ratio of the product fiber length (D50 and D90, respectively) to the input length I.
[0114] Fiber length was determined by burning pellets, as well as by optical image analysis using Fibreshape® software and a FibreShape M scanner. Tape starting material contains continuous fibers aligned in the tape direction. Cutting the tape into flakes produces an initial fiber length equal to the flake length. The flake length is the input length. In contrast, cutting TPC starting material (e.g., fiber mats or laminate or woven parts / production waste) results in a wide range of input fiber lengths.
[0115] The results demonstrate that a good fiber length retention rate was achieved.
[0116] In Table 1, the nozzle diameter refers to the die. The input length indicates the initial fiber length, and in this example, it represents the length of the chip / flake fed into the extruder.
[0117] For reference extruder processes using various starting materials, the D90 / I ratio was typically between 17% and 32%.
[0118] [Table 1]
[0119] [Table 2] [Explanation of Symbols]
[0120] 1. Extrusion System 2. Extruder 3 barrels 4 Single Screws 5 Outlet opening 6. First entrance opening, first entrance section 7. Second entrance opening, second entrance section 8 channels 9 Mixed Zone 10 Heating element 11 shafts 12 Flights 13 Third entrance opening, third entrance section 14. Second mixed zone 15 Dies 16 First feeder 17. Second feeder 18. Third feeder 19 Controllers 20 Die Heads 21 Fibers A First feed thermoplastic material, first feed material, first feedstream B TPC feed material, second feedstream C. First compounding material, first mixed material D Extruded material E. Third feedstream ED extrusion direction F. Second ingredient I. Initial fiber length ΔS1 distance ΔS2 distance ΔS3 distance
Claims
1. 1. A method for producing a long fiber thermoplastic (LFT) extruded material, comprising: A) providing a first feed stream (A) comprising a thermoplastic material; B) providing a second feed stream (B) comprising a thermoplastic composite (TPC) feed material, the TPC feed material comprising pieces, e.g., flakes or chips, the pieces individually comprising both fibers and thermoplastic material; Including, The method comprises an extrusion step carried out in an extrusion system (1), The extrusion system (1) comprises an extruder (2), The extruder (2) comprises a barrel (3), a single screw (4) and an exit opening (5) and has an extrusion direction (ED), the screw (4) providing a channel (8) within the extruder (2); The barrel comprises a first inlet opening (6) and a second inlet opening (7), the first inlet opening and the second inlet opening being separate and spaced apart from each other (S1), the second inlet opening being located downstream of the first inlet opening in the extrusion direction, The extrusion step includes: C) feeding the first feed stream (A) through the first inlet opening (6) into the channel (8) in the extruder (2) and conveying the first feed stream by the screw from the first inlet opening to the second inlet opening; D) feeding said second feed stream (B) through said second inlet opening (7) into said channel (8) in said extruder (2), thereby combining and mixing said first and second feed streams inside said channel (8) in a first mixing zone (9) of said extruder (2) to provide a first blended material (C); F) conveying a stream comprising said first blended material (C) through said outlet opening (5) to provide an LFT extrusion material (D); A method comprising:
2. 2. The method of claim 1, comprising the step of selectively heating a portion of the screw (4) by means of at least one heating element (10), the at least one heating element (10) being arranged in the screw at a predetermined position in the extrusion direction downstream of the second inlet opening.
3. E1) providing a third feed stream (E) comprising a TPC feed material, said extruder comprising a third inlet opening (13) for said third feed stream, said third inlet opening being spaced downstream from said second inlet opening (7); and the extrusion step further comprises: E2) conveying said first blended material (C) from said first mixing zone (9) to said third inlet opening (13) by said screw; E3) feeding said third feed stream (E) through said third inlet opening (13) into said channel (8) in said extruder (2), thereby combining and mixing said first blended material with the third feed stream inside said channel (8) in a second mixing zone (14) of said extruder (2) to give a second blended material (F); and conveying a stream comprising said second blended material (F) through said outlet opening (5) to give a LFT extrusion material (D); The method of claim 1 or 2, further comprising:
4. 4. The method of claim 1, wherein the TPC feed material comprises flakes or chips or crushed material from a continuous fiber reinforced thermoplastic (CFRT) waste stream.
5. Step B is B1) providing a dry, continuous fiber; B2) impregnating the fibers with a thermoplastic resin to provide a continuous sheet of impregnated fibers having edges; B3) separating at least a portion of the edge from the continuous sheet of impregnated fibers to provide flakes and a continuous sheet of trimmed fibers, the flakes being separated edge pieces, the flakes individually containing fibers and thermoplastic material; B4) using the flakes as at least a portion of the second feed; The method according to any one of claims 1 to 3, comprising:
6. 5. The method according to claim 1, wherein the long fibre reinforced thermoplastic material obtained by the method comprises 20 to 75% by weight of fibres, preferably 30 to 60% by weight of fibres, relative to the total weight of the long fibre reinforced thermoplastic material.
7. The thermoplastic material contained in the second and / or third feed streams has a glass transition temperature T g and the melting temperature T m and steps B and / or E include heating said second and / or third feedstream materials to a predetermined temperature, said predetermined temperature being: i) The temperature T g It exceeds ii) the temperature T m and preferably less than or equal to T m or, most preferably, less than 10.0° C. lower than 5.0° C.; 7. The method of claim 1, further comprising the step of: feeding the heated second and / or third feed streams through the second or third inlet opening.
8. 8. The method of any one of claims 1 to 7, further comprising pelletizing the LFT extrusion material into LFT pellets, the pellets being suitable for LFT injection molding and / or LFT extrusion.
9. A method according to any one of claims 1 to 8, wherein the fibres comprise pieces of thermoplastic composite (TPC) feed material having a length of 0.5 mm to 50 mm.
10. A long fibre thermoplastic (LFT) material obtainable by the method according to any one of claims 1 to 8.
11. 1. A single screw extrusion system for producing long fiber reinforced thermoplastic materials, comprising: an extruder barrel (3); an extruder screw (4) axially rotatable within the extruder barrel; and a die (15) comprising an outlet opening (5), the screw comprising a shaft (11) and one or more helical flights (12), the barrel (3) comprising a first inlet section (6) and a second inlet section (7), the first inlet section (6), the second inlet section (7), and the outlet section (5) being spaced apart from one another, the first inlet section (6) comprising a first feeder (16), and the second inlet section (7) comprising a second feeder (17).
12. 12. The single screw extrusion system according to claim 11, wherein the axially rotatable extruder screw (4) comprises a heating element (10), the heating element (10) being arranged inside the screw at the second inlet section or in a zone between the second inlet section and the outlet section.
13. the first feeder is configured to provide a first feed stream to a first inlet opening, and the second feeder is configured to deliver a second feed stream, different from the first feed stream, to a second inlet opening, the second feeder being an imbedded feeder or a side feeder; 13. The single screw extrusion system of claim 11 or 12, wherein the second feeder includes a gravimetric sensor for measuring the density of the second feed stream, and the extrusion system includes a controller, the controller coupled to the first feeder and the second feeder and adapted to control the first feeder and the second feeder using signals from the gravimetric sensor.
14. 14. The single screw extrusion system of any one of claims 11 to 13, wherein the die (15) comprises a tapered die head, the die head being optionally configured to be heated by a heating means.
15. The single screw extrusion system of claim 14, wherein the system further comprises a pelletizer for pelletizing the LFT extrusion material into LFT pellets.
16. A single screw extrusion system as described in any one of claims 11 to 15, further comprising a cooler downstream of the outlet portion configured to cool the continuous extruded strand received from the outlet portion and the pelletizer downstream of the cooler to convert the strand into pellets.
17. A pellet comprising fibers and a thermoplastic material, the pellet having a length and a diameter, at least some of the fibers within the pellet are not oriented along the length of the pellet and have a length that is at least 50% of the length of the pellet.
18. A pellet as described in claim 17, which is obtainable by a method described in any one of claims 1 to 8.
19. A pellet as described in claim 17 or 18, wherein the pellet has a ratio of D90 fiber length to initial fiber length (I) of at least 50%.
20. 20. The pellet of claim 17, wherein at least some of the fibers are oriented along the length of the pellet and at least some of the fibers are curved.
21. 10. The long fiber thermoplastic (LFT) material of claim 9 having a ratio of D90 fiber length to initial fiber length (I) of at least 50%.