Cell pouch film having improved formability and method for preparing the same
The cell pouch film with specific surface roughness and elastic modulus, manufactured using a 1P3C process, addresses the cracking issue during high molding, enhancing formability and energy density for medium- and large-sized batteries.
Patent Information
- Application Number
- JP2024061644
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-06
- Filing Date
- 2024-04-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing cell pouch films face challenges in forming thick edge portions without cracking during high molding, which affects the formability and capacity of medium- and large-sized secondary batteries, particularly for applications like electric vehicles and energy storage systems.
A cell pouch film with a surface roughness of 1.5 μm or less on the barrier layer side and elastic modulus of 2450 N/mm² or less in the MD direction, combined with a 60 μm thickness barrier layer and 34 μm or more residual metal layer at the edge portion, is achieved through a 1P3C manufacturing process, ensuring excellent moldability.
The solution prevents cracking at the edge portion, allowing for thicker formation and improved energy density in secondary batteries, particularly suitable for medium- and large-sized batteries used in electric vehicles and energy storage devices.
Smart Images

Figure 2024149469000001_ABST
Abstract
Description
[Technical field]
[0001] The present specification relates to a cell pouch film having improved formability, a manufacturing method thereof, a cell pouch and a secondary battery using the same, and a manufacturing method thereof, and more particularly to a cell pouch film that can be formed thick without cracking at edges that arise during high forming of the secondary battery pouch film, and thus has excellent formability and is particularly suitable for medium and large batteries, a manufacturing method thereof, a cell pouch and a secondary battery using the same, and a manufacturing method thereof. [National research and development project that supported this invention] [Project unique number]1415185612 [Subject number] 20022450 [Department name] Ministry of Trade, Industry and Energy [Name of issue management (specialized) organization] Korea Institute for Industrial Technology Evaluation and Management [Research Project Name] Material Parts Package Type (Top Company) [Research title] Development of next-generation secondary battery pouches capable of achieving more than twice the adhesive strength (60℃) [Contribution rate] 1 / 1 [Name of project execution organization] Kurimura Chemical Co., Ltd. [Research period] 2023.01.01~2023.12.31 [Background technology]
[0002] Lithium secondary batteries (LiBs) have been used in many applications due to their various advantages such as high energy density and excellent output.
[0003] The cell pouch film is a multi-layered packaging laminate film that surrounds the electrodes and electrolyte of a cell such as a secondary battery, and is a key component material that determines the safety, life characteristics, and operational durability of the battery. It is required to have mechanical flexibility and strength, high oxygen / water vapor barrier properties, high thermal sealing strength, chemical resistance to the electrolyte, electrical insulation, and high temperature safety.
[0004] As the application of lithium secondary batteries expands from small to medium to large sizes for use in automobiles and ESS, cell pouch films are also required to have properties suitable for medium to large sizes, and in particular, they need to be highly safe and have excellent formability.
[0005] In relation to this, the cell size of lithium secondary batteries (LiB) for automobiles and the molding depth of the cell pouch are factors that greatly affect the capacity of the secondary battery. In the case of cell size, the size is larger than that of general small batteries and high molding is required, but since the molding depth of the cell determines the cell capacity, it can be said that the deeper the molding depth is, the essential condition for reaching the required capacity of 700Wh / L for next-generation secondary batteries.
[0006] Meanwhile, cell pouches are generally manufactured in the following order: the first process is to perform a surface treatment on one side of the metal layer, the second process is to perform a surface treatment on the other side of the metal layer, the third process is to laminate an outer layer on one side, and the fourth process is to laminate a sealant layer on the other side. In each process, coating, drying, winding, and other processes are repeated in sequence. However, in this case, there is an increased probability of running loss and process defects occurring when feeding the raw material, and improvements are required. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Republic of Korea Patent Publication No. 10-2016-0070468 [Patent Document 2] Republic of Korea Patent Publication No. 10-2022-0031820 Summary of the Invention [Problem to be solved by the invention]
[0008] In one aspect, an object of the present invention is to provide a cell pouch film and a secondary battery packaged with the same, which can suppress the occurrence of cracks at the edges during high molding of the cell pouch film, thereby making it possible to form thick edges. In one aspect, an object of the present invention is to provide a cell pouch film having excellent molding properties and a secondary battery packaged with the cell pouch film. [Means for solving the problem]
[0009] In an exemplary embodiment of the present invention, there is provided a cell pouch film (the cell pouch film according to claim 1) which is formed by sequentially laminating at least an outer layer, a barrier layer, and a sealant layer, and which has a surface roughness Ra of 1.5 μm or less on the peeled surface on the barrier layer side after peeling between the outer layer and the barrier layer of the cell pouch film.
[0010] In an exemplary embodiment of the present invention, a cell pouch film is provided, which is made by sequentially laminating at least an outer layer, a barrier layer, and a sealant layer, and the outer layer is laminated with nylon and polyethylene terephthalate (PET) and has an elastic modulus in the MD direction of 2450 N / mm 2 The elastic modulus in the TD direction is 2400 N / mm 2 The present invention provides a cell pouch film (the cell pouch film according to claim 2) which is as follows:
[0011] In an exemplary embodiment, the cell pouch film described in claim 1 and / or the cell pouch film described in claim 2 may be a cell pouch film (cell pouch film described in claim 3) in which the barrier layer has a thickness of 60 μm before molding and the remaining thickness of the metal layer at the edge of the cell pouch film measured as follows is 34 μm or more. [Measurement of remaining metal layer thickness at edge] A cell pouch film of 240 mm (MD) x 266 mm (TD) is formed using a molding machine, and after forming it to 12 mm, the edge part is cut using a cross-section cutting machine, and the maximum thickness of the metal layer cross section of the cell pouch film is measured using a SEM.
[0012] In an exemplary embodiment, the cell pouch film (the cell pouch film according to any one of claims 1 to 3) may be a cell pouch film (the cell pouch film according to claim 4) having a maximum molding depth of 16 mm or more, measured as follows. [Measurement of formability] The cell pouch film is cut into test pieces measuring 240mm (MD) x 266mm (TD), and the moldability is evaluated using a molding machine. The moldability is evaluated by measuring the maximum molding depth of the pouch formed without cracks in 10 measurements.
[0013] In an exemplary embodiment of the present invention, there is provided a method for producing the above-mentioned cell pouch film (the cell pouch film according to any one of claims 1 to 4), which includes a double-sided surface treatment step of performing a surface treatment on both sides of a metal raw material included in a barrier layer; a step of drying the metal raw material subjected to the double-sided surface treatment; an outer adhesive layer coating step of applying an adhesive to one side of the metal raw material subjected to the surface treatment to form an outer adhesive layer; and an outer layer lamination step of laminating an outer layer raw material on the outer adhesive layer, in which the drying temperature of the metal raw material after the double-sided surface treatment is 160°C or higher (the method for producing the cell pouch film according to claim 5).
[0014] In an exemplary embodiment, the method (the method for manufacturing a cell pouch film as described in claim 5) may include a step of first laminating nylon and polyethylene terephthalate (PET) films, and then laminating the laminated nylon and polyethylene terephthalate (PET) films with aluminum as a barrier layer (the method for manufacturing a cell pouch film as described in claim 6).
[0015] In an exemplary embodiment, in the method (the method for manufacturing a cell pouch film as described in claim 5 or 6), the double-sided surface treatment step may be a method in which, after surface treatment on one side of the metal raw material, surface treatment on the other side of the metal raw material is immediately performed without performing a drying step (the method for manufacturing a cell pouch film as described in claim 7).
[0016] In an exemplary embodiment, in the method (the method for manufacturing a cell pouch film described in any one of claims 5 to 7), the drying step may be a method of drying the metal raw material having surface treatments applied to both sides using a floating method (the method for manufacturing a cell pouch film described in claim 8).
[0017] In an exemplary embodiment, in the method (the method for manufacturing a cell pouch film according to any one of claims 5 to 8), the double-sided surface treatment step may include performing a first coating on one side of the metal raw material web by applying a water-based and solvent-based coating liquid by a combined method of direct coating and RKC (Reverse Kiss Coating), and performing a second coating on the other side of the metal raw material web by applying a coating liquid by a method of RKC and film up / down coating (the method for manufacturing a cell pouch film according to claim 9).
[0018] In an exemplary embodiment, the method (the method for manufacturing a cell pouch film according to any one of claims 5 to 9) may include a step of performing a first winding after the outer layer lamination step; a step of forming an inner adhesive layer on the other side of the surface-treated metal raw material on which the outer layer is not laminated after the first winding; a step of laminating a sealant layer raw material under the inner adhesive layer; and a step of performing a second winding after laminating the sealant layer raw material (the method for manufacturing a cell pouch film according to claim 10).
[0019] In an exemplary embodiment of the present invention, there is further provided a cell pouch made of the above-mentioned cell pouch film (the cell pouch film according to any one of claims 1 to 4) or a secondary battery packaged using the same (the secondary battery according to claim 11).
[0020] In addition, in an exemplary embodiment of the present invention, there is provided a method for manufacturing a secondary battery (a method for manufacturing a secondary battery as described in claim 12), which includes the step of exteriorizing a secondary battery with the above-mentioned cell pouch film (a cell pouch film as described in any one of claims 1 to 4). Effect of the Invention
[0021] In an exemplary embodiment of the present invention, the edge portion of the pouch film for secondary batteries can be thickened by suppressing the occurrence of cracks at the edge portion during high forming of the pouch film for secondary batteries, thereby providing a pouch film for secondary batteries having excellent forming characteristics. Such a cell pouch film can improve the energy density of the secondary battery, and is therefore particularly useful as a medium- to large-sized pouch film for electric vehicles, energy storage devices, etc. [Brief description of the drawings]
[0022] [Figure 1] 1 is a schematic cross-sectional view of a cell pouch film according to an exemplary embodiment of the present invention; [Diagram 2] 1 is a schematic diagram of a cell pouch film manufacturing apparatus according to an exemplary embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Definition of Terms In this specification, singular expressions may include plural expressions unless the context clearly indicates otherwise. In this application, the terms "comprise" or "have" are intended to indicate the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and do not exclude the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0024] In this specification, terms such as first, second, etc. are used to refer to features separated from one another, but not to a particular order, unless otherwise specified.
[0025] In this specification, the expression "formed on" a particular layer includes not only direct formation on the layer, but also formation via another additional layer.
[0026] In this specification, the term "cell" refers to a battery, and has the broadest meaning including all types of batteries such as secondary batteries such as lithium ion batteries and lithium polymer batteries, and portable storage batteries.
[0027] In this specification, the term "cell pouch" or "cell pouch film" refers to a cell pouch in which cell components such as a positive electrode, a negative electrode, and a separator are impregnated with an electrolyte and housed, and has the broadest meaning including all laminated films processed into a bag or box shape in consideration of gas barrier properties, bendability, electrolyte resistance, thermal adhesiveness, etc., to house the cell components.
[0028] In this specification, the term "final structure" refers to the final layer structure of the cell pouch film. This final structure may vary slightly depending on the types of various manufacturing processes. For example, the final structure may consist of an outer cover substrate (or outer layer), a first adhesive layer, an outer surface treatment layer, a reference substrate (or barrier layer), an inner surface treatment layer, a second adhesive layer, and an inner cover substrate (or sealant layer). Or, the final structure may consist of an outer cover substrate (or outer layer), a first adhesive layer, an outer surface treatment layer, a reference substrate (or barrier layer), an inner surface treatment layer, an extrusion coating layer, and an inner cover substrate (or sealant layer). Or, the final structure may consist of an outer cover substrate (or outer layer), a first adhesive layer, an outer surface treatment layer, a reference substrate (or barrier layer), an inner surface treatment layer, a second adhesive layer, an extrusion coating layer, and an inner cover substrate (or sealant layer).
[0029] In this specification, the intermediate structure refers to a structure formed during the manufacturing process of the cell pouch film, and various intermediate structures of the cell pouch may be produced depending on the manufacturing process. For example, a first intermediate structure may be produced that is composed of an outer cover substrate (or outer layer), a first adhesive layer (or outer adhesive layer), an outer surface treatment layer, a reference substrate (or barrier layer), an inner surface treatment layer, and a second adhesive layer (or inner adhesive layer). Alternatively, a second intermediate structure may be produced that is composed of an outer cover substrate (or outer layer), a first adhesive layer (or outer adhesive layer), an outer surface treatment layer, a reference substrate (or barrier layer), and an inner surface treatment layer.
[0030] In this specification, an in-line process refers to a roll-to-roll process in which the web makes one pass between the unwinder and the rewinder (take-up roll).
[0031] In this specification, one rewind does not mean that the take-up roll rotates once (the take-up roll may of course rotate multiple times), but rather that the film is wound onto the take-up roll and completes the first run. Thus, two rewinds mean that the film completes the first run, then starts running again and completes the second run during the manufacturing process.
[0032] In this specification, the raw material may refer to the material of the barrier layer or metal layer provided during the manufacturing process.
[0033] In this specification, the functional base fabric may mean a resin base fabric that forms a sealant layer and / or an outer layer.
[0034] In this specification, the edge portion means a corner of a molded portion. For example, during molding, a pouch is manufactured into a rectangular cup shape with dimensions of 185 mm (X axis) x 85 mm (Y axis) x 12 mm (Z axis). The edge portion means a portion from the tip of the corner of the rectangular cup to 0.5 mm x 0.5 mm x 0.5 mm.
[0035] In this specification, the release surface on the barrier layer side does not mean the metal surface itself that is the material of the barrier layer, but means the surface (release surface) on the barrier layer side on which a part of the substance peeled off from the outer layer film side remains after peeling when the outer layer of the cell pouch film and the barrier layer are peeled off. Therefore, the surface roughness of the release surface on the barrier layer side does not mean the surface roughness of the metal surface itself that is the material of the barrier layer, but the surface roughness of the release surface on the barrier layer side on which the substance (residue) that was peeled off from the outer layer film and remained on the barrier layer side remains. The surface roughness of the release surface caused by the residue is different from the surface roughness of the metal layer surface itself.
[0036] Description of exemplary embodiments Hereinafter, exemplary embodiments of the present invention will be described in detail. Since cracks are likely to occur at the edges during high molding of the cell pouch film, it is difficult to make the edges thick. In other words, how thick the edges can be made can be a measure for evaluating high moldability. How thick the edges can be made can be evaluated by the remaining thickness of the barrier layer at the edge after molding (thickness after molding), as described below.
[0037] The inventors discovered that the surface roughness of the peeled surface when the outer layer and barrier layer of the cell pouch film are peeled off and / or the elastic modulus in the MD direction and the elastic modulus in the TD direction of the outer layer of the cell pouch film, which is a laminate of nylon and PET, are related to the thickness of the edge portion during high-precision molding and the resulting high-precision moldability, and after extensive research, they arrived at the present invention.
[0038] Specifically, in an example embodiment of the present invention, the cell pouch film has a surface roughness Ra of 1.5 μm or less on the barrier layer side after peeling between the outer layer of the cell pouch film and the barrier layer.
[0039] In non-limiting examples, the surface roughness Ra may be 0.82 to 1.5 μm or 0.82 to 1.13 μm. In non-limiting examples, the surface roughness Ra may be 1.49 μm or less, 1.48 μm or less, 1.47 μm or less, 1.46 μm or less, 1.45 μm or less, 1.44 μm or less, 1.43 μm or less, 1.42 μm or less, 1.41 μm or less, 1.40 μm or less, 1.39 μm or less, 1.38 μm or less, 1.37 μm or less, 1.36 μm or less, 1.35 μm or less, 1. 34μm or less, 1.33μm or less, 1.32μm or less, 1.31μm or less, 1.30μm or less, 1.29μm or less, 1.28μm or less, 1.27μm or less, 1.26μm or less, 1 .25μm or less, 1.24μm or less, 1.23μm or less, 1.22μm or less, 1.21μm or less, 1.20μm or less, 1.19μm or less, 1.18μm or less, 1.17μm or less, 1.16μm or less, 1.15μm or less, 1.14μm or less, 1.13μm or less, 1.12μm or less, 1.11μm or less, 1.10μm or less, 1.09μm or less, 1.08μm or less , 1.07μm or less, 1.06μm or less, 1.05μm or less, 1.04μm or less, 1.03μm or less, 1.02μm or less, 1.01μm or less, 1.0μm or less, 0.99μm or less , 0.98 μm or less, 0.97 μm or less, 0.96 μm or less, 0.95 μm or less, 0.94 μm or less, 0.93 μm or less, 0.92 μm or less, 0.91 μm or less, 0.90 μm or less, 0.89 μm or less, 0.88 μm or less, 0.87 μm or less, 0.86 μm or less, 0.85 μm or less, 0.84 μm or less, 0.83 μm or less, or 0.82 μm.
[0040] If the surface roughness Ra of the barrier layer side after peeling between the outer layer and the barrier layer of the cell pouch film exceeds 1.5 μm, as can be confirmed from the experimental example described later, the remaining aluminum thickness at the edge after forming to 12 mm becomes insufficient and the formability also deteriorates.
[0041] The surface roughness of the barrier layer side may be adjusted by the manufacturing process described below, and is thought to be affected in particular by the drying temperature in the drying chamber after double-sided surface treatment in the 1P3C process and / or whether or not nylon and PET are separately laminated, the MD and TD elastic moduli of nylon / PET, etc.
[0042] In an exemplary embodiment, in the cell pouch film, the outer layer formed by laminating nylon and PET preferably has an elastic modulus of 2450 or less in the MD direction and an elastic modulus of 2400 or less in the TD direction.
[0043] The elastic modulus in the MD direction and the TD direction was evaluated as follows. That is, the cell pouch film is cut into pieces measuring 150 mm x 1.5 mm (two pieces of MD and TD specimens are prepared) using a specimen cutter, and then the Ny / PET is manually peeled off from the pouch. The elastic modulus of each specimen is then evaluated using a universal testing machine (UTM). The evaluation conditions for the elastic modulus are speed: 50 mm / min, grip gap: 50 mm, and evaluation is performed at room temperature of 25°C and humidity of 30%. The evaluation of the elastic modulus is determined using the slope of the elastic modulus section in the SS curve.
[0044] In non-limiting examples, the elastic modulus in the MD direction of the outer layer formed by laminating nylon and PET may be 2450 or less, 2400 or less, 2350 or less, 2300 or less, 2250 or less, 2200 or less, 2150 or less, 2100 or less, or 2050 or less. Alternatively, it may be 2000 or more, 2050 or more, 2100 or more, 2150 or more, 2200 or more, 2250 or more, 2300 or more, 2350 or more, or 2400 or more. If the elastic modulus in the MD direction is lower than the above range, resistance to external impact may be reduced.
[0045] If the elastic modulus in the MD direction of the outer layer formed by laminating nylon and PET exceeds 2450, moldability may deteriorate, as will be seen from the experimental examples described later.
[0046] In non-limiting examples, the elastic modulus in the TD direction of the outer layer formed by laminating nylon and PET may be 2400 or less, 2350 or less, 2300 or less, 2250 or less, 2200 or less, 2150 or less, 2100 or less, or 2050 or less. Alternatively, it may be 2000 or more, 2050 or more, 2100 or more, 2150 or more, 2200 or more, 2250 or more, 2300 or more, or 2350 or more. If the elastic modulus in the MD direction is lower than the above range, resistance to external impact may be reduced.
[0047] If the elastic modulus in the TD direction of the outer layer formed by laminating nylon and PET exceeds 2400, moldability may deteriorate, as will be seen from the experimental examples described later.
[0048] The MD and TD moduli of the outer layer formed by laminating nylon and PET may also be adjusted depending on the manufacturing process. Even if the same materials are used, they are considered to be affected by factors such as the drying temperature in the drying chamber after double-sided surface treatment in the 1P3C process and / or whether or not nylon and PET are laminated separately.
[0049] In an illustrative embodiment, the remaining thickness of the metal layer at an edge portion of the cell pouch film (thickness of the metal layer before molding is 60 μm) measured as follows may be 34 μm or more, 34.5 μm or more, 35 μm or more, 35.5 μm or more, 36 μm or more, 36.5 μm or more, 37 μm or more, 37.5 μm or more, 38 μm or more, 38.5 μm or more, 39 μm or more, or 39.5 μm or more, for example, 34 to 40 μm. [Measurement of remaining metal layer thickness at edge] A 240mm (MD) x 266mm (TD) cell pouch film is molded using a chrome (Cr) coated one-cup molding machine, and after molding to 12mm, the edge is cut using a cross-section cutting machine, and the maximum thickness of the cross-section of the metal layer in the pouch film, i.e., the remaining thickness, is measured using a SEM. Here, the thickness of the metal layer in the pouch film before molding is 60μm.
[0050] In an exemplary embodiment, the maximum forming depth of the cell pouch film measured as described below may be 16 mm or more, 16.5 mm or more, 17 mm or more, 17.5 mm or more, 18 mm or more, 18.5 mm or more, 19 mm or more, 19.5 mm or more, 20 mm or more, 20.5 mm or more, 21 mm or more, 21.5 mm or more, or 22 mm. [Measurement of formability] The moldability of a 240mm (MD) x 266mm (TD) cell pouch film is measured using a chrome (Cr)-coated one-cup molding machine. The measurement was carried out 10 times, and the maximum forming depth formed without cracks was evaluated. The pressure during forming was fixed at 0.3 MPa, and the R value (corner curvature radius value) of the forming machine was 4R (4 mm). The forming size during forming was 90 mm wide x 120 mm, and single forming was performed.
[0051] Meanwhile, referring to FIG. 1, an exemplary embodiment of the present invention may include a sealant layer 500; an inner adhesive layer 400 laminated on the sealant layer 500; a barrier layer 300 laminated on the inner adhesive layer 400; an outer adhesive layer 200 laminated on the barrier layer 300; and an outer layer 100 formed on the outer adhesive layer 200.
[0052] In an exemplary embodiment, the outer layer 100 of the cell pouch film may be nylon, PET (polyethylene terephthalate), PBT (polybutylene terephthalate), etc., and may preferably be composed of a mixed layer of nylon and PET (a laminate film of nylon and PET).
[0053] In an exemplary embodiment, the nylon film of the outer layer 100 has a thickness of preferably 20 μm or more, more preferably 25 μm or more, from the viewpoint of formability, but if the thickness of the nylon film exceeds 30 μm, the dielectric breakdown voltage may decrease. Therefore, the preferred thickness of the nylon film may be 20 μm to 30 μm, preferably 25 μm to 30 μm. If the nylon film is less than 20 μm, the formability may be deteriorated.
[0054] In an exemplary embodiment, the thinner the PET film and the thicker the nylon film of the outer layer 100, the more advantageous the formability. In addition, the thinner the PET film, the more disadvantageous it may be in terms of breakdown voltage. From this viewpoint, the thickness of the PET film is preferably 7 μm to 12 μm.
[0055] In an exemplary embodiment, the PET film may have MD and TD elongations of 90-110%, 95-105%, or 100%, respectively. The nylon film may have MD elongations of 100-200%, 110-150%, or 110-125%, and TD elongations of 70-200%, 70-150%, or 74-138%. For example, when the MD elongation of the nylon film is about 125%, the TD elongation may be about 75%, or when the MD elongation is about 110%, the TD elongation may be about 138%.
[0056] In an example embodiment, the sealant layer 500 may include a thermal adhesive resin, i.e., a sealing resin for thermal adhesion. Specifically, the sealant layer may include at least one selected from the group consisting of polyolefins such as polypropylene (PP) and polyethylene (PE), copolymers, terpolymers or derivatives thereof, and ethylene vinyl acetate (EVA). The copolymer or terpolymer may include an ethylene / propylene copolymer or an ethylene / propylene / butadiene terpolymer. In one embodiment, the sealant layer may have a thickness of 20 to 100 μm or 20 to 80 μm. The sealant layer may be composed of a plurality of layers. The thickness of the polypropylene (CPP) layer of the sealant layer 500 may be, for example, 20 to 80 μm.
[0057] As an example, the sealant layer 500 may be made of a polypropylene layer (PP), such as a non-oriented polypropylen (CPP) film, and the polypropylene layer (PP) and the barrier layer may be bonded via an adhesive coating layer and / or an extrusion coating (EC) layer of a polypropylene-based resin. The sealant layer 500 itself may be formed by extrusion. The polypropylene layer (PP) may contain various additives (rubbers, elastomers, slip agents, etc.) depending on the required physical properties.
[0058] In an example embodiment, the outer adhesive layer 200 is an adhesive layer for adhering the barrier layer 300 and the outer layer 100 .
[0059] In example embodiments, the outer adhesive layer 200 may include one or more of an epoxy adhesive, a polyurethane adhesive, a phenolic resin adhesive, a polyolefin adhesive, and a polyester adhesive. In one embodiment, the outer adhesive layer may have a thickness of 0.5 μm to 10 μm.
[0060] In example embodiments, the inner surface adhesive layer 400 may be an adhesive coating layer or an extrusion coating layer for bonding the barrier layer 300 and the sealant layer 500. Alternatively, in another embodiment, the inner surface adhesive layer may include an adhesive coating layer and an extrusion coating layer.
[0061] The inner adhesive layer 400 may include one or more of an epoxy-based adhesive, a polyurethane-based adhesive, a phenolic resin-based adhesive, a polyolefin-based adhesive, and a polyester-based adhesive. In one embodiment, the inner adhesive layer 400 may have a thickness of 0.5 μm to 10 μm. In one embodiment, the extrusion resin layer may improve the bendability, adhesiveness, insulation, etc. of the pouch. In one embodiment, the extrusion coating layer may include an olefin-based resin such as a polypropylene-based resin. In one embodiment, the extrusion coating layer may have a thickness of about 5 to 80 μm.
[0062] In example embodiments, the barrier layer 300 may include a metal layer or a surface treatment layer uniformly coated on both sides of the metal layer, and the metal layer may be a thin metal film or a metal deposition layer. The thin metal film may be a metal foil. The metal deposition layer may be formed by vacuum-depositing a metal on a separate plastic film, for example, a film of polyethylene terephthalate (PET), polyethylene (PE), or polypropylene (PP).
[0063] In one embodiment, the metal of the metal layer is not particularly limited as long as it has the above-mentioned barrier properties, and examples thereof include at least one selected from the group consisting of aluminum (Al), iron (Fe), copper (Cu), nickel (Ni), tin (Sn), zinc (Zn), indium (In), and tungsten (W) (single metal or mixture of single metals), or an alloy of two or more selected from the group consisting of aluminum or its alloy, titanium or its alloy, tungsten or its alloy, molybdenum or its alloy, copper or its alloy, and stainless steel. More specifically, it may include aluminum. In one embodiment, the surface treatment layer may be a surface treatment layer made of phosphate, chromium, zirconium, cerium, lanthanum, scandium, yttrium, etc. to provide corrosion resistance of the metal.
[0064] In one embodiment, the barrier layer 300 may have a thickness of 20 μm to 80 μm. If the thickness of the barrier layer is less than 20 μm, pinholes, microcracks, etc. may occur during processes such as molding, making it difficult to ensure safety, and if the thickness of the barrier layer is more than 80 μm, the energy density may be low during battery fabrication. In one illustrative embodiment, the total thickness of the cell pouch film may be, for example, 60 to 185 μm. In one embodiment, the cell pouch film may be 153 μm or more or 113 μm or less.
[0065] Meanwhile, in an exemplary embodiment of the present invention, there is provided a method for manufacturing the above-mentioned cell pouch film, the method including: a double-sided surface treatment step of performing a surface treatment on both sides of a metal raw material included in a barrier layer; a step of drying the metal raw material having been subjected to the double-sided surface treatment; an outer adhesive layer coating step of applying an adhesive to one side of the metal raw material having been subjected to the surface treatment to form an outer adhesive layer; and an outer layer lamination step of laminating an outer layer raw material on the outer adhesive layer; and the drying temperature of the metal raw material after the double-sided surface treatment is 160°C or more.
[0066] In this regard, the conventional technology generally includes a step of i) coating one side of a metal layer with a surface treatment layer, drying the layer, and winding the layer up (first winding step), coating the other side of the metal layer with another surface treatment layer, drying the layer, and winding the layer up again (second winding step); ii) forming an outer adhesive layer on one side of the surface-treated metal layer, laminating an outer layer, drying the layer, and winding the layer up (third winding step); and iii) forming an inner adhesive layer on the other side of the surface-treated metal layer, laminating a sealant layer, and drying the layer. When multiple steps are repeated in this manner, not only the probability of running loss and process defects increases, but also the moldability may deteriorate.
[0067] Therefore, in an exemplary embodiment of the present invention, unlike the conventional method of manufacturing a film for a cell pouch by sequentially repeating processes such as coating, drying, and winding for each layer lamination process, the film is manufactured by a 1P3C (1 Pass 3 Coating) method in which three or more coating processes can be performed in one run of the raw roll in a single in-line process, thereby solving the problems of the conventional technology and improving formability.
[0068] In an exemplary embodiment, the method may include the steps of first laminating nylon and polyethylene terephthalate (PET) films; and laminating the laminated nylon and polyethylene terephthalate (PET) films with a metal layer, preferably aluminum, which is a barrier layer.
[0069] More specifically, in a typical Solvent Dry Lamination (SDL) process, nylon film is laminated onto a barrier layer (usually made of aluminum) in the first step, and then polyethylene terephthalate (PET) film is laminated on top of that in the second step. At this time, since aluminum, being a metal, does not have a good elongation rate, it is laminated with as much tension as possible to prevent thermal shrinkage of nylon. However, the nylon film, which has already been stretched at this time, will already have high resistance to pulling when made into a pouch. This can result in a decrease in excellent formability.
[0070] In contrast, when the 1P3C process is adopted and the nylon film and PET film are pre-laminated, the outer layer formed by the laminate of the nylon film and PET film is then laminated with a barrier layer (laminating with the nylon film side facing the barrier layer), the formability may be superior to that of the process described above.
[0071] Furthermore, in the case where the metal raw material included in the barrier layer is dried after surface treatment on both sides (step (5) in Figure 2), the formability may be better if the drying temperature, i.e., the temperature of the drying chamber, is 160°C or higher. In a non-limiting example, the temperature of the drying chamber may be 160° C. to 200° C. Within this range, there is no significant difference in the physical properties of the produced film.
[0072] For example, the temperature of the drying chamber may be 160°C or more, 165°C or more, 170°C or more, 175°C or more, 180°C or more, 185°C or more, 190°C or more, 195°C or more, or 200°C or less, 195°C or less, 190°C or less, 185°C or less, 180°C or less, 175°C or less, 170°C or less, 165°C or less. If the chamber temperature is lower than the above range, the effect of the surface treatment may be particularly reduced and the physical properties after the surface treatment (such as outer layer peel strength and electrolytic resistance) may be reduced. Such a tendency may be more pronounced, especially when the temperature is 140°C or less.
[0073] In one exemplary embodiment, the method may include laminating the laminated nylon and polyethylene terephthalate (PET) film with a barrier layer, and then laminating a resin for forming a sealant layer, such as a polypropylene (PP) resin film, on the opposite side of the laminated nylon and polyethylene terephthalate (PET) film.
[0074] In an exemplary embodiment, the method may include a double-sided coating step of performing a surface treatment by applying a first and second coating to both sides of a metal layer serving as a barrier layer; a coating step of applying an adhesive to both sides of the surface-treated metal layer and drying the applied adhesive; and a step of laminating a resin film and an outer layer film (a laminate film of nylon and PET) for forming the above-mentioned sealant layer to both sides of the metal layer to which the adhesive has been applied and dried.
[0075] In one embodiment, the two-sided surface treatment step may be performed by a two-sided double coating means including a first coater and a second coater, in which the other side of the metal web is immediately treated without a drying step after the surface treatment of one side of the metal web.
[0076] In one embodiment, the double-sided surface treatment step may include performing a first coating on one side of the metal web by applying a water-based or solvent-based coating liquid by a combined direct coating and reverse kiss coating (RKC) method, and performing a second coating on the other side of the metal web by applying a coating liquid by a RKC and film up / down coating method.
[0077] Specifically, the first coating is performed by applying water-based and solvent-based coating liquids by a first coater in a combined method of direct coating and reverse kiss coating (RKC), so that the physical properties and changes of the coating liquid can be taken into consideration. The other side of the metal roll may be subjected to a second coating by applying a coating liquid by RKC and film up / down coating. Meanwhile, the position of the substrate contact surface forming the outer layer, the coating roll, and the doctor can be adjusted, so that the coating uniformity and the work speed can be improved. More specifically, a chamber method (sealed piping) is configured to precisely control the coating agent, so that the viscosity of the coating agent can be adjusted and the inflow of foreign matter can be fundamentally blocked.
[0078] In one embodiment, the double-sided surface treatment step may more specifically include a web supplying process for unwinding and supplying a wound metal web; a foreign matter removing process for removing foreign matter present on the surface of the supplied metal web; a tension adjusting process for adjusting the tension of the metal web from which the foreign matter on the surface has been removed; and a double-sided coating process for coating both sides of the metal web while maintaining a constant tension.
[0079] In one embodiment, the foreign matter removal process may include a first foreign matter removal process of removing oil by performing an electric discharge treatment on both sides of the metal web. The foreign matter removal process may further include a pinhole inspection process of checking whether pinholes have occurred on both sides of the metal web from which the oil has been removed. The foreign matter removal process may further include a second foreign matter removal process of removing foreign matter occurring on both sides of the metal web after the pinhole inspection by a roll method.
[0080] In addition, the method according to an embodiment may further include a property stabilization drying step of drying the metal raw material having both surfaces treated in a floating manner between the both surface treatment step and the outer adhesive layer coating step to stabilize the physical properties. According to the floating method, both sides of the metal raw material having the surface treatment can be dried simultaneously, and contact between the roll and the raw material can be minimized, so that the occurrence of poor appearance runnability such as transfer of foreign matter due to the roll and puncture of the raw material can be significantly reduced.
[0081] In one embodiment, the drying step in the method may be to stabilize the physical properties and dry the metal web having both sides surface-treated in a floating manner. That is, an air floating method may be applied so that the web having both sides surface-treated can be dried in a non-contact manner while floating. In this way, the metal web coated on both sides can be dried while minimizing contact with components such as a feed roll. Then, the method may further include a cooling step of cooling the dried metal web and a surface inspection step of inspecting the surface of the cooled metal web.
[0082] In one embodiment, the outer adhesive layer coating step of coating one side of the surface-treated metal roll with an adhesive to form an outer adhesive layer is a process of coating one side of the metal roll that has been surface-treated by two coatings, and may be performed by a third coater, and is prepared for lamination through processes such as drying. After coating the adhesive, the metal roll on which the adhesive is coated is dried to form an adhesive layer, and the thickness of the dried adhesive layer is measured, and the surface of the adhesive layer is corona-treated to strengthen the adhesive force.
[0083] In one embodiment, the method may further include forming an inner adhesive layer on the other side of the metal sheet where the outer layer is not laminated after the laminating step. Also, in one embodiment, the method may further include a drying step after the inner adhesive layer forming step. In one embodiment, the method may further include laminating a sealant layer sheet under the inner adhesive layer.
[0084] In one embodiment, the method may include a total of two or less winding steps until the final structure of the cell pouch is manufactured in order to prevent punctures and / or indentations from occurring in the raw material used in each step up to the outer layer lamination step. Specifically, it is most preferable to manufacture the final structure of the cell pouch film by a total of two or less winding steps, more preferably a total of one winding step.
[0085] In one embodiment, the winding step may be performed after the outer layer lamination step or after the sealant layer lamination step. For example, the winding step may be performed in step (10) in FIG. 2.
[0086] In one embodiment, the lamination step of laminating an outer layer raw material on the outer adhesive layer and the step of laminating a sealant layer raw material under the inner adhesive layer are processes of laminating a functional raw material on one side of a metal raw material coated with an adhesive, and the inner side may be laminated with a sealant layer raw material for mainly stabilizing the heat resistance and cold resistance of the battery, and the outer side may be laminated with an outer layer raw material for heat resistance, pinhole resistance, abrasion resistance, etc. In one embodiment, each lamination step may be a step of laminating a previously prepared outer layer raw material or a sealant raw material.
[0087] In one embodiment, between the third coating step and the laminating step, an adhesive drying step of drying the adhesive-coated metal substrate to form an adhesive layer; an adhesive layer thickness measuring step of measuring the thickness of the dried adhesive layer; and an adhesive layer surface treatment step of corona-treating the surface of the adhesive layer to enhance adhesive strength may be further included.
[0088] In one embodiment, the method may further include a surface inspection step of inspecting the surfaces of the sealant layer and the outer layer after the lamination step.
[0089] In one embodiment, in order to minimize the occurrence of foreign matter and scratches during the process of feeding each raw web, both a Tendency structure in which the substrate contact roll and the shaft are separated and movable, and an integrated movable shaft structure may be applied to the guide roll. A general driving method of the guide roll is a mechanism in which the rotation from the motor is transmitted to the guide roll with the shaft integrated therewith to drive it at a 1:1 speed, whereas the Tensile driving method is a mechanism in which the guide roll and the shaft are separated to mutually correct the rotation speed of the fine rolls, and may be appropriately applied in the required section. As an example, a rewinder unit and an unwinder unit (raw web supply unit) may be separately configured so that they can be operated separately when a problem occurs in the operation of the equipment.
[0090] In addition, in one embodiment, a suction roll may be applied in the tension control section to minimize the generation of foreign matter and scratches during the feeding of the raw web, and a contact type clean roll may be applied to remove foreign matter generated during the running of the web and prevent the foreign matter from adhering to the roll and causing poor appearance (punctures, scratches, etc.).
[0091] Meanwhile, in an exemplary embodiment of the present invention, a maturing step may be further included. The maturing step is a step necessary for improving the reliability of adhesive strength, electrolyte resistance, peel strength, etc., during the manufacture of the cell pouch, but since it takes a somewhat long time, an optimal maturing step is essential. It is preferable in terms of productivity to manufacture the product through only one maturing step for the final structure of the cell pouch. Specifically, the method may include two or less maturing steps. More specifically, the method may apply an adhesive to one side of the surface-treated metal raw material without a maturing step after the both-side surface treatment step, and the maturing step may be included after the lamination step of the outer layer and / or sealant layer. For example, if a maturing step is included in the both-side surface treatment step before the lamination step, the film in the middle of the manufacturing process may be exposed to air for a certain period of time or more, and the surface treatment agent that is not laminated may be desorbed. For example, if a maturing step is included in the adhesive layer formation step, a blocking phenomenon may occur in which the adhesive layer is partially reacted and then adheres to another layer.
[0092] Meanwhile, in an exemplary embodiment of the present invention, a manufacturing apparatus for a film for a cell pouch may be provided, which includes a double-sided surface treatment means including a first coater 3 and a second coater 4 for performing a surface treatment on both sides of a metal raw material forming a barrier layer, a third coater 7 for applying an adhesive to one side of the metal raw material that has been subjected to the surface treatment, and a laminating unit 9 for laminating a functional raw material on one side of the adhesive layer. Figure 2 is a schematic diagram of a manufacturing apparatus for a film for a cell pouch according to an embodiment of the present disclosure.
[0093] In one embodiment, the double-sided surface treatment means may include a web supply unit 1, a foreign matter removal unit 2, a tension adjustment unit, a first coater 3, and a second coater 4. The web supply unit 1 unwinds and supplies a wound metal web. The foreign matter removal unit 2 removes foreign matter present on the surface of the supplied metal web. The tension adjustment unit adjusts the tension of the metal web from which the foreign matter on the surface has been removed. The first coater 3 and the second coater 4 coat both sides of the metal web while maintaining a constant tension.
[0094] In one embodiment, the foreign matter removing means 2 may include a primary foreign matter removing unit that performs discharge treatment on both sides of the metal web to remove oil. Also, it may further include a pinhole inspection unit that checks for pinholes on both sides of the metal web from which the oil has been removed. If no abnormality is found as a result of the inspection, it may further include a secondary foreign matter removing unit that removes foreign matter generated on both sides of the metal web by a roll method.
[0095] In one embodiment, a property stabilization drying unit 5 may be provided between the double-sided surface treatment means and the third coater 7, which dries the metal web coated on both sides in a floating manner to stabilize the property. In this case, the drying method may be an air floating method so that the coated substrate can be dried in a non-contact manner while floating. This allows the metal web coated on both sides to be dried while minimizing contact with components such as a feed roll. Then, the dried metal web may be cooled by a cooling unit 6, and the surface of the cooled metal web may be inspected by a surface inspection unit.
[0096] In one embodiment, the adhesive drying unit 8 may be further provided between the third coater 7 and the laminating unit 9, for drying the adhesive-coated metal substrate to form an adhesive layer; an adhesive layer measuring unit for measuring the thickness of the dried adhesive layer; and an adhesive layer surface treatment unit for corona-treating the surface of the adhesive layer to enhance adhesive strength.
[0097] In one embodiment, the laminating unit 9 may further include a surface inspection unit for inspecting the surfaces of the sealant layer and the outer layer.
[0098] According to one embodiment, the film for cell pouches may be manufactured by the manufacturing apparatus shown in Fig. 2. In one embodiment, a fourth coater (not shown) that applies adhesive to the other side of the metal raw material that has been surface-treated, a drying unit (not shown), a functional raw material (outer layer, sealant layer) lamination unit (not shown), an extrusion unit (including co-extrusion) (not shown), etc. may be added as necessary between the lamination unit 9 and the final rewind unit (End, 2nd Rewind) in Fig. 2.
[0099] Meanwhile, in an exemplary embodiment of the present invention, a secondary battery packaged with the above-mentioned cell pouch film is provided. The secondary battery may be a lithium secondary battery, and may be a medium- to large-sized secondary battery for electric vehicles (EVs) and energy storage systems (ESSs).
[0100] In addition, an exemplary embodiment of the present invention provides a method for manufacturing a secondary battery, the method including: packaging a secondary battery with the cell pouch film. EXAMPLES
[0101] The illustrative embodiments of the present invention will be described in more detail through the following examples. However, the embodiments disclosed herein are merely illustrative and are not to be construed as being limited to the embodiments disclosed herein, as the present invention may be embodied in various forms.
[0102] [Experimental Method] <Production of Examples and Comparative Examples> The pouch films of the examples and comparative examples are laminated with an outer layer, a barrier layer, and a sealant layer, the outer layer being a laminate film of an outermost polyethylene terephthalate (PET) film (thickness 12 μm) and an inner nylon (Ny) film (thickness 25 μm), the barrier layer being made of aluminum (thickness 60 μm), and the sealant layer being a polypropylene layer (thickness 80 μm). The total thickness, including the thickness of the adhesive layer, is 183 μm.
[0103] The Examples and Comparative Examples were manufactured in the same manner, except that the method of bonding the outer layer of the pouch film was different as follows, and the temperature of the drying chamber in the drying process after both sides were surface-treated ((5) in Figure 2) was different as shown in Table 1 below.
[0104] First, the pouch film of the comparative example was laminated with a metal layer as an outer layer by the solvent dry lamination (SDL) method. Specifically, a surface treatment agent was coated on both sides of the aluminum layer, which was the metal layer, and then nylon, which was the outer layer, was primarily laminated on top of that, and PET was then secondarily laminated on top of that. The drying temperature after the surface treatment was 140°C or more and 150°C or less. Next, a polypropylene (PP) layer, which was the inner layer (sealant layer), was extruded to manufacture a pouch film. In this process, since nylon on the aluminum, which is a hard metal, is prone to thermal shrinkage, the nylon was laminated with as much tension as possible to prevent thermal shrinkage.
[0105] On the other hand, the pouch film of the embodiment was prepared by laminating the already laminated nylon film and PET film to the aluminum in one step (laminating the nylon film facing the aluminum), and then extruding and laminating a polypropylene (PP) layer as an inner layer (sealant layer) on the opposite side. The drying temperature after the surface treatment was 160°C or higher.
[0106] [Table 1]
[0107] Each pouch film was produced with dimensions of 240 mm (MD) x 266 mm (TD).
[0108] The peeling and the peeled surface roughness on the barrier layer side, the remaining aluminum thickness at the edge, and the maximum forming depth for evaluating the formability in the examples and comparative examples were evaluated as follows.
[0109] <Peeling> A pouch film measuring 2.5 cm (TD) x 15 cm (MD) was immersed in a container containing an electrolyte, and the container was then sealed. The sealed container was placed in an oven at 85°C and left for one day, after which the pouch film that had been immersed in the electrolyte was taken out and cut to a size of 1.5 cm (TD) x 15 cm (MD) to prepare a sample.
[0110] A shallow cut was made only in the outer layer so as not to damage the barrier layer, and then the metal layer and part of the peeled sealant layer were peeled off using a universal testing machine (UTM). The sample was then attached flat to a glass slide using double-sided tape, and again the sample was pulled using the universal testing machine (UTM) to peel off more than 30 mm, with both ends held so that the metal layer and the peeled sealant layer were at an angle of 180 degrees (speed 50 mm / min).
[0111] <Surface roughness measurement> The metal (aluminum) layer side of the peeled sealant layer is 1×1 cm 2 The sample was cut to size and attached flat to a glass slide using double-sided tape. The surface was photographed using a surface roughness measuring device (NV-2200 3D profiler, Nano System). The Ra in the histogram column was measured using an analysis program (NanoMap, Nano System) based on the obtained data.
[0112] <Measurement of the elastic modulus of the outer layer (nylon / PET)> After cutting the cell pouch film to a size of 150mm x 1.5mm using a specimen cutter (2 MD and 2 TD specimens were cut), the Ny / PET was manually peeled off from the pouch. The elastic modulus was then evaluated using a universal testing machine (UTM). The evaluation conditions for the elastic modulus were speed: 50mm / min, grip gap: 50mm, and the evaluation was performed at room temperature of 25℃ and humidity of 30%. The elastic modulus was evaluated using the slope of the elastic modulus section in the SS curve.
[0113] <Measurement of formability and remaining aluminum thickness at edges after forming> A cell pouch film of 240 mm (MD) x 266 mm (TD) was molded using a chromium (Cr)-coated one-cup molding machine, and its moldability and the remaining aluminum thickness at the edge were evaluated. The formability results were evaluated as the maximum forming depth at which the molding was complete without cracks in all 10 measurements. The pressure during molding was fixed at 0.3 MPa, and the R value (corner curvature radius value) of the molding machine was 4R (4 mm). The forming size during molding was 90 mm wide x 120 mm long, and single forming was performed.
[0114] The remaining thickness of the aluminum at the edge after molding was evaluated by molding 12 mm, cutting the edge with a cross-section cutter, and measuring the thickness of the aluminum (maximum thickness, remaining thickness after molding) after cross-sectional evaluation of the aluminum in the pouch film using an SEM. Measuring the remaining thickness of the aluminum at the edge of the pouch film (thickness after molding) in this way is because the remaining thickness of the barrier layer after molding has the greatest effect on moldability.
[0115] The evaluation results of the peel surface roughness Ra, outer layer elastic modulus (nylon / PET elastic modulus), remaining aluminum thickness at the edge (unit: μm), and formability (unit: mm) of the pouch films of the examples and comparative examples are shown in Tables 2 to 5, respectively.
[0116] [Table 2]
[0117] [Table 3]
[0118] [Table 4]
[0119] [Table 5]
[0120] As can be seen from these tables, compared to the comparative examples in which the peeled surface roughness Ra on the barrier layer side after peeling the outer layer and barrier layer exceeds 1.5 μm, the examples in which the surface roughness Ra is 1.5 μm or less have a larger remaining aluminum thickness at the edge after forming and are far more excellent in formability. Furthermore, in the examples in which the MD elastic modulus of the outer layer formed by laminating nylon and PET is 2450 or less, and in which the TD elastic modulus of the outer layer formed by laminating nylon and PET is 2400 or less, the remaining aluminum thickness at the edge after molding is greater than in the comparative examples, and the examples are found to have far superior moldability.
[0121] Although non-limiting and exemplary embodiments of the present invention have been described above, the technical concept of the present invention is not limited to the accompanying drawings or the above description. It is obvious to those skilled in the art that various modifications can be made without departing from the technical concept of the present invention, and such modifications are within the scope of the claims of the present invention.
Claims
1. A cell pouch film, At least an outer layer, a barrier layer, and a sealant layer are laminated in this order, A cell pouch film, characterized in that after peeling between an outer layer of the cell pouch film and a barrier layer, the surface on the peeled surface side of the barrier layer has a surface roughness Ra of 1.5 μm or less.
2. A cell pouch film, At least an outer layer, a barrier layer, and a sealant layer are laminated in this order, The outer layer, which is made by laminating nylon and polyethylene terephthalate (PET), has an MD elastic modulus of 2450 N / mm 2 The elastic modulus in the TD direction is 2400 N / mm 2 A cell pouch film characterized by the following:
3. The barrier layer has a thickness of 60 μm before molding, 3. The cell pouch film according to claim 1, wherein the remaining thickness of the metal layer at the edge of the cell pouch film is 34 μm or more, as measured as follows. [Measurement of remaining metal layer thickness at edge] A cell pouch film of 240 mm (MD) x 266 mm (TD) is formed by a molding machine, and after forming to 12 mm, the edge portion is cut by a cross-section cutting machine, and the maximum thickness of the cross section of the metal layer of the cell pouch film is measured using a SEM.
4. 4. The cell pouch film according to claim 3, wherein the maximum forming depth of the cell pouch film measured as described below is 16 mm or more. [Measurement of moldability] The cell pouch film is cut into test pieces measuring 240 mm (MD) x 266 mm (TD), and the moldability is evaluated using a molding machine. The moldability is evaluated by measuring the maximum molding depth of the pouch formed without cracks in 10 measurements.
5. A method for producing the cell pouch film according to claim 1 or 2, a double-sided surface treatment step of performing a surface treatment on both sides of the metal raw material included in the barrier layer; drying the metal sheet having been subjected to the surface treatment on both sides; An outer adhesive layer coating step of applying an adhesive to one side of the surface-treated metal sheet to form an outer adhesive layer; and an outer layer lamination step of laminating an outer layer raw material onto the outer adhesive layer; Including, A method for producing a cell pouch film, characterized in that the drying temperature of the metal raw material after both sides are surface-treated is 160°C or higher.
6. The method for producing a cell pouch film according to claim 5, further comprising the steps of: first laminating nylon and polyethylene terephthalate (PET) films; and laminating the laminated nylon and polyethylene terephthalate (PET) films with a barrier layer.
7. 6. The method for manufacturing a cell pouch film according to claim 5, wherein in the double-sided surface treatment step, after the surface treatment on one side of the metal web, the surface treatment on the other side of the metal web is immediately performed without a drying step.
8. 6. The method of claim 5, wherein the drying step comprises drying the metal sheet having both sides surface-treated by a floating method.
9. In the double-sided surface treatment step, a first coating is performed on one side of the metal sheet by applying a water-based or solvent-based coating liquid using a direct coating method and a reverse kiss coating method (RKC).
6. The method of claim 5, further comprising: applying a coating liquid to the other side of the metal roll by RKC and film up / down coating.
10. The method comprises: performing a first winding after the outer layer lamination step; forming an inner adhesive layer on the other side of the surface-treated metal web, on which the outer layer is not laminated, after the first winding; laminating a sealant layer sheet under the inner adhesive layer; and The method for producing a cell pouch film according to claim 5, further comprising the step of: performing a second winding after laminating the sealant layer web.
11. A secondary battery, which is packaged with the cell pouch film according to claim 1 or 2.
12. A method for manufacturing a secondary battery, comprising: A method for manufacturing a secondary battery, comprising: packaging a secondary battery with the cell pouch film according to claim 1 or 2.
Citation Information
Patent Citations
Method for manufacturing outer packaging material for lithium ion battery
JP2012238453A
Lithium ion secondary battery exterior material
JP2017126565A
Outer casing material for electricity storage devices, and electricity storage device using said outer casing material
WO2016181867A1
Casing for power storage device, and power storage device
WO2022131190A1
Cell pouch and method of manufacturing the same
KR1020160070468A