Slab and continuous casting method
By adding Zr, Hf, and Y to high-Al steels to form stabilizing nitrides, the method addresses transverse cracking issues during continuous casting, ensuring stable and crack-free processing.
Patent Information
- Application Number
- JP2023050304
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
Smart Images

Figure 2024139391000001_ABST
Abstract
Description
[Technical field]
[0001] In particular, the present invention relates to a slab containing a large amount of Al and a continuous casting method thereof. [Background technology]
[0002] In recent years, alloy steels containing large amounts of Al have been widely produced as high-strength steel materials to improve their mechanical properties. However, the more Al added, the more susceptible the steel is to transverse cracks on the surface of the slab during continuous casting, which is problematic in terms of both operation and product quality.
[0003] At the straightening point in a curved or vertical bending type continuous casting machine, a straightening stress is applied to the slab. It is known that transverse cracks occur along the prior austenite grain boundaries on the surface of the slab, and the transverse cracks occur when the straightening stress is concentrated on the austenite grain boundaries embrittled by the precipitation of AlN, NbC, etc., or on the film-like ferrite formed along the prior austenite grain boundaries. In addition, these transverse cracks tend to occur particularly in a temperature range slightly higher than the phase transformation region from austenite to ferrite, but transverse cracks also occur in non-transformation compositions. Therefore, a method is usually adopted to control the surface temperature of the slab so as to avoid the temperature range (embrittlement temperature range) where ductility decreases at the straightening point, thereby suppressing the occurrence of transverse cracks.
[0004] However, controlling the surface temperature of a slab to avoid the embrittlement temperature range is often difficult because it imposes significant constraints on operation. Therefore, Patent Document 1 discloses a technique in which Ti is added in an amount of more than 0.010 mass% and not more than 0.025 mass%, and the surface temperature of the slab in the upper part of the secondary cooling zone, where the solidified shell thickness of the slab is 10 mm to 30 mm, is made equal to or higher than the precipitation temperature of AlN. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-22498 A Summary of the Invention [Problem to be solved by the invention]
[0006] In recent years, high-Al steel containing 0.2 mass% or more of Al has been produced to further improve mechanical properties. As the Al concentration increases, AlN precipitates at a higher temperature, expanding the embrittlement temperature range. Therefore, when the steel contains 0.2 mass% or more of Al, the embrittlement temperature range expands significantly, making it almost impossible to perform bending and straightening while avoiding the embrittlement temperature range, and transverse cracks cannot be avoided.
[0007] Furthermore, the method described in Patent Document 1 targets low-carbon aluminum-killed steel with an Al concentration of 0.063 mass % to 0.093 mass %, and its effect on high-Al steel containing 0.2 mass % or more of Al is unclear.
[0008] In view of the above-mentioned problems, an object of the present invention is to provide a slab of high-Al steel containing 0.2 mass % or more of Al, which has excellent cracking susceptibility, and a method for continuous casting of the same. [Means for solving the problem]
[0009] The inventors of the present invention have focused on the fact that the high-temperature embrittlement of high-Al steel slabs is caused by the precipitation of a large amount of AlN, and have investigated the control of nitride precipitation. Specifically, they have investigated the high-temperature ductility of steels to which Zr, Hf, and Y, which have a higher N fixing ability than Al, have been added. As a result, they have found that the addition of these elements significantly improves high-temperature ductility. Zr, Hf, and Y form ZrN, HfN, and YN, or composite nitrides of these elements, respectively, and fix N, thereby suppressing the precipitation of a large amount of AlN at grain boundaries, and it has been found that the high-temperature embrittlement of high-Al steels can be drastically improved.
[0010] In particular, Hf and Y have a higher affinity with nitrogen than Zr, and the thermal stability of the nitrides is improved. Therefore, it was found that the addition of Hf and / or Y more stably suppresses the precipitation of large amounts of AlN, thereby more reliably suppressing transverse cracks.
[0011] Based on the above, the present invention is as follows. [1] In mass%, C: 0.02% to 0.50%, Si: 0.20% to 3.00%, Mn: 0.50%~4.00%, Al: 0.20% to 2.00% N: 0.01% or less, Zr: 0% to 0.05%, Hf: 0%~0.05%, Y: 0%~0.05%, Ti: 0% to 0.002%, Nb: 0% to 0.1%, V: 0%~0.1%, B: 0%~0.005%, Cr: 0%~0.1%, Ni: 0% to 0.5%, and Cu: 0% to 0.5%, The remainder is made of Fe and impurities, The contents of Zr, Hf, and Y satisfy the following formulas (1) and (2), A cast slab, characterized in that the total number ratio of ZrN, HfN, YN or composite nitrides thereof to all nitrides at a position 5 mm deep from the surface of the cast slab is 50% or more. [Zr]+91 / 178×[Hf]+91 / 89×[Y]≧4 / 3×[Al]×[N] ···(1) [Hf]+[Y]≧0.001% (2) Here, [Zr], [Hf], [Y], [Al], and [N] each represent the content (mass%) in the cast slab. [2] The continuous casting method according to the above [1], The method for continuous casting of a slab, wherein bending and straightening of the slab are performed at a surface temperature in the range of 800°C to 1000°C. [3] The method for continuous casting of a slab according to the above [2], characterized in that the average cooling rate in the surface layer of the slab is 60°C / min or less. Effect of the Invention
[0012] According to the present invention, it is possible to provide a slab of high Al steel containing 0.2 mass % or more of Al and having excellent cracking susceptibility, and a continuous casting method for obtaining the slab. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a diagram showing the relationship between the Zr, Hf, and Y contents and the Al and N contents. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be described below with reference to the drawings. First, the chemical composition of a slab according to an embodiment of the present invention will be described. In the following description, "%", which is the unit of the content of each element contained in the slab, means "mass%" unless otherwise specified. Furthermore, a numerical range expressed using "to" means a range including the numerical values written before and after "to" as the lower and upper limits. Furthermore, examples of impurities include those contained in raw materials such as ores and scraps, and those contained in the manufacturing process. Furthermore, examples of slabs containing the following components include steel slabs such as slabs and blooms.
[0015] <C:0.02%~0.50%> C is an element that improves the strength of steel, and if the C content is less than 0.02%, the steel will not meet the requirements for use as a high-strength steel plate. If the C content exceeds 0.50%, the hardness will be too high and the necessary bendability cannot be ensured. Therefore, the C content is set to 0.02% to 0.50%.
[0016] <Si:0.20%~3.00%> Si is an element that improves the strength of steel. If the Si content is less than 0.20%, it cannot meet the requirements for use as a high-strength steel plate. Also, if the Si content exceeds 3.00%, it will have an adverse effect on weldability. Therefore, the Si content is set to 0.20% - 3.00%.
[0017] <Mn: 0.50% - 4.00%> Mn is an element that improves the strength of steel. If the Mn content is less than 0.50%, it cannot meet the requirements for use as a high-strength steel plate. Also, if the Mn content exceeds 4.00%, since Mn is a segregation element, it may cause uneven strength in the slab or steel plate. Therefore, the Mn content is set to 0.50% - 4.00%.
[0018] <Al: 0.20% - 2.00%> Al is an element necessary to improve mechanical properties. In this embodiment, it is assumed that Al is contained at 0.20% or more. On the other hand, if the Al content exceeds 2.00%, as will be described later, the contents of Zr, Hf, and Y also need to be increased, resulting in an unnecessary cost increase. Therefore, the Al content is set to 0.20% - 2.00%.
[0019] <N: 0.01% or less> N is an element contained through normal refining processes and continuous casting processes. Since it inevitably exists in steel and forms nitrides, which have an adverse effect on high-temperature ductility, the lower the N content, the better the ductility tends to be. Therefore, the N content is set to 0.01% or less. Also, although less N is more preferable, considering the cost in the refining process, the N content is preferably 0.001% or more.
[0020] <Zr: 0% - 0.05%> Zr is an element that reacts with nitrogen to form nitrides, and inhibits the precipitation of AlN, greatly improving the high-temperature ductility of high-Al steel. As will be described in detail later, when a specified amount of Hf and / or Y is contained, Zr is not essential and may be 0%. On the other hand, if the Zr content exceeds 0.05%, not only will the effect saturate, but coarse Zr inclusions will form, which will become the starting point of defects during the rolling process and cause deterioration of material properties, so the Zr content is set to 0.05% or less.
[0021] <Hf:0%~0.05%> Hf is an element that reacts with nitrogen to form nitrides, suppressing the precipitation of AlN and greatly improving the high-temperature ductility of high-Al steel. As will be described in detail later, when a certain amount of Y is contained, Hf is not essential and can be 0%. On the other hand, if the Hf content exceeds 0.05%, the effect saturates, resulting in unnecessary cost increases. Therefore, the Hf content is set to 0.05% or less.
[0022] <Y:0%~0.05%> Y is an element that reacts with nitrogen to form nitrides, suppressing the precipitation of AlN and greatly improving the high-temperature ductility of high-Al steel. As will be described in detail later, when a specified amount of Hf is contained, Y is not essential and may be 0%. On the other hand, if the Y content exceeds 0.05%, the effect saturates, resulting in unnecessary cost increases. Therefore, the Y content is set to 0.05% or less.
[0023] The balance other than the above is Fe and impurities, but some other components may be included in place of a portion of Fe. Specifically, the cast slab according to this embodiment may further include Ti: 0% to 0.002%, Nb: 0% to 0.1%, V: 0% to 0.1%, B: 0% to 0.005%, Cr: 0% to 0.1%, Ni: 0% to 0.5%, and Cu: 0% to 0.5%.
[0024] <Ti:0%~0.002%> Ti reacts with nitrogen to form complex nitrides together with Zr and other elements, suppressing the formation of AlN and improving high-temperature ductility. However, if Ti is included in excess, the effect saturates, resulting in unnecessary costs. Therefore, the Ti content is set to 0.002% or less.
[0025] <Nb:0%~0.1%> Nb is an element that reacts with nitrogen to form nitrides, and also contributes to improving strength. However, if there is an excessive amount of Nb, the effect saturates, resulting in unnecessary costs. Furthermore, the nitrides that form expand the embrittlement temperature range, just like AlN. Therefore, the Nb content is set to 0.1% or less.
[0026] <V:0%~0.1%> V is an element that reacts with nitrogen to form nitrides, and also contributes to improving strength. However, if there is an excessive amount of V, the effect saturates, resulting in unnecessary costs. Furthermore, the nitrides that are formed expand the embrittlement temperature range, just like AlN. Therefore, the V content is set to 0.1% or less.
[0027] <B:0%~0.005%> B segregates to the austenite grain boundaries in steel, strengthening the grain boundaries and improving the high-temperature ductility of high-Al steel. However, if B is included in excess, the effect saturates and unnecessary costs are incurred. Therefore, the B content is set to 0.005% or less.
[0028] <Cr:0%~0.1%> Cr is an element that reacts with nitrogen to form nitrides, and also contributes to improving strength. However, if Cr is included in excess, the effect saturates, resulting in unnecessary costs. Furthermore, the nitrides that are formed expand the embrittlement temperature range, just like AlN. Therefore, the Cr content is set to 0.1% or less.
[0029] <Ni:0%~0.5%> Ni is also an element that contributes to improving strength and toughness. However, if Ni is contained in excess, the effect becomes saturated and unnecessary costs are incurred. Therefore, the Ni content is set to 0.5% or less.
[0030] <Cu:0%~0.5%> Cu exists in steel as fine particles and contributes to improving strength. However, excessive Cu content can deteriorate the material properties of steel. Therefore, the Cu content is set to 0.5% or less.
[0031] In addition, when analyzing these chemical compositions, the sample is taken from a position representative of the composition of the slab, that is, 1 / 4 width part and 1 / 4 thickness part on the upper surface side of the cross section perpendicular to the casting direction, and each element is analyzed by a known method.
[0032] Next, conditions for preventing transverse cracks from occurring in high Al steel will be described. First, in the continuous casting of high Al steel, it is necessary to prevent transverse cracks from occurring due to the straightening stress at the straightening point during continuous casting. Since it is difficult to make the temperature at the straightening point outside the brittle temperature range, the inventors performed a high-temperature tensile test to confirm the extent to which high-temperature ductility is improved by adding Zr, Hf, and Y, on the premise that the straightening of the slab is performed in a general temperature range at the straightening point. In the high-temperature tensile test, a high-frequency induction heating type high-temperature tensile test device with a cold crucible was used, and the tensile test piece was melted and then cooled to a predetermined tensile temperature at a cooling rate of 1.0°C / s, and then was held at the predetermined tensile temperature while straining at a strain rate of 3.3×10 -4 The specimen was subjected to tension at a speed of (1 / s) until fracture. The area reduction rate (%) was calculated as (cross-sectional area of the tensile test specimen before the test - cross-sectional area of the tensile test specimen after fracture) / cross-sectional area of the tensile test specimen before the test x 100. As a result, it was found that the addition of Zr, Hf, and Y increases the area reduction rate, especially in the temperature range of 800 to 1000°C, and improves high-temperature ductility.
[0033] Next, tests were conducted to confirm how much Zr, Hf, and Y needed to be added to prevent transverse cracks. Specifically, the tensile temperature was set to 900°C, and a number of samples with different amounts of Al, N, Zr, Hf, and Y were prepared and subjected to high-temperature tensile tests to determine the cross-sectional shrinkage (%) of each. The specific method of the high-temperature tensile test was the same as that described above. As a guideline, it was determined that transverse cracks would not occur if the cross-sectional shrinkage was 50% or more.
[0034] As a result of the tests, it was found that the contents of Zr, Hf, and Y are correlated with the product of the Al content and the N content. By converting Zr, Hf, and Y into molar ratios based on Zr, it was found that if the value of Zr content + (91 / 178) × Hf content + (91 / 89) × Y content is 4 / 3 times or more the product of the Al content and the N content, the cross-sectional reduction rate will be 50% or more, and transverse cracks due to straightening stress at the straightening point during continuous casting can be prevented.
[0035] From the above experimental results, the cast piece according to this embodiment contains Zr, Hf and Y in amounts that satisfy the following formula (1). [Zr]+91 / 178×[Hf]+91 / 89×[Y]≧4 / 3×[Al]×[N] (1) Here, [Zr], [Hf], [Y], [Al], and [N] each represent the content (mass%) in the continuously cast slab.
[0036] On the other hand, it was found that when the amount of Hf and / or Y is extremely small, cracks may occur when the resulting slab is heated and hot rolled. The reason for this is thought to be that Zr has a higher affinity with nitrogen than Al, but a lower affinity with nitrogen than Hf and Y, and the thermal stability of the nitrides is not sufficient. In other words, by including a certain amount of Hf and / or Y nitrides, the proportion of Zr, Hf, and Y nitrides increases, and a high crack prevention effect is obtained even when the slab is heated and hot rolled.
[0037] For the above reasons, the cast piece according to this embodiment further contains Hf and / or Y in an amount that satisfies the following formula (2). [Hf]+[Y]≧0.001% (2)
[0038] FIG. 1 is a diagram showing the relationship between the content of Zr, Hf, and Y and the content of Al and N. In FIG. 1, the straight line 10 represents the boundary line that satisfies formula (1), and the area above the straight line represents the condition that satisfies formula (1). Also, the circle marks represent examples in which transverse cracks were not confirmed in the slab and were not confirmed after hot rolling, and the cross marks represent examples in which transverse cracks were confirmed in the slab or hot-rolled sheet. As shown in FIG. 1, it was found that no cracks occurred in any of the cases except for plot 11 under the conditions to the left of the straight line 10. Note that all of the examples in plot 11 are examples in which formula (1) is satisfied but formula (2) is not satisfied, and in all cases, transverse cracks were not confirmed in the slab, but transverse cracks were confirmed after hot rolling.
[0039] Next, the nitrides in the slab will be described. As described above, Zr, Hf, and Y generate ZrN, HfN, and YN, respectively, and fix N, so that the precipitation of a large amount of AlN at the grain boundaries can be suppressed, and the high-temperature embrittlement of high-Al steel can be drastically improved. Therefore, in the slab according to this embodiment, as a guideline for the depth of the transverse crack, the total number ratio of ZrN, HfN, YN, or composite nitrides of these in all nitrides at a position 5 mm deep from the surface is 50% or more. It is preferably 60% or more, and more preferably 75% or more.
[0040] Here, the total number ratio of ZrN, HfN, YN or these composite nitrides in all nitrides can be measured by the following method. First, a surface 5 mm from the surface of the slab is observed (field of view is, for example, 50 μm × 50 μm) with a scanning electron microscope (SEM) equipped with an energy dispersive X-ray analyzer (EDS), and nitrides with a circle equivalent diameter of 200 nm to 5000 nm are identified. Next, the identified nitrides are separated into nitrides in which the total of Zr, Hf, and Y is 50 mass% or more in the nitrides and nitrides in which the total of Zr, Hf, and Y is not 50 mass% in the nitrides, and the number ratio is calculated by dividing the number of nitrides in which the total of Zr, Hf, and Y is 50 mass% or more in the nitrides by the total number of nitrides. When the area of the observation range is 50 mm 2 If this is the case, it can be regarded as the number density at a position 5 mm from the surface of the slab.
[0041] Next, the above-mentioned continuous casting method for the slab will be described. In this embodiment, since there is no need to avoid the embrittlement temperature range, a method that is particularly common in continuous casting can be used for the slab having the above-mentioned composition. From the above-mentioned experimental results, it is preferable to bend and straighten the slab when the surface temperature of the slab is 800°C to 1000°C, as this is particularly effective.
[0042] In order to stably produce ZrN, HfN, YN or composite nitrides thereof, when cooling a slab having the above-mentioned composition, it is preferable to set the average cooling rate at the surface layer of the slab to 60°C / min or less. Here, the average cooling rate refers to the average cooling rate from 1450 to 1000°C, and the surface layer of the slab refers to a position 5 mm deep from the surface of the center of the width of the slab. As a measurement method, the surface temperature of the center of the width of the slab is measured using a thermocouple or the like, and the average cooling rate at a position 5 mm deep is calculated by two-dimensional heat transfer calculation. If the average cooling rate is too small, the operating time will be unnecessarily long, so it is preferable that the average cooling rate at the surface layer of the slab is 5°C / min or more. EXAMPLES
[0043] Next, an embodiment of the present invention will be described, but the conditions are merely examples of conditions for confirming the feasibility and effects of the present invention, and the present invention is not limited to the description of the embodiment. The present invention can be implemented in various ways to achieve the object of the present invention without departing from the gist of the present invention.
[0044] Seventeen types of molten steel, the compositions of which are shown in Table 1, were prepared and each was poured into a mold and continuously cast using a continuous casting machine. The continuous casting machine used was a vertical bending type continuous casting machine with a mold size of 250 mm thick x 1200 mm wide, and the casting speed was 1.2 m / min. The surface temperature of the cast slab was set to 850°C at the straightening point in all cases. The average cooling rate was adjusted by the amount of secondary cooling water, and experiments were performed with two patterns: rapid cooling at 120°C / min and slow cooling at 60°C / min.
[0045] From each of the cast pieces produced under the above conditions, a representative sample of about 10 m was cut out, and the cast pieces were evaluated for cracking. First, the front and back surfaces of the cast pieces were ground with a 0.7 mm grinder, and the presence or absence of cracks was visually confirmed. In addition, for cast pieces for which no cracks were found to have occurred as a result of visual inspection, they were subjected to the next hot rolling process without any maintenance (no crack checking with a grinder), and the presence or absence of cracks thereafter was also confirmed. Specifically, the cast pieces were heated to 1250°C, then rough rolled, and finish rolled at a finish rolling temperature of 930°C to a plate thickness of 3 mm, and cooled at an average cooling rate of 600°C / min to obtain hot-rolled sheets. The presence or absence of cracks was then confirmed by visual inspection or by inspection for defects using a camera on the surface of the hot-rolled sheet. If there were no cracks in the cast piece and no cracks occurred after hot rolling, it was evaluated as "◎", and if there were no cracks in the cast piece but cracks occurred after hot rolling, it was evaluated as "△". If cracks were found in the slab, it was rated as “×.” The experimental results are shown in Table 2.
[0046] For each slab, a surface 5 mm deep from the surface was taken out and mirror-polished, and an area of 10 mm x 10 mm was observed with an SEM to calculate the total number ratio of ZrN, HfN, YN or composite nitrides of these in all nitrides by the method described above. Furthermore, for some slabs, a high-temperature tensile test was performed at a tensile temperature of 900°C to determine the cross-sectional shrinkage (%). The specific method of the high-temperature tensile test was the same as that described above. The test results are also shown in Table 2.
[0047] [Table 1]
[0048] [Table 2]
[0049] The underlined parts in Table 2 are examples that did not satisfy the conditions of the present invention. As shown in Table 2, when the conditions of formulas (1) and (2) were satisfied, no cracks were present in the slab, and no cracks occurred after hot rolling, regardless of the Al and N contents.
[0050] On the other hand, in Comparative Examples No. 10 and 11, which satisfied only formula (1) but not formula (2), the number density was 50.0% or more and no cracks were present in the slab, but the thermal stability of the nitrides was insufficient, causing cracks in the hot-rolled sheet after hot rolling. Also, in Comparative Examples No. 12 to 17, which did not satisfy formula (1), the number density was less than 50.0%, and the generation of AlN could not be suppressed, causing cracks in the slab. [Explanation of symbols]
[0051] 10 straight line 11 Plot
Claims
1. In mass percent, C: 0.02% to 0.50%, Si: 0.20% to 3.00%, Mn: 0.50% to 4.00%, Al: 0.20% to 2.00% N: 0.01% or less, Zr: 0% to 0.05%, Hf: 0% to 0.05%, Y: 0% to 0.05%, Ti: 0% to 0.002%, Nb: 0% to 0.1%, V: 0% to 0.1%, B: 0% to 0.005%, Cr: 0% to 0.1%, Ni: 0% to 0.5%, and Cu: 0% to 0.5%; The remainder of the cast piece is made of Fe and impurities, The contents of Zr, Hf, and Y satisfy the following formulae (1) and (2), A cast slab, characterized in that the total number ratio of ZrN, HfN, YN or composite nitrides thereof to all nitrides at a position 5 mm deep from the surface of the cast slab is 50% or more. [Zr]+91 / 178×[Hf]+91 / 89×[Y]≧4 / 3×[Al]×[N] ...(1) [Hf]+[Y]≧0.001%...(2) Here, [Zr], [Hf], [Y], [Al], and [N] each represent the content (mass%) in the cast slab.
2. The method for continuous casting of a cast piece according to claim 1, The method for continuous casting of a slab is characterized in that, when bending and straightening the slab, bending and straightening are performed at a surface temperature in the range of 800°C to 1000°C.
3. 3. The method for continuous casting of a slab according to claim 2, wherein an average cooling rate in the surface layer of the slab is set to 60° C. / min or less.
Citation Information