Chemical-mechanical polishing slurry and method for manufacturing semiconductor element using the same

The use of a chemical mechanical polishing slurry with controlled temperature and composition addresses the issues of flatness and time in semiconductor manufacturing by optimizing etch and removal rates, thereby improving the efficiency of metal layer polishing.

JP2024137847APending Publication Date: 2024-10-07SAMSUNG ELECTRONICS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024043363
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-03-19
Publication Date
2024-10-07

Smart Images

  • Figure 2024137847000001_ABST
    Figure 2024137847000001_ABST
Patent Text Reader

Abstract

To provide a chemical-mechanical polishing slurry used for chemical-mechanical polishing of metal layers and a method for manufacturing a semiconductor element using the same.SOLUTION: A chemical-mechanical polishing slurry has an aqueous solution containing deionized water, abrasive particles, and a temperature-sensitive oxidizing agent, and the temperature-sensitive oxidizing agent is configured to adjust both the static etch rate of the metal layer and the removal rate of the metal layer during the chemical-mechanical polishing process when the polishing temperature of the chemical-mechanical polishing process is between 10°C and 75°C.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a chemical mechanical polishing slurry and a method for manufacturing a semiconductor device using the same, and more particularly to a chemical mechanical polishing slurry for chemical mechanical polishing of a metal layer and a method for manufacturing a semiconductor device using the same. [Background technology]

[0002] As integration density increases in semiconductor devices (or integrated circuit devices), multi-layer wiring structures are used to interconnect functional elements such as transistors, capacitors, and resistors. To manufacture semiconductor devices with multi-layer wiring structures, a chemical mechanical polishing process is required to planarize the metal layer. A chemical mechanical polishing slurry is used in the chemical mechanical polishing process of the metal layer. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-80436 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made in consideration of the above-mentioned conventional technology, and an object of the present invention is to provide a chemical mechanical polishing slurry that improves the flatness of a metal layer during chemical mechanical polishing of the metal layer and reduces the chemical mechanical polishing time, and a method for manufacturing a semiconductor device using the same. [Means for solving the problem]

[0005] In order to achieve the above object, according to one aspect of the present invention, a chemical mechanical polishing slurry comprises an aqueous solution containing deionized water, abrasive particles, and a temperature sensitive oxidant, and the temperature sensitive oxidant is configured to be capable of controlling both a static etch rate of a metal layer and a removal rate of the metal layer during a chemical mechanical polishing process when the polishing temperature of the chemical mechanical polishing process is 10°C to 75°C.

[0006] In accordance with another aspect of the present invention, a chemical mechanical polishing slurry is provided, which comprises deionized water, abrasive particles, and an aqueous solution including a temperature-sensitive oxidant capable of controlling both a static etch rate and a removal rate of the tungsten layer during a chemical mechanical polishing process when the polishing temperature is 10° C. to 75° C., a pH adjuster, and a catalyst.

[0007] According to one aspect of the present invention, there is provided a method for manufacturing a semiconductor device, the method comprising the steps of: forming an insulating pattern on a substrate to have a plurality of openings spaced apart from one another in a horizontal direction; forming a metal layer on the insulating pattern to fill the openings; and performing a chemical mechanical polishing process on the metal layer on a polishing pad using a chemical mechanical polishing slurry with the insulating pattern as an etch stop film, the chemical mechanical polishing process being performed at a polishing temperature in the range of 10° C. to 75° C., the chemical mechanical polishing slurry comprising an aqueous solution containing deionized water, abrasive particles, and a temperature sensitive oxidant, the temperature sensitive oxidant being capable of controlling both a static etch rate of the metal layer and a removal rate of the metal layer during the chemical mechanical polishing process when the polishing temperature of the chemical mechanical polishing process is 10° C. to 75° C. Effect of the Invention

[0008] The chemical mechanical polishing slurry of the present invention is an aqueous solution containing deionized water, abrasive particles, and a temperature-sensitive oxidant capable of controlling both the static etch rate and the removal rate of the metal layer when the polishing temperature of the chemical mechanical polishing is 10°C to 75°C. Therefore, when the chemical mechanical polishing step (or process) of the metal layer is performed using the chemical mechanical polishing slurry of the present invention, the flatness of the metal layer can be improved and the polishing time can be reduced. [Brief description of the drawings]

[0009] [Figure 1] 1 is a schematic cross-sectional view showing an example of a chemical mechanical polishing apparatus using a chemical mechanical polishing slurry according to one embodiment of the present invention; [Diagram 2] FIG. 2 is a schematic top view of an example of a chemical mechanical polishing apparatus using a chemical mechanical polishing slurry in accordance with one embodiment of the present invention. [Diagram 3] 1 is a cross-sectional view illustrating a method for manufacturing a semiconductor device including a chemical mechanical polishing step using a chemical mechanical polishing slurry according to an embodiment of the present invention. [Figure 4] 1 is a cross-sectional view illustrating a method for manufacturing a semiconductor device including a chemical mechanical polishing step using a chemical mechanical polishing slurry according to an embodiment of the present invention. [Diagram 5] FIG. 4 illustrates the change in polishing temperature over time during a chemical mechanical polishing step according to one embodiment of the present invention. [Figure 6] FIG. 4 illustrates the change in polishing temperature over time during a chemical mechanical polishing step according to one embodiment of the present invention. [Figure 7] FIG. 4 is a diagram showing the static etch rate of a metal layer as a function of polishing temperature when using a chemical mechanical polishing slurry according to an embodiment of the present invention. [Figure 8] FIG. 8 is a diagram showing the static etching rate of a metal layer as a function of polishing temperature when a comparative example chemical mechanical polishing slurry is used for comparison with FIG. 7. [Figure 9]FIG. 13 is a diagram showing the removal rate of a metal layer depending on the polishing temperature when using a chemical mechanical polishing slurry according to an embodiment of the present invention and a chemical mechanical polishing slurry of a comparative example. [Figure 10] FIG. 4 is a diagram showing the recess depth of a metal pattern as a function of polishing temperature when using a chemical mechanical polishing slurry according to an embodiment of the present invention. [Figure 11] FIG. 11 is a diagram showing the recess depth of a metal pattern depending on the polishing temperature when a comparative example of a chemical mechanical polishing slurry is used for comparison with FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, specific examples of the embodiments of the present invention will be described in detail with reference to the drawings. The following embodiments of the present invention may be embodied alone or in combination with one or more of the following embodiments. Therefore, the technical idea of ​​the present invention should not be interpreted as being limited to one embodiment.

[0011] In this specification, the singular form of an element may include the plural form unless the context clearly indicates otherwise. In this specification, the drawings are exaggerated in order to more clearly explain the present invention.

[0012] The present inventors have invented a chemical mechanical polishing slurry that can improve the flatness of a metal layer, such as a tungsten layer, during chemical mechanical polishing of the metal layer and reduce the polishing time.

[0013] In one embodiment, the chemical mechanical polishing slurry is an aqueous solution including deionized water, abrasive particles, and a temperature-sensitive oxidizing agent capable of controlling both the static etch rate and the removal rate of the metal layer when the polishing temperature of the chemical mechanical polishing is 60°C to 75°C.

[0014] In one embodiment, the abrasive particles include at least one of silica, alumina, ceria, titania, zirconia, magnesia, germania, and mangania, and the concentration of the abrasive particles is 1% by weight (wt%) to 10% by weight (wt%) in the aqueous solution. In one embodiment, the abrasive particles are silica, and the concentration of the silica is 1% by weight (wt%) to 10% by weight (wt%) in the aqueous solution.

[0015] In one embodiment, the temperature sensitive oxidizer comprises at least one of sodium persulfate, sodium percarbonate, sodium perborate, sodium perborate monohydrate, and sodium perborate tetrahydrate.

[0016] In one embodiment, the temperature sensitive oxidizing agent is sodium persulfate, and the concentration of sodium persulfate in an aqueous solution is 0.5% by weight (wt%) to 5% by weight (wt%).

[0017] In one embodiment, the aqueous solution constituting the chemical mechanical polishing slurry further includes a pH adjusting agent. In one embodiment, the pH adjusting agent is potassium hydroxide (KOH), ammonium hydroxide (NH 4At least one of tetramethylamine (TMA), tetramethylammonium hydroxide (TMAH), and tetraethylamine (TEA). In one embodiment, the aqueous solution has a pH of 1 to 8. In one embodiment, the aqueous solution has a pH of 1 to 3.

[0018] In one embodiment, the aqueous solution constituting the chemical mechanical polishing slurry further comprises a catalyst, which may include at least one of ferric nitrate, potassium ferricyanide, iron chloride, iron sulfate, iron fluoride, iron bromide, copper chloride, copper fluoride, and copper bromide.

[0019] In one embodiment, the catalytic agent is ferric nitrate, and the concentration of ferric nitrate is 1 weight percent (wt%) to 2 weight percent (wt%) in an aqueous solution.

[0020] An example of a chemical mechanical polishing apparatus using the chemical mechanical polishing slurry of the present invention will now be described.

[0021] FIG. 1 is a schematic cross-sectional view showing an example of a chemical mechanical polishing apparatus using a chemical mechanical polishing slurry according to one embodiment of the present invention, and FIG. 2 is a schematic top view showing an example of a chemical mechanical polishing apparatus using a chemical mechanical polishing slurry according to one embodiment of the present invention.

[0022] Specifically, the chemical mechanical polishing apparatus 20 includes a rotatable, disk-shaped platen 24 on which a polishing pad 30 is positioned. The chemical mechanical polishing apparatus 20 is referred to as a polishing station. The platen 24 rotates about a central axis 25. The platen 24 rotates about the central axis 25 as indicated by arrow A in FIG. 2. A motor 22 rotates a drive shaft 28 to rotate the platen 24.

[0023] In one embodiment, polishing pad 30 is a dual polishing pad having a lower polishing pad 34 and an upper polishing pad 32. Upper polishing pad 32 is made of a softer material than lower polishing pad 34. Chemical mechanical polishing apparatus 20 includes a polishing fluid delivery system 50 for delivering a chemical mechanical polishing slurry 52 (or polishing fluid) onto polishing pad 30 through port 54.

[0024] Polishing fluid supply system 50 includes an arm 56 supported by a base 58 for extending over platen 24. A port 54 is disposed at the end of arm 56. Port 54 is coupled through a control valve 60 and piping 61 to a polishing fluid supply 62, such as a reservoir or tank that stores chemical mechanical polishing slurry 52.

[0025] A carrier head 70 operates to support the substrate 10 in contact with the polishing pad 30. As will be described below, the substrate 10 is a substrate structure having a metal layer formed thereon. The carrier head 70 is referred to as a polishing head. The carrier head 70 is coupled to a support structure 72. The carrier head 70 is rotated about an axis 71 by being coupled to a rotational motor 76 by a drive shaft 74.

[0026] Carrier head 70 includes a flexible membrane 80 having a substrate mounting surface for contacting the back (or rear) surface of substrate 10, and a pressure chamber 82 for applying pressure onto substrate 10. Carrier head 70 includes a retaining ring 84 for supporting (holding) substrate 10. Retaining ring 84 includes a lower retaining ring 86 and an upper retaining ring 88.

[0027] During operation of the chemical mechanical polishing apparatus 20, the platen 24 rotates about its central axis 25 and the carrier head 70 rotates about its central axis 71, as shown by arrow B in FIG. 2, and moves laterally across the top surface of the polishing pad 30, as shown by arrow C in FIG. 2.

[0028] Chemical mechanical polishing apparatus 20 includes a pad conditioner 90 having a conditioner disk 92 held by a conditioner head 93 at the end of a conditioner arm 94. Conditioner disk 92 is used to maintain the surface roughness of polishing pad 30. Conditioner arm 94 is supported by a conditioner base 95.

[0029] The chemical mechanical polishing apparatus 20 includes a temperature sensor 64 for monitoring the temperature of the chemical mechanical polishing slurry 52 on the polishing pad 30 and / or the polishing pad 30. For example, the temperature sensor 64 is an infrared (IR) sensor, such as an IR camera, located on the polishing pad 30 and configured to measure the temperature of the chemical mechanical polishing slurry 52 on the polishing pad 30 and / or the polishing pad 30.

[0030] The temperature sensor 64 is configured to measure the temperature at multiple points along the radius of the polishing pad 30 to generate a radial temperature profile. For example, the IR camera that constitutes the temperature sensor 64 has a field of view that spans the radius of the polishing pad 30.

[0031] 1, the temperature sensor 64 is a contact sensor, rather than a non-contact sensor. For example, the temperature sensor 64 is a thermocouple or IR thermometer located on or at the platen 24. The temperature sensor 64 directly contacts the polishing pad 30. In one embodiment, the temperature sensors 64 are positioned at multiple spaced radial locations on the polishing pad 30 to provide the temperature at multiple points along the radius of the polishing pad 30.

[0032] Temperature sensor 64 is positioned to monitor the temperature of polishing pad 30 and / or chemical mechanical polishing slurry 52 on polishing pad 30, and as illustrated in Figure 1, temperature sensor 64 is positioned inside carrier head 70 to measure the temperature of substrate 10. Temperature sensor 64 is a contact sensor that directly contacts substrate 10, i.e., a semiconductor wafer.

[0033] The chemical mechanical polishing apparatus 20 includes a temperature control system 100 for controlling the temperature of the chemical mechanical polishing slurry 52 on the polishing pad 30 and / or the polishing pad 30. The temperature control system 100 delivers a temperature controlled fluid onto the polishing surface 36 of the polishing pad 30. The temperature control system 100 delivers a temperature controlled fluid (118, 138) onto the chemical mechanical polishing slurry 52 already present on the polishing pad 30. The temperature control system 100 includes a heating system 102 and a cooling system 104.

[0034] The heating system 102 delivers a heating fluid 118, such as hot water or steam. The cooling system 104 delivers a cooling fluid 138, such as cold water or chilled air. The heating fluid 118 and the cooling fluid 138 are delivered through apertures (114, 134) and nozzles 116 provided by the arms (110, 130).

[0035] In one embodiment, the heating system 102 includes an arm 110 that extends over the platen 24 and polishing pad 30 from the edge of the polishing pad 30 to or at least near the center of the polishing pad 30. The arm 110 is supported by a base 112. The base 112 is supported on the same frame 40 as the platen 24.

[0036] Base 112 includes one or more actuators, such as a linear actuator for raising or lowering arm 110 and / or a rotational actuator for swinging arm 110 laterally over platen 24. Arm 110 is positioned to avoid collisions with other hardware components, such as carrier head 70, pad conditioning disk 92, chemical mechanical polishing slurry delivery arm 56, and cooling fluid delivery arm 130.

[0037] A number of openings 114 are formed in the bottom surface of the arm 110. The openings 114 are configured to direct a heated fluid 118, such as a gas or vapor (or steam), onto the polishing pad 30. In one embodiment, the openings 114 are connected to nozzles 116 that direct the heated fluid 118, which is discharged in a spray form, onto the polishing pad 30. Although the openings 114 and the nozzles 116 are shown separately in FIG. 1, the openings 114 and the nozzles 116 may be the same, or the nozzles 116 may not be connected and may directly discharge the heated fluid 118 in a spray form through the openings 114.

[0038] The openings 114 direct the heating fluid 118 to radiating features 124 on the polishing pad 30. Although the openings 114 are illustrated in Figure 2 as being evenly spaced apart, this is not a requirement. The openings 114 may be more densely spaced toward the center of the polishing pad 30. Although nine openings 114 are illustrated in Figure 2, there may be more or fewer openings 114.

[0039] The arm 110 is supported by a base 112 so as to be spaced apart from the polishing pad 30. A separation distance 126 between the opening 114 (and / or the nozzle 116) and the polishing pad 30 is 0.5 to 5 mm. In particular, the separation distance 126 is selected so that heat from the heating fluid 118 is not significantly dissipated before the heating fluid 118 reaches the polishing pad 30. For example, the separation distance 126 is selected so that the heating fluid 118 discharged from the opening 114 does not condense before it reaches the polishing pad 30.

[0040] The heating system 102 includes a source 120 of heating fluid 118 that is coupled to the arm 110 through a control valve 122 and fluid piping 123. In one embodiment, the source 120 is a steam generator, such as a vessel in which water is boiled to produce steam gas.

[0041] The heating fluid 118 may be mixed with other gases (e.g., air) and / or liquids (e.g., heated water), or the heating fluid 118 may be substantially pure steam. When steam is used as the heating fluid 118, the temperature of the steam is between 90°C and 200°C when the steam is generated in the fluid source 120. The temperature of the steam is between 90°C and 150°C when the steam is distributed through the openings 114, e.g., due to heat losses during transport. In one embodiment, the steam is delivered through the openings 114 at a temperature between 60°C and 100°C, e.g., between 60°C and 75°C.

[0042] The chemical mechanical polishing apparatus 20 includes a cooling system 104. The cooling system 104 is configured similarly to the heating system 102 as described above. An arm 130 is supported by a base 132. The arm 130 is connected to a source 140 through a control valve 142 and piping 143. However, the source 140 is a source of cooling fluid 138, and the cooling system 104 supplies the cooling fluid 138 in the form of a spray onto the polishing pad 30.

[0043] The cooling fluid 138 is a liquid, such as water at or below 20° C., a gas at or below 20° C., or a mixture of liquid and gas. The cooling fluid is air with aerosolized water droplets. The openings 134 have the same configuration as the openings 114 that supply the heating fluid described above. The openings 134 have the same connection configuration as the nozzles 116 described above.

[0044] The chemical mechanical polishing apparatus 20 includes a controller 200 for controlling the operation of various components, such as the polishing fluid supply system 50 and the temperature control system 100. The controller 200 is configured to receive temperature measurements from the temperature sensor 64. The controller 200 compares the measured temperature to a target temperature and controls the control valves 122 and / or 142 to control the flow of heating and / or cooling fluid onto the polishing pad 30 to achieve the target temperature.

[0045] 3 and 4 are cross-sectional views illustrating a method for manufacturing a semiconductor device including a chemical mechanical polishing step using a chemical mechanical polishing slurry according to an embodiment of the present invention.

[0046] 3 and 4 includes a chemical mechanical polishing step, which is performed using the chemical mechanical polishing apparatus 20 of FIGS.

[0047] 3, an insulating pattern 202 having a plurality of openings 204 spaced apart from one another in the horizontal direction is formed on a substrate 10. The insulating pattern 202 is obtained by forming an insulating film on the substrate 10 and then selectively etching the insulating film using a photolithography process to form openings 204 that expose predetermined regions of the substrate 10.

[0048] The substrate 10 may be any of various substrates used in the manufacture of semiconductor devices. In one embodiment, the substrate 10 may be a silicon substrate. The insulating pattern 202 may include an oxide film-based and / or nitride film-based material. For example, the insulating pattern 202 may be formed using any one of boron phosphosilicate glass (BPSG), phosphosilicate glass (PSG), high density plasma (HDP), tetraethyl orthosilicate (TEOS), and undoped silica glass (USG).

[0049] The insulating pattern 202 is formed by using a physical vapor deposition (PVD) method, a chemical vapor deposition (CVD) method, a metal organic CVD (MOCVD) method, or an atomic layer deposition (ALD) method. The insulating pattern 202 includes an opening 204 that exposes a predetermined region of the substrate 10 to form wiring and / or plugs. The opening 204 is a linear trench.

[0050] A barrier layer 206 is formed on the insulating pattern 202 and the substrate 10. The barrier layer 206 is formed of titanium nitride or the like. The barrier layer 206 is not formed if necessary. Subsequently, a metal layer 208 is formed on the barrier layer 206 so as to sufficiently fill the opening 204. In one embodiment, the metal layer 208 is a tungsten film.

[0051] Referring to FIG. 4, as described above, the metal layer 208 is chemically mechanically polished using the surface 214 of the insulating pattern 202 as an etch stop film using a chemical mechanical polishing slurry (52 in FIG. 1) on a polishing pad (30 in FIG. 1 and FIG. 2) of a chemical mechanical polishing apparatus (20 in FIG. 1 and FIG. 2).

[0052] A barrier pattern 210 and a metal pattern 212 are formed in the opening 204 by chemical mechanical polishing of the metal layer 208. The metal pattern 212 is recessed from a surface 214 of the insulating pattern 202 by chemical mechanical polishing. If the recess depth 216 of the metal pattern 212 is shallow, the planarity of the metal pattern 212 is improved. In one embodiment, the recess depth 216 is 1% to 5% or less of the height h1 of the insulating pattern 202.

[0053] The chemical mechanical polishing step is accomplished by a combination of mechanical abrasion and chemical etching of the metal layer 208 on the substrate 10 at the interface between the metal layer 208 and the polishing pad 30 using a chemical mechanical polishing slurry (52 in FIG. 1).

[0054] As described above, the chemical mechanical polishing step (process) controls the polishing temperature, for example, the temperature of the chemical mechanical polishing slurry (52 in FIG. 1) itself or by supplying a heating fluid or a cooling fluid to the chemical mechanical polishing slurry (52 in FIG. 1) supplied onto the polishing pad (30 in FIGS. 1 and 2).

[0055] As a result, the inventors have invented a chemical mechanical polishing slurry that can adjust the static etch rate and removable rate (polishing rate) of the metal layer 208 by controlling the polishing temperature in the chemical mechanical polishing step (process).

[0056] When the chemical mechanical polishing slurry of the present invention is used, the chemical mechanical polishing step can shorten the polishing time and improve the flatness of the metal pattern 212. This will be described in more detail later. First, the change in the polishing temperature over time in the chemical mechanical polishing step (process) will be described.

[0057] 5 and 6 are diagrams illustrating the change in polishing temperature over time during the chemical mechanical polishing step according to one embodiment of the present invention.

[0058] Specifically, the chemical mechanical polishing step is performed using the chemical mechanical polishing apparatus 20 of Figures 1 and 2. The chemical mechanical polishing step is the chemical mechanical polishing of the metal layer 208 of Figures 3 and 4. The chemical mechanical polishing step includes a first standby step (SB1), a first chemical mechanical polishing step (CMP1), a second chemical mechanical polishing step (CMP2), and a second standby step (SB2).

[0059] The first standby stage (SB1) and the second standby stage (SB2) are at a polishing temperature, i.e., the temperature of the chemical mechanical polishing slurry (52 in FIG. 1 and FIG. 2) of T1. In one embodiment, T1 is 20°C.

[0060] In one embodiment, the first chemical mechanical polishing step (CMP1) increases the temperature of the chemical mechanical polishing slurry to T2, for example, 25° C. to 75° C., to perform the first chemical mechanical polishing of the metal layer 208. In one embodiment, the first chemical mechanical polishing step (CMP1) increases the temperature of the chemical mechanical polishing slurry to T2, for example, 60° C. to 75° C., to perform the first chemical mechanical polishing of the metal layer 208.

[0061] In Fig. 5, the polishing temperature is increased rapidly from the first standby stage (SB1) to the first chemical mechanical polishing stage (CMP1), whereas in Fig. 6, the polishing temperature is increased gradually from the first standby stage (SB1) to the first chemical mechanical polishing stage (CMP1).

[0062] In the second chemical mechanical polishing step (CMP2), the temperature of the chemical mechanical polishing slurry is lowered to a temperature T3, for example, 10°C to 20°C, to perform the second chemical mechanical polishing of the metal layer 208. In FIG. 5, the polishing temperature is suddenly lowered from the first chemical mechanical polishing step (CMP1) to the second chemical mechanical polishing step (CMP2). In FIG. 6, the polishing temperature is gradually lowered from the first chemical mechanical polishing step (CMP1) to the second chemical mechanical polishing step (CMP2). In FIG. 6, the polishing temperatures in the second chemical mechanical polishing step (CMP2) and the second standby step (SB2) are approximately the same.

[0063] In the chemical mechanical polishing step of the present invention, the chemical mechanical polishing slurry (52 in FIG. 1) shortens the polishing time and improves the flatness of the metal pattern 212 in a polishing temperature range of T1 to T3, for example, 15° C. to 75° C. Furthermore, in the chemical mechanical polishing step of the present invention, the chemical mechanical polishing slurry (52 in FIG. 1) shortens the polishing time and improves the flatness of the metal pattern 212 in a polishing temperature range of T2, for example, 60° C. to 75° C.

[0064] FIG. 7 is a graph showing the static etch rate of a metal layer as a function of polishing temperature when using a chemical mechanical polishing slurry according to one embodiment of the present invention, and FIG. 8 is a graph showing the static etch rate of a metal layer as a function of polishing temperature when using a comparative chemical mechanical polishing slurry for comparison with FIG. 7.

[0065] Specifically, the chemical mechanical polishing slurry EMB according to an embodiment of the present invention shown in Fig. 7 is manufactured as follows. 0.1 wt% silica as abrasive particles and ferric nitrate as a catalyst were added to deionized water. Sodium persulfate as a temperature sensitive oxidant was added to deionized water containing silica and ferric nitrate to manufacture the chemical mechanical polishing slurry EMB according to an embodiment of the present invention.

[0066] The chemical mechanical polishing slurry CEX according to the comparative example shown in Figure 8 was manufactured as follows. 0.1 wt% silica as abrasive particles and ferric nitrate as a catalyst were added to deionized water. In the comparative example, hydrogen peroxide was added as an oxidizing agent to deionized water containing silica and ferric nitrate to manufacture the chemical mechanical polishing slurry CEX.

[0067] The static etch rate (SER) of a substrate was evaluated using the chemical mechanical polishing slurry EMB according to an embodiment of the present invention and the chemical mechanical polishing slurry CEX according to a comparative example. The static etch rate SER was measured by measuring the amount of the metal layer etched away after the substrate was immersed in the chemical mechanical polishing slurry EMB according to an embodiment of the present invention and the chemical mechanical polishing slurry CEX according to a comparative example, respectively, to etch the metal layer.

[0068] When using the chemical mechanical polishing slurry EMB according to one embodiment of the present invention, the static etching rate SER of a metal layer, for example a tungsten layer, is 1 Å / min at a polishing temperature of 25° C., and the static etching rate SER of the metal layer is 11 Å / min at a polishing temperature of 60° C. When using the chemical mechanical polishing slurry EMB according to one embodiment of the present invention, even when the polishing temperature is increased from 25° C. to 60° C., the static etching rate SER of the metal layer does not increase significantly and remains low.

[0069] When the comparative example chemical mechanical polishing slurry CEX is used, the static etching rate SER of the metal layer is 32 Å / min at a polishing temperature of 25° C., and the static etching rate SER of the metal layer is 696 Å / min at a polishing temperature of 60° C. When the comparative example chemical mechanical polishing slurry CEX is used, the static etching rate SER of the metal layer increases significantly when the polishing temperature is increased from 25° C. to 60° C.

[0070] When the comparative chemical mechanical polishing slurry CEX is used, the static etching rate of the metal layer increases significantly with an increase in polishing temperature, so that the recess depth of the metal pattern increases with an increase in polishing temperature, resulting in a lower flatness of the metal pattern. On the other hand, when the chemical mechanical polishing slurry EMB of the present invention is used, the static etching rate of the metal layer does not increase significantly with an increase in polishing temperature, so that the recess depth of the metal pattern decreases with an increase in polishing temperature, resulting in a higher flatness of the metal pattern.

[0071] FIG. 9 is a diagram showing the metal layer removal rate RR depending on the polishing temperature when the chemical mechanical polishing slurry according to the embodiment of the present invention and the chemical mechanical polishing slurry of the comparative example are used.

[0072] In particular, the process for preparing the chemical mechanical polishing slurry EMB according to the embodiment of the present invention and the chemical mechanical polishing slurry CEX according to the comparative example have been described with reference to FIGS. 7 and 8, so that the description thereof will be omitted here.

[0073] The removal rate RR (or polishing rate) of a metal layer during chemical mechanical polishing of a metal layer (e.g., a tungsten layer) was evaluated using the chemical mechanical polishing slurry EMB according to an embodiment of the present invention and the chemical mechanical polishing slurry CEX of a comparative example. The chemical mechanical polishing has been described in FIG. 3 and FIG. 4, so the description thereof will be omitted here.

[0074] When using the chemical mechanical polishing slurry EMB according to an embodiment of the present invention, the removal rate RR of the metal layer, for example the tungsten layer, is 723 Å / min at a polishing temperature of 25° C., and the removal rate RR of the metal layer is 1021 Å / min at a polishing temperature of 60° C. When using the chemical mechanical polishing slurry EMB according to an embodiment of the present invention, the removal rate RR of the metal layer increases as the polishing temperature increases from 25° C. to 60° C.

[0075] When the comparative chemical mechanical polishing slurry CEX is used, the metal layer removal rate RR is 785 Å / min at a polishing temperature of 25° C., and the metal layer removal rate RR is 1202 Å / min at a polishing temperature of 60° C. When the comparative chemical mechanical polishing slurry CEX is used, the metal layer removal rate RR increases as the polishing temperature increases from 25° C. to 60° C. When the chemical mechanical polishing slurry EMB of the present invention is used, the metal layer removal rate RR increases with an increase in polishing temperature, and the polishing time can be reduced.

[0076] FIG. 10 is a graph showing the recess depth of a metal pattern depending on the polishing temperature when using a chemical mechanical polishing slurry according to one embodiment of the present invention, and FIG. 11 is a graph showing the recess depth of a metal pattern depending on the polishing temperature when using a comparative chemical mechanical polishing slurry for comparison with FIG. 10.

[0077] In particular, the process for preparing the chemical mechanical polishing slurry EMB according to the embodiment of the present invention and the chemical mechanical polishing slurry CEX according to the comparative example have been described with reference to FIGS. 7 and 8, so that the description thereof will be omitted here.

[0078] The recess depth of a metal pattern during chemical mechanical polishing of a metal layer (e.g., a tungsten layer) was evaluated using the chemical mechanical polishing slurry EMB according to an embodiment of the present invention and the chemical mechanical polishing slurry CEX of a comparative example. The chemical mechanical polishing has been described in FIG. 3 and FIG. 4, so the description thereof will be omitted here.

[0079] When using the chemical mechanical polishing slurry EMB according to one embodiment of the present invention, the recess depth of the metal pattern, e.g., the tungsten pattern, of the substrate edge portion CE is 69 Å at a polishing temperature of 25°C, and the recess depth of the metal pattern of the substrate edge portion CE is 87 Å at a polishing temperature of 60°C.

[0080] In addition, when using the chemical mechanical polishing slurry EMB according to one embodiment of the present invention, the recess depth of the metal pattern in the central portion CC of the substrate is 94 Å at a polishing temperature of 25°C, and the recess depth of the metal pattern in the central portion CE of the substrate is 105 Å at a polishing temperature of 60°C.

[0081] When the comparative chemical mechanical polishing slurry CEX is used, the recess depth of the metal pattern at the substrate edge portion CE is 168 Å at a polishing temperature of 25° C., and the recess depth of the metal pattern at the substrate edge portion CE is 273 Å at a polishing temperature of 60° C.

[0082] When the comparative chemical mechanical polishing slurry CEX is used, the recess depth of the metal pattern in the central portion CC of the substrate is 215 Å at a polishing temperature of 25°C, and the recess depth of the metal pattern in the central portion CE of the substrate is 324 Å at a polishing temperature of 60°C.

[0083] When the chemical mechanical polishing slurry EMB according to the embodiment of the present invention is used, the recess depth of the metal pattern is decreased depending on the polishing temperature, and the recess depth of the metal pattern does not increase significantly even when the polishing temperature is increased, compared to when the chemical mechanical polishing slurry CEX of the comparative example is used. Therefore, when the chemical mechanical polishing slurry EMB of the present invention is used, the recess depth of the metal pattern can be decreased depending on the polishing temperature, and the flatness of the metal pattern can be improved.

[0084] Although the embodiments of the present invention have been described in detail above with reference to the drawings, the present invention is not limited to the above-described embodiments and can be modified in various ways without departing from the technical spirit of the present invention. [Explanation of symbols]

[0085] 10 Substrate 20 Chemical mechanical polishing equipment 22 Motor 24 Platen 25 Center axis 28 Drive shaft 30 Polishing Pad 32, 34 Upper and lower polishing pads 36 Polished surface 40 frames 50 Polishing Fluid Supply System 52 Chemical Mechanical Polishing Slurry 54 Port 56 (for chemical mechanical polishing slurry supply) arm 58, 112, 132 base 60, 122, 142 Control valve 61, 143 Piping 62 Polishing liquid supply section 64 Temperature Sensor 70 Career Head 71 Axis 72 Support structure 74 Drive shaft 76 Rotational Motor 80 Flexible Membrane 82 Pressurized Chamber 84 Retaining ring 86, 88 Lower and upper retaining rings 90 Pad Conditioner 92 Pad conditioning disc 93 Conditioner Head 94 Conditioner Arm 95 Conditioner Base 100 Temperature Control System 102 Heating System 104 Cooling System 110 Arm 114, 134 aperture 116 Nozzle 0 118 Heating fluid 120 (Fluid) Source 123 Fluid Piping 124 Radiation form 126 Separation distance 130 (for cooling fluid supply) arm 138 Cooling fluid 140 Source 200 Controller 202 Insulation Pattern 204 Opening 206 Barrier Layer 208 Metal layer 210 Barrier Pattern 212 Metal Pattern 214 Surface 216 Recess depth

Claims

1. Deionized water; Abrasive particles; An aqueous solution containing a temperature sensitive oxidant is provided, The chemical mechanical polishing slurry is characterized in that the temperature sensitive oxidant is configured to be capable of controlling both a static etch rate and a removal rate of the metal layer during the chemical mechanical polishing process when the polishing temperature of the chemical mechanical polishing process is 10° C. to 75° C.

2. The abrasive particles include at least one of silica, alumina, ceria, titania, zirconia, magnesia, germania, and mangania; 2. The chemical mechanical polishing slurry of claim 1, wherein the temperature sensitive oxidizing agent comprises at least one of sodium persulfate, sodium percarbonate, sodium perborate, sodium perborate monohydrate, and sodium perborate tetrahydrate.

3. The aqueous solution further comprises a pH adjuster; The pH adjuster may be potassium hydroxide (KOH), ammonium hydroxide (NH 4 OH), tetramethylamine (TMA), tetramethylammonium hydroxide (TMAH), and tetraethylamine (TEA); 2. The chemical mechanical polishing slurry of claim 1, wherein the aqueous solution has a pH of 1-8.

4. The aqueous solution further comprises a catalytic agent; 2. The chemical mechanical polishing slurry of claim 1, wherein the catalytic agent comprises at least one of ferric nitrate, potassium ferricyanide, iron chloride, iron sulfate, iron fluoride, iron bromide, copper chloride, copper fluoride, and copper bromide.

5. Deionized water; Abrasive particles; A temperature-sensitive oxidant configured to adjust both a static etch rate and a removal rate of the tungsten layer during a chemical mechanical polishing process when the polishing temperature of the chemical mechanical polishing process is 10° C. to 75° C.; A pH adjuster; and A chemical mechanical polishing slurry comprising an aqueous solution containing a catalyst.

6. The temperature-sensitive oxidizing agent is sodium persulfate.

6. The chemical mechanical polishing slurry of claim 5, wherein the concentration of the sodium persulfate in the aqueous solution is 0.5 to 5 weight percent (wt%).

7. forming an insulating pattern on a substrate, the insulating pattern having a plurality of openings spaced apart from one another in a horizontal direction; forming a metal layer on the insulating pattern to fill the opening; performing a chemical mechanical polishing process on the metal layer through the etch stop layer of the insulating pattern using a chemical mechanical polishing slurry on a polishing pad; The chemical mechanical polishing process is carried out at a polishing temperature in the range of 10° C. to 75° C. The chemical mechanical polishing slurry is Deionized water; Abrasive particles; a temperature sensitive oxidant; The temperature-sensitive oxidant is configured to be capable of controlling both a static etch rate and a removal rate of the metal layer during a chemical mechanical polishing process when the polishing temperature of the chemical mechanical polishing process is 10° C. to 75° C.

8. 8. The method of claim 7, wherein the step of performing the chemical mechanical polishing process includes: increasing a temperature of the chemical mechanical polishing slurry to 60° C. to 75° C. to perform a first chemical mechanical polishing of the metal layer; and decreasing a temperature of the chemical mechanical polishing slurry to 10° C. to 20° C. to perform a second chemical mechanical polishing of the metal layer.

9. performing a chemical mechanical polishing process includes chemically mechanically polishing the metal layer to form a plurality of metal patterns filled in the openings; the metal pattern has a recess depth recessed into a surface of the insulating pattern; 8. The method of claim 7, wherein the recess depth is 1% to 5% or less of the height of the insulating pattern.

10. The temperature sensitive oxidizing agent contained in the chemical mechanical polishing slurry is sodium persulfate, 8. The method of claim 7, wherein the concentration of the sodium persulfate in the aqueous solution is 0.5% by weight to 5% by weight.

Citation Information

Patent Citations

  • Polishing slurry and method of manufacturing semiconductor device

    JP2021080436A