Light-emitting element

Triarylamine derivatives with wide energy gaps, featuring phenylene or biphenylene-naphthyl structures, address inefficiencies in OLEDs by enhancing blue and green phosphorescence, improving energy and luminous efficiency, and simplifying device fabrication.

JP2024147705AActive Publication Date: 2024-10-16SEMICON ENERGY LAB CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024113987
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2009-02-03
Filing Date
2024-07-17
Publication Date
2024-10-16
Estimated Expiration
2029-05-14

Smart Images

  • Figure 2024147705000061
    Figure 2024147705000061
  • Figure 2024147705000062
    Figure 2024147705000062
  • Figure 2024147705000063
    Figure 2024147705000063
Patent Text Reader

Abstract

To provide a novel triarylamine derivative which has a large energy gap and can be used for a transporting layer or a host material of a light-emitting element.SOLUTION: A triarylamine derivative represented by the general formula (G1) in the figure is provided. In the formula, α represents a naphthyl group, and β represents either hydrogen or a naphthyl group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a triarylamine derivative. The present invention relates to a light-emitting substance, a light-emitting element, and an electronic device using the same. [Background technology]

[0002] Due to its advantages of being thin and lightweight, having high speed response, and low power consumption, organic EL display devices are expected to play an important role as next-generation display devices. The development of display devices using light-emitting elements (organic electroluminescence (EL) elements) that use chemical compounds as light-emitting materials is accelerating. Although there were various obstacles in the development, OLED TVs are now available on the market. Technology has advanced to such an extent.

[0003] In an organic EL element, a light-emitting layer is sandwiched between electrodes, and when a voltage is applied, light is injected from the electrodes. The electrons and holes recombine to excite the luminescent material, and the excited state changes to the ground state. The wavelength of light emitted by a luminescent material is unique to that material, and different By using a variety of organic compounds as luminescent materials, it is possible to emit light of various wavelengths, i.e., various colors. A light emitting element that emits light can be obtained.

[0004] In the case of display devices designed to display images, such as monitors, full-color To reproduce an image, it is necessary to obtain at least three colors of light: red, green, and blue. This involves the use of a light-emitting element that emits light with an emission spectrum in a wide wavelength range and a color filter. A combination method combines a light-emitting element that emits light with a shorter wavelength than the desired color with a color conversion layer. and using a light-emitting element that emits light of the desired wavelength. Among the methods, the last one, which directly obtains the desired color, is the most preferable structure because it has the least energy loss. It can be said that this is a success.

[0005] The aforementioned organic EL televisions that have been released for sale also use this method, but in addition to that In addition to using color filters, the light-emitting element has a microcavity structure, which improves color purity. OLED TVs have many advantages, but as next-generation TVs, It is expected that high quality images will be provided by the users, and in order to meet this expectation, It is essential to obtain a light-emitting element that emits light of the desired color.

[0006] As mentioned earlier, the light emitted by a light-emitting material is unique to that material. The many color purity improvements that are available in LEDs mean that they can emit good color light while still having a long life. It is extremely difficult to obtain a light-emitting element that satisfies other important properties such as low power consumption and low photoluminescence. Furthermore, important properties of light-emitting elements, such as lifetime and power consumption, are determined by the properties of the material that emits light. It does not depend only on the quality of the layers other than the light-emitting layer, the device structure, and the relationship between the light-emitting material and the host. Therefore, in order to assess the maturity of this field, it is necessary to examine many different types of There is no doubt that materials for optical devices will be required. As a result, light-emitting devices with various molecular structures will be developed. Materials for devices have been proposed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication No. 07 / 058127 Brochure Summary of the Invention [Problem to be solved by the invention]

[0008] However, the light-emitting elements that have been developed so far emit light in the range of red to green. Compared to the characteristics of the elements, the characteristics of the light-emitting element that emits blue light are poor, which is a problem. In order to emit blue light, a luminescent material with a large energy gap is required. The host material dispersing the light-emitting material and the transport layer adjacent to the light-emitting region in the light-emitting layer are One reason for this is that the materials used require larger energy gaps.

[0009] A material that does not have a sufficiently large energy gap is placed in the host material or in a layer adjacent to the light-emitting region. If it is used as a material for the light emitting element, the energy of the excitons will be transferred to the material, resulting in the emission of the light emitting element. This causes problems such as a decrease in light efficiency and a decrease in color purity. In one embodiment, the compound has a wide energy gap and is used as a transport layer or a host material in a light-emitting device. The objective of the present invention is to provide a novel triarylamine derivative which can be used in the present invention. [Means for solving the problem]

[0010] The present inventors have developed a material for a light-emitting element having a wide energy gap and an appropriate carrier transport property. As a material that can be suitably used as the starting material, there are The compound is a triarylamine derivative bonded to the central nitrogen through a phenylene group or a biphenylene group. It was possible to achieve this.

[0011] That is, a triarylamine derivative according to one embodiment of the present invention is represented by the following general formula (G1): It is a triarylamine derivative.

[0012] [ka]

[0013] In the formula, Ar is either a substituted or unsubstituted phenyl group or a substituted or unsubstituted biphenyl group. represents a substituted or unsubstituted naphthyl group, and β represents a hydrogen atom or a substituted or unsubstituted naphthyl group. In addition, n and m each independently represent 1 or 2, and R 1 ~R 8 are each independently , hydrogen, an alkyl group having 1 to 6 carbon atoms, or a phenyl group.

[0014] In the formula, Ar specifically represents a group represented by the following structural formulas (Ar-1) to (Ar-4). Examples include:

[0015] [ka]

[0016] In addition, in the formula, α specifically represents a group represented by the following structural formula (α-1) or (α-2). Examples include:

[0017] [ka] In addition, β in the formula specifically represents a group represented by the following structural formulas (β-1) to (β-3). Examples include:

[0018] [ka] Effect of the Invention

[0019] The triarylamine derivative according to one embodiment of the present invention having the above structural formula has a wide range of energy A new trilayer with a -gap that can be used as a transport layer or host material in light-emitting devices That is, the triarylamine derivative of one embodiment of the present invention is A large energy gap, or the energy difference between the ground state and the triplet excited state (see below) In some cases, this is called triplet energy, and light-emitting devices that provide blue fluorescence and green phosphorescence The compound is also excellent as a host material for the light-emitting device to be provided and as a carrier transport material (particularly a hole transport material). Therefore, the triarylamine derivative according to one embodiment of the present invention can be preferably used. The compound is a host material or catalyst for luminescent substances that have emission wavelengths in a wide range of the visible region (blue to red). It can be used as a carrier transport material and can emit light efficiently. During the element formation process, in the case of a light-emitting device consisting of multiple pixels such as red, green, and blue, The type of material or carrier transport material can be standardized, simplifying the process. This is preferable because it allows for good material utilization efficiency. [Brief description of the drawings]

[0020] [Figure 1] 1A to 1C are conceptual diagrams of a light-emitting element (Embodiments 3 to 5). [Diagram 2] FIG. 13 is a conceptual diagram of an organic semiconductor element (sixth embodiment). [Diagram 3] FIG. 13 is a conceptual diagram of an active matrix light emitting device (Embodiment 7). [Figure 4] FIG. 13 is a conceptual diagram of a passive matrix light-emitting device (Embodiment 7). [Diagram 5] FIG. 13 is a diagram showing an electronic device (embodiment 8). [Figure 6] FIG. 13 is a diagram showing an electronic device (embodiment 8). [Figure 7] FIG. 13 is a diagram showing a lighting device (embodiment 8). [Figure 8] FIG. 13 is a diagram showing a lighting device (embodiment 8). [Figure 9] 1H NMR chart of αNBA1BP. [Figure 10] Absorption spectrum of αNBA1BP. [Figure 11] Emission spectrum of αNBA1BP. [Figure 12] 1H NMR chart of αNBB1BP. [Figure 13] Absorption spectrum of αNBB1BP. [Figure 14] Emission spectrum of αNBB1BP. [Figure 15] 13 shows voltage-luminance characteristics of the light-emitting element fabricated in Example 9. [Figure 16] 13 shows the luminance-current efficiency characteristics of the light-emitting element fabricated in Example 9. [Figure 17] 13 shows the luminance-power efficiency characteristics of the light-emitting element fabricated in Example 9. [Figure 18] 13 is an emission spectrum of the light-emitting element fabricated in Example 9. [Figure 19] 13 shows current density-luminance characteristics of the light-emitting element fabricated in Example 10. [Figure 20] 13 shows the luminance-current efficiency characteristics of the light-emitting element fabricated in Example 10. [Figure 21] 13 shows the luminance-power efficiency characteristics of the light-emitting element fabricated in Example 10. [Figure 22] 13 shows voltage-luminance characteristics of the light-emitting element fabricated in Example 10. [Diagram 23] 13 shows voltage-luminance characteristics of the light-emitting element fabricated in Example 11. [Figure 24] 13 shows the luminance-current efficiency characteristics of the light-emitting element fabricated in Example 11. [Diagram 25] 13 shows the luminance-power efficiency characteristics of the light-emitting element fabricated in Example 11. [Figure 26] 13 is an emission spectrum of the light-emitting element fabricated in Example 11. [Figure 27] 13 shows time-normalized luminance characteristics of the light-emitting element fabricated in Example 11. [Figure 28] Wavelength-transmittance characteristics of composite materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The following describes the preferred embodiment of the present invention. However, the present invention can be embodied in many different ways. It is possible to modify the form and details without departing from the spirit and scope of the present invention. It will be readily understood by those skilled in the art that various modifications may be made to the details. It should not be construed as being limited to the description of the embodiments.

[0022] (Embodiment 1) In the embodiment, the triarylamine derivative has a naphthyl group represented by α. Triarylamines attached to the central nitrogen through a phenylene or biphenylene group The triarylamine derivative is a derivative in which the naphthyl group is replaced with a phenylene group or It has one or two structures bonded to the central nitrogen via a biphenylene group. . In the case where the number of naphthyl groups is two, the second naphthyl group is represented by the general formula (G1). In this case, it corresponds to β. The naphthyl group is bonded to a phenylene group or a biphenylene group at a substitution position. The naphthyl group may further have a substituent. It's fine if it is.

[0023] In addition, the triarylamine derivative in the present embodiment has three nitrogen atoms in the center. A phenylene group having a naphthyl group bonded to one or two of the four bonds. or biphenylene group is bonded, but the remaining two or one of the bonds is A phenylene group or a biphenyl group is bonded to the phenylene group or the biphenyl group. The aryl group may further have a substituent.

[0024] The triarylamine derivative of the present embodiment having such a structure has sufficient hole transport properties. A light-emitting device having both excellent optical properties and a wide energy gap and providing blue light emission. It is a substance that can be used very suitably as a material for

[0025] The triarylamine derivative according to the present embodiment can be represented by the following general formula (G1): It can be represented.

[0026] [ka]

[0027] In the formula, Ar represents either a phenyl group or a biphenyl group, α represents a naphthyl group, β represents hydrogen, Each of Ar, α, and β further represents one or more substituents. The substituent may be an alkyl group having 1 to 6 carbon atoms, a phenyl group, or the like. In addition, when the substituent is an alkyl group having 1 to 6 carbon atoms, it is not acyclic alkyl group. Not only a cyclic group but also a cyclic alkyl group may be used.

[0028] In addition, n and m each independently represent 1 or 2. That is, when n and m each represent 1, represents a phenylene group, and when n and m are each 2, represents a biphenylene group. 1 ~R 8 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a phenyl group; Represents R 1 ~R 8 When is an alkyl group having 1 to 6 carbon atoms, not only acyclic alkyl groups but also , and may be a cyclic alkyl group.

[0029] In addition, when n or m is 2, R 1 ~R 8is the phenylene group bonded to the amine The phenylene groups bonded to the phenylene groups may be different. When n or m is 2, the group in the brackets in the above general formula is a biphenyl having two phenylene groups linked together. The phenylene group may have two linked phenylene groups with different substituents. It is decided.

[0030] In the formula, Ar specifically represents a group represented by the following structural formulas (Ar-1) to (Ar-4). Examples include:

[0031] [ka]

[0032] In addition, in the formula, α specifically represents a group represented by the following structural formula (α-1) or (α-2). Examples include:

[0033] [ka]

[0034] In addition, β in the formula specifically represents a group represented by the following structural formulas (β-1) to (β-3). Examples include:

[0035] [ka]

[0036] In addition, in the formula R 1 ~R 8 Specifically, the following structural formulas (R-1) to (R-9) are used: Examples of the groups include [ka]

[0037] Specific examples of the triarylamine derivative represented by the general formula (G1) include those having the following structures: Examples include triarylamine derivatives represented by formulae (1) to (87). However, the present invention is not limited to this.

[0038] [ka]

[0039] [ka]

[0040] [ka]

[0041] [ka]

[0042] [ka]

[0043] [ka]

[0044] [ka]

[0045] [ka]

[0046] [ka]

[0047] [ka]

[0048] [ka]

[0049] [ka]

[0050] [ka]

[0051] [ka]

[0052] [ka]

[0053] The triarylamine derivative according to the present embodiment has a large energy Gap, or the energy difference between the ground state and the triplet excited state (hereafter referred to as the triplet energy The light-emitting element has a blue fluorescence and the light-emitting element has a green phosphorescence. It can be very suitably used as a host material and a carrier transport material (particularly a hole transport material). Therefore, the triarylamine derivative according to the present embodiment can exhibit a wide range of visible light. A host material or carrier transport material for a light-emitting substance having an emission wavelength in the blue to red region In addition, the light emitting device can be formed by using the same material as the light emitting device. In the case of a light-emitting device having multiple pixels such as red, green, and blue, Since the types of materials transported can be standardized, the process can be simplified and material utilization can be improved. This is also preferable because the usage efficiency is good.

[0054] (Embodiment 2) Next, in this embodiment, a method for synthesizing a triarylamine derivative described in Embodiment 1 will be described. The following is shown.

[0055] <Synthesis method 1> In this synthesis method, the following compound M, which is the triarylamine derivative described in embodiment 1, is The compound is synthesized by two methods, namely, <Synthesis Method 1-1> and <Synthesis Method 1-2>. In the synthesis method, the compound M is first synthesized according to the reaction scheme (A-1). In the method (A-1), a dihalogenated aryl compound (compound E2) is used as the starting material to produce a secondary aryl aryl After coupling with amine (compound D1) and coupling with arylboronic acid, The method for synthesizing the compound M is shown below. Compound D1 has a central nitrogen atom represented by Ar. It is a secondary arylamine having an aryl group having a β-group and an aryl group having a β-group.

[0056] [ka]

[0057] In the synthesis method according to the reaction scheme (A-1), a secondary arylamine (compound D1) or Which of the arylboronic acids is coupled first with the aryl halide (compound E2)? This is also fine.

[0058] <Synthesis method 1-1> Here, we use dihalogenated aryl amines (compound E2) and secondary aryl amines (compound D1). is coupled to synthesize a tertiary arylamine, and then the tertiary arylamine is A method for coupling an arylboronic acid is shown.

[0059] A secondary arylamine (compound D1) and an aryl halide (compound E2) are coupled For ring formation, a synthesis method using a metal catalyst in the presence of a base can be applied. This allows the synthesis of compound A2, which is a tertiary arylamine. represents an aryl group represented by Ar, an aryl group having a substituent β, and a halogen atom represented by X. It is a tertiary arylamine in which an aryl group bearing a group is attached to a central nitrogen.

[0060] The above reaction is shown using the Hartwig-Buchwald reaction. As the metal catalyst, a palladium catalyst can be used. As the palladium catalyst, a bis(phenylene) catalyst can be used. (dibenzylideneacetone)palladium(0), palladium(II) acetate, etc. The ligand of the palladium catalyst may be tri(tert-butyl)phosphine or Tri(n-hexyl)phosphine, tricyclohexylphosphine, 1,1-bis( Diphenylphosphino)ferrocene (abbreviation: DPPF) and the like. Examples of substances that can be used include organic bases such as sodium tert-butoxide and Examples of suitable bases include inorganic bases such as potassium carbonate. The preferred solvent is toluene, xylene, benzene, etc. However, the above-mentioned usable catalysts and their ligands, bases, and solvents are It is not limited to.

[0061] In the above reaction, the Ullmann reaction is used. The metal catalyst is a copper catalyst. The copper catalyst may be copper(I) iodide or copper(II) acetate. In addition, examples of substances that can be used as a base include inorganic bases such as potassium carbonate. The above reaction is preferably carried out in a solution. Examples include 1,3-dimethyl-3,4,5,6-tetrahydro-2(1H)-pyrimidino Examples of the solvent include dimethyl ether (DMPU), toluene, xylene, and benzene. The catalyst, base and solvent that can be used are not limited to these.

[0062] In the Ullmann reaction, the desired product can be obtained in a shorter time and with a higher yield when the reaction temperature is 100°C or higher. Therefore, it is preferable to use DMPU or xylene, which has a high boiling point, as a solvent. In addition, since the reaction temperature is more preferably 150°C or higher, it is more preferable to use D Uses MPU.

[0063] The tertiary arylamine having a halogen group (compound A2) obtained as above is The arylboronic acid is coupled with the aryl boronic acid in the presence of a base using a metal catalyst to obtain the desired aryl boronic acid. Compound M, which is a triarylamine derivative as described in embodiment 1, can be synthesized. The boronic acid used has an aryl group represented by α.

[0064] As described above, the arylboron compound (compound A2) is added to the tertiary arylamine having a halogen group. There are various reactions for coupling carboxylic acids. One example is the Suzuki–Miya reaction. The Ura reaction can be mentioned.

[0065] The above reaction is carried out using the Suzuki-Miyaura reaction. Examples of the palladium catalyst include palladium(II) acetate and tetrahydrofuran. Trachys(triphenylphosphine)palladium(0), Bis(triphenylphosphine ) Palladium (II) dichloride, etc. Also, the ligand of the above palladium catalyst is Examples include tri(ortho-tolyl)phosphine, triphenylphosphine, and tricyclophosphine. In addition, examples of substances that can be used as the base include The bases are organic bases such as sodium tert-butoxide and inorganic bases such as potassium carbonate. The reaction is preferably carried out in a solution, and examples of the solvent that can be used include For example, a mixed solvent of toluene and water, a mixed solvent of toluene and alcohol such as ethanol and water, Mixed solvents of xylene and water, mixed solvents of xylene and alcohol such as ethanol and water, Mixtures of alcohols and water, such as benzene and ethanol, and ethylene glycol. Examples of the solvent include a mixture of ethers such as dimethyl ether and water. The catalyst and its ligand, base, and solvent that can be used are not limited to these. In the above scheme, instead of arylboronic acid, organoaluminum or organodiamine can be used. Ru, organozinc, organotin compounds, etc. may also be used.

[0066] <Synthesis method 1-2> In this synthesis method, an aryl dihalide (compound E2) is first reacted with an arylboronic acid to form a carboxylate. The aryl monohalide (compound E1) is then synthesized by coupling with the Coupling of secondary arylamine (compound D1) to aryl halide (compound E1) In this reaction, the arylboronic acid is represented by α. A compound having a aryl group is used.

[0067] To couple an aryl dihalide (compound E2) with an arylboronic acid, The reaction can be carried out using a metal catalyst in the presence of a base. An example of this reaction is the Suzuki-Miyaura reaction. For the case of carrying out the reaction using the Suzuki-Miyaura reaction, see Synthesis Method 1-1. The synthesis can be performed in the same manner as described above. Since the explanation is repetitive, detailed explanation is omitted. Please refer to the description of the Suzuki-Miyaura reaction in Synthesis Method 1-1. Compound E1, which is a monohalogenated aryl having a substituent α, can be synthesized.

[0068] Then, the synthesized monohalogenated aryl (compound E1) and secondary arylamine (compound Compound D1) is coupled with compound D2) in the presence of a base using a metal catalyst to obtain the compound D3. Compound M, which is the triarylamine derivative described in embodiment 1, can be synthesized. There are various types of coupling reactions that can be used in this reaction, but the most representative is the Hartmann coupling reaction. Examples of such reactions include the Hartwig-Buchwald reaction and the Ullmann reaction. The reaction using the Ruth reaction and the Ullmann reaction was described in detail in Synthesis Method 1-1. The reaction can be carried out in the same manner, so the repeated description will be omitted. See the descriptions of the Twick-Buchwald and Ullmann reactions.

[0069] <Synthesis method 2> In this synthesis method, the following compound M, which is the triarylamine derivative described in embodiment 1, is is synthesized according to reaction scheme (A-2). In reaction scheme (A-2), Starting from an amine (compound B3), the terminal aryl group of compound B3 is halogenated. After that, the product coupled with arylboronic acid (compound B1) and the product coupled with halogenated arylboronic acid (compound B2) were The following describes a method for synthesizing compound M by coupling with

[0070] [ka]

[0071] In this reaction scheme (A-2), a compound which is a secondary arylamine having a substituent β is The hydrogen at the end of the aryl group of B3 is first halogenated using a halogenating agent to form the substituent β. The halogenation agent is a secondary arylamine halide (compound B2). , N-bromosuccinimide (abbreviation: NBS) and N-iodosuccinimide (abbreviation: NI S), bromine, iodine, potassium iodide, etc. can be used as halogenating agents. -The synthesis is cheaper if bromides such as bromosuccinimide (abbreviated as NBS) or bromine are used. This is preferable because it allows

[0072] Subsequently, compound B2 is coupled with an arylboronic acid to obtain a compound represented by compound B1. Synthesize secondary arylamines. Secondary arylamines with halogen groups (compound B2) To couple with arylboronic acids, the reaction is carried out in the presence of a base using a metal catalyst. An example of such a reaction is the Suzuki-Miyaura reaction. When using this reaction, the synthesis can be carried out in the same manner as in Synthesis Method 1-1. Detailed description is omitted to avoid repetition. This reaction produces secondary arylamines bearing substituents α and β. A certain compound B1 can be synthesized. The halogenating agent used for halogenation is Iodides such as N-iodosuccinimide (NIS), iodine, and potassium iodide The use of iodine as the halogen substitute makes this coupling reaction shorter. This is preferred because it reacts efficiently in a short time.

[0073] Next, a secondary arylamine, compound B1, and a halogenated arylamine, compound C1, are reacted with each other. The triarylamine derivative described in embodiment 1 is obtained by coupling with an aryl. Compound M can be synthesized. Various coupling reactions can be used in this reaction. Representative examples include the Hartwig-Buchwald reaction and the Ullmann reaction. The Hartwig-Buchwald reaction and Ullmann reaction are described in the synthesis section. As described in detail in Method 1-1, this reaction can be carried out in a similar manner, so the following description is repeated. Regarding the Hartwig-Buchwald reaction and Ullmann reaction in Synthesis Method 1-1, Please refer to the relevant description.

[0074] As described above, compound B1 is a halogenated secondary arylamine (compound B3). and coupling with an arylboronic acid, as shown in reaction scheme (A-3): As shown above, primary arylamines (compound S1) and monohalogenated aryls (compound E1) are There is also a method for synthesizing the compound by coupling with the There are various types of cycloaddition reactions, but the most representative are the Hartwig-Buchwald reaction and the Examples include the Hartwig-Buchwald reaction and the Ullmann reaction. The reaction was described in detail in Synthesis Method 1-1, but this reaction can also be carried out in the same manner. The Wick-Buchwald reaction and Urethane in Synthesis Method 1-1 are See the description of the Mann reaction.

[0075] [ka]

[0076] The synthesis of the above secondary arylamine (compound B1) was carried out using the Hartwig-Buchwald reaction. Using this reaction, a primary arylamine (compound S1) and an aryl halide are reacted in a ratio of 1:1 equivalent. This is preferred because it allows the reaction to proceed in good yield.

[0077] <Synthesis method 3> In this synthesis method, the following compound M, which is the triarylamine derivative described in embodiment 1, is is synthesized according to reaction scheme (A-4). In reaction scheme (A-4), Starting from an amine (compound A3), the terminal aryl group of compound A3 is halogenated. Then, the boronized material (compound A1) and the aryl halide are reacted. The following describes a method for synthesizing the compound M by coupling the following:

[0078] [ka]

[0079] The tertiary arylamine (compound A3) is the triarylamine derivative described in embodiment 1. In the compound M, the moiety represented by α is hydrogen. By halogenating the atomic portion, the portion represented by α in compound M becomes halogen. The aryl halide (compound A2) is synthesized, which is represented by the following halogenation: The halogenation can be carried out using a halogenating agent such as N-bromosuccinimide (abbreviation: N-iodosuccinimide (abbreviation: NIS), bromine, iodine, potassium iodide As a halogenating agent, N-bromosuccinimide (abbreviation: N It is preferable to use a bromide such as bromine or BS, since it can be synthesized more inexpensively.

[0080] The resulting aryl halide (compound A2) is then boronated to give the aryl boronate. The synthesis of the arylboronic acid (compound A1) is carried out by using an organic boronic acid. This can be done by using organolithium and an organoboronic acid. The organic boronic acid may be triborate, methylborate, or the like. Methyl, isopropyl borate, etc. can be used.

[0081] Then, the synthesized arylboronic acid (compound A1) and the aryl group represented by α and halogen The compound according to embodiment 1 can be prepared by coupling an aryl halide having an isopropyl group to the compound. Compound M can be synthesized, which is a triarylamine derivative of the following arylboronic acid: (Compound A1) and a halogenated aryl having an aryl group and a halogen bonded thereto, represented by α, are used as the compound. To couple the compounds, a reaction can be carried out in the presence of a base using a metal catalyst. The Suzuki-Miyaura reaction is an example of such a reaction. Regarding this compound, the synthesis can be carried out in the same manner as described in Synthesis Method 1-1. Please refer to the description of the Suzuki-Miyaura reaction in Synthesis Method 1-1. In addition, N-iodosuccinimide (abbreviation: NI) was used as a halogenating agent for halogenation. S), iodine, potassium iodide, etc., are used as the halogen to be substituted. This selection is preferred because the coupling reaction proceeds more efficiently in a shorter time.

[0082] In the following reaction scheme (A-5), the compound used as the starting material in reaction scheme (A-4) is This reaction scheme (A-5) shows a method for synthesizing compound A3. A method for coupling an amine (compound B3) with an aryl halide (compound C1), Coupling of arylamines (compound D1) with aryl halides (compound E3) Method, two aryl halides (compounds C1 and F1) and primary arylamines ( The method of coupling with compound G1) is shown, but the method of synthesizing compound A3 is similar to these. Not limited.

[0083] [ka]

[0084] The above-mentioned coupling reaction may be carried out using a metal catalyst. There are various such reactions, but the most representative are the Hartwig-Buchwald reaction and the Ur The Hartwig-Buchwald reaction and the Ullmann reaction are examples of such reactions. The reaction was described in detail in Synthesis Method 1-1, but this reaction can also be carried out in the same way. The Wick-Buchwald reaction and Urethane in Synthesis Method 1-1 are Please refer to the description of the Mann reaction. In the method of coupling the compound F1) with a primary arylamine (compound G1), Compound C1 and compound F1 are the same (X may be different) to obtain compound A3 in a higher yield. In this reaction, it is preferable to use the above-mentioned Ullmann reaction to obtain a primary aryl group. It is possible to efficiently react two equivalents of aryl halide with arylamine. I wish.

[0085] <Synthesis method 4> In this synthesis method, the following compound M, which is the triarylamine derivative described in embodiment 1, is The above-mentioned compound is synthesized by two schemes, Reaction Scheme (A-6) and Reaction Scheme (A-7). In reaction scheme (A-6), an aryl halide (compound C1) and a secondary aryl aryl The tertiary arylamine (compound P2) is synthesized by coupling with the tertiary arylamine (compound P3), Of the three aryl groups in the tertiary arylamine (compound P2), two of the aryl groups The terminals are halogenated to synthesize a dihalide of a tertiary arylamine (compound P1), Thereafter, the compound P1 is coupled with an arylboronic acid to give A method for synthesizing M is shown below.

[0086] [ka]

[0087] First, an aryl halide (compound C1) and a secondary arylamine (compound P3) were mixed together. The tertiary arylamine (compound P2) is synthesized by pulling the arylamine. Compound P2 is a compound M which is a triarylamine derivative as described in embodiment 1. The compound is one in which both α and β are hydrogen. The coupling reaction is carried out using a metal catalyst. Coupling reactions can be used. There are various types of such reactions, but the most representative is Hartwig-Buchwald reaction and Ullmann reaction are examples. The Hubert reaction and the Ullmann reaction were described in detail in Synthesis Method 1-1. The reaction can be carried out in the same manner, so the repeated description will be omitted. See the descriptions of the Wick-Buchwald and Ullmann reactions.

[0088] Next, compound M, which is a triarylamine derivative of compound P2 described in embodiment 1, By halogenating the hydrogens corresponding to the α and β positions in The halogenation reaction is carried out using a halogenating agent. The halogenating agent is N-bromosuccinimide (abbreviation: NBS) or N- Use iodosuccinimide (abbreviation: NIS), bromine, iodine, potassium iodide, etc. Halogenating agents include N-bromosuccinimide (abbreviation: NBS) and bromine. It is preferable to use a bromide since it can be synthesized more inexpensively. It is preferable to use 2 equivalents or more relative to 2, preferably 2 equivalents (normality).

[0089] Then, a dihalogenated aryl compound (compound P1) and an aryl group represented by α are reacted with each other. The arylboronic acid represented by β is coupled with an arylboronic acid having an aryl group. By this, compound M, which is the triarylamine derivative described in embodiment 1, is synthesized. Arylboronic acid and aryl dihalide (compound P1) can be coupled to To achieve this, a reaction can be carried out using a metal catalyst in the presence of a base. The Suzuki-Miyaura reaction can be used as an example. The synthesis can be carried out in the same manner as described in Synthesis Method 1-1. Detailed description is omitted. Please refer to the description of the Suzuki-Miyaura reaction in Synthesis Method 1-1. As a halogenating agent, N-iodosuccinimide (abbreviation: NIS) Iodine, potassium iodide, or other iodides are used, and iodine is selected as the halogen to be substituted. This is preferable because the coupling reaction can be carried out efficiently in a short time. In this reaction, an arylboronic acid having a group represented by α as an aryl group and When the aryl group is the same as the arylboronic acid having a group represented by β, the reaction can be performed in good yield. This is preferable because compound M can be obtained.

[0090] In reaction scheme (A-6), a halogenation of a tertiary arylamine (compound P2) The coupling was carried out simultaneously on two aryl groups, but as shown in the reaction scheme (A-7 ) halogenation of tertiary arylamine (compound P2) with respect to two aryl groups and A method for sequential coupling with arylboronic acids is shown.

[0091] [ka]

[0092] First, one aryl group of the tertiary arylamine (compound P2) is converted to aryl by a halogenating agent. The halogenation agent is then halogenated to synthesize an aryl halide (compound Q3). , N-bromosuccinimide (abbreviation: NBS) and N-iodosuccinimide (abbreviation: NI S), bromine, iodine, potassium iodide, etc. can be used as halogenating agents. -The synthesis is cheaper if bromides such as bromosuccinimide (abbreviated as NBS) or bromine are used. It is preferable to use 1 equivalent (normality) of the halogenating agent relative to compound P2. This is preferable because it improves the yield.

[0093] Next, an aryl halide (compound Q3) and a aryl group having α or β are By coupling with an arylboronic acid (α in Reaction Scheme A-7), Tertiary arylamines having α or β (α in Reaction Scheme A-7) introduced therein (Compound Q2) The following is synthesized by coupling an aryl halide (compound Q3) with an arylboronic acid: To achieve this, the reaction can be carried out in the presence of a base using a metal catalyst. The Suzuki-Miyaura reaction can be used as an example. The synthesis can be carried out in the same manner as described in Synthesis Method 1-1. Please refer to the description of the Suzuki-Miyaura reaction in Synthesis Method 1-1. The halogenating agent used for halogenation is N-iodosuccinimide (NIS), Iodine, potassium iodide, or other iodides are used, and iodine is selected as the halogen to be substituted. This is preferable because the coupling reaction can be carried out more efficiently in a shorter time.

[0094] The resulting tertiary arylamine, compound Q2, is then halogenated to give a halogenated arylamine. The halogenation can be carried out using a halogenating agent. The genating agents include N-bromosuccinimide (abbreviation: NBS) and N-iodosuccinimide. Nitrogen (abbreviation: NIS), bromine, iodine, potassium iodide, etc. can be used. When N-bromosuccinimide (abbreviation: NBS) or bromides such as bromine are used as the silylating agent, It is preferable to use 1 equivalent of the halogenating agent relative to compound Q2 because it can be synthesized more inexpensively. The use of (normality) is preferred since it improves the yield.

[0095] Finally, the aryl halide (compound Q1) and the aryl group represented by α or β are By coupling with an arylboronic acid (β in Reaction Scheme A-7), and a compound which is the triarylamine derivative according to embodiment 1, in which α and β are introduced. M can be synthesized by reacting an aryl halide (compound Q1) with an arylboronic acid. To couple the above, the reaction can be carried out in the presence of a base using a metal catalyst. An example is the Suzuki-Miyaura reaction. In this case, the synthesis can be carried out in the same manner as described in Synthesis Method 1-1. Therefore, detailed description is omitted. Please refer to the description of the Suzuki-Miyaura reaction in Synthesis Method 1-1. In addition, N-iodosuccinimide (abbreviation) is used as a halogenating agent. Iodine, potassium iodide, and other iodides are used, and iodine is used as the substitute halogen. The choice of iodine is favored because this coupling reaction is more efficient and takes less time. It is nice.

[0096] <Synthesis method 5> In this synthesis method, the following compound M, which is the triarylamine derivative described in embodiment 1, is is synthesized according to reaction scheme (A-8). In reaction scheme (A-8), An amine (compound R1) is combined with an aryl halide (compound E1) with an α-terminated terminal and a β-linked aryl halide (compound F1) are simultaneously coupled to the compound A method for synthesizing compound M is shown below.

[0097] [ka]

[0098] In this reaction, a compound R1, which is a primary arylamine having an aryl group represented by Ar, Compound E1 is an aryl halide having an aryl group represented by α, and compound E2 is an aryl halide having an aryl group represented by β. and a compound F1, which is an aryl halide having a substituent, are simultaneously reacted with the compound F2 in the presence of a metal catalyst. By coupling, the triarylamine derivative described in embodiment 1 is obtained. Compound M is synthesized. There are various such reactions, but the most representative is the Hartwig-Buchbacher reaction. The Hartwig-Buchwald reaction and the Ullmann reaction are The reaction using the cycloaddition reaction was described in detail in Synthesis Method 1-1, but this reaction can also be carried out in the same manner. Therefore, the repetitive description will be omitted. Please refer to the description of the Ullmann reaction and the Ullmann reaction. (Compound E1 and Compound F1) and a primary arylamine (Compound R1) are coupled. In this method, it is more efficient if compound E1 and compound F1 are the same (X may be different). This is preferable because it allows compound M to be obtained efficiently. In addition, in this reaction, the above-mentioned Ullmann reaction is used. The reaction of two equivalents of aryl halide with primary arylamine is more efficient when This is possible and preferable.

[0099] In the reaction schemes (A-1) to (A-8), X represents a halogen group. and it is a chloro group, a bromo group or an iodo group, preferably a bromo group or an iodo group. Ar is a phenyl group or a biphenyl group, α is a naphthyl group, and β is a hydrogen or a naphthyl group. R is a butyl group. 1 ~R 8 each independently represents hydrogen or an alkyl group having 1 to 6 carbon atoms or a phenyl group, and n and m are each independently a value of 1 or 2. Although many reaction schemes have been given as examples, the triazine compound described in the first embodiment can be used as well. Compound M, which is an arylamine derivative, may be synthesized by any other synthesis method. stomach.

[0100] (Embodiment 3) FIG. 1 shows one mode of a light-emitting element using the triarylamine derivative described in Embodiment 1. 1(A) is shown below.

[0101] The light-emitting element in this embodiment has a plurality of layers between a pair of electrodes. The light-emitting element includes a first electrode 102, a second electrode 104, and a first electrode 102 and a second electrode 104. The first electrode 104 is disposed between the first electrode 104 and the EL layer 103. The first electrode 102 functions as an anode and the second electrode 104 functions as a cathode. In other words, the first electrode 102 has a higher potential than the second electrode 104. When a voltage is applied between the first electrode 102 and the second electrode 104, light is emitted. It is structured as follows.

[0102] The substrate 101 is used as a support for the light emitting device. The substrate 101 is, for example, glass. In addition, a material that functions as a support for the light-emitting element may be used. Anything other than these may be used as long as it is suitable.

[0103] The first electrode 102 is made of a metal or alloy having a large work function (specifically, 4.0 eV or more). It is preferable to use gold, a conductive compound, or a mixture thereof. For example, indium tin oxide (ITO), silicon Indium oxide-tin oxide and indium oxide-zinc oxide containing silicon oxide or silicon oxide (IZO: Indium Zinc Oxide), containing tungsten oxide and zinc oxide These conductive metal oxide films are The film is usually formed by sputtering, but it may also be formed by applying the sol-gel method. For example, indium oxide-zinc oxide (IZO) is a material that contains 1 to 20 wt% of zinc oxide relative to indium oxide. It can be formed by a sputtering method using a target containing zinc oxide. Indium oxide containing tungsten oxide and zinc oxide (IWZO) is It contains 0.5-5wt% tungsten oxide and 0.1-1wt% zinc oxide. It can be formed by sputtering using a gold (Au) target. , Platinum (Pt), Nickel (Ni), Tungsten (W), Chromium (Cr), Molybdenum (Mo), iron (Fe), cobalt (Co), copper (Cu), palladium (Pd), or gold Examples of the nitride include nitrides of metal materials (for example, titanium nitride).

[0104] The stacked structure of the EL layer 103 is not particularly limited, and may be a layer including a substance having a high electron transporting property. or a layer containing a substance with high hole transporting properties, a layer containing a substance with high electron injecting properties, a layer including a bipolar substance (a substance having high electron and hole transport properties), The layers including the triarylamine derivative of one embodiment of the present invention described in Embodiment 1 are appropriately combined. For example, a hole injection layer, a hole transport layer, a light emitting layer, an electron transport layer, an electron injection layer, In this embodiment, the EL layer 103 is A hole injection layer 111, a hole transport layer 112, and a light emitting layer 11 are laminated in this order on the first electrode 102. 3. A structure having an electron transport layer 114 is shown. The materials for forming each layer are detailed below. Physically demonstrate.

[0105] The hole injection layer 111 is a layer containing a substance with high hole injection properties. Use of tungsten oxide, manganese oxide, etc. In addition, phthalocyanine (abbreviation: H2Pc) and copper phthalocyanine (CuPC) can be used. Phthalocyanine compounds such as 4,4'-bis[N-(4-diphenylaminophenyl )-N-phenylamino]biphenyl (abbreviation: DPAB), 4,4'-bis(N-{4- [N-(3-methylphenyl)-N-phenylamino]phenyl}-N-phenylamino Aromatic amine compounds such as poly(3,4-ethyl)biphenyl (abbreviation: DNTPD) or poly(3,4-ethyl) PEDOT / PSS) The hole injection layer 111 can also be formed from a polymer such as The triarylamine derivatives described in the above can also be used as hole injection materials.

[0106] In addition, the hole-injecting layer 111 may be formed by adding an acceptor substance to a substance having a high hole-transporting property. A composite material in which a substance having a high hole transporting property is an acceptor substance can also be used. By using a material containing the compound, it is possible to select a material for forming the electrode regardless of the work function of the electrode. In other words, not only a material with a large work function but also a material with a specific Materials with small charge functions can be used. 8-Tetracyano-2,3,5,6-tetrafluoroquinodimethane (abbreviation: F4-TCN Q), chloranil, etc. Also, transition metal oxides can be mentioned. Further, oxides of metals belonging to groups 4 to 8 of the periodic table can be mentioned. Specifically, vanadium oxide, niobium oxide, tantalum oxide, chromium oxide, molybdenum oxide, Libdenum oxide, tungsten oxide, manganese oxide, and rhenium oxide are preferred because of their high electron-accepting properties. Among them, molybdenum oxide is particularly stable in the air, has low hygroscopicity, and is easy to handle. Therefore, it is preferable.

[0107] As a substance having a high hole transporting property used in the composite material, an aromatic amine compound, carbazole, Derivatives, aromatic hydrocarbons, polymer compounds (oligomers, dendrimers, polymers, etc.) Various organic compounds can be used. In particular, it is preferable that the organic compound has a high hole transporting property. -6 cm 2 / Vs However, it is preferable that the material has a hole mobility of 100 or more. Other materials may be used as long as they have high conductivity. Specific examples of organic compounds that can be used as the substance with high transport properties are listed below.

[0108] For example, the aromatic amine compound is N,N'-di(p-tolyl)-N,N'-diphenyl Phenyl-p-phenylenediamine (DTDPPA), 4,4'-bis[N-(4- Diphenylaminophenyl)-N-phenylamino]biphenyl (abbreviation: DPAB), 4 ,4'-Bis(N-{4-[N-(3-methylphenyl)-N-phenylamino]phenyl 1,3,5-tris[N -(4-diphenylaminophenyl)-N-phenylamino]benzene (abbreviation: DPA3 B) and the like can be mentioned.

[0109] Specific examples of carbazole derivatives that can be used in composite materials include 3-[N- (9-Phenylcarbazol-3-yl)-N-phenylamino]-9-phenylcarbazol 3,6-bis[N-(9-phenylcarbazole-3 -yl)-N-phenylamino]-9-phenylcarbazole (abbreviation: PCzPCA2) , 3-[N-(1-naphthyl)-N-(9-phenylcarbazol-3-yl)amino] -9-phenylcarbazole (abbreviation: PCzPCN1), etc.

[0110] Another carbazole derivative that can be used in composite materials is 4,4'-dicarbazole. (N-carbazolyl)biphenyl (abbreviation: CBP), 1,3,5-tris[4-(N-carbazolyl) 9-[4-(10-phenyl-9 -anthryl)phenyl]-9H-carbazole (abbreviation: CzPA), 1,4-bis[4 -(N-carbazolyl)phenyl]-2,3,5,6-tetraphenylbenzene and the like. It is possible.

[0111] In addition, examples of aromatic hydrocarbons that can be used in the composite material include 2-tert -Butyl-9,10-di(2-naphthyl)anthracene (abbreviation: t-BuDNA), 2- tert-Butyl-9,10-di(1-naphthyl)anthracene, 9,10-bis(3, 5-Diphenylphenyl)anthracene (abbreviation: DPPA), 2-tert-butyl-9 ,10-Bis(4-phenylphenyl)anthracene (abbreviation: t-BuDBA), 9,1 0-Di(2-naphthyl)anthracene (abbreviation: DNA), 9,10-diphenylanthracene 2-tert-butylanthracene (abbreviation: DPAnth), 2-tert-butylanthracene (abbreviation: t-BuAn th), 9,10-bis(4-methyl-1-naphthyl)anthracene (abbreviation: DMNA) , 2-tert-butyl-9,10-bis[2-(1-naphthyl)phenyl]anthracene 9,10-bis[2-(1-naphthyl)phenyl]anthracene, 2,3,6,7- Tetramethyl-9,10-di(1-naphthyl)anthracene, 2,3,6,7-tetramethyl 9,10-di(2-naphthyl)anthracene, 9,9'-bianthryl, 10,1 0'-Diphenyl-9,9'-bianthryl, 10,10'-bis(2-phenylphenyl) 10,10'-bis[(2,3,4,5,6-pentafluorophenyl) phenyl)phenyl]-9,9'-bianthryl, anthracene, tetracene, rubrene, perylene, 2,5,8,11-tetra(tert-butyl)perylene, etc. In addition, pentacene, coronene, etc. can also be used. is 1×10 -6 cm 2 In addition to having a hole mobility of 1000 nm or more, the aromatic hydrocarbon When forming a film by vapor deposition, it is important to select a method that is suitable for the deposition property during deposition and the film quality after deposition. The ring more preferably has 14 to 42 carbon atoms.

[0112] The aromatic hydrocarbon that can be used in the composite material may have a vinyl skeleton. Examples of aromatic hydrocarbons having a vinyl group include 4,4'-bis(2,2- Diphenylvinyl)biphenyl (abbreviation: DPVBi), 9,10-bis[4-(2,2- diphenylvinyl)phenyl]anthracene (abbreviation: DPVPA), and the like.

[0113] In addition, poly(N-vinylcarbazole) (abbreviation: PVK) and poly(4-vinyltriphenylphosphine) nylamine) (abbreviation: PVTPA), poly[N-(4-{N'-[4-(4-diphenyl Amino)phenyl]phenyl-N'-phenylamino}phenyl)methacrylamide]( Abbreviation: PTPDMA) Poly[N,N'-bis(4-butylphenyl)-N,N'-bis( It is also possible to use polymer compounds such as poly(phenyl)benzidine (abbreviation: Poly-TPD). Cut.

[0114] The triarylamine derivative described in the first embodiment is also an organic compound in a composite material. It can be used as:

[0115] The hole transport layer 112 is a layer containing a substance with a high hole transport property. The triarylamine derivative described in the first embodiment is used as the transport layer.

[0116] In addition, the hole injection layer 111 and the hole transport layer 112 are both made of the compound of the present invention described in the first embodiment. In this case, the device can be easily fabricated. This is convenient and improves the efficiency of material utilization. Since the energy diagrams of the hole injection layer 111 and the hole injection layer 112 are the same or close to each other, This can facilitate the movement of carriers to and from the transport layer 112 .

[0117] The light-emitting layer 113 is a layer containing a light-emitting substance. The light-emitting layer 113 is a film of a light-emitting substance alone. The light-emitting element may be constructed as a film having a light-emitting substance dispersed in a host material.

[0118] In the light-emitting layer 113, the material that can be used as the light-emitting substance is not particularly limited. The light emitted by these materials may be fluorescent or phosphorescent. Examples of such measures include the following:

[0119] The fluorescent material is N,N'-bis[4-(9H-carbazol-9-yl)fluorene]. [phenyl]-N,N'-diphenylstilbene-4,4'-diamine (abbreviation: YGA2S) , 4-(9H-carbazol-9-yl)-4'-(10-phenyl-9-anthryl) In addition to triphenylamine (abbreviation: YGAPA), 4-(9 H-Carbazol-9-yl)-4'-(9,10-diphenyl-2-anthryl)trimethyl Phenylamine (abbreviation: 2YGAPPA), N,9-diphenyl-N-[4-(10-phenyl PCA PA), Perylene, 2,5,8,11-tetra-tert-butylperylene (abbreviation: TB P), 4-(10-phenyl-9-anthryl)-4'-(9-phenyl-9H-carba N,N''-(2-t-phenyl-3-yl)triphenylamine (abbreviation: PCBAPA), ert-Butylanthracene-9,10-diyldi-4,1-phenylene)bis[N,N ',N'-triphenyl-1,4-phenylenediamine] (abbreviation: DPABPA), N, 9-Diphenyl-N-[4-(9,10-diphenyl-2-anthryl)phenyl]-9 H-Carbazole-3-amine (abbreviation: 2PCAPPA), N-[4-(9,10-difluorophenyl) (phenyl-2-anthryl)phenyl]-N,N',N'-triphenyl-1,4-phenyl Diamine (abbreviation: 2DPAPPA), N,N,N',N',N'',N'',N'' ',N'''-Octaphenyldibenzo[g,p]chrysene-2,7,10,15-tetrahydrofuran DBC1, Coumarin 30, N-(9,10-diphenyl-2-anthracene) (aryl)-N,9-diphenyl-9H-carbazol-3-amine (abbreviation: 2PCAPA) , N-[9,10-bis(1,1'-biphenyl-2-yl)-2-anthryl]-N, 9-Diphenyl-9H-carbazol-3-amine (abbreviation: 2PCABPhA), N-( 9,10-diphenyl-2-anthryl)-N,N',N'-triphenyl-1,4-f Phenylenediamine (abbreviation: 2DPAPA), N-[9,10-bis(1,1'-biphenyl -2-yl)-2-anthryl]-N,N',N'-triphenyl-1,4-phenyl 2DPABPhA, 9,10-bis(1,1'-biphenyl-2- 4-(9H-carbazol-9-yl)phenyl)-N-phenyl ant Helical-2-amine (abbreviation: 2YGABPhA), N,N,9-triphenylanthracene DPhAPhA, Coumarin 545T, N,N'-Diphenyl Nacridone (abbreviation: DPQd), rubrene, 5,12-bis(1,1'-biphenyl-4 -yl)-6,11-diphenyltetracene (abbreviation: BPT), 2-(2-{2-[4- (Dimethylamino)phenyl]ethenyl}-6-methyl-4H-pyran-4-ylidene) Propanedinitrile (abbreviation: DCM1), 2-{2-methyl-6-[2-(2,3,6, 7-Tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4 H-pyran-4-ylidene}propanedinitrile (abbreviation: DCM2), N,N,N',N '-Tetrakis(4-methylphenyl)tetracene-5,11-diamine (abbreviation: pm PhTD), 7,13-diphenyl-N,N,N',N'-tetrakis(4-methylphenyl) Acenaphtho[1,2-a]fluoranthene-3,10-diamine (abbreviation: p-mP hAFD), 2-{2-isopropyl-6-[2-(1,1,7,7-tetramethyl-2 ,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethy nyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCJTI), 2- {2-tert-butyl-6-[2-(1,1,7,7-tetramethyl-2,3,6,7 -Tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl]-4H -pyran-4-ylidene}propanedinitrile (abbreviation: DCJTB), 2-(2,6-biphenyl S(2-[4-(dimethylamino)phenyl]ethenyl)-4H-pyran-4-ylidene )propanedinitrile (abbreviation: BisDCM), 2-{2,6-bis[2-(8-methoxy 1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H-benzo[b] Zo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene}propane dinitrile (abbreviation: BisDCJTM), etc.

[0120] Phosphorescent materials include bis[2-(4',6'-difluorophenyl)pyridinate] -N,C 2' ]Iridium(III) tetrakis(1-pyrazolyl)borate (abbreviation: FI In addition to r6), bis[2-(4',6' -Difluorophenyl)pyridinato-N,C 2' ]Iridium(III) picolinate (abbreviation Name: FIrpic), bis[2-(3',5'-bistrifluoromethylphenyl)pyridine Ginat-N,C 2' ]Iridium(III) picolinate (abbreviation: Ir(CF3ppy)2( pic)), bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2' ]stomach Lithium(III) acetylacetonate (abbreviation: FIracac), emission wavelength is 500 nm (green emission) or higher, tris(2-phenylpyridinato)iridium(III) (abbreviation : Ir(ppy)3), bis(2-phenylpyridinato)iridium(III) acetyl Acetonate (abbreviation: Ir(ppy)2(acac)), tris(acetylacetonate) (Monophenanthroline)terbium(III) (abbreviation: Tb(acac)3(Phen )), bis(benzo[h]quinolinato)iridium(III) acetylacetonate (abbreviation Name: Ir(bzq)2(acac)), bis(2,4-diphenyl-1,3-oxazola To-N,C 2') Iridium(III) acetylacetonate (abbreviation: Ir(dpo)2( acac)), bis[2-(4'-perfluorophenylphenyl)pyridinato]irid Ir(III) acetylacetonate (abbreviation: Ir(p-PF-ph)2(acac)) , Bis(2-phenylbenzothiazolato-N,C 2' ) Iridium(III) acetylacetone Tonat (abbreviation: Ir(bt)2(acac)), bis[2-(2'-benzo[4,5- α]Thienyl)pyridinato-N,C 3' ]Iridium(III) acetylacetonate (abbreviation Name: Ir(btp)2(acac)), bis(1-phenylisoquinolinato-N,C 2' ) Iridium(III) acetylacetonate (abbreviation: Ir(piq)2(acac)), (Acetylacetonato)bis[2,3-bis(4-fluorophenyl)quinoxalinato] Iridium(III) (abbreviation: Ir(Fdpq)2(acac)), (acetylacetonate Bis(2,3,5-triphenylpyrazinate)iridium(III) (abbreviation: Ir( tppr)2(acac)), 2,3,7,8,12,13,17,18-octaethyl -21H,23H-Porphyrin platinum(II) (abbreviation: PtOEP), tris(1,3- Diphenyl-1,3-propanedionato)(monophenanthroline)europium(II) I) (abbreviation: Eu(DBM)3(Phen)), tris[1-(2-thenoyl)-3,3 ,3-Trifluoroacetonato](monophenanthroline)europium(III)(abbreviation Eu(TTA)3(Phen) and others.

[0121] The triarylamine derivative according to the first embodiment has an energy gap or triplet energy. Because of its high energy, it is very suitable as a material for forming a hole transport layer that is provided in contact with a light-emitting layer. Among the above, fluorescent light with an emission wavelength of 450 nm or more (blue emission) can be used. Photoluminescent substances, with emission wavelengths of 470 nm or more, preferably 500 nm or more (green emission) The use of the phosphorescent material is preferable because it is difficult for the luminous efficiency and color purity to decrease. do.

[0122] The material that can be used as the host material is not particularly limited, but examples thereof include For example, tris(8-quinolinolato)aluminum(III) (abbreviation: Alq), tris( 4-Methyl-8-quinolinolato)aluminum(III) (abbreviation: Almq3), bis( 10-Hydroxybenzo[h]quinolinato)beryllium(II) (abbreviation: BeBq2), Bis(2-methyl-8-quinolinolato)(4-phenylphenolato)aluminum(II) I) (abbreviation: BAlq), bis(8-quinolinolato)zinc(II) (abbreviation: Znq), Bis[2-(2-benzoxazolyl)phenolato]zinc(II) (abbreviation: ZnPBO), Bis[2-(2-benzothiazolyl)phenolato]zinc(II) (abbreviation: ZnBTZ) Which metal complex, 2-(4-biphenylyl)-5-(4-tert-butylphenyl)-1 ,3,4-Oxadiazole (abbreviation: PBD), 1,3-bis[5-(p-tert-butyl) OXD-1,3,4-oxadiazol-2-yl]benzene 7), 3-(4-biphenylyl)-4-phenyl-5-(4-tert-butylphenyl) )-1,2,4-triazole (abbreviation: TAZ), 2,2',2''-(1,3,5-benzyl 1-phenyl-1H-benzimidazole (TPBI) ), Bathophenanthroline (abbreviation: BPhen), Bathocuproine (abbreviation: BCP), 9-[4-(5-phenyl-1,3,4-oxadiazol-2-yl)phenyl]-9 Heterocyclic compounds such as H-carbazole (abbreviation: CO11), 4,4'-bis[N-(1- naphthyl)-N-phenylamino]biphenyl (abbreviation: NPB or α-NPD), N, N'-Bis(3-methylphenyl)-N,N'-diphenyl-[1,1'-biphenyl] -4,4'-diamine (abbreviation: TPD), 4,4'-bis[N-(spiro-9,9'-bi Fluoren-2-yl)-N-phenylamino]-1,1'-biphenyl (abbreviation: BSP B) and other aromatic amine compounds. Condensation of benzo[g,p]chrysene derivatives, pyrene derivatives, chrysene derivatives, etc. Polycyclic aromatic compounds are examples of this. Specifically, 9,10-diphenylanthracene (abbreviation :DPAnth), N,N-diphenyl-9-[4-(10-phenyl-9-anthryl )phenyl]-9H-carbazol-3-amine (abbreviation: CzA1PA), 4-(10- Phenyl-9-anthryl)triphenylamine (abbreviation: DPhPA), 4-(9H-ca 4'-(10-phenyl-9-anthryl)-4'-(10-phenyl-9-anthryl)triphenylamine YGAPA, N,9-diphenyl-N-[4-(10-phenyl-9-an N,9-tolyl)phenyl]-9H-carbazol-3-amine (abbreviation: PCAPA) Diphenyl-N-{4-[4-(10-phenyl-9-anthryl)phenyl]phenyl }-9H-carbazol-3-amine (abbreviation: PCAPBA), N,9-diphenyl-N -(9,10-diphenyl-2-anthryl)-9H-carbazol-3-amine (abbreviation :2PCAPA), 6,12-dimethoxy-5,11-diphenylchrysene, N,N,N ',N',N'',N'',N''',N'''-Octaphenyldibenzo[g,p]c Ricen-2,7,10,15-tetraamine (abbreviation: DBC1), 9-[4-(10-fu CzPA, 3,6 -Diphenyl-9-[4-(10-phenyl-9-anthryl)phenyl]-9H-cal DPCzPA (abbreviation: DPCzPA), 9,10-bis(3,5-diphenylphenyl)an DPPA, 9,10-di(2-naphthyl)anthracene (DN A), 2-tert-butyl-9,10-di(2-naphthyl)anthracene (abbreviation: t- BuDNA), 9,9'-bianthryl (abbreviation: BANT), 9,9'-(stilbene- 3,3'-diyl)diphenanthrene (abbreviation: DPNS), 9,9'-(stilbene-4 ,4'-diyl)diphenanthrene (abbreviation: DPNS2), 3,3',3''-(benzene Examples of such compounds include tripyrene-1,3,5-triyl) tripyrene (abbreviation: TPB3). Among known materials, we have selected materials with an energy gap larger than that of the luminescent material. In addition, when the light-emitting substance is a phosphorescent substance, the host material The material is determined by the triplet energy (energy difference between the ground state and the triplet excited state) of the luminescent material. It is only necessary to select a substance having a triplet energy that is the largest possible.

[0123] The light-emitting layer 113 may be formed of two or more layers. When the light-emitting layer 113 is formed by laminating the first light-emitting layer and the second light-emitting layer in this order from the hole transport layer side, A substance having hole transport properties is used as the host material for the first light-emitting layer, and a substance having electron transport properties is used as the second light-emitting layer. Any material having a transport property can be used.

[0124] When the light-emitting layer having the above structure is made of multiple materials, it can be formed by vacuum deposition. or a mixed solution thereof, by the inkjet method, spin coating method, or dip coating method. It can be prepared by using a method such as a dipping method.

[0125] The electron transport layer 114 is a layer containing a substance having a high electron transporting property. Aluminum (Alq), tris(4-methyl-8-quinolinolato) Aluminum (abbreviation: Almq3), bis(10-hydroxybenzo[h]quinolinato) Beryllium (abbreviation: BeBq2), bis(2-methyl-8-quinolinolato)(4-phenyl Quinoline skeleton such as (aluminum quinolate) aluminum (abbreviation: BAlq) or benzoquinone skeleton The layer is made of a metal complex having a bis[2-(2-hydroxyphenyl)-2-pyridine skeleton. phenyl)benzoxazolato]zinc (abbreviation: Zn(BOX)2), bis[2-(2-phenyl oxazo[1,2-hydroxyphenyl]benzothiazolato[1,2-hydroxyphenyl]zinc (abbreviation: Zn(BTZ)2) Metal complexes having aryl or thiazole ligands can also be used. In addition to the complex, 2-(4-biphenylyl)-5-(4-tert-butylphenyl)-1 ,3,4-Oxadiazole (abbreviation: PBD) and 1,3-bis[5-(p-tert- butylphenyl)-1,3,4-oxadiazol-2-yl]benzene (abbreviation: OXD -7), 3-(4-biphenylyl)-4-phenyl-5-(4-tert-butylphenyl) 1,2,4-triazole (abbreviation: TAZ), bathophenanthroline (abbreviation: BP hen), vasocuproine (abbreviation: BCP), etc. can also be used. The material is mainly 10 -6 cm 2 / Vs or more. Any other substance than those mentioned above may be used for the electron transport layer as long as it has a high electron transporting property. stomach.

[0126] The electron transport layer may be a single layer or a laminate of two or more layers of the above-mentioned materials. It may also be possible to use the same method.

[0127] In addition, a layer for controlling the movement of electron carriers may be provided between the electron transport layer and the light emitting layer. This is achieved by adding a small amount of a substance with high electron trapping properties to a material with high electron transport properties as described above. A layer that adjusts the carrier balance by suppressing the movement of electron carriers. This type of structure prevents light from being emitted by electrons passing through the light-emitting layer. This is highly effective in suppressing problems that arise (such as a decrease in element life).

[0128] In addition, an electron injection layer is provided between the electron transport layer and the second electrode 104 and in contact with the second electrode 104. The electron injection layer may be formed using lithium fluoride (LiF), cesium fluoride (C sF), calcium fluoride (CaF2), or other alkali metals or alkaline earth metals For example, the compound can be used in the layer made of a substance having an electron transport property. In particular, For example, magnesium (Mg) may be contained in Alq. As the injection layer, an alkali metal or alkaline earth metal is added to a layer made of a substance having an electron transporting property. By using a material containing the metal, electron injection from the second electrode 104 can be performed efficiently. This is more preferable because

[0129] The material for forming the second electrode 104 is a material having a small work function (specifically, 3.8 eV Metals, alloys, electrically conductive compounds, and mixtures thereof can be used. Examples of such cathode materials include elements belonging to Groups 1 and 2 of the Periodic Table. , i.e., alkali metals such as lithium (Li) and cesium (Cs), and magnesium Alkaline earth metals such as Mg, Ca, and Sr, Alloys containing these elements (MgAg, AlLi), europium (Eu), ytterbium (Y b) rare earth metals and alloys containing these. However, the second electrode By providing an electron injection layer between the electron transport layer and the junction 104, the electron transport layer can be formed regardless of the magnitude of the work function. First, indium oxide-silicon oxide containing Al, Ag, ITO, silicon or silicon oxide. Various conductive materials such as zinc can be used as the second electrode 104. The film can be formed by sputtering, inkjet printing, spin coating, etc. It is Noh.

[0130] The EL layer 103 can be formed by a variety of methods, including a dry method and a wet method. For example, a vacuum deposition method, an inkjet method, a spin coating method, or the like can be used. Also, each electrode or each layer may be formed using a different film formation method. In addition, when the triarylamine derivative described in embodiment 1 is formed into a film by a vacuum deposition method, When refining by sublimation purification, etc., the influence of heating on the triarylamine derivative should be avoided. Therefore, the molecular weight of the triarylamine derivative is preferably 1000 or less. It is preferable to select one having a molecular weight of 800 or less. In addition, when using a wet method, it is necessary to select one having a molecular weight of 800 or less. In order to enhance solubility, the triarylamine derivative described in embodiment 1 may be substituted with It is preferable to use one in which an alkyl group has been introduced.

[0131] The electrodes may be formed by a wet method using the sol-gel method, or by a paste of a metal material. Alternatively, the insulating layer 12 may be formed by a dry method such as a sputtering method or a vacuum deposition method. It may be formed using.

[0132] The light-emitting element according to one embodiment of the present invention having the above-described structure has a first electrode 102 and a second electrode 103. A current flows due to a potential difference between the electrode 104 and the light-emitting layer 105, which is a layer containing a highly luminescent material. In the light-emitting layer 113, holes and electrons recombine to emit light. The structure is such that a light emitting region is formed.

[0133] Light is emitted through either the first electrode 102 or the second electrode 104, or both. Therefore, either the first electrode 102 or the second electrode 104 Or both of them are made of an electrode having optical transparency. Only the first electrode 102 is an electrode having optical transparency. In this case, the emitted light is extracted from the substrate side through the first electrode 102. In the case where only the first electrode 104 is an electrode having light transmitting properties, light is emitted through the second electrode 104 to the substrate 1. The light is taken out from the opposite side to the first electrode 101. The first electrode 102 and the second electrode 104 are both transparent. In the case where the electrodes have a refractive index of 102 or 104, light is emitted through the first electrode 102 and the second electrode 104. The electrons are taken out from both the substrate side and the side opposite the substrate.

[0134] The structure of the layers provided between the first electrode 102 and the second electrode 104 is the same as that described above. However, the present invention is not limited to the above. The first electrode 102 is preferably made of a thin metal, so that quenching caused by the proximity of the first electrode 102 to the metal to be used is suppressed. and a light-emitting region where holes and electrons recombine is provided at a location away from the second electrode 104. The order of stacking layers is not limited to the above, and the second electrode, the electron injection layer, and the like may be stacked from the substrate side. The layer, the electron transport layer, the light emitting layer, the hole transport layer, the hole injection layer, and the first electrode shown in FIG. may be a laminate structure in which the layers are laminated in the reverse order.

[0135] In addition, the hole transport layer and the electron transport layer directly contacting the light emitting layer, particularly the light emitting region in the light emitting layer 113 The carrier (electron or hole) transport layer adjacent to the near side of the region transports electrons and holes from the excitons generated in the light-emitting layer. In order to suppress energy transfer, the energy gap is also Or, the energy gap is larger than the energy gap of the light-emitting material contained in the light-emitting layer. It is preferable that the material be made of a material having a gap.

[0136] The light-emitting element in this embodiment uses a material having a large energy gap as a hole transport layer. Since the triarylamine derivative according to the first embodiment is used, the luminescent material is an emissive material. Even for substances that emit blue light with a large energy gap, it is possible to efficiently produce blue light with good color purity. This makes it possible to provide a light-emitting element with lower power consumption. Specifically, the triarylamine derivative described in the first embodiment has an energy Since the energy gap is about 3.0 eV to 3.4 eV, In a light-emitting element having a light-emitting layer containing a light-emitting substance, the light-emitting efficiency and color purity due to energy transfer are improved. The blue light emitting material can be used without causing a decrease in the energy density. The energy gap is approximately 2.7 eV to 3.0 eV.

[0137] In this embodiment, a light emitting element is fabricated on a substrate made of glass, plastic, or the like. By fabricating multiple light-emitting elements on one substrate, a passive matrix type In addition, a light-emitting device can be manufactured on a substrate made of glass, plastic, etc. For example, a thin film transistor (TFT) is formed, and a light emitting element is formed on an electrode electrically connected to the TFT. A photonic device may be fabricated. This allows the TFT to control the driving of the light-emitting element. It is to be noted that the structure of the TFT is not particularly limited. The TFT may be a staggered type or an inverted staggered type. The crystallinity of the semiconductor is not particularly limited, and an amorphous semiconductor or a crystalline semiconductor may be used. In addition, the driving circuit formed on the TFT substrate may also include N-type and P-type TFTs. Alternatively, it may be composed of either an N-type TFT or a P-type TFT. It may be only from.

[0138] In addition, the triarylamine derivative according to one embodiment of the present invention has a large energy gap. Therefore, when used as a luminescent material, it is a luminescent material with a sufficiently short wavelength and high color purity for blue emission. You can get a child.

[0139] (Embodiment 4) In this embodiment mode, a light-emitting element having a different structure from that shown in Embodiment Mode 3 will be described.

[0140] The light-emitting layer 113 shown in the third embodiment is formed by the triarylamine derivative described in the first embodiment. A configuration in which a luminescent material is dispersed in a conductor to obtain light emission from the material; That is, the triarylamine derivative described in the first embodiment is used as a host material for the light-emitting layer 113. The configuration used is shown below.

[0141] The triarylamine derivative described in embodiment 1 has a large energy gap Therefore, it can effectively excite and emit light from other luminescent materials, and is therefore suitable for use as a host material. It is possible to obtain light emission originating from the luminescent material. It is possible to obtain a light-emitting element with high luminous efficiency and low energy loss. Therefore, it is possible to provide a light emitting device that can easily obtain light of a desired color. It also becomes easy to obtain a light-emitting element that exhibits high light emission.

[0142] Here, the luminescent material to be dispersed in the triarylamine derivative described in embodiment 1 is There is no particular limitation on the material, and various materials can be used.

[0143] Specifically, the fluorescent material is N,N'-bis[4-(9H-carbazole-9 -yl)phenyl]-N,N'-diphenylstilbene-4,4'-diamine (abbreviation: Y GA2S), 4-(9H-carbazol-9-yl)-4'-(10-phenyl-9-a In addition to triphenylamine (abbreviation: YGAPA), etc., emission wavelength is 450 nm or more 4-(9H-carbazol-9-yl)-4'-(9,10-diphenyl-2-anthracene N,9-diphenyl-N-[4- (10-phenyl-9-anthryl)phenyl]-9H-carbazol-3-amine (abbreviation Name: PCAPA), Perylene, 2,5,8,11-tetra-tert-butylperylene ( Abbreviation: TBP), 4-(10-phenyl-9-anthryl)-4'-(9-phenyl-9 H-carbazol-3-yl)triphenylamine (abbreviation: PCBAPA), N,N'' -(2-tert-butylanthracene-9,10-diyldi-4,1-phenylene)bi [N,N',N'-triphenyl-1,4-phenylenediamine] (abbreviation: DPABP A) N,9-diphenyl-N-[4-(9,10-diphenyl-2-anthryl)phenyl] N-[4-(9, 10-diphenyl-2-anthryl)phenyl]-N,N',N'-triphenyl-1, 4-Phenylenediamine (abbreviation: 2DPAPPA), N,N,N',N',N'',N' ',N''',N'''-Octaphenyldibenzo[g,p]chrysene-2,7,10, 15-Tetraamine (abbreviation: DBC1), Coumarin 30, N-(9,10-diphenyl- 2-Anthryl)-N,9-diphenyl-9H-carbazol-3-amine (abbreviation: 2P CAPA), N-[9,10-bis(1,1'-biphenyl-2-yl)-2-anthracene 2PCABPhA ), N-(9,10-diphenyl-2-anthryl)-N,N',N'-triphenyl- 1,4-Phenylenediamine (abbreviation: 2DPAPA), N-[9,10-bis(1,1' -Biphenyl-2-yl)-2-anthryl]-N,N',N'-triphenyl-1,4 -Phenylenediamine (abbreviation: 2DPABPhA), 9,10-bis(1,1'-biphenyl N-[4-(9H-carbazol-9-yl)phenyl]-N-phenyl Nylanthracene-2-amine (abbreviation: 2YGABPhA), N,N,9-triphenyl Anthracene-9-amine (abbreviation: DPhAPhA), Coumarin 545T, N,N'-di Phenylquinacridone (abbreviation: DPQd), rubrene, 5,12-bis(1,1'-biphenyl) phenyl-4-yl)-6,11-diphenyltetracene (abbreviation: BPT), 2-(2-{ 2-[4-(Dimethylamino)phenyl]ethenyl}-6-methyl-4H-pyran-4- 2-{2-methyl-6-[2-(2-phenylindylene)propanedinitrile (abbreviation: DCM1), ,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethy N,Nyl]-4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCM2) ,N',N'-Tetrakis(4-methylphenyl)tetracene-5,11-diamine (abbreviation Name: p-mPhTD), 7,13-diphenyl-N,N,N',N'-tetrakis(4- Methylphenyl)acenaphtho[1,2-a]fluoranthene-3,10-diamine (abbreviation :p-mPhAFD), 2-{2-isopropyl-6-[2-(1,1,7,7-tetramethylphenyl) Methyl-2,3,6,7-tetrahydro-1H,5H-benzo[ij]quinolizine-9- 4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCJT I), 2-{2-tert-butyl-6-[2-(1,1,7,7-tetramethyl-2, 3,6,7-Tetrahydro-1H,5H-benzo[ij]quinolizin-9-yl)ethenyl 4H-pyran-4-ylidene}propanedinitrile (abbreviation: DCJTB), 2-( 2,6-Bis{2-[4-(dimethylamino)phenyl]ethenyl}-4H-pyran-4 -ylidene)propanedinitrile (abbreviation: BisDCM), 2-{2,6-bis[2-( 8-Methoxy-1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H, 5H-Benzo[ij]quinolizin-9-yl)ethenyl]-4H-pyran-4-ylidene }propanedinitrile (abbreviation: BisDCJTM), etc.

[0144] Phosphorescent materials include bis[2-(4',6'-difluorophenyl)pyridinate] -N,C 2' ]Iridium(III) tetrakis(1-pyrazolyl)borate (abbreviation: FI In addition to r6), bis[2-(4',6' -Difluorophenyl)pyridinato-N,C 2' ]Iridium(III) picolinate (abbreviation Name: FIrpic), bis[2-(3',5'-bistrifluoromethylphenyl)pyridine Ginat-N,C 2' ]Iridium(III) picolinate (abbreviation: Ir(CF3ppy)2( pic)), bis[2-(4',6'-difluorophenyl)pyridinato-N,C 2' ]stomach Lithium(III) acetylacetonate (abbreviation: FIracac), emission wavelength is 500 nm (green emission) or higher, tris(2-phenylpyridinato)iridium(III) (abbreviation : Ir(ppy)3), bis(2-phenylpyridinato)iridium(III) acetyl Acetonate (abbreviation: Ir(ppy)2(acac)), tris(acetylacetonate) (Monophenanthroline)terbium(III) (abbreviation: Tb(acac)3(Phen )), bis(benzo[h]quinolinato)iridium(III) acetylacetonate (abbreviation Name: Ir(bzq)2(acac)), bis(2,4-diphenyl-1,3-oxazola To-N,C 2' ) Iridium(III) acetylacetonate (abbreviation: Ir(dpo)2( acac)), bis[2-(4'-perfluorophenylphenyl)pyridinato]irid Ir(III) acetylacetonate (abbreviation: Ir(p-PF-ph)2(acac)) , bis(2-phenylbenzothiazolato-N,C 2' ) Iridium(III) acetylacetone Tonat (abbreviation: Ir(bt)2(acac)), bis[2-(2'-benzo[4,5- α]Thienyl)pyridinato-N,C 3' ]Iridium(III) acetylacetonate (abbreviation Name: Ir(btp)2(acac)), bis(1-phenylisoquinolinato-N,C 2' ) Iridium(III) acetylacetonate (abbreviation: Ir(piq)2(acac)), (Acetylacetonato)bis[2,3-bis(4-fluorophenyl)quinoxalinato] Iridium(III) (abbreviation: Ir(Fdpq)2(acac)), (acetylacetonate Bis(2,3,5-triphenylpyrazinate)iridium(III) (abbreviation: Ir( tppr)2(acac)), 2,3,7,8,12,13,17,18-octaethyl -21H,23H-Porphyrin platinum(II) (abbreviation: PtOEP), tris(1,3- Diphenyl-1,3-propanedionato)(monophenanthroline)europium(II) I) (abbreviation: Eu(DBM)3(Phen)), tris[1-(2-thenoyl)-3,3 ,3-Trifluoroacetonato](monophenanthroline)europium(III)(abbreviation Eu(TTA)3(Phen) and others.

[0145] Among these, the following luminescent substances are available: fluorescent substances with an emission wavelength of 450 nm or more; The wavelength is 450 nm or more (preferably 470 nm or more, more preferably 500 nm or more). When phosphorescent materials are used, the luminous efficiency and color purity are less likely to decrease, and the luminous efficiency is good. It is possible to obtain a light-emitting element with high color purity. In addition, it is possible to provide the triarylamine derivative according to the first embodiment. In addition to the luminescent material dispersed therein, other organic compounds may be dispersed therein at the same time. In this case, a substance that improves the carrier balance of the light-emitting layer is preferable, and the above-mentioned high electron transporting However, as with the triarylamine derivative of one embodiment of the present invention, It is preferable that the material has a large energy gap.

[0146] Note that, except for the light-emitting layer 113, the structure shown in Embodiment 3 can be used as appropriate. As the material for the hole transport layer 112, in addition to the materials shown in the third embodiment, 4,4'-bis[N-( 1-naphthyl)-N-phenylamino]biphenyl (abbreviation: NPB) and N,N'-bis( 3-Methylphenyl)-N,N'-diphenyl-[1,1'-biphenyl]-4,4'- Diamine (abbreviation: TPD), 4,4',4''-tris(N,N-diphenylamino) Triphenylamine (abbreviation: TDATA), 4,4',4''-tris[N-(3-methyl 4,4-phenyl)-N-phenylamino]triphenylamine (abbreviation: MTDATA) '-Bis[N-(spiro-9,9'-bifluoren-2-yl)-N-phenylamino] -1,1'-biphenyl (abbreviation: BSPB) and other aromatic amine compounds with hole transport properties The materials mentioned here are mainly 10 -6 cm 2 / Vs However, if the material has a higher hole transporting property than the electron transporting property, For example, other materials may be used. The material may be a laminate of two or more layers of the above-mentioned materials.

[0147] The hole transport layer 112 is made of poly(N-vinylcarbazole) (abbreviation: PVK) or Uses polymer compounds such as poly(4-vinyltriphenylamine) (abbreviation: PVTPA) It is also possible.

[0148] (Embodiment 5) In this embodiment, a light emitting element having a structure in which a plurality of light emitting units are stacked (hereinafter, referred to as a stacked element) is The embodiment of the light-emitting element (also referred to as a "light-emitting element") will be described with reference to FIG. 1(B). The light-emitting element has a plurality of light-emitting units between the first electrode and the second electrode. The EL layer 103 may have a structure similar to that of the EL layer 103 described in Embodiment 3 or 4. That is, the light-emitting element described in embodiment 3 or embodiment 4 has one light-emitting unit. The light-emitting element of this embodiment is a light-emitting element having a plurality of light-emitting units. It can be called a child.

[0149] In FIG. 1B, a first light-emitting unit is disposed between a first electrode 501 and a second electrode 502. The knit 511 and the second light-emitting unit 512 are laminated, and the first light-emitting unit 511 A charge generating layer 513 is provided between the first electrode and the second light-emitting unit 512. The first electrode 102 and the second electrode 502 are the same as the first electrode 102 and the second electrode 502 in the third embodiment. This corresponds to the pole 104, and the same one as that explained in the third embodiment can be applied. In addition, the first light emitting unit 511 and the second light emitting unit 512 may have the same configuration but different The configuration may be as follows.

[0150] The charge generating layer 513 includes a composite material of an organic compound and a metal oxide. The composite material of the compound and the metal oxide is the composite material shown in the embodiment 3, and is an organic compound and and metal oxides such as vanadium oxide, molybdenum oxide, and tungsten oxide. Organic compounds include aromatic amine compounds, carbazole derivatives, aromatic hydrocarbons, and polymers. Various compounds such as oligomers, dendrimers, polymers, etc. can be used. As the organic compound, a hole-transporting organic compound having a hole mobility of 10 -6 cm 2 However, it is preferable to use a material having a higher hole transporting property than an electron transporting property. Other substances may be used as long as they are the same. The composite of an organic compound and a metal oxide is Excellent carrier injection and transport properties enable low-voltage and low-current operation. It is possible.

[0151] The charge generating layer 513 is made of a layer containing a composite material of an organic compound and a metal oxide and other materials. For example, a layer composed of a combination of an organic compound and a metal oxide may be formed. A layer including a composite material, a compound selected from electron donating substances, and a compound having high electron transport properties. A layer containing an organic compound and a metal oxide may be combined. Alternatively, the light-transmitting layer may be formed by combining a layer containing a material with a transparent conductive film.

[0152] In any case, the battery sandwiched between the first light-emitting unit 511 and the second light-emitting unit 512 When a voltage is applied between the first electrode 501 and the second electrode 502, the charge generating layer 513 It is sufficient that the light-emitting unit injects electrons into the light-emitting unit and the light-emitting unit injects holes into the other light-emitting unit. For example, in FIG. 1B, the potential of the first electrode is higher than the potential of the second electrode. When a voltage is applied so that the charge generating layer 513 emits electrons to the first light-emitting unit 511, It is sufficient that the second light-emitting unit 512 injects holes into the first light-emitting unit 512.

[0153] In this embodiment, a light emitting element having two light emitting units has been described. The same can be applied to a light-emitting element having three or more stacked light-emitting units. As in the light-emitting device according to the present embodiment, a plurality of light-emitting units are electrically connected between a pair of electrodes. By separating the layers, the current density is kept low and long-life elements can be produced in the high-brightness region. In addition, when applied to lighting, the voltage drop caused by the resistance of the electrode material can be reduced. This allows uniform light emission over a large area. It is possible to realize a light emitting device with low light emission.

[0154] In addition, by making the emission color of each light-emitting unit different, For example, a light-emitting element having two light-emitting units can be used. In the above, the luminous color of the first light-emitting unit and the luminous color of the second light-emitting unit are in a complementary color relationship. By doing so, it is possible to obtain a light emitting element that emits white light as a whole. In addition, complementary colors are colors that become achromatic when mixed together. By mixing light from materials that emit light of certain colors, white light can be obtained. The same applies to the case of a light-emitting element having three light-emitting units. For example, the first light-emitting unit The emission color of the first light-emitting unit is red, the emission color of the second light-emitting unit is green, and the emission color of the third light-emitting unit is red. When the light emitted from the dot is blue, the light emitting element as a whole can emit white light.

[0155] The light-emitting element of this embodiment mode contains the triarylamine derivative described in Embodiment 1. Therefore, a light-emitting element having good luminous efficiency can be obtained. The light-emitting unit containing the body can obtain light from the light-emitting material with good color purity, so the entire light-emitting element This makes it easier to adjust the color.

[0156] Note that this embodiment mode can be appropriately combined with other embodiment modes.

[0157] (Embodiment 6) In this embodiment, the triarylamine derivative described in embodiment 1 is used as an organic semiconductor element. The following shows an example of a form in which the active layer is used in a vertical transistor (SIT), which is a type of transistor.

[0158] The structure of the element is as shown in FIG. 2, in which the triarylamine derivative described in the first embodiment is used. A thin-film active layer 1202 containing a conductor is connected to a source electrode 1201 and a drain electrode 1203. The gate electrode 1204 is embedded in the active layer 1202. 204 is electrically connected to a means for applying a gate voltage and the source electrode 12 The source-drain voltage is controlled by the drain electrode 1203 and the source-drain voltage is controlled by the drain electrode 1204. are electrically connected.

[0159] In such an element structure, when no gate voltage is applied, the source-drain When a voltage is applied between the gate and the transistor, current flows (the transistor is in the ON state). When voltage is applied, a depletion layer is generated around the gate electrode 1204, and no current flows (OFF (The state becomes negative.) The above mechanism allows it to function as a transistor.

[0160] In vertical transistors, like light-emitting devices, the material must have both carrier transport properties and good film quality. A material having such a property is required for the active layer, and the triarylamine derivative described in the first embodiment is It fully meets the above conditions and is useful.

[0161] (Embodiment 7) In this embodiment, a compound prepared using the triarylamine derivative described in Embodiment 1 is A light emitting device will now be described.

[0162] In this embodiment, a compound prepared using the triarylamine derivative described in Embodiment 1 is The light-emitting device will be described with reference to FIG. 3. FIG. 3(A) is a top view showing the light-emitting device. FIG. 3B is a cross-sectional view taken along lines A-A' and B-B' in FIG. 3A. The device includes a drive circuit section (source side drive circuit) shown by the dotted line for controlling the light emission of the light emitting element. The pixel portion 602 includes a driver circuit portion (gate side driver circuit) 603. In addition, 604 is a sealing substrate, 605 is a seal material, and the inside surrounded by the seal material 605 is It is space 607.

[0163] The lead wiring 608 is connected to the source side driver circuit 601 and the gate side driver circuit 603. The wiring is for transmitting the input signal, and the FPC (flexible printed circuit board) is the external input terminal. Video signal, clock signal, start signal, reset signal from Lint Circuit 609 Although only the FPC is shown here, the FPC has a printed circuit board. A printed wiring board (PWB) may be attached. This includes not only the device itself, but also the state in which an FPC or PWB is attached to it. do.

[0164] Next, a cross-sectional structure will be described with reference to FIG. A source side driver circuit 601, which is a driver circuit section, and a pixel section are formed in this example. 6, one pixel in the pixel section 602 is shown.

[0165] The source side driver circuit 601 includes an n-channel TFT 623 and a p-channel TFT 62 4 is combined to form a CMOS circuit. The driving circuit is also a variety of CMOS circuits. Alternatively, the substrate may be a PMOS circuit or an NMOS circuit. Although the driver integrated type with the drive circuit is shown above, this is not necessarily required. It may also be formed externally rather than on the substrate.

[0166] The pixel section 602 includes a switching TFT 611, a current control TFT 612, and A plurality of pixels each including a first electrode 613 electrically connected to the drain are arranged. An insulator 614 is formed to cover the end of the first electrode 613. In this case, a positive type photosensitive acrylic resin film is used for the formation.

[0167] In order to improve the covering property, the upper end or the lower end of the insulator 614 is provided with a curvature. For example, the material of the insulator 614 is a positive photosensitive adhesive. When using krill, the insulator 614 has a radius of curvature (0.2 μm to 3 μm) only at the top end. It is preferable that the insulator 614 has a curved surface that is irradiated with light. Negative type that becomes insoluble in etchant, or becomes soluble in etchant when irradiated with light Any positive type resin can be used.

[0168] An EL layer 616 and a second electrode 617 are formed on the first electrode 613. Here, the material used for the first electrode 613 functioning as an anode is a material having a large work function. For example, ITO film or silicon-containing indium tin oxide (ISTO) film is preferable. Indium oxide film containing 2 to 20 wt% zinc oxide, titanium nitride film, chromium film, In addition to single-layer films such as tungsten film, Zn film, and Pt film, titanium nitride film and aluminum film are also available. a laminated film of a titanium nitride film, a film mainly composed of aluminum, and a titanium nitride film; A three-layer structure film such as the above can be used. In addition, the resistance of the wiring is low when the film is made into a laminate structure. This allows for good ohmic contact.

[0169] The EL layer 616 is formed by deposition using a deposition mask, inkjet printing, spin coating, etc. The EL layer 616 is formed by the triaxial growth method shown in the first embodiment. In addition, other materials constituting the EL layer 616 include low The compound may be a molecular compound or a polymer compound (including an oligomer or a dendrimer).

[0170] In addition, the material used for the second electrode 617 formed on the EL layer 616 and functioning as a cathode As the material, materials with a small work function (Al, Mg, Li, Ca, or alloys or compounds of these) It is preferable to use materials such as MgAg, MgIn, AlLi, LiF, CaF2, etc. In addition, when the light generated in the EL layer 616 is to be transmitted through the second electrode 617, 7, a thin metal film and a transparent conductive film (ITO, 2-20 wt% zinc oxide Indium oxide containing silicon, indium tin oxide containing silicon, zinc oxide (ZnO, etc.) It is preferable to use a laminated structure with

[0171] The light-emitting element 618 is formed by the first electrode 613, the EL layer 616, the second electrode 61 The light emitting element 618 is formed of any one of the elements according to the third embodiment to the element according to the fifth embodiment. Furthermore, the pixel portion is formed of a plurality of light emitting elements, and in this embodiment, In the light emitting device in this embodiment, the light emitting element having the configuration described in the third to fifth embodiments is The light-emitting element may include both a light-emitting element having a light-emitting element and a light-emitting element having other configurations.

[0172] In addition, the sealing substrate 604 is bonded to the element substrate 610 with the sealant 605, A light emitting element is disposed in a space 607 surrounded by an element substrate 610, a sealing substrate 604, and a sealant 605. 618. The space 607 is filled with a filler. In some cases, an inert gas (such as nitrogen or argon) is used, and in other cases, a seal material 605 is used. In some cases, it is possible.

[0173] It is preferable to use an epoxy resin for the sealing material 605. It is preferable that the sealing substrate 604 is made of a material that is as impermeable to moisture and oxygen as possible. In addition to glass and quartz substrates, FRP (Fiberglass-Reinforced Plastics) is also used as a material for unforced Plastics), PVF (Polyvinyl fluoride), Polyester Alternatively, a plastic substrate made of acrylic or the like can be used.

[0174] As described above, the compound prepared by using the triarylamine derivative described in the first embodiment A light emitting device having such a structure can be obtained.

[0175] The light-emitting device of one embodiment of the present invention uses the triarylamine derivative described in Embodiment 1. Therefore, good characteristics can be obtained. Arylamine derivatives have a large energy gap and facilitate the transfer of energy from luminescent materials. Therefore, in one embodiment of the present invention, a light-emitting element with high emission efficiency can be provided. It is possible to provide a light emitting device with reduced power consumption. It is possible to obtain high-purity light emission, especially good blue light emission, and therefore has excellent color reproducibility and display This results in a light emitting device with high display quality.

[0176] As described above, in this embodiment, an active matrix light emitting device will be described. However, a passive matrix type light emitting device may also be used. FIG. 4(A) is a perspective view of a passive matrix type light-emitting device manufactured by applying the above method. 4(B) is a cross-sectional view taken along the line XY in FIG. 4(A). In FIG. 4, an EL layer 955 is disposed between an electrode 952 and an electrode 956 on a substrate 951. The end of the electrode 952 is covered with an insulating layer 953. A partition layer 954 is provided on the substrate 3. The sidewall of the partition layer 954 becomes thinner as it approaches the substrate surface. Thus, the distance between one side wall and the other side wall is gradually narrowed. The cross section of the partition layer 954 in the short side direction is trapezoidal, and the bottom side (similar to the surface direction of the insulating layer 953) The side in contact with the insulating layer 953 is oriented in the same direction as the surface direction of the insulating layer 953. The side of the partition layer 954 facing the insulating layer 953 is shorter than the side of the partition layer 954 not in contact with the insulating layer 953. This makes it possible to prevent defects in the light-emitting element caused by static electricity, etc. The light-emitting device of the present invention can also be driven at a low voltage. This allows the device to be driven with low power consumption.

[0177] (Embodiment 8) In this embodiment, a light-emitting device according to one embodiment of the present invention including the light-emitting device described in Embodiment 7 as a part thereof will be described. The electronic device according to one embodiment of the present invention is a triaxial cable as described in Embodiment 1. The electronic device includes a display unit that contains a phenolamine derivative and thus has reduced power consumption. In addition, the present invention provides an electronic device having a display section with excellent color reproducibility and high display quality. It is possible to do so.

[0178] A light-emitting element manufactured using the triarylamine derivative described in Embodiment 1 Electronic devices include cameras such as video cameras and digital cameras, goggle-type displays, Navigation systems, audio playback devices (car audio, audio components, etc.), Computers, game devices, personal digital assistants (mobile computers, mobile phones, handheld games Digital video recorders, electronic books, etc.), image playback devices equipped with recording media (specifically Digital Ver A display device that can play recording media such as digital still discs (DVDs) and display the images. Examples of such electronic devices are shown in Figure 5.

[0179] FIG. 5A illustrates a television device according to one embodiment of the present invention. The television device includes a housing 9101 and a support stand 9102. The television includes a display portion 9103, a speaker portion 9104, a video input terminal 9105, and the like. In the display device, the display unit 9103 is the same as that described in any one of Embodiments 3 to 5. The light emitting element is configured by arranging light emitting elements similar to those described above in a matrix. The light emitting element has good light efficiency and is capable of emitting light of good color. Therefore, the power consumption of a television device having the display portion 9103 formed of the light-emitting element is Furthermore, the present invention provides a television apparatus having excellent color reproducibility and high display quality. It is possible to make the following:

[0180] FIG. 5B shows a computer according to one embodiment of the present invention. The computer includes a main body 9201 and a housing 9202. , a display unit 9203, a keyboard 9204, an external connection port 9205, a pointing device In this computer, the display unit 9203 is the same as that in the third embodiment. The light emitting element is arranged in a matrix, similar to that described in any one of the first to fifth embodiments. The light-emitting element has good light-emitting efficiency. The display unit 9 is made up of the light-emitting element. 203, the computer may be a reduced power computer. Moreover, it is possible to provide a computer with excellent color reproducibility and high display quality.

[0181] FIG. 5C shows a mobile phone according to one embodiment of the present invention. The mobile phone includes a main body 9401, a housing 9402, a front display unit 9403, audio input unit 9404, audio output unit 9405, operation keys 9406, external connection The mobile phone includes a port 9407, an antenna 9408, and the like. The light-emitting element similar to that described in any one of the third to fifth embodiments is arranged in a matrix. The light emitting element has a good light emitting efficiency. Therefore, a display device composed of the light-emitting element is The mobile phone having the unit 9403 can be a mobile phone with reduced power consumption. Moreover, it is possible to provide a mobile phone with excellent color reproducibility and high display quality.

[0182] FIG. 5D shows a camera according to one embodiment of the present invention, which includes a main body 9501, a display portion 9502, a housing 9503, and a casing 9504. Body 9503, external connection port 9504, remote control receiver 9505, image receiver 9506, The device includes a telephoto display 9507, a voice input unit 9508, operation keys 9509, and an eyepiece 9510. In the camera, the display unit 9502 is the same as that described in any one of the third to fifth embodiments. The light emitting element is configured by arranging light emitting elements similar to those described above in a matrix. The efficiency is good. In addition, the light emitting element is capable of emitting light of a good color. Therefore, the camera having the display portion 9502 formed of the light-emitting element consumes less power. In addition, the camera can be made to have excellent color reproducibility and high display quality. is possible.

[0183] As described above, the light emitting device according to the seventh embodiment has a very wide range of applications. The present invention can be applied to electronic devices in a wide range of fields. By using diamine derivatives, it is possible to obtain electronic devices with reduced power consumption. Also, the present invention provides an electronic device having a display unit capable of providing a high-quality display with excellent color reproducibility. can be obtained.

[0184] The light-emitting device described in the seventh embodiment can also be used as a lighting device. An embodiment in which the light-emitting device according to the seventh embodiment is used as a lighting device will be described with reference to FIG.

[0185] FIG. 6 is a diagram showing an example of a liquid crystal display device using the light emitting device according to the seventh embodiment as a backlight. The liquid crystal display device shown in FIG. 6 includes a housing 901, a liquid crystal layer 902, a backlight unit 903, and a The liquid crystal layer 902 is connected to a driver IC 905. In addition, the backlight unit 903 uses the light-emitting device described in the seventh embodiment. , terminal 906 supplies electrical current.

[0186] By using the light-emitting device according to the seventh embodiment as a backlight for a liquid crystal display device, In this way, a backlight with reduced power consumption can be obtained. is a surface-emitting lighting device that can be made large, making it possible to make the backlight larger. In addition, the light-emitting device according to the seventh embodiment can be used in a liquid crystal display device having a large area. Since the display device is thin, it is possible to make the display device thinner.

[0187] FIG. 7 shows a case where the light-emitting device according to the seventh embodiment is used as a desk lamp, which is a lighting device. The desk lamp shown in FIG. 7 has a housing 2001 and a light source 2002. As No. 02, the light emitting device described in the seventh embodiment is used.

[0188] FIG. 8 shows an example in which the light-emitting device according to the seventh embodiment is used as an indoor lighting device 3001. Since the light emitting device described in the seventh embodiment has reduced power consumption, the power consumption In addition, the light-emitting device according to the seventh embodiment can be a lighting device with reduced light emission. Since the device can be integrated, it can be used as a large-area lighting device. The light-emitting device described in No. 7 is thin and can be used as a thin lighting device. In this way, the light emitting device according to the seventh embodiment is used as an indoor lighting device 3001. A television device 3002 according to an embodiment of the present invention as described with reference to FIG. 5(A) was installed in the room. It can also be installed to watch public broadcasts and movies. EXAMPLES

[0189] <Synthesis Example 1> This example relates to a triarylamine derivative shown in structural formula (3) in Embodiment 1. 4-(1-naphthyl)-4'-phenyltriphenylamine (abbreviation: αNBA1BP The structure of αNBA1BP is shown below.

[0190] [ka]

[0191] <Step 1: Synthesis of 4-phenyltriphenylamine> 4-Bromobiphenyl 9.3g (40mmol), diphenylamine 6.8g (40m mol), sodium tert-butoxide 5.0g (50mmol), bis(dibenzoyl) 10 mg of diphenyl acetone palladium (0) was placed in a 300 mL three-neck flask. To the mixture, add 100 mL of xylene, tri(tert-butyl)phosphine (10 wt% hexane The mixture was degassed under reduced pressure with stirring and then cooled to 0.6 mL of dimethylformamide (DMSO solution). The mixture was heated and stirred at 130°C for 3.5 hours under reduced pressure. After stirring, 250 mL of toluene was added to the reaction mixture. Well, this is Celite (Wako Pure Chemical Industries, Ltd., catalog number: 531-16855 used) (hereinafter the same), alumina, Florisil (Wako Pure Chemical Industries, Ltd., Catalog number: 540 The filtrate was washed with water and filtered through a 100% aqueous solution of 1,000 sulphate. The mixture was passed through Celite, alumina, and Florisil. The filtrate was concentrated, methanol was added, and the mixture was recrystallized by ultrasonication. The desired white powder was obtained in an amount of 11 g and a yield of 89%. The synthesis scheme for step 1 is shown below (a- 1).

[0192] [ka]

[0193] <Step 2: Synthesis of 4-bromo-4'-phenyltriphenylamine> 6.4 g (20 mmol) of 4-phenyltriphenylamine, 250 mL of ethyl acetate, 150 mL of toluene was added to a 500 mL Erlenmeyer flask and stirred. 3.6 g (20 mmol) of NBS was added and the mixture was stirred for 27.5 hours. The resulting suspension was washed with water, and then the moisture was removed with magnesium sulfate. The product was dried and the target product was obtained as a white powder in an amount of 7.7 g and a yield of 96%. The team is shown in (b-1).

[0194] [ka]

[0195] <Step 3: 4-(1-naphthyl)-4'-phenyltriphenylamine (abbreviation: αN Synthesis of BA1BP) 8.0 g (20 g) of 4-bromo-4'-phenyltriphenylamine synthesized in step 2 mmol), 1-naphthaleneboronic acid 3.4 g (20 mmol), palladium(II) acetate ) 44mg (0.2mmol), tri(o-tolyl)phosphine 60mg (0.4mmol) l) was placed in a 100 mL three-neck flask, and 20 mL of toluene and ethanol were added to the mixture. 10 mL of 2 mol / L potassium carbonate solution was added, and the mixture was heated under reduced pressure. The mixture was degassed while stirring, and then heated and stirred at 90°C for 2.5 hours under a nitrogen atmosphere to cause a reaction. After the reaction, 150 mL of toluene was added to the reaction mixture, and the mixture was washed with Florisil, silica gel, and The mixture was filtered through Celite. The filtrate was washed with water and magnesium sulfate was added to the mixture. This was filtered through Florisil, alumina, silica gel, and Celite. The filtrate was concentrated, methanol was added, and the mixture was subjected to ultrasonic waves to recrystallize. The target product, a white solid, was obtained in an amount of 8.6 g and a yield of 97%. The system is shown in (c-1).

[0196] [ka]

[0197] Rf value in silica gel thin layer chromatography (TLC) (eluent: ethyl acetate:hexane) The target compound was 0.43, 4-bromo-4'-phenyltriphenylamine. Min was 0.50.

[0198] The compound obtained in step 3 above was analyzed by nuclear magnetic resonance ( 1 1 H NMR) was used to measure the The measurement data is shown below.

[0199] 1 H NMR(CDCl3,300MHz):δ(ppm)=7.07 (t, J=7 .5Hz, 1H), 7.22-7.61 (m, 17H), 7.83 (d, J=7.8Hz, 1H), 7.88-7.91 (m, 1H), 8.02-8. 05 (m, 1H)

[0200] Also, 1 The H NMR chart is shown in Figure 9(A). This chart shows an expanded range of 6 ppm to 9 ppm.

[0201] The molecular weight of the compound was then determined by time-of-flight mass spectrometry. TOF-MS (Waters The measurements were performed using a Waters Micromass LCT Premier (Waters, Inc.). The solvent was a mixture of acetonitrile and 0.1% formic acid (mixture ratio 80 / 20 vol / vol ) was used. This resulted in a peak with a main molecular weight of 448.21 (mode ES+). was detected.

[0202] From the above measurement results, it was found that the triaryl aryl compound represented by the above structural formula (3) was synthesized by this synthesis example. It was found that the amine derivative αNBA1BP was obtained.

[0203] Next, the absorption spectrum of a toluene solution of αNBA1BP and the absorption spectrum of a thin film are shown in Fig. The spectrum of the toluene solution is shown in Fig. 10. The absorption spectrum after subtracting the absorption spectrum of the quartz cell and toluene is shown. The absorption spectrum of the thin film was measured by evaporating αNBA1BP onto a quartz substrate. The absorption spectrum of the quartz substrate was subtracted from that of the quartz substrate. In this figure, the horizontal axis represents the wavelength (nm) and the vertical axis represents the absorption intensity (arbitrary unit). The absorption peak on the long wavelength side in the toluene solution of BP is around 332 nm, The absorption peak on the long side was found to be around 339 nm.

[0204] Figure 11 shows the emission spectrum of a toluene solution of αNBA1BP and the emission spectrum of a thin film. The emission spectrum of the toluene solution was obtained by placing a toluene solution of αNBA1BP in a quartz cell. The emission spectrum of the thin film was measured by evaporating αNBA1BP onto a quartz substrate. As shown in Figure 11, the maximum emission wavelength of αNBA1BP in a toluene solution was is around 404 nm (excitation wavelength 365 nm), and the maximum emission wavelength in the thin film is around 423 nm (excitation wavelength 340 nm).

[0205] In addition, the thin film of αNBA1BP was analyzed by photoelectron spectroscopy (Riken Keiki Co., Ltd., AC-2 The absorption spectrum of the thin film in Fig. 10 was measured at 1000 K and the HOMO level was -5.52 eV. The absorption edge of αNBA1BP was 3.27 eV from the Tauc plot of 100 mV. The solid-state energy gap is estimated to be 3.27 eV, which corresponds to the This means that the LUMO level of αNBA1BP is -2.25 eV. It was found to have a wide energy gap of 3.27 eV in the solid state.

[0206] The oxidation reaction properties of αNBA1BP were also measured. The measurements were performed using an electrochemical analyzer (CV). ALS model 600A or 600C (manufactured by A.S. Co., Ltd.) was used.

[0207] The solution used in the CV measurement was dehydrated N,N-dimethylformamide (DM F) (Sigma-Aldrich, 99.8%, Catalog No. 22705-6) The supporting electrolyte was tetra-n-butylammonium perchlorate (abbreviation: n-Bu4 NClO4) (Tokyo Chemical Industry Co., Ltd., catalog number: T0836) at 100 mmol / L The measurement target is then dissolved to a concentration of 2 mmol / L. The working electrode was a platinum electrode (PTE platinum, manufactured by BAS Co., Ltd.). The auxiliary electrode was a platinum electrode (B.A.S. Co., Ltd., PtCa for VC-3). The counter electrode (5 cm) was used as the reference electrode, and Ag / Ag + Electrode (B.A.S. ( The measurements were performed at room temperature (20 to 25 The scan rate for the CV measurements was standardized to 0.1 V / s.

[0208] The measurement was performed by changing the potential of the working electrode relative to the reference electrode from 0.22 V to 0.70 V. After that, the voltage was changed from 0.70V to 0.22V, which was defined as one cycle. The voltage was measured for 100 cycles. It was determined.

[0209] The results of the measurement showed that even after 100 cycles, there was no significant change in the oxidation peak. BA1BP shows good properties in repeating redox cycles between oxidized and neutral states. Understood.

[0210] The HOMO level of αNBA1BP was also calculated from the results of CV measurements.

[0211] First, the reference electrode (Ag / Ag + potential of the electrode relative to the vacuum level The electron energy (eV) was calculated. + The Fermi level of the electrode was calculated. The redox potential of ferrocene in methanol is +0.61 vs. the standard hydrogen electrode. 0V [vs. SHE] (Reference: Christian R. Goldsmith et al., J.Am.Chem.Soc., Vol.12 4, No.1, 83-96, 2002). On the other hand, using the reference electrode used in this example, The redox potential of ferrocene in methanol was found to be +0.11 V [vs .Ag / Ag + Therefore, the potential energy of the reference electrode used in this example was The energy was found to be 0.50 eV lower than that of the standard hydrogen electrode.

[0212] Here, the potential energy of the standard hydrogen electrode from the vacuum level is -4.44 eV. It is known that (References: Toshihiro Ohnishi and Tamami Koyama, Polymer EL Materials (Kyoritsu Shuppan), From the above, the potential of the reference electrode used in this example with respect to the vacuum level The potential energy was calculated to be -4.44-0.50=-4.94[eV]. .

[0213] Next, we will explain in detail how to calculate the HOMO level of αNBA1BP from the CV measurement. BA1BP oxidation peak potential E pa The reduction peak potential E pc is 0 Therefore, the half-wave potential (E pa and E pc The intermediate potential between the two is calculated to be 0.57 V. This means that αNBA1BP is 0.57 [V vs. Ag / Ag + ] Electricity This indicates that the electron is oxidized by the energy, which corresponds to the HOMO level. As described above, the potential energy of the reference electrode used in this embodiment with respect to the vacuum level is The energy is -4.94 eV, so the HOMO level of αNBA1BP is -4. It was found that 94-0.57=-5.51[eV]. EXAMPLES

[0214] <Synthesis Example 2> This example relates to a triarylamine derivative shown in the structural formula (10) in Embodiment 1. 4,4'-di-(1-naphthyl)-4''-phenyltriphenylamine (abbreviation: This is an example of the synthesis of αNBB1BP. The structure of αNBB1BP is shown below.

[0215] [ka]

[0216] <Step 1: Synthesis of 4-phenyltriphenylamine> The synthesis was carried out in the same manner as in Step 1 of Synthesis Example 1.

[0217] <Step 2: Synthesis of 4,4'-dibromo-4''-phenyltriphenylamine> 4.8 g (15 mmol) of 4-phenyltriphenylamine synthesized in step 1, acetic acid Add 150 mL of ethyl acetate and 100 mL of toluene to a 300 mL Erlenmeyer flask and stir. Add 5.3 g (30 mmol) of N-bromosuccinimide (NBS) to this and mix for 2 The mixture was stirred for 7.5 hours. The resulting suspension was washed with water and then dehydrated with magnesium sulfate. The suspension was concentrated to dryness, and the target product was obtained as a white powder in a yield of 7.1 g and 99%. The synthetic scheme for step 2 is shown in (b-2).

[0218] [ka]

[0219] <Step 3: 4,4'-di-(1-naphthyl)-4''-phenyltriphenylamine Synthesis of (abbreviation: αNBB1BP)> 1,4'-Dibromo-4''-phenyltriphenylamine synthesized in step 2 .4g (3.0mmol), 1-naphthaleneboronic acid 1.1g (6.6mmol), acetic acid Palladium(II) 33mg (0.15mmol), Tri(o-tolyl)phosphine 91 mg (0.3 mmol) was placed in a 100 mL three-neck flask, and 2 mL of toluene was added to the mixture. 0 mL, ethanol 5 mL, and 2.5 mL of 2 mol / L potassium carbonate aqueous solution were added. The mixture was degassed under reduced pressure while stirring, and after degassing, the mixture was heated at 90° C. under a nitrogen atmosphere. The mixture was heated and stirred for 6 hours to react. After the reaction, 150 mL of toluene was added to the reaction mixture. The mixture was filtered through Florisil, alumina, and Celite. The filtrate was washed with water and sulfuric acid. Magnesium was added and dried. After drying, this was mixed with Florisil, alumina, and celite. The filtrate was concentrated, methanol was added, and ultrasonic waves were applied to the filtrate. After that, recrystallization was performed, and the target white solid was obtained in an amount of 1.2 g and a yield of 53%. The synthetic scheme of trip 3 is shown in (c-2).

[0220] [ka]

[0221] Rf value in silica gel thin layer chromatography (TLC) (eluent: ethyl acetate:hexane) 0.59 of the target product, 4,4'-dibromo-4''-phenyltrimethylsilyl ether (1:10) Phenylamine was 0.74.

[0222] The compound obtained in step 3 above was analyzed by nuclear magnetic resonance ( 1 1 H NMR) was used to measure the The measurement data is shown below.

[0223] 1 H NMR(CDCl3,300MHz):δ(ppm)=7.30-7.64 (m , 25H), 7.85 (d, J=7.8Hz, 2H), 7.90-7.93 (m, 2H), 8.04-8.08 (m, 2H)

[0224] Also, 1 The H NMR chart is shown in FIG. 12(A). ) is an expanded chart showing the range from 6 ppm to 9 ppm.

[0225] The molecular weight of the above compound was measured using a TOF-MS detector (Waters, Waters Mic The measurement was performed using a romass LCT Premier. The solvent was acetonitrile and A mixture of 0.1% formic acid and water (mixture ratio 80 / 20 vol / vol) was used. A main peak with a molecular weight of 574.25 (mode ES+) was detected.

[0226] From the above measurement results, it was found that the triaryl aryl compound represented by the above structural formula (10) was synthesized by this synthesis example. It was found that the amine derivative, αNBB1BP, was obtained.

[0227] Next, the absorption spectrum of the toluene solution of αNBB1BP and the absorption spectrum of the thin film are shown in Fig. The spectrum of the toluene solution is shown in Fig. 13. The absorption spectrum after subtracting the absorption spectrum of the quartz cell and toluene is shown. The absorption spectrum of the thin film was measured by evaporating αNBB1BP onto a quartz substrate. The absorption spectrum of the quartz substrate was subtracted from that of the quartz substrate. In this figure, the horizontal axis represents the wavelength (nm) and the vertical axis represents the absorption intensity (arbitrary unit). The absorption peak on the long wavelength side in the toluene solution of BP is around 341 nm, The absorption peak on the long side was found to be around 351 nm.

[0228] Figure 14 shows the emission spectrum of the toluene solution of αNBB1BP and the emission spectrum of the thin film. The emission spectrum of the toluene solution was obtained by placing the toluene solution of αNBB1BP in a quartz cell. The emission spectrum of the thin film was measured by evaporating αNBB1BP onto a quartz substrate. As shown in Figure 14, the maximum emission wavelength of αNBB1BP in a toluene solution was The maximum emission wavelength in the thin film is 426 nm (excitation wavelength 340 nm). It was found that the wavelength of the ion beam was 368 nm.

[0229] In addition, the thin film of αNBB1BP was analyzed by photoelectron spectroscopy (Riken Keiki Co., Ltd., AC-2 The absorption spectrum of the thin film in Fig. 13 was measured at 1000 K and the HOMO level was -5.58 eV. The absorption edge of αNBB1BP was 3.21 eV from the Tauc plot of the torr. The solid-state energy gap is estimated to be 3.21 eV, which corresponds to the This means that the LUMO level of αNBB1BP is -2.37 eV. It was found to have a wide energy gap of 3.21 eV in the solid state.

[0230] The oxidation reaction characteristics of αNBBlBP were also measured. The results were examined in the same manner as in Example 1 by CV measurement.

[0231] As a result of the measurement, even after 100 cycles, there was no significant change in the oxidation peak. P was found to exhibit good properties in repeating redox reactions between oxidized and neutral states. .

[0232] In addition, the HOMO level of αNBB1BP was calculated from the results of CV measurement in the same manner as in Example 1. The HOMO level of αNBB1BP (abbreviation) was found to be -5.50 [eV]. Ta. EXAMPLES

[0233] <Synthesis Example 3> This example relates to a triarylamine derivative shown in the structural formula (1) in the first embodiment. This is a synthesis example of 4-(1-naphthyl)-triphenylamine (abbreviation: αNBA1P). The structure of αNBA1P is shown below.

[0234] [ka]

[0235] <Step 1: Synthesis of 4-bromotriphenylamine> In a solution of 54.0 g (220 mmol) of triphenylamine in 1.5 L of ethyl acetate, Add 35.6g (200mmol) of bromosuccinimide (abbreviation: NBS) and leave for 24 hours. The resulting suspension was concentrated to 1 L and then washed with 1 L of 5% sodium acetate aqueous solution. After washing, the solution was concentrated to about 50 mL and precipitated by adding methanol. The resulting precipitate was collected by filtration and dried to obtain 46.5 g of the target product as a white powder in a yield of 7. The synthesis scheme of step 1 is shown in (b-3).

[0236] [ka]

[0237] Step 2: Synthesis of 4-(1-naphthyl)-triphenylamine (abbreviation: αNBA1P) > 9.7 g (30 mmol) of 4-bromotriphenylamine synthesized in step 1, 1- Naphthaleneboronic acid 5.7 g (33 mmol), palladium(II) acetate 67 mg (0. 3mmol), tri(o-tolyl)phosphine 91mg (0.3mmol), Add 50 mL of toluene, 20 mL of ethanol, and 2 mL of 20 mL of 1 / L potassium carbonate aqueous solution was added. The mixture was degassed under reduced pressure while stirring. After degassing, the mixture was heated and stirred at 90° C. for 2 hours under a nitrogen atmosphere to cause a reaction. After that, 150 mL of toluene was added to the reaction mixture, and the suspension was separated using Florisil, silica gel, and The filtrate was washed with an aqueous solution of sodium bicarbonate and water, in that order. After drying, it was washed, added magnesium sulfate, and dried. The filtrate was filtered through silica gel and celite. The filtrate was concentrated and dried to obtain the target compound. The target product, αNBA1P, was obtained as a white solid in an amount of 11 g and a yield of 99%. The scheme is shown in (c-3).

[0238] [ka]

[0239] Rf value in silica gel thin layer chromatography (TLC) (eluent: ethyl acetate:hexane) The ratio of the target substance to 4-bromotriphenylamine was 0.48 and 0.55, respectively. I did.

[0240] The molecular weight of the white solid obtained in step 2 was measured using a TOF-MS detector (Waters, W The solvent was A. A mixture of acetonitrile and 0.1% formic acid (mixture ratio 80 / 20 vol / vol) was used. This resulted in the detection of a main peak at molecular weight 372.17 (mode ES+). It was confirmed that the desired product, αNBA1P, was obtained. EXAMPLES

[0241] <Synthesis Example 4> This example relates to a triarylamine derivative shown in the structural formula (7) in the first embodiment. Synthesis of 4,4'-di-(1-naphthyl)triphenylamine (abbreviation: αNBB1P) For example, the structure of αNBBlP is shown below.

[0242] [ka]

[0243] <Step 1: Synthesis of 4,4'-dibromotriphenylamine> 12 g (50 mmol) of triphenylamine was dissolved in ethyl acetate in a 500 mL Erlenmeyer flask. After dissolving in 250 mL of alcohol, 18 g ( 100 mmol) was added and the mixture was stirred at room temperature for 24 hours to react. The mixture was washed with water, and magnesium sulfate was added to remove moisture. The filtrate was concentrated to dryness to obtain the target white solid in an amount of 20 g and a yield of 99%. The synthesis scheme of 1 is shown in (b-4).

[0244] [ka]

[0245] <Step 2: 4,4'-di-(1-naphthyl)triphenylamine (abbreviation: αNBB1 Synthesis of P) 6.0 g (15 mmol) of 4,4'-dibromotriphenylamine synthesized in step 1 ), 1-naphthaleneboronic acid 5.2g (30mmol), palladium(II) acetate 2.0 mg (0.01 mmol), tri(o-tolyl)phosphine 6.0 mg (0.02 mmol) l) was placed in a 100 mL three-neck flask, and 20 mL of toluene and ethanol were added to the mixture. 5 mL of 2 mol / L potassium carbonate solution was added, and the mixture was stirred under reduced pressure. The mixture was degassed while stirring, and after degassing, the mixture was heated and stirred at 90°C for 4.5 hours under a nitrogen atmosphere. After the reaction, 150 mL of toluene was added to the reaction mixture, and the suspension was The filtrate was washed with water, and magnesium sulfate was added. The suspension was passed through Florisil, alumina, silica gel, and Celite. The filtrate was concentrated, methanol was added, and the mixture was sonicated. Then, recrystallization gave the target white solid in an amount of 6.4 g and a yield of 86%. The synthetic scheme of 2 is shown in (c-4).

[0246] [ka]

[0247] Rf value in silica gel thin layer chromatography (TLC) (eluent: ethyl acetate:hexane) The amount of the target compound was 0.53 and that of 4,4'-dibromotriphenylamine was 0. It was .69.

[0248] The molecular weight of the white solid obtained in step 2 was measured using a TOF-MS detector (Waters, W The solvent was A. A mixture of acetonitrile and 0.1% formic acid (mixture ratio 80 / 20 vol / vol) was used. This resulted in the detection of a main peak at molecular weight 498.22 (mode ES+). It was confirmed that the desired product, αNBB1P, was obtained. EXAMPLES

[0249] <Synthesis Example 5> This embodiment relates to a triarylamine derivative shown in structural formula (2) in Embodiment 1. α-Naphthyl-4-phenyl-4-yl-diphenylamine (abbreviation: αNT This is an example of the synthesis of αNTA1P. The structure of αNTA1P is shown below.

[0250] [ka]

[0251] <Step 1: Synthesis of 4-(4-bromophenyl)-triphenylamine> 22 g (70 mmol) of 4,4'-dibromobiphenyl, 8.5 g ( 50mmol), copper(I) iodide 1.9g (10mmol), 18-crown-6-acetate 2.6g (10mmol) of tert-butyl ether, 6.9g (50mmol) of potassium carbonate, Chil-3,4,5,6-tetrahydro-2(1H)-pyrimidinone (abbreviation: DMPU)5 0 mL was placed in a 500 mL three-neck flask and stirred at 180°C for 37 hours under a nitrogen atmosphere. After the reaction, 500 mL of toluene was added to the reaction mixture, and the suspension was The mixture was filtered through silica gel, silica gel, and celite. The filtrate was washed with water and diluted with mag- nesium sulfate. The water was removed by adding sodium hydroxide. The filtrate was concentrated and purified by silica gel column chromatography. The resulting fraction was purified by elution with a developing solvent of toluene:hexane=1:4. The fraction was concentrated, hexane and methanol were added, and the mixture was subjected to ultrasonic waves, after which it was recrystallized. The target product, a white powder, was obtained in an amount of 5.3 g and a yield of 27%. The synthesis scheme for step 1 is shown below. As shown in b'-5).

[0252] [ka]

[0253] Rf value in silica gel thin layer chromatography (TLC) (eluent: ethyl acetate:hexane) The yield of the target substance was 0.5 and that of 4,4'-dibromobiphenyl was 0.59. Ta.

[0254] <Step 2: [4'-(1-naphthyl)biphenyl-4-yl]diphenylamine (abbreviation Synthesis of αNTA1P) 4.0 g (1 g) of 4-(4-bromophenyl)-triphenylamine synthesized in step 1 0mmol), 1-naphthaleneboronic acid 1.7g (10mmol), palladium acetate (I I) 11 mg (0.05 mmol), tri(o-tolyl)phosphine 15 mg (0.05 mmol) 20 mL of toluene and 100 mL of ethanol were added to the mixture. 5 mL of alcohol and 10 mL of 2 mol / L aqueous potassium carbonate solution were added. After degassing while stirring under nitrogen atmosphere, the mixture was heated and stirred at 90° C. for 7 hours to carry out the reaction. After the reaction, 150 mL of toluene was added to the reaction mixture, and the suspension was chromatographed on silica gel, alumina, The mixture was filtered through Celite. The filtrate was washed with water and magnesium sulfate was added to the mixture. The residue was removed. The mixture was filtered through silica gel, alumina, and celite to obtain a filtrate. The filtrate was concentrated, methanol was added, and the mixture was subjected to ultrasonic waves. The product was then recrystallized to obtain the desired product. The white powder was obtained in an amount of 3.6 g and a yield of 80%. The synthesis scheme for step 2 is shown below (c-5). As shown in.

[0255] [ka]

[0256] Rf value in silica gel thin layer chromatography (TLC) (eluent: ethyl acetate:hexane) Xanthane = 1:10) was 0.58, 1-(4'-bromobiphenyl-4-yl) Naphthalene was 0.65.

[0257] The white solid obtained in step 2 above was analyzed by nuclear magnetic resonance ( 1 1 H NMR). The measurement data is shown below.

[0258] 1 H NMR(CDCl3,300MHz):δ(ppm)=7.05 (t, J=7 .8Hz, 2H), 7.12-7.58 (m, 18H), 7.70 (d, J=7.8Hz, 2H), 7.87 (d, J=8.1Hz, 1H), 7.9 2 (d, J=7.8Hz, 1H), 7.99 (d, J=8.7Hz, 1H )

[0259] The molecular weight of the above white solid was determined using a TOF-MS detector (Waters, Waters Mi The measurement was performed using a cromass LCT Premier. The solvent was acetonitrile and A mixture of 0.1% formic acid and water (mixture ratio 80 / 20 vol / vol) was used. A main peak with a molecular weight of 448.20 (mode ES+) was detected.

[0260] From the above measurement results, it was found that the compound represented by the above structural formula (2) according to one embodiment of the present invention was synthesized by this synthesis example. It was found that the triarylamine derivative αNTA1P was obtained. EXAMPLES

[0261] <Synthesis Example 6> This example relates to a triarylamine derivative shown in the structural formula (19) in Embodiment 1. The compound 4,4'-di-(2-naphthyl)triphenylamine (abbreviation: βNBB1P) The structure of βNBB1P is shown below.

[0262] [ka]

[0263] <Step 1: Synthesis of 4,4'-dibromotriphenylamine> The synthesis was carried out in the same manner as in Step 1 of Synthesis Example 4.

[0264] <Step 2: 4,4'-di-(2-naphthyl)triphenylamine (abbreviation: βNBB1 Synthesis of P) 6.0 g (15 mmol) of 4,4'-dibromotriphenylamine synthesized in step 1 ), 2-naphthaleneboronic acid 6.2 g (36 mmol), palladium(II) acetate 16 m g (0.1 mmol), tri(o-tolyl)phosphine 21 mg (0.1 mmol), Put into a 300mL three-neck flask and add 50mL of toluene and 20mL of ethanol to this mixture. Then, 20 mL of 2 mol / L aqueous potassium carbonate solution was added. The mixture was stirred under reduced pressure. After degassing, the mixture was heated and stirred at 90°C for 4.5 hours under a nitrogen atmosphere to react. To this reaction mixture was added 150 mL of toluene, and the mixture was then separated into Florisil, silica gel, and Celite. The filtrate was washed with water and magnesium sulfate was added to remove moisture. The mixture was filtered through Florisil, alumina, silica gel, and Celite. The filtrate was concentrated, hexane was added, and the mixture was recrystallized after ultrasonic treatment. The target product, a white powder, was obtained in an amount of 5.6 g and a yield of 75%. The synthesis scheme for step 2 is shown in (c -6).

[0265] [ka]

[0266] Rf value in silica gel thin layer chromatography (TLC) (eluent: ethyl acetate:hexane) The amount of the target compound was 0.53 and that of 4,4'-dibromotriphenylamine was 0. It was .78.

[0267] The molecular weight of the white powder obtained in step 2 was measured using a TOF-MS detector (Waters, Wa The measurements were performed using a meter Micromass LCT Premier. A mixture of trinitrile and 0.1% formic acid (mixture ratio 80 / 20 vol / vol) was used. This resulted in the detection of a main peak at molecular weight 498.22 (mode ES+). It was confirmed that the desired βNBB1P was obtained. EXAMPLES

[0268] <Synthesis Example 7> This example relates to a triarylamine derivative shown in structural formula (3) in Embodiment 1. 4-(1-naphthyl)-4'-phenyltriphenylamine (abbreviation: αNBA1BP ) is a synthesis example using a method different from that of Synthesis Example 1. The structure of αNBA1BP is shown below. As shown in.

[0269] [ka]

[0270] <Step 1: Synthesis of 4-phenyl-diphenylamine> 4-Bromobiphenyl 51g (220mmol), aniline 23g (250mmol) , sodium tert-butoxide 50g (500mmol), bis(dibenzylidene Add 250 mg (0.4 mmol) of palladium(0) in 1000 mL three-neck flask. The mixture was poured into a flask and the atmosphere in the flask was replaced with nitrogen. 500 mL of dehydrated toluene was added to this mixture. The mixture was degassed under reduced pressure with stirring. After degassing, tri(tert-butyl) Then, 3.0 mL (1.5 mmol) of 10 wt% hexane solution was added. The mixture was then heated and stirred at 90° C. for 4.5 hours under a nitrogen atmosphere to react. After the reaction, 600 mL of toluene was added to the reaction mixture, which was then passed through Florisil and Celite. The filtrate was washed with water and magnesium sulfate was added to remove moisture. The mixture was filtered through Florisil and Celite to obtain a filtrate. The filtrate was concentrated to give After adding hexane and applying ultrasonic waves, the product was recrystallized to obtain the desired product, 4-phenyl-di The white powder of phenylamine was obtained in an amount of 40 g and a yield of 73%. is shown in (a-7).

[0271] [ka]

[0272] <Step 2: Synthesis of 1-(4-bromophenyl)-naphthalene> 4-Bromoiodobenzene 46g (160mmol), 1-naphthaleneboronic acid 24g (140mmol), palladium(II) acetate 45mg (0.2mmol), tri(o- Put 60 mg (0.2 mmol) of (tolyl)phosphine into a 500 mL three-neck flask. To the mixture, add 100 mL of toluene, 20 mL of ethanol, and 2 mol / L aqueous potassium carbonate solution. The mixture was degassed under reduced pressure while stirring, and then, The mixture was heated and stirred at 90° C. for 4 hours to react. After the reaction, 500 mL of toluene was added to the reaction mixture. The mixture was filtered through Florisil and Celite. The filtrate was washed with water and Magnesium sulfate was added to remove moisture. The mixture was filtered through Florisil and Celite. The filtrate was concentrated and purified by silica gel column chromatography (development). The fraction was concentrated and the target product was obtained. The colorless transparent liquid was obtained in an amount of 25 g and a yield of 62%. The synthesis scheme for step 2 is shown below. ) as shown in

[0273] [ka]

[0274] The Rf value in silica gel thin layer chromatography (TLC) (eluent: hexane) ) was 0.38 for the target substance and 0.57 for 4-bromoiodobenzene.

[0275] <Step 3: Synthesis of 4-(1-naphthyl)-4'-phenyltriphenylamine> 5.7 g (20 mmol) of 1-(4-bromophenyl)naphthalene synthesized in step 2 ), 4.9 g (20 mmol) of 4-phenyl-diphenylamine synthesized in step 1, Sodium tert-butoxide 2.5g (25mmol), bis(dibenzylidene a Add 11 mg (0.02 mmol) of palladium(0) to a 300 mL three-neck flask. The atmosphere in the flask was replaced with nitrogen. 50 mL of dehydrated xylene was added to this mixture. The mixture was degassed under reduced pressure while stirring, and after degassing, tri(tert-butyl) phosphate was added. 0.1 mL (0.06 mmol) of sphingosine (10 wt% hexane solution) was added to this mixture. The mixture was reacted by heating and stirring at 110° C. for 6.5 hours under a nitrogen atmosphere. 150 mL of toluene was added to the reaction mixture, which was then passed through Florisil, silica gel, and Celite. The filtrate was washed with water and magnesium sulfate was added to remove moisture. The mixture was filtered through Florisil, silica gel, and Celite to obtain a filtrate. The liquid was concentrated and purified by silica gel column chromatography (eluent: toluene:hexane = 1 The resulting fraction was concentrated, and acetone and hexane were added to the concentrate. After applying ultrasonic waves to the mixture, the product was recrystallized to obtain a white powder (7.3 g, 98% yield). The synthetic scheme for step 3 is shown in (c-7).

[0276] [ka]

[0277] Rf value in silica gel thin layer chromatography (TLC) (eluent: ethyl acetate:hexane) For the hexane = 1:10), the target product was 0.31, 1-(4-bromophenyl)-naphthalene Talen was 0.60 and 4-phenyl-diphenylamine was 0.16.

[0278] The molecular weight of the white powder obtained in step 3 was measured using a TOF-MS detector (Waters, W The solvent was A. A mixture of acetonitrile and 0.1% formic acid (mixture ratio 80 / 20 vol / vol) was used. This resulted in the detection of a main peak at molecular weight 448.21 (mode ES+). From the measurement results, it was found that the triarylamine represented by the above structural formula (3) was obtained by this synthesis example. It was found that the αNBA1BP derivative was obtained. EXAMPLES

[0279] Synthesis Example 8 This example relates to a triarylamine derivative shown in the structural formula (7) in the first embodiment. Regarding 4,4'-di-(1-naphthyl)triphenylamine (abbreviation: αNBB1P), This is a synthesis example by a method different from that of Synthesis Example 4. The structure of αNBBlP is shown below.

[0280] [ka]

[0281] <Step 1: Synthesis of 1-(4-bromophenyl)-naphthalene> The synthesis was carried out in the same manner as in Step 2 of Synthesis Example 7.

[0282] <Step 2: 4,4'-di-(1-naphthyl)triphenylamine (abbreviation: αNBB1 Synthesis of P) 3.4 g (12 mmol) of 1-(4-bromophenyl)-naphthalene synthesized in step 1 l), aniline 0.5 g (5 mmol), sodium tert-butoxide 1.5 g ( 15mmol), palladium(II) acetate 10mg (0.05mmol), 1,1-bis (Diphenylphosphino)ferrocene (abbreviation: DPPF) 10mg (0.05mmol) Then, 15 mL of toluene was placed in a 100 mL three-neck flask. The contents of the flask were stirred under reduced pressure. After degassing with stirring, the mixture was heated and stirred at 80°C for 5 hours under a nitrogen atmosphere to cause a reaction. To the reaction mixture was added 150 mL of toluene, and the mixture was filtered through Florisil and Celite. The filtrate was concentrated and purified by silica gel column chromatography (eluent: The resulting fraction was concentrated and purified with methanol (toluene:hexane = 1:4). After adding alcohol and applying ultrasonic waves, the product was recrystallized, yielding 1.9 g of the desired white powder. The synthesis scheme of step 2 is shown in (c-8).

[0283] [ka]

[0284] Rf value in silica gel thin layer chromatography (TLC) (eluent: ethyl acetate:hexane) For the hexane = 1:10), the target product was 0.22, 1-(4-bromophenyl)-naphthalene Talen was 0.53. EXAMPLES

[0285] In this example, the triarylamine derivative described in Embodiment 1 was used as a blue fluorescent material. The two light-emitting elements (light-emitting element 2) were fabricated using the material constituting the hole transport layer adjacent to the light-emitting layer. The light-emitting devices 3) were fabricated and their performance tests were also carried out. For comparison, light-emitting devices (light-emitting devices 1 and 4) not using the triarylamine derivative were also fabricated. They were also manufactured and performance tests were carried out.

[0286] The organic compounds used in this example (αNBA1BP and αNBB1BP are the same as those in Example 1 and The molecular structure of the compound (the structure was shown in Example 2 and is therefore omitted) is shown in the following structural formulas (i) to (vi). In FIG. 1A, the structure is an electron injection layer between the electron transport layer 114 and the second electrode 104. The structure is provided with

[0287] [ka]

[0288] <Fabrication of Light-emitting Elements 1 to 4> First, a silicon-containing indium tin oxide ( A glass substrate 101 on which an ITSO film was formed was prepared. The ITSO surface had a 2 mm square area. The periphery was covered with a polyimide film so that the surface was exposed at a depth of 2 mm, and the electrode area was 2 mm × 2 mm. As a pretreatment for forming a light-emitting element on this substrate, the substrate surface was washed with water and heated at 200°C. After baking for 1 hour, UV ozone treatment was performed for 370 seconds. -4 Within about Pa The substrate was introduced into a vacuum deposition apparatus in which the pressure in the vacuum deposition section was reduced, and the substrate was heated to 170° C. in a heating chamber in the vacuum deposition apparatus. After vacuum baking at RT for 30 minutes, the substrate was allowed to cool for about 30 minutes.

[0289] Next, the surface on which ITSO was formed was placed facing down in the chamber in which the holder was installed in the vacuum deposition device. The substrate 101 was fixed to a holder so that the substrate 101 could be fixed in place.

[0290] The vacuum deposition equipment was -4 After reducing the pressure to 10 Pa, 4,4'-biphenyl represented by the above structural formula (i) was [N-(1-naphthyl)-N-phenylamino]biphenyl (abbreviation: NPB) and oxidized molybdenum NPB:molybdenum oxide (VI) was mixed with molybdenum oxide (VI) in a ratio of 4:1 (by mass). The hole injection layer 111 was formed by co-evaporation with the above. The film thickness was set to 50 nm. Co-evaporation is a deposition method in which different substances are evaporated simultaneously from different evaporation sources. do.

[0291] Next, NPB, which is widely used as a material for the hole transport layer, was used as the light-emitting element 1. The molecule 2 is a triarylamine derivative, αNBA1BP, described in the first embodiment, and a luminescent element. The molecule 3 is a triarylamine derivative, αNBB1BP, which is described in the first embodiment, and a luminescent element. The molecule 4 is a known substance represented by the above structural formula (ii), 4-(1-naphthyl)-4'-phenylacetone. By depositing 10 nm of each of phenyltriphenylamine (abbreviation: αNBABP), A hole transport layer 112 was formed.

[0292] Further, on the hole transport layer 112, a 9-[4-(10-fluoro) CzPA) and the above structure 4-(10-phenyl-9-anthryl)-4'-(9-phenyl) represented by formula (iv) (9H-carbazol-3-yl)triphenylamine (abbreviation: PCBAPA) and Light was emitted by co-evaporation at a mass ratio of zPA:PCBAPA = 1:0.1. A layer 113 was formed to a thickness of 30 nm.

[0293] Next, tris(8-quinolinolato)aluminum (III) represented by the above structural formula (v) ) (abbreviation: Alq) was applied to 10 nm, and bathophenan (VI) represented by the above structural formula was applied to Alq. Electron transport layer 114 is formed by depositing 20 nm of troline (abbreviation: BPhen). Furthermore, lithium fluoride was evaporated onto the electron transport layer 114 to a thickness of 1 nm. Finally, an electron injection layer was formed by applying a ZnO film as a second electrode 104 functioning as a cathode. A 200 nm thick aluminum film was then formed, completing the light-emitting elements 1 to 4. In all cases, the deposition was performed using a resistance heating method.

[0294] <Operation characteristics of light-emitting elements 1 to 4> The light-emitting elements 1 to 4 obtained as described above were placed in a glove box with a nitrogen atmosphere. After sealing the light emitting elements so that they are not exposed to the atmosphere, the operating characteristics of these light emitting elements are The measurements were carried out at room temperature (an atmosphere maintained at 25°C).

[0295] FIG. 15 shows the voltage-luminance characteristics of each light-emitting element, and FIG. 16 shows the luminance-current efficiency characteristics. The power efficiency characteristics are shown in Fig. 17. In Fig. 15, the vertical axis is the luminance (cd / m 2 ), the horizontal axis is voltage (V) In Fig. 16, the vertical axis shows the current efficiency (cd / A) and the horizontal axis shows the luminance (cd / m 2 ) is shown. In 17, the vertical axis is power efficiency (lm / W) and the horizontal axis is brightness (cd / m 2 ) is shown.

[0296] As can be seen from the figure, the triarylamine derivative described in the first embodiment is used as a hole transport layer. Light-emitting element 2 and light-emitting element 3 have better luminance-current efficiency characteristics than light-emitting element 1 and light-emitting element 4. It is clear that the luminous efficiency is good. 2 Each in The power efficiency of the elements (lm / W) was 4.1 for light-emitting element 1, 6.3 for light-emitting element 2, and The light-emitting element 2 and the light-emitting element 3 had a refractive index of 6.2 and 5.3, respectively. It is possible to drive the light-emitting element 1 and the light-emitting element 4 with lower power consumption, and the light-emitting element 1 and the light-emitting element 4 are excellent. Understood.

[0297] The emission spectra when a current of 1 mA was applied to the fabricated light-emitting elements 1 to 4 are shown in FIG. In FIG. 18, the horizontal axis indicates the emission wavelength (nm) and the vertical axis indicates the emission intensity. The values ​​are shown as relative values ​​with the same maximum light emission intensity. It can be seen that all of them exhibit good blue luminescence due to the luminescent substance PCBAPA.

[0298] Next, the initial luminance is set to 1000cd / m 2and operate the device under constant current density conditions. The 50% half-life of each element showed similarly good characteristics. EXAMPLES

[0299] In this example, the triarylamine derivative described in Embodiment 1 was used as a compound having a phosphorescent property emitting green light. The material constituting the hole transport layer adjacent to the light-emitting layer was used in one light-emitting element (light-emitting element 7). ) was prepared and a performance test was also carried out on it. We also fabricated light-emitting devices (light-emitting devices 5 and 6) that did not use arylamine derivatives. Performance tests were conducted.

[0300] The molecular structure of the organic compound used in this example (those already shown are omitted) is represented by the following structural formula (v The element structure is shown in FIG. 1A, which includes an electron transport layer 114 and a second An electron injection layer was provided between the first electrode 104 and the second electrode 104.

[0301] [ka]

[0302] <Fabrication of Light-emitting Elements 5 to 7> First, a silicon-containing indium tin oxide ( A glass substrate 101 on which an ITSO film was formed was prepared. The ITSO surface had a 2 mm square area. The periphery was covered with a polyimide film so that the surface was exposed at a depth of 2 mm, and the electrode area was 2 mm × 2 mm. As a pretreatment for forming a light-emitting element on this substrate, the substrate surface was washed with water and heated at 200°C. After baking for 1 hour, UV ozone treatment was performed for 370 seconds. -4 Within about Pa The substrate was introduced into a vacuum deposition apparatus in which the pressure in the vacuum deposition section was reduced, and the substrate was heated to 170° C. in a heating chamber in the vacuum deposition apparatus. After vacuum baking at RT for 30 minutes, the substrate was allowed to cool for about 30 minutes.

[0303] Next, the surface on which ITSO was formed was placed facing down in the chamber in which the holder was installed in the vacuum deposition device. The substrate 101 was fixed to a holder so that the substrate 101 could be fixed in place.

[0304] The vacuum deposition equipment was -4 After reducing the pressure to 10 Pa, 4,4'-biphenyl represented by the above structural formula (i) was [N-(1-naphthyl)-N-phenylamino]biphenyl (abbreviation: NPB) and oxidized molybdenum NPB:molybdenum oxide (VI) was mixed with molybdenum oxide (VI) in a ratio of 4:1 (by mass). The hole injection layer 111 was formed by co-evaporation with the above. The thickness of the layer was set to 40 nm. Co-evaporation is a deposition method in which different substances are evaporated simultaneously from different evaporation sources. do.

[0305] Next, NPB, which is widely used as a material for the hole transport layer, was used as the light-emitting element 5. The light-emitting element 6 is αNBABP, the structure of which is shown as (ii) in Example 6, and the light-emitting element 7 is αNBA1BP, which is a triarylamine derivative according to one embodiment of the present invention described in embodiment 1, The hole transport layer 112 was formed by depositing each of them to a thickness of 20 nm.

[0306] Further, on the hole transport layer 112, a 4-(9H-carbazone) compound represented by the above structural formula (vii) is 4'-(5-phenyl-1,3,4-oxadiazol-2-yl) Triphenylamine (abbreviation: YGAO11) and the bis[ 2-Phenylpyridinato-N,C 2' ]Iridium(III) acetylacetonate (abbreviation :Ir(ppy)2acac), YGAO11:Ir(ppy)2acac=1:0.0 The light-emitting layer 113 was formed by co-evaporation so that the ratio of the layers was 40 to 5 (mass ratio). nm.

[0307] Next, bathophenanthroline (abbreviation: BPhen) represented by the above structural formula (vi) is 100 nm thick was evaporated to form an electron transport layer 114. Then, lithium fluoride was evaporated to a thickness of 1 nm to form an electron injection layer. After that, an aluminum film is formed to a thickness of 200 nm as the second electrode 104 that functions as a cathode. Optical elements 5 to 7 were completed. In the deposition process described above, the deposition was all performed using the resistance heating method. there was.

[0308] <Operation characteristics of light-emitting elements 5 to 7> The light-emitting devices 5 to 7 obtained as described above were placed in a glove box with a nitrogen atmosphere. After sealing the light emitting elements so that they are not exposed to the atmosphere, the operating characteristics of these light emitting elements are The measurements were carried out at room temperature (an atmosphere maintained at 25°C).

[0309] The current density-luminance characteristics of each light-emitting element are shown in FIG. 19, the luminance-current efficiency characteristics are shown in FIG. 20, and the luminance-power The efficiency characteristics are shown in Fig. 21, and the voltage-luminance characteristics are shown in Fig. 22. In Fig. 19, the vertical axis is the luminance (cd / m 2 ), the horizontal axis is the current density (mA / cm 2 In Figure 20, the vertical axis indicates current efficiency (cd / A), The horizontal axis is luminance (cd / m 2 In Fig. 21, the vertical axis represents power efficiency (lm / W) and the horizontal axis represents luminance. Degree (cd / m 2 In Figure 22, the vertical axis indicates luminance (cd / m 2 ), the horizontal axis indicates voltage (V) .

[0310] As can be seen from the figure, the triarylamine derivative described in the first embodiment is used as a hole transport layer. The light-emitting element 7 exhibits better luminance-current efficiency characteristics than the light-emitting elements 5 and 6, and the light-emitting efficiency It can be seen that the image quality is good at 1000 cd / m 2 The power of each light-emitting element in The efficiency (lm / W) was 33 for light-emitting element 5, 40 for light-emitting element 6, and 50 for light-emitting element 7. This shows that the light-emitting element 7 can be driven with lower power consumption than the light-emitting elements 5 and 6. It was found to be a good light-emitting element.

[0311] Also, 1000cd / m 2 The CIE chromaticity coordinates of the light-emitting elements 5 to 7 in (0.35, 0.62), both of which emit green light from Ir(ppy)2acac. presented.

[0312] From the above results, it can be seen that the triarylamine derivative described in the first embodiment emits green phosphorescence. Since high luminous efficiency is observed even when the layer is used as a hole transport layer adjacent to a light emitting layer, It can be seen that this is a substance with high triplet energy. EXAMPLES

[0313] In this example, the triarylamine derivative described in Embodiment 1 is treated with an acceptor substance. Four light-emitting devices (light-emitting devices) were fabricated using a composite material containing the above as a material for the hole injection layer. The elements 9 to 12) were fabricated and performance tests were carried out on them. For comparison, a light-emitting device (light-emitting device 8) was prepared without using the triarylamine derivative. Performance tests were also carried out on this.

[0314] In addition, since all the organic compounds used in this example have already been described in this specification, the molecular structures The structure of the element is omitted. In FIG. 1A, the light-emitting layer 113 is a two-layer light-emitting layer. In addition, an electron injection layer was provided between the electron transport layer 114 and the second electrode 104.

[0315] <Fabrication of Light-emitting Elements 8 to 12> First, a silicon-containing indium tin oxide ( A glass substrate 101 on which an ITSO film was formed was prepared. The ITSO surface had a 2 mm square area. The periphery was covered with a polyimide film so that the surface was exposed at a depth of 2 mm, and the electrode area was 2 mm × 2 mm. As a pretreatment for forming a light-emitting element on this substrate, the substrate surface was washed with water and heated at 200°C. After baking for 1 hour, UV ozone treatment was performed for 370 seconds. -4 Within about Pa The substrate was introduced into a vacuum deposition apparatus in which the pressure in the vacuum deposition section was reduced, and the substrate was heated to 170° C. in a heating chamber in the vacuum deposition apparatus. After vacuum baking at RT for 30 minutes, the substrate was allowed to cool for about 30 minutes.

[0316] Next, the surface on which ITSO was formed was placed facing down in the chamber in which the holder was installed in the vacuum deposition device. The substrate 101 was fixed to a holder so that the substrate 101 could be fixed in place.

[0317] The vacuum deposition equipment was -4 After the pressure was reduced to 10 Pa, the light-emitting element 8, which is a comparative element, was treated with NPB and oxidized Molybdenum (VI) was added to NPB:molybdenum (VI) oxide at a mass ratio of 4:1. The hole-injection layer 111 was formed by co-evaporation as shown in FIG. The light-emitting elements 9 to 12, which are examples of the elements, are the same as those described in Embodiment 1, instead of NPB. The arylamine derivative αNBA1BP was used, and the αNBA1BP and molybdenum oxide were (VI) was co-evaporated to form the hole injection layer 111. The mass ratio of P to molybdenum (VI) oxide is αNBA1BP:molybdenum oxide ( VI)=8:1, the light-emitting element 10 has an αNBA1BP:molybdenum oxide (VI)=4:1, The optical element 11 and the light-emitting element 12 have an αNBA1BP:molybdenum (VI) oxide ratio of 2:1. The thickness of the hole injection layer was set to 50 nm. This is a deposition method in which multiple substances are evaporated simultaneously from different evaporation sources.

[0318] Next, in the light-emitting elements 8 to 11, a material that is widely used as a hole transport layer is The light-emitting element 12 is a triarylamine derivative, αN BA1BP was evaporated to a thickness of 10 nm to form a hole transport layer 112.

[0319] Furthermore, after depositing PCBAPA at 25 nm on the hole transport layer 112, CzPA and PCB APA is co-deposited to a thickness of 30 nm so that CzPA:PCBAPA=10:1 (mass ratio). In this way, the light emitting layer 113 was formed.

[0320] Next, 10 nm of Alq was deposited and 20 nm of Bphen was deposited on the Alq. The transport layer 114 was formed. Furthermore, lithium fluoride was formed on the electron transport layer 114 to a thickness of 1 nm. Finally, a second layer, which acts as a cathode, was deposited on the As the electrode 104, an aluminum film of 200 nm was formed, and the light-emitting elements 8 to 12 were completed. In the above-mentioned deposition processes, the deposition was all carried out by a resistance heating method.

[0321] <Operation characteristics of light-emitting elements 8 to 12> The light-emitting devices 8 to 12 obtained as described above were placed in a glove box with a nitrogen atmosphere. After sealing the light emitting elements so that they are not exposed to the atmosphere, the operation of these light emitting elements is The characteristics were measured at room temperature (an atmosphere maintained at 25°C).

[0322] FIG. 23 shows the voltage-luminance characteristics of each light-emitting element, and FIG. 24 shows the luminance-current efficiency characteristics. The power efficiency characteristics are shown in Fig. 25. In Fig. 23, the vertical axis is the luminance (cd / m 2 ), the horizontal axis is voltage (V) In Fig. 24, the vertical axis shows the current efficiency (cd / A) and the horizontal axis shows the luminance (cd / m 2 ) is shown. 25, the vertical axis is power efficiency (lm / W) and the horizontal axis is brightness (cd / m 2 ) is shown.

[0323] From FIG. 24, it can be seen that the triarylamine derivative described in the first embodiment is an acceptor substance. The light-emitting elements 9 to 12, in which the composite material is used in the hole injection layer, are the same as those described in the first embodiment. The light-emitting device 8 using NPB instead of the triarylamine derivative described above exhibited better luminance-current properties. It was found that the light-emitting element had good luminous efficiency. 000cd / m 2 The power efficiency (lm / W) of each light-emitting element in the vicinity is Light emitting element 8 is 4.7, light emitting element 9 is 4.9, light emitting element 10 is 4.9, light emitting element 11 is 4.8, The light emitting element 12 was 5.0. From this, it can be seen that the light emitting elements 9 to 12 have a lower It was found that the device could be driven with low power consumption and was a good light-emitting device.

[0324] FIG. 1 shows the emission spectra when a current of 1 mA was applied to the fabricated light-emitting elements 8 to 12. In FIG. 26, the horizontal axis indicates the emission wavelength (nm) and the vertical axis indicates the emission intensity. The maximum light emission intensity is shown as a relative value. It was found that both of them exhibited good blue luminescence due to the luminescent substance PCBAPA. Ta.

[0325] Next, the time-normalized luminance characteristics of each element are shown in Figure 27. The horizontal axis is time (h) and the vertical axis is normalized luminance. The initial brightness is 1000cd / m 2 The current density is set to constant. When these elements were driven, as shown in Figure 27, the reliability of each element showed similarly good characteristics. In FIG. 27, the graph appears to have a single locus, but it is the same for each light-emitting element (light-emitting element 8). 1 to 12) follow almost the same trajectory.

[0326] In the light-emitting elements 8 to 12, the triarylamine derivative described in Embodiment 1 acts as an acceptor. It has been found that the above-mentioned organic compound can be suitably used for the hole injection layer 111 together with the photosensitive material. The optical element 12 can be used for both the hole injection layer 111 and the hole transport layer 112 at the same time. This has made it easier to fabricate devices and has improved material utilization. The efficiency of use was also improved. EXAMPLES

[0327] A compound of a material with high hole transport properties and an acceptor substance such as molybdenum (VI) oxide is When the composite material is used in the hole injection layer of a light-emitting device, it can be used as a material for forming an electrode regardless of the work function. However, when light is to be emitted from the anode side, In this case, the light that passes through the composite material is emitted to the outside of the light-emitting element, so the absorption characteristics of the composite material In some cases, this may have an adverse effect on the light emitting element.

[0328] NPB and αNBA1BP, which is the triarylamine derivative described in embodiment 1, The wavelength-transmittance characteristics when co-evaporated with molybdenum oxide (VI) are shown in Figure 28. In the figure, the horizontal axis indicates the wavelength (nm) and the vertical axis indicates the transmittance (%). NPB: Molybdenum oxide (VI ), and αNBA1BP:molybdenum(VI) oxide were adjusted to a mass ratio of 4:1. The films were vacuum-deposited on quartz substrates. The thickness of each film was 50 nm. The spectra were The transmission spectrum of

[0329] As shown in Figure 28, the composite film using NPB has a broad spectrum from 420 to 550 nm. Absorption from 420 to 550 nm is in the blue to green emission region. When this composite material is used in a light-emitting element that emits blue to green light, it absorbs the emitted light. However, this may have a negative effect on chromaticity and luminous efficiency. It can be seen that the absorption of the film made of has a broad absorption on the longer wavelength side than 700 nm. However, since the absorption region is not in the visible light region, the effect on the light emitting element is small.

[0330] In this way, αNBA1BP, which is the triarylamine derivative described in embodiment 1, The composite material co-evaporated with molybdenum(VI) oxide has low absorption of visible light. It was found that the present invention can be suitably used in any light-emitting element that emits visible light. [Industrial Applicability]

[0331] The triarylamine derivative according to one embodiment of the present invention has a large energy gap or ground state. The energy difference between the triplet excited state and the triplet excited state (hereinafter referred to as the triplet energy) is Therefore, it can be used as a host material for a light-emitting element that provides blue fluorescence or a light-emitting element that provides green phosphorescence. In addition, it can be very suitably used as a carrier transport material (particularly a hole transport material). In addition, the triarylamine derivative according to one embodiment of the present invention emits light in a wide range of the visible light range (blue to red). It can also be used as a host material or carrier transport material for light-emitting substances having wavelengths. In addition, in the process of forming the light-emitting element, Even if the host material or The type of carrier transport material can be unified, simplifying the process. The material utilization efficiency is also favorable. The body can be used as a luminescent material, in which case the energy gap as described above can be Because the wavelength is large, it is possible to obtain a light-emitting element with a sufficiently short wavelength and high color purity for blue light emission. The triarylamine derivative according to one embodiment of the present invention has the above-mentioned excellent Since the luminous efficiency of the light emitting element is excellent, the consumption In addition, it is possible to provide a light emitting device that consumes less power. Since blue light can also be emitted, the light-emitting device has excellent color reproducibility and high display quality. It is also possible to provide a lighting device with reduced power consumption, in which case It is possible to reduce the area and the thickness. [Explanation of symbols]

[0332] 101 Substrate 102 First electrode 103 EL layer 104 Second electrode 111 Hole injection layer 112 Hole transport layer 113 Light-emitting layer 114 Electron transport layer 501 First electrode 502 Second electrode 511 First Light Emitting Unit 512 Second Light Emitting Unit 513 Charge generation layer 601 Drive circuit section (source side drive circuit) 602 Pixel section 603 Drive circuit section (gate side drive circuit) 604 Sealing substrate 605 Sealing material 607 Space 608 Wiring 609 FPC (Flexible Printed Circuit) 610 Element Substrate 611 Switching TFT 612 Current Control TFT 613 First electrode 614 Insulation 616 EL layer 617 Second Electrode 618 Light-emitting element 623 n-channel TFT 624 p-channel TFT 901 Case 902 Liquid crystal layer 903 Backlight unit 904 Case 905 Driver IC 906 Terminal 951 Board 952 Electrode 953 Insulation Layer 954 Partition layer 955 EL layer 956 Electrode 1201 Source electrode 1202 Active layer 1203 Drain electrode 1204 Gate electrode 2001 Case 2002 light source 3001 Lighting equipment 9101 Case 9102 Support stand 9103 Display section 9104 Speaker section 9105 Video input terminal 9201 Main unit 9202 Case 9203 Display section 9204 Keyboard 9205 External connection port 9206 Pointing Device 9401 Main unit 9402 Case 9403 Display section 9404 Audio input section 9405 Audio output unit 9406 Operation key 9407 External connection port 9408 Antenna 9501 Main unit 9502 Display section 9503 Case 9504 External connection port 9505 Remote control receiver 9506 Image receiving unit 9507 Battery 9508 Audio input section 9509 Operation key 9510 Eyepiece

Claims

[Claim 1] A triarylamine derivative represented by the following general formula (G1): 【Chemistry 1】 In the formula, Ar represents a substituted or unsubstituted phenyl group or a substituted or unsubstituted biphenyl group, α represents a substituted or unsubstituted naphthyl group, and β represents a hydrogen atom or a substituted or unsubstituted naphthyl group. In addition, n and m each independently represent 1 or 2, and R 1 ~R 8 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or a phenyl group.

Citation Information

Patent Citations

  • Electrophotographic photoreceptor, process cartridge and electrophotographic apparatus

    JP1999184108A

  • Electroluminescent material, electroluminescent element and color transformation filter

    JP2001143869A

  • Organic electroluminescence element, material for organic electroluminescence element and display device

    JP2002249765A

  • Laminates for light-emitting components

    JP2008509565A

  • Organic electroluminescent element, and display device

    JP2010186983A