AI Technical Summary
Existing polyamide compositions fail to provide high flame retardancy, heat resistance, and moldability, particularly in thin-walled applications, which are essential for electrical and electronic components and automobile parts as they become smaller and thinner.
A polyamide composition containing a semi-aromatic polyamide with a melting point of 280°C or higher, a brominated flame retardant, and an aromatic vinyl copolymer with a glass transition temperature of 140°C or higher, blended in specific proportions, enhances flame retardancy and moldability.
The composition achieves high flame retardancy and excellent heat resistance, enabling the production of thin-walled molded articles with improved mechanical properties and moldability.
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyamide composition and a molded article made of the polyamide composition. [Background technology]
[0002] Polyamides are excellent in mechanical properties, moldability, etc., and are therefore used in a variety of applications, such as electric and electronic parts, automobile parts, machine parts, industrial parts, fibers, films, sheets, etc. In particular, applications to electric and electronic parts require a high level of flame retardancy based on the UL-94 standard, and therefore methods for making polyamide compositions flame-retardant using various flame retardants have been proposed.
[0003] For example, Patent Document 1 proposes a polyamide composition containing a specific polyamide, specific glass fibers, and a brominated flame retardant, and describes that the composition has excellent fluidity and other properties. In addition, Patent Documents 2 and 3 propose flame-retardant polyamide resin compositions containing polyamide having a terminal amino group ratio or terminal carboxyl group ratio within a specific range, brominated polystyrene, and a copolymer of an aromatic vinyl compound and an α,β-unsaturated dicarboxylic acid anhydride, and state that the compositions have excellent flame retardancy, extrusion processability, molding processability, etc. when thin-walled. Patent Document 4 proposes a polyamide composition comprising a polyamide having a melting point in a specific range, a flame retardant, and an anti-dripping agent, in which a fluororesin and at least one polymer selected from the group consisting of an ionomer and a modified aromatic vinyl polymer are used as the anti-dripping agent in a mass ratio within a specific range, and describes that the polyamide composition has excellent flame retardancy, heat resistance, moldability (fluidity), etc., making it suitable as a material for molding electronic components having thin walls. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2003-82228 A [Patent Document 2] JP 2007-291249 A [Patent Document 3] JP 2007-291250 A [Patent Document 4] International Publication No. 2009 / 017043 Summary of the Invention [Problem to be solved by the invention]
[0005] Here, in the case of electric and electronic components, as the size and weight of the product are reduced and the components are made smaller and thinner in their mounting, higher flame retardancy is required in the thin-walled form. In addition, in electric and electronic components that require reflow solder heat resistance due to the recent progress in surface mounting technology (SMT) and in automobile parts and the like that are increasingly required for heat resistance, further improvement in heat resistance and moldability of polyamide compositions is required. However, the techniques of Patent Documents 1 to 3 are not fully satisfactory in terms of high flame retardancy, heat resistance, and moldability in the thin-walled form. In addition, although the technique of Patent Document 4 improves flame retardancy, heat resistance, moldability, etc., further improvement in performance is desired.
[0006] In view of the above circumstances, an object of the present invention is to provide a polyamide composition having high flame retardancy even when thin, and also having excellent heat resistance and moldability, and a molded article made of said polyamide composition. [Means for solving the problem]
[0007] Means for Solving the Problems The present inventors have found that the above-mentioned problems can be solved by a polyamide composition comprising a specific polyamide, a flame retardant, and an aromatic vinyl-based copolymer, wherein the aromatic vinyl-based copolymer contains specific structural units, has a glass transition temperature in a specific range, and contains the aromatic vinyl-based copolymer in a specific ratio. Based on this finding, the inventors have conducted further studies and have completed the present invention. That is, the present invention relates to the following [1] to
[13] . [1] A polyamide composition comprising a polyamide (A) having a melting point of 280°C or higher, a flame retardant (B), and an aromatic vinyl copolymer (C), the aromatic vinyl copolymer (C) contains a structural unit derived from an aromatic vinyl and a structural unit derived from an α,β-unsaturated dicarboxylic acid anhydride, and the glass transition temperature of the aromatic vinyl copolymer (C) is 140° C. or higher; The polyamide composition has a content of the aromatic vinyl copolymer (C) of 0.3 to 2.0 mass % based on the total content of the polyamide (A), the flame retardant (B) and the aromatic vinyl copolymer (C). [2] The polyamide composition according to [1], wherein the polyamide (A) is a semi-aromatic polyamide. [3] The polyamide composition according to [2], wherein, in the semi-aromatic polyamide, more than 50 mol % of the dicarboxylic acid-derived structural units constituting the semi-aromatic polyamide are aromatic dicarboxylic acid-derived structural units, and more than 50 mol % of the diamine-derived structural units constituting the semi-aromatic polyamide are aliphatic diamine-derived structural units having 4 to 18 carbon atoms. [4] The polyamide composition according to [3], wherein the aliphatic diamine is at least one selected from the group consisting of 1,6-hexanediamine, 1,9-nonanediamine, 2-methyl-1,8-octanediamine, and 1,10-decanediamine. [5] The polyamide composition according to any one of [1] to [4], wherein the flame retardant (B) is a brominated flame retardant. [6] The polyamide composition according to any one of [1] to [5], wherein the structural units derived from aromatic vinyl include structural units derived from at least one selected from the group consisting of styrene and α-methylstyrene. [7] The polyamide composition according to any of [1] to [6], wherein the α,β-unsaturated dicarboxylic acid anhydride is at least one selected from the group consisting of maleic anhydride and a monoalkylmaleic anhydride having an alkyl group having 1 to 3 carbon atoms. [8] The polyamide composition according to any one of [1] to [7], wherein the content of structural units derived from an α,β-unsaturated dicarboxylic acid anhydride in the aromatic vinyl copolymer (C) is 18 to 50 mass%. [9] The polyamide composition according to any one of [1] to [8], wherein the aromatic vinyl copolymer (C) has a weight average molecular weight (Mw) of 10,000 to 500,000.
[10] The polyamide composition according to any one of [1] to [9], further comprising a filler (D).
[11] The polyamide composition according to any one of [1] to [9], which is obtained by melt-kneading a polyamide (A), a flame retardant (B), and an aromatic vinyl copolymer (C).
[12] The polyamide composition according to
[10] , wherein the polyamide composition is obtained by melt-kneading a polyamide (A), a flame retardant (B), an aromatic vinyl copolymer (C), and a filler (D).
[13] A molded article comprising any one of the polyamide compositions [1] to
[12] . Effect of the Invention
[0008] According to the present invention, it is possible to provide a polyamide composition having a high degree of flame retardancy even when thin, and also having excellent heat resistance and moldability, and a molded article made of said polyamide composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Polyamide composition] The polyamide composition of the present invention contains a polyamide (A) having a melting point of 280° C. or higher (hereinafter also simply referred to as "polyamide (A)"), a flame retardant (B), and an aromatic vinyl copolymer (C) (hereinafter also referred to as "copolymer (C)"). The copolymer (C) contains structural units derived from aromatic vinyl and structural units derived from α,β-unsaturated dicarboxylic anhydride, the glass transition temperature of the copolymer (C) is 140° C. or higher, and the content of the copolymer (C) is 0.3 to 2.0 mass% based on the total content of the polyamide (A), the flame retardant (B), and the copolymer (C).
[0010] The polyamide composition of the present invention contains a polyamide (A) having a specific melting point, a flame retardant (B), and a specific aromatic vinyl copolymer (C), and contains the aromatic vinyl copolymer in a specific ratio, so that the polyamide composition has high flame retardancy even in a thin wall, and also has excellent heat resistance and moldability. The reason for this is unclear, but is presumed to be as follows. The melting point of the polyamide (A) according to the present invention is 280°C or higher, and the glass transition temperature of the copolymer (C) is 140°C or higher, so that the heat resistance is improved. In addition, it is believed that the α,β-unsaturated dicarboxylic anhydride unit in the copolymer (C) reacts with the carboxyl group terminal or amino group terminal of the polyamide (A), thereby increasing the viscosity of the polyamide composition, improving the melt tension, and suppressing dripping. Furthermore, the amount of carboxyl group terminals is reduced by the reaction, so that the decomposition of the polyamide (A) at high temperatures is also suppressed. As a result, it is believed that the flame retardancy of the thin wall can be improved. In addition, it is believed that by setting the content of the copolymer (C) in the polyamide composition at a specific ratio, the viscosity of the polyamide composition does not become too high, and both high flame retardancy and excellent moldability of the thin wall can be achieved.
[0011] <Polyamide (A)> The polyamide composition of the present invention contains a polyamide (A) having a melting point of 280° C. or higher. Examples of the polyamide (A) include condensation polymers of dicarboxylic acids and diamines, ring-opening polymers of cyclic lactams, and condensation polymers of aminocarboxylic acids. In this specification, the term "unit" (where "" indicates a monomer) means "a structural unit derived from", for example, a "dicarboxylic acid unit" means "a structural unit derived from a dicarboxylic acid", and a "diamine unit" means "a structural unit derived from a diamine".
[0012] Examples of the dicarboxylic acid include aliphatic dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, dimethylmalonic acid, 2,2-diethylsuccinic acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid; 1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, cycloheptanedicarboxylic acid, and cyclohexanedicarboxylic acid; and aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,4-phenylenedioxydiacetic acid, 1,3-phenylenedioxydiacetic acid, diphenic acid, diphenylmethane-4,4'-dicarboxylic acid, diphenylsulfone-4,4'-dicarboxylic acid, and 4,4'-biphenyldicarboxylic acid. These dicarboxylic acids can be used alone or in combination of two or more. The polyamide (A) may further contain structural units derived from a polyvalent carboxylic acid having three or more valences, such as trimellitic acid, trimesic acid, or pyromellitic acid, to the extent that melt molding is possible, as long as the effects of the present invention are not impaired.
[0013] The diamines include aliphatic diamines, alicyclic diamines, aromatic diamines, etc. Examples of the aliphatic diamines include linear aliphatic diamines such as ethylenediamine, 1,2-propanediamine, 1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, and 1,12-dodecanediamine; 1-butyl-1,2-ethanediamine, 1,1-dimethyl-1,4-butanediamine, 1-ethylenediamine, 1,2-ethylenediamine, 1,3-ethylenediamine, 1,4-ethylenediamine, 1,5-ethylenediamine, 1,6-ethylenediamine, 1,7-ethylenediamine, 1,8-ethylenediamine, 1,9-ethylenediamine, 1,10-ethylenediamine, 1,11-ethylenediamine, 1,12-ethylenediamine, 1,11-ethylenediamine, 1,2 ...3-ethylenediamine, 1,4-ethylenediamine, 1,5-ethylenediamine, 1,6-ethylenediamine, 1,7-ethylenediamine, 1,8-ethylenediamine, 1,9-ethylenediamine, 1,2-dimethyl-1,4-butanediamine, 1,3-dimethyl-1,4-butanediamine, 1,4-dimethyl-1,4-butanediamine, 2,3-dimethyl-1,4-butanediamine, 2-methyl-1,5-pentanediamine, 3-methyl-1,5-pentanediamine, 2,5-dimethyl-1,6-hexanediamine, 2,4-dimethyl-1,6-hexanediamine, 3,3-dimethyl-1,6-hexanediamine, 2,2-dimethyl-1,6-hexa hexanediamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 2,4-diethyl-1,6-hexanediamine, 2,2-dimethyl-1,7-heptanediamine, 2,3-dimethyl-1,7-heptanediamine, 2,4-dimethyl-1,7-heptanediamine, 2,5-dimethyl-1,7-heptanediamine, 2-methyl-1,8-octanediamine, 3-methyl-1,8-octanediamine, 4-methyl-1,8-octanediamine Examples of branched chain aliphatic diamines include amines, 1,3-dimethyl-1,8-octanediamine, 1,4-dimethyl-1,8-octanediamine, 2,4-dimethyl-1,8-octanediamine, 3,4-dimethyl-1,8-octanediamine, 4,5-dimethyl-1,8-octanediamine, 2,2-dimethyl-1,8-octanediamine, 3,3-dimethyl-1,8-octanediamine, 4,4-dimethyl-1,8-octanediamine, and 5-methyl-1,9-nonanediamine.
[0014] Examples of the alicyclic diamine include cyclohexane diamine, methylcyclohexane diamine, isophorone diamine, norbornane dimethylamine, and tricyclodecane dimethylamine. Examples of the aromatic diamine include p-phenylenediamine, m-phenylenediamine, p-xylylenediamine, m-xylylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, and 4,4'-diaminodiphenyl ether. These diamines can be used alone or in combination of two or more. The polyamide (A) may further contain structural units derived from a polyvalent amine having three or more valences, such as bis(hexamethylene)triamine, to the extent that melt molding is possible, provided that the effects of the present invention are not impaired.
[0015] Examples of the cyclic lactams include acetolactam, propiolactam, butyrolactam, valerolactam, caprolactam, enantholactam, caprylolactam, pelargolactam, caprinolactam, and laurolactam. Examples of the aminocarboxylic acid include aminopropionic acid, aminobutyric acid, aminovaleric acid, aminocaproic acid, aminoenanthic acid, aminocaprylic acid, aminopelargonic acid, aminocapric acid, and aminolauric acid.
[0016] The polyamide (A) is preferably an aliphatic polyamide, a wholly aromatic polyamide, or a semi-aromatic polyamide, which is prepared by appropriately combining monomers such as the above-mentioned dicarboxylic acids, diamines, cyclic lactams, aminocarboxylic acids, trivalent or higher polyvalent carboxylic acids, and trivalent or higher polyvalent amines so that the melting point is 280°C or higher. In the present invention, the term "wholly aromatic polyamide" refers to a polyamide in which more than 50 mol % of the dicarboxylic acid units constituting the polyamide are aromatic dicarboxylic acid units and more than 50 mol % of the diamine units constituting the polyamide are aromatic diamine units. In the present invention, the term "semi-aromatic polyamide" refers to a polyamide in which more than 50 mol % of the dicarboxylic acid units constituting the polyamide are aromatic dicarboxylic acid units and more than 50 mol % of the diamine units constituting the polyamide are aliphatic diamine units, or a polyamide in which more than 50 mol % of the dicarboxylic acid units constituting the polyamide are aliphatic dicarboxylic acid units and more than 50 mol % of the diamine units constituting the polyamide are aromatic diamine units. Among these, from the viewpoints of flame retardancy, heat resistance and moldability in a thin wall, at least one selected from the group consisting of aliphatic polyamides and semi-aromatic polyamides is preferred, and semi-aromatic polyamides are more preferred.
[0017] Examples of the aliphatic polyamide include a ring-opening polymer of the cyclic lactam, a condensation polymer of the aminocarboxylic acid, or a condensation polymer of the aliphatic dicarboxylic acid and the aliphatic diamine. Among these, from the viewpoints of flame retardancy, heat resistance, and moldability in a thin wall, the condensation polymer of the aliphatic dicarboxylic acid and the aliphatic diamine is preferred, and from the viewpoint of ease of production, polyamide 46 is more preferred.
[0018] From the viewpoints of flame retardancy, heat resistance and moldability in a thin film, the semi-aromatic polyamide is preferably one in which more than 50 mol % of the dicarboxylic acid units constituting the semi-aromatic polyamide are aromatic dicarboxylic acid units and more than 50 mol % of the diamine units constituting the semi-aromatic polyamide are aliphatic diamine units.
[0019] The aromatic dicarboxylic acid constituting the semi-aromatic polyamide may be the aromatic dicarboxylic acid mentioned above. Among them, phthalic acid, isophthalic acid, and terephthalic acid are preferred, isophthalic acid and terephthalic acid are more preferred, and terephthalic acid is even more preferred. The content of aromatic dicarboxylic acid units in all dicarboxylic acid units constituting the semi-aromatic polyamide is preferably 60 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and even more preferably 90 mol% or more, and 100 mol% or less, from the viewpoint of heat resistance. The semi-aromatic polyamide may contain other dicarboxylic acid units other than the aromatic dicarboxylic acid units. Examples of such other dicarboxylic acids include the above-mentioned aliphatic dicarboxylic acids and alicyclic dicarboxylic acids. The content of other dicarboxylic acid units in the total dicarboxylic acid units constituting the semi-aromatic polyamide is preferably 40 mol% or less, more preferably 30 mol% or less, even more preferably 20 mol% or less, and even more preferably 10 mol% or less.
[0020] The aliphatic diamine constituting the semi-aromatic polyamide may be the aliphatic diamine described above. The carbon number of the aliphatic diamine is preferably 4 or more, more preferably 6 or more, and even more preferably 8 or more, from the viewpoint of excellent physical properties such as heat resistance and low water absorption, and is preferably 18 or less, more preferably 12 or less. As the aliphatic diamine, from the viewpoint of excellent physical properties such as heat resistance and low water absorption, at least one selected from the group consisting of 1,6-hexanediamine, 1,9-nonanediamine, 2-methyl-1,8-octanediamine, and 1,10-decanediamine is preferable, at least one selected from the group consisting of 1,9-nonanediamine and 2-methyl-1,8-octanediamine is more preferable, and a combination of 1,9-nonanediamine and 2-methyl-1,8-octanediamine is even more preferable. The content of aliphatic diamine units in all diamine units constituting the semi-aromatic polyamide is preferably 60 mol % or more, more preferably 70 mol % or more, even more preferably 80 mol % or more, and even more preferably 90 mol % or more, and 100 mol % or less. The semi-aromatic polyamide may contain other diamine units other than the aliphatic diamine units. Examples of such other diamines include the above-mentioned aromatic diamines and alicyclic diamines. The content of the other diamine units in the total diamine units constituting the semi-aromatic polyamide is preferably 40 mol% or less, more preferably 30 mol% or less, even more preferably 20 mol% or less, and even more preferably 10 mol% or less.
[0021] When 1,9-nonanediamine and 2-methyl-1,8-octanediamine are used in combination as the aliphatic diamine, from the viewpoint of heat resistance, the molar ratio of 1,9-nonanediamine to 2-methyl-1,8-octanediamine (1,9-nonanediamine / 2-methyl-1,8-octanediamine) is preferably in the range of 95 / 5 to 40 / 60, more preferably in the range of 90 / 10 to 50 / 50, and even more preferably in the range of 90 / 10 to 60 / 40.
[0022] The semi-aromatic polyamide may contain structural units derived from cyclic lactams and / or aminocarboxylic acids. Examples of such structural units include structural units derived from cyclic lactams such as caprolactam and laurolactam; and aminocarboxylic acids such as 11-aminoundecanoic acid and 12-aminododecanoic acid. The total content of cyclic lactam units and aminocarboxylic acid units in the semi-aromatic polyamide is preferably 40 mol% or less, more preferably 20 mol% or less, based on 100 mol% of the total of dicarboxylic acid units and diamine units constituting the semi-aromatic polyamide.
[0023] Specific examples of the semi-aromatic polyamide include polytetramethylene terephthalamide (polyamide 4T), polyhexamethylene terephthalamide (polyamide 6T), polynonamethylene terephthalamide (polyamide 9T), polydecamethylene terephthalamide (polyamide 10T), polyhexamethylene isophthalamide (polyamide 6I), a copolymer of polyamide 6I and polyamide 6T (polyamide 6I / 6T), and a copolymer of polyamide 6T and polyundecane amide (polyamide 11) (polyamide 6T / 11). Among them, at least one selected from the group consisting of polyamide 4T, polyamide 6T, polyamide 9T, and polyamide 10T is preferred, at least one selected from the group consisting of polyamide 9T and polyamide 10T is more preferred, and polyamide 9T is even more preferred.
[0024] The polyamide (A) used in the present invention has preferably 10% or more of the terminal groups of its molecular chain capped with a terminal capping agent, and more preferably the proportion of the terminal groups of the molecular chain capped with the terminal capping agent (terminal capping rate) is 20% or more. As the end-capping agent, a monofunctional compound having reactivity with the amino group or carboxyl group at the polyamide end can be used, and from the viewpoints of reactivity and stability of the blocked end, a monocarboxylic acid or a monoamine is preferred, and from the viewpoints of ease of handling, a monocarboxylic acid is more preferred. In addition, monoisocyanates, monoacid halides, monoesters, monoalcohols, etc. can also be used as the end-capping agent.
[0025] As the monocarboxylic acid used as the terminal blocking agent, those having reactivity with amino groups can be used, and examples thereof include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclohexane carboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, α-naphthalene carboxylic acid, β-naphthalene carboxylic acid, methylnaphthalene carboxylic acid, and phenyl acetic acid; and any mixtures thereof. Among these, from the viewpoints of reactivity, stability of blocked terminals, cost, and the like, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, and benzoic acid are preferred.
[0026] The monoamine used as the terminal blocking agent may be one having reactivity with a carboxyl group, and examples of such monoamines include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; aromatic monoamines such as aniline, toluidine, diphenylamine, and naphthylamine; and any mixtures thereof. Among these, butylamine, hexylamine, octylamine, decylamine, stearylamine, cyclohexylamine, and aniline are preferred from the viewpoints of reactivity, boiling point, stability of blocked terminals, and cost.
[0027] The terminal capping rate of polyamide (A) is calculated by measuring the number of carboxyl terminals, amino terminals, and terminal groups capped with a terminal capping agent present in polyamide (A) and then calculating the terminal capping rate according to the following formula (1). From the viewpoints of accuracy and simplicity, the number of each terminal group is calculated as follows: 1 It is preferable to determine it from the integral value of the characteristic signal corresponding to each terminal group by 1 H-NMR. End sealing rate (%)=[(TS) / T]×100 (1) [In the formula, T represents the total number of terminal groups in the molecular chain of polyamide (A) (which is usually equal to twice the number of polyamide molecules), and S represents the total number of carboxyl terminals and amino terminals remaining uncapped.]
[0028] The polyamide (A) used in the present invention can be produced by any method known as a method for producing crystalline polyamides. For example, it can be produced by a solution polymerization method or an interfacial polymerization method using dicarboxylic acid and diamine in the form of acid chloride as raw materials, a melt polymerization method, a solid-state polymerization method, a melt extrusion polymerization method, etc. using dicarboxylic acid and diamine as raw materials.
[0029] The polyamide (A) can be produced, for example, by first adding diamine, dicarboxylic acid, and if necessary, a catalyst and an end-capping agent all at once to produce a nylon salt, then heating and polymerizing the prepolymer at a temperature of 200 to 250°C, and further solid-phase polymerizing the prepolymer, or polymerizing the prepolymer using a melt extruder. When the final stage of the polymerization is carried out by solid-phase polymerization, it is preferable to carry out the polymerization under reduced pressure or in an inert gas flow. If the polymerization temperature is within the range of 200 to 280°C, the polymerization rate is high, productivity is excellent, and coloring and gelation can be effectively suppressed. When the final stage of the polymerization is carried out using a melt extruder, the polymerization temperature is preferably 370°C or less, and when polymerization is carried out under such conditions, polyamide (A) with little decomposition and little deterioration can be obtained.
[0030] Examples of catalysts that can be used in producing polyamide (A) include phosphoric acid, phosphorous acid, hypophosphorous acid, and salts or esters thereof. Examples of the above salts or esters include salts of phosphoric acid, phosphorous acid, or hypophosphorous acid with metals such as potassium, sodium, magnesium, vanadium, calcium, zinc, cobalt, manganese, tin, tungsten, germanium, titanium, and antimony; ammonium salts of phosphoric acid, phosphorous acid, or hypophosphorous acid; ethyl esters, isopropyl esters, butyl esters, hexyl esters, isodecyl esters, octadecyl esters, decyl esters, stearyl esters, and phenyl esters of phosphoric acid, phosphorous acid, or hypophosphorous acid. Among these, sodium hypophosphite monohydrate or phosphorous acid is preferred.
[0031] The polyamide (A) has an intrinsic viscosity [η] of preferably 0.60 to 1.2 dl / g, more preferably 0.65 to 1.1 dl / g, measured at 30° C. using concentrated sulfuric acid as a solvent. If a polyamide (A) having an intrinsic viscosity [η] of 0.60 dl / g or more is used, the mechanical properties of the molded product obtained will be good. If a polyamide (A) having an intrinsic viscosity [η] of 1.2 dl / g or less is used, the moldability will be further improved. The intrinsic viscosity [η] of the polyamide (A) is measured by the method described in the Examples.
[0032] The melting point of the polyamide (A) is 280°C or higher, preferably 290°C or higher, and more preferably 300°C or higher, from the viewpoint of heat resistance and in order to more significantly exhibit the effects of the present invention, and is preferably 350°C or lower, more preferably 340°C or lower, and even more preferably 330°C or lower, from the viewpoint of suppressing thermal decomposition of the polyamide during melt molding. The melting point of the polyamide (A) is measured by the method described in the Examples.
[0033] <Flame retardant (B)> The polyamide composition of the present invention contains a flame retardant (B). Examples of the flame retardant (B) include phosphorus-based flame retardants; and halogen-based flame retardants such as bromine-based flame retardants and chlorine-based flame retardants. Examples of phosphorus-based flame retardants include red phosphorus; aliphatic phosphoric acid esters such as trimethyl phosphate and triethyl phosphate; aromatic phosphoric acid esters such as triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, cresyl di-2,6-xylenyl phosphate, tris(t-butylated phenyl) phosphate, tris(i-propylated phenyl) phosphate, and 2-ethylhexyl diphenyl phosphate; tris(dichloropropyl) phosphate, tris(β-chloropropyl) phosphate, tris(chloroethyl) phosphate, Examples of such phosphate esters include halogen-containing phosphate esters such as tris(tribromoneopentyl)phosphate; aromatic condensed phosphate esters such as 1,3-phenylene bis(diphenyl phosphate), 1,3-phenylene bis(dixylenyl)phosphate, and bisphenol A bis(diphenyl phosphate); halogen-containing condensed phosphate esters such as 2,2-bis(chloromethyl)trimethylene bis(bis(2-chloroethyl)phosphate) and polyoxyalkylene bisdichloroalkyl phosphate; phosphoric acid amides; phosphate salts such as ammonium polyphosphate and melamine polyphosphate; and phosphazene compounds.
[0034] Examples of chlorine-based flame retardants include chlorinated paraffin, chlorinated polyethylene, dodecachloropentacyclooctadeca-7,15-diene (manufactured by Occidental Chemical Company, trade name "Dechlorane Plus 25"), and HET anhydride. Examples of brominated flame retardants include brominated polystyrene (which may be polybrominated styrene); brominated polyphenylene oxide; brominated bisphenol-type epoxy polymers; brominated styrene-maleic anhydride polymers; brominated epoxy resins; brominated phenoxy resins; brominated polybenzyl (meth)acrylates such as polypentabromobenzyl acrylate; bromine-containing polycyclic compounds such as bis(pentabromophenyl)ethane, 1,2-bis(2,4,6-tribromophenoxy)ethane, 2,4,6-tris(2,4,6-tribromophenoxy)-1,3,5-triazine, 2,6-dibromophenol, 2,4-dibromophenol, and polybromophenylindane; tetrabromobisphenol A, tetrabromobisphenol A-bis(dibromopropyl ether), tetrabromobisphenol A-bis(aryl ... Examples of the flame retardant include tetrabromobisphenol A and its derivatives such as sphenol A polycarbonate and tetrabromobisphenol A epoxy oligomer; tetrabromobisphenol S and its derivatives such as tetrabromobisphenol S and tetrabromobisphenol S-bis(dibromopropyl ether); polybrominated diphenyl ethers such as decabromodiphenyl ether and octabromodiphenyl ether; polybrominated biphenyls such as decabromobiphenyl; brominated polycarbonates; bromine-containing cyclic aliphatic compounds such as hexabromocyclododecane; brominated crosslinked aromatic polymers; bromine-containing phthalic acid compounds such as tetrabromophthalic anhydride and N,N-ethylenebis(tetrabromophthalic)imide; bromine-containing isocyanuric acid compounds such as tris(pentabromobenzyl)isocyanurate and tris(dibromopropyl)isocyanurate. These flame retardants can be used alone or in combination of two or more. The content of bromine atoms in the brominated flame retardant is preferably 15 to 87 mass %.
[0035] From the viewpoints of flame retardancy, heat resistance and moldability in a thin wall, the flame retardant (B) is preferably at least one selected from the group consisting of phosphorus-based flame retardants and bromine-based flame retardants, and more preferably a bromine-based flame retardant. The brominated flame retardant is preferably at least one selected from the group consisting of brominated polystyrene, brominated polyphenylene oxide, brominated epoxy resin, brominated polybenzyl (meth)acrylate, bromine-containing polycyclic compounds, tetrabromobisphenol A and its derivatives, tetrabromobisphenol S and its derivatives, polybrominated diphenyl ether, bromine-containing cyclic aliphatic compounds, bromine-containing phthalic acid compounds, and bromine-containing isocyanuric acid compounds. Examples of the brominated flame retardant include brominated polystyrene, brominated polyphenylene oxide, brominated epoxy resin, polypentabromobenzyl acrylate, bis( At least one selected from the group consisting of pentabromophenyl)ethane, 2,4,6-tris(2,4,6-tribromophenoxy)-1,3,5-triazine, polybromophenylindane, tetrabromobisphenol A-bis(dibromopropyl ether), tetrabromobisphenol A polycarbonate, tetrabromobisphenol S-bis(dibromopropyl ether), decabromodiphenyl ether, hexabromocyclododecane, N,N-ethylenebis(tetrabromophthalic)imide, and tris(dibromopropyl)isocyanurate is more preferred. Among them, from the viewpoint of being able to withstand molding at high temperatures, at least one selected from the group consisting of brominated polystyrene, brominated epoxy resin, and N,N-ethylenebis(tetrabromophthalic)imide is more preferred, and brominated polystyrene is even more preferred. The method for producing brominated polystyrene is not particularly limited. For example, the brominated polystyrene can be produced by a method in which styrene is polymerized to produce polystyrene and then the benzene ring of the polystyrene is brominated, or by a method in which brominated styrene (bromostyrene, dibromostyrene, tribromostyrene, etc.) is polymerized. The content of bromine atoms in the brominated polystyrene is preferably 55 to 75% by mass. When the content of bromine atoms is 55% by mass or more, the content of brominated polystyrene required for satisfying the amount of bromine required for flame retardancy can be reduced, and high flame retardancy can be imparted to a thin wall without reducing mechanical properties and heat resistance. When the content of bromine atoms is 75% by mass or less, the decrease in thermal stability of the brominated polystyrene and thermal decomposition during melt molding can be reduced, and gas generation and discoloration due to heat can be suppressed.
[0036] <Flame retardant synergist> The polyamide composition of the present invention preferably contains a flame retardant assistant in addition to the bromine-based flame retardant from the viewpoint of imparting excellent flame retardancy in a thin wall with a small amount of flame retardant. Examples of the flame retardant assistant include antimony trioxide, antimony pentoxide, sodium antimonate, sodium oxide, tin oxide, zinc stannate, zinc oxide, iron oxide, magnesium hydroxide, calcium hydroxide, zinc borate, kaolin clay, and calcium carbonate. These flame retardant assistants may be used alone or in combination of two or more. These flame retardant assistants may be treated with a silane coupling agent, a titanium coupling agent, or the like. Among them, zinc borate and zinc stannate are preferred, and zinc stannate is more preferred.
[0037] <Aromatic vinyl copolymer (C)> The polyamide composition of the present invention contains an aromatic vinyl copolymer (C) (copolymer (C)). Here, the copolymer (C) contains an aromatic vinyl unit and an α,β-unsaturated dicarboxylic anhydride unit, and the glass transition temperature of the copolymer (C) is 140° C. or higher. Such aromatic vinyl is a compound having an aromatic ring and a vinyl group, and examples thereof include styrene, 2-methylstyrene, α-methylstyrene, p-methylstyrene, etc. Among these, styrene and α-methylstyrene are preferred, and styrene is more preferred. Examples of the α,β-unsaturated dicarboxylic acid anhydride include maleic anhydride, monoalkyl maleic anhydride having an alkyl group with 1 to 3 carbon atoms, and dialkyl maleic anhydride having an alkyl group with 1 to 3 carbon atoms. Among these, at least one selected from the group consisting of maleic anhydride and monoalkyl maleic anhydride is preferred, at least one selected from the group consisting of maleic anhydride and citraconic anhydride is more preferred, and maleic anhydride is even more preferred.
[0038] The content of α,β-unsaturated dicarboxylic anhydride units in the copolymer (C) is preferably 18 to 50% by mass. When the content of α,β-unsaturated dicarboxylic anhydride units is 18% by mass or more, the α,β-unsaturated dicarboxylic anhydride units in the copolymer (C) react with the carboxyl group terminal or amino group terminal of the polyamide (A), thereby increasing the viscosity of the polyamide composition, improving the melt tension, and suppressing dripping. Furthermore, the amount of carboxyl group terminals is reduced by the reaction, so that the decomposition of the polyamide (A) at high temperatures is suppressed, and the flame retardancy of the thin wall can be improved. When the content of α,β-unsaturated dicarboxylic anhydride units is 50% by mass or less, the viscosity of the polyamide composition does not become too high, and high flame retardancy and excellent moldability of the thin wall can be achieved at the same time. From this viewpoint, the content of the α,β-unsaturated dicarboxylic anhydride unit in the copolymer (C) is more preferably 19% by mass or more, even more preferably 20% by mass or more, and more preferably 40% by mass or less, even more preferably 30% by mass or less, even more preferably 28% by mass or less, and particularly preferably 25% by mass or less. The content of the α,β-unsaturated dicarboxylic anhydride unit in the copolymer (C) is more preferably 18 to 40% by mass, even more preferably 19 to 30% by mass, even more preferably 20 to 28% by mass, and particularly preferably 20 to 25% by mass. The copolymer (C) may further have structural units other than aromatic vinyl units and α,β-unsaturated dicarboxylic anhydride units, but the total content of aromatic vinyl units and α,β-unsaturated dicarboxylic anhydride units in the copolymer (C) is preferably 80 mass% or more, more preferably 90 mass% or more, and even more preferably 100 mass%.
[0039] The glass transition temperature of the copolymer (C) is 140° C. or higher, preferably 145° C. or higher, more preferably 150° C. or higher, from the viewpoint of flame retardancy and heat resistance in a thin wall, and is preferably 200° C. or lower, more preferably 180° C. or lower, and even more preferably 160° C. or lower, from the viewpoint of suppressing thermal decomposition of the polyamide during melt molding. The glass transition temperature of the copolymer (C) is preferably in the range of 140 to 200° C., more preferably 145 to 180° C., and even more preferably 150 to 160° C. The glass transition temperature of the copolymer (C) is measured by the method described in the Examples. From the viewpoint of flame retardancy and heat resistance in a thin wall, the weight average molecular weight (Mw) of the copolymer (C) is preferably 10,000 or more, more preferably 20,000 or more, even more preferably 30,000 or more, even more preferably 40,000 or more, particularly preferably 50,000 or more, and is preferably 500,000 or less, more preferably 400,000 or less, even more preferably 300,000 or less, particularly preferably 200,000 or less. The range of the weight average molecular weight (Mw) of the copolymer (C) is more preferably 10,000 to 500,000, more preferably 20,000 to 400,000, particularly preferably 30,000 to 300,000, and most preferably 50,000 to 200,000. The weight average molecular weight (Mw) is measured in terms of polystyrene by gel permeation chromatography (GPC). The copolymer (C) may be a commercially available product or may be synthesized by a known method. The bonding form between the aromatic vinyl unit and the α,β-unsaturated dicarboxylic anhydride unit is not particularly limited, and may be any of random polymerization, block polymerization, and graft polymerization, but the bonding form is preferably random polymerization or block polymerization, since the effect of the present invention is more prominent, and the copolymer (C) is preferably obtained by reacting the aromatic vinyl with the α,β-unsaturated dicarboxylic anhydride. Commercially available copolymers (C) include the DYLARK series (trade name, manufactured by NOVA Chemicals) and the XIRAN series (trade name, manufactured by Polyscope).
[0040] <Filler (D)> The polyamide composition of the present invention preferably further contains a filler (D) from the viewpoint of improving flame retardancy, heat resistance, moldability and mechanical strength in a thin walled product. The filler (D) may have various forms such as fiber, plate, needle, powder, cloth, etc. Specific examples include fibrous fillers such as glass fiber, carbon fiber, aramid fiber, liquid crystal polymer (LCP) fiber, gypsum fiber, brass fiber, ceramic fiber, and boron whisker fiber; flat fillers such as glass flakes, mica, and talc; needle fillers such as potassium titanate whiskers, aluminum borate whiskers, calcium carbonate whiskers, magnesium sulfate whiskers, wollastonite, sepiolite, xonotlite, and zinc oxide whiskers; silica, alumina, barium carbonate, magnesium carbonate, aluminum nitride, boron nitride, and potassium titanate. , titanium oxide, aluminum silicate (kaolin, clay, pyrophyllite, bentonite), calcium silicate, magnesium silicate (attapulgite), aluminum borate, calcium sulfate, barium sulfate, magnesium sulfate, asbestos, glass beads, carbon black, graphite, carbon nanotubes, silicon carbide, sericite, hydrotalcite, molybdenum disulfide, phenolic resin particles, crosslinked styrene-based resin particles, crosslinked acrylic resin particles, and other powdered fillers; cloth fillers such as glass cloth, and the like. These may be used alone or in combination of two or more. The surface of these fillers (D) may be treated with a polymeric compound such as a silane coupling agent, a titanium coupling agent, an acrylic resin, a urethane resin, or an epoxy resin, or with other low molecular weight compounds, for the purpose of improving dispersibility in the polyamide (A) or for the purpose of improving adhesion to the polyamide (A).
[0041] Among the fillers (D), at least one selected from the group consisting of fibrous fillers and needle-shaped fillers is preferred because it is low cost and can produce molded products with high mechanical strength. As the filler (D), glass fiber is preferred from the viewpoint of high strength and low cost, and needle-shaped fillers are preferred from the viewpoint of producing molded products with high surface smoothness. As the filler (D), at least one selected from the group consisting of glass fiber, wollastonite, potassium titanate whisker, calcium carbonate whisker, and aluminum borate whisker is preferred, at least one selected from the group consisting of glass fiber and wollastonite is more preferred, and glass fiber is even more preferred.
[0042] The average fiber length of the glass fibers is preferably 1 to 10 mm, more preferably 1 to 7 mm, and further preferably 2 to 4 mm. From the viewpoint of obtaining mechanical strength, the average fiber diameter of the glass fibers is preferably 6 to 20 μm, and more preferably 6 to 15 μm. The average fiber length and average fiber diameter of the glass fibers can be determined by measuring the fiber length and fiber diameter of 400 arbitrarily selected glass fibers by image analysis using an electron microscope, and calculating the weight average value of each. The average fiber length and average fiber diameter of glass fibers in a polyamide composition or in a molded article made of the polyamide composition can be determined, for example, by dissolving the polyamide composition or the molded article in an organic solvent, extracting the glass fibers, and subjecting the extracted glass fibers to image analysis using an electron microscope in the same manner as described above.
[0043] <Other ingredients> The polyamide composition of the present invention may further contain, as necessary, other components in addition to those described above, such as an anti-drip agent such as polytetrafluoroethylene powder; an antioxidant such as a phenolic or phosphorus-based antioxidant; a release agent such as a polyolefin wax; a light stabilizer; a colorant; an antistatic agent; a crystal nucleating agent; a plasticizer; and a lubricant.
[0044] <Content of each component in the polyamide composition> The content of polyamide (A) in the polyamide composition of the present invention is preferably 20 to 80% by mass. When the content of polyamide (A) is 20% by mass or more, molding is easy and the heat resistance and mechanical properties of the obtained molded article are good, and when the content of polyamide (A) is 80% by mass or less, the flame retardancy is good. From this viewpoint, the content of polyamide (A) is more preferably 30 to 70% by mass, and further preferably 35 to 60% by mass.
[0045] The content of the flame retardant (B) in the polyamide composition of the present invention is preferably 1 to 100 parts by mass relative to 100 parts by mass of the polyamide (A). When the content of the flame retardant (B) is 1 part by mass or more, the flame retardancy is improved, and when the content of the flame retardant (B) is 100 parts by mass or less, the deterioration of the mechanical properties of the obtained polyamide composition can be suppressed. From this viewpoint, the content of the flame retardant (B) is more preferably 5 to 90 parts by mass, further preferably 10 to 70 parts by mass, further more preferably 20 to 60 parts by mass, and particularly preferably 30 to 55 parts by mass relative to 100 parts by mass of the polyamide (A). When a flame retardant auxiliary is used, the content of the flame retardant auxiliary is preferably from 0.1 to 50 parts by mass, and more preferably from 1 to 30 parts by mass, based on 100 parts by mass of the polyamide (A).
[0046] The content of copolymer (C) in the polyamide composition of the present invention is 0.3-2.0% by mass based on the total content of polyamide (A), flame retardant (B) and copolymer (C). Here, the constituent part of copolymer (C) in which copolymer (C) reacts with polyamide is also calculated as the content of copolymer (C) in the polyamide composition. When the content of copolymer (C) is 0.3% by mass or more, the α,β-unsaturated dicarboxylic anhydride unit in copolymer (C) reacts with the carboxyl group terminal or amino group terminal of polyamide (A), thereby increasing the viscosity of the polyamide composition, improving the melt tension, and suppressing dripping. Furthermore, the amount of carboxyl group terminals is reduced by the reaction, so that the decomposition of polyamide (A) at high temperatures is suppressed, and the flame retardancy in thin walls can be improved. In addition, when the content of copolymer (C) is 2.0% by mass or less, the viscosity of the polyamide composition does not become too high, and high flame retardancy in thin walls and excellent moldability can be achieved at the same time. From this viewpoint, the content of the copolymer (C) is preferably 0.4% by mass or more, more preferably 0.5% by mass or more, even more preferably 0.6% by mass or more, even more preferably 0.7% by mass or more, particularly preferably 1.0% by mass or more, most preferably 1.3% by mass or more, and more preferably 1.8% by mass or less, even more preferably 1.7% by mass or less, and even more preferably 1.6% by mass or less, based on the total content of the polyamide (A), the flame retardant (B) and the copolymer (C). The range of the copolymer (C) is preferably 0.4 to 2.0% by mass, more preferably 0.5 to 1.8% by mass, more preferably 0.6 to 1.8% by mass, even more preferably 0.7 to 1.7% by mass, particularly preferably 1.0 to 1.7% by mass, and most preferably 1.3 to 1.6% by mass. The total content of the polyamide (A), the flame retardant (B) and the copolymer (C) in the polyamide composition of the present invention is not particularly limited, but from the viewpoints of flame retardancy, heat resistance and moldability in a thin wall, it is preferably 40 mass% or more, more preferably 50 mass% or more, and even more preferably 60 mass% or more.
[0047] When the polyamide composition of the present invention contains a filler (D), the content thereof is preferably 1 to 100 parts by mass, more preferably 5 to 90 parts by mass, and even more preferably 10 to 80 parts by mass, per 100 parts by mass of the polyamide (A), from the viewpoint of obtaining a molded article having high mechanical strength. When the above-mentioned other components are used, the content of the other components in the polyamide composition of the present invention is preferably 30% by mass or less, more preferably 20% by mass or less, and further preferably 10% by mass or less.
[0048] The polyamide composition of the present invention can be prepared by mixing the above-mentioned components according to a known method. More specific preparation methods include, for example, a method of adding each component during the polycondensation reaction of polyamide (A), a method of dry blending polyamide (A) and each component, and a method of melt-kneading each component using an extruder. Among these, a method of melt-kneading each component using an extruder is preferred because it is easy to operate and can obtain a uniform composition. The extruder used in this case is preferably a twin-screw type, and the melt-kneading temperature is preferably within a range of 5°C higher than the melting point of polyamide (A) to 370°C or lower from the viewpoint of achieving both dispersibility and prevention of resin deterioration, and more preferably a temperature range of 10°C to 20°C higher than the melting point. There is no particular limitation on the form of the polyamide composition, and it can be, for example, pelletized.
[0049] The polyamide composition of the present invention has good moldability, and can be molded into molded products by molding methods generally used for thermoplastic resin compositions, such as injection molding, extrusion molding, press molding, blow molding, calendar molding, and casting molding. A molding method that combines the above molding methods can also be used. In particular, injection molding is preferred in terms of ease of molding, mass productivity, cost, etc. The polyamide composition of the present invention can also be composite molded with other polymers. Furthermore, the polyamide composition of the present invention can also be composited with a molded body or fabric made of metal.
[0050] In the polyamide composition of the present invention, the flow length when the melt of the polyamide composition is injection molded in a mold having a thickness of 0.5 mm and a width of 40 mm under the conditions of a cylinder temperature 20° C. higher than the melting point of polyamide (A), an injection pressure of 74 MPa, and a mold temperature of 140° C. is preferably 40 mm or more. This allows both high flame retardancy and excellent moldability in a thin wall to be achieved. From this viewpoint, the flow length is more preferably 45 mm or more, even more preferably 48 mm or more, even more preferably 50 mm or more, and particularly preferably 53 mm or more, and is preferably 70 mm or less, more preferably 65 mm or less, even more preferably 60 mm or less, even more preferably 56 mm or less, and may be 54 mm or less, or even 52 mm or less. The flow length is the average value of the flow lengths Ln of five test pieces obtained when five test pieces are produced under the above conditions using a mold having a thickness of 0.5 mm and a width of 40 mm, and is specifically measured by the method described in the examples.
[0051] The melt flow rate (MFR) of the polyamide composition of the present invention at a temperature of 320°C and a load of 2.16 kg is preferably 15 g / 10 min or less. This allows both high flame retardancy and excellent moldability in a thin wall. From this viewpoint, the melt flow rate is more preferably 1 to 13 g / 10 min, further preferably 2 to 10 g / 10 min, and even more preferably 3 to 7 g / 10 min. The MFR can be determined by measuring the amount of molten resin (g / 10 min) flowing out of a standard die (diameter 2.095 mm, length 8.000 mm) at a temperature of 320°C and a load of 2.16 kg in accordance with JIS K 7210-1:2014.
[0052] [Molded products] The molded article of the present invention is made of the polyamide composition of the present invention and can be used as an electric / electronic part, an automobile part, an industrial part, a fiber, a film, a sheet, a household product, or any other molded article of any shape and for any purpose after undergoing the molding process described above.
[0053] Examples of electrical and electronic components include connectors such as FPC connectors, BtoB connectors, card connectors, SMT connectors (coaxial connectors, etc.), memory card connectors, etc.; SMT relays; SMT bobbins; sockets such as memory sockets, CPU sockets, etc.; switches such as command switches, SMT switches, etc.; optical components such as optical fiber components, optical sensors, etc.; LED application components such as LED reflectors; and electronic boards such as solar cell boards, LED mounting boards, flexible printed wiring boards, and resin molded circuit boards.
[0054] Automotive parts include, for example, cooling parts such as thermostat housings, radiator tanks, radiator hoses, water outlets, water pump housings, and rear joints; intake and exhaust system parts such as intercooler tanks, intercooler cases, turbo duct pipes, EGR cooler cases, resonators, throttle bodies, intake manifolds, and tail pipes; fuel system parts such as fuel delivery pipes, gasoline tanks, quick connectors, canisters, pump modules, fuel piping, oil strainers, lock nuts, and seals; structural parts such as mounting brackets, torque rods, and cylinder head covers; bearing retainers, gear tensioners, headlamp actuator gears, and sliding doors. These include drive system parts such as rollers and clutch peripheral parts; brake system parts such as air brake tubes; automotive electrical parts such as wire harness connectors in the engine bay, motor parts, sensors, ABS bobbins, combination switches, and in-vehicle switches; and interior and exterior parts such as sliding door dampers, door mirror stays, door mirror brackets, inner mirror stays, roof rails, engine mount brackets, air cleaner inlet pipes, door checkers, plastic chains, emblems, clips, breaker covers, cup holders, airbags, fenders, spoilers, radiator supports, radiator grilles, louvers, air scoops, hood bulges, back doors, and fuel sender modules.
[0055] Examples of industrial parts include gas pipes, oil field drilling pipes, hoses, anti-termite cables (communication cables, pass cables, etc.), paint parts of powder coated products (inner coatings of water pipes, etc.), undersea oil field pipes, pressure resistant hoses, hydraulic tubes, paint tubes, fuel pumps, separators, supercharge ducts, butterfly valves, conveyor roller bearings, railway sleeper spring supports, outboard motor engine covers, generator engine covers, irrigation valves, large switches, and monofilaments (extruded threads) for fishing nets, etc.
[0056] Examples of the fibers include airbag base fabrics, heat-resistant filters, reinforcing fibers, bristles for brushes, fishing lines, tire cords, artificial turf, carpets, and fibers for seating.
[0057] Examples of films and sheets include heat-resistant adhesive tapes such as heat-resistant masking tape and industrial tape; magnetic tape materials such as cassette tapes, magnetic tapes for storing data for digital data storage, and video tapes; food packaging materials such as pouches for retort foods, individual packages for confectionery, and packages for processed meat products; and electronic component packaging materials such as packages for semiconductor packages.
[0058] In particular, since the polyamide composition of the present invention has excellent flame retardancy, heat resistance and moldability, particularly in thin-walled portions, it can be suitably used for electric and electronic components, and can be suitably used for electric and electronic components including SMT processes, more specifically, SMT-compatible connectors, SMT relays, SMT bobbins, sockets, command switches, SMT switches, etc. EXAMPLES
[0059] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples. The evaluations in the examples and comparative examples were carried out according to the methods described below.
[0060] (Melting Point) The melting point of polyamide (A) was determined as the peak temperature (°C) of the melting peak that appeared when the temperature was raised from 30°C to 360°C at a rate of 10°C / min under a nitrogen atmosphere using a differential scanning calorimeter "DSC822" manufactured by Mettler Toledo Co., Ltd. When there were multiple melting peaks, the peak temperature of the melting peak on the highest temperature side was determined as the melting point.
[0061] (Intrinsic viscosity [η]) Concentrated sulfuric acid solutions (sample solutions) of polyamide (A) were prepared using concentrated sulfuric acid (concentration: 98% by mass) as the solvent, with solution concentrations c of 0.05, 0.1, 0.2, and 0.4 g / dl, respectively, and the flow time t0 of the solvent and the flow time t1 of the sample solutions of each concentration were measured using an Ubellohde viscometer in a thermostatic bath at 30°C. The inherent viscosity (η inh ) and calculate the inherent viscosity (η inh ) was extrapolated to a concentration of 0 to determine the intrinsic viscosity [η] of polyamide (A). η inh (dl / g)=[ln(t1 / t0)] / c [In the formula, t0 represents the flow time (seconds) of the solvent, t1 represents the flow time (seconds) of the sample solution, and c represents the solution concentration (g / dl).]
[0062] (glass transition temperature) The glass transition temperature of the copolymer (C) was measured by a method in accordance with JIS K 7121:1987.
[0063] (Flame retardant) Flame retardancy was evaluated according to the UL-94 standard. Using the polyamide compositions obtained in each Example and Comparative Example, injection molding (mold temperature: 140°C) was performed at a cylinder temperature about 20°C higher than the melting point of the polyamide to obtain a test piece with a thickness of 0.3 mm, a width of 13 mm, and a length of 125 mm. Next, the upper end of the test piece was clamped to fix the test piece vertically, and a predetermined flame was applied to the lower end for 10 seconds and released, and the burning time of the test piece (first time) was measured. Immediately after the fire was extinguished, the lower end was again exposed to a flame and released, and the burning time of the test piece (second time) was measured. The same measurement was repeated for five test pieces, and a total of 10 data were obtained, including five data for the first burning time and five data for the second burning time. The total of the 10 data was designated T, and the maximum value of the 10 data was designated M, and the data was evaluated according to the following evaluation criteria. The presence or absence of dripping during application of flame was also visually confirmed. [Evaluation Criteria] V-0: T was 50 seconds or less, M was 10 seconds or less, the flame did not reach the clamp, and the flaming molten material did not ignite the cotton 12 inches below when it fell. V-1: T was less than 250 seconds, M was less than 30 seconds, the flame did not reach the clamp, and the flaming molten material did not ignite the cotton 12 inches below when it fell. V-2: T was less than 250 seconds, M was less than 30 seconds, the flame did not rise to the clamp, and the flaming molten material fell and ignited the cotton 12 inches below.
[0064] (Deformation amount) The deformation in length of the test pieces subjected to the flame retardancy evaluation was evaluated by the following method. Test pieces that had drips during the flame retardancy evaluation were excluded, and the lengths of n test pieces that had no drips were measured before and after the flame retardancy evaluation, and the deformation was calculated according to the following formula. If drips occurred in all test pieces, the deformation was marked as x. The smaller the deformation value, the better the flame retardancy. Deformation amount = [(total length of n test pieces after flame retardancy evaluation) - (total length of n test pieces before flame retardancy evaluation)] / n
[0065] (Moldability (flow length)) Using an injection molding machine UH-1000 (mold clamping force 80t) manufactured by Nissei Plastic Industrial Co., Ltd., five test pieces were prepared one by one in a mold having a thickness of 0.5 mm and a width of 40 mm under the conditions of a cylinder temperature 20°C higher than the melting point of polyamide (A), an injection pressure of 74 MPa, and a mold temperature of 140°C. The average value of the flow length Ln of the five test pieces prepared was calculated and used as the flow length of the polyamide composition. This was used as an index for evaluating moldability. The higher the flow length value, the better the moldability, and a flow length of 40 mm or more can be used in practical use.
[0066] Production Example 1 (Production of Polyamide PA1) 7882.0g of terephthalic acid, 7742.9g of a diamine mixture of 1,9-nonanediamine:2-methyl-1,8-octanediamine = 85:15 (molar ratio), 280.8g of benzoic acid as an end-capping agent, 16.0g of sodium hypophosphite monohydrate, and 4L of distilled water were placed in an autoclave with an internal volume of 40L and substituted with nitrogen. The internal temperature was raised to 200°C over 2 hours. At this time, the autoclave was pressurized to 2MPa. Thereafter, the internal temperature was kept at 215°C, and the water vapor was gradually removed to keep the pressure at 2MPa while reacting for 2 hours. Next, the pressure was lowered to 1.2MPa over 30 minutes to obtain a prepolymer. This prepolymer was crushed to a size of 6mm or less and dried at 120°C under reduced pressure for 12 hours. This was subjected to solid-phase polymerization for 10 hours under conditions of a temperature of 230°C and a pressure of 13.3 Pa, to obtain polyamide PA1 having a melting point of 306°C and an intrinsic viscosity [η] of 0.93 dl / g.
[0067] Examples 1 to 9, Comparative Examples 1 to 2 The components other than the filler (D) were fed from the most upstream hopper of a twin-screw extruder (screw diameter 26 mmφ, L / D=46, rotation speed 150 rpm, discharge rate 10 kg / h) manufactured by Toshiba Machine Co., Ltd., so that the blending composition of polyamide (A), flame retardant (B), copolymer (C), filler (D), flame retardant assistant, and other components was as shown in Table 1, and the filler (D) was fed from a side feeder and melt-kneaded at 320 ° C. The melt-kneaded polyamide composition was extruded in the form of a strand, cooled, and cut to obtain pellets of the polyamide composition. Using the obtained pellets, test pieces of a predetermined shape were prepared according to the above-mentioned method, and various physical properties were evaluated. The results are shown in Table 1.
[0068] The components shown in Table 1 are as follows. [Polyamide (A)] Polyamide PA1 obtained in Production Example 1 [Flame retardant (B)] Brominated flame retardant B1: Chemtura, product name "Firemaster CP-44HF" (glycidyl methacrylate modified polybrominated styrene) Phosphorus-based flame retardant B2: Clariant, product name "Exolit OP1230" [Copolymer (C)] Copolymer C1: Polyscope, product name "XIRAN SZ 23110" (styrene-maleic anhydride copolymer, maleic anhydride content: 23% by mass, glass transition temperature: 150°C, weight average molecular weight (Mw): 110,000) Copolymer C2: Polyscope, product name "XIRAN SZ 28065" (styrene-maleic anhydride copolymer, maleic anhydride content: 28% by mass, glass transition temperature: 165°C, weight average molecular weight (Mw): 65,000) Copolymer C3: Polyscope, product name "XIRAN SZ 26180" (styrene-maleic anhydride copolymer, maleic anhydride content: 26% by mass, glass transition temperature: 160°C, weight average molecular weight (Mw): 180,000) [Filler (D)] Filler D1: Nitto Boseki Co., Ltd., product name "CS-3G-225S" (glass fiber, cross-sectional shape: round, average fiber diameter: 9.5 μm, average fiber length: 3 mm) [Flame retardant synergist] Flame retardant assistant 1: Nippon Light Metal Co., Ltd., product name "Flamtard S" (zinc stannate)
[0069] [Other ingredients] Anti-drip agent: Mitsui DuPont Fluorochemicals Co., Ltd., product name "640-J" (polytetrafluoroethylene powder) Antioxidant: Sumitomo Chemical Co., Ltd., trade name "Sumilizer GA-80" (3,9-bis{1,1-dimethyl-2-[β-(3-t-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro[5.5]undecane) Release agent: Mitsui Chemicals, Inc., product name "Hiwax 200P" (polyolefin wax) Nucleating agent: Fuji Talc Industries Co., Ltd., product name "ML112" (talc)
[0070] [Table 1] *1: Indicates the content of copolymer (C) relative to the total content of polyamide (A), flame retardant (B) and copolymer (C). *2: Regarding Example 1, since dripping did not occur in three of the five test pieces, the deformation amount was calculated using the three test pieces in which dripping did not occur.
[0071] As shown in Table 1, the polyamide composition of the present invention can provide a thin-walled molded article having excellent flame retardancy, and is also excellent in heat resistance and moldability.
Claims
1. A polyamide composition comprising: a polyamide (A) having a melting point of 280° C. or higher; a flame retardant (B); and an aromatic vinyl copolymer (C); the aromatic vinyl copolymer (C) contains a structural unit derived from an aromatic vinyl and a structural unit derived from an α,β-unsaturated dicarboxylic acid anhydride, and the glass transition temperature of the aromatic vinyl copolymer (C) is 140° C. or higher and 165° C. or lower; the content of structural units derived from an α,β-unsaturated dicarboxylic acid anhydride in the aromatic vinyl copolymer (C) is 18 to 28% by mass, The content of the aromatic vinyl copolymer (C) is 0.3 to 2.0 mass % based on the total content of the polyamide (A), the flame retardant (B) and the aromatic vinyl copolymer (C).
2. 2. The polyamide composition according to claim 1, wherein the polyamide (A) is a semi-aromatic polyamide.
3. The polyamide composition according to claim 2, wherein, in the semi-aromatic polyamide, more than 50 mol% of the dicarboxylic acid-derived constituent units constituting the semi-aromatic polyamide are aromatic dicarboxylic acid-derived constituent units, and more than 50 mol% of the diamine-derived constituent units constituting the semi-aromatic polyamide are aliphatic diamine-derived constituent units having 4 to 18 carbon atoms.
4. The polyamide composition according to claim 3, wherein the aliphatic diamine is at least one selected from the group consisting of 1,6-hexanediamine, 1,9-nonanediamine, 2-methyl-1,8-octanediamine, and 1,10-decanediamine.
5. The polyamide composition according to any one of claims 1 to 4, wherein the flame retardant (B) is a brominated flame retardant.
6. The polyamide composition according to any one of claims 1 to 5, wherein the structural units derived from aromatic vinyl include structural units derived from at least one selected from the group consisting of styrene and α-methylstyrene.
7. The polyamide composition according to any one of claims 1 to 6, wherein the α,β-unsaturated dicarboxylic acid anhydride is at least one selected from the group consisting of maleic anhydride and a monoalkyl maleic anhydride having an alkyl group having 1 to 3 carbon atoms.
8. The polyamide composition according to any one of claims 1 to 7, wherein the aromatic vinyl copolymer (C) has a weight average molecular weight (Mw) of 10,000 to 500,000.
9. The polyamide composition according to any one of claims 1 to 8, further comprising a filler (D).
10. The polyamide composition according to any one of claims 1 to 9, which is obtained by melt-kneading a polyamide (A), a flame retardant (B), and an aromatic vinyl copolymer (C).
11. The polyamide composition according to claim 10, which is obtained by melt-kneading a polyamide (A), a flame retardant (B), an aromatic vinyl copolymer (C), and the filler (D).
12. A molded article comprising the polyamide composition according to any one of claims 1 to 11.