Styrenic resin extrusion foam molding and method for manufacturing the same

By extruding and stretching styrenic resin foam within defined temperature and ratio ranges, the method addresses edge chipping in styrenic resin moldings, enhancing machinability and maintaining compressive strength.

JP2024137823APending Publication Date: 2024-10-07KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024041847
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-22
Filing Date
2024-03-18
Publication Date
2024-10-07

Smart Images

  • Figure 2024137823000001_ABST
    Figure 2024137823000001_ABST
Patent Text Reader

Abstract

To provide a styrenic resin extrusion foam molding which can suppress chipping of an end when cutting, while securing plane compressive strength, and a method for manufacturing the same.SOLUTION: A method for manufacturing a styrenic resin extrusion foam molding 100 includes Step Sa and Sep Sb. Step Sa extrudes a styrenic resin composition containing a styrenic resin and a foaming agent from a high pressure area to a low pressure area through a die lip 11, and thereby obtains an extrusion foam 20. Step Sb stretches the extrusion foam 20 obtained in Step Sa in an extrusion direction of the Step Sa while heating. A heating temperature of the extrusion foam 20 in Step Sb is 95°C or higher and 145°C or lower. An stretching ratio of the extrusion foam 20 in Step Sb is 1.01 times or more and 1.35 times or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an extruded styrene resin foam and a method for producing the same. [Background technology]

[0002] Since styrene-based resin extrusion foams have good heat insulating properties, they are used as heat insulating materials for houses and buildings, etc. (more specifically, heat insulating materials for tatami mats, etc.) The styrene-based resin extrusion foams are continuously produced, for example, by melt-kneading a styrene-based resin and a foaming agent in an extruder, optionally cooling the resulting composition, and extruding it through a die lip (for example, a die slit) into a low pressure region.

[0003] For example, Patent Document 1 discloses a production method that makes it possible to obtain extruded styrene-based resin foamed articles with beautiful surfaces by controlling the pressure release rate when a composition containing a styrene-based resin and a foaming agent is extruded into a low pressure region. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2013-124281 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the technology described in Patent Document 1 has room for improvement in terms of preventing chipping of the ends of the obtained styrene-based resin extruded foam molded body when the styrene-based resin extruded foam molded body is cut for use in a tatami mat or the like, while ensuring the plane compressive strength of the resulting styrene-based resin extruded foam molded body.

[0006] In view of the above, an object of the present invention is to provide an extruded styrene resin foam that can suppress chipping of the edges during cutting while ensuring planar compressive strength, and a method for producing the same. [Means for solving the problem]

[0007] <Aspects of the present invention> The present invention includes the following aspects.

[0008] [1] A step Sa of extruding a styrene-based resin composition containing a styrene-based resin and a foaming agent from a high-pressure region through a die lip to a low-pressure region to obtain an extruded foam; A step Sb of stretching the extruded foam in the extrusion direction of the step Sa while heating the extruded foam; A method for producing an extruded styrene resin foam comprising: The heating temperature of the extruded foam in the step Sb is 95° C. or higher and 145° C. or lower; The method for producing an extruded styrene resin foam, wherein the stretch ratio of the extruded foam in the step Sb is 1.01 times or more and 1.35 times or less.

[0009] [2] The method for producing an extruded styrene resin foam according to [1] above, wherein the heating temperature of the extruded foam in the step Sb is 115°C or higher and 145°C or lower.

[0010] [3] The method for producing an extruded styrene resin foam according to [1] or [2] above, wherein the stretch ratio of the extruded foam in the step Sb is 1.01 times or more and 1.20 times or less.

[0011] [4] A styrene-based resin extrusion foam molding containing a styrene-based resin, When stored for 24 hours at a temperature of 85°C, the deformation in the longitudinal direction is 10 mm or less, and the flat compressive strength is 25 N / cm 2 The above is the styrene-based resin extrusion foam molded product. Effect of the Invention

[0012] According to the present invention, it is possible to provide an extruded styrene resin foam that can suppress chipping of the end portion during cutting while ensuring plane compressive strength, and a method for producing the same. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a schematic diagram for explaining an example of a method for producing an extruded styrene resin foam according to the present invention. [Diagram 2] FIG. 2 is a plan view for explaining a method for measuring the deformation amount of a styrene-based resin extruded foam. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Preferred embodiments of the present invention will be described in detail below, but the present invention is not limited thereto. In addition, all academic and patent documents described in this specification are incorporated herein by reference.

[0015] Hereinafter, the compound and its derivatives may be collectively referred to by adding "based" after the compound name. In addition, when the polymer name is represented by adding "based" after the compound name, it means that the repeating unit of the polymer is derived from the compound or its derivative, unless otherwise specified. In addition, acrylic and methacrylic may be collectively referred to as "(meth)acrylic". In addition, acrylonitrile and methacrylonitrile may be collectively referred to as "(meth)acrylonitrile".

[0016] Unless otherwise specified, the components and functional groups exemplified in this specification may be used alone or in combination of two or more kinds.

[0017] The drawings referred to in the following description are intended to illustrate each component in a schematic manner for ease of understanding, and the size, number, shape, etc. of each component shown in the drawings may differ from the actual size, number, shape, etc., for convenience of drawing. Also, for convenience of explanation, in the drawings described later, the same components as those in the drawings described earlier may be given the same reference numerals, and explanations thereof may be omitted.

[0018] <First embodiment: Method for producing styrene-based resin extrusion foam> The method for producing a styrene-based resin extruded foam according to the first embodiment of the present invention includes steps Sa and Sb. In step Sa, a styrene-based resin composition containing a styrene-based resin and a foaming agent is extruded from a high-pressure region to a low-pressure region through a die lip to obtain an extruded foam. In step Sb, the extruded foam obtained in step Sa is stretched in the extrusion direction of step Sa while being heated. In the first embodiment, the heating temperature of the extruded foam in step Sb is 95°C or more and 145°C or less. Also, in the first embodiment, the stretch ratio of the extruded foam in step Sb is 1.01 times or more and 1.35 times or less.

[0019] Hereinafter, the "styrene-based resin extrusion foam" may be simply referred to as the "extrusion foam". The "extrusion direction of step Sa" may be simply referred to as the "extrusion direction". The "step Sa" may be simply referred to as the "extrusion step". The "step Sb" may be simply referred to as the "stretching step".

[0020] According to the manufacturing method of the extruded styrene-based resin foam according to the first embodiment, it is possible to manufacture an extruded styrene-based resin foam that can suppress chipping of the end portion during cutting while ensuring the plane compressive strength. The reason for this is presumed to be as follows.

[0021] In the first embodiment, the extruded foam obtained in the extrusion step is stretched at a stretch ratio of 1.01 or more while being heated at a temperature of 95°C or more. This allows the orientation direction of the bubbles to be appropriately aligned in the width direction (direction perpendicular to the stretching direction) of the obtained extruded foam, improving the cutting processability of the end portion of the extruded foam when cutting the obtained extruded foam along the width direction. Thus, according to the first embodiment, it is possible to produce an extruded foam that can suppress chipping of the end portion during cutting.

[0022] Moreover, if the temperature or stretch ratio is excessively increased in the stretching step, the cells tend to be too flattened, resulting in a low plane compressive strength of the extruded foam. In contrast, in the first embodiment, the upper limit of the heating temperature in the stretching step is set to 145°C, and the upper limit of the stretch ratio in the stretching step is set to 1.35 times, thereby preventing the cells from being excessively flattened. Thus, according to the first embodiment, the plane compressive strength of the extruded foam can be sufficiently ensured.

[0023] In the first embodiment, in order to further suppress chipping of the ends during cutting, the heating temperature of the extruded foam in the stretching step is preferably 100°C or higher, more preferably 105°C or higher, even more preferably 110°C or higher, even more preferably 115°C or higher, and may be 120°C or higher, 125°C or higher, or 130°C or higher.

[0024] In the first embodiment, in order to more easily ensure the plane compressive strength, the heating temperature of the extruded foam in the stretching step is preferably 140° C. or lower, and more preferably 135° C. or lower.

[0025] In the first embodiment, in order to further suppress chipping of the edges during cutting, the stretch ratio of the extruded foam in the stretching step is preferably 1.05 times or more, and more preferably 1.10 times or more.

[0026] In the first embodiment, in order to more easily ensure the plane compressive strength, the stretching ratio of the extruded foam in the stretching step is preferably 1.30 times or less, more preferably 1.25 times or less, and even more preferably 1.20 times or less.

[0027] In the first embodiment, in order to further suppress chipping of the ends during cutting while ensuring the planar compressive strength, the heating temperature of the extruded foam in the stretching step is preferably 115°C or higher and 145°C or lower, more preferably 115°C or higher and 140°C or lower, even more preferably 120°C or higher and 140°C or lower, even more preferably 125°C or higher and 140°C or lower, and particularly preferably 125°C or higher and 135°C or lower.

[0028] In the first embodiment, in order to more easily ensure the plane compressive strength while suppressing chipping of the end portion during cutting, the stretching ratio of the extruded foam in the stretching step is preferably 1.01 times or more and 1.20 times or less, more preferably 1.05 times or more and 1.20 times or less, and even more preferably 1.10 times or more and 1.20 times or less.

[0029] In the first embodiment, in order to more easily ensure planar compressive strength while more effectively suppressing chipping of the ends during cutting, it is preferable to satisfy the following condition 1, it is more preferable to satisfy the following condition 2, it is even more preferable to satisfy the following condition 3, it is even more preferable to satisfy the following condition 4, and it is particularly preferable to satisfy the following condition 5. Condition 1: The heating temperature of the extruded foam in the stretching step is 115° C. or more and 145° C. or less, and the stretch ratio of the extruded foam in the stretching step is 1.01 times or more and 1.20 times or less. Condition 2: The heating temperature of the extruded foam in the stretching step is 115° C. or more and 140° C. or less, and the stretch ratio of the extruded foam in the stretching step is 1.05 times or more and 1.20 times or less. Condition 3: The heating temperature of the extruded foam in the stretching step is 120° C. or more and 140° C. or less, and the stretch ratio of the extruded foam in the stretching step is 1.10 times or more and 1.20 times or less. Condition 4: The heating temperature of the extruded foam in the stretching step is 125° C. or more and 140° C. or less, and the stretch ratio of the extruded foam in the stretching step is 1.10 times or more and 1.20 times or less. Condition 5: The heating temperature of the extruded foam in the stretching step is 125° C. or more and 135° C. or less, and the stretch ratio of the extruded foam in the stretching step is 1.10 times or more and 1.20 times or less.

[0030] Hereinafter, an example of the method for producing an extruded styrene-based resin foam according to the first embodiment will be described with reference to the drawings as appropriate. Fig. 1 is a schematic diagram for explaining an example of the method for producing an extruded styrene-based resin foam according to the first embodiment.

[0031] 1, in the first embodiment, a styrene-based resin composition containing a styrene-based resin and a foaming agent is extruded through a die lip 11 of an extrusion device 10 to obtain an extruded foam 20 (extrusion step). At this time, the internal pressure of the extrusion device 10 is made higher than the pressure in the region where the styrene-based resin composition is extruded (e.g., atmospheric pressure), and the styrene-based resin composition is extruded from the high-pressure region of the extrusion device 10 to a low-pressure region, whereby the styrene-based resin composition is foamed to become the extruded foam 20.

[0032] In the example shown in FIG. 1, after obtaining the extruded foam 20, the thickness and width of the extruded foam 20 are adjusted by a molding die 30 installed in close contact with or close to the die lip 11 and a roll molding machine 40 installed downstream of the molding die 30. The molding die 30 includes two molding plates (not shown) installed at a predetermined interval. The roll molding machine 40 includes at least a pair of molding rolls 41 and 42. The thickness and width of the extruded foam 20 are adjusted by passing the extruded foam 20 between the two molding plates of the molding die 30 and then between the molding rolls 41 and 42. Although the molding die and roll molding machine are used in the example shown in FIG. 1, the molding die and roll molding machine may not be used in the present invention.

[0033] Next, the extruded foam 20 whose thickness and width have been adjusted is stretched in the extrusion direction (direction X in FIG. 1) (stretching step) by being drawn by a roll-type take-up machine 60 installed downstream of the heating furnace 50 while being heated in the heating furnace 50 installed downstream of the roll molding machine 40, to obtain an extruded foam 100. The roll-type take-up machine 60 has a pair of take-up rolls 61 and 62. In the example shown in FIG. 1, the stretch ratio in the extrusion direction of the extruded foam 20 is calculated by the formula "stretch ratio = rotation speed (linear speed) of the take-up rolls 61 and 62 of the roll-type take-up machine 60 / rotation speed (linear speed) of the molding rolls 41 and 42 of the roll molding machine 40". When the roll molding machine 40 has two or more pairs of molding rolls, the rotation speed of the molding roll in the above formula when calculating the stretch ratio is the rotation speed of the molding roll installed at the most downstream. Hereinafter, unless otherwise specified, the "rotation speed of the molding roll" refers to the rotation speed of the molding roll installed at the most downstream side. In the first embodiment, the heating temperature of the extruded foam 20 in the stretching step is 95°C or more and 145°C or less. In the first embodiment, the stretch ratio of the extruded foam 20 in the stretching step is 1.01 times or more and 1.35 times or less.

[0034] Next, each step of the method for producing a styrenic resin extrusion foam according to the first embodiment will be described. The method for producing a styrenic resin extrusion foam according to the first embodiment includes an extrusion step and a stretching step. The method for producing a styrenic resin extrusion foam according to the first embodiment may include steps other than the extrusion step and the stretching step. Steps other than the extrusion step and the stretching step include a resin composition preparation step and a melt-kneading step, which will be described below.

[0035] [Resin composition preparation process] In the resin composition preparation step, each material of the extrusion foam is blended to prepare a styrene-based resin composition. The styrene-based resin composition contains at least a styrene-based resin and a foaming agent. The foaming agent may be injected into the styrene-based resin composition containing materials other than the foaming agent in the subsequent melt-kneading step. An example of the material constituting the styrene-based resin composition will be described below.

[0036] (styrene resin) Examples of the styrene resin include homopolymers of styrene monomers, copolymers of two or more styrene monomers, and copolymers of styrene monomers and other monomers. The content of structural units derived from styrene monomers in the styrene resin is preferably 70% by weight or more, more preferably 80% by weight or more, and even more preferably 90% by weight or more. Examples of the copolymer include random copolymers, block copolymers, and graft copolymers.

[0037] Examples of styrene-based monomers include styrene, methylstyrene, dimethylstyrene, ethylstyrene, diethylstyrene, isopropylstyrene, bromostyrene, dibromostyrene, tribromostyrene, chlorostyrene, dichlorostyrene, trichlorostyrene, vinyltoluene, and vinylxylene. Examples of other monomers include polyfunctional vinyl compounds such as divinylbenzene; (meth)acrylic acid; (meth)acrylic acid ester compounds such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, and butyl methacrylate; cyanide vinyl compounds such as (meth)acrylonitrile; diene compounds such as butadiene; unsaturated carboxylic acid anhydrides such as maleic anhydride and itaconic anhydride; and N-alkyl-substituted maleimide compounds such as N-methylmaleimide, N-butylmaleimide, N-cyclohexylmaleimide, and N-phenylmaleimide. These may be used alone or in combination of two or more.

[0038] The styrene resin may be a blend of a homopolymer or copolymer of the above-mentioned styrene monomer and a homopolymer or copolymer of the above-mentioned other monomer. For example, the styrene resin may be blended with rubber-reinforced polystyrene (e.g., diene-rubber-reinforced polystyrene, acrylic-rubber-reinforced polystyrene, etc.), polyphenylene ether resin, etc.

[0039] As the styrene-based resin, from the viewpoints of being relatively inexpensive and suitable for extrusion foam molding, polystyrene (homopolymer of styrene), styrene-acrylonitrile copolymer, styrene-(meth)acrylic acid copolymer, styrene-maleic anhydride copolymer, and styrene-diene compound copolymer (for example, styrene-butadiene copolymer) are preferred. From the viewpoint of cost, the content of copolymer (for example, styrene-(meth)acrylic acid copolymer, etc.) in the styrene-based resin is preferably less than 25% by weight, more preferably less than 10% by weight. From the viewpoint of cost, a particularly preferred styrene-based resin is polystyrene.

[0040] The styrene resin may have a branched structure for the purpose of adjusting the melt flow rate, melt viscosity during molding, melt tension, etc. Hereinafter, the melt flow rate is referred to as MFR. The MFR of the styrene resin is preferably 40 g / 10 min or less, more preferably 1 g / 10 min or more and 30 g / 10 min or less. If the MFR of the styrene resin is 40 g / 10 min or less, it is easy to uniformly disperse the foaming agent in the styrene resin in the extrusion device, so that extrusion and foam molding can be performed stably, and as a result, production stability is improved. In this specification, the MFR of the styrene resin is a value measured according to the measurement method specified in JIS K7210 under conditions of a temperature of 200 ° C. and a load of 5 kg.

[0041] (foaming agent) Examples of the blowing agent include carbon dioxide, water, dimethyl ether, saturated hydrocarbons having 3 to 5 carbon atoms, alcohols having 1 to 4 carbon atoms, inorganic gases (more specifically, nitrogen, etc.), and organic fluorine compounds having a small global warming potential (more specifically, hydrofluoroolefins, hydrochlorofluoroolefins, etc.). These may be used alone or in combination of two or more.

[0042] Examples of saturated hydrocarbons having 3 to 5 carbon atoms include propane, normal butane, isobutane, normal pentane, isopentane, and neopentane. From the viewpoint of foamability, propane, normal butane, isobutane, and mixtures thereof are preferred. Also, from the viewpoint of heat insulating performance of extrusion foamed products, normal butane, isobutane, and mixtures thereof are preferred.

[0043] Examples of the alcohol having 1 to 4 carbon atoms include ethanol, methanol, propyl alcohol, isopropyl alcohol, butyl alcohol, isobutyl alcohol, and tert-butyl alcohol.

[0044] The amount of the foaming agent used (when multiple types of foaming agents are used, the total amount used) is preferably 1 part by weight or more and 20 parts by weight or less, and more preferably 5 parts by weight or more and 10 parts by weight or less, per 100 parts by weight of the styrene-based resin. When the amount of the foaming agent used is 1 part by weight or more and 20 parts by weight or less, the foaming power of the styrene-based resin composition is ensured, and it becomes easier to stably obtain an extruded foam molded article having a desired thickness.

[0045] (Flame retardant) As the flame retardant, a bromine-based flame retardant is preferably used. Specific examples of the bromine-based flame retardant include brominated bisphenol-based compounds such as tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl)ether and tetrabromobisphenol A-bis(2,3-dibromopropyl)ether; bromine-containing polymers such as brominated styrene-butadiene block copolymers, brominated styrene-butadiene random copolymers, and brominated styrene-butadiene graft copolymers; tetrabromocyclooctane; hexabromocyclododecane; tris(2,3-dibromopropyl)isocyanurate; and the like. These may be used alone or in combination of two or more.

[0046] From the viewpoint of economic efficiency and its influence on other required physical properties, the amount of the flame retardant used is preferably 0.5 parts by weight or more and 10 parts by weight or less, and more preferably 0.5 parts by weight or more and 7 parts by weight or less, per 100 parts by weight of the styrene-based resin.

[0047] The styrene-based resin composition may contain, as other additives, water-absorbing substances (bentonite, silica, etc.), cell size regulators (talc, etc.), lubricants (sodium stearate, calcium stearate, etc.), radical generators (2,3-dimethyl-2,3-diphenylbutane, poly-1,4-diisopropylbenzene, etc.), flame retardant assistants (triphenylphosphine oxide, etc.), stabilizers (epoxy compounds, polyhydric alcohol ester compounds, phenolic stabilizers, phosphite stabilizers, etc.), surfactants, flame retardant regulators (iron oxide, iron complexes, diphenylalkanes, diketones, etc.), processing aids (fatty acid metal salts, fatty acid amides, fatty acid esters, liquid paraffin, olefin waxes, etc.), antistatic agents, colorants (pigments, dyes, etc.), ultraviolet absorbers, fluorescent brighteners, plasticizers, fillers, etc. As the above-mentioned surfactants, alkylbenzenesulfonic acid, sodium alkylbenzenesulfonic acid salts, and sodium α-olefinsulfonic acid salts are preferred. Specific examples of the above surfactant include lauryl sulfates such as sodium lauryl sulfate, ammonium lauryl sulfate, and triethanolamine lauryl sulfate; and polyoxyethylene lauryl ether salts such as sodium polyoxyethylene lauryl ether sulfate, sodium polyoxyethylene lauryl ether acetate, and ammonium laureth sulfate.

[0048] [Melting and kneading process] In the melt-kneading step, the styrene-based resin composition is supplied to an extrusion device, and the styrene-based resin composition is melt-kneaded in the extrusion device. Examples of the extrusion device include an extrusion device equipped with an extruder using a screw. Examples of the extruder using a screw include a single-screw extruder and a twin-screw extruder. When a twin-screw extruder is used, the rotation directions of the screws may be the same or different.

[0049] The extrusion device may also include a first extruder for melt-kneading the foaming agent and a material other than the foaming agent, and a second extruder for further melt-kneading and cooling the melt-kneaded product obtained by the first extruder. When the extrusion device includes the second extruder, the foaming agent may be supplied to the second extruder. The type of the first extruder and the type of the second extruder may be the same or different. Furthermore, the extrusion device may include a cooler downstream of the extruder for the purpose of adjusting the temperature to a suitable temperature for foaming the styrene-based resin composition. At the most downstream of the extrusion device, a die lip is provided as an opening for extruding the styrene-based resin composition. For example, the die lip has a longitudinal length of 100 mm or more and 500 mm or less, and a lateral length of 1 mm or more and 7 mm or less.

[0050] The temperature when the styrene-based resin composition is melt-kneaded is, for example, 150° C. or more and 250° C. or less. When a cooler is used, the melt-kneaded product is preferably cooled in the cooler to a temperature of, for example, 100° C. or more and 140° C. or less.

[0051] [Extrusion process] In the extrusion step, the styrene resin composition (e.g., the molten mixture obtained in the melt-kneading step) is extruded from a high-pressure region through a die lip into a low-pressure region (e.g., into the atmosphere) to foam the styrene resin composition and obtain an extruded foam. The pressure (pressure in the high-pressure region) applied to the styrene resin composition immediately before being extruded from the die lip is, for example, 1.5 MPa or more and 15 MPa or less. As described above, the thickness and width of the extruded foam obtained in the extrusion step may be adjusted using a molding die and a roll molding machine.

[0052] [Stretching process] In the stretching step, the extruded foam obtained in the extrusion step is stretched in the extrusion direction while being heated. The heating temperature of the extruded foam in the stretching step is 95°C or more and 145°C or less. The heating time of the extruded foam in the stretching step is preferably 10 seconds or more and 240 seconds or less, more preferably 20 seconds or more and 90 seconds or less. The stretch ratio of the extruded foam in the stretching step is 1.01 times or more and 1.35 times or less. For example, as described above, when the roll molding machine, the heating furnace, and the roll type take-off machine are installed in this order, the rotation speed ratio of the rolls (rotation speed of the take-off roll of the roll type take-off machine / rotation speed of the molding roll of the roll molding machine) is the stretch ratio of the extruded foam in the stretching step. The rotation speed (linear speed) of the molding roll of the roll molding machine can be appropriately adjusted according to the production speed of the extruded foam, and is, for example, 2 m / min or more and 18 m / min or less.

[0053] In the first embodiment, after the stretching step, a step of cutting the obtained extruded foam according to the application may be provided.

[0054] [Extruded styrene resin foam obtained by the manufacturing method according to the first embodiment] Next, the extruded styrene resin foam molded product (hereinafter, sometimes referred to as "extruded foam molded product FM") obtained by the production method according to the first embodiment will be described.

[0055] Since the extruded foam FM is produced by the production method according to the first embodiment, it is possible to suppress chipping of the edge during cutting while ensuring the plane compressive strength. The extruded foam FM has a plane compressive strength of, for example, 25 N / cm when measured by the same method as in the examples described later. 2 More than 28N / cm 2 The extruded foam FM has an end chipped area of, for example, 500 mm2, as measured by the same method as in the Examples described below. 2 Less than or equal to 460 mm, preferably 2 The following is the result.

[0056] In order to further suppress chipping of the end portion during cutting, the amount of deformation in the longitudinal direction of the extruded foam molded product FM when stored for 24 hours at a temperature of 85° C. is preferably 10 mm or less, and more preferably 8 mm or less. Hereinafter, the amount of deformation in the longitudinal direction of the extruded foam molded product when stored for 24 hours at a temperature of 85° C. may be simply referred to as the "amount of deformation." The lower limit of the amount of deformation is not particularly limited, and may be 0 mm.

[0057] The method for measuring the amount of deformation will be described with reference to FIG. 2. FIG. 2 is a plan view for explaining the method for measuring the amount of deformation of an extruded foam molded product. First, a straight line L1 is drawn passing through both ends in the width direction at one end in the longitudinal direction (direction Y in FIG. 2) of the extruded foam molded product 100 after storage for 24 hours under a temperature condition of 85° C. Next, a straight line L2 is drawn along the width direction of the extruded foam molded product 100 at an interval of 50 mm from the straight line L1. Next, the shortest distance D1 (unit: mm) from the straight line L2 to the end in the longitudinal direction of the extruded foam molded product 100 is measured. Then, the amount of deformation D2 (unit: mm) is calculated according to the formula "D2=50-D1".

[0058] The deformation amount of the extruded foam FM can be adjusted, for example, by changing at least one of the heating temperature of the extruded foam in the stretching step and the stretch ratio of the extruded foam in the stretching step.

[0059] The thickness of the extruded foam FM is not particularly limited and is appropriately selected depending on the application. For example, in the case of a heat insulating material used for applications such as building materials (more specifically, a heat insulating material for tatami mats, etc.), in order to impart preferable heat insulating properties, bending strength, and plane compressive strength, the thickness of the extruded foam FM is preferably 10 mm or more, more preferably 15 mm or more, and even more preferably 20 mm or more. In addition, from the viewpoint of the processability of the extruded foam FM, the thickness of the extruded foam FM is preferably 150 mm or less, more preferably 100 mm or less, and even more preferably 50 mm or less.

[0060] In addition, in the case of extruded styrene-based resin foam molded products, after foam molding to give them a shape, the surface layer (skin layer) that was in contact with the mold may be removed by about 5 mm in the thickness direction to produce the final product, and the thickness of the extruded foam molded product FM is the thickness of the extruded foam molded product before the skin layer is removed.

[0061] In order to obtain a lightweight extruded foam molded product FM that is excellent in heat insulation, bending strength, and flat compressive strength, the density of the extruded foam molded product FM is 15 kg / m 3 More than 60kg / m 3 It is preferable that the thickness is less than 20 kg / m 3 More than 40kg / m 3 It is more preferable that:

[0062] In order to obtain an extruded foam FM having excellent heat insulation, bending strength, and plane compressive strength, the average cell diameter of the extruded foam FM is preferably 0.05 mm or more and 1.00 mm or less, more preferably 0.10 mm or more and 0.80 mm or less, even more preferably 0.15 mm or more and 0.60 mm or less, and particularly preferably 0.20 mm or more and 0.50 mm or less. In order to obtain an extruded foam FM having high heat insulation, the closed cell ratio of the extruded foam FM is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more. Since the extruded foam FM has good heat insulation, it can be used as a heat insulation material for houses and buildings (more specifically, a heat insulation material for tatami mats, etc.).

[0063] <Second embodiment: styrene-based resin extrusion foam> Next, a styrene-based resin extruded foam according to a second embodiment of the present invention will be described. In the following description, the description of the same content as in the first embodiment may be omitted.

[0064] The styrene-based resin extrusion foam according to the second embodiment contains a styrene-based resin. The styrene-based resin extrusion foam according to the second embodiment has a deformation amount (D2 in FIG. 2) of 10 mm or less and a plane compressive strength of 25 N / cm 2The styrene-based resin extrusion foam according to the second embodiment has a deformation amount of 10 mm or less and a plane compressive strength of 25 N / cm 2 For the above reasons, chipping of the end portion during cutting can be suppressed while ensuring the plane compressive strength.

[0065] The method for producing a styrene-based resin extrusion foam according to the second embodiment is to adjust the deformation amount to 10 mm or less while increasing the plane compressive strength to 25 N / cm 2 There are no particular limitations on the method as long as it can adjust the deformation to 10 mm or less. However, it is also possible to adjust the plane compressive strength to 25 N / cm 2 In order to easily adjust the above, the method for producing the styrenic resin extruded foam molded product according to the first embodiment is preferable as the method for producing the styrenic resin extruded foam molded product according to the second embodiment. When the styrenic resin extruded foam molded product according to the second embodiment is produced by the production method according to the first embodiment, the deformation amount and planar compressive strength can be adjusted, for example, by changing at least one of the heating temperature of the extruded foam in the stretching step and the stretch ratio of the extruded foam in the stretching step.

[0066] In order to further suppress chipping of the ends during cutting, it is preferable that the styrene-based resin extrusion foam according to the second embodiment does not contain methacrylic acid-modified polystyrene, or that the content of methacrylic acid-modified polystyrene is less than 25 weight % relative to the total amount of the styrene-based resin.

[0067] Other points of the second embodiment are the same as those described in the section [Extruded styrene resin foam obtained by the production method according to the first embodiment] above. EXAMPLES

[0068] Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0069] <Material preparation> The following materials were prepared as materials for producing extruded foam molded articles of the Examples and Comparative Examples.

[0070] [Styrene-based resin] Styrene resin (PS Japan "G9401", MFR: 2.2g / 10min)

[0071] [Flame retardant] Brominated styrene-butadiene block copolymer (LANXESS "EMERALD INNOVATION 3000", bromine content: 65% by weight)

[0072] [Water-absorbing substance] Bentonite (BYK "Bentolite L") Silica (Evonik Degussa Japan "Carplex BS-304F")

[0073] [Radical generator] Poly-1,4-diisopropylbenzene (United Initiators "CUROX CC-P3")

[0074] [Stabilizer] Bisphenol A diglycidyl ether (ADEKA "EP-13") Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyhydrocinnamate)] (Rianlon "RIANOX 1010FF") 3,9-bis(2,4-di-tert-butylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane (SONGWON "SONGNOX 6260FF") Orthocresol novolac epoxy resin (DIC "EPICLON N-680") Reaction mixture of dipentaerythritol and adipic acid (Ajinomoto Fine-Techno Co., Ltd. "Plenriser ST210")

[0075] [Lubricant] Calcium stearate ("SC-P" manufactured by Sakai Chemical Industry Co., Ltd.)

[0076] [Bubble size adjuster] Talc (Hayashi Kasei "KHP-400")

[0077] [Surfactants] Sodium lauryl sulfate (Kao Corporation's "Emeral 10PT")

[0078] [Foaming agent] Odorless butane (Iwatani Corporation, a mixture of isobutane and normal butane, weight ratio: isobutane / normal butane = 30 / 70) Dimethyl ether (manufactured by Iwatani Corporation) Water (tap water)

[0079] <Preparation of extruded foam> The methods for producing the extruded foams of Examples 1 to 6 and Comparative Examples 1 to 5 will be described below.

[0080] [Example 1] (Resin composition preparation process) 100 parts by weight of a styrene-based resin, 2.6 parts by weight of a brominated styrene-butadiene block copolymer, 0.1 parts by weight of poly-1,4-diisopropylbenzene, 0.2 parts by weight of a reaction mixture of dipentaerythritol and adipic acid, 0.2 parts by weight of bisphenol A diglycidyl ether, 0.26 parts by weight of pentaerythritol tetrakis [3- (3,5-di-tert-butyl-4-hydroxyhydrocinnamate)], and 3,9-bis A resin composition was prepared by dry blending 0.013 parts by weight of (2,4-di-tert-butylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, 0.13 parts by weight of orthocresol novolac epoxy resin, 1.0 parts by weight of talc, 0.2 parts by weight of calcium stearate, 0.5 parts by weight of bentonite, 0.3 parts by weight of silica, and 0.06 parts by weight of sodium lauryl sulfate.

[0081] (Melting and kneading process) The obtained resin composition was fed at a feed rate of 800 kg / hour into the first extruder of an extrusion device in which a single screw extruder (first extruder) with a diameter of 150 mm, a single screw extruder (second extruder) with a diameter of 200 mm, and a cooler were connected in series in this order. Then, the resin composition was melt-kneaded in the first extruder while being heated at a temperature of 230°C to obtain a melt-kneaded product. Next, 3.5 parts by weight of odorless butane, 3.0 parts by weight of dimethyl ether, and 0.7 parts by weight of water were injected into the melt-kneaded product near the outlet of the first extruder with respect to 100 parts by weight of styrene-based resin. Then, the mixture was kneaded in the second extruder connected to the first extruder, and the temperature (resin temperature) of the melt-kneaded product was cooled to 123°C by a cooler connected to the second extruder.

[0082] (Extrusion process) Next, the molten mixture (styrene resin composition) was extruded into the air from a die lip (length of the opening in the longitudinal direction: 400 mm, length of the opening in the transverse direction: 2 mm) having a rectangular opening provided at the tip of the cooling machine, and foamed. The pressure applied to the styrene resin composition immediately before being extruded from the die lip was 7 MPa. Next, the extruded styrene resin composition was passed through a molding die (gap between two molding plates: 22 mm) placed in close contact with the die lip and a roll molding machine (gap between upper and lower molding rolls: 25 mm, rotation speed of molding rolls: 13 m / min) placed downstream of the die lip, to obtain an extruded foam (plate-shaped extruded foam) having a rectangular cross-sectional shape of 35 mm thick x 1000 mm wide. Then, the stretching process shown below was carried out continuously from this extrusion process.

[0083] (Stretching process) The extruded foam obtained in the above extrusion step was stretched in the extrusion direction by being taken up by a roll-type take-up machine installed downstream while being heated for 40 seconds in a heating furnace set at an internal atmospheric temperature of 130° C., thereby obtaining the extruded foam of Example 1. When the extruded foam was taken up, the stretch ratio in the extrusion direction of the extruded foam (= rotation speed of the take-up roll of the roll-type take-up machine / rotation speed of the molding roll of the roll molding machine) was adjusted to be 1.17 times.

[0084] The obtained extruded foam was cut with a cutter to a thickness of 25 mm × width of 910 mm × length of 1820 mm to obtain a measurement sample. When adjusting the thickness of the extruded foam, the skin layers on both sides that had been in contact with the mold were removed.

[0085] [Examples 2 to 6 and Comparative Examples 1 to 5] Extruded foams (measurement samples) of Examples 2 to 6 and Comparative Examples 1 to 5 were obtained in the same manner as in Example 1, except that the heating temperature and stretch ratio of the extruded foam in the stretching step were as shown in Table 1 below.

[0086] <Measurement method> [Deformation amount] After preparation, the extruded foam (measurement sample) was cut at room temperature for 14 days to obtain a molded product having a thickness of 25 mm, a width of 910 mm, and a length (length in the extrusion direction) of 300 mm. The obtained molded product was heated for 24 hours in a thermostatic chamber (dry oven) set at an internal atmospheric temperature of 85° C., and then the heated molded product was removed from the thermostatic chamber and allowed to stand for 24 hours in an atmosphere at a temperature of 25° C. Next, the deformation amount of the molded product (D2 in FIG. 2) was measured by the above-mentioned measurement method.

[0087] [Plane Compressive Strength] After preparation, the extruded foam (measurement sample) was left at room temperature for 14 days, and the flat compressive strength was measured according to JIS K7220:2006. The flat compressive strength was 25N / cm 2 In the above cases, it was evaluated that "the plane compressive strength of the extruded foam is ensured." On the other hand, if the plane compressive strength is 25N / cm 2 When the compressive strength was less than this, it was evaluated that "the plane compressive strength of the extruded foam could not be ensured."

[0088] [Edge chip area] After preparation, the extruded foam molded product (measurement sample) was cut at room temperature for 14 days to obtain a molded product having a thickness of 25 mm × width of 300 mm × length (length in the extrusion direction) of 350 mm. A region from one short side end face (side face) of the obtained molded product to 60 mm was cut with a knife blade at a cutting speed of 500 mm / min and an insertion angle of the cutting blade of 45°. The dimensions of the cut region (cut region) were a thickness of 25 mm × width of 300 mm × length (length in the extrusion direction) of 60 mm. The area of ​​the chipped region (end chipped area) at the end (corner) on the cut side of the molded product from which the cut region had been removed was calculated. When the end chipped area was 500 mm 2 In the following cases, it was evaluated that "chipping at the edge during cutting can be suppressed." On the other hand, when the area of ​​chipped edge is 500 mm 2 If the chipping area exceeds 100%, it is evaluated as "not being able to suppress chipping of the edge during cutting." Note that the "chipped edge area" refers to the area of ​​the larger of the two surfaces (main surfaces) perpendicular to the thickness direction of the chipped area.

[0089] [density] After preparation, the extruded foam (measurement sample) was cut at room temperature for 14 days to obtain a molded product having a thickness of 25 mm, a width of 100 mm, and a length (length in the extrusion direction) of 100 mm. The density of the obtained molded product was measured in accordance with JIS A9521:2020.

[0090] <Result> For Examples 1 to 6 and Comparative Examples 1 to 5, the heating temperature of the extruded foam in the stretching step, the stretch ratio of the extruded foam in the stretching step, the deformation amount, the planar compressive strength, and the end chipped area are shown in Table 1. In Table 1, "heating temperature" and "stretch ratio" mean "heating temperature of the extruded foam in the stretching step" and "stretch ratio of the extruded foam in the stretching step", respectively.

[0091] [Table 1]

[0092] As shown in Table 1, in Examples 1 to 6, the heating temperature of the extruded foam in the stretching step was 95° C. or more and 145° C. or less. In Examples 1 to 6, the stretch ratio of the extruded foam in the stretching step was 1.01 times or more and 1.35 times or less.

[0093] As shown in Table 1, in Examples 1 to 6, the plane compressive strength was 25 N / cm 2 Thus, in Examples 1 to 6, the planar compressive strength of the obtained extruded foams was ensured. 2 Thus, in Examples 1 to 6, chipping of the edges when cutting the obtained extruded foam molded articles was suppressed.

[0094] As shown in Table 1, in Comparative Examples 1 and 2, the heating temperature of the extruded foam in the stretching step was less than 95° C. In Comparative Example 3, the heating temperature of the extruded foam in the stretching step exceeded 145° C. In Comparative Examples 1 and 5, the stretch ratio of the extruded foam in the stretching step was less than 1.01 times. In Comparative Example 4, the stretch ratio of the extruded foam in the stretching step exceeded 1.35 times.

[0095] As shown in Table 1, in Comparative Examples 3 and 4, the plane compressive strength was 25 N / cm 2 Therefore, the planar compressive strength of the extruded foams obtained in Comparative Examples 3 and 4 was not ensured. 2 Therefore, in Comparative Examples 1, 2 and 5, chipping of the end portions when the obtained extruded foam molded articles were cut could not be suppressed.

[0096] The above results demonstrate that the present invention can provide an extruded styrene resin foam that can suppress chipping of the edges during cutting while ensuring planar compressive strength. [Explanation of symbols]

[0097] 11: Die Lip 20: Extruded foam 100: Extruded foam (styrene-based resin extruded foam)

Claims

1. A step Sa of extruding a styrene-based resin composition containing a styrene-based resin and a foaming agent from a high pressure region through a die lip to a low pressure region to obtain an extruded foam; A step Sb of stretching the extruded foam in the extrusion direction of the step Sa while heating the extruded foam; A method for producing an extruded styrene resin foam comprising: The heating temperature of the extruded foam in the step Sb is 95° C. or higher and 145° C. or lower; The method for producing an extruded styrene-based resin foam, wherein the stretch ratio of the extruded foam in the step Sb is 1.01 times or more and 1.35 times or less.

2. The method for producing a styrene-based resin extruded foam according to claim 1, wherein the heating temperature of the extruded foam in the step Sb is 115°C or higher and 145°C or lower.

3. The method for producing an extruded styrene resin foam according to claim 1 or 2, wherein a stretch ratio of the extruded foam in the step Sb is 1.01 times or more and 1.20 times or less.

4. A styrene-based resin extrusion foam molding containing a styrene-based resin, When stored for 24 hours at a temperature of 85°C, the deformation in the longitudinal direction is 10 mm or less, and the plane compressive strength is 25 N / cm 2 The above is the styrene-based resin extrusion foam molded product.

Citation Information

Patent Citations

  • Method for producing polystyrene-based resin extruded foam

    JP2013124281A