Rubber composition for tire and tire
The rubber composition for tires, incorporating rosin-modified phenolic resin and carbon black, addresses the trade-offs in existing tire technologies by enhancing dry grip, stability, and wear resistance while maintaining hardness.
Patent Information
- Application Number
- JP2023050321
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
Smart Images

Figure 2024139404000001 
Figure 2024139404000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition for tires and a tire using the same, and more particularly to a rubber composition for tires having improved dry grip performance and excellent steering stability and abrasion resistance, and a tire using the same. [Background technology]
[0002] Generally, tires are required to have a wide range of performance characteristics, among which grip performance, driving stability, and wear resistance must be maintained at a high level. This requirement also exists for racing tires intended for circuit driving. In the prior art, a technique of compounding a large amount of a filler with a high specific surface area or a resin with a high softening point (high softening point resin) is known, but compounding a large amount of a filler with a high specific surface area causes a problem of deterioration in abrasion resistance due to a decrease in breaking strength, and compounding a large amount of a resin with a high softening point causes a problem of deterioration in steering stability due to a decrease in hardness.
[0003] In addition, the following Patent Document 1 describes a rubber composition having a nitrogen adsorption specific surface area (N2SA) of 100 to 500 m for 100 parts by mass of diene rubber including styrene-butadiene copolymer rubber. 2 This paper discloses a rubber composition for tires, which is characterized by blending 50 to 200 parts by mass of carbon black having an acid value of 30 mgKOH / g or more and a hydroxyl value of 5 mgKOH / g or more and 5 to 50 parts by mass of a terpene phenol resin having an acid value of 30 mgKOH / g or more and a hydroxyl value of 5 mgKOH / g or more. However, it does not disclose or suggest a rosin-modified phenol resin having an acid value of less than 30 mgKOH / g, which will be described below. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6791277 Summary of the Invention [Problem to be solved by the invention]
[0005] Accordingly, an object of the present invention is to provide a rubber composition for tires having improved dry grip performance, excellent steering stability and abrasion resistance, and a tire using the same. [Means for solving the problem]
[0006] As a result of extensive research, the inventors have discovered that the above-mentioned problems can be solved by blending a specific amount of a rosin-modified phenolic resin having an acid value within a specific range with a diene rubber, and have thus completed the present invention.
[0007] That is, the present invention provides a rubber composition for tires, characterized by blending 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g with 100 parts by mass of diene rubber. Effect of the Invention
[0008] The rubber composition for tires of the present invention is characterized by comprising 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g per 100 parts by mass of diene rubber, and therefore can provide a rubber composition for tires having improved dry grip performance, excellent steering stability and abrasion resistance, and a tire using the same.
[0009] The rosin-modified phenolic resin used in the present invention has excellent compatibility with diene rubber, and because of its low acid value, it is possible for alkaline components in the rubber composition (e.g., vulcanization accelerators) to fully exhibit their functions, and it is believed to improve dry grip performance, handling stability, and abrasion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will now be described in further detail.
[0011] (Diene rubber) The diene rubber used in the present invention may be any diene rubber that can be blended into a normal rubber composition, such as natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR), etc. These may be used alone or in combination of two or more. There are no particular limitations on the molecular weight or microstructure, and the diene rubber may be terminally modified with amine, amide, silyl, alkoxysilyl, carboxyl, hydroxyl, etc., or may be epoxidized. Among these diene rubbers, SBR is preferred in terms of the effects of the present invention. For example, in the case of racing applications, the blending amount of SBR is preferably 80 parts by mass or more, more preferably 100 parts by mass.
[0012] Furthermore, when the SBR has a styrene content of less than 35% by mass, the effects of the present invention, particularly dry grip performance, can be further enhanced.The styrene content is more preferably 30 to 10% by mass.
[0013] (rosin modified phenolic resin) The rosin modified phenolic resin used in the present invention can be a reaction product of a rosin-based resin, a phenol, formaldehyde and a polyol. Examples of rosin-based resins include unmodified rosins such as gum rosin, tall oil rosin, and wood rosin; polymerized rosins derived from unmodified rosin; disproportionated products or hydrogenated products of unmodified rosin or polymerized rosin; and unsaturated carboxylic acid-modified rosins obtained by reacting unmodified rosin or polymerized rosin with an unsaturated carboxylic acid. Examples of the phenols include phenol; alkylphenols such as methylphenol (cresol), butylphenol, pentylcresol, octylphenol, nonylphenol, decylphenol, dodecylphenol, tetradecylphenol, and hexyldecylphenol; and the like. Examples of formaldehyde include formalin and paraformaldehyde. Examples of polyols include diols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 3-methyl-1,5-pentanediol; triols such as glycerin, trimethylolpropane, and trimethylolethane; and tetraols such as pentaerythritol, diglycerin, ditrimethylolpropane, and ditrimethylolethane.
[0014] The amounts of the rosin resin, formaldehyde, phenols, and polyol used are not particularly limited, and may be appropriately determined in consideration of, for example, the desired molecular weight, softening point, etc. In addition, the reaction method may be, for example, a method in which the rosin resin, phenols / formaldehyde (condensate), and polyol are charged all at once and reacted, and the reaction temperature is usually about 100 to 300° C., and the reaction time is usually about 1 to 24 hours.
[0015] The rosin-modified phenolic resin used in the present invention must have an acid value adjusted to less than 30 mgKOH / g. The method of adjusting the acid value to less than 30 mgKOH / g is not particularly limited, but a suitable embodiment is, for example, a method of esterifying the rosin-modified phenolic resin prepared as described above or a commercially available rosin-modified phenolic resin (usually having an acid value of 30 mgKOH / g or more) to reduce the acid value to less than 30 mgKOH / g. The esterification may be carried out by a conventional method, using a polyhydric alcohol as the alcohol, and can be carried out at a reaction temperature of 150 to 300°C. Since the use of a dihydric alcohol such as ethylene glycol results in a resin with a low softening point, it is preferable to use a trihydric or higher alcohol. The acid value can be adjusted by the amount of alcohol charged. The rosin-modified phenolic resin prepared by the above suitable embodiment contains an ester bond inside, which increases the compatibility with diene rubber, and further enhances the effect of the rosin-modified phenolic resin. The acid value of the rosin-modified phenolic resin used in the present invention is preferably from 5 to 25 mgKOH / g, and more preferably from 10 to 20 mgKOH / g.
[0016] The rosin-modified phenolic resin used in the present invention preferably has a weight-average molecular weight of 2000 to 5000, more preferably 2500 to 4500, from the viewpoint of further enhancing the effects of the present invention. The softening point is preferably 100 to 160°C, more preferably 110 to 150°C. The weight-average molecular weight in the present invention means a weight-average molecular weight in terms of polystyrene analyzed by gel permeation chromatography (GPC). The softening point is measured in accordance with JIS K6220-1.
[0017] (Mixing ratio) The rubber composition of the present invention is characterized in that it is obtained by compounding 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g with 100 parts by mass of diene rubber. If the amount of the rosin-modified phenolic resin is less than 1 part by mass, the amount is too small to achieve the effects of the present invention, whereas if it exceeds 100 parts by mass, the hardness and breaking strength are reduced, and the handling stability and abrasion resistance cannot be improved. The amount of the rosin-modified phenolic resin to be mixed is preferably from 5 to 85 parts by mass, and more preferably from 10 to 70 parts by mass, based on 100 parts by mass of the diene rubber.
[0018] From the viewpoint of further improving the effects of the present invention, the rubber composition for a tire of the present invention has a nitrogen adsorption specific surface area (N 2 SA) is 100~500m 2 It is preferable to compound carbon black having a carbon black content of 0.1 wt. / g. The nitrogen adsorption specific surface area (N 2 SA) is 125~450m 2 It is even more preferred that the weight ratio is / g. The amount of carbon black to be blended is preferably 50 to 200 parts by mass, more preferably 80 to 170 parts by mass, based on 100 parts by mass of the diene rubber (A). 2 SA) is a value determined in accordance with JIS K6217-2.
[0019] (Liquid aromatic vinyl-conjugated diene rubber) The rubber composition for tires of the present invention is preferably blended with a liquid aromatic vinyl-conjugated diene rubber having a glass transition temperature (Tg) of -40°C or higher. By blending such a liquid aromatic vinyl-conjugated diene rubber, the glass transition temperature (Tg) of the rubber composition is increased, and the dry grip performance can be improved. In addition, the liquid aromatic vinyl-conjugated diene rubber is compatible with the diene rubber and enhances the dispersibility of the rosin-modified phenolic resin used in the present invention, thereby enhancing the effects of the present invention. As the liquid aromatic vinyl-conjugated diene rubber, liquid styrene-butadiene copolymer (liquid SBR) is preferred. The liquid SBR has a weight average molecular weight of 2000 to 40000, preferably 3000 to 20000. The glass transition temperature of the liquid SBR is -40°C or higher, more preferably -20°C to -5°C, as described above. As the liquid SBR, commercially available liquids can be used, such as RICON 100 manufactured by Cray Valley and L-SBR 820 manufactured by Kuraray Co., Ltd. The Tg referred to in the present invention is the midpoint temperature of the transition region measured by differential scanning calorimetry (DSC) at a temperature rise rate of 20°C / min. The liquid aromatic vinyl-conjugated diene rubber used in the present invention is liquid at 23° C. Therefore, it is distinguished from the diene rubber which is solid at this temperature. The amount of the liquid aromatic vinyl-conjugated diene rubber compounded is preferably 5 to 50 parts by mass, and more preferably 10 to 45 parts by mass, based on 100 parts by mass of the diene rubber.
[0020] (Other ingredients) In addition to the above-mentioned components, the rubber composition of the present invention may contain various additives that are generally incorporated in rubber compositions, such as vulcanizing or crosslinking agents, vulcanizing or crosslinking accelerators, zinc oxide, various fillers such as clay, talc, and calcium carbonate, antioxidants, and plasticizers, and these additives can be kneaded by a general method to form a composition, which can be used for vulcanization or crosslinking. The amounts of these additives may be conventional amounts, as long as they do not go against the object of the present invention.
[0021] In addition, other resins besides the rosin-modified phenolic resin can be blended as necessary. For example, phenolic resins (e.g., phenolic resin, phenol-acetylene resin, phenol-formaldehyde resin), coumarone resins (e.g., coumarone resin, coumarone-indene resin, coumarone-indene-styrene resin), terpene resins (e.g., terpene resin, modified terpene resin (aromatic modified terpene resin, etc.), terpene phenolic resin), styrene resin, acrylic resin, petroleum resin (e.g., C5-based petroleum resin such as dicyclopentadiene resin, C9-based petroleum resin, alicyclic petroleum resin, C5 / C9 copolymerized petroleum resin), xylene resins (e.g., xylene resin, xylene-acetylene resin, xylene-formaldehyde resin), α-pinene resin, aliphatic saturated hydrocarbon resin, etc. can be mentioned. The blending amount of these other resins is, for example, 10 to 150 parts by mass relative to 100 parts by mass of diene rubber.
[0022] The rubber composition of the present invention has improved dry grip performance and excellent steering stability and abrasion resistance, and therefore can be suitably used for tire treads, particularly cap treads, preferably racing tire treads, particularly cap treads. The tire of the present invention is preferably a pneumatic tire, and can be filled with air, an inert gas such as nitrogen, and other gases. EXAMPLES
[0023] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0024] Standard Examples 1-2, Examples 1-10 and Comparative Examples 1-7 Sample preparation In the formulation (parts by mass) shown in Table 1 or 2, the components other than the vulcanization accelerator and sulfur were kneaded in a 1.7-liter closed Banbury mixer for 5 minutes, and the rubber was discharged outside the mixer and cooled at room temperature. The rubber was then placed back into the mixer, and the vulcanization accelerator and sulfur were added and further kneaded to obtain a rubber composition. The obtained rubber composition was then press-vulcanized in a specified mold at 160°C for 20 minutes to obtain a vulcanized rubber test piece, and the physical properties of the vulcanized rubber test piece were measured by the test methods shown below.
[0025] Dry grip performance: Based on JIS K6394, tan δ (100°C) was measured using a viscoelasticity spectrometer manufactured by Toyo Seiki Seisakusho Co., Ltd. under the conditions of initial strain = 10%, amplitude = ±2%, and frequency = 20Hz, and the dry grip performance was evaluated based on this value. The results were expressed as an index, with the value of standard example 1 or 2 being 100. The higher the index, the better the dry grip performance. Hardness (100° C.): Measured at 100° C. in accordance with JIS K6253. The results are expressed as an index, with the value of Standard Example 1 or 2 being 100. A larger index indicates higher hardness and more excellent handling stability. Breaking strength: According to JIS K6251, a No. 3 dumbbell-shaped sample piece was punched out from the vulcanized rubber test piece, and a tensile test was carried out at a tensile speed of 500 mm / min to measure the breaking elongation (%). The results were expressed as an index, with the value of standard example 1 or 2 being 100. A higher index indicates better breaking strength and better abrasion resistance. The results are shown in Tables 1 and 2. Reference Example 1 is compared with Examples 1 to 6 and Comparative Examples 1 to 3, and Reference Example 2 is compared with Examples 7 to 10 and Comparative Examples 4 to 7.
[0026] [Table 1]
[0027] [Table 2] *1: SBR1 (ZEON Nipol 1739 (styrene content = 40% by mass)) *2: SBR2 (ZEON Nipol 1723 (styrene content = 23.5% by mass)) *3: Carbon black 1 (Cabot Japan Co., Ltd. Show Black N339, N 2 SA=94m 2 / g) *4: Carbon black 2 (Tokai Carbon Co., Ltd., Seast 9, N 2 SA=142m 2 / g) *5: Resin 1 (Yasuhara Chemical Co., Ltd. YS Polystar S145, phenol-modified terpene resin, acid value = 0 mg KOH / g) *6: Resin 2 (Tamanol 803L, rosin phenolic resin, acid value = 52 mg KOH / g, manufactured by Arakawa Chemical Industries, Ltd.) *7: Resin 3 (Marquid No. 5, maleic acid modified rosin resin, acid value = 19 mg KOH / g, manufactured by Arakawa Chemical Industries, Ltd.) *8: Resin 4 (Arakawa Chemical Industries, Ltd., Pencel KK, rosin ester resin, acid value = 19 mg KOH / g) *9: Resin 5 (rosin modified phenolic resin: reaction product of rosin, phenols, formaldehyde and polyol. Acid value = 15 mg KOH / g) *10: Resin 6 (rosin modified phenolic resin: reaction product of rosin, phenols, formaldehyde and polyol. Acid value = 17 mg KOH / g) *11: Resin 7 (ENEOS Neopolymer 140) *12: Liquid SBR (RICON 100 manufactured by Cray Valley, weight average molecular weight = 6400, Tg = -15℃) *13: Oil (Extract No. 4 S manufactured by Showa Shell Sekiyu K.K.) *14: Stearic acid (Beads Stearic Acid YR manufactured by NOF Corporation) *15: Zinc oxide (3 types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd.) *16: Anti-aging agent (Flexis 6PPD) *17: Vulcanization accelerator (Noccela CZ-G manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) *18: Sulfur (Kinka-in oil-filled fine sulfur manufactured by Tsurumi Chemical Industry Co., Ltd.)
[0028] The results in Tables 1 and 2 show that the rubber compositions of the examples contain 1 to 100 parts by mass of rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g per 100 parts by mass of diene rubber, and therefore have improved dry grip performance, handling stability and abrasion resistance compared to standard examples 1 and 2. In contrast, in Comparative Example 1, the acid value of the rosin-modified phenolic resin exceeded the upper limit specified in the present invention, and therefore the dry grip performance and hardness were deteriorated. Comparative Example 2 was an example in which a maleic acid modified rosin resin was used, and therefore the dry grip performance was deteriorated. Comparative Example 3 was an example in which a rosin ester resin was used, and therefore the dry grip performance was deteriorated. In Comparative Example 4, the acid value of the rosin-modified phenolic resin exceeded the upper limit specified in the present invention, and therefore the dry grip performance and hardness were deteriorated. Comparative Example 5 was an example in which a maleic acid modified rosin resin was used, and therefore the dry grip performance was deteriorated. Comparative Example 6 was an example in which a rosin ester resin was used, and therefore the dry grip performance was deteriorated. In Comparative Example 7, the amount of the rosin-modified phenolic resin blended exceeded the upper limit specified in the present invention, and so the hardness and breaking strength were deteriorated.
[0029] The present disclosure includes the following inventions. Invention [1]: A rubber composition for tires, characterized by comprising 100 parts by mass of diene rubber and 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g. Invention [2]: For 100 parts by mass of the diene rubber, a nitrogen adsorption specific surface area (N 2 SA) is 100~500m 2 2. The rubber composition according to claim 1, further comprising 50 to 200 parts by mass of carbon black having a molecular weight of 1 / g. Invention [3]: The rubber composition according to Invention 1 or 2, characterized in that the diene rubber contains a styrene-butadiene copolymer rubber having a styrene content of less than 35 mass%. Invention [4]: A rubber composition according to any one of Inventions 1 to 3, further comprising a liquid aromatic vinyl-conjugated diene rubber having a glass transition temperature (Tg) of -40°C or higher per 100 parts by mass of the diene rubber. Invention [5]: A tire using the rubber composition for tires according to any one of Inventions 1 to 4 in a cap tread.
Claims
1. A rubber composition for tires, comprising 100 parts by mass of diene rubber and 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g.
2. Further, a nitrogen adsorption specific surface area (N 2 SA) is 100 to 500m 2 2. The rubber composition for tires according to claim 1, characterized in that 50 to 200 parts by mass of carbon black having a molecular weight of 1 / g is blended.
3. 2. The rubber composition for tires according to claim 1, wherein the diene rubber contains a styrene-butadiene copolymer rubber having a styrene content of less than 35% by mass.
4. 2. The rubber composition for tires according to claim 1, further comprising a liquid aromatic vinyl-conjugated diene rubber having a glass transition temperature (Tg) of −40° C. or higher, based on 100 parts by mass of the diene rubber.
5. A tire using the rubber composition for tires according to claim 1 in a cap tread.
Citation Information
Patent Citations
Flame-retardant chlorinated polyethylene waterproof roll and preparation method thereof
CN110539540A
Light-colored low-molecular-weight phenol-modified rosin ester
JP2002526592A
Rubber composition for tire
JP2009051975A
Adhesive tape
JP2017200978A
Rubber composition for tires and pneumatic tire using same
JP6791277B2