Cellulose particles and cellulose particle dispersion
Patent Information
- Application Number
- JP2023222108
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-11-29
AI Technical Summary
【0012】 本発明によると、軽量であり、水系液体への再分散性が改善されたセルロース粒子及びセルロース粒子分散液となる。
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to cellulose particles and a cellulose particle dispersion. [Background technology]
[0002] Fine fibrous cellulose obtained by micronizing cellulose fibers has a low environmental impact and in recent years has been the subject of research into its applications in a variety of fields, with expectations being placed on its use in fields such as plastic materials, cosmetics, clothing, and construction.
[0003] Fine fibrous cellulose is generally used in an aqueous dispersion with a concentration of 5% by mass or less, and when it is dried, it has the property of agglomerating to each other and becoming particulate depending on the storage conditions. Once fine fibrous cellulose becomes particulate, it maintains its particulate state even when put into water, and it is difficult for it to be easily redispersed by breaking down the agglomerates, etc.
[0004] In this regard, there are several technologies that focus on the dispersibility of fine fibrous cellulose, and for example, these are disclosed in Patent Document 1. Patent Document 1 discloses a technology in which the problem to be solved by the invention is to provide a powdered nanofiber that can improve dispersibility in a matrix component such as a resin, and the means for solving the problem is a powdered nanofiber blended with a dispersant, in which the dispersant is at least one selected from the group consisting of a P-OH group, a -COOH group, a -SO3H group, and / or a metal base thereof, and an imidazoline group bonded thereto.
[0005] Furthermore, Patent Document 2, which discloses a related technology, aims to provide cellulose particles that have a small diameter while maintaining flexibility and reducing irritation to the skin, and provides a solution to this problem by providing cellulose particles that have an average particle size D50 of 1 μm or more and 50 μm or less, a bulk density of 0.30 g / mL or less, a specific volume of 3.0 mL / g or more, and a linseed oil absorption of 100 mL / 100 g or more.
[0006] However, the technology disclosed in Patent Document 1 aims to improve the dispersibility of powdered nanofibers in a matrix component that is a solid such as a resin, and does not disclose any knowledge regarding whether the powdered nanofibers will break down and be well dispersed and mixed when the matrix component is an aqueous liquid.
[0007] In addition, although the technology of Patent Document 2 assumes the use of cellulose particles as an additive in makeup products, there is no description of what to use as the matrix component, and therefore no knowledge of dispersibility in aqueous liquids is disclosed. Patent Document 3 is a technology related to porous cellulose particles with high sphericity, and is poorly related to the problem of the present invention. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2017-210596 A [Patent Document 2] JP 2019-206662 A [Patent Document 3] JP 2020-50840 A Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide cellulose particles and a cellulose particle dispersion having improved redispersibility in an aqueous liquid. [Means for solving the problem]
[0010] The above problem is solved by the following aspects. (First aspect) The cellulose ester contains 50% by mass or more of fine fibrous cellulose having an average fiber diameter of 1000 nm or less and has a packed bulk density of 0.1 to 200 mg / cm 3and having an average particle size of 0.1 to 1000 μm.
[0011] The cellulose particles of the above embodiment contain 50% by mass or more of fine fibrous cellulose having an average fiber diameter of 1000 nm or less, and are composed of relatively fine cellulose fibers that are mainly aggregated together. 3 The cellulose particles are relatively large, lightweight, and bulky, and it is presumed that when dispersed in an aqueous dispersion medium, the fibers constituting the cellulose particles are partially unraveled, etc., resulting in a physically dispersed state. Therefore, the cellulose particles are unlikely to precipitate even when redispersed in an aqueous liquid. Effect of the Invention
[0012] According to the present invention, there are obtained cellulose particles and a cellulose particle dispersion which are lightweight and have improved redispersibility in aqueous liquids. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is an explanatory diagram of a spray-freezing granulation device. [Diagram 2] 1 is an SEM image of cellulose particles. [Diagram 3] 1 is an SEM image of cellulose particles. [Figure 4] 1 is an SEM image of cellulose particles. [Diagram 5] 1 is an SEM image of cellulose particles. [Figure 6] FIG. 2 is a cross-sectional view of FIG. [Figure 7] FIG. 13 is a diagram showing the results of a redispersion test. [Figure 8] 1 is an SEM image of particles of Comparative Example 1. [Figure 9] FIG. 13 is a side view of a dryer according to another embodiment. [Figure 10] FIG. 10 is a view of the dryer in FIG. 9 as seen from the Y direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] An embodiment of the present invention will be described below. Note that the embodiment is an example of the present invention. The scope of the present invention is not limited to the scope of the embodiment.
[0015] The cellulose particles according to the present invention contain 50% by mass or more of fine fibrous cellulose having an average fiber diameter of 1000 nm or less and have a packed bulk density of 0.1 to 200 mg / cm 3 and has an average particle size of 0.1 to 1000 μm. Before describing the cellulose particles, the fine fibrous cellulose, which is the raw material of the cellulose particles, will be described.
[0016] (Fine fibrous cellulose) Fine fibrous cellulose can be obtained by defibrating (refining) raw pulp, and can be produced by known processing methods such as chemical processing and mechanical processing.
[0017] As the raw material pulp for the fine fibrous cellulose, one or more of wood pulp made from broadleaf trees, coniferous trees, etc., non-wood pulp made from straw, bagasse, cotton, hemp, bast fiber, etc., waste paper pulp (DIP) made from brown waste paper, envelope paper, magazine paper, flyer paper, cardboard paper, white waste paper, imitation waste paper, reclaimed waste paper, recycled waste paper, and broke paper, etc., can be selected and used. The above various raw materials may be in the form of a pulverized material called cellulose-based powder, for example. In recent years, the demand for products containing organic components that are environmentally friendly has been increasing, so wood pulp made from broadleaf trees or coniferous trees derived from plants other than waste paper is particularly suitable.
[0018] As the wood pulp, one or more types may be selected and used from chemical pulps such as hardwood kraft pulp (LKP), softwood kraft pulp (NKP), sulfite pulp (SP), dissolving pulp (DP), etc., and mechanical pulp (TMP). In particular, chemical pulps such as hardwood kraft pulp (LKP) and softwood kraft pulp (NKP), which are wood pulps that increase the cellulose component, are preferred, and bleached pulp (BKP) is suitable.
[0019] As the mechanical pulp, for example, one or more types can be selected and used from stone ground pulp (SGP), pressed stone ground pulp (PGW), refiner ground pulp (RGP), chemi-ground pulp (CGP), thermo-ground pulp (TGP), ground pulp (GP), thermo-mechanical pulp (TMP), chemi-thermomechanical pulp (CTMP), refiner mechanical pulp (RMP), bleached thermo-mechanical pulp (BTMP), etc.
[0020] From the viewpoint of producing fine fibrous cellulose having a relatively small average fiber diameter, it is preferable to use kraft pulp, which is easy to defibrate and has high dispersibility. In particular, when applied to white products (lotions, gels, etc.), it is convenient that the fine fibrous cellulose itself is white, and from the viewpoint of improving the high whiteness, it is more preferable to use LBKP and NBKP.
[0021] The fine fibrous cellulose may be pretreated prior to defibration. For example, the pretreatment may involve mechanically pre-beating the raw pulp or chemically modifying the raw pulp. The method of pre-beating is not particularly limited, and any known method may be used.
[0022] Examples of pretreatment of raw material pulp by chemical techniques include hydrolysis of polysaccharides with acids (e.g., sulfuric acid, etc.) (acid treatment), hydrolysis of polysaccharides with enzymes (enzyme treatment), swelling of polysaccharides with alkali (alkali treatment), oxidation of polysaccharides with an oxidizing agent (e.g., ozone, etc.) (oxidation treatment), reduction of polysaccharides with a reducing agent (reduction treatment), oxidation with a TEMPO catalyst (oxidation treatment), anionization (anion treatment) and cationization (cation treatment) by phosphate esterification, carbamate formation, etc.
[0023] Examples of the alkali used in the alkali treatment include organic alkali such as sodium hydroxide, lithium hydroxide, potassium hydroxide, aqueous ammonia solution, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrabutylammonium hydroxide, and benzyltrimethylammonium hydroxide. From the viewpoint of production costs, it is preferable to use sodium hydroxide.
[0024] By subjecting the fine fibrous cellulose to an enzyme treatment, an acid treatment, or an oxidation treatment, it is possible to lower the water retention of the fine fibrous cellulose, increase the crystallinity, and increase the homogeneity. If the water retention of the fine fibrous cellulose is low, it is preferable because it is easy to dehydrate and dry.
[0025] When raw pulp is treated with an enzyme, acid, or oxidation, the hemicellulose and amorphous regions of cellulose contained in the pulp are decomposed, and as a result, the energy required for the fine pulp refining process can be reduced and the uniformity and dispersibility of the cellulose fibers can be improved. The dispersibility of the cellulose fibers contributes to improving the uniformity of the molded body, for example. However, since the pretreatment reduces the aspect ratio of the fine fibrous cellulose, excessive pretreatment is preferably avoided.
[0026] Examples of fine fibrous cellulose that has been modified by anionization through the introduction of anionic functional groups include fine fibrous cellulose that has been esterified with phosphorus oxoacid, fine fibrous cellulose that has been carbamate-treated, and fine fibrous cellulose in which the hydroxyl groups of the pyranose rings have been directly oxidized to carboxyl groups.
[0027] Fine fibrous cellulose modified by the introduction of anionic functional groups has relatively high dispersibility, which is presumably because the anionic functional groups cause localized charge bias and easily form hydrogen bonds with water and organic solvents in the dispersion.
[0028] When cellulose fibers are subjected to esterification with phosphorus oxoacid, which is an example of anionization, the fiber raw material can be finely divided, and the fine fibrous cellulose produced has a large aspect ratio, excellent strength, high light transmittance and high viscosity. Esterification with phosphorus oxoacid can be performed by the method described in JP 2019-199671 A. For example, modified fine fibrous cellulose in which hydroxyl groups of cellulose fibers are modified to introduce phosphite ester groups can be mentioned.
[0029] The cellulose fibers can be defibrated by the following defibration devices and methods. The defibration can be performed by using one or more means selected from homogenizers such as high-pressure homogenizers and high-pressure homogenizers, grinders, grinders, and other mill-type friction machines, refiners such as conical refiners and disk refiners, and various bacteria. However, it is preferable to defibrate the cellulose fibers using a water flow, particularly a high-pressure water flow, and a device or method for finely pulverizing the fibers. This device or method provides very high dimensional uniformity and dispersion uniformity for the fine fibrous cellulose obtained. In contrast, for example, when a grinder that grinds between rotating grindstones is used, it is difficult to uniformly pulverize the cellulose fibers, and in some cases, there is a risk that some fiber lumps will remain undisintegrated.
[0030] Grinders used to defibrate cellulose fibers include, for example, the Masscolloider manufactured by Masuko Sangyo Co., Ltd. Devices that use high-pressure water flow to pulverize materials include, for example, Starburst (registered trademark) manufactured by Sugino Machine Co., Ltd. and Nanovater (registered trademark) manufactured by Yoshida Kikai Kogyo Co., Ltd. High-speed rotary homogenizers used to defibrate cellulose fibers include the Clearmix-11S manufactured by M Technique Co., Ltd.
[0031] The present inventors have found that when cellulose fibers are defibrated using both a method of grinding between rotating grinding wheels and a method of refining with a high-pressure water jet, and the resulting fibers are observed under a microscope, the fibers obtained using the method of refining with a high-pressure water jet have a more uniform fiber width.
[0032] Defibration using a high-pressure water stream is preferably performed by pressurizing a dispersion of cellulose fibers with a pressure booster to, for example, 30 MPa or more, preferably 100 MPa or more, more preferably 150 MPa or more, and particularly preferably 220 MPa or more (high pressure condition), spraying it from a nozzle with a pore diameter of 50 μm or more, and reducing the pressure so that the pressure difference is, for example, 30 MPa or more, preferably 80 MPa or more, and more preferably 90 MPa or more (reduced pressure condition). The pulp fibers are defibrated by the cleavage phenomenon caused by this pressure difference. If the pressure of the high-pressure condition is low or the pressure difference from the high-pressure condition to the reduced pressure condition is small, the defibration efficiency decreases, and repeated defibration (spraying from the nozzle) becomes necessary to achieve the desired fiber width.
[0033] As a device for defibrating with a high-pressure water flow, it is preferable to use a high-pressure homogenizer. A high-pressure homogenizer is a homogenizer capable of ejecting a slurry of cellulose fibers at a pressure of, for example, 10 MPa or more, preferably 100 MPa or more. When cellulose fibers are treated with a high-pressure homogenizer, the cellulose fibers are effectively defibrated due to the action of collisions between the cellulose fibers, pressure differences, microcavitation, etc. Therefore, the number of defibration treatments can be reduced, and the production efficiency of fine fibrous cellulose can be improved.
[0034] It is preferable to use a high-pressure homogenizer that causes the cellulose fiber slurry to collide in a straight line. Specifically, for example, a high-pressure homogenizer of the counter-collision type (MICROFLUIDIZER (registered trademark), wet jet mill) is used. In this device, two upstream flow paths are formed so that the pressurized cellulose fiber slurry collide in a counter-collision manner at the junction. The cellulose fiber slurry collides at the junction, and the collided cellulose fiber slurry flows out from the downstream flow path. The downstream flow path is provided perpendicular to the upstream flow path, and a T-shaped flow path is formed by the upstream flow path and the downstream flow path. When such a counter-collision type high-pressure homogenizer is used, the energy provided by the high-pressure homogenizer is converted to collision energy to the maximum extent, so that the cellulose fibers can be defibrated more efficiently.
[0035] The fine fibrous cellulose obtained by defibration can be dispersed in an aqueous medium to prepare a dispersion liquid prior to mixing with inorganic fine particles. The aqueous medium is particularly preferably entirely water (aqueous solution). However, the aqueous medium may be partially other liquids that are compatible with water. As the other liquids, for example, lower alcohols having 3 or less carbon atoms can be used.
[0036] In this specification, fine fibrous cellulose in which the hydroxyl groups of cellulose fibers have been substituted (modified) and phosphorus oxo acid ester groups have been introduced is referred to as modified fine fibrous cellulose (hereinafter also referred to as "modified CNF"), and may be distinguished from unmodified fine fibrous cellulose in which the hydroxyl groups of cellulose fibers have not been substituted (hereinafter also referred to as "unmodified CNF"). Therefore, fine fibrous cellulose is a concept that includes modified fine fibrous cellulose and unmodified fine fibrous cellulose.
[0037] The fine fibrous cellulose forming the cellulose particles of this embodiment may consist of only unmodified fine fibrous cellulose, may consist of only modified fine fibrous cellulose, or may contain both unmodified fine fibrous cellulose and unmodified fine fibrous cellulose.
[0038] When the cellulose particles are formed from modified fine fibrous cellulose, the dispersion liquid in which the cellulose particles are dispersed in a dispersion medium exhibits a transparent color. On the other hand, when the cellulose particles are formed from unmodified fine fibrous cellulose, the dispersion liquid in which the cellulose particles are dispersed in a dispersion medium exhibits a white color. By adjusting the ratio of modified fine fibrous cellulose and unmodified fine fibrous cellulose in the fine fibrous cellulose forming the cellulose particles, a dispersion liquid having an intermediate color between white and transparent can be produced. To produce this dispersion liquid, for example, when producing cellulose particles as the dispersoid of the dispersion liquid, it is preferable to use a mixture of modified fine fibrous cellulose and unmodified fine fibrous cellulose as the fine fibrous cellulose, which is the raw material of the cellulose particles.
[0039] The cellulose particles are in the form of a white powder whether the raw material is modified or unmodified fine fibrous cellulose. Since modified fine fibrous cellulose has a smaller average fiber diameter than unmodified fine fibrous cellulose, when compared with cellulose particles of the same mass, the cellulose particles formed from modified fine fibrous cellulose tend to have a larger specific surface area than the cellulose particles formed from unmodified fine fibrous cellulose.
[0040] The raw material pulp is preferably defibrated so that the physical properties of the resulting fine fibrous cellulose have the desired values or evaluations as shown below.
[0041] <Average fiber diameter> The upper limit of the average fiber diameter (average fiber width; average diameter of a single fiber) of fine fibrous cellulose is 1000 nm or less, preferably 500 nm or less, more preferably 100 nm or less, and particularly preferably 50 nm or less. If the average fiber diameter of fine fibrous cellulose exceeds 1000 nm, the formed cellulose particles will have a relatively small specific surface area, i.e., a poorly porous shape. On the other hand, the average fiber diameter of fine fibrous cellulose has no particular lower limit.
[0042] The average fiber diameter of the fine fibrous cellulose can be adjusted, for example, by the selection of raw pulp, pretreatment, defibration, etc.
[0043] The method for measuring the average fiber diameter of the fine fibrous cellulose is as follows. First, 100 ml of an aqueous dispersion of fine fibrous cellulose with a solid content concentration of 0.01 to 0.1% by mass is filtered through a Teflon (registered trademark) membrane filter, and the solvent is replaced once with 100 ml of ethanol and three times with 20 ml of t-butanol. Next, the sample is freeze-dried and osmium-coated to obtain a sample. This sample is observed using an electron microscope SEM image at a magnification of 3,000 to 30,000 times depending on the width of the fibers that constitute it. Specifically, two diagonal lines are drawn on the observed image, and three straight lines passing through the intersections of the diagonal lines are arbitrarily drawn. Furthermore, the widths of a total of 100 fibers that intersect with these three straight lines are visually measured. The median diameter of the measured values is then taken as the average fiber diameter.
[0044] <Average fiber length> The average fiber length of the fine fibrous cellulose (average length of a single fiber) is, for example, preferably 0.01 to 1000 μm, more preferably 0.05 to 500 μm. If the average fiber length exceeds 1000 μm, the fibers will be intricately entangled with each other when the fine fibrous cellulose is dried, making it easier to support other substances, and the intricate entanglement will make it difficult for the particles to come apart when redispersed.
[0045] The average fiber length can be adjusted as desired by, for example, selecting the raw pulp, pre-treating, defibrating, and the like.
[0046] The average fiber length of the fine fibrous cellulose is measured in the same manner as in the case of the average fiber diameter, by visually measuring the length of each fiber. The median length of the measured values is taken as the average fiber length.
[0047] <Axle ratio> The axial ratio of the fine fibrous cellulose (average fiber length / average fiber width) is preferably 10 to 1,000,000, more preferably 50 to 500,000, and particularly preferably 100 to 100,000. When the axial ratio of the fine fibrous cellulose is less than 10, the cellulose component is almost in a particulate form, making it difficult to form cellulose particles. On the other hand, when the axial ratio exceeds 1,000,000, the degree of entanglement between the fibers becomes large, making it difficult to obtain cellulose particles with the desired average particle size.
[0048] <Crystallization degree> The crystallinity of the fine fibrous cellulose has a lower limit of 50 or more, more preferably 60 or more, and particularly preferably 65 or more, and an upper limit of 100 or less, more preferably 95 or less, and particularly preferably 90 or less. If the crystallinity is less than 50, the entanglement of the fibers will be weakened due to the influence of temperature changes during drying, etc., and the retention of other substances will be weakened, making it difficult to form cellulose particles of the desired particle size.
[0049] The crystallinity is a value measured by X-ray diffraction in accordance with JIS-K0131 (1996) "General Rules for X-ray Diffraction Analysis." Note that fine fibrous cellulose has an amorphous portion and a crystalline portion, and the crystallinity refers to the proportion of the crystalline portion in the entire fine fibrous cellulose.
[0050] <Pseudo particle size distribution> The peak value in the pseudo particle size distribution curve of the fine fibrous cellulose is preferably one peak. When there is one peak, the fine fibrous cellulose has high uniformity in fiber length and fiber diameter, and the fine fibrous cellulose easily becomes entangled with each other during the production of cellulose particles, so that the produced cellulose particles are difficult to be unraveled even when redispersed. In addition, the cellulose particles have a small variation in particle size. If the cellulose particles are in the form of inorganic fine particles supported, the cellulose particles are sufficiently dispersed in the cosmetic when the cellulose particles are blended as one component of the cosmetic.
[0051] The peak value of the fine fibrous cellulose is measured in accordance with ISO-13320 (2009). More specifically, a particle size distribution measuring device (Laser Diffraction / Scattering Particle Size Distribution Meter manufactured by Seishin Enterprise Co., Ltd.) is used to examine the volumetric particle size distribution of the aqueous dispersion of the fine fibrous cellulose. Then, the most frequent diameter of the fine fibrous cellulose is measured from this distribution. This most frequent diameter is taken as the peak value. It is preferable that the fine fibrous cellulose has a single peak in a pseudo particle size distribution curve measured by a laser diffraction method in an aqueous dispersion state. In this way, the fine fibrous cellulose having one peak is preferable because it has been sufficiently refined and can exhibit good physical properties as fine fibrous cellulose. The peak value of the pseudo particle size distribution of the particle size of the fine fibrous cellulose having the single peak is, for example, preferably 300 μm or less, more preferably 200 μm or less, and particularly preferably 100 μm or less. If the peak value exceeds 300 μm, there are many relatively large fibers, the particle size of the cellulose particles varies greatly, and the shape of the cellulose particles tends to be non-uniform.
[0052] The peak value in the particle size and the median diameter in the pseudo-particle size distribution of the fine fibrous cellulose can be adjusted, for example, by the selection of raw pulp, pretreatment, defibration, etc.
[0053] <Water retention> The water retention of the fine fibrous cellulose is not particularly limited, but for example, in the case of unmodified fine fibrous cellulose, it is 500% or less, more preferably 100 to 500%. If the water retention exceeds 500%, the fine fibrous cellulose itself has high water retention and poor dehydration, so even if it is produced through a drying process, the drying time becomes long and productivity is poor. The lower limit of the water retention of the fine fibrous cellulose is not particularly limited, but if it is 100% or more, the dispersibility of the fine fibrous cellulose is improved, so it is preferable.
[0054] The water retention of the fine fibrous cellulose can be adjusted as desired by, for example, selecting the raw pulp, pre-treating it, defibrating it, and the like.
[0055] The water retention of the fine fibrous cellulose is a value measured in accordance with JAPAN TAPPI No. 26 (2000).
[0056] <Pulp viscosity> The pulp viscosity of the defibrated fine fibrous cellulose is 1 to 10 cps, more preferably 2 to 9 cps, and particularly preferably 3 to 8 cps. The pulp viscosity is the viscosity of the solution obtained by dissolving cellulose in a copper ethylenediamine solution, and a higher pulp viscosity indicates a higher degree of polymerization of cellulose, which also affects the strength of the fiber itself.
[0057] (Additives) Additives can be added to improve the dispersibility of the cellulose particles produced through the drying process in a solvent. The additives can be added to the fine fibrous cellulose before freezing, and may be mixed uniformly. As the additives, one or more selected from the group consisting of polyhydric alcohols, polysaccharides, and water-soluble polymers may be used. The compounding ratio of the additives (=additives:fine fibrous cellulose) is 1:99 to 50:50, preferably 50:50, based on the solid content. If the compounding ratio of the additives to the fine fibrous cellulose is high, the dried product (cellulose particles) becomes sticky, the lightness of the cellulose particles of the present invention is lost, and the handling properties are deteriorated. On the other hand, if the compounding ratio is too low, the dispersion effect in the target solvent may be deteriorated.
[0058] As the additive, polyhydric alcohols such as glycerin, propylene glycol, butylene glycol, pentanediol, dipropylene glycol, hexanediol, heptanediol, etc. can be used, but are not limited to these. Glycerin is particularly preferred from the viewpoint of thickening properties and dispersibility of composite particles.
[0059] Examples of polysaccharides that can be used include, but are not limited to, quince seed, veegum, xanthan gum, hyaluronate, etc. Hyaluronate is particularly preferred from the viewpoint of thickening properties and dispersibility of cellulose particles.
[0060] Examples of the water-soluble polymer include, but are not limited to, polyvinyl alcohol, polyvinylpyrrolidone, carboxyvinyl polymer, and polyethylene glycol. In particular, polyvinylpyrrolidone is preferred from the viewpoints of viscosity increasing property and dispersibility of cellulose particles.
[0061] (Inorganic fine particles) The cellulose particles may contain inorganic fine particles. The inorganic fine particles can impart various functions to the cellulose particles. For example, metal-based inorganic fine particles have the effect of diffusely reflecting incident light, so that the cellulose particles can be imparted with the effect of diffusely reflecting light by containing inorganic fine particles in the cellulose particles. For example, the cellulose particles containing inorganic fine particles can be used as one component of a cosmetic to provide a cosmetic with a sunlight transmission suppression effect. The cosmetic with a sunlight transmission suppression effect can be applied to the skin to provide a sunscreen effect.
[0062] The content of inorganic fine particles in the cellulose particles may be set at an upper limit of 50% by mass, preferably 45% by mass or less, and at a lower limit of 0% by mass, preferably 5% by mass or more. If the content exceeds 50% by mass, the ratio of inorganic fine particles to the fine fibrous cellulose is large, the specific gravity of the cellulose particles is large, and there is a risk of high redispersibility in the dispersion medium being impaired. On the other hand, if the content is 5% by mass or more, the effect of suppressing the transmission of sunlight is sufficiently exhibited.
[0063] The upper limit of the primary particle diameter of the inorganic fine particles is preferably 10 μm, more preferably 5 μm or less, and more preferably 1 μm or less. If the primary particle diameter of the inorganic fine particles exceeds 10 μm, the inorganic fine particles are difficult to support by the fine fibrous cellulose. In addition, the surface area of the cellulose particles is not sufficiently large. The inorganic fine particles are not particularly limited in terms of the lower limit, but are preferably 1 nm, more preferably 2 nm or more, and more preferably 3 nm or more. If the primary particle diameter of the inorganic fine particles is 1 nm or more, when the inorganic fine particles are mixed with a slurry of the fine fibrous cellulose, the inorganic fine particles are easily dispersed and cling to the fine fibrous cellulose.
[0064] The primary particle size of the inorganic fine particles can be measured by observation under an electron microscope, and the average value of the obtained particle sizes is taken as the measured value.
[0065] The inorganic fine particles can be used as they are, but it is preferable to subject them to hydrophilic treatment, since it makes them more compatible with the aqueous dispersion of fine fibrous cellulose. The surface treatment agent used for hydrophilic treatment has the effect of suppressing the surface activity of the inorganic fine particles, improving the dispersibility of the inorganic fine particles, and improving transparency and squeaking. The surface treatment agent for the inorganic fine particles is not particularly limited as long as it is a treatment agent that can be dispersed in the aqueous dispersion of fine fibrous cellulose, but it is preferable to use one that contains silicic anhydride or hydrated silicic acid.
[0066] The inorganic fine particles are not particularly limited and known inorganic fine particles can be used, for example, barium titanate, lead zirconate titanate, silicon carbide, silicon nitride, aluminum nitride, alumina, zirconia, zircon, titanium oxide, zinc oxide, iron oxide, cerium oxide, etc. Cellulose particles having these powders and fine fibrous cellulose are preferable because they have excellent redispersibility in liquid. From the viewpoint of suppressing the transmission of sunlight, for example, one or a combination of two or more selected from the group consisting of titanium oxide, zinc oxide, iron oxide, and cerium oxide can be used. In particular, when the inorganic fine particles are titanium oxide, rutile type is preferable because it improves the suppression of the transmission of sunlight in the cosmetic composition.
[0067] The shape of the inorganic fine particles that can be contained in the cellulose particles is not particularly limited, and can be, for example, spherical, rod-like, needle-like, spindle-like, plate-like, polygonal, or the like.
[0068] The inorganic fine particles may be attached to the surface of the fine fibrous cellulose in the cellulose particles, or may be encapsulated in the fine fibrous cellulose. When the inorganic fine particles are encapsulated in the fine fibrous cellulose, the cellulose particles can support the inorganic fine particles not only on the surface but also inside, and have excellent transmittance suppression against irradiation of sunlight from various angles. Here, encapsulation can refer to a state in which a part of the surface of the inorganic fine particles is covered with the fine fibrous cellulose, or a state in which the inorganic fine particles are covered with the fine fibrous cellulose and cannot be observed when the cellulose particles are observed from the outside.
[0069] The inorganic particles can be added to the fine fibrous cellulose before freezing and mixed until homogeneous.
[0070] (Cellulose particles) The cellulose particles according to the present embodiment preferably contain 50% by mass or more of fine fibrous cellulose, more preferably 60% by mass or more, and even more preferably 70% by mass or more, with the upper limit being 100% by mass. If the mass percentage of fine fibrous cellulose in the cellulose particles is less than 50% by mass, the desired bulk density and specific surface area of the cellulose particles of the present invention may not be obtained.
[0071] The cellulose particles according to the present embodiment preferably have a packed bulk density of 0.1 to 200 mg / cm 3 and the average particle size is in the range of 0.1 to 1000 μm, and more preferably the packed bulk density is in the range of 0.1 to 150 mg / cm 3 and the average particle size is in the range of 0.1 to 700 μm, and more preferably the packed bulk density is in the range of 0.1 to 100 mg / cm 3 The packed bulk density and the average particle size are factors that are strongly related to redispersibility. For example, even if the average particle size is 1000 μm, which is the upper limit of the above range, the packed bulk density is 200 mg / cm, which is the upper limit of the above range. 3 If the average particle size exceeds 1000 μm, which is the upper limit of the above range, the packed bulk density will be 0.1 mg / cm3, which is the lower limit of the above range. 3 Below this density, the cellulose particles become extremely light and porous, but they cannot retain their shape in the air for long periods of time and tend to disintegrate, making them very difficult to handle.
[0072] The average particle size of cellulose particles was measured using a measuring device conforming to ISO-13320 (2009), specifically, the laser diffraction / scattering particle size distribution measuring device (particle size distribution) "LA-960V2", using a dry method without removing the moisture adhering to the cellulose particles.
[0073] (specific surface area) The specific surface area of the cellulose particles is preferably 20 m 2 / g or more, more preferably 30m 2 / g or more, more preferably 40m 2 / g or more, and the upper limit of the specific surface area is not particularly limited, but is 5000 m 2 / g. The specific surface area is 20m 2 If the specific surface area is less than 5000 m / g, the contact area between the cellulose particles and the dispersion medium is small, making them difficult to blend together and resulting in poor redispersibility. 2 A particle size exceeding this limit is preferable in terms of reducing the particle weight and redispersibility, but is very difficult to produce.
[0074] The specific surface area was measured by the BET method. Specifically, the measurement was performed using a Quantachrome Instruments NOVA4200e measuring instrument, using the nitrogen gas adsorption method. The test method used was JIS Z8830:2013.
[0075] (viscosity) Cellulose particles have many hydrogen bond points in the cellulose fibers, and when they are mixed with a dispersion medium that has affinity for cellulose particles (such as water or an organic solvent), they disperse and become a dispersion liquid. The dispersed cellulose particles lose their degree of freedom as the polar groups of the cellulose particles themselves bond with other cellulose particles through hydrogen bonds or the like, resulting in a viscous liquid.
[0076] In the dispersion, the cellulose particles are bonded to each other by hydrogen bonds and the like while dispersed, giving the cellulose particles viscosity. When shear force is applied to the dispersion, the hydrogen bonds weaken and the viscosity decreases. This gives the cellulose particles thixotropy. The viscosity varies depending on the concentration of the cellulose particles in the dispersion and the raw material of the cellulose particles.
[0077] When a dispersion containing 2% by mass of cellulose particles (in this specification, the dispersion medium when measuring the B-type viscosity is water) is measured under conditions of 25°C and 6 rpm, the B-type viscosity is preferably 1000 cps or more, preferably 1000 to 30000 cps, and more preferably 1500 to 20000 cps. If the B-type viscosity is less than 1000 cps, the redispersibility in the dispersion medium may be weak. When a dispersion containing 2% by mass of cellulose particles is measured under conditions of 25°C and 60 rpm, the B-type viscosity is preferably 100 cps or more, preferably 100 to 10000 cps, and more preferably 200 to 9000 cps. If the B-type viscosity is less than 100 cps, the ratio to the B-type viscosity at 6 rpm is small, and the redispersibility in the dispersion medium may be weak.
[0078] The Ti value at 25°C of a dispersion containing 2% by mass of cellulose particles is preferably 2 or more, more preferably 3 or more, and even more preferably 4 or more. The Ti value indicates the property of decreasing viscosity when subjected to shear stress (pseudoplasticity), and the larger the value, the better the spread of a dispersion containing 2% by mass of cellulose particles when applied to the skin, for example. The closer the Ti value of a cellulose particle dispersion is to the Ti value measured when a 2% by mass dispersion of fine fibrous cellulose required to produce the cellulose particles is measured under the same conditions as those under which the cellulose particle dispersion was measured (i.e., the B-type viscosity of the dispersion at 25°C and 6 rpm and the B-type viscosity of the dispersion at 25°C and 60 rpm), the higher the redispersibility can be said to be.
[0079] The Ti value can be calculated using the following formula 1. [Formula 1] (Ti value) = (B-type viscosity of dispersion at 25°C and 6 rpm) / (B-type viscosity of dispersion at 25°C and 60 rpm)
[0080] Here, the B-type viscosity was measured in accordance with JIS-Z8803 (2011) "Method of measuring viscosity of liquids." B-type viscosity is the resistance torque when stirring a dispersion liquid, and the higher the viscosity, the more energy is required for stirring.
[0081] The B-type viscosity and Ti value of the dispersion can be adjusted by several factors. For example, the B-type viscosity can be adjusted by changing the properties of the cellulose particles themselves and the concentration of cellulose particles in the dispersion. When the cellulose particles are not modified, a high redispersibility is exhibited in the dispersion when the concentration of cellulose particles in the dispersion is 1 to 3 mass%. When the cellulose particles are modified, a high redispersibility is exhibited in the dispersion when the concentration of cellulose particles in the dispersion is 0.5 to 2.0 mass%. If the concentration exceeds the above range, the amount of cellulose particles in the dispersion is too large, so the B-type viscosity increases extremely, and if the concentration is below the above range, the amount of cellulose particles is small, so the viscosity is the same as that of water.
[0082] When either fine fibrous cellulose or cellulose particles are dispersed in water to form a dispersion, the dispersion has a certain B-type viscosity. If the B-type viscosity of the fine fibrous cellulose dispersion is V0 and the B-type viscosity of a dispersion of cellulose particles produced using the fine fibrous cellulose as a raw material (i.e., cellulose particle dispersion) is V1, the viscosity change rate PV can be expressed by the following formula. PV(%)=(V1 / V0)×100 Since the B-type viscosity of the dispersion changes depending on whether the fine fibrous cellulose is modified or unmodified, when the fine fibrous cellulose is unmodified, the fine fibrous cellulose concentration (or cellulose particle concentration) in the dispersion should be measured at 2 mass%, and when the fine fibrous cellulose is modified, the fine fibrous cellulose concentration (or cellulose particle concentration) in the dispersion should be measured at 0.5 mass%.
[0083] The viscosity change rate PV varies depending on the rotation speed when measuring the B-type viscosity, and for the fine fibrous cellulose and cellulose particles of this embodiment, the viscosity change rate PV at a rotation speed of 6 rpm is preferably 30% or more, more preferably 40% or more. If the viscosity change rate PV is less than 30%, the cellulose particles will have a high solidity and a poor lightness. Furthermore, for the fine fibrous cellulose and cellulose particles of this embodiment, when the rotation speed is 60 rpm, the viscosity change rate PV is preferably 40% or more, more preferably 45% or more.
[0084] (moisture content) The moisture content of the cellulose granules is preferably 50% or less, more preferably 40%, and even more preferably 30% or less. If the moisture content exceeds 50%, the amount of water adsorbed by the cellulose granules becomes large, and the lightweight feel is lost.
[0085] (Bulk density) The bulk density of the cellulose particles of this embodiment is preferably 0.1 to 200 mg / cm3. 3 , more preferably 0.1 to 150 mg / cm 3 , and more preferably 0.1 to 100 mg / cm 3 The compacted bulk density is 0.1 mg / cm 3 If the packed bulk density is less than 200 mg / cm, the powder will easily disintegrate in the air and handling will be impaired. 3 If the density exceeds this range, the fibers will form strong agglomerates and will have poor dispersibility.
[0086] (Degree of compression) In addition, the cellulose particles have a packed bulk density of 0.1 to 200 mg / cm3 as described above. 3and the degree of compression is preferably 50% or less, more preferably 45% or less, and even more preferably 40%. Since the cellulose particles of this embodiment are relatively light, the voids are eliminated during the process of performing the compression operation for measuring the packed bulk density after measuring the loose bulk density (i.e., the cellulose particles are densely packed together in the container due to the voids being eliminated), and the change in density of the cellulose particles themselves is small, and the collapse of the particle shape is unlikely to occur. In addition, since the cellulose particles are not spherical with excellent sphericity, but are uneven granules (although it is difficult to express), many voids of various shapes and sizes are generated when the cellulose particles are filled in a container. If the degree of compression exceeds 50%, the voids between the particles are filled, and the collapse of the cellulose particles is suggested, so that the lightness of the particles may be lost. Note that, in the case of cellulose particles produced by hot drying, even if the degree of compression is 50%, the bulk density is 200 mg / cm 3 Above this value, the fibers are tightly aggregated to form solid particles, so they simply fill the gaps between the particles, and the particles themselves do not collapse easily.
[0087] The packed bulk density and loose bulk density are items used to calculate the Carr fluidity index, and were measured in accordance with the ASTM D6393-99 Compressibility Measurement Method. The measurements were performed using a multi-function powder property measuring instrument, Multitester MT-02 (manufactured by Seishin Enterprise Co., Ltd.).
[0088] (Manufacturing) The cellulose particles can be produced by freeze-drying the cellulose nanofiber raw material, drying under reduced pressure, heat drying, spray drying, or the spray-type freezing and vacuum drying method of the present embodiment, but the spray-type freezing and vacuum drying method is particularly preferred because it allows the production of porous cellulose particles. If the cellulose particles are porous, it is possible to support another substance in the numerous pores formed in the cellulose particles, or to utilize the large surface area. This allows the cellulose particles to be endowed with properties not found in cellulose.
[0089] The cellulose particles according to the present invention can be produced by a freeze-drying process. For example, a spray-type freeze granulation apparatus 1 shown in Fig. 1 is preferable because it can produce particles with a relatively small specific gravity. The spray-type freeze granulation apparatus 1 comprises a freeze granulation tank 8, a spray mechanism unit 7 that sprays raw material M onto the upper part of the freeze granulation tank 8, and a drying unit 6 that is provided below the freeze granulation tank 8 and dries the frozen cellulose particles. The raw material M sprayed into the freeze granulation tank 8 is instantly frozen in the freeze granulation tank 8 to become a frozen body P. The frozen body P falls naturally into the drying unit 6 and is stored therein. The drying unit 6 is separably connected to the freeze granulation tank 8, and is separated from the freeze granulation tank 8 when the frozen body P is stored therein, and is sealed so that the frozen body P can be dried to obtain cellulose particles.
[0090] Examples of the raw material M include a slurry or dispersion of fine fibrous cellulose. The fine fibrous cellulose used in the raw material M may be fine fibrous cellulose consisting of one group, or may be a combination of fine fibrous cellulose consisting of two groups. When a combination of fine fibrous cellulose consisting of two groups is used, it may be a combination of fine fibrous cellulose group C1 having an average particle diameter R of 11 to 1000 nm and fine fibrous cellulose group C2 having an average particle diameter R of 1 to 10 nm, in a mixing ratio of 1:99 to 99:1.
[0091] The spray mechanism 7 has a raw material flow path to which the raw material M is supplied, a compressed gas flow path to which the compressed gas A is supplied, and a nozzle 5 (also called a two-fluid nozzle) that sprays a mixed fluid of the supplied raw material M and compressed gas A into the freeze granulation tank 8. Examples of the type of the nozzle 5 include a three-fluid type, a four-fluid type, a pressurized type, an ultrasonic type, and a centrifugal spray type.
[0092] The raw material flow path has a base end connected to a raw material tank that stores raw material M, and a pump provided in the raw material flow path causes raw material M to flow from the raw material tank to nozzle 5. The compressed gas flow path has a base end connected to a compressed gas supply device such as a compressor or a cylinder, and when the compressed gas supply device is started, compressed gas flows into nozzle 5. Examples of compressed gas include air, nitrogen, and rare gases.
[0093] In addition to the fine fibrous cellulose, the raw material M may contain additives and inorganic fine particles, and may further contain the following materials. As the materials, plasticizers (phthalic acid esters, citrate esters, etc.), emulsifiers (e.g., nonionic surfactants, anionic surfactants, cationic surfactants, amphoteric surfactants, phospholipids, etc.) can be used, and in particular, it is preferable to use ester-type or ester-ether-type nonionic surfactants, and for example, glycerin fatty acid esters, polyglycerin, fatty acid esters, propylene glycol fatty acid esters, sorbitan fatty acid esters, and fatty acid esters of sorbitol, as well as their alkylene glycol adducts, polyalkylene glycol fatty acid esters, sucrose fatty acid esters, polysorbate 20, polysorbate 60, polysorbate 80, polyoxyalkylene alkyl ethers, polyoxyethylene alkylphenyl ethers, etc. can be added to the raw material M.
[0094] The freezing granulation tank 8 is composed of three tanks, specifically, three cylinders with different diameters arranged concentrically with the same axis in the vertical direction. These three cylinders are, in order from the inside, an inner tank wall 2, a middle tank wall 3, and an outer tank wall 4. The inner tank surrounded by the inner tank wall 2 is a freezing tank 12 for freezing the raw material M, the bottomed middle layer surrounded by the inner tank wall 2 and the middle tank wall 3 is a cooling medium filled tank 13 filled with a cooling medium, and the bottomed outer tank surrounded by the outer tank wall 4 and the middle tank wall 3 is a vacuum insulation tank 14 for keeping the temperature inside the tank constant. The freezing tank 12 is preferably configured so that the lower end of the inner tank wall 2 is detachably connected to a flange portion 4a formed at the upper end of the drying section 6.
[0095] The freezing tank 12 freezes the raw material M sprayed from a nozzle 5 provided near the top surface to form a frozen body P. The temperature of the freezing tank 12 is preferably kept at -10°C to -200°C by the cooling medium supplied from a cooling medium filling tank 13.
[0096] The cooling medium tank 13 is filled with a cooling medium for cooling the freezing tank 12. As the cooling medium, for example, liquid nitrogen, liquid argon, liquid helium, dry ice, etc. can be used.
[0097] The vacuum insulation tank 14 is surrounded by an inner tank wall 2 and an outer tank wall 4, with the upper end of the inner tank wall 2 and the upper end of the outer tank wall 4 closed, and the lower end of the inner tank wall 2 and the lower end of the outer tank wall 4 closed, so that no fluid flows into the vacuum insulation tank 14 from the outside, a vacuum state is maintained, and heat transfer between the cooling medium filled in the cooling medium filled tank 13 and the outside air is unlikely to occur.
[0098] The cooling medium tank 13 has a cooling medium supply pipe 15 extending from the outside into the cooling medium tank 13, and is configured so that the cooling medium N is supplied into the cooling medium tank 13, and has a cooling medium introduction pipe 16 that introduces the cooling medium gas vaporized from the cooling medium N in the cooling medium tank 13 into the freezing tank 12, and is configured so that the cooling medium gas is introduced into the freezing tank 12.
[0099] The frozen body P formed in the freeze granulation tank 8 is stored in the drying section 6 which is detachably provided to the freeze granulation tank 8. After a predetermined amount of frozen body P is stored in the drying section 6, the drying section 6 is separated from the freeze granulation tank 8 and sealed, and then freeze-drying is performed to obtain cellulose particles. The configuration of the dryer 100 according to this embodiment will be described below.
[0100] The dryer 100 has a drying section 6 and a vacuum mechanism. The drying section 6 can have a cylindrical wall with an axis in the vertical direction and a bottom continuous with the wall. The cylindrical wall can be provided with an openable and closable exhaust section (not shown), and the gas in the drying section 6 can be exhausted from the exhaust section as exhaust gas D. The upper edge of the cylindrical wall is a flange section 4a, which is detachably connected to the lower edge of the freeze granulation tank 8. After the frozen body P generated in the freeze granulation tank 8 falls into the drying section 6, the drying section 6 is removed from the freeze granulation tank 8, and the flange section 4a is covered with a top lid and sealed to freeze-dry the frozen body P.
[0101] The drying process of the frozen body P can be performed as follows. The drying section 6 is configured so that the base end of a gas pipe 21 for vacuum drawing can be connected, and the gas sucked into the gas pipe 21 is led to a cold trap 22 connected to the tip of the gas pipe 21, where a part of the gas is concentrated and separated as a concentrated liquid or concentrated solid, and the remaining gas is sucked by a vacuum pump 24 provided at the other end of a gas pipe 23 connected to the cold trap 22. When the vacuum pump 24 is started with the drying section 6 sealed, the air pressure inside the drying section 6 decreases, and the sublimable or vaporizable substance contained in the frozen body P (for example, water when the raw material M is a dispersion liquid consisting of water and fine fibrous cellulose) sublimes or vaporizes and is sucked into the vacuum pump 24, and the remainder becomes cellulose particles. In the process of drying, it is preferable to rock or vibrate the drying section 6 so that the frozen bodies P do not aggregate with each other and to dry each frozen body P evenly. The vibration or rocking of the drying section 6 may be performed manually, or a vibration mechanism or a rocking mechanism may be provided. When vibrating, for example, both ends of the diameter of the flange portion formed in a substantially circular shape (parts indicated by symbols 4a and 4a in FIG. 1) can be grasped and swung left and right, and when rocking, for example, the diameter can be used as the axis of rotation to rotate alternately clockwise and counterclockwise. The pivot angle to the right or left is not particularly limited, but a value of 30° to 100° is sufficient to rock the frozen body P in the drying section 6. In the drying process, rocking or vibration is not essential, and the frozen body P may be vacuum-dried while stationary. Although this cannot be said in general, rocking or vibration during drying may result in a relatively higher bulk density of the cellulose particles produced.
[0102] A dryer 200 according to another embodiment will be described with reference to Figs. 9 and 10. The difference from the dryer 100 in Fig. 1 described above is that a shaft core 30 for rocking the drying section 6 is provided. By providing a rocking mechanism on the shaft core 30, the drying section 6 can be configured to rotate, for example, 100° clockwise or counterclockwise on the paper surface of Fig. 10 around the shaft core 30.
[0103] Cellulose particles 11, 12 produced by the above-mentioned production method are shown in Figs. 2 to 5. The cellulose particles 11 shown in Figs. 2 and 3 were produced by using a spray-type freeze granulation apparatus 1 using a 2% by mass aqueous dispersion of unmodified fine fibrous cellulose (ELLEX (registered trademark)-S) as a raw material. Numerous pores 11a were confirmed in the cellulose particles 11. The cellulose particles 11 shown in Figs. 4 and 5 were produced by using a spray-type freeze granulation apparatus 1 using a 2% by mass aqueous dispersion of modified fine fibrous cellulose (ELLEX (registered trademark)-Star) as a raw material. Numerous pores 12a were confirmed in the cellulose particles 12. The drying process was carried out by placing the particles in a vacuum dryer ("EYELA FDU-2110" manufactured by Tokyo Rikakikai Co., Ltd.) and vacuum drying while the particles were left stationary. An example of the freeze granulation tank 8 is "Freeze Granulation Chamber CS30" manufactured by Priss Co., Ltd., and an example of the dryer 200 is "TFD-10" manufactured by Priss Co., Ltd. EXAMPLES
[0104] (Adjustment of Test Examples and Comparative Examples) <Test Example 1> Examples are shown below. Test Example 1 was produced as follows. A dispersion liquid in which unmodified fine fibrous cellulose ("ELLEX (registered trademark)-S" manufactured by Daio Paper Co., Ltd.) was dispersed in water to a concentration of 2% by mass was supplied to a spray-type freeze granulation device as a raw material to obtain cellulose particles, which were used as Test Example 1. The average fiber diameter of the fine fibrous cellulose was 50 nm. The raw material was sprayed into the spray-type freeze granulation device and frozen to obtain a frozen body as an intermediate, and this frozen body was vacuum-dried to obtain cellulose particles. The fine fibrous cellulose was frozen using Priss's "Freeze Granulation Chamber CS30", and after obtaining the frozen body, the frozen body was dried while being shaken using Priss's barrel freeze drying unit "TFD-10" until the frozen body was completely dried.
[0105] <Test Example 2> Test Example 2 was produced as follows. Using the same dispersion liquid as that used in Test Example 1 as a raw material, fine fibrous cellulose was supplied to a Priss "Freeze Granulation Chamber CS30" to obtain a frozen body as an intermediate, and this frozen body was vacuum dried to obtain cellulose particles, which was used as Test Example 2. In order to dry the frozen body while it was left stationary, the frozen body was placed in a vacuum dryer (Tokyo Rikakikai Co., Ltd. "EYELA FDU-2110") and vacuum dried while it was left stationary.
[0106] <Test Example 3> Test Example 3 was produced as follows. A mixture was obtained by mixing the same unmodified fine fibrous cellulose ("ELLEX (registered trademark)-S" manufactured by Daio Paper Co., Ltd.) as the fine fibrous cellulose used in Test Example 1 with a citric acid ester in a mixing ratio of 75%:25%. This mixture was dispersed in water to a concentration of 2% by mass, and the resulting dispersion was used as a raw material for freezing using a Priss Co., Ltd. "Freeze Granulation Chamber CS30". After obtaining a frozen body, the frozen body was dried while being shaken using a Priss Co., Ltd. barrel freeze drying unit "TFD-10" manufactured by Priss Co., Ltd. until the frozen body was completely dried. The cellulose particles obtained after drying were used as Test Example 3.
[0107] <Test Example 4> Test Example 4 was produced as follows. Fine fibrous cellulose in which hydroxyl groups have been modified to phosphite groups (product "ELLEX (registered trademark)-Star" manufactured by Daio Paper Co., Ltd.) was dispersed in water to a concentration of 0.5% by mass, and the dispersion was frozen using Priss's "Freeze Granulation Chamber CS30" to obtain a frozen body. The frozen body was then dried while being shaken using Priss's barrel freeze drying unit "TFD-10" until the frozen body was completely dried. The cellulose particles obtained after drying were used as Test Example 4. The average fiber diameter of the fine fibrous cellulose was 4 nm.
[0108] <Test Example 5> Test Example 5 was produced as follows: the same dispersion liquid as that used in Test Example 4 was supplied as a raw material to a "freeze granulation chamber CS30" manufactured by Priss to obtain a frozen body as an intermediate, and this frozen body was vacuum dried to obtain cellulose particles, which was used as Test Example 5. In order to dry the frozen body while it was left stationary, the frozen body was placed in a vacuum dryer ("EYELA FDU-2110" manufactured by Tokyo Rikakikai Co., Ltd.) and vacuum dried while it was left stationary.
[0109] <Comparative Example 1> In Comparative Example 1, unmodified fine fibrous cellulose (ELLEX (registered trademark)-S, a product manufactured by Daio Paper Co., Ltd.) and glycerin (glycerin, Fujifilm Wako Pure Chemical Industries, Ltd.) were mixed in a mixing ratio of 71%:29% to obtain a mixture, which was then fed into a drum dryer and dried by heat drying to obtain a dried product which was then pulverized to obtain cellulose particles with an average particle size of 53.1 μm, which was designated Comparative Example 1. An SEM image of the particles of Comparative Example 1 is shown in FIG. 8. Compared to the cellulose particles of this embodiment, the particles of Comparative Example 1 have a solid interior, a small specific surface area, and a high density.
[0110] <Comparative Example 2> Comparative Example 2 is a cellulose granule produced by the same production method as Comparative Example 1, except that the cellulose granules had an average particle size of 238.8 μm.
[0111] <Comparative Example 3> Comparative Example 3 was produced as follows. Comparative Example 3 was an aqueous dispersion of unmodified fine fibrous cellulose (ELLEX (registered trademark)-S, a product manufactured by Daio Paper Co., Ltd.) adjusted to a concentration of 2 mass %.
[0112] <Comparative Example 4> Comparative Example 4 was produced as follows. An aqueous dispersion of fine fibrous cellulose (ELLEX (registered trademark)-Star, a product of Daio Paper Corporation) in which hydroxyl groups had been modified to phosphite groups was adjusted to a concentration of 0.5% by mass, and used as Comparative Example 4. (Comparative Examples 3 and 4 are aqueous dispersions of fine fibrous cellulose before processing into cellulose particles.)
[0113] The physical properties of the test examples and comparative examples were measured, including the degree of compression, loose bulk density, packed bulk density, specific surface area, moisture content, average particle size, median size, cumulative 10% size, and cumulative 90% size.
[0114] Compressibility is one of the items used to calculate Carr's fluidity index, and was measured in accordance with ASTM D6393-99 Compressibility Measurement Method. The measurement was performed using a multi-function powder property measuring instrument, Multitester MT-02 (manufactured by Seishin Enterprise Co., Ltd.). The specific surface area was measured according to the BET multipoint method (N2 gas adsorption method). The instruments used for the measurement were "3Flex" (Micromeritics) and "Smart VacPrep (pretreatment device)" (Micromeritics). The cellulose particles prepared in the test examples and comparative examples were degassed (dried under reduced pressure) in the pretreatment device at 60°C for 20 hours, and then the specific surface area was measured by the N2 gas adsorption method. The equipment used to measure the average particle size, median size, cumulative 10% size, and cumulative 90% size was a "laser diffraction / scattering type particle size distribution measuring device (particle size distribution) LA-960V2 (dry measurement)" (manufactured by HORIBA).
[0115] The blending ratios of the raw materials for the test examples and comparative examples are shown in Table 1, and the physical properties are shown in Table 2.
[0116] [Table 1]
[0117] [Table 2]
[0118] (Viscosity test, etc.) The cellulose particles prepared in each of the test examples and comparative examples were added to water to the concentration (redispersion concentration) shown in Table 3, and dispersed in a homogenizer at 8000 rpm for 1 minute to obtain a redispersion liquid. The homogenizer used was a "T-25" manufactured by IKA.
[0119] The B-type viscosity of each redispersion liquid was measured twice under different measurement conditions. The first measurement was for a B-type viscosity at a water temperature of 25°C and 6 rpm, and the second measurement was for a B-type viscosity at a water temperature of 25°C and 60 rpm. The Ti value was calculated as follows: Ti value = (B-type viscosity measured under measurement conditions of 25°C and 6 rpm) / (B-type viscosity measured under measurement conditions of 25°C and 60 rpm)
[0120] The viscosity change rate (6 rpm) was calculated using [Formula 2], and the viscosity change rate (60 rpm) was calculated using [Formula 3]. [Formula 2] 1. Test Examples 1 to 3 and Comparative Examples 1 and 2 (Viscosity change rate (6 rpm)) = (B-type viscosity of X (6 rpm)) / (B-type viscosity of Comparative Example 3 (6 rpm)) × 100 Here, X is any one of Test Example 1, Test Example 2, Test Example 3, Comparative Example 1, and Comparative Example 2. 2. Test Examples 4 and 5 (Viscosity change rate (6 rpm)) = (B-type viscosity of Y (6 rpm)) / (B-type viscosity of Comparative Example 4 (6 rpm)) × 100 Here, Y is Test Example 4 or Test Example 5.
[0121] [Formula 3] 1. Test Examples 1 to 3 and Comparative Examples 1 and 2 (Viscosity change rate (60 rpm)) = (B-type viscosity of X (60 rpm)) / (B-type viscosity of Comparative Example 3 (60 rpm)) × 100 Here, X is any one of Test Example 1, Test Example 2, Test Example 3, Comparative Example 1, and Comparative Example 2. 2. Test Examples 4 and 5 (Viscosity change rate (60 rpm)) = (B-type viscosity of Y (60 rpm)) / (B-type viscosity of Comparative Example 4 (60 rpm)) × 100 Here, Y is Test Example 4 or Test Example 5.
[0122] The viscosity change rate (average) is the sum of the viscosity change rate (6 rpm) and the viscosity change rate (60 rpm) divided by 2.
[0123] [Table 3]
[0124] Comparing Comparative Example 1 and Comparative Example 2 with Test Examples 1 to 5 for the B-type viscosity (6 rpm), Test Examples 1 to 5 showed higher values. The same tendency was observed for the B-type viscosity (60 rpm). In addition, comparing Comparative Example 1 and Comparative Example 2 with Test Examples 1 to 5 for the Ti value, Test Examples 1 to 5 showed higher values. It can be seen that Test Examples 1 to 5 are excellent in thixotropy.
[0125] The viscosity change rate is a numerical expression of the type B viscosity of cellulose particles produced from fine fibrous cellulose as the starting material, when the type B viscosity of the raw material fine fibrous cellulose is taken as 100%. The closer the viscosity change rate is to 100%, the closer the type B viscosity of the cellulose particles is to the type B viscosity of the raw material fibrous cellulose, and the closer the viscosity change rate is to 0%, the more the type B viscosity of the cellulose particles deviates from the type B viscosity of the raw material fibrous cellulose.
[0126] (Redispersion test) The following redispersion test was carried out: In the relevant drawings, reference numeral 20 denotes an interface.
[0127] For the produced cellulose particles (Test Examples 1 to 5, Comparative Examples 1 and 2), Test Examples 1 to 3 and Comparative Examples 1 and 2 were dispersed in water to a concentration of 2.0% by mass, and Test Examples 4 and 5 were dispersed in water to a concentration of 0.5%. The particles were then dispersed in water at 8000 rpm for 1 minute using a homogenizer (IKA's "T-25") to obtain a redispersion (Comparative Example 3 was an aqueous dispersion of microfibrous cellulose with a concentration of 2.0% by mass, and Comparative Example 4 was an aqueous dispersion of microfibrous cellulose with a concentration of 0.5% by mass, which correspond to the aqueous dispersion before processing into cellulose particles). After dispersion, the particles were transferred to a stoppered bottle and left to stand for 20 minutes, and the dispersed state was photographed as shown in FIG. 7.
[0128] In all of the test examples 1 to 5, the cellulose particles were widely dispersed in the water, and no clear interface between the cellulose particles was observed. The redispersions in the test examples 4 and 5 were highly transparent because the fine fibrous cellulose used had excellent transparency. On the other hand, in the comparative examples 1 and 2, the interface 20 was observed.
[0129] In the case of Test Examples 4 and 5, the particles dispersed in water were transparent. This can be considered as follows. Test Examples 4 and 5 are made of microfibrous cellulose, which is highly hydrophilic and has excellent transparency. When the particles are dispersed in water, water penetrates between the fibers constituting the cellulose particles, and the hydrogen bonds between the fibers are dissociated, resulting in redispersion in the dispersion medium with high dispersibility, which is thought to be why Test Examples 4 and 5 were transparent. In addition, in the case of Comparative Example 3, the particles were less likely to settle when dispersed in water.
[0130] (others) Unless otherwise specified, the JIS, TAPPI and other tests and measurement methods shown in the above specification are performed at room temperature, particularly 25°C, and at atmospheric pressure, particularly 1 atm. [Industrial Applicability]
[0131] The cellulose particles and cellulose particle dispersion of the present invention can be provided as particles having improved redispersibility in aqueous liquids. [Explanation of symbols]
[0132] 11 Cellulose particles 11a Pore of cellulose particles 12 Cellulose particles 12a Pore of cellulose particles 20 Interface
Claims
1. A cellulose particle containing fine fibrous cellulose having an average fiber diameter of 1000 nm or less, The freeze-dried particles have a specific surface area of 30 m 2 / g or more. The axial ratio of the fine fibrous cellulose is 10 to 1,000,000. A cellulose particle characterized by:
2. The pulp viscosity of the fine fibrous cellulose is 1 to 10 cps. The cellulose particles according to claim 1.
3. The crystallinity of the fine fibrous cellulose is 50 or more and 100 or less. The cellulose particles according to claim 1.