Resistively switching polymer films and methods of manufacture

JP2023546304A5Inactive Publication Date: 2024-10-29APPLIED MATERIALS INC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021568570
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-10-23
Filing Date
2021-10-20
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The semiconductor industry faces challenges in manufacturing next-generation data storage devices with nanoscale features due to complex manufacturing steps and theoretical and practical limitations, such as void formation and non-uniform deposition, which affect device performance and processing.

Method used

A method involving molecular layer deposition (MLD) is used to form resistive switching polymer films using precursors like terephthaloyl chloride and ethylenediamine to create polyamide or polyazomethine films, allowing precise control over thickness, composition, and conformality, suitable for high aspect ratio structures.

Benefits of technology

The method enables precise control over polymer film properties, facilitating device scaling with improved switching durability and retention, and supports integration into existing semiconductor processes at low temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Devices including resistively switching polymer films are described. Methods of manufacturing devices including resistively switching polymer films are also described.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field

[0001] TECHNICAL FIELD Embodiments of the present disclosure relate to electronic devices, and in particular to electronic devices and manufacturing methods that include resistive switching polymer films. [Background technology]

[0002]

[0002] The semiconductor industry faces many challenges in pursuing next generation data storage technology. Traditional Si-based data storage techniques have been widely explored. The focus is on faster, higher density, lower power data storage devices.

[0003]

[0003] One way to improve device performance is to use nanoscale features. Features may be characterized by a higher aspect ratio (eg, greater than 5:1). Such features require complex manufacturing steps such as multiple lithography steps and the integration of high performance materials. However, this approach faces theoretical and practical limitations. For example, deposition can occur on the top of the feature and along the sidewalls, so that continued deposition can pinch off the feature, including between the sidewalls within the feature, creating voids within the feature. This can affect device performance and subsequent processing steps. In the manufacture of electronic devices such as memory devices, e.g. resistive memory (RRAM) or other bistable / multistable electrical devices, one or more of the thickness, composition, morphology and conformality of the polymer film There is a need to provide materials and methods that allow precise control. [Summary of the invention]

[0004] One aspect of the present disclosure relates to a device that includes a first electrically conductive material, a second electrically conductive material, and a resistive switching polymer membrane separating the first and second electrically conductive materials. The resistive switching polymer membrane of some embodiments includes one or more of polyamide, polyazomethine, polyurea, polyurethane, and derivatives thereof.

[0005] Another aspect of the present disclosure relates to a method of depositing resistive switching polymer films by a molecular layer deposition (MLD) process. The method of some embodiments includes: flowing a first deposition precursor to a substrate processing region to form a compound layer on the substrate; and removing the first deposition precursor from the substrate processing region. reacting the compound layer with a second deposition precursor in the substrate processing region to form a resistive switching film on the substrate; and removing the second deposition precursor from the substrate processing region.

[0006] Another aspect of the present disclosure relates to a method of forming a device. The method of some embodiments includes patterning a first conductive material on a substrate, cross-patterning a resistive switching polymer film on the first conductive material, and cross-patterning a resistive switching polymer film on the first conductive material. 2, depositing a conductive material. The resistive switching polymer membrane of some embodiments includes one or more of polyamide, polyazomethine, polyurea, polyurethane, and derivatives thereof.

[0007]

[0007] In order that the above features of the present disclosure may be understood in detail, a more specific description of the present disclosure briefly summarized above is provided by reference to embodiments, some of which are illustrated in the accompanying drawings. This can be done by referring to . The accompanying drawings, however, depict only typical embodiments of the disclosure and therefore should not be considered as limiting its scope, as the disclosure may appreciate other equally effective embodiments. Please note. [Brief explanation of drawings]

[0008]

Figure 1

Figure 2

[0009]

[0010] Before describing some exemplary embodiments of the invention, it is to be understood that the invention is not limited to the details of construction or process steps set forth in the following description. The invention is capable of other embodiments and of being practiced or carried out in various ways.

[0010]

[0011] As used herein, "substrate" or "substrate surface" refers to any portion of a substrate or material surface formed on a substrate on which film processing is performed. For example, substrate surfaces on which processing can be performed include materials such as silicon, silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, and sapphire, as well as metals, metal nitrides, and metals, depending on the application. Other materials are included, such as alloys, and other conductive materials. Substrates include, but are not limited to, semiconductor wafers. The substrate may be exposed to a pretreatment process to polish, etch, reduce, oxidize, hydroxylate, anneal, UV cure, e-beam cure, and / or bake the substrate surface. In addition to film processing directly onto the surface of the substrate itself, any of the film processing steps disclosed in this disclosure also apply to underlying layers formed on the substrate, as disclosed in more detail below. The term "substrate surface" is intended to include underlying layers as the context indicates. Thus, for example, where a film / layer or partial film / layer is deposited onto a substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate.

[0011]

[0012] As used herein, "atomic layer deposition," "molecular layer deposition," or "cyclic deposition" refers to the sequential exposure of two or more reactive compounds to deposit layers of material onto a substrate. refers to a process that includes

[0012]

[0013] As used herein, the term "flexible" is used interchangeably to mean a material with a species that can bend or twist without breaking.

[0013]

[0014] As used herein and in the appended claims, "reactive compound," "reactive gas," "reactive species," "precursor," "process gas," "deposition precursor," etc. The terms are used interchangeably to refer to a substance with a species capable of reacting with a substrate or a material on a substrate in a surface reaction (eg, chemisorption, oxidation, reduction, cycloaddition). A substrate, or a portion of a substrate, is sequentially exposed to two or more reactive compounds introduced into a reaction zone of a processing chamber.

[0014]

[0015] As used herein, "metal" refers to metals, metal alloys, metal oxides, including copper, cobalt, nickel, tungsten, ruthenium, chromium, iron, platinum, gold, silver, molybdenum, gallium, and indium. , metal nitride, or a combination thereof.

[0015]

[0016] As used herein, "metal surface" refers to any part of a substrate or any part of a material surface that is formed of metal. The metal surface can be exposed to a pretreatment process to polish, coat, dope, etch, reduce, oxidize, hydroxylate, anneal, UV cure, e-beam harden, and / or bake the substrate. In addition to pre-treating directly on the metal surface itself, any of the metal surface treatments disclosed in this disclosure can also be performed on underlying metal surfaces, as disclosed in more detail below. , the term "metallic surface" is intended to include the underlying layer as the context indicates. Thus, for example, where a film / layer or partial film / layer is deposited on a metal surface, the exposed surface of the newly deposited film / layer becomes the metal surface.

[0016]

[0017] As used herein, "dielectric surface" or "dielectric film" refers to any portion of a substrate or material surface formed of a dielectric material. Non-limiting examples of dielectric materials include SiO x ,Si x N y , Si, SiON, AlO x , HfO x , ZrO 2 , TiO x , TiN, Ta x O 5 ,Y 2 O 3 , La 2 O 3 , AlN, MgO, CaF 2 , LiF, SrO, SiC, BaO, HfSiO 4 , LaAlO 3 ,Nb 2 O 5 , BaTiO 3 , SrTiO 3 , Bi 4 Ti 3 O 12 , Pb(Zr,Ti)O 3 , CaCu 3 Ti 4 O 12 , LiNbO 3 , BaTiO 3 , LiNbO 3 ,KNbO 3is included. The dielectric surface can be exposed to a pretreatment process to polish, coat, dope, etch, reduce, oxidize, hydroxylate, anneal, UV cure, e-beam harden, and / or bake the substrate. In addition to pre-treating directly to the dielectric surface itself, this disclosure provides that any of the dielectric surface treatments disclosed may also be performed on underlying metal surfaces, as disclosed in more detail below. The term "dielectric surface" is intended to include underlying layers as the context indicates. Thus, for example, where a film / layer or partial film / layer is deposited on a metal surface, the exposed surface of the newly deposited film / layer becomes the metal surface.

[0017]

[0018] Embodiments of the present disclosure provide a device that includes a first conductive material, a second conductive material, and a resistive switching polymer membrane separating the first conductive material and the second conductive material. In one or more embodiments, electronic devices such as memory devices, eg, resistive random access memory (RRAM) or other bistable / multistable electrical devices, and methods of manufacturing the same are provided. In some embodiments, the method provides more precise control of one or more of polymer film thickness, composition, morphology, and conformality. In some embodiments, the method provides for device scaling and the deposition process can be performed at low temperatures, eg, from room temperature (eg, 25°C) to 150°C. In one or more embodiments, the resistive switching polymer film has a thickness in the range of 1 nm to 100 nm.

[0018]

[0019] The resistive switching polymer membrane of some embodiments has a high resistance state and a low resistance state when applying different voltages across the resistive switching polymer membrane. The ratio of high resistance states to low resistance states is, in some embodiments, 10 1 from 10 8 is within the range of Also, according to one or more embodiments, each resistance state (low resistance state and low resistance state) is at a temperature ranging from -200°C to 200°C and 100°C. 2 seconds to 10 10 Retained for a duration in the range of seconds.

[0019]

[0020] In some embodiments, one or more of the first conductive material and the second conductive material of the device has a thickness in the range of 1 nm to 100 nm. One or more of the first conductive material and the second conductive material is TiN, TaN, Ti, Ni, Ag, Al, Au, Cu, Pt, ZrN x , Ru, Pd, p- or n-doped Si, p-doped Ge or n-doped Ge, indium tin oxide (ITO), SrRuO 3 , carbon nanotubes, graphene, and conductive polymers. Conductive polymers include one or more of polyacetylene, polypyrrole, polyindole, polyaniline, poly(3-alkylthiophene) and derivatives thereof.

[0020]

[0021] The device of some embodiments further includes one or more dielectric films. The dielectric film of some embodiments is disposed between the resistive switching polymer film and the first conductive material or between the resistive switching polymer film and the second conductive material. The dielectric film of some embodiments is SiO x ,Si x N y , Si, SiON, Ge, ITO, AlO x , HfO x , ZrO 2 , TiO x , TiN, Ta x O 5 ,Y 2 O 3 , La 2 O 3 , AlN, MgO, CaF 2 , LiF, SrO, SiC, BaO, HfSiO 4 , LaAlO 3 ,Nb 2 O 5 , BaTiO 3 , SrTiO 3 , Bi 4 Ti 3 O 12 , Pb(Zr,Ti)O 3 , CaCu 3 Ti 4 O 12 , LiNbO 3 , BaTiO 3 , LiNbO 3 ,KNbO 3 , or a combination thereof.

[0021]

[0022] In some embodiments, the device further includes a substrate, and in certain embodiments the device is mounted on the substrate. The substrate of some embodiments is SiO x ,Si x N y , Si, SiON, Ge, ITO, AlO x , HfO x , ZrO 2 , TiO x , TiN, Ta x O 5 ,Y 2 O 3 , La 2 O 3 , AlN, MgO, CaF 2 , LiF, SrO, SiC, BaO, HfSiO 4 , LaAlO 3 ,Nb 2 O 5 , BaTiO 3 , SrTiO 3 , Bi 4 Ti 3 O 12 , Pb(Zr,Ti)O 3 , CaCu 3 Ti 4 O 12 , LiNbO 3 , BaTiO 3 , LiNbO 3 ,KNbO 3 , polyethylene naphthalate, or a combination thereof.

[0022]

[0023] The device of one or more embodiments is a bistable or multistable electrical device. The device of some embodiments is a resistive memory (RRAM) device. The device of some embodiments is such that one or more of the first conductive material, the second conductive material, and the resistive switching polymer film are flexible and / or transparent.

[0023]

[0024] According to one or more embodiments, a completely dry process is provided that is compatible with current semiconductor manufacturing processes and can be performed at low process temperatures. This process can be used to deposit films on high aspect ratio structures. High aspect ratios are 5:1~20:1, 6:1~20:1, 7:1~20:1, 8:1~20:1, 9:1~20:1, 10:1~20 :1, 5:1~15:1, 6:1~15:1, 7:1~15:1, 8:1~15:1, 9:1~15:1, 10:1~15:1 , 5:1~10:1, 6:1~10:1, 7:1~10:1, 8:1~10:1, or 9:1~10:1. One or more embodiments may include large memory windows (e.g., on / off >10 5 ). In some embodiments, different switching operations with different metal electrodes are provided to provide multi-level resistance states. Some embodiments provide devices with good switching durability and retention.

[0024]

[0025] In one or more embodiments, the resistive switching polymer membrane is made of polyamide or derivative, polyazomethine or derivative, polyurea or derivative, polyurethane or derivative, polyvinylidene chloride or derivative, polystyrene or derivative, polyethylene or derivative, polyimide or derivative, poly Methyl methacrylate (PMMA) or derivatives, polyethyl methacrylate (PEMA) or derivatives, polybutyl methacrylate (PBMA) or derivatives, carbonized polyfurfuryl alcohol or derivatives, polyacetylene or derivatives, polybenzene or derivatives, polyaniline or derivatives, polytetrabutyltin or derivatives, polyvinyl fluoride or derivatives, polycarbonate-graphite composites or derivatives, polyacrylonitrile (PAN) or derivatives, and combinations thereof. In some embodiments, the resistive switching polymer membrane comprises polyamide or derivative, polyazomethine or derivative, polyurea or derivative, polyurethane or derivative, and combinations thereof.

[0025]

[0026] In one or more embodiments of this method, the first electrically conductive material and the second electrically conductive material include a first electrode and a second electrode, respectively. In some embodiments of this method, each electrode (first electrode and second electrode) comprises a metal, carbon nanotubes, graphene, a conductive polymer, or a combination thereof. Metals include metals, metal alloys, metal oxides, metal nitrides, or combinations thereof. Non-limiting examples of electrodes include TiN, TaN, Ti, Ni, Ag, Al, Au, Cu, Pt, ZrN x , Ru, Pd, p- or n-doped Si, p-doped Si or n-doped Ge, indium tin oxide (ITO), SrRuO 3 , carbon nanotubes, graphene, conductive polymers, or combinations thereof. Non-limiting examples of conductive polymers include one or more of polyacetylene, polypyrrole, polyindole, polyaniline, poly(3-alkylthiophene) and derivatives thereof.

[0026]

[0027] In some embodiments, the device is a bistable or multistable electrical device. In some embodiments, the device is a resistive memory (RRAM) device. In one or more embodiments, one or more of the first conductive material, the second conductive material, the resistive switching polymer, the dielectric film, and the substrate are flexible and / or transparent. In one or more embodiments, one or more of the first conductive material, the second conductive material, the resistive switching polymer, the dielectric film, and the substrate are flexible. In one or more embodiments, one or more of the first conductive material, the second conductive material, the resistive switching polymer, the dielectric film, and the substrate are transparent.

[0027]

[0028] Referring to FIG. 2, embodiments of the present disclosure provide a method 200 of depositing a resistive switching polymer film by a deposition process. The deposition process of one or more embodiments includes a molecular layer deposition (MLD) process, a chemical vapor deposition process, or a plasma enhanced chemical vapor deposition process. In certain embodiments, the deposition process is a molecular layer deposition (MLD) process. In some embodiments of the method, the deposition process includes flowing a first deposition precursor to the substrate processing region at 210 to form a compound layer at 220. The method 200 includes removing a first deposition precursor from a substrate processing region at 230 and reacting a compound layer with a second deposition precursor in the substrate processing region at 240 to form a resistive switching film at 250. , further including. The method further includes removing the second precursor from the substrate processing region at 260.

[0028]

[0029] The first deposition precursor can be represented by the first equation below. X1-R1-X2 Here, R1 includes one or more of an alkyl group, an aromatic group, and a cycloalkyl group, X1 contains one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group, X2 contains one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group.

[0029]

[0030] The first deposition precursor of some embodiments is selected from the group consisting of terephthaloyl chloride, terephthalaldehyde, and 1,4-phenylene diisocyanate.

[0030]

[0031] The second deposition precursor can be represented by the second equation below. Y1-R2-Y2 Here, R2 includes one or more of an alkyl group, an aromatic group, and a cycloalkyl group, Y1 contains one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group, Y2 contains one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group.

[0031]

[0032] The second deposition precursor of some embodiments is selected from the group consisting of ethylenediamine, tris(2-aminoethyl)amine, phenylenediamine, and 1,4-diaminocyclohexane.

[0032]

[0033] The molecular layer deposition (MLD) process of some embodiments is repeated until the resistive switching film has a thickness in the range of 1 nm to 100 nm. The methods of some embodiments are performed at temperatures ranging from 1°C to 200°C.

[0033]

[0034] In some embodiments of the method, at 260, the deposition process is repeated at least once. In some embodiments of this method, the resistive switching polymer film of the device has a thickness of 0.1 nm to 200 nm, 0.1 nm to 180 nm, 0.1 nm to 160 nm, 0.1 nm to 140 nm, 0.1 nm to 120 nm, 0.1 nm to 100 nm, 0.1 nm ~80nm, 0.1nm~60nm, 0.1nm~40nm, 0.1nm~20nm, 0.1nm~10nm, 1nm~200nm, 1nm~180nm, 1nm~160nm, 1nm~140nm, 1nm~120nm, 1nm~100nm, 1nm~80nm , 1nm~60nm, 1nm~40nm, 1nm~20nm, 1nm~10nm, 5nm~200nm, 5nm~180nm, 5nm~160nm, 5nm~140nm, 5nm~120nm, 5nm~100nm, 5nm~80nm, 5nm~60nm, 5nm ~40nm, 5nm~20nm, 5nm~10nm, 10nm~200nm, 10nm~180nm, 10nm~160nm, 10nm~140nm, 10nm~120nm, 10nm~100nm, 10nm~80nm, 10nm~60nm, 10nm~40nm, or 1 0nm~ The deposition process is repeated until it has a thickness in the range of 20 nm.

[0034]

[0035] In some embodiments of this method, the deposition process is performed at a temperature ranging from 1°C to 500°C, 1°C to 400°C, 1°C to 300°C, 1°C to 200°C, or 1°C to 100°C. be done.

[0035]

[0036] In some embodiments of this method, the resistive switching polymer film is deposited by molecular layer deposition (MLD). In some embodiments of the method, molecular layer deposition (MLD) includes flowing a first deposition precursor into a substrate processing region to form a compound layer; reacting the compound layer with a second deposition precursor in the substrate processing region to form a resistive switching film; and removing the second deposition precursor from the substrate processing region. include. Removal of the first deposition precursor or removal of the second deposition precursor is accomplished by suction, purging, or both.

[0036]

[0037] In some embodiments of the method, molecular layer deposition (MLD) is repeated at least once. In some embodiments of this method, the molecular layer deposition (MLD) process is repeated until the resistive switching polymer film of the device has a thickness within the range provided herein.

[0037]

[0038] In some embodiments of this method, molecular layer deposition (MLD) is performed in a range of 1°C to 500°C, 1°C to 400°C, 1°C to 300°C, 1°C to 200°C, or 1°C to 100°C. performed at a temperature of

[0038]

[0039] In some embodiments of the method, the first deposition precursor is represented by the first equation below. X1-R1-X2 here, R1 includes one or more of an alkyl group, an aromatic group and a cycloalkyl group, X1 contains one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group, X2 contains one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group.

[0039]

[0040] In some embodiments of this method, the first deposition precursor is selected from the group consisting of terephthaloyl chloride, terephthalaldehyde, and 1,4-phenylene diisocyanate.

[0040]

[0041] In some embodiments of this method, the second deposition precursor is represented by the first equation below. Y1-R1-Y2 here, R1 includes one or more of an alkyl group, an aromatic group and a cycloalkyl group, Y1 contains one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group, Y2 contains one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group.

[0041]

[0042] In some embodiments of this method, the second deposition precursor is selected from the group consisting of ethylenediamine, tris(2-aminoethyl)amine, phenylenediamine, and 1,4-diaminocyclohexane.

[0042]

[0043] In some embodiments, the substrate processing region is in a modular system comprising multiple chambers that perform various functions including substrate center detection and orientation, degassing, annealing, deposition, and / or etching. According to one or more embodiments, a modular system includes at least a first processing chamber and a central transfer chamber. A central transfer chamber can house a robot that can shuttle substrates between the processing chamber and the load lock chamber. The transfer chamber is typically maintained under vacuum and provides an intermediate stage for moving substrates from one chamber to another and / or to a load lock chamber located at the front end of the cluster tool. Two well-known modular systems that can be adapted to the present disclosure are Centura® and Endura®, available from Applied Materials, Inc. of Santa Clara, California. However, the exact arrangement and combination of chambers may be varied for the purpose of performing particular steps of the process as described herein. Other processing chambers that can be used include molecular layer deposition (MLD), cyclic layer deposition (CLD), atomic layer deposition (ALD), chemical vapor deposition (CVD), physical vapor deposition (PVD), etching, pre- These include, but are not limited to, cleaning, chemical cleaning, thermal treatments such as RTP, plasma nitridation, degassing, orientation, hydroxylation, and other substrate processes. By performing the process in the processing chamber of the modular system, surface contamination of the substrate by atmospheric impurities can be avoided without oxidation before depositing the next film.

[0043]

[0044] According to one or more embodiments, the substrate is constantly in a vacuum or "load-lock" condition and is not exposed to ambient air as it is moved from one chamber to the next. The transfer chamber is therefore under vacuum and is "pumped down" under vacuum pressure. An inert gas may be present within the processing chamber or transfer chamber. In some embodiments, an inert gas is used to purge or remove some or all of the reactants (eg, reactants). According to one or more embodiments, an inert gas is present in the processing chamber to prevent reactants (e.g., reactants, deposition precursors) from moving from the processing chamber to the transfer chamber and / or additional processing chambers. is injected into the outlet. The flow of inert gas thus forms a curtain at the outlet of the chamber.

[0044]

[0045] Substrates can be processed within a single substrate deposition chamber, where a single substrate is loaded, processed, and unloaded before another substrate is processed. Substrates can also be processed continuously, similar to a conveyor system, where multiple substrates are individually loaded into a first part of the chamber, moved through the chamber, and transferred to a second part of the chamber. It is unloaded from the section. The shape of the chamber and associated conveyor system can form a straight or curved path. Additionally, the processing chamber may be a carousel in which multiple substrates are moved around a central axis and exposed to processes such as deposition, etching, annealing, cleaning, etc. throughout the carousel path.

[0045]

[0046] During processing, the substrate can be heated or cooled. Such heating or cooling can be accomplished by any suitable means including, but not limited to, changing the temperature of the substrate support and flowing heated or cooled gases over the substrate. In some embodiments, the substrate support includes a heater / cooler that can be controlled to conductively vary the substrate temperature. In one or more embodiments, the gas being used (either a reactive gas or an inert gas) is heated or cooled to locally change the substrate temperature. In some embodiments, a heater / cooler is placed within the chamber adjacent to the substrate to convectively vary the substrate temperature.

[0046]

[0047] The substrate can be stationary or rotated during processing. The rotating substrate can be rotated (about the substrate axis) continuously or in discrete steps. For example, the substrate may be rotated throughout the process, or the substrate may be rotated only a small amount between exposures to different reactive or purge gases. Rotating the substrate (continuously or stepwise) during processing helps to produce more uniform deposition or etching, for example by minimizing the effects of local variations in the shape of the gas flow.

[0047]

[0048] In spatial deposition processes, reactive gases containing deposition precursors are flowed to different processing regions within a processing chamber. Different processing zones are separated from adjacent processing zones to prevent mixing of reactive gases. The substrates can be moved between processing zones to individually expose the substrates to the reactive gas. During movement of the substrate, different parts of the substrate, or different parts of the material on the substrate, may be exposed to more than one reactive gas at the same time, such that any given point on the substrate is not exposed to substantially more than one reactive gas at the same time. exposed to reactive gases. As will be understood by those skilled in the art, a small portion of the substrate may be exposed to multiple reactive gases simultaneously due to gas diffusion within the processing chamber, but unless otherwise specified, simultaneous exposure is not intended.

[0048]

[0049] In another embodiment of the spatial deposition process, the reactive gases are supplied to the reaction zone simultaneously but separated by an inert gas curtain and / or a vacuum curtain. The gas curtain can be a combination of a flow of inert gas entering the processing chamber and a flow of a vacuum stream exiting the processing chamber. The substrate is moved relative to the gas supply apparatus such that any given point on the substrate is exposed to only one reactive gas.

[0049]

[0050] As used herein, "pulse" or "dose" refers to an amount of source gas that is introduced into the process chamber intermittently or discontinuously. The amount of a particular compound within each pulse may vary over time depending on the duration of the pulse. A particular process gas may include a single compound or a mixture / combination of two or more compounds.

[0050]

[0051] In some embodiments of time-domain deposition processes, exposure to each reactive gas allows each compound to adhere to and / or react at the substrate surface and then be purged from the processing chamber. separated by a time delay. Reactive gases are prevented from mixing by purging the processing chamber between subsequent exposures.

[0051]

[0052] Another aspect of the time domain deposition process of some embodiments is that there is a time delay between pulses of reactive gas. During each time delay, a purge gas, such as argon, is introduced into the processing chamber to purge or otherwise remove residual reactive gases or reaction products or byproducts from the reaction zone. . Residual reactive gases or reaction products or by-products may be removed by pumping them out of the substrate deposition area without combination with a gas flow or purge process. Pumping can be performed by applying suction. In some embodiments, residual reactive gases or reaction products or byproducts can be removed by one or more purges, purge-pumps, pump-purges, pumps, or combinations thereof. Alternatively, the purge gas can flow continuously throughout the deposition process such that only the purge gas flows during the time delays between pulses of reactive gas. Alternatively, the reactive gas is pulsed multiple times with pulses of purge gas in between.

[0052]

[0053] The duration of each pulse / dose is variable and can be adjusted, for example, to accommodate the volumetric capacity of the processing chamber as well as the capacity of the vacuum system coupled thereto. Additionally, the dose time of the reactive gas varies depending on the flow rate of the reactive gas, the temperature of the process gas, the type of control valve, the type of process chamber used, as well as the ability of the components of the process gas to adsorb to the substrate. It is possible. Dose times may also vary based on the type of layer being formed and the shape of the device being formed. The dose time must be long enough to provide a sufficient amount of the compound to adsorb / chemisorb onto substantially the entire surface of the substrate and form a layer of process gas components thereon.

[0053]

[0054] Embodiments of the present disclosure provide methods for making devices with resistive switching polymer films. The device includes a first conductive material, a second conductive material, and a resistive switching polymer membrane separating the first conductive material and the second conductive material. Some embodiments of the device further include a substrate. In some embodiments of the device, the device is mounted on a substrate. This method includes patterning a first conductive material on a substrate, cross-patterning a resistive polymer film on the first conductive material, and cross-patterning a second conductive material on the resistive switching polymer film. and depositing.

[0054]

[0055] In some embodiments of the methods and devices described herein, the substrate is SiO x ,Si x N y , Si, SiON, Ge, ITO, AlO x , HfO x , ZrO 2 , TiO x , TiN, Ta x O 5 ,Y 2 O3 , La 2 O 3 , AlN, MgO, CaF 2 , LiF, SrO, SiC, BaO, HfSiO 4 , LaAlO 3 ,Nb 2 O 5 , BaTiO 3 , SrTiO 3 , Bi 4 Ti 3 O 12 , Pb(Zr,Ti)O 3 , CaCu 3 Ti 4 O 12 , LiNbO 3 , BaTiO 3 , LiNbO 3 ,KNbO 3 , polyethylene naphthalate, or a combination thereof.

[0055]

[0056] In some embodiments of the methods and devices described herein, the substrate includes a dielectric film. A non-limiting example of a dielectric film is SiO x ,Si x N y , Si, SiON, Ge, ITO, AlO x , HfO x , ZrO 2 , TiO x , TiN, Ta x O 5 ,Y 2 O 3 , La 2 O 3 , AlN, MgO, CaF 2 , LiF, SrO, SiC, BaO, HfSiO 4 , LaAlO 3 ,Nb 2 O 5 , BaTiO 3 , SrTiO 3 , Bi 4 Ti 3 O 12 , Pb(Zr,Ti)O 3 , CaCu 3 Ti 4 O 12 , LiNbO 3 , BaTiO 3 , LiNbO 3 ,KNbO 3 , or a combination thereof.

[0056]

[0057] In one or more embodiments of the methods and devices described herein, the resistive switching polymer membrane is a polyamide or derivative, polyazomethine or derivative, polyurea or derivative, polyurethane or derivative, polyvinylidene chloride or derivative, polystyrene or derivative , polyethylene or derivatives, polyimide or derivatives, polymethyl methacrylate (PMMA) or derivatives, polyethyl methacrylate (PEMA) or derivatives, polybutyl methacrylate (PBMA) or derivatives, carbonized polyfurfuryl alcohol or derivatives, polyacetylene or derivatives, polybenzene or derivatives, including polyaniline or derivatives, polytetrabutyltin or derivatives, polyvinyl fluoride or derivatives, polycarbonate-graphite composites or derivatives, polyacrylonitrile (PAN) or derivatives, and combinations thereof. In some embodiments of the methods and devices, the resistive switching polymer membrane comprises polyamide or derivative, polyazomethine or derivative, polyurea or derivative, polyurethane or derivative, and combinations thereof.

[0057]

[0058] In one or more embodiments of the methods and devices described herein, the resistive switching polymer film has at least two resistance states when different voltages are applied across the resistive switching polymer film. In some embodiments of the method and device, the resistive switching polymer film has a high resistance state and a low resistance state when applying different voltages across the resistive switching polymer film. In some embodiments of the method and device, the ratio of high resistance states to low resistance states is 10 1 ~10 10 ,Ten 1 ~10 9 ,Ten 1 ~10 8 ,Ten 1 ~10 7 ,Ten 1 ~10 6 ,Ten 1 ~10 5 ,Ten 1 ~10 4 ,Ten 1 ~10 3 ,Ten 1 ~10 2 ,Ten 2 ~10 10 ,Ten 2 ~10 9 ,Ten 2 ~10 8 ,Ten 2 ~10 7 ,Ten 2 ~10 6 ,Ten 2 ~10 5 ,Ten 2 ~10 4 ,Ten 2 ~10 3 ,Ten 3 ~10 10 ,Ten 3 ~10 9 ,Ten 3 ~10 8 ,Ten 3 ~10 7 ,Ten 3 ~10 6 ,Ten 3 ~10 5 ,Ten 3 ~10 4 ,Ten 4 ~10 10 ,Ten 4 ~10 9 ,Ten 4 ~10 8 ,Ten 4 ~10 7 ,Ten 4 ~10 6 , or 10 4 ~10 5 within the range of

[0058]

[0059] In one or more embodiments of the methods and devices described herein, the resistive switching polymer film is heated at -250°C to 250°C, -200°C to 250°C, -150°C to 250°C. , -100°C~250°C, -50°C~250°C, 0°C~250°C, 50°C~250°C, 100°C~250°C, 150°C~250°C , 200°C~250°C, -250°C~200°C, -200°C~200°C, -150°C~200°C, -100°C~200°C, -50°C~ 200°C, 0°C~200°C, 50°C~200°C, 100°C~200°C, 150°C~200°C, -250°C~150°C, -200°C~ 150°C, -150°C~150°C, -100°C~150°C, -50°C~150°C, 0°C~150°C, 50°C~150°C, 100°C ~150°C, -250°C~100°C, -200°C~100°C, -150°C~100°C, -100°C~100°C, -50°C~100°C, 0°C~100°C, 50°C~100°C, -250°C~50°C, -200°C~50°C, -150°C~50°C, -100°C~50° C, -50°C~50°C, or at temperatures ranging from 0°C~50°C, 10 1 seconds~10 10 seconds, 10 1 seconds~10 9 seconds, 10 1 seconds~10 8 seconds, 10 1 seconds~10 7 seconds, 10 1 seconds~10 6 seconds, 10 1 seconds~10 5 seconds, 10 1 seconds~10 4 seconds, 10 1 seconds~10 3 seconds, 10 1 seconds~10 2 seconds, 10 2 seconds~10 10 seconds, 10 2 seconds~10 9 seconds, 10 2 seconds~10 8 seconds, 10 2 seconds~10 7 seconds, 10 2 seconds~10 6 seconds, 10 2 seconds~10 5 seconds, 10 2 seconds~10 4 seconds, 10 2 seconds~10 3 seconds, 10 3 seconds~10 10 seconds, 10 3 seconds~10 9 seconds, 10 3 seconds~10 8 seconds, 10 3 seconds~10 7 seconds, 10 3 seconds~10 6 seconds, 10 3 seconds~10 5 seconds, 10 3 seconds~10 4 seconds, 10 4 seconds~10 10 seconds, 10 4 seconds~10 9 seconds, 10 4 seconds~10 8 seconds, 10 4 seconds~10 7 seconds, 10 4 seconds~10 6 seconds, or 10 4 seconds~10 5Remains in a low resistance state for a duration in the range of seconds. In some embodiments of the methods and devices, the resistive switching polymer film is heated at a temperature range of 10°C to 50°C. 2 Second ~ 10 4 Remains in a low resistance state for a duration in the range of seconds.

[0059]

[0060] In one or more embodiments of the methods and devices described herein, the resistive switching polymer film is heated at -250°C to 250°C, -200°C to 250°C, -150°C to 250°C. , -100°C~250°C, -50°C~250°C, 0°C~250°C, 50°C~250°C, 100°C~250°C, 150°C~250°C , 200°C~250°C, -250°C~200°C, -200°C~200°C, -150°C~200°C, -100°C~200°C, -50°C~ 200°C, 0°C~200°C, 50°C~200°C, 100°C~200°C, 150°C~200°C, -250°C~150°C, -200°C~ 150°C, -150°C~150°C, -100°C~150°C, -50°C~150°C, 0°C~150°C, 50°C~150°C, 100°C ~150°C, -250°C~100°C, -200°C~100°C, -150°C~100°C, -100°C~100°C, -50°C~100°C, 0°C~100°C, 50°C~100°C, -250°C~50°C, -200°C~50°C, -150°C~50°C, -100°C~50° C, -50°C~50°C, or at temperatures ranging from 0°C~50°C, 10 1 Second ~ 10 10 Second, 10 1 Second ~ 10 9 Second, 10 1 Second ~ 10 8 Second, 10 1 Second ~ 10 7 Second, 10 1 Second ~ 10 6 Second, 10 1 Second ~ 10 5 Second, 10 1 Second ~ 10 4 Second, 10 1 seconds~10 3 seconds, 10 1 seconds~10 2 seconds, 10 2 seconds~10 10 seconds, 10 2 seconds~10 9 seconds, 10 2 seconds~10 8 seconds, 10 2 seconds~10 7 seconds, 10 2 seconds~10 6 seconds, 10 2 seconds~10 5 Second, 10 2 Second ~ 10 4 Second, 10 2 秒~10 3 Second, 10 3 Second ~ 10 10 Second, 10 3 Second ~ 10 9 Second, 10 3 秒~10 8 秒、10 3 秒~10 7 seconds, 10 3 秒~10 6 秒、10 3 秒~10 5 秒、10 3 seconds~10 4 seconds, 10 4 seconds~10 8 seconds, 10 4 seconds~10 7 seconds, 10 4 seconds~10 6 seconds, or 10 4 seconds~10 5 Remains in a high resistance state for a duration in the range of seconds. In some embodiments of the methods and devices, the resistive switching polymer film is heated at 20°C to 50°C for 10 2 seconds~10 4 Remains in a high resistance state for a duration in the range of seconds.

[0060]

[0061] In one or more embodiments of the methods and devices described herein, the first electrically conductive material and the second electrically conductive material include a first electrode and a second electrode, respectively. In some embodiments of the method and device, each electrode (first electrode and second electrode) comprises a metal, carbon nanotubes, graphene, a conductive polymer, or a combination thereof. Metals include metals, metal alloys, metal oxides, metal nitrides, or combinations thereof. Non-limiting examples of electrodes include TiN, TaN, Ti, Ni, Ag, Al, Au, Cu, Pt, ZrN x 、Ru、Pd、p型またはn型ドープされたSi、p型またはn型ドープされたGe、酸化インジウムスズ(ITO)、SrRuO 3 、カーボンナノチューブ、グラフェン、導電性ポリマー、またはそれらの組み合わせが含まれる。 Non-limiting examples of conductive polymers include one or more of polyacetylene, polypyrrole, polyindole, polyaniline, poly(3-alkylthiophene) and derivatives thereof.

[0061]

[0062] In one or more embodiments of the methods and devices described herein, the thickness of the first conductive material is between 1 nm and 200 nm, between 1 nm and 180 nm, between 1 nm and 160 nm, between 1 nm and 140 nm, between 1 nm and 120 nm, between 1 nm and 1 nm. ~100nm、1nm~80nm、1nm~60nm、1nm~40nm、1nm~20nm、1nm~10nm、5nm~200nm、5nm~180nm、5nm~160nm、5nm~140nm、5nm~120nm、5nm~100nm、5nm~80nm , 5nm~60nm, 5nm~40nm, 5nm~20nm, 5nm~10nm, 10nm~200nm, 10nm~180nm, 10nm~160nm, 10nm~140nm, 10nm~120nm, 10nm~100nm, 10nm~80nm, 10nm~60n m, 10nm ~40nm, or in the range of 10nm to 20nm.

[0062]

[0063] In one or more embodiments of the methods and devices described herein, the second conductive material has a thickness of 1 nm to 200 nm, 1 nm to 180 nm, 1 nm to 160 nm, 1 nm to 140 nm, 1 nm to 120 nm, 1 nm. ~100nm、1nm~80nm、1nm~60nm、1nm~40nm、1nm~20nm、1nm~10nm、5nm~200nm、5nm~180nm、5nm~160nm、5nm~140nm、5nm~120nm、5nm~100nm、5nm~80nm , 5nm~60nm, 5nm~40nm, 5nm~20nm, 5nm~10nm, 10nm~200nm, 10nm~180nm, 10nm~160nm, 10nm~140nm, 10nm~120nm, 10nm~100nm, 10nm~80nm, 10nm~60n m, 10nm ~40nm, or in the range of 10nm to 20nm.

[0063]

[0064] 方法およびデバイスの1つ以上の実施形態は、1つ以上の誘電体膜をさらに含む。 In some embodiments of the methods and devices, the one or more dielectric films are between the resistive switching polymer film and the first conductive material, between the resistive switching polymer film and the second conductive material, or between the resistive switching polymer film and the second conductive material. placed on both. A non-limiting example of a dielectric film is SiO x ,Si x N y , Si, SiON, Ge, ITO, AlO x , HfO x , ZrO 2 , TiO x , TiN, Ta x O 5 ,Y 2 O 3 , La 2 O 3 , AlN, MgO, CaF 2 , LiF, SrO, SiC, BaO, HfSiO 4 , LaAlO 3 ,Nb 2 O 5 , BaTiO 3 , SrTiO 3 , Bi 4 Ti 3 O 12 , Pb(Zr,Ti)O 3 , CaCu 3 Ti 4 O 12 , LiNbO 3 , BaTiO 3 , LiNbO 3 ,KNbO 3 , or a combination thereof.

[0064]

[0065] In one or more embodiments of the methods and devices described herein, the dielectric film has a thickness of 1 nm to 200 nm, 1 nm to 180 nm, 1 nm to 160 nm, 1 nm to 140 nm, 1 nm to 120 nm, 1 nm to 100 nm, 1nm~80nm、1nm~60nm、1nm~40nm、1nm~20nm、1nm~10nm、5nm~200nm、5nm~180nm、5nm~160nm、5nm~140nm、5nm~120nm、5nm~100nm、5nm~80nm、5nm~ 60nm, 5nm~40nm, 5nm~20nm, 5nm~10nm, 10nm~200nm, 10nm~180nm, 10nm~160nm, 10nm~140nm, 10nm~120nm, 10nm~100nm, 10nm~80nm, 10nm~60nm, 10n m~40nm, Or in the range of 10nm to 20nm.

[0065]

[0066] FIG. 1 shows a device 100 that includes a resistive switching polymer membrane 104. The device 100 includes a substrate 101, a dielectric film 102 on the substrate, a first electrode 103 on the dielectric film, a resistive switching polymer film 104 on the first electrode 103, and a second resistive switching polymer film 104 on the resistive switching polymer film 104. Includes electrode 105. In some embodiments, substrate 101 includes Si. In some embodiments, dielectric film 102 is SiO 2 including. In some embodiments, first electrode 103 includes TiN. In some embodiments, the first electrode has a thickness of 50 nm. In some embodiments, the resistive switching polymer film is deposited by a molecular layer deposition (MLD) process. In some embodiments, the second electrode includes Pt or Ag. In some embodiments, the second electrode is deposited by an electron beam evaporation process.

[0066]

[0067] In some embodiments of the methods and devices, one or more of the first conductive material, the second conductive material, the resistive switching polymer, the dielectric film, and the substrate are flexible and / or transparent. It is. In some embodiments of the method and device, one or more of the first conductive material, the second conductive material, the resistive switching polymer, the dielectric film, and the substrate are flexible. In some embodiments of the method and device, one or more of the first conductive material, the second conductive material, the resistive switching polymer, the dielectric film, and the substrate are transparent.

[0067]

[0068] In some embodiments of this method, one or more of the resistive switching polymer films are formed by molecular layer deposition, glow discharge polymerization, vacuum thermal evaporation, deposition from solution, electron beam deposition, gamma radiation polymerization, thermal polymerization, isothermal polymerization, Formed by a process involving immersion techniques or plasma polymerization.

[0068]

[0069] In one aspect of the present disclosure, processes are generally stored in memory as software routines that, when executed by a controller or processor, cause a substrate processing chamber to perform the processes of the present disclosure described herein. The software routines may also be stored and / or executed by a second controller or processor (not shown) that is located remotely from the hardware being controlled by the first controller or processor. Some or all of the methods of this disclosure may be performed in hardware. Accordingly, the processes may be implemented in software and executed using a computer system, or may be implemented in hardware, for example, as an application-specific integrated circuit or other type of hardware implementation; Alternatively, it may be implemented as a combination of software and hardware. The software routines, when executed by a processor or controller, transform a general purpose computer into a special purpose computer (controller) that controls the operation of the chamber so that the process is performed. Instructions for performing one or more process steps described herein, including instructions that, when executed by a controller of a substrate processing chamber, cause the substrate processing chamber to generate a resistive switching film may be non-transitory. Can be stored on a computer readable medium.

[0069]

[0070] Example

[0070]

[0071] The following non-limiting examples illustrate principles in accordance with one or more embodiments of the present disclosure.

[0071]

[0072] RRAM device with TiN / resistive switching polyamide film / Pt

[0072]

[0073] RRAM devices were fabricated using resistive switching polyamide membranes. The method included patterning a first electrode on a substrate, cross-patterning a resistive switching polyamide film, and depositing a second electrode. The substrate is Si / SiO 2 It consisted of The first electrode was TiN. The thickness of the first electrode was 50 nm.

[0073]

[0074] Polyamide films were deposited by a molecular layer deposition (MLD) process. The molecular layer deposition (MLD) process includes flowing a first deposition precursor, terephthaloyl chloride, into a substrate processing region to form a compound layer and removing the terephthaloyl chloride from the substrate processing region. , reacting a second deposition precursor, ethylene diamine, with the compound layer in the substrate processing region to form a resistive switching polyamide film, removing the ethylene diamine from the substrate processing region, and determining the thickness of the resistive switching polyamide film. repeating this process until the particle size is 10 nm. The second electrode was Pt. The thickness of the second electrode was 60 nm.

[0074]

[0075] Devices with TiN and Pt electrodes and a resistive switching polyamide membrane sandwiched between the electrodes exhibit a low compliance current of 100 μA. 5 demonstrated very large memory windows over , excellent stability over at least 100 switching cycles, and robust data retention for over 3 hours. The bipolar current vs. voltage curve for high and low resistance states is 4.4x10 5 The ratio of high resistance state to low resistance state is shown. Multilevel current (MLC) characteristics of polyamide membranes were recorded and graphed at compliance currents of 1 μA, 10 μA, 20 μA, 40 μA, and 100 μA. By varying CC from 1μA to 100μA, 2 bits (2 2 Tests have demonstrated that a multilevel state of =4) can be obtained. Cycle-to-cycle uniformity properties were tested, demonstrating the reproducibility of the resistive switching polyamide membrane over 100 switching cycles. Furthermore, this membrane has a larger memory window (>10 5 ) showed robust data retention characteristics for more than 3 hours.

[0075]

[0076] RRAM device with TiN / resistive switching polyamide film / Ag

[0076]

[0077] RRAM devices were fabricated using resistive switching polyamide membranes. The method included patterning a first electrode on a substrate surface, cross-patterning a resistive switching polyamide film, and depositing a second electrode. The substrate surface is Si / SiO 2 It consisted of The first electrode was TiN. The thickness of the first electrode was 50 nm. Polyamide films were deposited by a molecular layer deposition (MLD) process. The molecular layer deposition (MLD) process includes flowing a first deposition precursor, terephthaloyl chloride, into a substrate processing region to form a compound layer and removing the terephthaloyl chloride from the substrate processing region. , reacting a second deposition precursor, ethylene diamine, with the compound layer in the substrate processing region to form a resistive switching polyamide film, removing the ethylene diamine from the substrate processing region, and determining the thickness of the resistive switching polyamide film. repeating this process until the particle size is 10 nm. The second electrode was Ag. The thickness of the second electrode was 60 nm. A device in which a bipolar current vs. voltage curve is generated and a resistive switching polyamide membrane is sandwiched between Ag and TiN electrodes is capable of producing 5x10 with a low compliance current of 10 μA. 2 was shown to exhibit a very large memory window. The polyamide membrane is observed to have low and high resistance states, and the ratio of high and low resistance states is 5x10 2 It was observed that The device operated at low currents, with a compliance current of 10 μA and a voltage of less than 1 V.

[0077]

[0078] RRAM device with TiN / resistive switching polyazomethine film / Ag

[0078]

[0079] RRAM devices were fabricated using resistive switching polyazomethine films. The method included patterning a first electrode on a substrate surface, cross-patterning a resistive switching polyazomethine film, and depositing a second electrode. The substrate surface is Si / SiO 2 It consisted of The first electrode was TiN. The thickness of the first electrode was 50 nm. Polyamide films were deposited by a molecular layer deposition (MLD) process. The molecular layer deposition (MLD) process consists of flowing a first deposition precursor, terephthalaldehyde, into a substrate processing region to form a compound layer, removing the terephthalaldehyde from the substrate processing region, and a second deposition precursor, terephthalaldehyde, to form a compound layer. Reacting the deposition precursor ethylenediamine with the compound layer in the substrate processing region to form a resistive switching polyazomethine film, removing the ethylenediamine from the substrate processing region, and reducing the thickness of the resistive switching polyazomethine film to 3 nm. repeating this process until . The second electrode was Ag. The thickness of the second electrode was 60 nm.

[0079]

[0080] A bipolar current vs. voltage curve is generated, and the device has a compliance current of 10 mA. 4 was shown to have a very large memory window exceeding . The polyamide film is observed to have low resistance states and high resistance states, and the ratio of high resistance states to low resistance states is 10 4 It was observed that The device was operated with a compliance current of 1mA. The device was observed to be stable for at least 60 switching cycles.

[0080]

[0081] Throughout this specification, references to "one embodiment," "a particular embodiment," "one or more embodiments," or "an embodiment" refer to the specific features, structures, and structures described in connection with the embodiment. , material, or property is included in at least one embodiment of the present disclosure. Therefore, the occurrences of phrases such as "in one or more embodiments," "in a particular embodiment," "in one embodiment," or "in an embodiment" in various places throughout this specification are not necessarily They are not necessarily referring to the same embodiments of the disclosure. Furthermore, the particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.

[0081]

[0082] Although the disclosure herein has been described with reference to particular embodiments, it is to be understood that these embodiments are merely illustrative of the principles and applications of the disclosure. It will be apparent to those skilled in the art that various modifications and variations can be made to the methods and apparatus of the present disclosure without departing from the spirit and scope of the disclosure. Accordingly, it is intended that this disclosure cover modifications and variations that come within the scope of the appended claims and their equivalents.

Claims

1. A first conductive material; a second conductive material; and a resistively switching polymer film separating the first conductive material and the second conductive material, the resistively switching polymer film comprising one or more of polyamide, polyazomethine, polyurea, polyurethane, and derivatives thereof; The device that contains

2. The device of claim 1 , wherein the resistively switching polymer film has a thickness in the range of 1 nm to 100 nm.

3. 10. The device of claim 1, wherein the resistively switching polymer film has a high resistance state and a low resistance state upon application of different voltages across it.

4. The ratio of the high resistance state to the low resistance state is 10 1 From 10 8 The device of claim 3, wherein the range is

5. The high resistance state and the low resistance state are each in a temperature range of −200° C. to 200° C. for 10 2 Seconds to 10 10 The device of claim 3 , wherein the signal is held for a duration in the range of seconds.

6. The device of claim 1 , wherein one or more of the first conductive material and the second conductive material have a thickness in the range of 1 nm to 100 nm.

7. One or more of the first conductive material and the second conductive material is selected from the group consisting of TiN, TaN, Ti, Ni, Ag, Al, Au, Cu, Pt, and ZrN. x , Ru, Pd, p-type doped Si, n-type doped Si, p-type or n-type doped Ge, indium tin oxide (ITO), SrRuO 310. The device of claim 1 comprising one or more of the following: carbon nanotubes, graphene, polyacetylene, polypyrrole, polyindole, polyaniline, poly(3-alkylthiophene), and derivatives thereof.

8. 10. The device of claim 1 , further comprising one or more dielectric films disposed between the resistively switching polymer film and at least one of the first conductive material and the second conductive material.

9. The one or more dielectric films are made of SiO x , Si x N y , Si, SiON, Ge, ITO, AlO x , HfO x , ZrO 2 , TiO x , TiN, Ta x O 5 , Y 2 O 3 , La 2 O 3 , AlN, MgO, CaF 2 , LiF, SrO, SiC, BaO, HfSiO 4 , LaAlO 3 , Nb 2 O 5 , BaTiO 3 , SrTiO 3 , Bi 4 Ti 3 O 12 , Pb(Zr,Ti)O 3 , CaCu 3 Ti 4 O 12 , LiNbO 3 , BaTiO 3 , LiNbO 3 , KNbO 3 or a combination thereof.

10. 10. The method of claim 1 further comprising: providing a substrate on which the device of claim 1 is mounted; the substrate being made of SiO. x , Si x N y, Si, SiON, Ge, ITO, AlO x , HfO x , ZrO 2 , TiO x , TiN, Ta x O 5 , Y 2 O 3 , La 2 O 3 , AlN, MgO, CaF 2 , LiF, SrO, SiC, BaO, HfSiO 4 , LaAlO 3 , Nb 2 O 5 , BaTiO 3 , SrTiO 3 , Bi 4 Ti 3 O 12 , Pb(Zr,Ti)O 3 , CaCu 3 Ti 4 O 12 , LiNbO 3 , BaTiO 3 , LiNbO 3 , KNbO 3 , polyethylene naphthalate, or a combination thereof.

11. The device of claim 1 which is a bistable or multistable electrical device.

12. 10. The device of claim 1 which is a resistive random access memory (RRAM) device.

13. The device of claim 1 , wherein one or more of the first conductive material, the second conductive material, and the resistively switching polymer film are transparent.

14. 1. A method for depositing a resistively switching polymer film by a molecular layer deposition (MLD) process, comprising: flowing a first deposition precursor into a substrate processing region to form a compound layer on the substrate; removing the first deposition precursor from the substrate processing region; reacting the compound layer with a second deposition precursor in the substrate processing region to form the resistively switching polymer film on the substrate; removing the second deposition precursor from the substrate processing region; and Including, The first deposition precursor is represented by a first formula: X1-R1-X2 During the ceremony, R1 comprises one or more of an alkyl group, an aromatic group, and a cycloalkyl group; X1 comprises one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group; X2 comprises one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group; The second deposition precursor is represented by a second formula: Y1-R2-Y2 During the ceremony, R2 comprises one or more of an alkyl group, an aromatic group, and a cycloalkyl group; Y1 comprises one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group; The method wherein Y2 comprises one or more of a hydroxide group, an aldehyde group, a ketone group, an acid group, an amino group, an isocyanate group, a thiocyanate group, and an acyl chloride group.

15. The method of claim 14, wherein the first deposition precursor is selected from the group consisting of terephthaloyl chloride, terephthalaldehyde, and 1,4-phenylene diisocyanate.

16. The method of claim 14, wherein the second deposition precursor is selected from the group consisting of ethylenediamine, tris(2-aminoethyl)amine, phenylenediamine, and 1,4-diaminocyclohexane.

17. 15. The method of claim 14, wherein the molecular layer deposition (MLD) process is repeated until the resistive switching polymer film has a thickness in the range of 1 nm to 100 nm.

18. 15. The method of claim 14, wherein the method is carried out at a temperature in the range of 1°C to 200°C.

19. 1. A method of forming a device, comprising: patterning a first conductive material on a substrate; cross-patterning a resistive switching polymer film on the first conductive material, the resistive switching polymer film comprising one or more of polyamide, polyazomethine, polyurea, polyurethane, and derivatives thereof; depositing a second conductive material on the resistive switching polymer film; The method includes:

20. The method further includes depositing one or more dielectric films, the dielectric films being SiO x , Si x N y , Si, SiON, AlO x , HfO x , ZrO 2 , TiO x , Ta x O 5 , Y 2 O 3 , La 2 O 3 , AlN, MgO, CaF 2 , LiF, SrO, SiC, BaO, HfSiO 4 , LaAlO 3 , Nb 2 O 5 , BaTiO 3 , SrTiO 3 , Bi 4 Ti 3 O 12 , Pb(Zr,Ti)O 3 , CaCu 3 Ti 4 O 12 , LiNbO 3, BaTiO 3 , LiNbO 3 , KNbO 3 or a combination thereof.