Polyester elastomer derived from biomass resource

JP2024100971A5Inactive Publication Date: 2024-12-03TOYOBO MC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024084700
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Benefits of technology

【0010】 本発明のバイオマス資源由来ポリエステルエラストマーは、バイオマス資源由来原料の使用割合を高めても、ポリエステルエラストマーの着色を防止することができ、化石燃料資源由来ポリエステルエラストマーが有する優れた機械特性、滞溜安定性、耐水老化性、及び耐熱老化性を保持することができる。そのため、本発明のバイオマス資源由来ポリエステルエラストマーは、化石燃料資源の枯渇問題等の世界的な環境問題の解決に大きく貢献することができる。

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide a polyester elastomer derived from a biomass resource, which is free from coloration and can retain excellent mechanical characteristics, residence stability, water-aging resistance, and heat-aging resistance.SOLUTION: Provided is a polyester elastomer in which a hard segment comprising an aromatic dicarboxylic acid and an aliphatic and / or alicyclic diol as constituent components and a soft segment comprising an aromatic dicarboxylic acid and an aliphatic polyether as constituent components are bonded, where the aromatic dicarboxylic acid and the aliphatic and / or alicyclic diol are derived from a fossil fuel resource, the aliphatic polyether is derived from a biomass resource, the polyester elastomer has a biomass degree of 20-85%, and the polyester elastomer has a reduced viscosity of 1.2 dl / g or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a biomass resource-derived polyester elastomer that is free of coloration even when it has a high bio-based content, and that can retain the excellent mechanical properties, residence stability, water aging resistance, and heat aging resistance that are characteristic of polyester elastomers derived from fossil fuel resources. [Background technology]

[0002] Polyester elastomers are materials with excellent injection and extrusion moldability, high mechanical strength, and rubber-like properties such as elastic recovery, impact resistance, and flexibility, as well as excellent heat and cold resistance, and are used in a wide range of applications, including automotive parts, electrical and electronic parts, fibers, films, and sports parts.

[0003] In recent years, concerns about the depletion of fossil fuel resources and the increase in atmospheric carbon dioxide have become global environmental issues, and as a result, the use of biomass for various polymers has been promoted. As biomass resources are renewable resources, they are expected to become an important design concept in future polymer development from the perspective of SDGs and carbon neutrality.

[0004] However, because biomass resource-derived raw materials contain impurities that cannot be completely removed in the refining process, increasing the proportion of biomass resource-derived raw materials in an attempt to increase the bio-based content of the polyester increases the amount of impurities, which results in the reaction being inhibited and the reduced viscosity not increasing, making it difficult to maintain the excellent properties of polyester derived from fossil fuel resources.

[0005] In response to this problem, it has been proposed to prevent the deterioration of the mechanical properties of polyester by reducing the sulfur atom content and the amount of acid end groups in polyester made from dicarboxylic acid and / or diol derived from biomass resources (see Patent Document 1). Although this biomass resource-derived polyester prevents the deterioration of mechanical properties to some extent, it causes coloring of the polyester, which leads to a problem of poor appearance of the molded product. In addition, it is not possible to maintain the excellent properties of polyester derived from fossil fuel resources in terms of retention stability, water aging resistance, and heat aging resistance. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 5303237 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in view of the current state of the prior art, and an object of the present invention is to provide a biomass resource-derived polyester elastomer that is free of coloration even when the proportion of biomass resource-derived raw materials in the polyester elastomer is increased, and that can retain the excellent mechanical properties, residence stability, water aging resistance, and heat aging resistance that are possessed by polyester elastomers derived from fossil fuel resources. [Means for solving the problem]

[0008] As a result of intensive research into achieving this object, the present inventors have found that by making the aromatic dicarboxylic acid component and the aliphatic and / or alicyclic diol of the polyester constituting the hard segment of a polyester elastomer derived from a fossil fuel resource, and by making the aromatic dicarboxylic acid and the aliphatic polyether constituting the soft segment, the aliphatic polyether is derived from a biomass resource, it is possible to provide a polyester elastomer derived from a biomass resource that is free of coloration and that can retain the excellent mechanical properties, residence stability, water aging resistance, and heat aging resistance of polyester elastomers derived from fossil fuel resources, and have completed the present invention.

[0009] That is, the present invention comprises the following (1) to (6). (1) A polyester elastomer comprising a hard segment made of a polyester having as its constituent components an aromatic dicarboxylic acid and an aliphatic and / or alicyclic diol, and a soft segment made of an aromatic dicarboxylic acid and an aliphatic polyether, wherein the aromatic dicarboxylic acid and the aliphatic and / or alicyclic diol are derived from fossil fuel resources, the aliphatic polyether is derived from a biomass resource, the biobased content of the polyester elastomer is 20 to 85%, and the reduced viscosity of the polyester elastomer is 1.2 dl / g or more. (2) The biomass resource-derived polyester elastomer according to (1), wherein the biomass resource-derived aliphatic polyether is polytetramethylene ether glycol. (3) The biomass resource-derived polyester elastomer according to (1) or (2), characterized in that the glass transition temperature (Tg) is −70 to 10° C. (4) A biomass resource-derived polyester elastomer according to (1) or (2), characterized in that the Co-b value of the polyester elastomer is 7 or less. (5) A biomass resource-derived polyester elastomer according to (1) or (2), characterized in that the polyester elastomer has a bio-based content of 35 to 85% and a reduced viscosity of 1.8 dl / g or more. (6) A biomass resource-derived polyester elastomer according to (1) or (2), characterized in that the hard segment of the polyester elastomer is a polyester composed of butylene terephthalate units. Effect of the Invention

[0010] The biomass resource-derived polyester elastomer of the present invention can prevent discoloration of the polyester elastomer even when the proportion of biomass resource-derived raw materials used is increased, and can retain the excellent mechanical properties, retention stability, water aging resistance, and heat aging resistance of fossil fuel resource-derived polyester elastomers. Therefore, the biomass resource-derived polyester elastomer of the present invention can greatly contribute to solving global environmental problems such as the depletion of fossil fuel resources. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The biomass resource-derived polyester elastomer of the present invention is a polyester elastomer in which a hard segment made of a polyester having as its constituent components an aromatic dicarboxylic acid and an aliphatic and / or alicyclic diol is bonded to a soft segment made of an aromatic dicarboxylic acid and an aliphatic polyether, and is characterized in that the aromatic dicarboxylic acid and the aliphatic and / or alicyclic diol are derived from fossil fuel resources, and the aliphatic polyether is derived from a biomass resource.

[0012] As the aromatic dicarboxylic acid constituting the polyester of the hard segment, a normal aromatic dicarboxylic acid is widely used, and as the main aromatic dicarboxylic acid, terephthalic acid or naphthalenedicarboxylic acid (among the isomers, 2,6-naphthalenedicarboxylic acid is preferred). The content of these aromatic dicarboxylic acids is preferably 70 mol% or more, more preferably 80 mol% or more, and even more preferably 90 mol% or more, and may be 100 mol% in the total dicarboxylic acids constituting the polyester of the hard segment. Examples of dicarboxylic acid components other than terephthalic acid and naphthalenedicarboxylic acid include aromatic dicarboxylic acids such as diphenyldicarboxylic acid, isophthalic acid, and 5-sodium sulfoisophthalic acid, alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid and tetrahydrophthalic anhydride, and aliphatic dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, dimer acid, and hydrogenated dimer acid. These can be used in a range that does not significantly lower the melting point of the resin, and the amount is preferably 30 mol% or less of the total acid components, more preferably 20 mol% or less, and even more preferably 10 mol% or less, and may be 0 mol%. When these dicarboxylic acids are used as raw materials for polyester elastomers, they may be in the form of esters of the dicarboxylic acids. For example, terephthalic acid and dimethyl terephthalate can be used as raw materials.

[0013] As the aliphatic or alicyclic diol constituting the polyester of the hard segment, a general aliphatic or alicyclic diol is widely used, and is not particularly limited, but is preferably an alkylene glycol having 2 to 8 carbon atoms. Specific examples include ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 1,4-cyclohexanedimethanol. Among these, either ethylene glycol or 1,4-butanediol is preferable.

[0014] As the component constituting the polyester of the above hard segment, those consisting of butylene terephthalate units (units consisting of terephthalic acid and 1,4-butanediol) or butylene naphthalate units (units consisting of 2,6-naphthalenedicarboxylic acid and 1,4-butanediol) are preferred from the viewpoints of physical properties, moldability, and cost performance.

[0015] In addition, when an aromatic polyester suitable as a polyester constituting a hard segment of a polyester elastomer is produced in advance and then copolymerized with a soft segment component, the aromatic polyester can be easily obtained according to a normal polyester production method. In addition, such a polyester preferably has a number average molecular weight of 10,000 to 40,000.

[0016] As the aromatic dicarboxylic acid constituting the soft segment of the polyester elastomer, the aromatic dicarboxylic acid constituting the polyester of the hard segment can be used. In a preferred embodiment, the aromatic dicarboxylic acid constituting the soft segment and the aromatic dicarboxylic acid constituting the hard segment are the same.

[0017] The aliphatic polyether constituting the soft segment of the polyester elastomer is preferably a glycol compound since it bonds with the polyester of the hard segment.Specific examples include poly(ethylene oxide) glycol, poly(propylene oxide) glycol, polytetramethylene ether glycol, polytrimethylene ether glycol, poly(hexamethylene oxide) glycol, a copolymer of ethylene oxide and propylene oxide, an ethylene oxide adduct of poly(propylene oxide) glycol, and a copolymer of ethylene oxide and tetrahydrofuran.Among these, polytetramethylene ether glycol and an ethylene oxide adduct of poly(propylene oxide) glycol are preferred from the viewpoint of elasticity properties.

[0018] In the present invention, it is preferable to use aliphatic polyethers derived from biomass resources, particularly polytetramethylene ether glycol (PTMG) derived from biomass resources, as the constituent of the soft segment. As such PTMG, commercially available products can be obtained and used, and for example, BioPTMG1000 and BioPTMG2000 manufactured by Mitsubishi Chemical Corporation are preferably used.

[0019] The polyester elastomer is preferably a copolymer mainly composed of terephthalic acid, 1,4-butanediol, and polytetramethylene ether glycol. Of the dicarboxylic acid components constituting the polyester elastomer, terephthalic acid is preferably 40 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and particularly preferably 90 mol% or more. Of the glycol components constituting the polyester elastomer, the total of 1,4-butanediol and polytetramethylene ether glycol is preferably 40 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, and particularly preferably 90 mol% or more.

[0020] The number average molecular weight of the polytetramethylene ether glycol is preferably 500 to 4000, more preferably 700 to 3000, and further preferably 800 to 2500. If the number average molecular weight is less than the above range, it may be difficult to exhibit elastomeric properties. On the other hand, if the number average molecular weight exceeds the above range, the compatibility with the hard segment component may decrease, making it difficult to copolymerize in a block form.

[0021] In the present invention, the mass of the hard segment refers to the mass of the component composed of aromatic dicarboxylic acid and aliphatic and / or alicyclic diol, and the mass of the soft segment refers to the mass of the component composed of aromatic dicarboxylic acid and aliphatic polyether. For example, in the case of a polyester elastomer composed of terephthalic acid, 1,4-butanediol, and polytetramethylene ether glycol (PTMG), the mass of the hard segment is the mass of butylene terephthalate unit (condensation unit of terephthalic acid and 1,4-butanediol), and the mass of the soft segment is the mass of condensation unit of terephthalic acid and polytetramethylene ether glycol (PTMG).

[0022] The mass ratio of hard segment / soft segment of the polyester elastomer is preferably 5 / 95 to 90 / 10, more preferably 10 / 90 to 85 / 15, and even more preferably 15 / 85 to 80 / 20. If the amount of hard segment is small (the amount of PTMG is large), the polyester elastomer may not have satisfactory heat aging resistance and moldability (crystallinity). On the other hand, if the amount of hard segment is large (the amount of PTMG is small), the compatibility of the hard segment component and the soft segment component may decrease, making it difficult to copolymerize them into blocks. The polyester elastomer preferably has a melting point of 150 to 230° C. If the melting point is below 150° C., the polyester elastomer may not have the desired heat aging resistance and moldability (crystallinity). Conversely, if the melting point is above 230° C., the polyester elastomer may not have the desired impact resilience, flexibility, and low-temperature mechanical properties because the polyester elastomer contains a large amount of hard segments, resulting in a correspondingly high glass transition temperature (Tg).

[0023] In order to produce the polyester elastomer of the present invention, it is preferable to make the polycondensation time longer than in the past. Usually, the polycondensation time in the production of polyester elastomer is about 50 to 90 minutes, but in the present invention, the polycondensation time is preferably 100 to 140 minutes, more preferably 105 to 135 minutes. It is also preferable to control the polycondensation temperature within a narrow range. Usually, the polycondensation temperature in the production of polyester elastomer is about 235 to 260°C, but in the present invention, the polycondensation temperature is preferably 235 to 255°C, more preferably 240 to 250°C. If the polycondensation time is short or the polycondensation temperature is low, the reduced viscosity of the polyester elastomer does not increase, and the elongation at break and tensile strength at break may not be sufficient to function as a polyester elastomer. On the other hand, if the polycondensation time is long or the polycondensation temperature is high, the polyester elastomer may be colored, causing a deterioration in appearance, or causing a decrease in reduced viscosity due to thermal degradation.

[0024] The bio-based content of the polyester elastomer of the present invention is 20 to 85%, preferably 30 to 85%, and more preferably 35 to 85%. Conventionally, biomass resource-derived raw materials contain impurities that could not be completely removed in the refining process, and therefore when the ratio of the biomass raw materials is increased in an attempt to increase the bio-based content, the amount of impurities increases, inhibiting the reaction and preventing the reduced viscosity from increasing, resulting in a problem of longer polymerization time and discoloration. For this reason, it has been difficult to obtain a biomass resource-derived polyester elastomer that can prevent discoloration without reducing production efficiency and that can retain excellent flexibility, low-temperature mechanical properties, heat aging resistance, and water resistance. As a result of extensive research into polymerization raw materials for polyester elastomers, the present inventors have succeeded in obtaining a biomass resource-derived polyester elastomer that is free of discoloration and can retain the excellent properties of fossil fuel resource-derived polyester elastomers by using fossil fuel resource-derived hard segments and aliphatic polyethers as biomass resource-derived raw materials only for the soft segments, and by adopting appropriate polycondensation reaction time and temperature.

[0025] The reduced viscosity (ηsp / c), which is an index of molecular weight, is extremely important as a characteristic of the polyester elastomer of the present invention. In the present invention, the reduced viscosity at which the polyester elastomer exhibits long-term durability (heat aging resistance, water resistance) is 1.2 dl / g or more, preferably 1.3 dl / g or more, more preferably 1.4 dl / g or more, and even more preferably 1.8 dl / g or more. If the reduced viscosity (ηsp / c) is low, the molecular weight is small, and therefore it may not be possible to obtain a polyester elastomer that satisfies the long-term durability (heat aging resistance, water resistance) functions.

[0026] As a characteristic of the polyester elastomer of the present invention, the glass transition temperature (Tg), which is an index of low-temperature mechanical properties, is important. The glass transition temperature varies depending on the soft segment ratio in the polyester elastomer. In the present invention, the glass transition temperature at which the polyester elastomer exhibits the functions of rebound resilience, flexibility, and low-temperature mechanical properties is preferably -70 to 10°C, more preferably -65 to 10°C. If the glass transition temperature is high, it may not be possible to obtain a polyester elastomer that satisfies the functions of rebound resilience, flexibility, and low-temperature mechanical properties.

[0027] As a characteristic of the polyester elastomer of the present invention, the Co-b value, which is an index of the appearance of the molded product, is important. The Co-b value varies depending on impurities in the biomass resource-derived raw material and polymerization conditions. In the present invention, the Co-b value for obtaining a good appearance is preferably 10 or less, more preferably 7 or less, and even more preferably 4 or less. If the Co-b value is large, the pellets prepared will turn yellow, which will significantly impair the appearance of the molded product, and a satisfactory product may not be obtained.

[0028] The composition and composition ratio of the polyester elastomer of the present invention can be determined by dissolving a sample in a solvent such as deuterated chloroform and measuring the composition. 1 It can also be calculated from the proton integral ratio of H-NMR. EXAMPLES

[0029] In order to demonstrate the effects of the present invention, examples are given below, but the present invention is not limited to these examples. The property values ​​were evaluated by the following methods. The raw materials used in the examples and those not specifically stated were derived from fossil fuel resources.

[0030] (1) Reduced viscosity (ηsp / c) 0.05 g of polyester elastomer was dissolved in 25 mL of a mixed solvent (phenol / tetrachloroethane = 60 / 40), and the viscosity was measured at 30°C using an Ubbelohde viscosity tube.

[0031] (2) Melting point (Tm) Using a differential scanning calorimeter "DSC220" manufactured by Seiko Denshi Kogyo Co., Ltd., 5 mg of the measurement sample was placed in an aluminum pan, the lid was pressed down and sealed, and the sample was melted in nitrogen at 250°C for 2 minutes. The temperature was then lowered to 50°C at a rate of 20°C / min, and the temperature was then increased from 50°C to 250°C at a rate of 20°C / min. The endothermic peak due to melting from the obtained thermogram curve was taken as the melting point.

[0032] (3) Glass transition temperature (Tg) A dynamic viscoelasticity measuring device Rheogel-E4000 (manufactured by UBM Co., Ltd.) was used, and the measurement sample was prepared by pressing with a hot plate heated to 200-250°C using an NF-type single-action compression molding machine (manufactured by Shinto Metal Industry Co., Ltd.) to create a 0.4 mm thick sheet. Measurements were performed at a measurement frequency of 11 Hz and a heating rate of 2°C / min, with the peak position of tan δ from -150°C to 150°C being taken as Tg.

[0033] (4) Acid value (AV) 0.2g of sample was weighed out, benzyl alcohol was added, and the sample was dissolved by heating. The sample was dissolved in 20ml of chloroform and titrated with 0.08N potassium hydroxide (ethanol solution). The acid value was calculated from the amount of potassium hydroxide required for neutralization. Phenol red ethanol solution was used as an indicator.

[0034] (5) Color difference The Co-b value (the higher the value, the greater the yellowness) was measured using an automatic color difference meter (manufactured by Toyo Rika Kogyo Co., Ltd.).

[0035] (6) Retention stability (ΔMFR) The pellets of the polyester elastomer compositions obtained in the examples and comparative examples were retained at 190°C (Examples 2-4, Reference Examples 2-4, Comparative Example 4) or 230°C (Examples 1, 5, 6, Reference Examples 1, 5, 6, Comparative Examples 1-3) for 25 minutes, and then the melt flow rate (MFR: g / 10 min) was measured at 2160 g according to the test method (Method A) described in JIS K7210. Compositions with a moisture content of 0.1 mass% or less were used for the measurement.

[0036] (7) Tensile elongation and strength at break The tensile elongation and strength at break of polyester elastomer were measured in accordance with JIS K6251. Test pieces were prepared by injection molding resin dried under reduced pressure at 100°C for 5 hours into a 100mm x 100mm x 2mm plate using an injection molding machine (Yamashiro Seiki Co., Ltd., model-SAV) at a cylinder temperature (Tm+20°C) and a mold temperature of 30°C, and then punching out a dumbbell-shaped No. 3 test piece from the plate.

[0037] (8) Water aging resistance (treatment time at which elongation retention at break after water aging test is 50%) After treating the test pieces in boiling water at 100°C, the elongation at break was measured by the above method. The elongation at break of test pieces that were not treated in boiling water was also measured, and the retention of elongation at break after boiling water treatment was calculated as follows. The initial elongation at break is the elongation at break before boiling water treatment. Elongation retention at break (%) = (elongation at break after boiling water treatment / initial elongation at break) x 100 The boiling water treatment time when the elongation retention at break reached 50% was measured as the elongation half-life.

[0038] (9) Heat aging resistance (treatment time at which elongation retention at break after heat aging test is 50%) The test pieces were treated in air at 140°C, and then the elongation at break was measured by the above method. The elongation at break of test pieces that were not heat-treated was also measured, and the retention rate of elongation at break after heat treatment was calculated as follows. The initial elongation at break is the elongation at break before heat treatment. Elongation retention at break (%) = (elongation at break after heat treatment / initial elongation at break) x 100 The heat treatment time when the elongation retention at break reached 50% was measured as the elongation half-life.

[0039] (10) Bio-based content The bio-based ratio is the ratio of monomer components derived from biomass resources, calculated from the mass of monomer components derived from biomass resources to the mass of all monomer components that make up the polyester elastomer. The bio-based ratio is the ratio of the amount of carbon contained only in raw materials derived from biomass resources to the total carbon contained in the polyester elastomer. 14 C carbon ( 12 The bio-based content of polyester elastomers is measured using an accelerator mass spectrometer (AMS) in accordance with ASTM D6866.

[0040] Example 1 2000g of dimethyl terephthalate (DMT, manufactured by SK Petrochemical), 1360g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 750g of polytetramethylene ether glycol derived from biomass resources (BioPTMG1000, number average molecular weight 1000, manufactured by Mitsubishi Chemical), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220 ° C. for 150 minutes to carry out an ester exchange reaction. Next, the pressure inside the autoclave was gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245 ° C. and 1 Torr or less for 75 minutes. The polymerization reaction was further carried out at 245 ° C. and 1 Torr or less for 135 minutes, and a polymer with a hard segment / soft segment mass ratio of 72 / 28 (mass%) was taken out in pellet form. The resulting polymer was designated as the polyester elastomer of Example 1.

[0041] Example 2 1200g of dimethyl terephthalate (DMT, manufactured by SK Petrochemical), 800g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 1780g of polytetramethylene ether glycol derived from biomass resources (BioPTMG1000, number average molecular weight 1000, manufactured by Mitsubishi Chemical), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 200 ° C. for 165 minutes to carry out an ester exchange reaction. Next, the pressure inside the autoclave was gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245 ° C. and 1 Torr or less for 90 minutes. The polymerization reaction was further carried out at 245 ° C. and 1 Torr or less for 115 minutes, and a polymer with a hard segment / soft segment mass ratio of 33 / 67 (mass%) was taken out in pellet form. The resulting polymer was designated as the polyester elastomer of Example 2.

[0042] Example 3 680 g of dimethyl terephthalate (DMT, manufactured by SK Petrochemical), 430 g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 2330 g of polytetramethylene ether glycol derived from biomass resources (BioPTMG2000, number average molecular weight 2000, manufactured by Mitsubishi Chemical), 2.4 g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0 g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 200 ° C. over 200 minutes to carry out an ester exchange reaction. Next, the pressure inside the autoclave was gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245 ° C. and 1 Torr or less over 90 minutes. Further, a polymerization reaction was carried out at 245 ° C. and 1 Torr or less for 115 minutes, and a polymer with a hard segment / soft segment mass ratio of 17 / 83 (mass%) was taken out in the form of pellets. The obtained polymer was designated as the polyester elastomer of Example 3.

[0043] Example 4 840 g of dimethyl terephthalate (DMT, manufactured by SK Petrochemical), 560 g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 2150 g of polytetramethylene ether glycol derived from biomass resources (BioPTMG2000, number average molecular weight 2000, manufactured by Mitsubishi Chemical), 2.4 g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0 g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 200 ° C. over 200 minutes to carry out an ester exchange reaction. Next, the pressure inside the autoclave was gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245 ° C. and 1 Torr or less over 90 minutes. Further, a polymerization reaction was carried out at 245 ° C. and 1 Torr or less for 120 minutes, and a polymer with a hard segment / soft segment mass ratio of 24 / 76 (mass%) was taken out in the form of pellets. The obtained polymer was designated as the polyester elastomer of Example 4.

[0044] Example 5 1790g of 2,6-dimethyl naphthalene dicarboxylate (NDC, manufactured by SK Petrochemical), 1020g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 1130g of polytetramethylene ether glycol derived from biomass resources (BioPTMG1000, number average molecular weight 1000, manufactured by Mitsubishi Chemical), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220°C over 90 minutes to carry out an ester exchange reaction. The pressure inside the autoclave was then gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 90 minutes. The polymerization reaction was then carried out for 110 minutes at 245°C and 1 Torr or less, and a polymer with a hard segment / soft segment mass ratio of 56 / 44 (mass%) was taken out in pellet form. The resulting polymer was designated as the polyester elastomer of Example 5.

[0045] Example 6 1920g of 2,6-dimethyl naphthalenedicarboxylate (NDC, manufactured by SK Petrochemical), 1120g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 960g of polytetramethylene ether glycol derived from biomass resources (BioPTMG1000, number average molecular weight 1000, manufactured by Mitsubishi Chemical), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220°C over 90 minutes to carry out an ester exchange reaction. The pressure inside the autoclave was then gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 90 minutes. The polymerization reaction was then carried out for 105 minutes at 245°C and 1 Torr or less, and a polymer with a hard segment / soft segment mass ratio of 62 / 38 (mass%) was taken out in pellet form. The resulting polymer was designated as the polyester elastomer of Example 6.

[0046] Reference example 1 2000g of dimethyl terephthalate (DMT, manufactured by SK Petrochemical), 1360g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 750g of polytetramethylene ether glycol (PTMG1000, number average molecular weight 1000, manufactured by BASF), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220°C over 150 minutes to carry out an ester exchange reaction. The pressure inside the autoclave was then gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 75 minutes. A polymerization reaction was further carried out for 90 minutes at 245°C and 1 Torr or less, and a polymer with a hard segment / soft segment mass ratio of 72 / 28 (mass%) was taken out in the form of pellets. The obtained polymer was designated as the polyester elastomer of Reference Example 1.

[0047] Reference example 2 1200g of dimethyl terephthalate (DMT, manufactured by SK Petrochemical), 800g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 1780g of polytetramethylene ether glycol (PTMG1000, number average molecular weight 1000, manufactured by BASF), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220°C over 90 minutes to carry out an ester exchange reaction. The pressure inside the autoclave was then gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 90 minutes. A polymerization reaction was then carried out for 105 minutes at 245°C and 1 Torr or less, and a polymer with a hard segment / soft segment mass ratio of 33 / 67 (mass%) was taken out in the form of pellets. The obtained polymer was designated as the polyester elastomer of Reference Example 2.

[0048] Reference example 3 680g of dimethyl terephthalate (DMT, manufactured by SK Petrochemical), 430g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 2330g of polytetramethylene ether glycol (PTMG2000, number average molecular weight 2000, manufactured by BASF), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220°C over 90 minutes to carry out an ester exchange reaction. The pressure inside the autoclave was then gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 90 minutes. A polymerization reaction was further carried out for 100 minutes at 245°C and 1 Torr or less, and a polymer with a hard segment / soft segment mass ratio of 17 / 83 (mass%) was taken out in the form of pellets. The obtained polymer was designated as the polyester elastomer of Reference Example 3.

[0049] Reference example 4 840g of dimethyl terephthalate (DMT, manufactured by SK Petrochemical), 560g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 2150g of polytetramethylene ether glycol (PTMG2000, number average molecular weight 2000, manufactured by BASF), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220°C over 90 minutes to carry out an ester exchange reaction. The pressure inside the autoclave was then gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 90 minutes. A polymerization reaction was further carried out at 245°C and 1 Torr or less for 95 minutes, and a polymer with a hard segment / soft segment mass ratio of 24 / 76 (mass%) was taken out in the form of pellets. The obtained polymer was designated as the polyester elastomer of Reference Example 4.

[0050] Reference example 5 1790g of dimethyl 2,6-naphthalenedicarboxylate (NDC, manufactured by SK Petrochemical), 1020g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 1130g of polytetramethylene ether glycol (PTMG1000, number average molecular weight 1000, manufactured by BASF), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220°C over 90 minutes to carry out an ester exchange reaction. The pressure inside the autoclave was then gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 90 minutes. A polymerization reaction was further carried out at 245°C and 1 Torr or less for 90 minutes, and a polymer with a hard segment / soft segment mass ratio of 56 / 44 (mass%) was taken out in the form of pellets. The obtained polymer was designated as the polyester elastomer of Reference Example 5.

[0051] Reference example 6 1920g of 2,6-dimethyl naphthalenedicarboxylate (NDC, manufactured by SK Petrochemical), 1120g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 960g of polytetramethylene ether glycol (PTMG1000, number average molecular weight 1000, manufactured by BASF), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220°C over 90 minutes to carry out an ester exchange reaction. The pressure inside the autoclave was then gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 90 minutes. A polymerization reaction was further carried out at 245°C and 1 Torr or less for 85 minutes, and a polymer with a hard segment / soft segment mass ratio of 62 / 38 (mass%) was taken out in the form of pellets. The obtained polymer was designated as the polyester elastomer of Reference Example 6.

[0052] Comparative Example 1 2000g of dimethyl terephthalate (DMT, manufactured by SK Petrochemical), 1360g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 750g of polytetramethylene ether glycol derived from biomass resources (BioPTMG1000, number average molecular weight 1000, manufactured by Mitsubishi Chemical), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220°C over 150 minutes to carry out an ester exchange reaction. Next, the pressure inside the autoclave was gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 75 minutes. A polymerization reaction was further carried out at 245°C and 1 Torr or less for 90 minutes, and a polymer with a hard segment / soft segment mass ratio of 72 / 28 (mass%) was taken out in the form of pellets. The obtained polymer was designated as the polyester elastomer of Comparative Example 1.

[0053] Comparative Example 2 2030g of dimethyl terephthalate (DMT, manufactured by SK Petrochemical), 1460g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 840g of biomass-derived dimer diol (C36DiOH, Pripol2033 manufactured by Croda), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220°C over 110 minutes to carry out an ester exchange reaction. Next, the pressure inside the autoclave was gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 75 minutes. A polymerization reaction was further carried out at 245°C and 1 Torr or less for 55 minutes, and a polymer with a hard segment / soft segment mass ratio of 65 / 35 (mass%) was taken out in the form of pellets. The obtained polymer was used as the polyester elastomer of Comparative Example 2.

[0054] Comparative Example 3 1815g of dimethyl terephthalate (DMT, manufactured by SK Petrochemical), 1665g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 860g of dimer acid derived from biomass resources (C36DiCOOH, Propol1009 manufactured by Croda), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 220°C over 120 minutes to carry out an ester exchange reaction and an esterification reaction. Next, the pressure inside the autoclave was gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 75 minutes. A polymerization reaction was further carried out for 60 minutes at 245°C and 1 Torr or less, and a polymer with a hard segment / soft segment mass ratio of 66 / 34 (mass%) was taken out in the form of pellets. The obtained polymer was designated as the polyester elastomer of Comparative Example 3.

[0055] Comparative Example 4 2110g of dimethyl furan dicarboxylate (FDME, manufactured by BASF) derived from biomass resources, 1540g of 1,4-butanediol (1,4-BDO, manufactured by Mitsubishi Chemical), 1780g of polytetramethylene ether glycol (PTMG1000, number average molecular weight 1000, manufactured by BASF), 2.4g of tetrabutyl titanate (TBT, manufactured by Nacalai Tesque), and 6.0g of AO-330 (manufactured by ADEKA) were charged into an autoclave, and the temperature was raised from room temperature to 180°C over 120 minutes to carry out an ester exchange reaction. Next, the pressure inside the autoclave was gradually reduced and the temperature was further raised, and the initial condensation reaction was carried out at 245°C and 1 Torr or less over 75 minutes. A polymerization reaction was further carried out at 245°C and 1 Torr or less for 46 minutes, and a polymer with a hard segment / soft segment mass ratio of 71 / 29 (mass%) was taken out in the form of pellets. The obtained polymer was designated as the polyester elastomer of Comparative Example 4.

[0056] Table 1 shows the compositions and evaluation results of the polyester elastomers of Examples 1 to 6, Reference Examples 1 to 6, and Comparative Examples 1 to 4.

[0057] [Table 1]

[0058] As is clear from Table 1, all of Examples 1 to 6, in which raw materials derived from biomass resources were used for the aliphatic polyether of the soft segment, were able to almost retain the excellent flexibility, low-temperature mechanical properties, heat aging resistance, and water resistance of the fossil fuel resource-derived polyester elastomers of Reference Examples 1 to 6, in which only raw materials derived from the same fossil fuel resource were used. On the other hand, Comparative Example 1 has the same composition as Example 1, but since the conventional polycondensation time was adopted, the reduced viscosity was low and it was no longer possible to retain the various excellent properties specific to the fossil fuel resource-derived polyester elastomers. In addition, Comparative Examples 2 to 4, raw materials derived from biomass resources were used in parts other than the aliphatic polyether of the soft segment, so it was not possible to retain the various excellent properties specific to the fossil fuel resource-derived polyester elastomers. [Industrial Applicability]

[0059] The biomass resource-derived polyester elastomer of the present invention is free from coloration and can retain the excellent flexibility, low-temperature mechanical properties, heat resistance, and water resistance of fossil fuel resource-derived polyester elastomers. Therefore, the biomass resource-derived polyester elastomer of the present invention contributes greatly to solving environmental problems such as the depletion of fossil fuel resources, and is extremely useful in the industry.

Claims

[Claim 1] A polyester elastomer comprising a hard segment made of a polyester having an aromatic dicarboxylic acid and an aliphatic and / or alicyclic diol as constituent components and a soft segment made of an aromatic dicarboxylic acid and an aliphatic polyether as constituent components bonded thereto, wherein the aromatic dicarboxylic acid and the aliphatic and / or alicyclic diol are derived from a fossil fuel resource, and the aliphatic polyether is polytetramethylene ether glycol derived from a biomass resource, the bio-based content of the polyester elastomer being 20 to 85%, the reduced viscosity of the polyester elastomer being 1.2 dl / g or more, as measured at 30°C by dissolving 0.05 g of the polyester elastomer in 25 mL of a mixed solvent of phenol / tetrachloroethane = 60 / 40 and using an Ubbelohde viscometer, and the tensile elongation at break of the polyester elastomer being 550% or more, or the tensile strength at break of the polyester elastomer being 16 MPa or more (excluding the case where the aromatic dicarboxylic acid is dimethyl furandicarboxylate).