Decorative mirror manufacturing method and decorative mirror

The use of silicon dioxide and calcium oxide glass substrates with precise polishing and UV-curable inkjet printing addresses the issues of ink peeling and lack of depth in existing methods, resulting in durable, high-quality decorative mirrors with three-dimensional images.

JP2024147672AActive Publication Date: 2024-10-16M&G KITADE CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024112323
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-04-06
Filing Date
2024-07-12
Publication Date
2024-10-16
Estimated Expiration
2040-09-18

Smart Images

  • Figure 2024147672000001_ABST
    Figure 2024147672000001_ABST
Patent Text Reader

Abstract

To provide a decorative mirror that has a high-quality image printed in color on the surface of glass.SOLUTION: A decorative mirror comprises: a transparent or translucent primer layer 3 printed on a glass substrate 1; an ultraviolet-curable white ink layer 4 partially printed on the primer layer 3; an ultraviolet-curable color ink layer 5 laminated on the entire surface of the white ink layer 4 and the exposed-state primer layer 3; and a reflective layer 2 provided on the entire back surface of the glass substrate. The glass substrate 1 contains silicon dioxide of 60-80 wt.% and calcium oxide of 2-20 wt.% as constituent materials, and has a nominal thickness of 0.3 mm to 8 mm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a decorative mirror having a high-quality image printed in color on its glass surface, and a method for manufacturing the same. [Background technology]

[0002] American cafes and bars are often decorated with decorative items called pub mirrors. A pub mirror is a decorative item with pictures or letters drawn on the surface of a mirror. It is hung on the wall or displayed on a shelf, creating a stylish atmosphere in the store.

[0003] Meanwhile, in Japan, this type of product is also becoming more popular, and is not only being used to decorate restaurants and izakayas, but is also attracting attention from individuals as products featuring their favorite anime characters. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Utility Model Application Publication No. 57-142971 [Patent Document 2] JP 2016-106674 A [Patent Document 3] Japanese Patent Application Publication No. 10-127449 [Patent Document 4] Utility Model Registration No. 3182102 [Patent Document 5] Japanese Patent Application Publication No. 06-030832 Summary of the Invention [Problem to be solved by the invention]

[0005] However, it is not easy to fix pictures or letters on glass, and the ink on the glass surface is prone to peeling off. Therefore, the general method is to print pictures or letters on the back side of the glass (Patent Documents 1 and 2), or to attach a printed sheet to the glass surface (Patent Documents 3 and 4).

[0006] There is also a document that describes a technology for thermally transferring an image onto the glass surface (Patent Document 5). However, in this invention, in order to leave the exposed glass area where the mirror surface is exposed, it is necessary to partially attach a masking film coated with an adhesive to the glass surface prior to the primer step, and due to the nature of the masking film, it is not possible to create fine patterns such as letters.

[0007] In addition, in the first place, in this invention, the image that is thermally transferred from a transfer sheet printed with an image of wood grain, stone grain, etc. is merely a simple repeated decoration that decorates the periphery of the mirror surface, lacking impact, and does not utilize the thickness of the mirror to express a three-dimensional effect.

[0008] The present invention has been made in consideration of the above problems, and has an object to provide a decorative mirror having a high-quality image printed in color on the glass surface, and a method for manufacturing such a decorative mirror. [Means for solving the problem]

[0009] In order to achieve the above object, the method for manufacturing a decorative mirror according to the present invention comprises the steps of: 2 The method includes the following steps: a polishing step in which the surface of a glass substrate having a nominal thickness of 0.3 mm to 8 mm and containing 60 to 80 wt% of magnesium oxide (MgO) and 2 to 20 wt% of calcium oxide (CaO) as constituent materials is polished to an arithmetic mean roughness Ra of 0.0007 to 0.0025 μm; a priming step in which a transparent or semi-transparent primer layer is formed on the surface of the glass substrate after the first step; a base step in which, prior to the color printing step, white ink is partially printed and cured with ultraviolet light to make important areas of the design white; and a color printing step in which color ink is printed on the glass surface or base layer that has been subjected to the primer step and cured with ultraviolet light.

[0010] The present invention also provides a decorative mirror comprising a transparent or semi-transparent primer layer printed on a glass substrate polished to an arithmetic mean roughness Ra of 0.0007 to 0.0025 μm, a white ink layer made of ultraviolet curable ink partially printed on the primer layer, and a color ink layer made of ultraviolet curable ink printed on the entire surface of the white ink layer and on the exposed primer layer, the glass substrate being made of silicon dioxide (SiO 2 It is characterized by containing 60 to 80 wt% of magnesium oxide (MgO) and 2 to 20 wt% of calcium oxide (CaO) as constituent materials and having a nominal plate thickness of 0.3 to 8 mm.

[0011] Although not particularly limited, in the present invention, the base printing step and the color printing step are preferably performed using one or more inkjet printers. More preferably, the primer step is also performed using an inkjet printer.

[0012] By inkjet printing the primer, it is possible to form any exposed portion of the glass mirror surface where no primer layer exists (i.e., exposed glass portion). In other words, by inkjet printing the primer, it is possible to form any shape of exposed glass portion, even if it has a minute and complicated pattern such as letters or logos.

[0013] In general, in an inkjet printer, ink is turned into fine particles by applying pressure or heat, and then sprayed onto a printing substrate, but in the present invention, it is preferable to adopt a configuration in which an ultraviolet curing process is performed consecutively to the printing process. After ultraviolet curing, the ink preferably has a pencil hardness of about 3H based on JIS K-5400 8.4.

[0014] In any case, in the present invention, since the polishing step is provided to polish the glass substrate, even slight oil stains and fingerprints that cannot be seen with the naked eye can be reliably removed, and the quality of the final finish is significantly improved. If the polishing step is not provided, stains that cannot be seen with the naked eye may be caused to stand out due to the influence of the ink printed thereafter.

[0015] Furthermore, in the present invention, a priming process is carried out prior to the color printing process in which key areas of the design are painted white, so that a silhouette of the key areas of the design is formed on the back surface of the glass through the thickness of the glass plate, resulting in the effect that the key areas appear to be slightly raised.

[0016] Here, when forming a decorative mirror from a single piece of glass substrate as in the first, second, and fourth embodiments, if the glass plate thickness is thinner than the nominal value of 2 mm (actual measured value of approximately 1.7 to 2.3 mm), the floating effect is somewhat lacking and there are strength problems, while if the glass plate thickness is 8 mm or more, it becomes heavy and looks somewhat unnatural.

[0017] Therefore, when forming a decorative mirror using a single glass substrate, a glass thickness of nominal value 3 mm (actual value 2.7 mm to 3.3 mm) or nominal value 5 mm (actual value 4.7 mm to 5.3 mm) is suitable, and a glass thickness of nominal value 2.0 mm to 8.0 mm, and optimally a nominal value of about 3 mm should be selected.

[0018] On the other hand, when a decorative mirror is formed by polymerizing the first and second substrates as in the third and fifth embodiments, the first substrate reinforces the second substrate, so from the standpoint of reducing weight, the thickness of the glass substrate should be 2 mm or less (preferably 1 mm or less), and the thickness can be reduced to approximately 0.3 mm.

[0019] The white ink is not particularly limited, but is preferably selected to contain 40-60Wt% of photosensitive resin, 10-20Wt% of acrylic acid ester, and 5-10Wt% of phosphine oxide derivative. Suitable examples of the acrylic acid ester include ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and 2-hydroxyethyl acrylate.

[0020] In addition, the white ink should preferably contain titanium oxide as a pigment. However, since a white ink of this composition has poor adhesion to glass, it is essential to provide a primer layer on the glass substrate in order to prevent peeling. The poor adhesion to glass is not limited to white ink, but is the same for other color inks.

[0021] The primer is not particularly limited as long as it has excellent adhesion to glass, but preferably, a primer containing acrylic esters, photosensitive resin, and phosphine oxide derivatives in a total amount of 98 to 99.9 Wt % is selected. It is also preferable that the primer further contains a polymerization inhibitor.

[0022] In any case, the primer layer should be transparent or semi-transparent, and since the primer layer is transparent or semi-transparent, it is possible to provide a difference in transparency between the main area of ​​the design drawn on the base layer and the background part of the design where the base layer is not provided. In other words, the background part, which is slightly transparent, and the main area, which is not transparent, are clearly distinguished visually, so that the main area is more clearly appealing. The main area is, for example, a display area of ​​an anime character, etc., and is preferably located approximately in the center of the glass surface, with the surrounding area being the background part.

[0023] The thickness of the white ink is not particularly limited, but should preferably be 20 μm to 50 μm, and more preferably about 30 μm. By providing a film thickness of this order, the color of the subsequent color ink is prevented from showing through the glass, and the finish of the color printed surface can be made more natural.

[0024] In general, it is preferable to print the white ink directly on the primer layer, but it is not prohibited to print the white ink over a black layer or a color layer printed on the primer layer. When the white ink is printed directly on the primer layer, a white silhouette is formed on the back surface of the glass, but by printing the black ink on the primer layer, a black silhouette can be formed on the back surface of the glass.

[0025] However, if color inks are printed by inkjet printing on top of the black ink layer that forms the black silhouette to realize the original design, the color ink particles will get caught between the fixed black ink particles, making the color dull and resulting in an unsatisfactory finish. Therefore, in this case, one or two white ink layers with a thickness of about 30 μm should be placed on top of the black ink layer, and then color inks should be printed to realize the original design.

[0026] Similarly, a silhouette similar to that on the front side can be formed on the back side of the glass by printing color ink on the primer layer. However, even if the same design is used, overlapping color inks will make the outline of the image unclear, so a white ink layer with a thickness of about 30 μm should be placed on top of the color print layer printed on the primer layer, or two layers, before printing color ink to achieve the original design.

[0027] As described above, in the present invention, in addition to the embodiment in which a white silhouette is formed on the back surface of the glass by directly printing a white ink on the primer layer, a black silhouette can be formed on the primer layer by printing a black ink, and a silhouette similar to that on the front surface can be formed by printing a color ink on the primer layer. However, when the manufacturing cost and the finish are evaluated comprehensively, it is generally optimal to print a layer of white ink directly on the primer layer.

[0028] In any case, in the present invention, a color image is printed on the glass surface excluding the glass exposed portion through a color printing process. That is, when the glass surface is viewed in plan before color printing, the glass surface is divided into a primer layer, a base layer in which white ink or the like is printed on the primer layer, and a glass exposed portion where no primer is present, and a color image is printed on the primer layer and the base layer excluding the glass exposed portion.

[0029] Here, the film thickness of the color ink should also be 20 μm to 50 μm, and more preferably, about 30 μm.

[0030] The color inks used in the color printing process include at least cyan, magenta, yellow, and black inks. These inks are not particularly limited as long as they are ultraviolet (UV) curable inks, but as the cyan ink, an ink containing 1-20 Wt% of photosensitive resin, 60-90 Wt% of acrylic acid esters, and 1-20 Wt% of phosphine oxide derivative as main components, and 1-5% of pigment, is preferably selected. Here, the pigment is preferably a copper compound. In addition to containing a photopolymerization initiator, the ink should also contain a polymerization inhibitor.

[0031] The photopolymerization initiator is a component that generates active species by receiving light and initiates a polymerization reaction of the photopolymerizable monomer, and examples of such a component include radical photopolymerization initiators, cationic photopolymerization initiators, etc. In the present invention, the ink contains a polymerization inhibitor, which suppresses the polymerization of the photopolymerizable monomer to a high level, thereby improving the storage stability and durability of the ink.

[0032] The above points are the same for magenta ink and yellow ink, and these inks should also preferably contain a photopolymerization initiator and a polymerization inhibitor. In addition, the main components are 1-20Wt% of photosensitive resin, 60-90Wt% of acrylic acid esters, and 1-20Wt% of phosphine oxide derivatives, and the magenta ink preferably contains 1-5% of magenta coloring material, and the yellow ink preferably contains a nickel compound pigment.

[0033] The black ink contains 1-5% carbon black as a coloring material, and preferably contains a photopolymerization initiator and a polymerization inhibitor, and preferably contains 1-10Wt% photosensitive resin, 60-90Wt% acrylic acid esters, and 5-10Wt% phosphine oxide derivative.

[0034] In addition, the glass surface after the color printing process may be provided with an appropriate protective layer or anti-reflection layer over its entirety. However, in order to increase the color and luster of the entire design, it is effective to print a gloss material with a thickness of 30 μm over the entire glass surface as a substitute for a protective layer. Here, it is preferable that the gloss material is also of the ultraviolet curing type, and the hardness after ultraviolet curing is preferably about 3H in pencil hardness based on JIS K-5400 8.4.

[0035] The glass substrate is made of silicon oxide (SiO 2 As long as the constituent materials are 60 to 80 Wt% of silicon oxide (SiO 2 ) 60~80Wt%, aluminum oxide (Al 2 O 3) 0-7Wt%, calcium oxide (CaO) 2-18Wt%, magnesium oxide (MgO) 0-8Wt%, sodium oxide (Na 2 O) and potassium oxide (K 2 A glass material with a total content of 5 to 25 wt% of O should be used.

[0036] Here, iron oxide (Fe 2 O 3 The content of should be kept below 1 Wt%, and if the content is kept below 0.05 Wt%, it is possible to manufacture products with high transparency and an even more luxurious feel.

[0037] Incidentally, in order to enhance the sense of luxury, it is preferable to provide a transfer process in which metal foil is thermally transferred to a required position following the color printing process. In this case, a metal foil sheet with metal foil evenly attached thereto is placed over the color ink layer, and laser light is irradiated in spots from above the metal foil sheet to thermally transfer the metal foil. It is also preferable to transfer the metal foil using heat and pressure instead of laser light. In these cases, the color ink layer is already laminated on the glass substrate, so that the metal foil can be thermally transferred. Effect of the Invention

[0038] According to the present invention described above, it is possible to realize a decorative mirror having a high-quality image printed in color on the glass surface. [Brief description of the drawings]

[0039] [Figure 1] 1 is a diagram for explaining a first embodiment; [Diagram 2] 11 is a diagram for explaining a second embodiment. [Diagram 3] 11 is a diagram for explaining a third embodiment. [Figure 4] 13 is a diagram for explaining a fourth embodiment. [Diagram 5] 13 is a diagram for explaining a fifth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0040] The manufacturing method of the decorative mirror of the embodiment will be described in more detail below, but the specific description does not limit the present invention in any way. First, Fig. 1(a) is a flow diagram showing the manufacturing method of the first embodiment, and Fig. 1(b) and Fig. 1(c) are cross-sectional views of a glass substrate showing the manufacturing process.

[0041] Fig. 1(a) shows the manufacturing process after a reflective layer made of aluminum or silver is formed on the back surface of the glass. The reflective layer is formed by, for example, vacuum deposition, and Fig. 1(b) shows a glass substrate 1 provided with a reflective layer 2.

[0042] The thickness of the glass substrate 1 is not particularly limited, but is preferably selected to have a nominal value of 3 mm (actual measurement value of about 2.7 mm to 3.3 mm). Such a glass substrate is brush-washed with warm water to remove surface dirt (ST10), and then cut to an appropriate size (ST11). The cut size is not particularly limited, but is preferably selected to have a size of about A2 (420 x 594 mm), A3 (297 x 420 mm), A4 (210 x 297 mm), or B5 (182 x 257 mm).

[0043] Once the above cutting process (ST11) is complete, polishing and cleaning with cesium is performed (ST12). Specifically, the glass surface that will become the printing surface is polished using cerium oxide particles with a particle size of about 1.2 to 1.4 μm. As a result of this polishing process, the glass powder generated during the cutting process, including any adhesions to the glass surface, is completely removed. Fingerprints and other oily stains are also completely removed.

[0044] The arithmetic mean roughness (Ra) of the glass surface after polishing is about 0.0007 to 0.0025 μm, preferably 0.0011 to 0.0020 μm, and more preferably 0.0011 to 0.0016 μm.

[0045] Next, a transparent primer layer 3 is provided on the flattened glass substrate to a thickness of about 30 μm (ST13). The primer may be applied or sprayed onto the glass surface, but in order to leave a fine pattern on the exposed glass, it is preferable to inkjet print the primer. In this embodiment, the processes of steps ST13 to ST15 and step ST17 are performed using an inkjet printer.

[0046] Next, the color image original depicting the anime characters or the like is subjected to appropriate color correction, and the main area depicting the characters or the like is extracted from the color-corrected image original. Then, image data specifying the main area is supplied to the printer, and an instruction is given to print this main area in white ink.

[0047] As a result, a white undercoat layer 4 of about 30 μm is formed in the important area of ​​the glass surface on which the primer layer 3 is provided (ST14). In the process of this step ST14, a UV-curable white ink is used, and after the important area is inkjet-printed in white, the important area is quickly UV-cured by irradiating it with UV light.

[0048] Next, the image data of the color-corrected image original composed of the main area and the background area is supplied to the printer, and the original image is color-printed on the glass surface (excluding the glass exposed area) divided into the base layer 4 and the primer layer 3 (ST15). In the color printing, cyan, magenta, yellow, and black inks are used, all of which are ultraviolet-curing inks.

[0049] After each part is inkjet printed in an appropriate color, the color ink is quickly cured by irradiating it with ultraviolet light. This color ink layer 5 also has a thickness of about 30 μm. Figure 1(c) shows a cross section of the glass substrate after the processing in step ST15.

[0050] Next, the metal foil is thermally transferred to the UV-cured color ink (ST16). Specifically, the glass substrate processed in step ST15 is placed in a thermal transfer machine, and a metal foil sheet is placed at the location where the metal foil is to be transferred. Then, by sending position data indicating the transfer position from a personal computer, a laser beam is irradiated at the required location, and the metal foil of the metal foil sheet is thermally transferred to the color ink (ST16).

[0051] Although not limited thereto, letters, symbols, logos, etc. are printed close to any of the four corners of the glass surface by thermal transfer of metal foil.

[0052] Finally, a gloss material is printed using an inkjet printer to increase the gloss (ST17). If gloss is not required, an appropriate protective layer is provided instead of the gloss layer. The hardness of the gloss layer and protective layer is about 3H in pencil hardness based on JIS K-5400 8.4.

[0053] As described above, in the first embodiment, the primer process (ST13) and the undercoat process (ST14) are carried out prior to the color printing process (ST15), so that the silhouette of the main area of ​​the design is formed on the back surface of the glass through the thickness of the glass sheet, which has the effect of making the main area appear slightly raised. In addition, the polishing process (ST12) is carried out first, so there is no risk of unintended patterns appearing.

[0054] Although an embodiment in which the base layer 4, which is the main region, is made white has been described above, it is also preferable to make the base layer black or to make it the original color. Figure 2 is a flow chart for explaining this second embodiment.

[0055] The processes in steps ST10 to ST13 are similar to those in the first embodiment, but in the base printing step (ST14), the base layer, which is the main region, is divided into a silhouette layer 6 and a white layer 4.

[0056] That is, first, black ink or color ink is printed on the main area where characters and the like are drawn to form the silhouette layer 6, and then white ink is printed to cover this silhouette layer 6 to form the white layer 4. When each ink layer is about 30 μm thick, the white ink particles get into the gaps between the black or colored ink particles, resulting in a dull color such as gray. Therefore, it is preferable to form a double white layer 4 to form a complete base layer without dullness.

[0057] After the white base layer 4 is formed in this manner, image data of the color-corrected image original consisting of the main area and background area is supplied to a printer, and the image original is color-printed on the glass surface (excluding the exposed glass area) divided into the base layer 4 and primer layer 3 (ST15). The subsequent processing is the same as in the first embodiment. In this embodiment, there is an effect that a black or natural color silhouette of the main area of ​​the design is formed on the back surface of the glass through the thickness of the glass plate.

[0058] As described above, in the first and second embodiments, a single glass substrate is provided with a reflective layer 2 on its back side and a color printed layer (3, 4, 5, 6, etc.) on its front side, but this is not particularly limited.

[0059] For example, as shown in Fig. 3, it is also suitable to prepare a first substrate BS1 (see Fig. 3(a)) having a reflective layer 2 on the front or back surface, and a second substrate BS2 (see Fig. 3(b)) having no reflective layer, provide a color printed layer (3-5 or 3-6, etc.) on the front or back surface of the second substrate BS2, and then overlay the first substrate BS1 on the color printed layer of the second substrate BS2 (see Fig. 3(c)). In this third embodiment, the second substrate BS2 is made of a glass material, but the first substrate BS1 is not necessarily limited to a glass material and may be made of a plastic material.

[0060] In this third embodiment, not only can a color printed surface with depth be expressed, but since the color printed surface is not exposed, there is an advantage that the color printed surface is reliably protected. From the viewpoint of protecting the printed surface, the configuration of Patent Document 2 can also be adopted, but in this case, during the process of vacuum-depositing a reflective layer on the printed surface of the glass substrate that has been through the printing steps (ST10 to ST17), defects due to dirt adhering to the printed surface may occur in the reflective layer, resulting in a drop in the yield rate. In contrast, in the third embodiment, the glass substrate BS1 can be reliably polished prior to the vacuum deposition of the reflective layer (see ST3 in FIG. 1(a)), so that defects occurring in the reflective layer can be prevented in advance.

[0061] In the third embodiment shown in FIG. 3, the first substrate BS1 and the second substrate BS2 are preferably made of the above-mentioned preferred glass material, that is, silicon oxide (SiO 2 ) 60~80Wt%, aluminum oxide (Al 2 O 3 ) 0-7Wt%, calcium oxide (CaO) 2-18Wt%, magnesium oxide (MgO) 0-8Wt%, sodium oxide (Na 2 O) and potassium oxide (K 2 A glass material having a total content of 5 to 25 Wt % of O is used.

[0062] However, the first substrate BS1 and the second substrate BS2 may be made of glass materials having compositions other than those mentioned above, and the first substrate BS1 may be made of a plastic material instead of a glass material. By using a plastic material for the first substrate BS1, the substrate can be made lighter than a glass substrate, and the second substrate BS2 made of glass is reinforced by the first substrate BS1 made of plastic, which has the advantage of being less likely to break.

[0063] Therefore, when using a glass material, it is preferable that the thickness of the second base material BS2 and / or the first base material BS1 is about 0.3 mm to 1.0 mm. This also applies to the fifth embodiment described below.

[0064] In the third embodiment, when a plastic material is used for the first substrate BS1, it is preferable to use a plastic material with a film mirror attached to one of the front and back surfaces, or a plastic material with a specular reflective layer 2 deposited on one of the front and back surfaces. Here, the film mirror means, for example, a polyester film that has been processed to have a mirror surface.

[0065] Suitable examples of plastic materials include ABS resin (Acrylonitrile butadiene styrene), which is excellent in rigidity, chemical resistance, and heat resistance; PET resin (Polyethylene terephthalate), which is excellent in transparency, toughness, rigidity, and heat resistance; and Polymethyl methacrylate resin (PMMA), which is particularly excellent in transparency and durability.

[0066] Regardless of whether the first substrate BS1 is made of glass or plastic, the contact surface between the first substrate BS1 and the second substrate BS2 does not necessarily need to be fixed by adhesion or the like. If they are not fixed, the periphery of the two overlapping substrates BS1 and BS2 may be held by an appropriate holding part FIX (see FIG. 3(c)). Note that they may be directly held by a frame or other member, but in any case, when a glass material is used as the first substrate BS1, it is preferable to suppress the total glass thickness t1+t2 to about 2 mm to 5 mm by making the thickness t1 of the first glass substrate BS1 thinner than the thickness t2 of the second glass substrate BS2.

[0067] From the viewpoint of weight reduction, it is also preferable to use a mirror-finished polyester film (film mirror) as the first substrate BS1. Fig. 4 shows this fourth embodiment, in which the first substrate BS1, called a film mirror, is attached to the printed surface of the second substrate BS. To ultimately reduce weight and increase breakage strength, the second substrate BS2 may also be made of a plastic material such as acrylic resin.

[0068] In addition, the first substrate BS1 shown in Fig. 3(a) and the second substrate BS2 shown in Fig. 3(b) do not necessarily need to be superimposed in the state shown in Fig. 3(c), and the stacking direction may be reversed. Fig. 5 shows a fifth embodiment showing such a configuration, which has the advantage that the second substrate BS2 functions as a decorative mirror, while the first substrate BS1 functions as a normal mirror. [Explanation of symbols]

[0069] 1. Glass substrate 2 reflective layer 3 Primer layer 4 White ink layer 5 color ink layers

Claims

1. Silicon dioxide (SiO 2 a polishing step of polishing a surface of a glass substrate having a nominal thickness of 0.3 mm to 8 mm, the surface of the glass substrate containing 60 to 80 wt % of tantalum oxide (Tb) and 2 to 20 wt % of calcium oxide (CaO) as constituent materials, to an arithmetic mean roughness Ra of 0.0007 to 0.0025 μm; A primer step of forming a transparent or translucent primer layer on the surface of the glass substrate after the first step; Prior to the color printing process, a base process is performed in which white ink is partially printed and then cured with ultraviolet light to make the main areas of the design white. A manufacturing method for decorative mirrors, comprising a color printing step of printing color ink on the glass surface or base layer that has been subjected to the primer step and curing the ink with ultraviolet light.

2. The method according to claim 1 , further comprising a back surface step of providing a reflective layer on the back surface of the glass substrate or on another auxiliary substrate.

3. The method according to claim 2 , further comprising an additional step of laminating the auxiliary substrate on the glass substrate that has been subjected to the color printing step, and holding them together.

4. The manufacturing method according to claim 1 , further comprising a polymerization step of fixing a reflective sheet to the front surface side of the glass substrate that has been subjected to the color printing step.

5. 5. The method for manufacturing a decorative mirror according to claim 1, wherein in the color printing step, characters are drawn in the main area.

6. 6. The method for manufacturing a decorative mirror according to claim 1, further comprising a foil forming step of fixing a metal foil at an appropriate position on the glass surface after the color printing step.

7. A method for manufacturing a decorative mirror according to any one of claims 1 to 6, further comprising a final step of printing a glazing material on the glass surface.

8. 4. The method for manufacturing a decorative mirror according to claim 2 or 3, wherein the auxiliary substrate is made of a plastic material or a glass material.

9. A transparent or semi-transparent primer layer printed on a glass substrate polished to an arithmetic mean roughness Ra of 0.0007 to 0.0025 μm; a white ink layer made of an ultraviolet-curable ink partially printed on the primer layer; a color ink layer made of ultraviolet curable ink printed on the entire surface of the white ink layer and on the exposed primer layer; A decorative mirror comprising: The glass substrate is made of silicon dioxide (SiO 2 % of calcium oxide (CaO) and 2 to 20 wt % of calcium oxide (CaO) as constituent materials, and the decorative mirror has a nominal thickness of 0.3 to 8 mm.

10. 10. The decorative mirror according to claim 9, wherein a metal foil is partially thermally transferred onto the color ink layer.

Citation Information

Patent Citations

  • Substrate for inkjet printing, and inkjet printed matter

    JP2005088493A

  • Decorative mirror

    JP2016106674A

  • rear mirror

    JP3126983U

  • decorative mirror

    JP3226584U

  • Primer for inkjet recording

    WO2012081703A1