Recording method

The recording method improves texture and productivity by forming layers with pigment ink and a treatment liquid on a transfer medium, then thermally transferring the image, addressing issues of texture impairment and space requirements in existing methods.

JP2024136674APending Publication Date: 2024-10-04SEIKO EPSON CORP

Patent Information

Application Number
JP2023047860
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

Smart Images

  • Figure 2024136674000001
    Figure 2024136674000001
  • Figure 2024136674000002
    Figure 2024136674000002
  • Figure 2024136674000003
    Figure 2024136674000003
Patent Text Reader

Abstract

To provide a recording method which can stably manufacture a recorded matter excellent in feeling and washing fastness, while suppressing the increase in the size of a manufacturing apparatus, by using an inkjet method.SOLUTION: A recording method includes the steps of: discharging pigment ink containing a pigment and water onto a transfer medium having a peeling layer from an inkjet head, and forming a first layer; discharging a treatment liquid from the inkjet head, and forming a second layer so as to overlap the first layer; heating a surface where the first layer and the second layer of the transfer medium are formed in a state of opposed to an absorptive transferred medium, and thereby thermally transferring the first layer and the second layer onto the transferred medium, wherein a content of the resin in the pigment ink is 15.0 mass% or less, the treatment liquid contains a resin and water, and a drying rate of the first layer when the treatment liquid is discharged is 0% or more and 80% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a recording method. [Background technology]

[0002] A transfer printing method is known in which a transfer sheet, which is a transfer medium on which an image is formed, is superimposed on a transfer medium such as a fabric, and the image is transferred to the transfer medium by applying heat and pressure. In such a method, when forming an image on the transfer sheet, an inkjet method is often used because it is advantageous in forming a fine image with high on-demand performance. In addition, when an absorbent transfer medium such as fabric or leather is used, washing fastness is also required.

[0003] In the transfer printing method described above, an image is generally formed on a transfer sheet having a release layer and a hot melt layer formed on the entire surface of a substrate, and then the transfer sheet is heated and pressed to a medium to be transferred.

[0004] However, in the recorded matter produced by such a method, the hot melt layer is transferred to the transfer medium together with the image, and the hot melt layer is formed on the transfer medium in areas other than the image, which causes a problem that the texture of the transfer medium is damaged. In particular, when the recorded matter is clothing, there is a problem that it is likely to cause discomfort to the wearer.

[0005] In order to solve the problems described above, a method has been proposed in which an image is formed on the surface of a transfer sheet using ink containing a pigment, a heat-melting powder is then sprinkled onto the surface of the transfer sheet so that the powder adheres to the entire surface of the ink without any gaps, the powder is removed from the non-image-forming areas, the transfer sheet is superimposed on an object to be transferred (the transfer medium), and the image-forming areas are heated and pressurized at a temperature at which the powder melts, thereby transferring the image from the transfer sheet to the object to be transferred (see Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2019-171840 A Summary of the Invention [Problem to be solved by the invention]

[0007] Although this method is somewhat improved compared to the method using a transfer sheet with a hot melt layer on the entire surface, it still does not provide a satisfactory texture. In addition, this method requires an image forming device that forms an image on the transfer sheet by the inkjet method, a transfer device that transfers the image by heating and pressing, and a space for manually sprinkling the powder or installing a powder sprinkling device, which causes a problem that the space required for producing the recorded product becomes large. In addition, a process is required to shake off or suck out the powder sprinkled on the transfer sheet that is not attached to the image, making it difficult to increase the productivity of the recorded product. [Means for solving the problem]

[0008] The present invention has been made to solve the above-mentioned problems, and can be realized as the following application examples.

[0009] A recording method according to an application example of the present invention includes a first layer forming step of forming a first layer by ejecting a pigment ink containing a pigment and water from an inkjet head onto a transfer medium having a release layer; a second layer forming step of ejecting a treatment liquid from an inkjet head to form a second layer so as to overlap the first layer; a thermal transfer step of thermally transferring the first layer and the second layer to an image-receiving medium by heating the surface of the transfer medium on which the first layer and the second layer are formed while the surface is opposed to the image-receiving medium having an absorbent property; The content of the resin in the pigment ink is 15.0% by mass or less, The treatment liquid contains a resin and water, The first layer has a drying rate of 0% or more and 80% or less when the treatment liquid is discharged.

[0010] A recording method according to another application example of the present invention includes a first layer forming step of ejecting a pigment ink containing a pigment, a resin having a glass transition temperature of −40° C. or more and 0° C. or less, an organic solvent having a boiling point of 280° C. or more, and water from an inkjet head onto a transfer medium having a release layer, to form a first layer; a second layer forming step of ejecting a treatment liquid from an inkjet head to form a second layer so as to overlap the first layer; a thermal transfer step of thermally transferring the first layer and the second layer to an absorbent medium, such as fabric or leather, by heating the surface of the transfer medium on which the first layer and the second layer are formed, while the surface is opposed to the absorbent medium, such as fabric or leather; the content of the resin in the pigment ink is 2.0% by mass or more and 15.0% by mass or less, the treatment liquid contains a resin having a glass transition temperature of -20°C or more and 50°C or less and a melting point of 80°C or more and 140°C or less, and water, but does not contain an organic solvent having a boiling point of 280°C or more; the resin contained in the treatment liquid is at least one selected from the group consisting of polyester, polyurethane, and polyvinyl chloride; The content of the resin in the treatment liquid is 5.0% by mass or more and 20.0% by mass or less, The first layer has a drying rate of 0% or more and 80% or less when the treatment liquid is discharged. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a process diagram showing a preferred embodiment of the recording method of the present invention. [Diagram 2] FIG. 2 is a table showing the compositions of the pigment inks of Preparation Examples A1 to A5. [Diagram 3] FIG. 3 is a table showing the compositions of the treatment liquids of Preparation Examples B1 to B5. [Figure 4] FIG. 4 is a table showing all the conditions of the recording methods in Examples 1 to 12. [Diagram 5] FIG. 5 is a table showing all the conditions of the recording method in Examples 13 to 19 and Comparative Examples 1 to 4. [Figure 6] FIG. 6 is a table showing the evaluation results of Examples 1 to 12. [Figure 7] FIG. 7 is a table showing the evaluation results of Examples 13 to 19 and Comparative Examples 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Preferred embodiments of the present invention will now be described in detail. [1] Recording method First, the recording method of the present invention will be described. FIG. 1 is a process diagram showing a preferred embodiment of the recording method of the present invention.

[0013] The recording method of the present invention includes a first layer forming step (1a) of ejecting a pigment ink 2' containing a pigment and water from an inkjet head 50 onto a transfer medium 1 having a peelable layer 12 to form a first layer 2, a second layer forming step (1b) of ejecting a treatment liquid 3' from the inkjet head 50' to form a second layer 3 so as to overlap the first layer 2, and a thermal transfer step (1c) of thermally transferring the first layer 2 and the second layer 3 onto an absorbent transfer-receiving medium 5 by heating the surface of the transfer medium 1 on which the first layer 2 and the second layer 3 have been formed while facing the transfer-receiving medium 5. The content of resin in the pigment ink 2' is 15.0% by mass or less, the treatment liquid 3' contains a resin and water, and the drying rate of the first layer 2 when ejecting the treatment liquid 3' is 0% or more and 80% or less.

[0014] With this configuration, it is possible to provide a recording method that uses an inkjet method to stably produce a recorded matter 100 that is excellent in texture, color development of the recording part 4, and washing fastness while suppressing an increase in size of the production equipment. Furthermore, by using a pigment ink 2' containing water and a pigment, it is possible to utilize, for example, a small and inexpensive inkjet recording device for water-based pigment ink that is widely used for home use, which is particularly advantageous in terms of providing a low-cost and simple recording method.

[0015] Such excellent effects are obtained for the following reasons. That is, according to the recording method of the present invention, since there is no need to sprinkle powder and no need to remove excess powder, a recorded matter can be produced in a narrow space with excellent productivity. In addition, since a pigment is used, a recorded matter with excellent color development can be suitably formed. In addition, in the present invention, a treatment liquid containing resin and water is applied so as to overlap with a first layer formed using a pigment ink before the first layer is excessively dried, and a second layer is formed, so that the recorded matter formed on the transfer medium is in a state in which the pigment and the resin are appropriately mixed, and when transferred to the transfer medium, a part of the mixture containing the pigment and the resin is easily and suitably permeated into the absorbent transfer medium. For this reason, the recorded matter after transfer has excellent adhesion to the transfer medium and excellent fastness to washing, and the texture of the produced recorded matter is also excellent. In addition, by making the content of the resin in the pigment ink equal to or less than a predetermined value, the inkjet method provides excellent ejection stability and suppresses clogging of the inkjet head nozzles, thereby reducing the maintenance work required for clearing clogging of the nozzles, enabling stable production of excellent recorded material and improving productivity of recorded material. Even if clogging of the inkjet head nozzles occurs, the inkjet head nozzles can be suitably restored by cleaning or the like.

[0016] On the other hand, if the above conditions are not met, satisfactory results will not be obtained. For example, when a dye is used instead of a pigment, the color development of the recorded portion cannot be made sufficiently excellent.

[0017] In addition, when a powder made of hot melt resin is used instead of the treatment liquid, the size of the recording material production device increases, the space required for producing the recording material increases, and the productivity of the recording material decreases. In addition, the texture of the recording material produced cannot be made sufficiently excellent. In this specification, the hot melt resin refers to a resin having a melting point of 100°C or more and 160°C or less and a glass transition temperature of 0°C or more and 50°C or less.

[0018] Furthermore, if the content of the resin in the pigment ink is too high, the ejection stability of the pigment ink when used in an inkjet method decreases, making it difficult to stably produce recorded matter. Also, the texture of the produced recorded matter decreases.

[0019] Furthermore, if the drying rate of the first layer when the treatment liquid is ejected is too high, the adhesion of the recording area to the transfer medium cannot be made sufficiently excellent, and the washing fastness of the recorded matter will be poor.

[0020] In the present invention, the absorbent transfer medium is a medium that is absorbent within 30 msec from the start of contact in the Bristow method. 1 / 2 Water absorption up to 10mL / m 2 This refers to a transfer medium that is more absorbent than the surface of the paper. The Bristow method is the most widely used method for measuring the amount of liquid absorbed in a short period of time, and is also used by the Japan Pulp and Paper Technology Association (JAPAN TAPPI). Details of the test method are described in Standard No. 51 "Paper and paperboard - Liquid absorbency test method - Bristow method" of the "JAPAN TAPPI Paper and Pulp Test Method 2000 Edition".

[0021] In the present invention, the drying rate of the first layer refers to the proportion of the liquid components removed by drying out of all the liquid components contained in the pigment ink used to form the first layer. Such a drying rate can be obtained by measuring the mass of the transfer medium to which the pigment ink is attached.

[0022] [1-1] First layer formation process In the first layer formation step, a pigment ink 2' containing a pigment and water is discharged from an inkjet head 50 onto a transfer medium 1 having a release layer 12 to form a first layer 2 (1a).

[0023] [1-1-1] Transfer media The transfer medium 1 may be any medium having a release layer 12, but in this embodiment, it has a substrate 11 and a release layer 12. This makes the transfer medium 1 easier to handle.

[0024] The shape of the transfer medium 1 is not particularly limited, but a sheet-like one is preferably used, which allows the first layer 2 and the second layer 3 to be more suitably formed by the inkjet method.

[0025] Examples of materials that may be used for the substrate 11 include paper, plastic materials, and metal materials.

[0026] Examples of the plastic material constituting the substrate 11 include polyesters such as polyethylene terephthalate, and polyolefins such as polyethylene and polypropylene.

[0027] The substrate 11 may be in any shape, but is preferably in the form of a sheet. When the substrate 11 is in a sheet form, the thickness of the substrate 11 is preferably 50 μm or more and 200 μm or less.

[0028] The release layer 12 is a layer having releasability. By having the release layer 12 in the transfer medium 1, it is possible to suitably prevent the constituent materials of the first layer 2 and the second layer 3 from unintentionally remaining on the transfer medium 1 after the thermal transfer process.

[0029] Examples of materials constituting the release layer 12 include polyethylene wax-based release agents, silicone-based release agents, and fluorine-based release agents.

[0030] The thickness of the release layer 12 is not particularly limited, but is preferably 5 μm or more and 80 μm or less, and more preferably 10 μm or more and 50 μm or less.

[0031] [1-1-2] Pigment ink The pigment ink 2' contains a pigment and water. The content of the resin in the pigment ink 2' is 15.0% by mass or less.

[0032] In this way, by making the content of the resin in the pigment ink 2' sufficiently small, it is possible to provide excellent ejection stability of the pigment ink 2' by the inkjet method, and to stably produce the recorded matter 100. In addition, it is possible to provide the recorded matter 100 to have an excellent texture.

[0033] [1-1-2-1] Pigments Various inorganic pigments and organic pigments can be used as the pigment contained in the pigment ink 2'. The pigment may be a combination of two or more components.

[0034] Examples of inorganic pigments include carbon blacks such as furnace black, lamp black, acetylene black, and channel black, iron oxide, and titanium oxide.

[0035] Examples of organic pigments include azo pigments such as insoluble azo pigments, condensed azo pigments, azo lakes, and chelate azo pigments; polycyclic pigments such as phthalocyanine pigments, perylene and perinone pigments, anthraquinone pigments, quinacridone pigments, dioxane pigments, thioindigo pigments, isoindolinone pigments, and quinophthalone pigments; dye chelates such as basic dye type chelates and acid dye type chelates; dye lakes such as basic dye type lakes and acid dye type lakes; nitro pigments, nitroso pigments, aniline black, and daylight fluorescent pigments.

[0036] More specifically, examples of carbon black used as black pigments include No. 2300, No. 900, MCF88, No. 33, No. 40, No. 45, No. 52, MA7, MA8, MA100, No. 2200B, etc. (all manufactured by Mitsubishi Chemical Corporation), Raven 5750, Raven 5250, Raven 5000, Raven 3500, Raven 1255, Raven 700, etc. (all manufactured by Columbia Carbon Corporation), Rega1 400R, Rega1 330R, Rega1 660R, Mogul L, Monarch 700, Monarch 800, Monarch 880, Monarch 900, Monarch 1000, Monarch 1100, Monarch 1300, Monarch 1400, etc. (all manufactured by Cabot Corporation), Color Black FW1, Color Black FW2, Color Black FW2V, Color Black FW18, Color Black FW200, Color Black S150, Color Black S160, Color Black S170, Printex 35, Printex U, Printex V, Printex 140U, Special Black 6, Special Black 5, Special Black 4A, Special Black 4 (all manufactured by Degussa), etc.

[0037] Examples of white pigments include CI Pigment White 6, 18, 21, and the like.

[0038] Examples of yellow pigments include CI Pigment Yellow 1, 2, 3, 4, 5, 6, 7, 10, 11, 12, 13, 14, 16, 17, 24, 34, 35, 37, 53, 55, 65, 73, 74, 75, 81, 83, 93, 94, 95, 97, 98, 99, 108, 109, 110, 113, 114, 117, 120, 124, 128, 129, 133, 138, 139, 147, 151, 153, 154, 167, 172, and 180.

[0039] Examples of red-purple pigments include CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 14, 15, 16, 17, 18, 19, 21, 22, 23, 30, 31, 32, 37, 38, 40, 41, 42, 48(Ca), 48(Mn), 57(Ca), 57:1, 88, 112, 114, 122, 123, 144, 146, 149, 150, 166, 168, 170, 171, 175, 176, 177, 178, 179, 184, 185, 187, 202, 209, 219, 224, and 245, and CI Pigment Violet. Examples include 19, 23, 32, 33, 36, 38, 43, and 50.

[0040] Examples of indigo purple pigments include CI Pigment Blue 1, 2, 3, 15, 15:1, 15:2, 15:3, 15:34, 15:4, 16, 18, 22, 25, 60, 65, and 66, and CI Bat Blue 4 and 60.

[0041] Examples of pigments other than the above include CI Pigment Green 7 and 10, CI Pigment Brown 3, 5, 25 and 26, and CI Pigment Orange 1, 2, 5, 7, 13, 14, 15, 16, 24, 34, 36, 38, 40, 43 and 63.

[0042] The pigment ink 2' may contain a self-dispersing pigment as the pigment. The self-dispersing pigment has a hydrophilic group on its surface, and examples of the hydrophilic group include -OM, -COOM, -CO-, -SO3M, -SO2M, -SON2NH2, -RSO2M, -PO3HM, -PO3M2, -SON2NHCOR, -NH3, and -NR3. In the formula, M represents a hydrogen atom, an alkali metal, ammonium, or an organic ammonium, and R represents an alkyl group having 1 to 12 carbon atoms or a naphthyl group which may have a substituent. In addition, for example, a phenyl group may be present between the pigment surface and the hydrophilic group.

[0043] The self-dispersing pigment can be produced, for example, by subjecting the pigment to a physical or chemical treatment to bond a hydrophilic group to the surface of the pigment. An example of such a physical treatment is vacuum plasma treatment. An example of a chemical treatment is wet oxidation in which the pigment is oxidized with an oxidizing agent in water.

[0044] As the self-dispersing pigment, for example, a self-dispersing pigment that has been surface-treated by oxidation treatment with hypohalous acid and / or hypohalite, oxidation treatment with ozone, or oxidation treatment with persulfuric acid and / or persulfate is preferable in terms of high color development. As the self-dispersing pigment, a commercially available product can also be used, and preferred examples include Microjet CW1 (manufactured by Orient Chemical Industry Co., Ltd.), CAB-O-JET250C, CAB-O-JET260M, CAB-O-JET270Y, CAB-O-JET444MP (all manufactured by Cabot Corporation), etc.

[0045] The pigment content in the pigment ink 2' is not particularly limited, but is preferably from 1.0% to 25.0% by mass, more preferably from 2.0% to 20.0% by mass, and even more preferably from 5.0% to 15.0% by mass.

[0046] This makes it easier to ensure sufficient color density in the recording area 4 formed using the pigment ink 2', and improves the color development on the transfer medium, while also improving the storage stability of the pigment ink 2', the ejection stability by the inkjet method, and the clogging recovery ability of the inkjet head.

[0047] [1-1-2-2]Water The pigment ink 2' contains water. Water is a component that functions as a dispersion medium for dispersing the pigment in the pigment ink 2'.

[0048] The water content in the pigment ink 2' is preferably 50.0% by mass to 75.0% by mass, more preferably 52.0% by mass to 70.0% by mass, and even more preferably 54.0% by mass to 65.0% by mass.

[0049] [1-1-2-3] Organic Solvents The pigment ink 2' may contain an organic solvent.

[0050] This makes it possible to suitably adjust the viscosity and surface tension of the pigment ink 2'. In addition, for example, the pigment ink 2' has excellent moisture retention, which more effectively prevents the solid content of the pigment ink 2' from unintentionally precipitating due to drying in an inkjet head or the like, improves clogging recovery, and improves the ejection stability of the pigment ink 2'.

[0051] As the organic solvent, a water-soluble organic solvent is preferably used. As such a water-soluble organic solvent, an organic solvent having a solubility in water at 25° C. of 10 g / 100 g water or more can be suitably used.

[0052] In particular, it is preferable that the pigment ink 2' contains an organic solvent having a boiling point of 280° C. or higher.

[0053] This makes it possible to improve the moisture retention of the pigment ink 2', and makes it easier for the drying rate of the first layer 2 when the treatment liquid 3' is ejected to satisfy the above-mentioned condition.

[0054] The organic solvent contained in the pigment ink 2', particularly the water-soluble organic solvent, includes, for example, polyol compounds, glycol ethers, cyclic amide compounds, etc., and one or more selected from these can be used in combination.

[0055] Examples of the polyol compound include polyol compounds having 2 to 6 carbon atoms in the molecule and optionally having one ether bond in the molecule, preferably diol compounds. Specific examples include 1,2-pentanediol, glycerin, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, polyoxyethylene polyoxypropylene glycol, 1,2-hexanediol, 1,2-heptanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, Examples of glycols include 2,3-butanediol, 2-methyl-3-phenoxy-1,2-propanediol, 3-(3-methylphenoxy)-1,2-propanediol, 3-hexyloxy-1,2-propanediol, 2-hydroxymethyl-2-phenoxymethyl-1,3-propanediol, 3-methyl-1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl-2,4-pentanediol, and 3-methyl-1,5-pentanediol.

[0056] Examples of the glycol ether include monoalkyl ethers of glycols selected from ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, and polyoxyethylene polyoxypropylene glycol. Examples of the monoalkyl ether include triethylene glycol monomethyl ether, triethylene glycol monobutyl ether, triethylene glycol monoethyl ether, and dipropylene glycol monopropyl ether.

[0057] Examples of cyclic amide compounds include 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethylimidazolidinone, 2-piperidone (δ-valerolactam), and N-cyclohexyl-2-pyrrolidone.

[0058] The content of the organic solvent in the pigment ink 2' is preferably 5.0% by mass to 35.0% by mass, more preferably 10.0% by mass to 30.0% by mass, and even more preferably 15.0% by mass to 25.0% by mass.

[0059] This allows the viscosity and surface tension of the pigment ink 2' to be more suitably adjusted. In addition, the moisture retention of the pigment ink 2' is improved, which more effectively prevents the solid content of the pigment ink 2' from unintentionally precipitating due to drying in an inkjet head or the like, improves clogging recovery, and improves the ejection stability of the pigment ink 2'. In addition, the drying rate of the first layer 2 when ejecting the treatment liquid 3' is more likely to satisfy the above-mentioned condition.

[0060] [1-1-2-4] Resin The pigment ink 2' may contain a resin.

[0061] This makes it possible, for example, to improve the adhesion of the recording portion 4 containing the pigment to the transfer medium 5. Also, the dispersion stability of the pigment in the pigment ink 2' can be improved.

[0062] However, the content of the resin in the pigment ink 2' is 15.0% by mass or less.

[0063] This ensures that the ejection stability of the pigment ink 2' by the inkjet method is sufficiently excellent, and makes it possible to stably produce the recorded matter 100. In addition, the texture of the recorded matter 100 produced can be made excellent.

[0064] The resin content in the pigment ink 2' may be 15.0% by mass or less, and the pigment ink 2' may not contain resin; however, the resin content in the pigment ink 2' is preferably 2.0% by mass or more and 13.0% by mass or less, more preferably 4.0% by mass or more and 12.0% by mass or less, and even more preferably 7.0% by mass or more and 11.0% by mass or less.

[0065] This makes it possible to sufficiently improve the ejection stability of the pigment ink 2' using the inkjet method, the production stability of the recorded matter 100, and the texture of the recorded matter 100, while also further improving the dispersion stability of the pigment in the pigment ink 2' and the adhesion of the recording section 4 to the transfer medium 5.

[0066] When the pigment ink 2' contains a resin, there is no particular limitation on the form of the resin in the pigment ink 2'. For example, the resin may be contained in the pigment ink 2' in a dispersed state or in a dissolved state, but is preferably contained in a dispersed state.

[0067] This makes it possible to improve the ejection stability of the pigment ink 2' by the inkjet method, and thus makes it possible to manufacture the recorded matter 100 more stably.

[0068] When the resin is contained in a dispersed state in the pigment ink 2', the average particle size of the resin is preferably 30 nm to 3 μm, more preferably 50 nm to 1 μm, and even more preferably 60 nm to 300 nm. This makes the above-mentioned effects more pronounced.

[0069] In this specification, the average particle size refers to the average particle size based on volume, and can be determined, for example, by adding a sample to methanol, dispersing the sample for 3 minutes using an ultrasonic disperser, and measuring the dispersion using a Coulter Counter particle size distribution measuring instrument (TA-II model manufactured by COULTER ELECTRONICS INS) with an aperture of 50 μm.

[0070] Examples of the resin contained in the pigment ink 2' include polyurethane, polyester, styrene acrylic resin, acrylic resin, polyvinyl chloride, etc., and one or more selected from these may be used in combination. Among these, polyurethane is preferred. This makes the above-mentioned effects more pronounced.

[0071] The glass transition temperature of the resin contained in the pigment ink 2' is preferably -40°C or higher and 0°C or lower, more preferably -35°C or higher and -5°C or lower, and even more preferably -30°C or higher and -10°C or lower.

[0072] This makes it possible to produce a printed matter 100 with better texture, washing fastness, and the like.

[0073] When the resin content in the pigment ink 2' is XR [mass %] and the pigment content is XP [mass %], it is preferable to satisfy the relationship 0.2≦XR / XP≦1.8, it is more preferable to satisfy the relationship 0.6≦XR / XP≦1.5, and it is even more preferable to satisfy the relationship 0.8≦XR / XP≦1.2.

[0074] This makes it easier to ensure sufficient color density in the recording portion 4 formed using the pigment ink 2', and improves the color development on the transfer medium, while improving the storage stability of the pigment ink 2', the ejection stability by the inkjet method, and the clogging recovery property of the inkjet head, etc. Also, the texture of the recorded matter 100 and the adhesion of the recording portion 4 to the transfer medium 5 can be improved.

[0075] [1-1-2-5] Surfactants The pigment ink 2' may contain a surfactant.

[0076] As the surfactant, various surfactants such as anionic surfactants, cationic surfactants, and nonionic surfactants can be used.

[0077] When the pigment ink 2' contains a surfactant, the content of the surfactant in the pigment ink 2' is preferably 0.02% by mass or more and 1.50% by mass or less, more preferably 0.05% by mass or more and 1.00% by mass or less, and even more preferably 0.10% by mass or more and 0.70% by mass or less.

[0078] [1-1-2-6] Other ingredients The pigment ink 2' may contain components other than those mentioned above. Hereinafter, in this section, such components are also referred to as "other components".

[0079] Other components include, for example, chelating agents, preservatives, mildew inhibitors, rust inhibitors, flame retardants, various dispersants, pH adjusters such as triethanolamine, dyes, antioxidants, ultraviolet absorbers, oxygen absorbers, dissolution aids, and penetrating agents.

[0080] Examples of the chelating agent include ethylenediaminetetraacetate, etc. Examples of the preservatives and antifungal agents include sodium benzoate, sodium pentachlorophenol, sodium 2-pyridinethiol-1-oxide, sodium sorbate, sodium dehydroacetate, 1,2-dibenzisothiazolin-3-one, 4-chloro-3-methylphenol, etc. Examples of the rust inhibitors include benzotriazole, etc.

[0081] As the preservative / antifungal agent, for example, a compound having an isothiazolinone ring structure in the molecule can be suitably used.

[0082] The content of other components in the pigment ink 2' is preferably 6.0% by mass or less, and more preferably 5.0% by mass or less. The lower limit of the content of other components is 0 mass %.

[0083] [1-1-2-7] Other conditions The viscosity of the pigment ink 2' at 25°C is preferably from 2 mPa·s to 10 mPa·s, and more preferably from 3 mPa·s to 8 mPa·s.

[0084] This makes it more difficult for the nozzles of the inkjet head to become clogged, improving the ejection stability of the pigment ink 2'. Even if the nozzles do become clogged, the nozzles can be capped to improve recovery.

[0085] The viscosity can be determined by measurement using a vibration viscometer, a rotational viscometer, a capillary viscometer, or a falling ball viscometer. For example, the viscosity can be determined by measurement using a vibration viscometer in accordance with JIS Z8809.

[0086] The surface tension of the pigment ink 2' at 25°C is not particularly limited, but is preferably 20 mN / m or more and 60 mN / m or less, more preferably 25 mN / m or more and 50 mN / m or less, and even more preferably 27 mN / m or more and 40 mN / m or less.

[0087] This makes it more difficult for the nozzles of the inkjet head to become clogged, improving the ejection stability of the pigment ink 2'. Even if the nozzles do become clogged, the nozzles can be capped to improve recovery.

[0088] The surface tension may be measured by the Wilhelmy method or the Ring method using a surface tensiometer (e.g., DY-300, DY-500, DY-700, etc., manufactured by Kyowa Interface Science Co., Ltd.).

[0089] [1-1-3] Discharge by the inkjet method The first layer 2 is formed by ejecting a pigment ink 2' by an inkjet method onto a transfer medium 1 having a release layer 12. More specifically, the pigment ink 2' is ejected so as to come into contact with the release layer 12 of the transfer medium 1.

[0090] Examples of the inkjet method include on-demand methods such as a charge deflection method, a continuous method, a piezoelectric method, and a bubble jet (registered trademark) method, and in particular, a piezoelectric method in which ink is ejected from an inkjet head using a piezoelectric vibrator is preferred.

[0091] This makes it possible to more effectively prevent unintended alteration of the constituents of the pigment ink 2' within the inkjet head 50, and to improve the ejection stability by the inkjet method.

[0092] Moreover, the inkjet head 50 may be a line head that performs printing by a line method, or a serial head that performs printing by a serial method.

[0093] In the line method using a line head, for example, an inkjet head having a width equal to or greater than the recording width of the transfer medium 1 is fixed to a recording device. Then, the transfer medium 1 is moved along the sub-scanning direction (the transport direction of the transfer medium 1), and ink droplets are ejected from the nozzles of the inkjet head 50 in conjunction with this movement, thereby forming a first layer 2 on the transfer medium 1.

[0094] In the serial method using a serial head, for example, an inkjet head 50 is mounted on a carriage that is movable in the width direction of the transfer medium 1. Then, the carriage is moved along the main scanning direction (width direction of the transfer medium 1), and ink droplets are ejected from the nozzles of the serial head, which is the inkjet head 50, in conjunction with this movement, thereby forming a first layer 2 on the transfer medium 1.

[0095] In this step, the first layer 2 is formed as a reverse image of the recording portion 4 to be formed on the transfer medium 5 .

[0096] In this step, multiple types of pigment inks 2' may be used. For example, multiple types of pigment inks 2' having different color tones, more specifically, black ink, cyan ink, magenta ink, and yellow ink may be used.

[0097] [1-2] Second layer formation process In the second layer forming step, a treatment liquid 3' is ejected from an inkjet head 50' to form a second layer 3 so as to overlap the first layer 2 formed on the transfer medium 1 (1b).

[0098] [1-2-1] Processing solution The treatment liquid 3' is used to form the second layer 3, and contains a resin and water.

[0099] [1-2-1-1] Resin The treatment liquid 3' contains a resin.

[0100] This makes it possible to provide excellent adhesion of the recording portion 4 to the transfer medium 5, and to provide the produced recorded matter 100 with excellent washing fastness.

[0101] Examples of resins contained in the treatment liquid 3' include polyester, polyurethane, polyvinyl chloride, styrene-acrylic resin, acrylic resin, etc., and one or more selected from these may be used in combination. However, one or more selected from the group consisting of polyester, polyurethane, and polyvinyl chloride are preferred, and polyurethane is more preferred.

[0102] This allows the texture and washing fastness of the recorded matter 100 to be compatible at a higher level.

[0103] The form of the resin in the treatment liquid 3' is not particularly limited. For example, the resin may be contained in the treatment liquid 3' in a dispersed state or in a dissolved state, but is preferably contained in a dispersed state.

[0104] This makes it possible to improve the ejection stability of the pigment ink 2' by the inkjet method, and to more stably produce the recorded matter 100. Also, it is possible to more effectively prevent liquid components from unintentionally remaining in the second layer 3 and the recording portion 4.

[0105] When the resin is contained in a dispersed state in the treatment liquid 3', the average particle size of the resin is preferably 30 nm to 3 μm, more preferably 50 nm to 1 μm, and even more preferably 60 nm to 300 nm. This makes the above-mentioned effects more pronounced.

[0106] The glass transition temperature of the resin contained in the treatment liquid 3' is preferably from -20°C to 50°C, more preferably from -10°C to 45°C, and even more preferably from 0°C to 40°C.

[0107] This allows the texture and washing fastness of the recorded matter 100 to be compatible at a higher level.

[0108] The melting point of the resin contained in the treatment liquid 3' is preferably 80°C or higher and 140°C or lower, more preferably 85°C or higher and 130°C or lower, and even more preferably 90°C or higher and 120°C or lower.

[0109] This allows the texture and washing fastness of the recorded matter 100 to be compatible at a higher level.

[0110] The resin content in the treatment liquid 3' is preferably 5.0% by mass to 20.0% by mass, more preferably 6.0% by mass to 17.0% by mass, and even more preferably 7.0% by mass to 15.0% by mass.

[0111] This allows the texture and washing fastness of the recorded matter 100 to be compatible at a higher level.

[0112] [1-2-1-2]Water The treatment liquid 3' contains water.

[0113] Water is a component in the treatment liquid 3' that functions, for example, as a dispersion medium for dispersing a resin or as a solvent for dissolving the resin.

[0114] The water content in the treatment liquid 3' is preferably 50.0% by mass or more and 85.0% by mass or less, more preferably 55.0% by mass or more and 80.0% by mass or less, and even more preferably 60.0% by mass or more and 75.0% by mass or less.

[0115] [1-2-1-3] Organic Solvents The treatment liquid 3' may contain an organic solvent.

[0116] This allows the viscosity and surface tension of the treatment liquid 3' to be suitably adjusted. In addition, for example, the moisturizing property of the treatment liquid 3' is improved, which more effectively prevents the solid content of the treatment liquid 3' from unintentionally precipitating due to drying in an inkjet head or the like, improves clogging recovery, and improves the ejection stability of the treatment liquid 3'.

[0117] However, it is preferable that the treatment liquid 3' does not contain an organic solvent having a boiling point of 280° C. or higher.

[0118] This improves the drying properties of the second layer 3 formed using the treatment liquid 3', and improves the peelability of the laminate having the first layer 2 and the second layer 3 from the transfer medium 1.

[0119] As the organic solvent, a water-soluble organic solvent is preferably used.

[0120] As such a water-soluble organic solvent, an organic solvent having a solubility in water at 25° C. of 10 g / 100 g water or more can be suitably used.

[0121] The organic solvent contained in the pigment ink 2', particularly the water-soluble organic solvent, includes, for example, polyol compounds, glycol ethers, cyclic amide compounds, etc., and one or more selected from these can be used in combination.

[0122] Examples of the polyol compound include polyol compounds having 2 to 6 carbon atoms in the molecule and optionally having one ether bond in the molecule, preferably diol compounds. Specific examples include 1,2-pentanediol, glycerin, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, polyoxyethylene polyoxypropylene glycol, 1,2-hexanediol, 1,2-heptanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, Examples of glycols include 2,3-butanediol, 2-methyl-3-phenoxy-1,2-propanediol, 3-(3-methylphenoxy)-1,2-propanediol, 3-hexyloxy-1,2-propanediol, 2-hydroxymethyl-2-phenoxymethyl-1,3-propanediol, 3-methyl-1,3-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2-methyl-2,4-pentanediol, and 3-methyl-1,5-pentanediol.

[0123] Examples of the glycol ether include monoalkyl ethers of glycols selected from ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol, and polyoxyethylene polyoxypropylene glycol. Examples of the monoalkyl ether include triethylene glycol monomethyl ether, triethylene glycol monobutyl ether, triethylene glycol monoethyl ether, and dipropylene glycol monopropyl ether.

[0124] Examples of cyclic amide compounds include 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethylimidazolidinone, 2-piperidone (δ-valerolactam), and N-cyclohexyl-2-pyrrolidone.

[0125] In particular, it is preferable that the treatment liquid 3' contains propylene glycol as an organic solvent.

[0126] This improves drying properties, facilitates curing of the resin when heated, and improves robustness.

[0127] In particular, when the treatment liquid 3' contains propylene glycol, the proportion of propylene glycol in the total organic solvents contained in the treatment liquid 3' is preferably 50 mass% or more, more preferably 70 mass% or more, and even more preferably 80 mass% or more. This makes the above-mentioned effects more pronounced.

[0128] The content of the organic solvent in the treatment liquid 3' is preferably 5.0% by mass to 35.0% by mass, more preferably 7.0% by mass to 30.0% by mass, and even more preferably 10.0% by mass to 25.0% by mass.

[0129] This makes it possible to more suitably adjust the viscosity and surface tension of the treatment liquid 3'. Also, the moisturizing property of the treatment liquid 3' is improved, which more effectively prevents the solid content of the treatment liquid 3' from unintentionally precipitating due to drying in an inkjet head or the like, improves clogging recovery, and improves the ejection stability of the treatment liquid 3'.

[0130] [1-2-1-4] Surfactants The treatment liquid 3' may contain a surfactant.

[0131] As the surfactant, various surfactants such as anionic surfactants, cationic surfactants, and nonionic surfactants can be used.

[0132] When the treatment liquid 3' contains a surfactant, the content of the surfactant in the pigment ink 2' is preferably 0.02% by mass or more and 1.50% by mass or less, more preferably 0.05% by mass or more and 1.00% by mass or less, and even more preferably 0.10% by mass or more and 0.70% by mass or less.

[0133] [1-2-1-5] Other ingredients The treatment liquid 3' may contain components other than those mentioned above. Hereinafter, in this section, such components are also referred to as "other components".

[0134] Other components include, for example, chelating agents, preservatives, mildew inhibitors, rust inhibitors, flame retardants, various dispersants, pH adjusters such as triethanolamine, antioxidants, ultraviolet absorbers, oxygen absorbers, dissolution aids, and penetrating agents.

[0135] The content of other components in the treatment liquid 3' is preferably 6.0% by mass or less, and more preferably 5.0% by mass or less. The lower limit of the content of other components is 0 mass %.

[0136] [1-2-1-6] Other conditions The viscosity of the treatment liquid 3' at 25°C is preferably from 2 mPa·s to 10 mPa·s, and more preferably from 3 mPa·s to 8 mPa·s.

[0137] This makes it more difficult for the nozzles of the inkjet head to become clogged, and improves the ejection stability of the treatment liquid 3'. Even if the nozzles do become clogged, the nozzles can be capped to improve recovery.

[0138] The surface tension of the treatment liquid 3' at 25°C is not particularly limited, but is preferably from 20 mN / m to 60 mN / m, more preferably from 25 mN / m to 50 mN / m, and even more preferably from 27 mN / m to 40 mN / m.

[0139] This makes it more difficult for the nozzles of the inkjet head to become clogged, and improves the ejection stability of the treatment liquid 3'. Even if the nozzles do become clogged, the nozzles can be capped to improve recovery.

[0140] [1-2-2] Discharge by the inkjet method The second layer 3 is formed by ejecting a treatment liquid 3' by an inkjet method onto the transfer medium 1 on which the first layer 2 has been formed.

[0141] Examples of the inkjet method include on-demand methods such as a charge deflection method, a continuous method, a piezoelectric method, and a bubble jet (registered trademark) method, and in particular, a piezoelectric method in which ink is ejected from an inkjet head using a piezoelectric vibrator is preferred.

[0142] This makes it possible to more effectively prevent unintended denaturation of the components of the treatment liquid 3' within the inkjet head 50', and to improve the ejection stability by the inkjet method.

[0143] The inkjet head 50' may be a line head that performs printing by a line method, or a serial head that performs printing by a serial method.

[0144] In this step, the second layer 3 is formed so as to overlap the first layer 2, and in particular so as to have the same pattern as the first layer 2.

[0145] Furthermore, the first layer 2 and the second layer 3 may be formed using different inkjet recording devices, but it is preferable to form them using the same inkjet recording device.

[0146] The dryness rate of the first layer 2 when the processing liquid 3' is ejected in this process may be 0% or more and 80% or less, but is preferably 10% or more and 75% or less, more preferably 20% or more and 70% or less, and even more preferably 35% or more and 65% or less.

[0147] This effectively prevents liquid components from unintentionally remaining in the final recorded matter 100, and the above-described effects of the present invention are more significantly exhibited.

[0148] The drying rate of the first layer 2 when the treatment liquid 3' is ejected in this process can be suitably adjusted, for example, by adjusting the composition of the pigment ink 2', as well as the temperature, humidity, and pressure of the atmosphere in which the transfer medium 1 is placed, and the time between when the pigment ink 2' is adhered to the transfer medium 1 and when the treatment liquid 3' is adhered thereto.

[0149] The temperature of the atmosphere in which the transfer medium 1 with the pigmented ink 2' is placed varies depending on the composition of the pigmented ink 2', but is preferably 1°C to 40°C, more preferably 5°C to 30°C.

[0150] The humidity of the atmosphere in which the transfer medium 1 with the pigmented ink 2' is placed varies depending on the composition of the pigmented ink 2', but is preferably 10% RH to 95% RH, and more preferably 20% RH to 90% RH.

[0151] The pressure of the atmosphere in which the transfer medium 1 with the pigmented ink 2' is placed varies depending on the composition of the pigmented ink 2', but is preferably 1 kPa to 150 kPa, and more preferably 10 kPa to 110 kPa.

[0152] Although it varies depending on the composition of the pigment ink 2', the time from when the pigment ink 2' is applied to the transfer medium 1 to when the treatment liquid 3' is applied is preferably at least 1 second and at most 60 seconds, and more preferably at least 2 seconds and at most 30 seconds. In this step, multiple types of treatment liquids 3' may be used.

[0153] [1-3] Thermal transfer process In the thermal transfer process, the surface of the transfer medium 1 on which the first layer 2 and the second layer 3 are formed is heated while facing an absorbent transfer medium 5, thereby thermally transferring the first layer 2 and the second layer 3 to the transfer medium 5 (1c).

[0154] [1-3-1]Transfer medium The transfer medium 5 may be any absorbent material, such as various types of paper, porous metal, porous ceramics, porous glass, porous plastic, cloth, leather, etc., with cloth or leather being preferred.

[0155] This makes it possible to transfer the printed matter to the finished product after sewing the fabric or leather anywhere, and provides good color development and abrasion resistance.

[0156] [1-3-2] Heating conditions The heating temperature in this step is not particularly limited, but is preferably from 120°C to 270°C, more preferably from 140°C to 250°C, and even more preferably from 150°C to 210°C.

[0157] This makes it possible to more effectively prevent the constituent materials of the first layer 2 and the second layer 3 from unintentionally remaining on the transfer medium 1, while also saving energy and improving the productivity of the recorded matter 100.

[0158] When the glass transition temperature of the resin contained in the treatment liquid 3' is Tg [°C] and the heating temperature in the thermal transfer process is Tp [°C], it is preferable to satisfy the relationship of 70≦Tp-Tg≦290, it is more preferable to satisfy the relationship of 95≦Tp-Tg≦260, and it is even more preferable to satisfy the relationship of 110≦Tp-Tg≦210.

[0159] This makes it possible to more effectively prevent the constituent materials of the first layer 2 and the second layer 3 from unintentionally remaining on the transfer medium 1, while also saving energy and improving the productivity of the recorded matter 100.

[0160] The heating time in this step is not particularly limited, but is preferably from 5 to 90 seconds, more preferably from 15 to 70 seconds, and even more preferably from 20 to 60 seconds.

[0161] This makes it possible to more effectively prevent the constituent materials of the first layer 2 and the second layer 3 from unintentionally remaining on the transfer medium 1, while also saving energy and improving the productivity of the recorded matter 100.

[0162] This process may be carried out by any method, provided that the surface of the transfer medium 1 on which the first layer 2 and the second layer 3 are formed is heated while facing the absorbent transfer medium 5, but is preferably carried out by heat pressing.

[0163] When this step is carried out by heat pressing, the pressure applied to the laminate of the transfer medium 1 and the transfer medium 5 is 0.1 N / cm 2 More than 30N / cm 2 Preferably, it is less than 0.6 N / cm 2 More than 15N / cm 2 More preferably, it is 1.5 N / cm 2 More than 5N / cm 2 It is even more preferable that:

[0164] [1-4] Records Through the above steps, a recorded matter 100 is obtained (1d).

[0165] The recorded matter 100 obtained as described above has a recorded portion 4 formed by a first layer 2 and a second layer 3.

[0166] It is preferable that at least a part of the recording portion 4 penetrates into the inside of the absorbent transfer medium 5 .

[0167] The recording section 4 is usually at least partially formed by integrating the constituent material of the first layer 2 with the constituent material of the second layer 3, but in the configuration shown in the figure, the entire recording section 4 is formed by integrating the constituent material of the first layer 2 with the constituent material of the second layer 3.

[0168] [1-5] Summary As described above, the recording method of the present invention includes a first layer forming step of ejecting a pigment ink containing a pigment and water from an inkjet head onto a transfer medium having a peelable layer to form a first layer, a second layer forming step of ejecting a treatment liquid from an inkjet head to form a second layer so as to overlap the first layer, and a thermal transfer step of thermally transferring the first layer and the second layer onto an absorbent transfer medium by heating the surface of the transfer medium on which the first layer and the second layer are formed, while facing the absorbent transfer medium, wherein the content of the resin in the pigment ink is 15.0 mass % or less, the treatment liquid contains a resin and water, and the drying rate of the first layer when the treatment liquid is ejected is 0% or more and 80% or less. The first layer forming step includes ejecting a pigment ink containing a pigment, a resin having a glass transition temperature of -40°C or more and 0°C or less, an organic solvent having a boiling point of 280°C or more, and water from an inkjet head onto a transfer medium having a peelable layer to form a first layer, The method includes a second layer forming step of ejecting a treatment liquid from an inkjet head to form a second layer so as to overlap the first layer, and a thermal transfer step of thermally transferring the first layer and the second layer to an absorbent transfer medium, such as fabric or leather, by heating the surface of the transfer medium on which the first layer and the second layer are formed while the surface is opposed to the absorbent transfer medium, such as fabric or leather, wherein the content of the resin in the pigment ink is 2.0% by mass or more and 15.0% by mass or less, the treatment liquid contains a resin having a glass transition temperature of -20°C or more and 50°C or less and a melting point of 80°C or more and 140°C or less, and water, but does not contain an organic solvent having a boiling point of 280°C or more, the resin contained in the treatment liquid is one or more types selected from the group consisting of polyester, polyurethane, and polyvinyl chloride, the content of the resin in the treatment liquid is 5.0% by mass or more and 20.0% by mass or less, and the drying rate of the first layer when the treatment liquid is ejected is 0% to 80%.

[0169] This allows the above-mentioned effects to act synergistically, resulting in particularly excellent effects.

[0170] [2] Ink and treatment liquid set Next, the ink / treatment liquid set according to the present invention will be described. The ink / treatment liquid set according to the present invention comprises the above-mentioned pigment ink and treatment liquid.

[0171] More specifically, the ink / treatment liquid set according to the present invention preferably comprises a pigment ink that satisfies the conditions explained in [1-1-2] above, and also comprises the treatment liquid explained in [1-2-1] above.

[0172] The ink / treatment liquid set according to the present invention may comprise at least one type of pigment ink and one type of treatment liquid, but may also comprise multiple types of pigment inks or multiple types of treatment liquid. Furthermore, the ink / treatment liquid set according to the present invention may further comprise other inks and treatment liquids in addition to the pigment ink and treatment liquid that satisfy the above conditions.

[0173] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to these.

[0174] For example, in the above explanation, an absorbent material is used as the transfer medium, but a non-absorbent material, such as a non-absorbent metal or plastic material, may also be used as the transfer medium.

[0175] In the above embodiment, the first layer of the desired pattern is completed on the transfer medium, then the treatment liquid is discharged to complete the second layer of the desired pattern, and then the thermal transfer process is performed, but in the present invention, multiple processes may be performed simultaneously. More specifically, for example, the discharge of the pigment ink and the discharge of the treatment liquid may be performed simultaneously on different parts of the same transfer medium. EXAMPLES

[0176] Next, specific examples of the present invention will be described. [3] Preparation of pigment ink

[0177] (Preparation example A1) By mixing each component in a specified ratio, a pigment ink with the composition shown in Figure 2 was obtained.

[0178] (Preparation examples A2 to A5) A pigment ink was prepared in the same manner as in Preparation Example A1, except that the types of components used in preparing the pigment ink and the blending ratio of each component were changed to obtain the composition shown in FIG.

[0179] The compositions of the pigment inks of Preparation Examples A1 to A5 are summarized in FIG. 2. The numerical values ​​indicated by "%" for each component in FIG. 2 indicate the content in units of mass%. In addition, in FIG. 2, CI Pigment Blue 15:3 is indicated as "PB15:3", polyurethane resin with a glass transition temperature of -20°C (solid content of Takelac W6110, manufactured by Mitsui Chemicals) is indicated as "polyurethane resin", hot melt resin (solid content of KT08701, manufactured by Unitika) is indicated as "hot melt resin", glycerin, which is a water-soluble organic solvent, is indicated as "Gly", and Silface SAG503A (manufactured by Nissin Chemical Industry Co., Ltd.) as a surfactant is indicated as "SAG503A". In addition, the average particle size of the resin contained in each of the pigment inks of Preparation Examples A1 to A5 was within the range of 60 nm to 300 nm. Furthermore, the pigment inks of Preparation Examples A1 to A5 all had a surface tension at 25° C. in the range of 30 mN / m or more and 40 mN / m or less, and a viscosity at 25° C. in the range of 3 mPa·s or more and 8 mPa·s or less. The surface tension was measured by the Wilhelmy method using a surface tensiometer (DY-300, manufactured by Kyowa Interface Science Co., Ltd.), and the viscosity was measured in accordance with JIS Z8809 using a vibration viscometer (VM-100, manufactured by Senicook Co., Ltd.).

[0180] [4] Preparation of processing solution (Preparation example B1) By mixing the components in a given ratio, a treatment liquid having the composition shown in FIG. 3 was obtained.

[0181] (Preparation examples B2 to B5) A treatment liquid was prepared in the same manner as in Preparation Example B1, except that the types of components used in preparing the treatment liquid and the blending ratio of each component were changed to obtain the composition shown in FIG.

[0182] The compositions of the treatment liquids of Preparation Examples B1 to B5 are summarized in FIG. 3. The numerical values ​​indicated by "%" for each component in FIG. 3 indicate the content in units of mass%. In addition, in FIG. 3, polyester resin (solid content of KT9204, manufactured by Unitika Ltd.) is indicated as "polyester resin", vinyl chloride resin (solid content of Vinyblan 715S, manufactured by Mitsui Chemicals, Inc.) is indicated as "vinyl chloride resin", polyurethane resin (solid content of Takelac W6061, manufactured by Mitsui Chemicals, Inc.) is indicated as "polyurethane resin", propylene glycol, which is a water-soluble organic solvent, is indicated as "PG", and Silface SAG503A (manufactured by Nissin Chemical Industry Co., Ltd.) as a surfactant is indicated as "SAG503A". In addition, the treatment liquids of Preparation Examples B1 to B5 all had an average particle size of the resin contained within a range of 60 nm to 300 nm. The treatment solutions of Preparation Examples B1 to B5 all had a surface tension of 30 mN / m or more and 40 mN / m or less at 25° C., and a viscosity of 3 mPa·s or more and 8 mPa·s or less at 25° C. The surface tension was measured by the Wilhelmy method using a surface tensiometer (DY-300, manufactured by Kyowa Interface Science Co., Ltd.), and the viscosity was measured in accordance with JIS Z8809 using a vibration viscometer (VM-100, manufactured by Senicook Co., Ltd.).

[0183] [5] Production of records Example 1 First, a transfer medium (print film for DTF, manufactured by Inkmania Co., Ltd.) was prepared, which had a release layer made of a release agent provided on a base material made of polyethylene terephthalate.

[0184] Next, an inkjet recording device (Seiko Epson Corporation, SC-F2150) was filled with the pigment ink obtained in Preparation Example A1 and the treatment liquid obtained in Preparation Example B1, and the pigment ink was ejected from an inkjet head onto the surface of the transfer medium on which the release layer was formed, to form a first layer of a predetermined pattern.

[0185] Next, a treatment liquid was discharged from an inkjet head so as to overlap the first layer, forming a second layer having the same pattern as the first layer. The drying rate of the first layer when the treatment liquid was discharged was 50%.

[0186] Next, the surface of the transfer medium 1 on which the first and second layers were formed was placed opposite an absorbent receiving medium, Nisshinbo cotton broadcloth (#4000), and heat-treated at 200°C for 40 seconds to thermally transfer the first and second layers to the receiving medium. Thereafter, the transfer medium was removed to obtain a recorded matter.

[0187] (Examples 2 to 19) A recorded material was produced in the same manner as in Example 1, except that the pigment ink, the type of treatment liquid, the heating conditions in the thermal transfer process, the type of transfer medium, and the drying rate of the first layer when the treatment liquid was ejected were changed as shown in Figures 4 and 5. In Example 7, the first layer was formed by first ejecting the pigment ink obtained in Preparation Example A1 from the inkjet head to form a predetermined pattern, and then ejecting the pigment ink obtained in Preparation Example A4 from the inkjet head so as to overlap the pattern of the pigment ink obtained in Preparation Example A1, thereby forming the same pattern as the first layer. That is, in Example 7, the first layer was formed as a laminate of a layer of the pigment ink obtained in Preparation Example A1 and a layer of the pigment ink obtained in Preparation Example A4.

[0188] Comparative Example 1 Instead of applying a processing liquid to the transfer medium having the first layer, a cascade shaker (made by Europort) was used to sprinkle hot melt powder PU (polyurethane) resin powder made by Inkmania as a heat-meltable powder, and then the excess resin powder was shaken off. A recorded material was produced in the same manner as in Example 1, except that a thermal transfer to the transfer medium was performed in the same manner as described above.

[0189] Comparative Example 2 A recorded matter was produced in the same manner as in Example 1, except that the drying rate of the first layer when the treatment liquid used to form the second layer was ejected was changed to 100%.

[0190] Comparative Example 3 A recorded matter was produced in the same manner as in Example 1, except that the pigment ink prepared in Preparation Example A5 was used to form the first layer, and the step of forming the second layer was omitted.

[0191] Comparative Example 4 A recorded matter was produced in the same manner as in Example 1, except that the step of forming the second layer was omitted.

[0192] The conditions for manufacturing the products of the above-mentioned Examples and Comparative Examples, that is, the conditions for the recording method, are summarized in Figures 4 and 5. In Figures 4 and 5, cotton broadcloth (#4000) manufactured by Nisshinbo Corporation as a medium for receiving transfer is indicated as "cotton broadcloth", TC4520 (manufactured by Toyoshima Co., Ltd., a blended fabric of 35% cotton and 65% polyester fiber by mass) as a medium for receiving transfer is indicated as "blend", Tropical (manufactured by Toray Industries, Inc., a polyester fabric) as a medium for receiving transfer is indicated as "polyester", PAREL Taffeta N2188 (manufactured by Toray Industries, Inc., a nylon fabric) as a medium for receiving transfer is indicated as "nylon", and natural leather cowhide (manufactured by Daiki Leather Co., Ltd.) as a medium for receiving transfer is indicated as "leather".

[0193] [6] Evaluation

[0194] [6-1] Texture The texture of the recorded matter according to each of the Examples and Comparative Examples was evaluated as follows.

[0195] Specifically, for each recorded material, a specific evaluator blindfolded the feel and performed a sensory evaluation according to the following criteria to evaluate the texture.

[0196] The evaluation results indicate superior feel in the order of A, B, and C. When the evaluation result is A or B, it can be said that the effects of the present invention are obtained.

[0197] A: It is soft and does not feel stiff. B: Slightly hard and slightly stiff to the touch. C: There is a noticeable stiffness to the touch.

[0198] [6-2] Dry friction fastness For the recorded matter according to each of the above-mentioned Examples and Comparative Examples, the dry rub fastness was evaluated as follows.

[0199] Specifically, each of the recorded materials was left to stand for 1 hour at 25°C after production, and the recorded surface of the recorded material was rubbed 20 times with a cotton cloth under a load of 200g using a Gakushin type rub fastness tester AB-301 (manufactured by Tester Sangyo Co., Ltd.). The peeling state of the recorded area and the transfer of ink to the cotton cloth were then visually confirmed, and the rub resistance was evaluated according to the following criteria. The less the color transfer and peeling, the better the rub resistance, and the better the robustness. B or higher was considered to be a good level.

[0200] A: No color transfer or peeling is observed. B: Slight color transfer and peeling are observed. C: Color transfer and peeling are clearly observed.

[0201] [6-3] Wet friction fastness For the recorded matter according to each of the Examples and Comparative Examples, wet friction fastness was evaluated as follows.

[0202] Specifically, each of the recorded materials was left to stand for 1 hour at 25°C after production, and the recorded surface of the recorded material was rubbed 20 times with a cotton cloth soaked in pure water and moistened under a load of 200g using a Gakushin type rub fastness tester AB-301 (manufactured by Tester Sangyo Co., Ltd.). The peeling state of the recorded area and the transfer of ink to the cotton cloth were then visually confirmed, and the rub resistance was evaluated according to the following criteria. The less the color transfer and peeling, the better the rub resistance, and the better the rub resistance, the better the fastness. B or higher was considered to be a good level.

[0203] A: No color transfer or peeling is observed. B: Slight color transfer and peeling are observed. C: Color transfer and peeling are clearly observed.

[0204] [6-4] Washing fastness The recorded matter according to each of the Examples and Comparative Examples was evaluated for washing fastness as follows.

[0205] Specifically, a washing fastness test was conducted in accordance with ISO 105 C10 (B2), and the washing fastness was evaluated according to the following criteria, with B or higher being considered a good level.

[0206] A: Washing fastness is grade 3 or higher. B: Washing fastness is grade 2 or higher but less than grade 3. C: Washing fastness is less than grade 2.

[0207] [6-5] Peelability For each of the above-mentioned Examples and Comparative Examples, the state of the transfer medium after the recording portion was transferred to the transfer medium was observed, and the peelability was evaluated according to the following criteria: B or higher was determined to be a good level.

[0208] A: 100% of the image area printed on the transfer medium is transferred. B: 80% or more but less than 100% of the image area printed on the transfer medium is transferred C: Less than 80% of the printed image area on the transfer media has been transferred

[0209] [6-6] Clogging The pigment ink and the treatment liquid used in the production of the recorded matter in each of the Examples and Comparative Examples were filled into an inkjet printer (product name PX-G930, manufactured by Seiko Epson Corporation) and left for one month with the cap open. After that, cleaning was performed three times, and the number of nozzles that were missing was determined and evaluated according to the following criteria. B or higher was considered to be a good level.

[0210] A: No missing nozzles. B: The number of missing nozzles is 1 to 5. C: The number of missing nozzles is 6 or more and 20 or less. D: 21 or more nozzles are missing.

[0211] [6-7] Device size The size of the installation area of ​​the devices used to manufacture the recorded matter in each of the above-mentioned Examples and Comparative Examples was compared. Specifically, the ratio of the installation area of ​​the devices used to form the first and second layers in each of the above-mentioned Examples and Comparative Examples to the sum of the installation areas of the inkjet recording device used to form the first and second layers in Comparative Example 1 and the cascade shaker (manufactured by Europort) was calculated, and the results were evaluated according to the following criteria.

[0212] A: The installation area of ​​the device is less than 50% of that of Comparative Example 1. B: The installation area of ​​the device is 50% or more and less than 100% of that of Comparative Example 1. C: The installation area of ​​the device is 100% or more of that of Comparative Example 1. These results are summarized in Figures 6 and 7.

[0213] As is clear from Figures 6 and 7, excellent results were obtained in the present invention. In contrast, satisfactory results were not obtained in the comparative example. [Explanation of symbols]

[0214] Reference Signs List 1...transfer medium, 11...substrate, 12...peeling layer, 2'...pigment ink, 2...first layer, 3'...treatment liquid, 3...second layer, 4...recording section, 5...receiving medium, 50...inkjet head, 50'...inkjet head, 100...recorded matter

Claims

1. a first layer forming step of forming a first layer by ejecting a pigment ink containing a pigment and water from an inkjet head onto a transfer medium having a release layer; a second layer forming step of ejecting a treatment liquid from an inkjet head to form a second layer so as to overlap the first layer; a thermal transfer step of thermally transferring the first layer and the second layer to an image-receiving medium by heating a surface of the transfer medium on which the first layer and the second layer are formed, while the surface is opposed to the image-receiving medium having an absorbent property; the content of the resin in the pigment ink is 15.0% by mass or less, The treatment liquid contains a resin and water, A recording method, wherein the drying rate of the first layer when the treatment liquid is discharged is 0% or more and 80% or less.

2. 2. The recording method according to claim 1, wherein the resin contained in the treatment liquid is at least one selected from the group consisting of polyester, polyurethane, and polyvinyl chloride.

3. 3. The recording method according to claim 1, wherein the glass transition temperature of the resin contained in the treatment liquid is −20° C. or higher and 50° C. or lower.

4. 3. The recording method according to claim 1, wherein the melting point of the resin contained in the treatment liquid is 80° C. or higher and 140° C. or lower.

5. 3. The recording method according to claim 1, wherein the content of the resin in the treatment liquid is from 5.0% by mass to 20.0% by mass.

6. 3. The recording method according to claim 1, wherein the treatment liquid does not contain an organic solvent having a boiling point of 280[deg.] C. or higher.

7. 3. The recording method according to claim 1, wherein the pigment ink contains a resin having a glass transition temperature of -40° C. or higher and 0° C. or lower.

8. 3. The recording method according to claim 1, wherein the pigment ink contains an organic solvent having a boiling point of 280[deg.] C. or higher.

9. 3. The recording method according to claim 1, wherein the medium is fabric or leather.

10. a first layer forming step of ejecting a pigment ink containing a pigment, a resin having a glass transition temperature of −40° C. or more and 0° C. or less, an organic solvent having a boiling point of 280° C. or more, and water from an inkjet head onto a transfer medium having a release layer to form a first layer; a second layer forming step of ejecting a treatment liquid from an inkjet head to form a second layer so as to overlap the first layer; a thermal transfer step of thermally transferring the first layer and the second layer to the transfer medium by heating the surface of the transfer medium on which the first layer and the second layer are formed while facing the absorbent transfer medium, which is fabric or leather; the content of the resin in the pigment ink is 2.0% by mass or more and 15.0% by mass or less, the treatment liquid contains a resin having a glass transition temperature of -20°C or more and 50°C or less and a melting point of 80°C or more and 140°C or less, and water, but does not contain an organic solvent having a boiling point of 280°C or more; the resin contained in the treatment liquid is at least one selected from the group consisting of polyester, polyurethane, and polyvinyl chloride; The content of the resin in the treatment liquid is 5.0% by mass or more and 20.0% by mass or less, A recording method, wherein a drying rate of the first layer when the treatment liquid is discharged is 0% or more and 80% or less.

Citation Information

Patent Citations

  • Transfer printing method

    JP2019171840A

Cited By

  • Method for manufacturing a transfer medium, method for recording a transfer, and adhesive colored ink composition

    JP2026162237A