Abrasive pad and manufacturing method thereof
The polishing pad with a resin base, pores, and specific abrasive particles improves polishing efficiency and reduces scratching by using sub-specific particles to support and replenish main particles, addressing the limitations of conventional pads.
Patent Information
- Application Number
- JP2023047546
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-24
- Publication Date
- 2024-10-04
Smart Images

Figure 2024136430000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a polishing pad and a method for manufacturing the same. [Background technology]
[0002] Patent Documents 1 to 3 disclose conventional polishing pads. As shown in FIG. 9, these polishing pads have a base material 90 and numerous abrasive particles 92. The base material 90 is mainly made of resin, and has a plurality of pores 90a formed therein. Examples of the resin that can be used include polyvinylidene fluoride, epoxy resin, and PES (polyethersulfone). The abrasive particles 92 are made of silica or the like, and are held in the base material 90 or the pores 90a.
[0003] These polishing pads are manufactured through a first step, a second step, a third step, and a fourth step. In the first step, a paste containing a base resin, abrasive particles 92, and a solvent is prepared. In the second step, the paste is molded into a sheet-like molded body. In the third step, the molded body is immersed in a replacement liquid, and the solvent in the molded body is replaced with the replacement liquid to form pores 90a, thereby obtaining a replacement body. In the fourth step, the replacement liquid is removed from the replacement body, and a polishing pad is obtained. When polishing a workpiece W, the polishing pad has its front and / or back surface dressed by a dresser or the like to form a polishing surface 94.
[0004] In the polishing pad thus obtained, the abrasive particles 92 are semi-fixedly held by the base material 90, and therefore a polishing method using a CMP (Chemical Mechanical Polishing) method can be carried out while employing a polishing liquid that does not contain abrasive particles 92 or simply water as the polishing liquid. In this case, compared to a free abrasive polishing method in which a pad that does not contain abrasive particles is used and a polishing liquid that contains abrasive particles, advantageous effects such as simplified management of the polishing liquid after polishing and simplified cleaning process of the polished object after polishing can be obtained. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2011-49256 A [Patent Document 2] Patent Publication No. 2021-61306 [Patent Document 3] Patent No. 6243009 Summary of the Invention [Problem to be solved by the invention]
[0006] However, it is desired that the conventional polishing pads exhibit better polishing ability. That is, with the conventional polishing pads, it is difficult to achieve a sufficiently high polishing rate even if the polishing pressure is increased in order to increase the amount of polished material per unit time.
[0007] The present invention has been made in consideration of the above-mentioned conventional situation, and has as its object to provide a polishing pad that can exhibit superior polishing ability while maintaining the advantageous effects of a polishing pad, such as simplifying the management of the polishing liquid after polishing and simplifying the cleaning process of the polished object after polishing. [Means for solving the problem]
[0008] The polishing pad of the present invention is a polishing pad that has a base material mainly made of resin and having a plurality of pores formed therein, and a countless number of abrasive particles held in the base material or in the pores, and that constitutes a polishing surface for polishing an object to be polished, The object to be polished is made of a solid material that is amorphous, crystalline, or an amorphous-crystalline composite material; Each of the abrasive particles is characterized by including main specific particles having a chemical mechanical polishing effect on the workpiece, and sub-specific particles having a Vickers hardness greater than that of the main specific particles and equal to or less than that of the workpiece.
[0009] According to the inventors' tests, in the polishing pad of the present invention, if the polishing pressure is increased to increase the amount of polishing of the object per hour, the polishing rate is also sufficiently high. That is, when the polishing pad is moved relative to the object to be polished while pressing the object to the polishing surface with a predetermined load, the main specific particles chemically and mechanically polish the object to be polished. During this time, it is presumed that the sub specific particles support the main specific particles within the matrix or pores because they have a Vickers hardness greater than that of the main specific particles. At this time, the sub specific particles do not polish the object to be polished because their Vickers hardness is equal to or smaller than that of the object to be polished, and therefore do not cause scratches on the object to be polished.
[0010] In addition, as with the conventional polishing pads, this polishing pad also has a base material that semi-fixes the abrasive particles, so that the polishing method by the CMP method can be carried out while using a polishing liquid that does not contain abrasive particles or simply water as the polishing liquid. Therefore, when the polishing pad is used to polish an object to be polished, it is possible to achieve advantageous effects such as simplifying the management of the polishing liquid after polishing and simplifying the cleaning process of the object to be polished after polishing, compared to the case where the object is polished by the free abrasive polishing method.
[0011] Therefore, this polishing pad can simplify the management of the polishing liquid after polishing and can simplify the cleaning process of the polished object after polishing, while maintaining the advantageous effects of the polishing pad, such as being able to exhibit better polishing ability.
[0012] The method for producing a polishing pad of the present invention includes a first step of preparing a paste containing a base resin, abrasive particles, and a solvent; A second step of forming the paste into a sheet-like molded body; a third step of immersing the molded body in a replacement liquid to replace the solvent in the molded body with the replacement liquid to form pores and obtain a replacement body; and a fourth step of removing the replaced liquid from the replaced body to obtain a polishing pad having a base material mainly composed of the base material resin and having a plurality of pores formed therein, and a countless number of abrasive particles held in the base material or the pores. The abrasive particles are characterized by including main specific particles having a chemical mechanical polishing action on a solid of an amorphous, crystalline, or amorphous-crystalline composite material, and sub-specific particles having a Vickers hardness greater than that of the main specific particles and equal to or less than that of the solid.
[0013] According to the manufacturing method of the present invention, the polishing pad of the present invention can be manufactured. Effect of the Invention
[0014] According to the polishing pad of the present invention, it is possible to simplify the management of the polishing liquid after polishing, and to simplify the cleaning process of the polished object after polishing, while maintaining the advantageous effects of the polishing pad, and it is possible to exhibit a more excellent polishing ability. Furthermore, according to the manufacturing method of the present invention, it is possible to manufacture the polishing pad of the present invention. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic enlarged cross-sectional view of a polishing pad according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a graph showing the relationship between the polishing pressure and the polishing rate in the polishing methods of the examples and the comparative examples in Test 1. [Diagram 3] FIG. 3 is an enlarged cross-sectional view similar to FIG. 1, showing a polishing pad according to the embodiment. [Figure 4] FIG. 4 is an enlarged cross-sectional view of a portion of FIG. 3 relating to the polishing pad of the embodiment. [Diagram 5] FIG. 5 is a graph showing the relationship between the proportion of silica particles and the polishing rate in Test 2. [Figure 6] FIG. 6 is a graph showing the relationship between the proportion of silica particles and the surface roughness in Test 2. [Figure 7] FIG. 7 is a graph showing the relationship between the proportion of silica particles and the polishing rate in Test 3. [Figure 8] FIG. 8 is a graph showing the relationship between the proportion of silica particles and the surface roughness in Test 3. [Figure 9]FIG. 9 is a schematic enlarged cross-sectional view of a conventional polishing pad. [Figure 10] FIG. 10 is a schematic enlarged cross-sectional view of a polishing pad of a comparative example. [Figure 11] FIG. 11 is a partially enlarged cross-sectional view of FIG. 10 relating to a polishing pad of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The resin constituting the base material may be polyethersulfone (PES), polysulfone (PSU), polyvinylidene fluoride (PVDF), polyvinyl fluoride, vinyl fluoride-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer, polyethylene, polymethyl methacrylate, polycarbonate, etc. These may be used alone or in a mixture of two or more.
[0017] The solvent may be anything that dissolves the resin that constitutes the base material, and examples of the solvent that can be used include N-methyl-2-pyrrolidone, 2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, and dimethylsulfoxide.
[0018] According to the test results of the inventors, it is preferable that the sub-specific particles have a smaller diameter than the main specific particles. The main specific particles protrude from the polishing surface and contact the workpiece to perform chemical mechanical polishing on the workpiece, and it is inferred that if the sub-specific particles have a smaller diameter than the main specific particles, the main specific particles can easily contact the workpiece and perform chemical mechanical polishing on the workpiece. On the other hand, since it is sufficient for the sub-specific particles to support the main polishing particles in the base material or in the pores, it is not necessary for them to protrude from the polishing surface and contact the workpiece, and it is inferred that if the sub-specific particles have a smaller diameter than the main specific particles, it is easier to support the main polishing particles in the base material or in the pores. In other words, it is inferred that if the sub-specific particles have a larger diameter than the main specific particles, the main specific particles cannot easily contact the workpiece to perform chemical mechanical polishing on the workpiece. On the other hand, if the sub specific particles have a larger diameter than the main specific particles, the sub specific particles tend to protrude from the polishing surface and come into contact with the workpiece, but it is presumed that this is because the sub specific particles are not required for chemical mechanical polishing of the workpiece. Specifically, it is preferable that the main specific particles have a diameter of 0.06 to 1.71 μm and the sub specific particles have a diameter of 0.01 to 5.00 μm.
[0019] The inventors have confirmed the effectiveness of the present invention when the object to be polished consists of a solid amorphous, crystalline or amorphous-crystalline composite material, and each abrasive particle contains main specific particles having a CMP effect on the object to be polished, and sub-specific particles having a Vickers hardness greater than that of the main specific particles and equal to or less than that of the object to be polished.
[0020] According to the inventors' tests, specifically, the polished object can be quartz or synthetic quartz, but the polished object can also be a lithium tantalate wafer, a silicon wafer, etc. These are examples of amorphous, crystalline, or amorphous-crystalline composite solids.
[0021] The Vickers hardness (GPa) of various materials is shown in Table 1. When polishing an object to be polished, particles having a chemical mechanical polishing effect on the object to be polished are selected as the main specified particles, and particles having a Vickers hardness greater than that of the main specified particles and equal to or less than that of the solid are selected as the sub-specified particles.
[0022] [Table 1]
[0023] For example, when the object to be polished is glass containing silicon, such as quartz, synthetic quartz, soda lime glass, or borosilicate glass, at least one of ceria (cerium oxide, CeO2), red iron oxide (iron trioxide, Fe2O3), and manganese oxide (iron trioxide, Mn2O3) is adopted as the main specific particle, and silica particles are selected as the secondary specific particle. The glass may be amorphous, crystalline, or an amorphous-crystalline composite material. It is known that red iron oxide has a CMP effect on glass, for example, from "Red Iron Ore as an Abrasive" (Funahashi Wataru, Precision Machinery, 19 (1940), p. 342) and "Abrasive for Glass" (Hanawa Kenzo, NEW GLASS, Vol. 27 (2012), No. 106). The fact that manganese oxide has a CMP effect on glass is known from, for example, JP-A-10-071571, JP-A-2002-210640, JP-A-2014-084420, JP-A-2014-118468, JP-A-2015-140402, and the like.
[0024] According to the inventors' test results, when the object to be polished is quartz crystal, the polishing rate is improved if the ceria particles are 45 volume % or more and 85 volume % or less, and the silica particles are 15 volume % or more and 55 volume % or less.
[0025] It is preferable that the base material has large pores formed therein, which can be opened on the polishing surface, communicate with the plurality of pores, and have a larger volume than each of the pores. According to tests by the inventors, in this case, if the polishing pressure is increased in order to increase the amount of polishing of the workpiece per hour, the polishing rate is also sufficiently increased.
[0026] The inventors speculate that the reason why the polishing pad of the present invention can exhibit high polishing ability is due to the micro-pumping effect of the main and sub specific particles. That is, while the polishing pad polishes the workpiece by pressing the workpiece against the polishing surface with a predetermined load and moving relative to the workpiece, the main and sub specific particles are replenished from the matrix or pores into the large pores opening on the polishing surface. During this time, the main and sub specific particles remaining in the large pores opening on the polishing surface move to the polishing surface with the flow of the polishing liquid generated by the workpiece. In the polishing pad of the present invention, the main and sub specific particles existing on the polishing surface increase compared to conventional polishing pads due to this micro-pumping effect of the main and sub specific particles, and therefore the polishing ability is increased.
[0027] On the other hand, in the conventional polishing pad, as shown in FIG. 9, there are many abrasive particles 92 in the base material 90 and pores 90a. However, the abrasive particles 92 are composed of non-active abrasive particles 92a that remain in the base material 90 and pores 90a, standby abrasive particles 92b that are dressed and exposed to the polishing surface 94 but do not contribute to polishing, and active abrasive particles 92c that are dressed and exposed to the polishing surface 94 and contribute to polishing. The non-active abrasive particles 92a that remain in the base material 90 and pores 90a are difficult to move to the polishing surface 94, the standby abrasive particles 92b are few, and only the active abrasive particles 92c exert a chemical mechanical polishing effect on the workpiece W. For this reason, even if the conventional polishing pad polishes the workpiece W by moving relative to the workpiece W while pressing the workpiece W against the polishing surface 94 with a predetermined load, the active abrasive particles 92c present on the polishing surface 94 are difficult to replenish. Therefore, in the conventional polishing pad, the number of active abrasive particles 92c present on the polishing surface 94 is smaller than that of the polishing pad of the present invention, and the polishing ability is low.
[0028] In the first step, the base resin, the main specified particles, the sub specified particles, and the solvent may be mixed at the same time to form a paste, but the first step preferably includes the following first, second, and third mixing steps. The first mixing step obtains a first paste containing the main specified particles and the solvent. The second mixing step obtains a second paste containing the sub specified particles and the solvent. The third mixing step obtains a paste containing the base resin, the first paste, and the second paste. This makes it easier to generate pores that hold the main specified particles and pores that hold the sub specified particles, making it easier for the sub specified particles to support the main specified particles and for a micropumping effect to occur.
[0029] In the first step, additives may be added to the paste as necessary, such as glycerin for adjusting the solubility of the resin in the solvent.
[0030] The second step is not particularly limited, and is performed by forming the mixture into a sheet-like molded product using a molding device such as a T-die. The molding method is not limited to this method as long as it can achieve a uniform thickness to a certain extent.
[0031] In the third step, the paste preferably contains a pore-forming agent capable of forming numerous large pores that are connected to the multiple pores and have a larger volume than each of the pores. This makes it possible to manufacture a polishing pad that produces a micro-pumping effect. When an aqueous replacement liquid is used, a water-soluble pore-forming agent can be used. Examples of water-soluble pore-forming agents that can be used include powdered sugar made by grinding granulated sugar into a powder, cornstarch, and the like. The size of the large pores can be adjusted by adjusting the particle size of the pore-forming agent.
[0032] In the third step, for example, the molded body is immersed in a water tank filled with temperature-controlled ion-exchanged water for a predetermined time to cause a nucleation-growth type phase separation process. This results in a large number of isolated, spherical, irregularly sized and positioned relative to one another, abrasive-particle-containing solvent-rich phases being dispersed in the resin-rich phase. During this process, the solvent in the solvent-rich phase is replaced by water by diffusing into the replacement liquid.
[0033] In this way, in the third step, when an aqueous solvent is used, an aqueous liquid such as ion-exchanged water is used as the replacement liquid, and the molded body is immersed in the replacement liquid to disperse the solvent-rich phase in the resin-rich phase through a nucleation-growth type phase separation process, and at the same time, the solvent in the solvent-rich phase is replaced with the replacement liquid to remove the solvent from the molded body. At this time, each isolated solvent-rich phase is communicated with the outside of the molded body through the pores formed in the resin-rich phase, and the solvent is replaced with the replacement liquid through the pores. When the solvent is removed from the molded body in this way, the resin-rich phase shrinks and hardens, and fine continuous pores are formed in the resin-rich phase. In addition, by using an aqueous liquid such as ion-exchanged water as the replacement liquid and immersing the molded body in the replacement liquid, the water-soluble pore-forming agent can also be removed at the same time.
[0034] The molded body from which the solvent and pore-forming agent have been removed is made into a polishing pad through a fourth step. When polishing an object to be polished, the polishing pad has its front and / or back surface dressed with a dresser or the like to form a polishing surface.
[0035] (Test 1) <1st process> The following base resin, abrasive particles (specific main particles, specific sub particles), solvent and pore-forming agent were prepared.
[0036] (Base resin) PES (Polyethersulfone) (abrasive particles, main specific particles) Ceria particles (average particle size: 0.75 μm) (abrasive particles, secondary specific particles) Silica particles (average particle size: 0.25 μm) (solvent) N-Methyl-2-pyrrolidone (pore forming agent) Granulated sugar powder
[0037] The above-mentioned base resin, abrasive particles, solvent and pore forming agent were mixed in the mixing ratio (parts by mass) of Table 2. In the examples, first, in the first mixing step, ceria particles as the main specific particles were dispersed in the solvent to obtain a first paste. In the second mixing step, silica particles as the sub specific particles were dispersed in the solvent to obtain a second paste. In the second mixing step, the base resin, the first paste and the second paste were mixed to obtain a paste. On the other hand, in the comparative examples, first, ceria particles as the main specific particles were dispersed in the solvent, and this dispersion and the pore forming agent were mixed into the base resin. In this way, each paste of the examples and comparative examples was obtained.
[0038] [Table 2]
[0039] <Second process> Each of the obtained pastes was used to obtain sheet-shaped molded bodies of the Examples and Comparative Examples using a T-die.
[0040] <3rd process> Each molded body was immersed in ion-exchanged water stored in a water tank and adjusted in temperature for a predetermined time. This caused a nucleation-growth type phase separation process in each molded body, dispersing a large number of spherical, isolated solvent-rich phases in the resin-rich phase, and replacing the solvent in each molded body with ion-exchanged water to remove the solvent from each molded body. In the molded bodies of the examples and comparative examples, the pore-forming agent was also removed at this time. In this way, each substituted body was obtained.
[0041] <4th process> The resulting substituted bodies were left in the air at room temperature for about 2 days to remove moisture from the substituted bodies, thereby obtaining polishing pads for the Examples and Comparative Examples. Each polishing pad was a disk shape with a diameter of 300 mm and a thickness of 2 mm.
[0042] The surfaces of the polishing pads of the examples and comparative examples are dressed with a dresser to form a polishing surface 14 for polishing an object to be polished W, as shown in Figures 1 and 10. The dresser has #400 diamond pellets.
[0043] 1, the polishing pad of the embodiment has a base material 10, main specific particles 12, and sub specific particles 13. The base material 10 is made of resin, and has a plurality of pores 10a, 10b, and a plurality of large pores 10c formed therein. The main specific particles 12 are mainly held in the pores 10a, and the sub specific particles 13 are mainly held in the pores 10b.
[0044] As shown in Fig. 10, the polishing pad of the comparative example has a base material 10 and main specific particles 12. The base material 10 is made of resin and has a plurality of pores 10a and a plurality of large pores 10c formed therein. The main specific particles 12 are held in the pores 10a.
[0045] The volume percentages of the resin, abrasive particles, pores 10a, 10b and large pores 10c in the polishing pads of the examples and comparative examples are as shown in Table 3. Table 3 also shows the durometer hardness (D scale) of the polishing pads of the examples and comparative examples.
[0046] [Table 3]
[0047] Two minutes after forming the polishing surface 14 on the polishing pads of the Example and Comparative Example, a polishing test was performed under the following conditions to examine the relationship between the polishing pressure (kPa) and the polishing rate (μm / min). The polishing test using the polishing pad of the Example was the polishing method of the Example, and the polishing test using the polishing pad of the Comparative Example was the polishing method of the Comparative Example. The results are shown in FIG. 2. Equipment: Engis EJW-380 (φ380 single-sided polishing machine) Workpiece to be polished (W): 1 piece of quartz (φ100mm x thickness 0.5mm) Plate rotation speed: 60 rpm Rotation speed of work W: 60 rpm Test duration: 30 minutes Polishing liquid: tap water (10ml / min) Polishing pressure: 20(kPa), 20(kPa), 30(kPa)
[0048] As is clear from Fig. 2, the polishing method of the embodiment achieves a higher polishing rate than the polishing method of the comparative example. In addition, in the polishing method of the embodiment, the polishing rate increases as the polishing pressure increases. In contrast, in the polishing method of the comparative example, the polishing rate remains low and almost flat even when the polishing pressure is increased.
[0049] 3, in the polishing pad of the embodiment, while the workpiece W is polished by moving relative to the workpiece W while pressing the workpiece W against the polishing surface 14 with a predetermined load, the main specific particles 12 and the sub specific particles 13 are replenished from the base material 10 or the pores 10a, 10b into the large pores 10c opening to the polishing surface 14. During this time, the main specific particles 12 and the sub specific particles 13 remaining in the large pores 10c opening to the polishing surface 14 are carried by the flow of the polishing liquid generated by the workpiece W and move to the polishing surface 14.
[0050] That is, in the polishing method of the embodiment, the main specific particles 12 are composed of unacted main specific particles 12a that remain held in the base material 10 or the pores 10a, standby main specific particles 12b that are replenished from the base material 10 or the pores 10a into the large holes 10c and remain in the large holes 10c, and acting main specific particles 12c that move from the large holes 10c to the polishing surface 14. The secondary specific particles 13 are composed of unacted secondary specific particles 13a that remain held in the base material 10 or the pores 10c, standby secondary specific particles 13b that are replenished from the base material 10 or the pores 10b into the large holes 10c and remain in the large holes 10c, and acting secondary specific particles 13c that move from the large holes 10c to the polishing surface 14.
[0051] When the polishing pad of the embodiment is moved relative to the workpiece W while pressing the workpiece W against the polishing surface 14 with a predetermined load, the main action specific particles 12c chemically and mechanically polish the workpiece W, as shown in Fig. 4. During this time, since the action sub specific particles 13c have a Vickers hardness greater than that of the main action specific particles 12c, it is presumed that the main action specific particles 12c are supported within the base material 10 or the pores 10a, 10b. At this time, since the Vickers hardness of the action sub specific particles 13c is equal to or smaller than that of the workpiece W, even if the action sub specific particles 13c come into contact with the workpiece W, they do not polish the workpiece W and do not cause scratches on the workpiece W.
[0052] In the polishing method of the embodiment, due to this micro-pumping effect of the main specific particles 12 and the sub specific particles 13, the acting main specific particles 12c present on the polishing surface 14 are successively replenished and increased by the standby main specific particles 12b, and the acting sub specific particles 13c present on the polishing surface 14 are successively replenished and increased by the standby sub specific particles 13b, thereby improving the polishing ability compared to conventional polishing pads.
[0053] In addition, since the polishing pad of the comparative example has large pores 10c in the base material 10 and has a micro-pumping effect of the main specific particles 12, the amount of the acting main specific particles 12c present on the polishing surface 14 increases compared to conventional polishing pads. However, since it does not have the acting sub specific particles 13c as shown in Figure 11, it is presumed that the acting main specific particles 12c are easily embedded in the base material 10 or the pores 10a, 10b.
[0054] Moreover, since the above results were obtained using ceria particles with an average particle size of 0.75 μm and silica particles with an average particle size of 0.25 μm, it is understood that the sub specific particles 13 preferably have a smaller diameter than the main specific particles 12. If the sub specific particles 13 are smaller than the main specific particles 12, they tend to get under the main specific particles 12, increasing the effect of strongly pressing the main specific particles 12. It is desirable for the size of the sub specific particles 13 to be half or less, and preferably one-third or less, of the diameter of the main specific particles 12.
[0055] (Test 2) The above base resin, abrasive particles, solvent and pore-forming agent components were mixed in the mixing ratios (parts by mass) shown in Table 4 to obtain pastes for test samples 1 to 5 in the same manner as in Test 1. Then, polishing pads for test samples 1 to 5 were obtained in the same manner as in Test 1.
[0056] [Table 4]
[0057] The volume percentages of the resin, abrasive particles, pores 10a, 10b and large pores 10c in the polishing pads of test samples 1 to 5 are as shown in Table 5. Table 5 also shows the durometer hardness (D scale) of the polishing pads of test samples 1 to 5.
[0058] [Table 5]
[0059] Two minutes after forming the polishing surface 14 on the polishing pads of test pieces 1 to 5, a polishing test similar to that of test 1 was conducted to investigate the relationship between the polishing pressure (kPa), the percentage (volume %) of silica particles, and the polishing rate (μm / min), as well as the relationship between the polishing pressure (kPa), the percentage (volume %) of silica particles, and the surface condition of the workpiece W after processing. The surface condition of the workpiece W after processing was evaluated by the surface roughness Sa (nm). The results are shown in Figure 5, Figure 6, Table 6, and Table 7.
[0060] [Table 6]
[0061] [Table 7]
[0062] 5, 6, Tables 6 and 7 show that when the workpiece W is quartz, if the ceria particles as the main specific particles 12 are 45 vol% or more and 85 vol% or less, and the silica particles as the sub specific particles 13 are 15 vol% or more and 55 vol% or less, the polishing rate improves regardless of the polishing pressure. It is also shown that within these ranges, the surface condition of the workpiece W after processing is good regardless of the polishing pressure.
[0063] (Test 3) The above base resin, abrasive particles, solvent and pore-forming agent components were mixed in the mixing ratios (parts by mass) in Table 8 to obtain pastes for test samples 6 to 8 in the same manner as in Test 1. Then, polishing pads for test samples 6 to 8 were obtained in the same manner as in Test 1.
[0064] [Table 8]
[0065] The volume percentages of the resin, abrasive particles, pores 10a, 10b, and large pores 10c in the polishing pads of test samples 6 to 8 are as shown in Table 9. Table 9 also shows the durometer hardness (D scale) of the polishing pads of test samples 6 to 8.
[0066] [Table 9]
[0067] Two minutes after forming the polishing surface 14 on the polishing pads of test pieces 6 to 8, a polishing test similar to that of test 1 was conducted. The workpiece W was synthetic quartz. The polishing pressure was 20 kPa. Then, the relationship between the percentage (volume %) of silica particles and the polishing rate (μm / min) and the relationship between the percentage (volume %) of silica particles and the surface condition of the workpiece W after processing were investigated. The results are shown in Figs. 7 and 8 and Table 10. Figs. 7 and 8 also show the results of test 2 in which the polishing pressure was set to 20 kPa.
[0068] [Table 10]
[0069] 7, 8 and Table 10 show that when the workpiece W is synthetic quartz instead of quartz, the polishing rate improves if the silica particles, which are the sub specific particles 13, are 0 to 60 volume %. Also, within this range, the surface condition of the workpiece W after processing is good regardless of the polishing pressure.
[0070] From the above, it is understood that the polishing pad of the embodiment can exhibit a superior polishing ability while maintaining the advantageous effects of the polishing pad, such as simplifying the management of the polishing liquid after polishing and simplifying the cleaning process of the polished object W after polishing. It is also understood that the polishing pad of the embodiment can be manufactured by the above manufacturing method.
[0071] In the above, the present invention has been described in accordance with Tests 1 to 3. However, the present invention is not limited to the above Tests 1 to 3 or Examples, and it goes without saying that the present invention can be modified and applied as appropriate within the scope of the invention. [Industrial Applicability]
[0072] The present invention can be used in a method for polishing solids of amorphous, crystalline or amorphous-crystalline composite materials. [Explanation of symbols]
[0073] 10...Base material 10a, 10b...pores 14...Polished surface 12...Abrasive particles, main specific particles (12a...unacted main specific particles, 12b...standby main specific particles, 12c...acting main specific particles) 13...Abrasive particles, sub-specific particles (13a...unacted sub-specific particles, 13b...standby sub-specific particles, 13c...active sub-specific particles) W: Workpiece to be polished 10c…Large hole
Claims
1. A polishing pad having a base material mainly made of resin and having a plurality of pores formed therein, and a countless number of abrasive particles held in the base material or in the pores, and constituting a polishing surface for polishing an object to be polished, The object to be polished is made of a solid material that is amorphous, crystalline, or an amorphous-crystalline composite material; A polishing pad characterized in that each of the abrasive particles includes main specific particles having a chemical mechanical polishing effect on the object to be polished, and sub-specific particles having a Vickers hardness greater than that of the main specific particles and equal to or less than that of the object to be polished.
2. 2. The polishing pad according to claim 1, wherein the secondary specific particles have a smaller diameter than the primary specific particles.
3. 3. The polishing pad according to claim 2, wherein the main specific particles have a size of 0.06 to 1.71 μm, and the sub specific particles have a size of 0.01 to 5.00 μm.
4. The object to be polished is quartz crystal or synthetic quartz, 3. The polishing pad according to claim 1, wherein the primary specific particles are ceria particles and the secondary specific particles are silica particles.
5. The ceria particles are 45% by volume or more and 85% by volume or less, 5. The polishing pad according to claim 4, wherein the silica particles are present in an amount of 15 volume % or more and 55 volume % or less.
6. the base material is formed with large pores that can be opened on the polishing surface, communicate with the plurality of pores, and have a larger volume than each of the pores; 2. The polishing pad according to claim 1, wherein while the polished object is polished by pressing the polished object against the polishing surface with a predetermined load and moving relative to the polished object, the main specific particles and the sub specific particles are replenished into the large pores from the base material or the pores, and the main specific particles and the sub specific particles remaining in the large pores move to the polishing surface.
7. A first step of preparing a paste containing a base resin, abrasive particles, and a solvent; A second step of forming the paste into a sheet-like molded body; a third step of immersing the molded body in a replacement liquid to replace the solvent in the molded body with the replacement liquid to form pores and obtain a replacement body; and a fourth step of removing the replacement liquid from the replacement body to obtain a polishing pad having a base material mainly composed of the base material resin and having a plurality of pores formed therein, and a countless number of abrasive particles held in the base material or the pores. A method for manufacturing a polishing pad, characterized in that each of the abrasive particles includes a main specific particle having a chemical mechanical polishing action on a solid of an amorphous, crystalline, or amorphous-crystalline composite material, and a sub-specific particle having a Vickers hardness greater than that of the main specific particle and equal to or less than that of the solid.
8. The first step includes a first mixing step of obtaining a first paste including the main specific particles and the solvent; a second mixing step of obtaining a second paste containing the sub specific particles and the solvent; 8. The method for producing a polishing pad according to claim 7, further comprising a third mixing step of obtaining the paste containing the base resin, the first paste and the second paste.
9. 9. The method for manufacturing a polishing pad according to claim 7, wherein the paste contains a pore-forming agent capable of forming in the third step numerous large pores that are in communication with the pores and have a larger volume than each of the pores.
Citation Information
Patent Citations
Polishing molding, polishing level block and polishing method using this polishing molding
JP1999216676A
Polishing cloth for semiconductor wafer, and polishing method of semiconductor wafer using the polishing cloth
JP2002231669A
Polishing element and method for manufacturing the same
JP2011049256A
Polishing sheet, polishing tool, and polishing method
JP2016140930A
Polymer polishing pad containing polishing particle
KR1020030049768A
Cited By
Method for manufacturing a glass polishing body, glass polishing body, glass polishing method, and glass polishing apparatus
JP2026134649A