Adhesive agent and adhesive tape

A pressure-sensitive adhesive tape with a resin component containing a specific phosphorus compound structure and (meth)acrylic monomers addresses the trade-off between flame retardancy and adhesiveness, enhancing both properties without additional flame retardants, making it suitable for construction use.

JP2024139420APending Publication Date: 2024-10-09MITSUBISHI CHEM CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023050353
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

Smart Images

  • Figure 2024139420000001
    Figure 2024139420000001
  • Figure 2024139420000002
    Figure 2024139420000002
  • Figure 2024139420000003
    Figure 2024139420000003
Patent Text Reader

Abstract

To provide an adhesive agent and an adhesive tape that offer high flame retardancy and adhesive performance without the incorporation of a flame retardant into an adhesive layer.SOLUTION: An adhesive agent includes a resin component (A), the resin component (A) including a constitutional unit derived from a monomer represented by the formula (a1). (n and m each represent 0 or 1, and R1 and R2 each represent a C1-18 alkyl group, phenyl group, or substituted phenyl group, which may be the same or different).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive and an adhesive tape, and more particularly to an adhesive and an adhesive tape having excellent adhesion and flame retardancy.

[0002] Methods for imparting flame retardancy to adhesive tapes include incorporating a flame retardant into the base material of the adhesive tape, and incorporating a flame retardant into the adhesive layer. However, in order to maintain the strength of the base material, the method of adding a flame retardant to the adhesive layer rather than incorporating the flame retardant into the base material is used. However, when a flame retardant is contained in the adhesive layer, in order to provide the adhesive tape with sufficient flame retardancy, it is necessary to increase the ratio of the flame retardant to the adhesive in the adhesive layer. Increasing the ratio of the flame retardant tends to reduce the adhesive properties of the adhesive layer, and therefore a flame retardant tape containing a flame retardant that can impart high flame retardancy even with a small amount of flame retardant has been desired. Generally, halogen-based flame retardants are highly flame-retardant, but they have the problem of generating halogen gas during combustion. In recent years, phosphorus-based flame retardants have mainly been used, but adhesive tapes containing phosphorus-based flame retardants do not have sufficient flame retardancy. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-114374 A [Patent Document 2] JP 2017-179329 A Summary of the Invention [Problem to be solved by the invention]

[0004] The adhesive tape of Patent Document 1 mentioned above contains 10 to 20 parts by mass of flame retardant per 100 parts by mass of the resin component of the adhesive layer, and the amount of flame retardant in the adhesive layer is relatively small. However, the examples of the adhesive tape also contain a flame retardant in the substrate, and it is shown that if the substrate does not contain a flame retardant, the flame retardancy is insufficient. The above-mentioned Patent Document 2 discloses an adhesive composition containing a small amount of a phosphate-based flame retardant in the adhesive layer, but the flame retardancy is not sufficient, and higher flame retardancy is required. Conversely, if the amount of the flame retardant is increased in order to improve the flame retardancy, the adhesiveness decreases.

[0005] Under such circumstances, an object of the present invention is to provide an adhesive and an adhesive tape that have high flame retardancy and adhesiveness without containing a flame retardant in the adhesive layer. [Means for solving the problem]

[0006] However, in light of these circumstances, the present inventor conducted extensive research and discovered that by including a resin component having a specific phosphorus compound structure in an adhesive, the adhesive can have high flame retardancy and adhesion without the addition of a flame retardant, and that an adhesive tape having this adhesive in its adhesive layer can have high flame retardancy and adhesion, thereby completing the present invention.

[0007] That is, the present invention has the following aspects. [1] A pressure-sensitive adhesive comprising a resin component (A), A pressure-sensitive adhesive, wherein the resin component (A) contains a structural unit derived from a monomer represented by the following formula (a1): [ka] (n and m are each 0 or 1, and R 1 , R 2 each represents an alkyl group having 1 to 18 carbon atoms, a phenyl group, or a phenyl group having a substituent, and may be the same or different.) [2] The pressure-sensitive adhesive according to [1], wherein the resin component (A) contains a structural unit derived from a (meth)acrylic monomer (a2) having a carboxy group and / or a (meth)acrylic monomer (a3) ​​having a hydroxyl group. [3] The pressure-sensitive adhesive according to [1] or [2], further comprising a crosslinking agent (B). [4] An adhesive tape having an adhesive layer formed from the adhesive according to any one of [1] to [3] on at least one surface of a substrate. [5] The adhesive tape according to [4], wherein the substrate comprises a flat yarn cloth. Effect of the Invention

[0008] The pressure-sensitive adhesive of the present invention is a pressure-sensitive adhesive containing a resin component, and the resin component has a structural unit derived from a specific phosphorus compound monomer, so that the pressure-sensitive adhesive has high flame retardancy and adhesion, and the obtained pressure-sensitive adhesive tape also has high flame retardancy and adhesion. Therefore, it can be suitably used as a pressure-sensitive adhesive for construction pressure-sensitive adhesive tapes that require particularly high flame retardancy and adhesion.

[0009] Furthermore, in the present invention, the adhesive further contains a resin component containing a structural unit derived from a (meth)acrylic monomer (a2) having a carboxy group and / or a (meth)acrylic monomer (a3) ​​having a hydroxyl group, thereby making it possible to obtain an adhesive with even better adhesive properties.

[0010] Furthermore, in the present invention, the pressure-sensitive adhesive further contains a crosslinking agent (B), whereby the pressure-sensitive adhesive can have even more excellent adhesive properties.

[0011] The adhesive tape of the present invention, which has an adhesive layer containing the above-mentioned adhesive on at least one surface of a substrate, can be an adhesive tape having high flame retardancy and excellent adhesiveness.

[0012] In the present invention, in particular, when the substrate contains a flat yarn cloth, the substrate can have excellent flame retardancy and ease of being cut by hand. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described below based on examples of the mode for carrying out the present invention. However, the present invention is not limited to the embodiment described below. In the present invention, "(meth)acrylic" means acrylic or methacrylic, "(meth)acryloyl" means acryloyl or methacryloyl, and "(meth)acrylate" means acrylate or methacrylate. Also, "acrylic resin" means a resin obtained by polymerizing a copolymerization component containing at least one (meth)acrylate monomer. In the present invention, the term "tape" includes the meanings of "film" and "sheet". In the present invention, the "main component" refers to the component that is most abundant in the target substance, and is usually 50 mass% or more of the target substance, preferably 60 mass% or more, more preferably 70 mass% or more, particularly preferably 80 mass% or more, especially preferably 90 mass% or more, and most preferably 100 mass%.

[0014] In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the intention that "greater than X is preferable" or "less than Y is preferable." In addition, "X and / or Y (X and Y are optional configurations)" means at least one of X and Y, and means the following three cases: X only, Y only, and X and Y.

[0015] <<Adhesive>> An adhesive according to one embodiment of the present invention (hereinafter sometimes referred to as "the adhesive") is an adhesive containing a resin component, and the resin component has a structural unit derived from a specific phosphorus compound monomer. Each of the constituent components used in the present pressure-sensitive adhesive will be described in detail below.

[0016] <Resin component> The resin component (A) used in the present pressure-sensitive adhesive is used as the main component of the present pressure-sensitive adhesive. The resin component is not particularly limited as long as it is a known resin component used in pressure-sensitive adhesives, but examples thereof include acrylic resins, epoxy resins, phenolic resins, polyester resins, etc., which can be used alone or in combination of two or more kinds. Among them, acrylic resins are preferably used. When an acrylic resin is used as the resin component, it is preferable to use the acrylic resin as the main component of the resin component.

[0017] The acrylic resin used in the present adhesive refers to a resin obtained by polymerizing a copolymerization component containing at least one (meth)acrylate monomer in addition to the specific phosphorus compound monomer, and for example, a homopolymer of alkyl (meth)acrylate and a copolymer obtained by polymerizing a monomer copolymerizable therewith can be mentioned. Each monomer that can constitute the acrylic resin will be described below.

[0018] In the present invention, the resin component (A) has a structural unit derived from a monomer represented by the following formula (a1): (a1) is a specific phosphorus compound monomer. [ka] (n and m are each 0 or 1, and R 1 , R 2 each represents an alkyl group having 1 to 18 carbon atoms, a phenyl group, or a phenyl group having a substituent, and may be the same or different.)

[0019] Above R 1 , R2 In the case of an alkyl group, R is usually an alkyl group having 1 to 18 carbon atoms, preferably 1 to 10 carbon atoms, such as a methylene group, and is preferably a methyl group or an ethyl group. 1 , R 2 may be a phenyl group or a phenyl group having a substituent, and among these, a phenyl group is preferred since it has higher flame retardancy.

[0020] Specifically, when the specific phosphorus compound monomer is a compound of the following formula (a1-1), a pressure-sensitive adhesive having higher flame retardancy can be obtained. [ka] (n and m are either 0 or 1.)

[0021] Specific examples of the monomer (a1) include dimethylvinylphosphonate, diethylvinylphosphonate, diphenylvinylphosphonate, dimethylvinylphosphine oxide, diethylvinylphosphine oxide, and diphenylvinylphosphine oxide.

[0022] The content of the structural unit derived from the monomer (a1) is usually 0.1 to 20 mass%, particularly 0.5 to 15 mass%, and further preferably 0.8 to 12 mass% of the entire resin component (A). If the content is too low, the flame retardancy decreases, and if it is too high, the molecular weight of the resin component (A) does not increase sufficiently during polymerization, and the adhesiveness tends to decrease.

[0023] When the resin component (A) is an acrylic resin, it has a structural unit derived from at least one (meth)acrylate monomer. Each monomer unit capable of constituting the acrylic resin will be described below.

[0024] [Carboxy group-containing (meth)acrylic monomer (a2) unit] The resin component (A) preferably has a structural unit derived from a carboxyl group-containing (meth)acrylic monomer (a2). Examples of copolymerizable monomers for forming the carboxyl group-containing monomer (a2) unit include (meth)acrylic acid, 2-(meth)acryloyloxyethylhexahydrophthalic acid, 2-(meth)acryloyloxypropylhexahydrophthalic acid, 2-(meth)acryloyloxyethylphthalic acid, 2-(meth)acryloyloxypropylphthalic acid, 2-(meth)acryloyloxyethylmaleic acid, 2-(meth)acryloyloxypropylmaleic acid, 2-(meth)acryloyloxyethylsuccinic acid, and 2-(meth)acryloyloxypropylsuccinic acid. Among these, (meth)acrylic acid is preferred.

[0025] The content of the structural unit derived from the carboxyl group-containing (meth)acrylic monomer (a2) is preferably 0.1 to 20 mass % of the entire resin component (A), more preferably 0.5 to 10 mass %, and further preferably 1 to 5 mass %. If the content is too low or too high, the adhesiveness tends to decrease.

[0026] [Hydroxyl group-containing (meth)acrylic monomer (a3) ​​unit] The resin component (A) preferably has a structural unit derived from a (meth)acrylic monomer (a3) ​​having a hydroxyl group. Examples of copolymerizable monomers for forming such hydroxyl group-containing (meth)acrylic monomer (a3) ​​units include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate, caprolactone-modified monomers such as caprolactone-modified 2-hydroxyethyl (meth)acrylate, oxyalkylene-modified monomers such as diethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate, N-methyl-N ... Examples of the monomers include hydroxyl group-containing (meth)acrylamides such as thyrol (meth)acrylamide, N-hydroxyethyl (meth)acrylamide, and N-methylolpropane (meth)acrylamide, primary hydroxyl group-containing monomers such as 2-acryloyloxyethyl-2-hydroxyethyl phthalic acid, secondary hydroxyl group-containing monomers such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate, and tertiary hydroxyl group-containing monomers such as 2,2-dimethyl-2-hydroxyethyl (meth)acrylate. These monomers can also be referred to as "hydroxyl group-containing (meth)acrylic acid ester monomers".

[0027] Among these, primary hydroxyl group-containing monomers are preferred because of their excellent reactivity with the crosslinking agent (B), and (meth)acrylic acid hydroxyalkyl esters are more preferred, with 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate being particularly preferred.

[0028] The hydroxyl group-containing monomer (a3) ​​unit is useful because it forms a crosslinking point with the crosslinking agent (B) described below, particularly with the isocyanate-based crosslinking agent (B). The content of the structural unit derived from the hydroxyl group-containing monomer (a1) is usually 0.01 to 5 mass%, preferably 0.05 to 3 mass%, and more preferably 0.05 to 2 mass%, based on the total resin component (A). If the monomer (a3) ​​unit is too small, the flame retardancy tends to decrease, and if it is too large, the adhesive strength tends to decrease. The content of the structural unit derived from the hydroxyl group-containing monomer (a3) ​​can be adjusted by the blending ratio of the monomers when producing the resin component (A), and can be analyzed by NMR or the like.

[0029] [Alkyl (meth)acrylate monomer (a4) unit] The resin component (A) preferably also has a structural unit derived from an alkyl (meth)acrylate monomer (a4) having an alkyl group having 4 to 24 carbon atoms. The copolymerizable monomer for forming such alkyl(meth)acrylate monomer (a4) units may be any alkyl(meth)acrylate monomer having an alkyl group having 4 to 24 carbon atoms, and it is particularly preferable to contain both an alkyl(meth)acrylate monomer (a4-1) having an alkyl group having 4 to 7 carbon atoms, and an alkyl(meth)acrylate monomer (a4-2) having an alkyl group having 8 to 24 carbon atoms. Incidentally, an alkyl (meth)acrylate monomer having an alkyl group with 4 to 24 carbon atoms and also having a hydroxyl group is classified as a hydroxyl group-containing monomer (a3).

[0030] Examples of the alkyl (meth)acrylate monomer (a3-1) having an alkyl group having 4 to 7 carbon atoms include n-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-hexyl (meth)acrylate, etc. Among these, n-butyl (meth)acrylate is preferred from the viewpoints of easy availability and excellent economical efficiency.

[0031] Examples of the alkyl (meth)acrylate monomer (a3-2) having an alkyl group with 8 to 24 carbon atoms include 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, isotridecyl (meth)acrylate, myristyl (meth)acrylate, isomyristyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and behenyl (meth)acrylate. Among these, alkyl (meth)acrylates having an alkyl group with 8 to 12 carbon atoms are preferred, in terms of low polarity and low glass transition temperature, and 2-ethylhexyl (meth)acrylate is particularly preferred.

[0032] The content of the monomer (a4) units is usually 55 to 97% by mass, preferably 70 to 98% by mass, and more preferably 80 to 95% by mass, based on the total mass of the resin component (A). If the content of the monomer (a4) units is too small, the adhesive strength tends to decrease, whereas if the content of the monomer (a4) units is too large, the adhesive strength and holding power tend to decrease.

[0033] When the monomer (a4-1) and the monomer (a4-2) are used in combination, the ratio of the monomer (a4-1) unit to the monomer (a4-2) unit is preferably (a4-1) / (a4-2)=15 / 85-85 / 15 by mass, more preferably 25 / 75-75 / 25, even more preferably 30 / 70-70 / 30, particularly preferably 40 / 60-60 / 40, and especially preferably 45 / 55-55 / 45. If the ratio of the monomer (a4-1) unit is too small, the holding power tends to decrease, and if it is too large, the flame retardancy tends to decrease.

[0034] [Monomer (a5) unit] The resin component (A) may further have structural units derived from an alkyl (meth)acrylate monomer (a5-1) having an alkyl group having 1 to 3 carbon atoms, a cyclic structure-containing monomer (a5-2), and a vinyl ester monomer (a5-3) having 3 to 10 carbon atoms. The monomers (a5-1) to (a5-3) are collectively referred to as monomer (a5). Furthermore, monomers that fall under the category of monomer (a5) but also contain a hydroxyl group are classified as hydroxyl-containing monomers (a3).

[0035] Examples of copolymerizable monomers for forming the alkyl(meth)acrylate monomer (a5-1) unit having an alkyl group having 1 to 3 carbon atoms include methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, etc. Among these, methyl(meth)acrylate and ethyl(meth)acrylate are preferred.

[0036] The copolymerizable monomer for forming the cyclic structure-containing monomer (a5-2) unit is usually a (meth)acrylic monomer having a substituent containing a cyclic structure, and examples thereof include heterocyclic ring-containing (meth)acrylates having a heterocyclic ring such as a morpholine ring, a piperidine ring, a pyrrolidine ring, or a piperazine ring, such as N-(meth)acryloylmorpholine, N-vinylpyrrolidone, N-vinylcaprolactam, N-(meth)acryloylpiperidine, or N-(meth)acryloylpyrrolidine, and further include phenyl(meth)acrylate, phenoxyethyl(meth)acrylate, or the like. Also included are phenyl diethylene glycol (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, benzyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, dicyclopentanyl (meth)acrylate, nonylphenol polyethylene glycol (meth)acrylate, nonylphenoxy polyethylene glycol (meth)acrylate, isobornyl (meth)acrylate, and biphenyloxyethyl (meth)acrylate. Other examples of non-(meth)acrylic monomers include styrene and α-methylstyrene. Among these, heterocyclic ring-containing (meth)acrylates having a morpholine ring are preferred because of their good balance of various physical properties, and N-(meth)acryloylmorpholine is particularly preferred because of its ease of availability and safety.

[0037] Examples of copolymerizable monomers for forming the vinyl ester monomer (a5-3) units having 3 to 10 carbon atoms include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, etc. Among these, vinyl acetate is preferred because of its easy availability.

[0038] The content of the structural unit derived from the monomer (a5) is usually 11% by mass or less, preferably 10% by mass or less, more preferably 8% by mass or less, based on the total amount of the resin component (A). If the monomer (a5) unit is too much, the adhesive strength to the adherend tends to decrease. The lower limit of the content of the monomer (a5) unit is usually 0% by mass, but is preferably 1% by mass or more.

[0039] [Other monomer (a6) units] The resin component (A) may contain other monomer (a6) units as necessary. Examples of copolymerizable monomers for forming the other monomer (a6) units include functional group-containing monomers such as acetoacetyl group-containing monomers, isocyanate group-containing monomers, glycidyl group-containing monomers, amino group-containing monomers, and amide group-containing monomers, and other copolymerizable monomers.

[0040] Examples of the acetoacetyl group-containing monomer include 2-(acetoacetoxy)ethyl (meth)acrylate and allyl acetoacetate.

[0041] Examples of the isocyanate group-containing monomer include 2-acryloyloxyethyl isocyanate, 2-methacryloyloxyethyl isocyanate, and alkylene oxide adducts thereof.

[0042] Examples of the glycidyl group-containing monomer include glycidyl (meth)acrylate and allyl glycidyl (meth)acrylate.

[0043] Examples of the amino group-containing monomer include monomers having an ethylenically unsaturated double bond and an amino group (unsubstituted or substituted amino group). For example, mono-substituted amino group-containing (meth)acrylic acid esters such as aminoalkyl (meth)acrylates such as aminomethyl (meth)acrylate, aminoethyl (meth)acrylate, aminopropyl (meth)acrylate, and aminoisopropyl (meth)acrylate, and (meth)acrylic acid esters of N-alkylaminoalkyls such as N-(t-butyl)aminoethyl (meth)acrylate; di-substituted amino group-containing (meth)acrylic acid esters such as N,N-dialkylaminoalkyls such as N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylate. dialkylaminoalkyl(meth)acrylamides such as N,N-dimethylaminopropyl(meth)acrylamide, and quaternary salts of these amino group-containing monomers; amino group-containing styrenes such as p-aminostyrene; styrenes having a dialkylamino group such as 3-(dimethylamino)styrene and dimethylaminomethylstyrene; dialkylaminoalkyl vinyl ethers such as N,N-dimethylaminoethyl vinyl ether and N,N-diethylaminoethyl vinyl ether; allylamine, 4-diisopropylamino-1-butene, trans-2-butene-1,4-diamine, and 2-vinyl-4,6-diamino-1,3,5-triazine.

[0044] The amide group-containing monomer includes a monomer having an ethylenically unsaturated double bond and an amide group (a group having an amide bond). For example, (meth)acrylamide; N-alkyl (meth)acrylamides such as N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-propyl (meth)acrylamide, N-isopropyl (meth)acrylamide, Nn-butyl (meth)acrylamide, N-isobutyl (meth)acrylamide, Ns-butyl (meth)acrylamide, Nt-butyl (meth)acrylamide, N-hexyl (meth)acrylamide, diacetone (meth)acrylamide, N,N'-methylenebis (meth)acrylamide, and N-(1,1-dimethyl-3-oxobutyl) (meth)acrylamide; N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, N,N-di(n-butyl) (meth)acrylamide, N,N-diisobutyl (meth)acrylamide, and N,N-di(s-butyl) (meth)acrylamide; N,N-dialkyl(meth)acrylamides such as N,N-di(t-butyl)(meth)acrylamide, N,N-dipentyl(meth)acrylamide, N,N-dihexyl(meth)acrylamide, N,N-diheptyl(meth)acrylamide, N,N-dioctyl(meth)acrylamide, N,N-diallyl(meth)acrylamide, and N,N-ethylmethylacrylamide; dialkylaminoalkyl(meth)acrylamides such as N,N-dimethylaminopropyl(meth)acrylamide; substituted amide group-containing monomers such as N-vinylacetamide, N-vinylformamide, (meth)acrylamide ethyl ethylene urea, and (meth)acrylamide-t-butylsulfonic acid; alkoxy group-containing (meth)acrylamides such as N-methoxymethyl(meth)acrylamide and N-(n-butoxymethyl)(meth)acrylamide; and quaternized salts of these amide group-containing monomers.

[0045] Examples of the other copolymerizable monomers include monomers containing an alkoxy group or an oxyalkylene group, such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and polypropylene glycol mono(meth)acrylate; acrylonitrile, methacrylonitrile, vinyl stearate, vinyl chloride, vinylidene chloride, alkyl vinyl ether, vinyl toluene, dialkyl itaconic acid ester, dialkyl fumaric acid ester, allyl alcohol, acrylic chloride, methyl vinyl ketone, allyl trimethylammonium chloride, and dimethylallyl vinyl ketone.

[0046] The other monomer (a6) can be used to adjust the physical properties according to the application, so long as the effect of the present invention is not impaired. For example, the content of the structural unit derived from the other monomer (a6) is usually 10 mass% or less, and the lower limit is usually 0 mass%, based on the total resin component (A).

[0047] Resin component (A) is obtained by polymerizing a monomer mixture containing monomer (a1), and it is preferable to appropriately polymerize a monomer mixture containing one or more monomers selected from the above monomers (a2) to (a6) in addition to monomer (a1). This results in a resin component (A) having the above monomer (a1) to (a6) units as appropriate, and preferably a resin component (A) having a structural unit derived from monomer (a2), more preferably monomer (a3), even more preferably monomer (a4), particularly preferably monomer (a5), and if necessary, monomer (a6). In addition to monomer (a1), each of these monomers (a2) to (a6) may be used alone or in combination of two or more types.

[0048] As the polymerization, it is preferable to adopt solution polymerization, since it is possible to safely and stably produce the resin component (A) with any monomer composition.

[0049] Such solution polymerization can be carried out according to a conventional method. For example, the monomers (a1) to (a6) and a polymerization initiator are mixed or dropped into an organic solvent, and polymerization can be carried out under reflux or at 50 to 98° C. for 0.1 to 20 hours. The resin component (A) polymerized in an organic solvent is an organic solvent-based resin.

[0050] As the polymerization initiator, a conventional radical polymerization initiator can be used. Specific examples include azo-based polymerization initiators such as azobisisobutyronitrile and azobisdimethylvaleronitrile; and peroxide-based polymerization initiators such as benzoyl peroxide, lauroyl peroxide, di-t-butyl peroxide, and cumene hydroperoxide. These polymerization initiators may be used alone or in combination of two or more. The amount of the polymerization initiator used is usually 0.001 to 5 parts by mass based on 100 parts by mass of the copolymerization components.

[0051] [Solubility parameter (SP value)] The resin component (A) used in this adhesive, particularly the acrylic resin, has a solubility parameter (SP value) of 10 (cal / cm 3 ) 1 / 2 Less than or equal to 9.9 (cal / cm 3 ) 1 / 2 Less than or equal to 9.8 (cal / cm 3 ) 1 / 2 The present invention is characterized in that: SP value is 10(cal / cm 3 ) 1 / 2 If it exceeds this value, the flame retardancy and adhesive properties will decrease. The lower limit of the SP value is 7 (cal / cm 3 ) 1 / 2 and preferably 8 (cal / cm 3 ) 1 / 2 , more preferably 8.5 (cal / cm 3 ) 1 / 2 , and more preferably 9.0 (cal / cm 3 ) 1 / 2 , and particularly preferably 9.5 (cal / cm 3 )1 / 2 It is.

[0052] The SP value can be calculated from the evaporation energy (ΔE), molar volume (ΔV) and molar ratio of the resin component (A) used in the adhesive, particularly the (meth)acrylic acid alkyl ester monomer and copolymerizable monomer that constitute the acrylic resin, and specifically, can be calculated by the following formula (1).

[0053] [formula] SP value (cal / cm 3 ) 1 / 2 =(ΔE / ΔV) 1 / 2 (1)

[0054] ΔE=(x×ΔEx / Mx)+(y×ΔEy / My)+...(n×ΔEn / Mn)×(1 / C) ΔV=(x×ΔVx / Mx)+(y×ΔVy / My)+...(n×ΔVn / Mn)×(1 / C) C=(x / Mx)+(y / My)+...(n / Mn) x: Content of monomer X in the copolymerization component (% by mass) ΔEx: Evaporation energy of monomer X ΔVx: Molar volume of monomer X Mx: molecular weight of monomer X y: Content of monomer Y in the copolymerization component (% by mass) ΔEy: Evaporation energy of monomer Y ΔVy: Molar volume of monomer Y My: Molecular weight of monomer Y n: Content of monomer N in the copolymerization component (mass%) ΔEn: Evaporation energy of monomer N ΔVn: Molar volume of monomer N Mn: Molecular weight of monomer N C: Molar ratio of resin components

[0055] The resin component (A) used in this adhesive, especially the acrylic resin, has an SP value of 10 (cal / cm 3 ) 1 / 2The following method may be, for example, a method of adjusting the type and content of the monomers (a1) to (a6), particularly the type and content of the functional group-containing monomer.

[0056] [Average molecular weight] The weight average molecular weight of the resin component (A) used in the present pressure-sensitive adhesive, particularly the acrylic resin, is usually 100,000 to 5,000,000, preferably 300,000 to 1,500,000, and more preferably 400,000 to 900,000. If the weight average molecular weight is too small, the durability tends to decrease, and if it is too large, the adhesive strength tends to decrease.

[0057] The resin component (A) used in the pressure-sensitive adhesive, particularly the acrylic resin, preferably has a degree of dispersion (weight average molecular weight / number average molecular weight) of 20 or less, more preferably 15 or less, even more preferably 10 or less, and particularly preferably 7 or less. If the degree of dispersion is too high, the durability of the pressure-sensitive adhesive layer tends to decrease and foaming and the like tends to occur easily. From the viewpoint of production limitations, the degree of dispersion is preferably 1.1 or more, more preferably 3 or more, and even more preferably 4 or more.

[0058] The weight average molecular weight of the resin component (A) used in this adhesive, particularly the acrylic resin, is the weight average molecular weight calculated based on the standard polystyrene molecular weight. The weight average molecular weight was calculated based on the standard polystyrene molecular weight conversion, and the ... 7 , Separation range: 100~2×10 7 The number average molecular weight is measured by using three columns in series (10000 / column, theoretical plate number: 10,000 plates / column, filler material: styrene-divinylbenzene copolymer, filler particle size: 10 μm), and the number average molecular weight can also be measured by the same method.

[0059] [Glass transition temperature] The glass transition temperature (Tg) of the resin component (A) used in the present pressure-sensitive adhesive, particularly the acrylic resin, is usually −80 to 10° C., preferably −70 to −10° C., and more preferably −65 to −20° C. If the glass transition temperature is too high, the tackiness tends to be insufficient, and if it is too low, the heat resistance tends to decrease.

[0060] The above glass transition temperature (Tg) is a value calculated by applying the glass transition temperature and mass fraction of each of the monomers constituting the resin component (A) as a homopolymer to the following Fox's formula.

[0061]

number

[0062] Tg: Glass transition temperature (K) of resin component (A) (especially acrylic resin) Tga: Glass transition temperature of homopolymer of monomer A (K) Wa: Mass fraction of monomer A Tgb: Glass transition temperature of homopolymer of monomer B (K) Wb: Mass fraction of monomer B Tgn: Glass transition temperature of homopolymer of monomer N (K) Wn: mass fraction of monomer N (Wa+Wb+···+Wn=1)

[0063] Here, the glass transition temperature of the resin component (A) used in this adhesive, particularly the monomer constituting the acrylic resin, when made into a homopolymer, is usually a value measured by a differential scanning calorimeter (DSC) using a method in accordance with JIS K7121-1987 or JIS K6240, or a value listed in a catalog.

[0064] The resin component (A) used in the present pressure-sensitive adhesive, particularly the acrylic resin, is usually adjusted in viscosity with a solvent or the like and is applied as a resin solution. The viscosity of the resin solution is preferably 500 to 20,000 mPa·s / 25°C, more preferably 1,000 to 18,000 mPa·s / 25°C, and even more preferably 2,000 to 15,000 mPa·s / 25°C, from the viewpoint of ease of handling. If the viscosity is too high, the fluidity tends to decrease and handling tends to become difficult, and if the viscosity is too low, application of the pressure-sensitive adhesive solution tends to become difficult. The solution concentration in this case is usually 10 to 70% by mass.

[0065] The solvent that can be used for viscosity adjustment is not particularly limited as long as it dissolves the resin component (A) used in the present pressure-sensitive adhesive, especially the acrylic resin, and can be, for example, ester-based solvents such as methyl acetate, ethyl acetate, methyl acetoacetate, and ethyl acetoacetate; ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; aromatic solvents such as toluene and xylene; and alcohol-based solvents such as methanol, ethanol, and propyl alcohol. Among these, ethyl acetate and methyl ethyl ketone are preferred, and ethyl acetate is more preferably used, from the viewpoints of solubility, drying property, and price. Any of the above-mentioned solvents may be used alone, or two or more of them may be used in combination.

[0066] The viscosity of the resin component (A) used in the present pressure-sensitive adhesive, particularly the acrylic resin solution, is measured by a rotational viscometer method using a B-type viscometer with the resin solution adjusted to 25°C.

[0067] <Crosslinking agent (B)> The pressure-sensitive adhesive may contain a crosslinking agent (B) in addition to the above components. Examples of the crosslinking agent (B) include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, melamine-based crosslinking agents, aldehyde-based crosslinking agents, amine-based crosslinking agents, and metal chelate-based crosslinking agents. These may be used alone or in combination of two or more.

[0068] The isocyanate-based crosslinking agent contains at least two isocyanate groups, and examples thereof include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate; aliphatic polyisocyanates such as hexamethylene diisocyanate; alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate; and biuret and isocyanurate forms thereof, as well as adducts which are reactants with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. In particular, an adduct of tolylene diisocyanate and trimethylolpropane is preferred. These can be used alone, or two or more can be used in combination.

[0069] Examples of the epoxy crosslinking agent include aliphatic epoxy crosslinking agents such as ethylene glycol diglycidyl ether, trimethylolpropane diglycidyl ether, and diglycidylamine; alicyclic epoxy crosslinking agents such as 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, and N,N,N',N'-tetraglycidyl-m-xylylenediamine; aromatic epoxy crosslinking agents such as diglycidylaniline; heterocyclic epoxy crosslinking agents such as 1,3,5-tris-(2,3-epoxybutyl)-isocyanurate, 1,3,5-tris-(3,4-epoxybutyl)-isocyanurate, and 1,3,5-tris-(4,5-epoxypentyl)-isocyanurate, among which alicyclic epoxy crosslinking agents are preferred. These can be used alone or in combination of two or more.

[0070] Examples of the aziridine crosslinking agent include diphenylmethane-4,4'-bis(1-aziridinecarboxamide), trimethylolpropane tri-β-aziridinylpropionate, tetramethylolmethane tri-β-aziridinylpropionate, toluene-2,4-bis(1-aziridinecarboxamide), triethylenemelamine, bisisophthaloyl-1-(2-methylaziridine), tris-1-(2-methylaziridine)phosphine, and trimethylolpropane tri-β-(2-methylaziridine)propionate.

[0071] Examples of the melamine-based crosslinking agent include melamine; methylolmelamine derivatives such as amino group-containing methylolmelamine, imino group-containing methylolmelamine, and hexamethylolmelamine obtained by condensing melamine with formaldehyde; and alkylated methylolmelamines such as partially or completely alkylated methylolmelamine and imino group-containing partially or completely alkylated methylolmelamine obtained by reacting a methylolmelamine derivative with a lower alcohol such as methyl alcohol or butyl alcohol to partially or completely etherify the methylolmelamine derivative.

[0072] Examples of the aldehyde crosslinking agent include aldehyde compounds that liberate aldehyde in an aqueous solution, such as formaldehyde, acetaldehyde, propionaldehyde, butylaldehyde, glyoxal, glutaraldehyde, dialdehyde starch, hexamethylenetetramine, 1,4-dioxane-2,3-diol, 1,3-bis(hydroxymethyl)-2-imidazolidine, dimethylol urea, N-methylol acrylamide, urea formalin resin, and melamine formalin resin, and aromatic aldehyde compounds, such as benzaldehyde, 2-methylbenzaldehyde, 4-methylbenzaldehyde, p-hydroxybenzaldehyde, and m-hydroxybenzaldehyde.

[0073] Examples of the amine-based crosslinking agent include 4,4'-methylene-bis(2-chloroaniline) (hereinafter abbreviated as "MOCA"), modified MOCA, and diethyltoluenediamine.

[0074] Examples of the metal chelate crosslinking agent include chelate compounds in which the metal atom is aluminum, zirconium, titanium, zinc, iron, tin, etc., and from the viewpoint of performance, aluminum chelate compounds are preferred. Examples of aluminum chelate compounds include diisopropoxyaluminum monooleyl acetoacetate, monoisopropoxyaluminum bisoleyl acetoacetate, monoisopropoxyaluminum monooleate monoethyl acetoacetate, diisopropoxyaluminum monolauryl acetoacetate, diisopropoxyaluminum monostearyl acetoacetate, and diisopropoxyaluminum monoisostearyl acetoacetate.

[0075] The crosslinking agent (B) may be one or more selected from the above crosslinking agents. It is preferable that the crosslinking agent (B) contains at least an isocyanate-based crosslinking agent. A crosslinking agent containing only an isocyanate-based crosslinking agent or a crosslinking agent containing an isocyanate-based crosslinking agent and one or more other crosslinking agents may be used. The content of the isocyanate-based crosslinking agent in the crosslinking agent (B) is preferably 50% by mass or more, more preferably 80% by mass or more, still more preferably 90% by mass or more, and particularly preferably 95 to 100% by mass, based on 100% by mass of the crosslinking agent.

[0076] The above-mentioned crosslinking agent (B) reacts with functional groups in the resin component (A) used in this adhesive, particularly in the acrylic resin, to form a crosslinked structure. By using an isocyanate-based crosslinking agent as the crosslinking agent (B), the effect of improving flame retardancy when the resin component (A) contains a structural unit derived from a specific phosphorus compound monomer is further increased. The reason why the flame retardancy improvement effect is further increased is not clear, but it is thought that because a pressure-sensitive adhesive layer with high crosslinking density can be formed by reacting an isocyanate-based crosslinking agent with functional groups, particularly hydroxyl groups, in the resin component (A), particularly the acrylic resin, it is possible to improve flame retardancy by including a structural unit derived from a specific phosphorus compound monomer in the resin component (A).

[0077] The content of the crosslinking agent (B) is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, further preferably 0.3 to 3 parts by mass, and particularly preferably 0.4 to 3 parts by mass, based on 100 parts by mass of the resin component (A), particularly the acrylic resin. If the content is too low, the holding power tends to decrease, whereas if the content is too high, the adhesive power tends to decrease.

[0078] Incidentally, the crosslinking agent (B) is usually used after being diluted with a solvent or the like, and the above content indicates the substantial (solid content) content of the crosslinking agent (B) excluding the solvent or the like.

[0079] In addition, the crosslinking agent (B) contained in the present adhesive may have the same structure as the unreacted crosslinking agent when mixed with the resin component (A), particularly the acrylic resin, or may have a structure that has reacted with a functional group in the resin component (A), particularly the acrylic resin. Therefore, the content of the crosslinking agent (B) contained in the present adhesive refers to the content of the crosslinking agent in both the unreacted and reacted structures, and is equivalent to the content of the crosslinking agent (B) when mixed with the resin component (A), particularly the acrylic resin, during the preparation of the present adhesive.

[0080] <Tackifier> The present pressure-sensitive adhesive may further contain a tackifier, although this is not an essential component, in order to further exhibit the excellent physical properties of the resin component (A) used in the present pressure-sensitive adhesive, particularly the acrylic resin. As the tackifier, a resin that is compatible with the resin component (A) used in the present adhesive, particularly with the acrylic resin, is used, and examples thereof include rosin-based resins, terpene-based resins, xylene-based resins, phenol-based resins, coumarone-based resins, and petroleum-based resins. These tackifiers may be used alone or in combination of two or more. Among them, rosin-based resins, terpene-based resins, and petroleum-based resins are preferred, and will be specifically described below.

[0081] Examples of the rosin resin include rosin ester resins obtained by hydrogenating, disproportionating, dimerizing, or adding an acid to raw rosin, and then esterifying the raw rosin with glycerin or pentaerythritol, and rosin phenol resins obtained by adding phenol to raw rosin. Any of the rosin resins can be used to further exhibit the excellent physical properties of the resin component (A) used in the present adhesive, particularly the acrylic resin. Among them, preferred are disproportionated rosin esters obtained by disproportionating raw rosin and esterifying it with glycerin or pentaerythritol to adjust the softening point to a range of 70 to 130°C, polymerized rosin esters obtained by dimerizing raw rosin and esterifying it with pentaerythritol to adjust the softening point to a range of 110 to 170°C, and rosin phenols obtained by adding phenol to raw rosin to adjust the softening point to a range of 120 to 160°C.

[0082] The terpene resin is a general term for compounds based on the isoprene principle and represented by the molecular formula (C5H8)n. Examples of tackifiers used in the present adhesive include resins obtained by homopolymerization or copolymerization of monoterpenes (e.g., α-pinene, β-pinene, limonene, etc.) with a Friedel-Crafts catalyst. Specifically, examples of resins obtained by homopolymerization or copolymerization of monoterpenes include α-pinene resins, β-pinene resins, dipentene resins, terpene phenol resins, aromatic modified terpene resins, and hydrogenated terpene resins obtained by hydrogenating these resins. Among these, terpene phenol resins are preferred because of their good compatibility with the resin component (A) used in the present adhesive, particularly with acrylic resins. Any of the terpene phenol resins can further exhibit the excellent physical properties of the resin component (A), particularly the acrylic resin. In particular, those having a softening point of 90 to 170°C and a hydroxyl value in the range of 20 to 250 (mgKOH / g) are preferred, and those having a softening point of 100 to 150°C and a hydroxyl value in the range of 50 to 150 (mgKOH / g) are more preferred.

[0083] The petroleum resin is obtained, for example, by polymerization and further hydrogenation of C4-C5 and C9-C11 fraction monomers produced by thermal decomposition of naphtha or the like. Depending on the type of raw material fraction, examples include pure monomer resins, aliphatic (C5) petroleum resins, aromatic (C9) petroleum resins, and hydrogenated petroleum resins. The use of any of the petroleum resins allows the resin component (A), particularly the acrylic resin, to exhibit its excellent physical properties. Among them, those having a softening point in the range of 90 to 130°C are preferred, and it is further preferred to use a copolymerization system of a styrene monomer and an aliphatic monomer.

[0084] The softening point of the tackifier can be measured by the ring and ball method of JIS K 2531, and the hydroxyl value can be measured by potentiometric titration in accordance with JIS K 0070.

[0085] When the present adhesive contains a tackifier, the content of the tackifier is usually 50 parts by mass or less, preferably 30 parts by mass or less, more preferably 20 parts by mass or less, based on 100 parts by mass of the resin component (A) used in the present adhesive, particularly the acrylic resin. The lower limit is 0 parts by mass, but is preferably 1 part by mass or more, more preferably 5 parts by mass or more. However, the tackifier may be blended in an appropriate amount depending on the physical properties required for the adhesive, and the content of the tackifier is not limited to the above range.

[0086] <Other ingredients> The adhesive may contain, as other components, various additives such as acrylic monomers, polymerization inhibitors, antioxidants, corrosion inhibitors, crosslinking promoters, radical generators, peroxides, UV absorbers, plasticizers, pigments, stabilizers, fillers, radical scavengers, metals, and resin particles, within the scope of the invention. These may be used alone or in combination of two or more. In addition to the above, the adhesive may contain a small amount of impurities contained in the manufacturing raw materials of the adhesive components.

[0087] When the adhesive contains other components, the content of the other components is preferably 5 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less, based on 100 parts by mass of the resin component (A) used in the adhesive, particularly the acrylic resin. The lower limit is usually 0 parts by mass. If the content is too high, the compatibility with the resin component (A) decreases, and the durability tends to decrease. However, for additives (pigments, fillers, metals, resin particles, etc.) that do not exert their effects at the above content, an appropriate amount may be added within a range that exerts the effect of the additive while not inhibiting the effects of the present invention.

[0088] The adhesive of the present invention is a pressure-sensitive adhesive composition containing the above-mentioned resin component (A), particularly an acrylic resin, and optionally a crosslinking agent (B), and further a tackifier, other components, etc., in which at least a part of the composition is crosslinked. That is, the adhesive composition includes not only a case in which almost the entirety of the pressure-sensitive adhesive composition is crosslinked, but also a case in which a part of the pressure-sensitive adhesive composition is in an uncrosslinked state, and a case in which a part of the pressure-sensitive adhesive composition is crosslinked. The above-mentioned pressure-sensitive adhesive or pressure-sensitive adhesive composition in which the resin component (A) is an organic solvent-based resin is an organic solvent-based pressure-sensitive adhesive or an organic solvent-based pressure-sensitive adhesive composition. The method for producing the pressure-sensitive adhesive composition is not particularly limited. In addition to the commonly known mechanical kneading dispersion method, known methods such as a solvent dispersion method and an ultrasonic dispersion method can be used as necessary.

[0089] In order to increase the holding power of the pressure-sensitive adhesive, the gel fraction is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more. The gel fraction can be adjusted by adjusting the type and content of the crosslinking agent (B). The upper limit of the gel fraction is preferably 70% by mass, more preferably 60% by mass, and even more preferably 50% by mass. If the gel fraction is too low, the holding power tends to decrease, and if the gel fraction is too high, the peel strength tends to decrease. Furthermore, if the gel fraction is too low, the flame retardancy tends to decrease, whereas if it is too high, the pressure-sensitive adhesive layer becomes too hard, and the substrate does not shrink, tending to decrease the flame retardancy.

[0090] The gel fraction is a measure of the degree of crosslinking (degree of hardening) and is determined by the method described below.

[0091] <<Adhesive tape>> An adhesive tape according to one embodiment of the present invention (hereinafter sometimes referred to as "the adhesive tape") has a substrate and an adhesive layer on at least one side (one side) of the substrate, and this adhesive layer contains an adhesive obtained by crosslinking the above-mentioned adhesive composition. For example, the pressure-sensitive adhesive composition is dissolved in a solvent such as ethyl acetate to prepare a pressure-sensitive adhesive composition solution for coating so that the solid content concentration is 10 to 70 mass %, and this solution is coated on a substrate and dried to crosslink the pressure-sensitive adhesive composition and form a pressure-sensitive adhesive layer containing the pressure-sensitive adhesive, thereby producing a pressure-sensitive adhesive tape.

[0092] The method for producing the present pressure-sensitive adhesive tape is not particularly limited, and a known method can be adopted. For example, the present pressure-sensitive adhesive tape can be produced by a method of coating one side of a substrate with a pressure-sensitive adhesive composition solution, and then laminating a release liner on the surface of the pressure-sensitive adhesive layer formed by drying, or by a method of coating one side of a release liner with a pressure-sensitive adhesive composition solution, and then laminating a substrate on the surface of the pressure-sensitive adhesive layer formed by drying. Among these, the method of coating one side of a release liner with a pressure-sensitive adhesive composition solution, and then laminating a substrate on the surface of the pressure-sensitive adhesive layer formed by drying is preferred from the viewpoint of handling, etc.

[0093] The substrate is preferably one that can be torn by hand. The surface of the substrate may be appropriately subjected to a known or conventional surface treatment, for example, a physical treatment such as a corona discharge treatment or a plasma treatment, or a chemical treatment such as an undercoat treatment.

[0094] The substrate is not particularly limited and may be any known substrate, such as rayon cloth, cotton cloth, polyester cloth, cloth made of blended yarn of rayon and polyester, woven fabric such as flat yarn cloth, nonwoven fabric, laminated film in which plastic film or the like is laminated on woven fabric such as flat yarn cloth, etc. Among these, substrates containing woven fabrics are preferred from the viewpoint of high tensile strength in the longitudinal direction, and substrates having flat yarn cloth are more preferred. The present pressure-sensitive adhesive tape using a substrate having flat yarn cloth can be further excellent in flame retardancy and ease of hand cutting.

[0095] In addition, the term "substrate having a flat yarn cloth" conceptually includes not only the flat yarn cloth itself but also a laminated film in which a plastic film or the like is laminated to a flat yarn cloth.

[0096] A flat yarn cloth is a woven fabric made by cutting a film called a flat yarn into strips and stretching it to give it strength, and the crossings of the flat yarns that cross vertically and horizontally of this woven fabric are usually fixed by heat fusion to prevent misalignment. As the material for the flat yarn, an olefin resin such as polyethylene or polypropylene is preferable, polyethylene is more preferable, and high-density polyethylene is even more preferable.

[0097] By using a base material containing flat yarn cloth as the base material of this adhesive tape, it is possible to make the adhesive tape more flame-retardant. Although the reason for this is unclear, it is thought that flat yarn cloth is made by weaving yarn stretched in one direction, and when an ignition source approaches and the temperature rises, it shrinks, and when the ignition source moves away, it becomes more difficult for the tape to catch fire.

[0098] It is preferable to use a substrate in which a plastic film is laminated on the flat yarn cloth, since stable adhesive properties and peelability can be obtained. This is because, in the case of a double-sided adhesive tape, the plastic film prevents the adhesive on one side from passing through the substrate and mixing with the adhesive on the other side, and inhibits additives contained in the adhesive on one side, such as the crosslinking agent (B) and plasticizer, from migrating to the adhesive on the other side. In addition, laminating a plastic film on the flat yarn cloth improves hand-cutting properties and linearity of the fracture surface, probably because the breaking point is smoothly propagated. As the plastic film to be laminated on the flat yarn cloth, a polyethylene film is preferable, and a low-density polyethylene film is more preferable.

[0099] In addition, the substrate in which the plastic film is laminated to the flat yarn cloth is preferably lightweight, and the plastic film is preferably thin. The thickness of the plastic film is preferably 10 to 80 μm. The plastic film may be laminated to only one side of the flat yarn cloth, or may be laminated to both sides. As for the method of laminating the film to the flat yarn cloth, extrusion lamination is preferable because it can reduce weight without using an adhesive.

[0100] The thickness of the substrate containing the flat yarn cloth is preferably 10 to 200 μm, more preferably 50 to 100 μm, and further preferably 60 to 90 μm. If the thickness is too thin, the hand tearability is improved but defects such as the inclusion of wrinkles during the production of the adhesive tape tend to increase, whereas if the thickness is too thick, defects during the production of the adhesive tape are reduced but a larger force is required to cut, and the hand tearability tends to decrease.

[0101] Examples of the release liner include paper obtained by laminating a film such as polyethylene onto glassine paper, craft paper, or clay-coated paper, paper coated with a resin such as polyvinyl alcohol or an acrylic acid ester copolymer, and synthetic resin film obtained by coating a release agent such as a fluorine-based resin or silicone-based resin onto a synthetic resin film such as polyester or polypropylene. These may be used alone or in combination of two or more kinds.

[0102] Among these, paper release liners are preferred because they can be easily torn by hand, and the basis weight of the base paper is 40 to 120 g / m 2 , preferably 50 to 80 g / m 2 Particularly preferred is a paper release liner having the above structure. Furthermore, the thickness of such a release liner is preferably 40 to 180 μm, more preferably 60 to 140 μm, and even more preferably 80 to 120 μm. If the thickness is too thin, wrinkles may occur during winding, making production difficult, while if the thickness is too thick, the ease of tearing by hand may decrease.

[0103] The coating device used when coating the pressure-sensitive adhesive composition on one side of the above-mentioned substrate or release liner can be any commonly used coating device, such as a roll knife coater, a die coater, a roll coater, a bar coater, a gravure roll coater, a reverse roll coater, a dipping coater, a blade coater, etc.

[0104] The thickness of the pressure-sensitive adhesive layer after drying is preferably from 5 to 200 μm, more preferably from 10 to 150 μm, and even more preferably from 15 to 130 μm. If the thickness is too thick, it tends to be difficult to apply the pressure-sensitive adhesive composition, whereas if the thickness is too thin, sufficient adhesive strength tends to be difficult to obtain.

[0105] The drying conditions for drying the adhesive composition solution may be such that the solvent and residual monomers in the adhesive composition are dried and removed, and the resin component (A) used in the adhesive, particularly the functional group of the acrylic resin, reacts with the crosslinking agent (B) to form a crosslinked structure. For example, the drying conditions are preferably 60 to 120°C and about 1 to 5 minutes. After drying, the sheet-like substrate is aged in a state where it is laminated with the adhesive layer, and the crosslinking reaction can be further promoted.

[0106] The pressure-sensitive adhesive tape may be a single-sided pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer on one side of a substrate, or a double-sided pressure-sensitive adhesive tape having a pressure-sensitive adhesive layer on each side of a substrate. In addition, both pressure-sensitive adhesive layers of the double-sided pressure-sensitive adhesive tape may be pressure-sensitive adhesive layers having the same composition, or pressure-sensitive adhesive layers having different compositions.

[0107] In addition, when a release liner is laminated on the adhesive layer of the double-sided adhesive tape, it is preferable to select the release liners laminated on both sides so that they have different peel strengths in order to improve workability. For example, the workability is improved by selecting a release liner with a lighter peel strength on the side of the double-sided adhesive tape that is first applied than the release liner on the side of the double-sided adhesive tape that is next applied.

[0108] The adhesive tape may be in the form of a roll or in the form of sheets, or may be further processed into various shapes. When the adhesive tape is a double-sided adhesive tape in a sheet state, it is preferable that a release liner be provided on the surface of both of the two adhesive layers, and when it is in a roll state, it is preferable that a release liner be provided on the surface of only one of the two adhesive layers.

[0109] Thus, the present adhesive tape is obtained, and it is preferable that the adhesive properties of the present adhesive tape are not deteriorated even when applied to an adherend or a substrate that deteriorates the adhesive properties. It is also preferable that the present adhesive tape has good holding power. Furthermore, when a substrate having hand-cuttability is used as the substrate, the tape can be easily cut by hand at any position in the width direction of the tape without using a tape cutter or the like, and the tape is particularly useful as an adhesive tape.

[0110] The adhesive strength of the adhesive layer in this adhesive tape is preferably 180° peel strength of 1 to 100N / 25mm against the adherend to be used. In particular, when a test plate made of SUS304 steel, which has a relatively high polarity, is used as the adherend, the 180° peel strength is preferably 10N / 25mm or more, particularly preferably 20N / 25mm or more, and further preferably 30N / 25mm or more. The upper limit is usually about 100N / 25mm.

[0111] The adhesive strength can be measured in accordance with JIS Z 0237. Specifically, an adhesive tape is cut to a width of 25 mm and a length of 150 mm, and the adhesive layer of the adhesive tape is pressed onto a test plate, and the adhesive tape is peeled off from the test plate at a peel angle of 180° and a speed of 300 mm / min, to measure the peel strength.

[0112] The adhesive strength varies depending on the composition (material) and surface condition (surface roughness) of the adherend, treatment (cleaning) conditions, etc., and is not limited to the above peel strength range.

[0113] When the test piece is a double-sided adhesive tape, the adhesive side not to be tested can be measured by covering it with a polyethylene terephthalate film (Lumirror S10, manufactured by Toray Industries, Inc.) having a nominal thickness of 25 μm as specified in JIS C2318.

[0114] Furthermore, when the holding strength of the adhesive layer in this adhesive tape is measured by the method described below, it is particularly preferable that the test piece does not fall off the test plate after 24 hours (1,440 minutes) has elapsed, and even if the test piece falls within 24 hours, the holding time is preferably 100 minutes or more, more preferably 150 minutes or more, and particularly preferably 500 minutes or more.

[0115] To measure holding power, an adhesive tape cut to a width of 25 mm and a length of 75 mm is pressed against a SUS plate so that the contact area between the adhesive layer and the SUS plate is 25 mm wide x 25 mm long, and then a 1000 g weight is attached so that the adhesive tape hangs vertically from the SUS plate. The holding power can be measured by measuring the time it takes for the adhesive tape to fall in an environment of 40°C.

[0116] The gel fraction of the adhesive layer of the present adhesive tape is the same as that of the adhesive, and is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more. The upper limit of the gel fraction is preferably 70% by mass or less, more preferably 60% by mass or less. By setting the gel fraction within the above range, a flame-retardant adhesive tape tends to be obtained.

[0117] The gel fraction is an indicator of the degree of crosslinking (degree of curing) and can be measured, for example, by the following method.

[0118] To measure the gel fraction, a 200-mesh SUS wire mesh large enough to encase the adhesive tape is prepared and its mass is measured (1). The paper release liner is peeled off from the adhesive tape and wrapped in the aforementioned SUS wire mesh, and the mass of the tape together with the wire mesh is measured (2). After immersion in toluene kept at 23°C for 48 hours, it is thoroughly dried and the mass of the tape together with the wire mesh is measured (3). After immersion, the tape is removed from the wire mesh, the remaining adhesive layer is removed, and the mass of the base material is measured (4). Subtraction is performed as shown in the formula below, and the mass percentage of the adhesive component after immersion compared to before immersion is determined as the gel fraction. [Formula] Gel fraction (%) = (mass of tape after immersion including the mass of SUS wire mesh (3) - mass of substrate (4) - mass of SUS wire mesh (1)) / (mass of tape before immersion including the mass of SUS wire mesh (2) - mass of substrate (4) - mass of SUS wire mesh (1)) x 100

[0119] The gel fraction of the pressure-sensitive adhesive can be adjusted to fall within the above range by adjusting the degree of polymerization of the resin component (A) and the type and amount of the crosslinking agent (B), for example.

[0120] The pressure-sensitive adhesive tape is evaluated by a flame retardancy test conforming to ISO 11925-2, which is an ignition test standard stipulated in the European building material fire safety standard EN 13501-1. In such a flame retardancy test, the burning length of the pressure-sensitive adhesive tape is preferably 195 mm or less, more preferably 185 mm or less, and even more preferably 180 mm or less.

[0121] The adhesive tape produced by the above method has excellent adhesiveness and high flame retardancy, and can therefore be suitably used as an adhesive tape for construction. EXAMPLES

[0122] The present invention will be further described below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are based on mass.

[0123] First, the acrylic resin (A) serving as the resin component was prepared as follows. The weight average molecular weight, dispersity, glass transition temperature and viscosity of the resin component (A), particularly the acrylic resin, were measured according to the methods described above.

[0124] <Resin component (A)> Prior to the production of the acrylic resin (A), the following were prepared as copolymerization components (monomers) to be used in the production. Monomer (a1): Diphenylvinylphosphonate Monomer (a2): acrylic acid Monomer (a3): 2-hydroxyethyl methacrylate Monomer (a4-1): n-butyl acrylate Monomer (a4-2): 2-Ethylhexyl acrylate Monomer (A5): Vinyl acetate

[0125] [Production of acrylic resin (A-1)] In a reactor equipped with a thermometer, a stirrer and a reflux condenser, 60 parts of ethyl acetate was charged as a solvent, and the temperature was raised to the reflux temperature of the solvent while stirring, and a mixture of 1 part of diphenylvinylphosphonate (a1), 2.9 parts of acrylic acid (a2), 0.1 parts of 2-hydroxyethyl methacrylate (a3), 45.5 parts of n-butyl acrylate (a4-1), 45.5 parts of 2-ethylhexyl acrylate (a4-2), 5 parts of vinyl acetate (a5), 2.6 parts of ethyl acetate, and 0.09 parts of azobisisobutyronitrile (AIBN) as a polymerization initiator was added dropwise over 2 hours as copolymerization components. After polymerization at the reflux temperature for 1 hour, a polymerization initiator solution in which 0.07 parts of AIBN were dissolved in 10 parts of ethyl acetate was added, and polymerization was continued for another 2 hours at the reflux temperature. Next, a mixed solution in which 0.06 parts of AIBN were dissolved in 5 parts of ethyl acetate was added and polymerized at reflux temperature for 2 hours. The reaction mixture was then diluted with ethyl acetate to obtain an acrylic resin (A-1) solution with a solid content of 50%. The weight average molecular weight of the obtained acrylic resin (A-1) was 600,000, the dispersity was 4.0, and the viscosity was 5,500 mPa·s / 25°C.

[0126] [Production of acrylic resin (A-2)] In a reactor equipped with a thermometer, a stirrer and a reflux condenser, 60 parts of ethyl acetate was charged as a solvent, and the temperature was raised to the reflux temperature of the solvent while stirring, and a mixture of 5 parts of diphenylvinylphosphonate (a1), 2.9 parts of acrylic acid (a2), 0.1 parts of 2-hydroxyethyl methacrylate (a3), 43.5 parts of n-butyl acrylate (a4-1), 43.5 parts of 2-ethylhexyl acrylate (a4-2), 5 parts of vinyl acetate (a5), 2.6 parts of ethyl acetate, and 0.09 parts of AIBN as a polymerization initiator was added dropwise over 2 hours as copolymerization components. After polymerization at the reflux temperature for 1 hour, a polymerization initiator solution in which 0.07 parts of AIBN were dissolved in 10 parts of ethyl acetate was added, and polymerization was continued for another 2 hours at the reflux temperature. Next, a mixed solution in which 0.06 parts of AIBN were dissolved in 5 parts of ethyl acetate was added and polymerized at reflux temperature for 2 hours. The reaction mixture was then diluted with ethyl acetate to obtain an acrylic resin (A-2) solution with a solid content of 50%. The weight average molecular weight of the obtained acrylic resin (A-2) was 500,000, the dispersity was 4.5, and the viscosity was 2,900 mPa·s / 25°C.

[0127] [Production of acrylic resin (A-3)] In a reactor equipped with a thermometer, a stirrer and a reflux condenser, 53.6 parts of ethyl acetate and 5.9 parts of acetone were charged as a solvent, and the temperature was raised to the reflux temperature of the solvent while stirring, and a mixture of 10 parts of diphenylvinylphosphonate (a1), 2.9 parts of acrylic acid (a2), 0.1 parts of 2-hydroxyethyl methacrylate (a3), 41 parts of n-butyl acrylate (a4-1), 41 parts of 2-ethylhexyl acrylate (a4-2), 5 parts of vinyl acetate (a5), 2.6 parts of ethyl acetate, and 0.07 parts of AIBN as a polymerization initiator was added dropwise over 2 hours as copolymerization components. After polymerization at the reflux temperature for 1 hour, a polymerization initiator solution in which 0.07 parts of AIBN was dissolved in 10 parts of ethyl acetate was added, and polymerization was continued for another 2 hours at the reflux temperature. Next, a mixed solution in which 0.06 parts of AIBN were dissolved in 5 parts of ethyl acetate was added and polymerized at reflux temperature for 2 hours. The reaction mixture was then diluted with ethyl acetate to obtain an acrylic resin (A-3) solution with a solid content of 50%. The weight average molecular weight of the obtained acrylic resin (A-3) was 500,000, the dispersity was 4.9, and the viscosity was 2700 mPa·s / 25°C.

[0128] [Production of acrylic resin (A-4) (containing no structural units derived from phosphorus compounds)] In a reactor equipped with a thermometer, a stirrer and a reflux condenser, 60 parts of ethyl acetate was charged as a solvent, and the temperature was raised to the reflux temperature of the solvent while stirring. As copolymerization components, 2.9 parts of acrylic acid (a2), 0.1 parts of 2-hydroxyethyl methacrylate (a3), 46 parts of n-butyl acrylate (a4-1), 46 parts of 2-ethylhexyl acrylate (a4-2), 5 parts of vinyl acetate (a5), 2.6 parts of ethyl acetate, and 0.09 parts of AIBN as a polymerization initiator were mixed and dissolved and dropped over 2 hours. After polymerization at the reflux temperature for 1 hour, a polymerization initiator solution in which 0.07 parts of AIBN were dissolved in 10 parts of ethyl acetate was added and polymerization was continued for another 2 hours at the reflux temperature. Next, a mixed solution in which 0.06 parts of AIBN were dissolved in 5 parts of ethyl acetate was added and polymerization was continued for 2 hours at the reflux temperature, and the reaction mixture was diluted with ethyl acetate to obtain an acrylic resin (A-1) solution with a solid content of 50%. The weight average molecular weight of the obtained acrylic resin (A-4) was 600,000, the dispersity was 4.8, and the viscosity was 7,500 mPa·s / 25°C.

[0129] <Crosslinking agent (B)> The following was prepared as the crosslinking agent (B). Isocyanate-based crosslinking agent: Takenate D-101E, manufactured by Mitsui Chemicals

[0130] <Example 1> [Preparation of adhesive tape] A pressure-sensitive adhesive composition solution was prepared by adding 1.5 parts of an isocyanate-based crosslinking agent and an appropriate amount of methyl ethyl ketone to 100 parts of the solid content of the acrylic resin (A-1) as the resin component (A) and mixing until uniform. The pressure-sensitive adhesive composition solution was then applied to a paper release liner (manufactured by Shinomura Chemical Industry Co., Ltd., product name "SSW-53FOAG": base paper basis weight 93 g / m 2The solution was applied to the heavy release surface of the adhesive tape (Agile) using an applicator so that the thickness after application would be 100 μm, and the adhesive tape was dried at 80° C. for 5 minutes, and then a flat yarn (manufactured by Diatex, thickness 130 μm) was attached to the adhesive tape. The adhesive tape was then subjected to heat aging treatment in a dryer at 40° C. for 7 days to obtain an adhesive tape.

[0131] <Example 2> An adhesive tape of Example 2 was obtained in the same manner as in Example 1 above, except that the acrylic resin (A-2) was used as the resin component (A) and the amount of the isocyanate-based crosslinking agent was changed to 2.0 parts.

[0132] <Example 3> An adhesive tape of Example 3 was obtained in the same manner as in Example 2 above, except that the acrylic resin (A-3) was used as the resin component (A).

[0133] <Comparative Example 1> An adhesive tape of Comparative Example 1 was obtained in the same manner as in Example 1 above, except that the acrylic resin (A-4) was used as the resin component (A) and the amount of the isocyanate-based crosslinking agent was changed to 0.75 parts.

[0134] The adhesive tapes obtained in the above Examples and Comparative Examples were subjected to the following evaluation tests. The results are summarized in Table 1.

[0135] <Flame retardancy test (EN13501-1 ISO11925-2)> Using the above adhesive tape, tests were conducted in accordance with ISO11925-2, an ignition test standard stipulated in the European building material fire safety standard EN13501-1, and flame retardancy was evaluated based on the average burning length and the presence or absence of drips.

[0136] <180° peel strength> The above adhesive tape was cut to a width of 25 mm and a length of 150 mm to prepare a test piece. In addition, a test plate of SUS304-BA (mirror surface finish) steel that had been heat-treated at 175°C for 1 hour was used as an adherend by cleaning the surface with methyl ethyl ketone and then leaving it to stand overnight in an atmosphere of 23°C and 50%RH. The paper release liner was peeled off from the above test piece, and the adhesive layer of the test piece was pressed onto the above test plate by two reciprocations of a roller weighing 2 kg at a pressing speed of 10 mm / s. After pressing, the test piece was left to stand for 72 hours in an atmosphere of 23°C and 50%RH, the play part of the test piece was folded back by 180° and peeled off by 30 mm, and then the test plate was fixed to the lower chuck of the peel strength tester and the end of the test piece was fixed to the upper chuck in the same atmosphere, and the adhesive tape was peeled off from the adherend at a peel angle of 180° and a speed of 300 mm / min, and the adhesive strength was measured.

[0137] [Table 1]

[0138] From the results of Table 1 above, Examples 1 to 3, which used an adhesive containing a resin component (A) containing a structural unit derived from a specific phosphorus compound monomer (a1), had a short burning length in the flame retardancy test and were excellent in flame retardancy. Furthermore, Examples 2 and 3, which contained many structural units derived from a specific phosphorus compound monomer (a1), did not drip and were even more excellent in flame retardancy. The peel strength was also sufficient for an adhesive tape.

[0139] In contrast, Comparative Example 1, which did not contain any structural units derived from the specific phosphorus compound monomer (a1), had a long burning length and dripping occurred, indicating that it was poor in flame retardancy. [Industrial Applicability]

[0140] The pressure-sensitive adhesive and pressure-sensitive adhesive tape of the present invention are excellent in adhesion and flame retardancy, and are particularly excellent as a construction pressure-sensitive adhesive tape, and are therefore highly anticipated.

Claims

1. A pressure-sensitive adhesive comprising a resin component (A), A pressure-sensitive adhesive, wherein the resin component (A) contains a structural unit derived from a monomer represented by the following formula (a1): 【Chemistry 1】 (n and m are each 0 or 1, R 1 , R 2 each represents an alkyl group having 1 to 18 carbon atoms, a phenyl group, or a phenyl group having a substituent, and may be the same or different.

2. The pressure-sensitive adhesive according to claim 1, wherein the resin component (A) contains a structural unit derived from a (meth)acrylic monomer (a2) having a carboxy group and / or a (meth)acrylic monomer (a3) ​​having a hydroxyl group.

3. The pressure-sensitive adhesive according to claim 1 or 2, further comprising a crosslinking agent (B).

4. 3. An adhesive tape comprising a substrate and an adhesive layer formed from the adhesive according to claim 1 or 2 on at least one surface of the substrate.

5. The adhesive tape according to claim 4 , wherein the substrate comprises a flat yarn cloth.

Citation Information

Patent Citations

  • adhesive composition

    JP2001524574A

  • high shear pressure sensitive adhesive

    JP2009529090A

  • Double-sided adhesive tape for fastening aircraft components

    JP2015143353A

  • Nanocrystalline cellulose-containing pressure-sensitive adhesive

    JP2017533289A

  • Adhesive and adhesive tape

    JP2022159098A