Sodium-ion batteries
By optimizing the C/A mass balance and using disordered carbon-containing anodes in sodium ion batteries, the anode capacity and cycling stability are enhanced, addressing safety and efficiency issues in sodium ion batteries.
Patent Information
- Application Number
- JP2024103664
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2018-12-13
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing sodium ion batteries face challenges in achieving high anode active material capacity and stable cycling characteristics, with issues such as sodium deposition leading to decreased coulombic efficiency and safety risks due to dendrite formation.
Optimizing the cathode to anode mass ratio (C/A mass balance) within the range of 0.833 to 2.70, using disordered carbon-containing materials for the anode with a mass less than 80 g/m² and thickness of 100 μm or less, and employing specific cathode active materials like TiS₂ and hard carbon composites to enhance anode capacity and stability.
The optimized C/A mass balance and anode structure result in significantly improved anode capacity and cycling stability, reducing sodium deposition risks and enhancing safety, with capacities up to 379 mAh/g and high cycling stability, independent of electrolyte and binder composition.
Smart Images

Figure 2024149486000001_ABST
Abstract
Description
[Technical field]
[0001] The present application relates to sodium-ion batteries that exhibit excellent anode active material capacity and stable cycling characteristics. Also provided herein are methods for making these sodium-ion secondary batteries, and batteries that include such sodium-ion secondary batteries. [Background technology]
[0002] Sodium-ion batteries are similar in many ways to the lithium-ion batteries commonly used today. Both are reusable, secondary batteries that contain an anode (negative electrode), a cathode (positive electrode), and an electrolyte material, and both are capable of energy storage and can be charged and discharged through similar reaction mechanisms. When a sodium-ion (or lithium-ion) battery is charged, Na + (or Li + ) ions deintercalate from the cathode and are inserted into the anode, while charge-balancing electrons pass from the cathode through an external circuit that includes the charger to the anode of the battery. During discharge, the same process occurs in reverse.
[0003] In recent years, lithium-ion battery technology has attracted much attention and is the preferred portable battery for most electronic devices in use today. However, lithium is not a cheap source of metal and is a concern due to its high cost for large-scale applications. On the other hand, sodium-ion battery technology is believed to offer many advantages. Sodium is much more abundant than lithium and is expected to provide a cheaper and more durable method for future energy storage, especially for large-scale applications such as storing energy in the power grid. Currently, research is underway to make sodium-ion batteries practical.
[0004] One area that requires more attention is the design of sodium-ion batteries to optimize their electrochemical performance.
[0005] WO 2017 / 073056 describes a method of passive voltage control in sodium-ion batteries as a way to achieve a useful secondary sodium battery. Specifically, the method includes controlling the ratio of the mass of negative active material to the mass of positive active material to be greater than 0.37 and less than 1.2. This corresponds to a cathode:anode active material mass ratio (referred to herein as the "C / A mass balance") in the range of 0.833 to 2.70. Although not explicitly disclosed in WO 2017 / 073056, collaboration with the inventors of this technology reveals that they have achieved a 100-130 gm per square meter anode substrate. -2 It is understood that the anode contains a negative electrode active material of Summary of the Invention [Problem to be solved by the invention]
[0006] It is an object of the present invention to provide a sodium-ion secondary battery that exhibits excellent anode and cathode active material capacity, as well as stable cycling characteristics. The sodium-ion secondary battery of the present invention is also cost-effective and easy to manufacture. To this end, applicants have unexpectedly discovered that while using a C / A mass ratio in the range of 0.833 to 2.70 is one way to provide a sodium-ion secondary cell with useful anode first desodiumation capability, these anode capacities can be further increased by selecting the C / A ratio in combination with other selected cell construction parameters. Below, applicants describe and demonstrate these surprising results. [Means for solving the problem]
[0007] Therefore, in the present invention, A sodium ion secondary battery having a cathode and an anode, the cathode having one or more positive active materials and the anode having a layer, preferably a uniform layer, of negative active material disposed on an anode substrate; the negative electrode active material comprises one or more disordered carbon-containing materials; i) The mass of the layer of the negative electrode active material is expressed in units of m 2 Each serving is 80g or less. ii) the ratio of the mass of the layer of positive electrode active material to the mass of the layer of negative electrode active material is from 0.1 to 10; iii) There is provided a sodium ion secondary battery, wherein the thickness of the layer of the negative electrode active material on the anode substrate is 100 μm or less, preferably 80 μm or less.
[0008] For clarification, the unit "gm -2 " (grams / square meter) is the mass per unit area of the substrate (m 2 ) and is also referred to herein as "GSM."
[0009] As used herein, an "anode electrode active material" is equivalent to an "negative electrode active material," and a "cathode electrode active material" is equivalent to a "positive electrode active material."
[0010] As shown in the following specific examples, the ratio of the mass of the cathode and anode electrode active materials is important. However, the applicant has found that the mass of the anode electrode active material has a greater control on the anode capacity results, and for a constant mass of the cathode electrode active material, significantly improved anode capacity results have been observed as the mass of the anode active material decreases. Also, the applicant has found that the mass of the anode electrode active material is not as high as 80 g because of the possibility of Na electrodeposition problems. -2It has been found that it is undesirable to use a mass of anode electrode active material exceeding 10 ... -2 Super, 80gm -2 The best anode initial sodium removal capacity results were obtained when the mass of the negative electrode active material layer per square meter of the anode substrate was 40 gm -2 From 75gm -2 , preferably 40gm -2 From 65gm -2 and at the same time, the highest cycling stability (i.e., the least capacity fade per unit cycle) is obtained when the mass of negative electrode active material per square meter is within these latter two ranges.
[0011] In particularly preferred sodium ion secondary batteries according to the present invention, the ratio of the mass of the positive electrode active material to the mass of the layer of the negative electrode active material (i.e., C / A mass balance) is 0.5 to 10, preferably 1.0 to 10, more preferably 1 to 5, ideally 2.0 to 3.5, and particularly preferably 2.0 to 2.75. Sodium ion batteries having a C / A mass balance within these preferred ranges exhibit extremely high anode first sodium removal capacity and provide the unexpected advantage of excellent cycle stability. The most preferred sodium ion batteries are those having a C / A ratio in the range of 2.05 to 2.90 and an anode electrode active material mass within the described preferred ranges.
[0012] During the manufacture of secondary battery cells, it is common to form a layer of anode or cathode electrode active material on a substrate, such as a current collector foil, and then "calendar" the coated substrate by passing the coated substrate through a series of rollers to obtain a uniform thickness of electrode material on the substrate. In a typical sodium-ion battery, the calendered thickness of the anode electrode active material ranges from 100 μm to 140 μm, and the thickness of the cathode electrode active material ranges from 80 to 110 μm. Surprisingly, the applicant has found that for layers of anode electrode active material of similar density, there is a clear relationship between the ability of sodium ions to be transported into the anode electrode active material during intercalation and deintercalation and the thickness of the anode electrode active material. In particular, the applicant has observed that a thin layer of anode electrode active material results in a disproportionately and unexpectedly high anode first desodium capacity compared to a thicker layer of anode electrode material having a comparable density. The thickness of the layer of negative electrode active material on the anode substrate used in the sodium ion secondary battery of the present invention is the value mentioned above, ie ≦100 μm, preferably ≦80 μm.
[0013] Sodium-ion secondary batteries according to the present invention may have any known positive electrode active material capable of inserting and removing sodium ions. Suitable examples include metal sulfide compounds such as TiS2, metal oxide compounds, phosphate-containing compounds, polyanion-containing compounds, Prussian blue analogues, and nickelate or non-nickelate compounds of the following general formula: A 1±δ M 1 V M 2 W M 3 X M 4 Y M 5 Z O 2-c Where: A is one or more alkali metals selected from sodium, potassium and lithium; M 1 has one or more redox-active metals in the oxidation state +2, preferably one or more redox-active metals in the oxidation state +2 selected from nickel, copper, cobalt, and manganese; M 2 has an oxidation state greater than 0 and a metal in an oxidation state of +4 or greater; M 3 has a metal in the +2 oxidation state, M 4 has a metal with an oxidation state greater than 0 and less than or equal to +4; M 5 has a metal in the +3 oxidation state, Where: 0≦δ≦1; V>0; W ≥ 0; X ≥ 0; Y ≥ 0; At least one of W and Y is greater than 0, Z ≥ 0; C is in the range of 0≦c<2, where V, W, X, Y, Z and C are selected to maintain electrochemical neutrality.
[0014] Ideally, metal M 2 has one or more transition metals, preferably selected from manganese, titanium and zirconium; M 3 preferably has one or more transition metals selected from magnesium, calcium, copper, tin, zinc and cobalt; M 4 has one or more transition metals, preferably selected from manganese, titanium and zirconium; M 5 is preferably one or more selected from aluminum, iron, cobalt, tin, molybdenum, chromium, vanadium, scandium and yttrium. Cathode active materials having any crystal structure may be used, preferably the structure is O3 or P2, or derivatives thereof. In particular, the cathode material may have a mixture of phases, i.e., a heterogeneous structure containing several different crystal forms.
[0015] As mentioned above, the negative active material anode is a carbon-based material with a disordered structure, and advantageously, such a material lends itself to the insertion and extraction of sodium ions during the charge / discharge process. The exact structure of the preferred carbon material has yet to be elucidated, but it is generally ideal if it has a non-graphitizable, non-crystalline, amorphous carbon structure. Although hard or soft carbon may be used, anodes comprising one or more "hard carbon" materials are particularly preferred. Although "hard carbon" has layers, these layers are not stacked in an orderly fashion, but rather have micropores / nanopores (micron- or nano-sized pores) formed between the disorderly stacked carbon layers. At a macroscopic level, hard carbon is isotropic. Typically, hard carbon suitable for use in the anode may be produced from a carbon-containing starting material (e.g., sucrose, biomass, corn starch, glucose, organic polymers (e.g., polyacrylonitrile or resorcinol-formaldehyde gel), cellulose, petroleum coke, coal tar, or pitch coke) that is first mixed with a thermoplastic binder such as a synthetic resin and then heated to about 1200° C. Commercially available hard carbons include those sold by Kureha Corporation, Kuraray Chemical Co., and Kureha Corporation.
[0016] In the sodium-ion cells according to the invention, the disordered carbon-based anode material may be used alone or in combination with any other suitable negative electrode (anode) active material (referred to as additional material) capable of storing sodium ions. Such additional materials may include metals, metal-containing compounds, metal alloys, non-metals, and non-metal-containing compounds. These include Na 15 Sn4, Na3Sb, Na3Ge, and Na 15The high capacity anode is defined as comprising Pb4 or a composite with one or more other materials, such as non-metals, metals, or metal alloys, capable of storing sodium ions as described above. The metals or non-metals may be in elemental or compound form. Particularly preferred anode active materials include hard carbon / X composites, where X is one or more selected from phosphorus, sulfur, indium, antimony, tin, lead, iron, manganese, titanium, molybdenum, and germanium. It is preferred that this is in elemental or compound form and has one or more selected from oxygen, carbon, nitrogen, phosphorus, sulfur, silicon, fluorine, chlorine, bromine, and iodine. Preferably, X is one or more selected from P, S, Sn, SnO, SnO2, SnF2, Fe2O3, Fe3O4, MoO3, TiO2, Sb, Sb2O3, SnSb, and SbO.
[0017] Secondary carbon-containing materials may also be used in combination with the aforementioned anode active materials to improve anode conductivity. Examples include activated carbon materials, particulate carbon black materials, graphene, carbon nanotubes, and graphite, among others. Examples of particulate carbon black materials include carbon black materials having a BET nitrogen surface area of about 62 m 2 / g, or BET nitrogen surface area of about <900 m 2 / g, preferably having a BET nitrogen surface area of about 770 m 2 / g. These are available commercially from Imerys Graphite and Carbon Corporation as specialty carbons for rubber compositions. 2 Carbon nanotubes with a BET nitrogen surface area of 2630 m / g, typically 2 / g and a surface area of >3000 m 2 Activated carbon materials having a BET nitrogen surface area of 100 / g may also be used.
[0018] Surprisingly, the anode substrate has a surface area of ≦80 gm per square meter. -2It is observed that the positive effect on the anode first desorption capacity as a result of using a mass of negative active material of 0.1 to 10, a C / A mass balance in the range of 0.1 to 10, and a thickness of negative active material on the anode substrate of ≦100 μm is maintained regardless of the composition of the electrolyte used in the cell and regardless of the type of binder used in fabricating the anode electrode. These observations are verified in the specific examples presented below.
[0019] According to the applicant, when the sodium ion secondary battery of the present invention is charged and the anode is sodiated, the potential (V) on the y-axis versus Na / Na + A graph of anode active material capacity (mAh / g) on the x-axis against Na shows a steep negative slope "gradient" region (starting at about 1.20-1.30 V at 0 mAh / g and rising to 0.10 V vs Na / Na + >0.10 V vs. Na / Na + ), it is noted that a "plateau" region that is substantially parallel to the X-axis is obtained. Importantly, as the mass and thickness of the active material on the anode decreases, the capacity resulting from the "plateau" region increases significantly compared to the capacity resulting from the "slope" region. Moreover, applicants have found that the relationship between decreasing anode active material mass and increasing anode specific capacity is linear. It is noteworthy that the thickness of the active material on the anode directly affects the reversible capacity of a sodium-ion battery, and it is believed to be the first time such a phenomenon has been recognized.
[0020] In this application, the "plateau capacity" is defined as the capacity at 0.15 V (vs. Na / Na) in the desodium curve of a hard carbon anode. + ) in the 3E cell at a constant current cycling rate of C / 10. On the other hand, the "gradient capacity" is defined as the capacity contribution from ~0.15 to 2 V vs. Na / Na in the 3E cell at a rate of C / 10. + The active capacity of the desodium-treated hard carbon anode during
[0021] In particular, the sodium-ion secondary battery of the present invention preferably has a particular range of plateau:slope capacity ratio of 0 to 6:1, more preferably 0.5 to 5:1, and advantageously 1 to 5:1. The most preferred plateau:slope capacity ratio is 1.2 to 5.0:1, and ideally 1.4 to 4.75:1.
[0022] Thus, the sodium-ion secondary battery of the present invention is characterized by a plateau:slope reversible capacity ratio of the anode electrode active material, derived from a plot between anode active material capacity (mAh / g) (x-axis) and cell potential (V) versus Na / Na+ (y-axis) of 0 to 6:1, preferably 0.5 to 5:1, more preferably 1 to 5:1, particularly preferably 1.2 to 5.0:1, and ideally 1.4 to 4.75:1, measured in a three or four or more electrode full cell configuration. A plateau reversible capacity of 0 mAh / g can be obtained by cycling the cell so that it does not reach the plateau region, for example by selecting a light C / A mass balance and / or de-rating the cell, for example, from 3.7 to 1.V. A P:S ratio of 0 means that all of the capacity contribution is due to the slope region.
[0023] In another aspect, the present invention provides a battery having at least two sodium-ion secondary cells as described above, preferably at least three sodium-ion cells.
[0024] In yet another embodiment, the present invention provides A method for producing the sodium ion secondary battery according to any one of the preceding claims, a. assembling a cathode having one or more positive electrode active materials with an anode having an anode substrate coated with a layer of negative electrode active material, and an electrolyte to form a sodium ion battery; b. cycling the sodium ion battery to a first voltage; having i) the mass of the layer of anode active material is 80 gm per square meter of the anode substrate; -2is as follows: ii) the ratio of the mass of the positive electrode active material to the mass of the layer of the negative electrode active material is 0.1 to 10; iii) a thickness of the layer of the negative electrode active material on the anode substrate is 100 μm or less.
[0025] Applicant has discovered another interesting and useful phenomenon, which can be used to further improve the performance of sodium-ion secondary batteries. When a sodium-ion secondary battery undergoes its first charge / discharge cycle, an irreversible loss of about 20% is observed in the capacity of a hard carbon anode. A similar irreversible capacity is observed for layered oxide active cathode materials. This is known as the "first cycle loss" of the cell. Conventional cell preparation procedures eliminate the effect of the "first cycle loss" (so that it does not appear in commercial cells) by employing a formation cycle that applies a voltage (typically C / 10 at 4.20-1.00 V) during the first four cell formation cycles, and then uses a lower or the same voltage in the subsequent ("post" or "operation") cell cycles (e.g., C / 5 at 4.00-1.00 V, 4.10-1.00 V, or 4.20-1.00 V). As with the treatment of the first cycle loss, this procedure is known to extend the life of the cell. Surprisingly, the applicant has found that an additional positive effect on post-formation cycle stability is observed. This is observed when the "post" formation cycle (i.e. when the cell is in operation) is "de-rated", i.e. the "post" formation cycle is carried out at C / 5 from 4.00 to 1.00 V, or at C / 5 from 4.10 to 1.00 V, instead of at C / 5 from 4.20 to 1.00 V. The applicant has also observed that by carrying out the formation cycle at C / 10 from 4.00 to 1.00 V (or at C / 10 from 4.10 to 1.00 V), instead of at C / 10 from 4.20 to 1.00 V, a significant improvement in the cathode and anode capacity during the "post-formation" (operation) cycle is obtained. Details of these observations are given in the specific examples below.
[0026] As discussed above and as demonstrated in the specific examples below, applicants have found that the low GSM effect of hard carbon does not result as a result of changes in the active material (type of hard carbon), binder or electrolyte, but rather occurs solely as a result of the GSM of the hard carbon used in the anode electrode, the C / A mass balance, and the thickness of the anode material.
[0027] In another embodiment of the present invention, there is provided a sodium ion secondary battery having a cathode and an anode, the cathode comprises one or more positive active materials and the anode comprises a layer, preferably a uniform layer, of a negative active material disposed on an anode substrate; the layer of negative electrode active material comprises one or more disordered carbon-containing materials; (i) The mass of the layer of the negative electrode active material is expressed in units of m 2 Each serving is ≦80g, (ii) the ratio of the mass of the layer of positive electrode active material to the mass of the layer of negative electrode active material is from 0.1 to 10; (iii) the thickness of the layer of the negative electrode active material on the anode substrate is ≦100 μm, preferably ≦80 μm; (iv) The layer of negative electrode active material has a volume specific surface area (VSSA) of more than about 0.8, preferably more than 0.8 to 500, particularly preferably 0.8 to 400, ideally 0.8 to 300, and particularly 0.8 to 200. A sodium ion secondary battery is provided.
[0028] In another aspect, the present invention provides a sodium ion secondary battery having a cathode and an anode, the cathode comprises one or more positive active materials and the anode comprises a layer, preferably a uniform layer, of a negative active material disposed on an anode substrate; the layer of negative electrode active material comprises one or more disordered carbon-containing materials; The layer of the negative electrode active material has a volume specific surface area (VSSA) of more than 0.8, preferably more than 0.8 to 500, particularly preferably 0.8 to 400, ideally 0.8 to 300, and particularly 0.8 to 200, thereby providing a sodium ion secondary battery.
[0029] The present invention will now be described with reference to the drawings. [Brief description of the drawings]
[0030] [Figure 1] Figure 1 shows the anodic profile for cycle 1 in a 3E full cell in terms of potential (V vs Na / Na+) versus active specific capacity of the anode (mAh / g) using a nickelate-based NaNiMnMgTiO cathode and a commercial hard carbon anode (available from Kuraray). Several different masses of anode active material were used, as listed in Table 1. [Diagram 2] FIG. 14 shows the effect of using different electrolytes on the anodic profile for cycle 1 in a 3E full cell in terms of potential (V vs Na / Na+) versus the active specific capacity (mAh / g) of the anode using a nickelate-based NaNiMnMgTiO cathode and a commercial hard carbon anode (available from Kuraray) with similar active GSM values. [Diagram 3] FIG. 14 shows the effect of using a commercial hard carbon derived from anthracite on the anodic profile for cycle 1 in a 3E full cell in terms of potential (V vs Na / Na+) versus active specific capacity of the anode (mAh / g) over a range of anode activity GSMs using a nickelate-based NaNiMnMgTiO cathode. [Figure 4]FIG. 14 shows the effect of commercial biomass-derived hard carbon on cycle 1 anodic profile in a 3E full cell in potential (V vs Na / Na+) versus active specific capacity of the anode (mAh / g) across two different anode active GSMs using a nickelate-based NaNiMnMgTiO cathode. [Diagram 5] Figure 14 shows the effect of using an aqueous binder in a hard carbon anode on the anodic profile for cycle 1 in a 3E full cell in terms of potential (V vs Na / Na+) versus active specific capacity of the anode (mAh / g) across two different anode active GSMs using a nickelate based NaNiMnMgTiO cathode and a commercial hard carbon anode (available from Kuraray). [Figure 6] FIG. 1 shows a plot of anode active specific capacity (mAh / g) versus cycle number to demonstrate the long term cycling performance in a 3E full cell using a nickelate based NaNiMnMgTiO cathode and a commercial hard carbon anode (available from Kuraray) with different anode active GSM and C / A mass balance. [Figure 7] FIG. 1 shows a plot of cathode active specific capacity (mAh / g) versus cycle number to show the long term cycling performance in a 3E full cell using a nickelate based NaNiMnMgTiO cathode and a commercial hard carbon anode (available from Kuraray) with different anode active GSM and C / A mass balance. [Figure 8] FIG. 1 shows a graph of anode active specific capacity (mAh / g) versus cycle number to illustrate the effect of derating and voltage window formation on the cathode (nickelate-based NaNiMnMgTiO) and anode active specific capacity and cycling stability using a commercial hard carbon anode (available from Kuraray). [Figure 9] FIG. 1 shows a graph of potential (V vs. Na / Na+) versus anode active specific capacity (mAh / g) to illustrate what happened to the anode profile in cycle 1 and cycle 4 at constant anode activity GSM and near constant C / A mass balance value using a 3E full cell with a nickelate-based NaNiMnMgTiO cathode and a commercial hard carbon anode (available from Kuraray). [Figure 10] Figure 1 shows the extended cycling of a 1 Ah full cell FPC180905 with an anode having 54.20 GSM anode electrode active material and a C / A mass balance of 2.71. The cathode is a nickelate-based NaNiMnMgTiO material and the anode is a commercial hard carbon (available from Kuraray). [Figure 11] FIG. 1 shows a graph of anode active specific capacity (mAh / g) versus anode active GSM using a 3E full cell with a nickelate-based NaNiMnMgTiO cathode and a commercial hard carbon anode (available from Kuraray Co., Ltd.), and the effect of anode active GSM on initial cycle stability. [Figure 12] FIG. 1 shows a graph of anode active specific capacity (mAh / g) versus C / A mass balance using a 3E full cell with a nickelate-based NaNiMnMgTiO cathode and a commercial hard carbon anode (available from Kuraray Co., Ltd.), and the effect of C / A mass balance on initial cycle stability. [Figure 13] FIG. 1 shows a graph between cathode active specific capacity (mAh / g) and cycle number for a sodium-ion battery having NaFeMnMgCuO cathode material and a commercial hard carbon (available from Kuraray) 40.25 GSM active anode. [Figure 14]Figure 1 shows a plot of potential (V vs Na / Na+) versus anode active specific capacity (mAh / g) for two cells using HC / Fe2P anode active material and a nickelate-based Na0.833Ni0.317Mn0.467Mg0.1Ti0.117O2 cathode. The anode active specific capacity of these cells is compared when the active anode material was used at a mass of 74.27 gm-2 in one cell (PCFA614) and at a mass of 55.25 gm-2 in the other cell (711042). [Figure 15] Figure 1 shows a plot of potential (V vs Na / Na+) versus anode active specific capacity (mAh / g) for a 3E full cell performance using HC anode active material and a nickelate-based NaNiMnMgTiO2 cathode. The anode active material is used at a mass of 52.2 gm-2 and a mass balance of 1.596 is used for the cell. [Figure 16] Figure 1 shows a plot of potential (V vs Na / Na+) versus anode active specific capacity (mAh / g) for a 3E full cell performance using HC anode active material and a pre-sodiated TiS2 cathode. The anode active material is used at a mass of 62.9 gm-2 and a mass balance of 0.918 is used for the cell. [Figure 17] Figure 1 shows a plot of anode active specific capacity (mAh / g) versus potential (V vs Na / Na+) for the performance of a cell using HC anode active material and an oxygen-deficient nickelate-based NaNiMnMgTiO-δ cathode. The anode active material is used at a mass of 52.9 gm-2 and a mass balance of 2.86 is used for the cell. [Figure 18] FIG. 1 shows a plot of capacity retention (%) versus cycle number on first charge for two 3E full cells according to the invention (A3PC268 and AC3PC238) and two comparative 3E full cells (A3PC231 and A3PC225). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] (Method of manufacturing a sodium ion battery according to the present invention) A sodium ion battery according to the present invention was fabricated using the following exemplary method.
[0032] The positive electrode is prepared by solvent casting a slurry of active material, conductive carbon, binder, and solvent onto a substrate. The conductive carbon used is commercially available from Timcal. The binder is polyvinylidene fluoride (PVdF) and the solvent is N-methyl-2-pyrrolidone (NMP). The slurry is cast onto aluminum foil and heated until most of the solvent evaporates, forming an electrode film. The electrode is then dried under dynamic vacuum at about 120°C. The electrode film has the following composition, expressed as weight percent: 89% active material (doped nickelate-containing composition), 5% conductive carbon, and 6% PVdF binder.
[0033] The negative electrodes are prepared by solvent casting a slurry of hard carbon active material (e.g., commercially available from Kuraray), conductive carbon, binder, and solvent onto a substrate. The conductive carbon used is commercially available, e.g., from Timcal. PVdF was used as the binder (unless otherwise noted in a particular example), and N-methyl-2-pyrrolidone (NMP) was used as the solvent. The slurry is cast onto aluminum foil and heated until most of the solvent evaporates, forming an electrode film. The electrode is then further dried under dynamic vacuum at about 120°C. In all of the cells evaluated in this study, the negative electrode film has the following composition, expressed as weight percent: 88% active material, 3% conductive carbon, and 9% PVdF binder, or 92% active material, 2% conductive carbon, and 6% PVdF binder. No practical electrochemical differences were observed between these electrode formulations.
[0034] Prior to cell fabrication, both the cathode and anode electrodes are calendered and dried under dynamic vacuum again overnight. Both electrodes are then placed in a pouch in an argon-filled glove box (O2 and H2O present less than 5 ppm). In the three-electrode (3E) cells, two separator layers are used, and in the two-electrode (2E) cells, only one separator layer is used. In all cells, except those shown in Table 1 below, a common polyethylene separator is used, available for example from Asahi Kasei. In the 3E cells, Na metal pieces are placed between the two separator layers and between the cathode and anode, ensuring that the Na pieces do not fall within the footprint of the anode and / or cathode. The cell assembly is then filled with electrolyte. The electrolyte is 0.5m NaPF6 in a 1:2:1 weight ratio of EC:DEC:PC except as shown in Table 1 below, and all cells, except as shown in Table 1 below, contain nickelate-based cathode active material Na 0.833 Ni 0.317 Mn 0.467 Mg 0.1 Ti 0.117 O2 is used, and commercially available hard carbon (e.g., available from Kuraray) is used for the anode. Finally, the pouch is sealed in a glove box using a vacuum sealer. The cell is then subjected to electrochemical evaluation.
[0035] (Cell evaluation) The cells are evaluated using galvanostatic cycling as follows.
[0036] The cells are cycled galvanostatically at a given current density between pre-set voltage limits. Commercially available battery cyclers from MTI (Richmond, CA, USA) or Maccor (Tulsa, OK, USA) are used. Upon charging, alkali ions are extracted from the cathode and inserted into the X / hard carbon anode material. Upon discharging, alkali ions are extracted from the anode and reinserted into the cathode active material.
[0037] A number of sodium-ion cells were prepared using the above method. Table 1 below shows the 3E cycling results using a range of active anode GSMs, thicknesses and C / A mass balances. The plateau capacity:slope capacity ratios (P:S ratios) are also shown. Two-electrode (2E) cell data is also shown.
[0038] [Table 1-1] [Table 1-2] [Table 1-3] The examples marked with an * are comparative examples, ie the compositions evaluated are not according to the invention.
[0039] (Effect of anode active material mass on anode active material capacity) As shown by the results shown in Table 1 above, the anode active first desodium specific capacity (mAh / g) in a sodium ion battery including a 3E full cell is about 85 gm -2 From about 20gm -2 It is observed that the anode active mass increases with decreasing mass over a range of 1000 mAh / g. Furthermore, particularly high anode active first desodium specific capacity (500 mAh / g or greater) is obtained when low anode active mass (low GSM) is combined with a high C / A mass balance ratio (e.g., C / A ratio greater than 7). Surprisingly, the mass of the anode active mass can be reduced to about 52 g. -2 (e.g., samples A3PC118, A3PC117, A3PC129, A3PC119, A3PC140, A3PC133, and A3PC103), the anode first sodium depletion capacity increases from about 272 mAh / g to 379 mAh / g, which is seen as a result of increasing the C / A mass ratio from 2.31 to 3.41.
[0040] Figure 1 shows the anode profile of 3E full cells with different masses (GSM) of hard carbon material (e.g., commercially available from Kuraray). The C / A mass balance of each cell is shown in the figure. In all cells, 0.5 m NaPF6 in the weight ratio EC:DEC:PC = 1:2:1 is used as electrolyte. The results confirm that the lighter GSM anodes provide significantly higher capacity than the heavier GSM anodes and that the anode potentials of the lighter GSM anodes are significantly higher than the heavier GSM anodes in their fully charged state under the corresponding charged conditions. This point is very important not only from the performance point of view but also from the safety point of view. That is, the higher absolute potential of the anode in the fully charged state indicates that it is the "sodium deposition potential" (vs. Na / Na + This means that the GSM anode is further away from the positive electrode potential (below 0 V at 100 V) and therefore enhances the safety of the battery. These facts indicate that the light GSM anode offers significant advantages over the heavy GSM anode from a commercial standpoint.
[0041] Also, Figure 1 shows that full cells using heavy GSM anodes and high C / A mass balances have drawbacks that lead to Na deposition, especially at low capacity values. -2 For a full cell using this active anode material, Na deposition begins at a sodiation capacity of about 335 mAh / g during the first charge cycle of the full cell. The Na deposition capacity is estimated to be about 68 mAh / g during the first sodiation process (this value corresponds to the Na / Na + (corresponding to the portion of the anodic cycling curve that was below 0 V vs. 0 V). This is evident from the characteristic overpotential spike indicated by the arrow in Figure 1. The initial sodium desalination capacity observed for this cell is 335 mAh / g, but when the Na electrodeposition capacity is taken into account, the initial available sodium desalination capacity due to sodium storage in the hard carbon active material drops to 267-300 mAh / g.
[0042] In contrast, as previously discussed, Figure 1 confirms that the lighter GSM anode full cells provide higher sodium depletion capacities (364 or 450 mAh / g for 53.09 or 36.88 GSM anodes, respectively) at significantly higher fully charged anode potentials (approximately 80-83 mV). It is therefore concluded that high GSM hard carbon anodes tend to induce Na electrodeposition in sodium-ion full cells, which occurs at significantly lower capacity values than sodium-ion cells using lower mass anode active materials.
[0043] (Effect of Different Electrolytes on the Capacity of Anode Active Materials) Experiments were conducted to evaluate whether the increase in anode capacity of cells using lower masses of anode active material was influenced by the composition of the sodium-ion electrolyte used. Two cells (A3PC47 and A3PC80) were prepared. The former used an electrolyte containing 0.5 m NaPF6 in a 1:2:1 weight ratio of EC:DEC:PC, while the latter used an ether-based electrolyte containing 1 m NaBF4 in tetraethylene glycol dimethyl ether (tetraglyme).
[0044] As shown in Figure 2, the anode profiles of the two 3E full cells A3PC47 and A3PC80 had negligible differences. The former cell exhibited a first desodium anode capacity of 518 mAh / g against a 29.27 GSM active material hard carbon electrode, and the latter cell exhibited a first desodium anode capacity of 520 mAh / g against a 24.90 GSM active material hard carbon electrode.
[0045] Thus, the favorable anode capacity exhibited by cells containing lower mass anode electrode active material was found to be independent of the sodium ion electrolyte used.
[0046] (Effect of using different hard carbon materials on anode active material capacity) Two further experiments were performed to evaluate whether the initial sodium depletion capacity of the anode was affected by the nature (composition and / or source) of the anode electrode active material.
[0047] In the first of these experiments, three 3E full cells were prepared using a commercially available hard carbon anode material made from anthracite (a type of coal) sold under the trade name "Welsh Anthracite" and available from Supaheat Full. One cell (A3PC64) contained 103.98 gm -2 The other cell (A3PC106) contained 62.16 gm of anode active material. -2 The final cell (A3PC107) contained 51.51 gm of anode active material. -2 The anode electrode active material was used.
[0048] As shown in FIG. 3, the lower mass of the anode material (51.51 gm, respectively) is consistent with the results previously described. -2 and 62.16 gm. -2 For the two 3E full cells containing 100.0 gm 2, the first cycle anode capacity profiles (300 mAh / g and 240 mAh / g) and C / A mass balance values (3.38 and 2.69, respectively) indicate that the anode active material has a high mass (103.98 gm 2). -2 ) cell's anode capacity (196 mAh / g) and C / A mass balance value (1.83) were both higher.
[0049] In the second experiment, two 3E full cells were prepared using a commercially available biomass-derived hard carbon anode material, sold under the trade name "BHC-240" by BTR Corporation, China. One cell (A3PC143) contained 81.36 gm -2 of anode electrode active material was used, and in the other cell (A3PC136), 42.58 gm -2 is used.
[0050] In FIG. 4, a low mass anode material (42.58 gm -2For the 3E full cell containing a high C / A mass balance value (3.63), the first cycle anode capacity profile (410 mAh / g) is due to the high mass of anode material (81.36 gm -2 ) and anode capacity (242 mAh / g) of a cell with a low C / A mass balance value (1.87).
[0051] These results are believed to indicate that the nature of the hard carbon used as the anode active material is not related to the anode capacity characteristics.
[0052] (Effect of using different binders in the anode on the anode active material capacity) In this experiment, we investigated whether the anode capacity was affected by using an aqueous carboxymethyl cellulose (CMC):styrene butadiene rubber (SBR) binder instead of a non-aqueous PVdF binder in a 3E full cell. Two cells were prepared. One (A3PC120) had an active anode material of 59.04 gm -2 , with a hard carbon anode with a C / A mass balance of 2.62, and the other (A3PC141) with an active anode material of 80.85 gm -2 A hard carbon anode with a mass balance of 1.92 was used. In all other respects, i.e., the use of an aqueous binder based on CMC and SBR, the selection of the cathode, and the selection of a commercially available hard carbon anode (e.g., available from Kuraray) were identical for the two cells. As shown in FIG. 5, -2 The heavier cell with 1.0 g of anode active material was able to achieve 234 mAh / g in the first discharge cycle of the full cell. -2 ), the capacity was 320 mAh / g. Thus, the increased capacity of hard carbon in cells using lower mass anode active material is not affected by the type of binder used, and this trend is expected to be observed for any binder species.
[0053] (Long-term cycling results of the 3E complete cell of the present invention) 6 and 7 show the long-term cycling characteristics of several 3E full cells with different masses of anode active material as shown in Table 1. Specifically, FIG. 6 shows the capacity vs. cycle life based on the specific capacity of the active anode, and FIG. 7 shows the corresponding graph of the active cathode specific capacity. For all cells, the first four cycles were performed at C / 10 (the "formation" cycle) before cycling at C / 5 (the "post-formation" cycle). It should be noted that in FIGS. 6 and 7, the capacity retention (relative to the fifth cycle capacity, or the first "post" cycle capacity) of the last cycle of selected cells is listed.
[0054] From the results shown in Figures 6 and 7 and Table 1, several trends can be identified: Light GSM anodes (e.g., GSM values around 52 or 62) with low C / A mass balance (i.e., C / A mass balance between 1.9 and 2.56) greatly promote cycling stability as opposed to high C / A mass balance (i.e., C / A mass balance greater than 3.0). For the 52 GSM anode, the cycling stability of A3PC118 is compared to that of A3PC119, while for the 62 GSM anode, the cycling stability of A3PC110 and A3PC91 is compared to that of A3PC93. For any light GSM anode (e.g., GSM values around 52 or 62), decreasing the C / A mass balance increases the cathode specific capacity (A3PC118 compared to A3PC119, A3PC110 or A3PC91 compared to A3PC93). The above observations are based on the lower coulombic efficiency observed with light GSM anodes as a result of deeper sodiation of the hard carbon when heavier C / A mass balances are used. For this reason, cells with high C / A mass balances (greater than about 5) and very low GSM anodes (less than 30 GSM) tend to show very low first cycle coulombic efficiency (less than 50-60%), which is why such cells show low cathode capacity and poor cycling stability. For example, A3PC127 with 17.11 GSM anode and 7.09 C / A mass balance gives a cathode capacity of only 72.8 mAh / g in the first discharge cycle.
[0055] (Effect of changing the rating of the voltage window formed on cycle stability and anode specific capacity) In this experiment, the effect of "de-rating" the formation voltage window on cycling stability and anode specific capacity is investigated.
[0056] 51.64gm at 66μm thickness -2 Cell A3PC140, with 1.0 V of active anode material and a C / A mass balance of 3.27, was cycled four times at C / 10 from 4.20 to 1.00 V (during the formation cycle) and then cycled at C / 5 from 4.00 to 1.00 V ("post-formation cycle"). As shown in Figures 6 and 7, after "de-rating" the "post" cycle, the cell showed extremely high stability over 134 "post" cycles. The cathode capacity retention is 94%.
[0057] To further investigate the effect of derating and protocol formation, a 52.36g 66μm thick plate was -2Another similar cell, A3PC153, was fabricated with 100% active anode material and a C / A mass balance of 3.32. It was then cycled four times at C / 10 from 4.00 to 1.00 V during the formation process. It was then cycled at C / 5 at the same voltage 4.00 to 1.00 V during the “post” cycle process. The principle behind this experiment is to investigate the effect of four formation cycles from 4.20 to 1.00 V and four formation cycles from 4.00 to 1.00. Figures 8 and 9 show the resulting cathode and anode capacities versus cycle number, respectively, as well as the anode profiles for the first and fourth formation cycles. Figure 8 also shows the capacity retention at the 100th “post” cycle (relative to the 1st “post” cycle capacity). The results show that: When these cells were then "post" cycled using four formation cycles from 4.00 to 1.00 V, the cathode and anode capacities were significantly improved at similar cycling stability (approximately 93% or 94.5% retention at 100 "post" cycles) compared to four formation cycles from 4.20 to 1.00 V (cathode: 85.5 vs. 80.5 mAh / g; anode: 284.1 vs. 264.8 mAh / g). The anode profile in Figure 9 shows the detrimental effect of formation from 4.20 to 1.00 V on the capacity. The reason for this is believed to be that from 4.20 to 1.00 V the sodiation of the anode becomes more pronounced in the fully charged state, which has a detrimental effect on the coulombic efficiency of the photo-GSM anode. As shown in Figure 9, the coulombic efficiency increases from 75.5% in cycle 1 (subjected to four formation cycles from 4.20 to 1.00 V) to 96.2% in cycle 4 for the A3PC140 cell, while the cell A3PC153 (subjected to four formation cycles from 4.00 to 1.00 V) shows a slightly higher coulombic efficiency (76.8%) in the first cycle but a significantly improved efficiency of 99.2% in the fourth cycle. This last observation is likely the result of reduced Na loss from the cathode when the lower cell formation voltages of 4.00 to 1.00 V were used, explaining why the initial high “post” discharge capacity of the cathode (and also of the anode) was observed.
[0058] From the above results, it is believed that de-rated light GSM anodes provide a good strategy to enhance cycling stability, first from 4.20 to 1.00 V (during the formation cycle), then from 4.00 to 1.00 V (during the "post" cycle), and then by using 4.00 to 1.00 V for both the formation and "post" formation cycles. Cycling from 4.00 to 1.00 V is extremely stable, and the capacity obtained in the "post" cycle is higher when the formation is performed from 4.00 to 1.00 V. Using such a de-rated cycling protocol, it is possible to use a heavier C / A mass balance (>3) even with light GSM anodes.
[0059] (Long-term cycling stability of the cell according to the present invention) Figure 10 is a graph of specific capacity versus cycle number for a 1 Ah full cell FPC180905. -2The cell has a mass of active anode material (e.g., commercially available from Kuraray) of 10 ...
[0060] (Effect of C / A anode mass balance change on specific energy) The following table provides various relative energy densities for all 1 Ah cells evaluated with light GSM anodes (approximately 50-54 active anode GSM) compared against a 97.23 heavy GSM anode. The energy densities listed are the energy densities at the first "post" cycle (after 4 formation cycles). As indicated, the different cells were cycled at different voltage windows. As these results show, the energy density of the cells of the present invention with light GSM anodes is significantly higher than that of the heavy (>80 gm -2 ) mass of anode active material.
[0061] [Table 2] (Further study on the effect of anode active material mass and C / A anode mass balance on initial cycle stability) Considering the above experimental results, it is clear that cells containing low mass anodes are highly advantageous in providing high anode capacity. However, such cells do not necessarily provide the best initial cycle stability during the formation process. This observation is clearly illustrated in FIG. 11, which shows that extremely low mass anodes, specifically those with a mass of about 30 gm -2For cells with a C / A mass balance of 7.5 and 6.0 (anode mass of 30 g) or less, the cells show the lowest cycling stability over the first three cycles, while the high mass anode shows a fairly stable C / A mass balance. Furthermore, as shown in FIG. 12, the C / A mass balance also influences the initial cycling stability over the first three cycles. For the same cells evaluated in FIG. 11, the cells with a mass balance of 7.5 and 6.0 (anode mass of 30 g) show a significantly higher C / A mass balance. -2 Cells with a mass balance of about 3.5 or less show the poorest initial cycle stability, while cells with a mass balance of about 3.5 or less show improved stability.
[0062] 11 and 12 may also be used to identify that there are optimal ranges for anode mass and C / A mass balance to produce cells with high anode capacity (preferably at least 270 mAh / g) and good initial cycle stability. Specifically, -2 ~75gm -2 Particularly preferred are cells having an anode mass of about 1.0 to 3.5 and a C / A mass balance of about 2.0 to 3.5.
[0063] (Investigation of the performance of cells with non-nickelate cathode active materials) As shown in Table 1 above, cell 811023 contained Na as the cathode active material. 0.833 Fe 0.200 Mn 0.483 Mg 0.0417 Cu 0.225 O2 and mass 40.25gm -2 and a C / A mass balance of 3.13. A graph of specific capacity versus cycle number is shown in Figure 13, which shows that the non-nickelate cathode active material when used in a cell according to the present invention very successfully achieved a first desodium capacity of 336.45 mAh / g and retained 97.2% of this after 20 cycles.
[0064] This result illustrates that the positive effect of increasing anode specific capacity with decreasing anode GSM is independent of the type of cathode used.
[0065] (Investigation into the effect of hard carbon / Fe2P anode on anode characteristics) It was investigated whether a hard carbon composite anode (hard carbon mixed with "X" above) would show a trend of increasing anode specific capacity with decreasing anode GSM. In this example, another type of hard carbon (called "Pharazion Hard Carbon") prepared from cornstarch was used. Table 1 above lists 74.27 gm -2 and 55.25 gm. -2 The compositions of cells PCFA614 and 711042 using different amounts of HC / Fe2P anode active material are shown in Figure 14. The cycle 104 performance of these two cells is plotted as anode specific capacity (mAh / g) versus potential (V vs. Na / Na + ) is shown, which not only confirms the general trend mentioned above of low mass anodes forming higher anode capacity, but also shows that such hard carbon / Fe2P(HC / X) anodes form cells with extremely high cycling stability. From these results, it is clear that the trend of increasing anode capacity with decreasing anode GSM is exhibited by different types of hard carbon / X composite anodes.
[0066] (Consideration of cathode / anode mass balance less than 1.0 and the effect of non-nickelate cathode materials) As shown in Figures 15 and 16, the anode profile of the 3E full cell uses a low mass (GSM) of hard carbon material (e.g., commercially available from Kuraray) and a low C / A mass balance (C / A = 1.596 for sample 50 and C / A = 0.918 for sample 51). In both cells, 0.5 m NaPF6 with EC:DEC:PC = 1:2:1 by mass ratio was used as the electrolyte. The results confirm that such light GSM anodes provide excellent capacity and that other non-nickelate materials, such as sodiated metal sulfide materials (TiS2), can be used as active cathode materials. It is also reiterated in this example that the C / A mass balance, when used in such cells, is highly dependent on the cathode and anode active materials used (thus the respective capacities of the cathode and anode active materials actually determine which range of C / A mass balance can be used).
[0067] (Study on the effect of using oxygen-deficient nickelate cathodic materials) FIG. 17 shows the anode specific capacity (mAh / g) versus potential (V vs. Na / Na + ) is a plot of the anode GSM in other cells according to the present invention. 2 (i.e., 52.9) and the C / A ratio is in the range of 0.1 to 10 (i.e., 2.86), and as observed, the cell with the oxygen-deficient nickelate cathode material performs in a similar manner to the cell using a fully oxygenated nickelate cathode material.
[0068] (Study to demonstrate the charging tolerance of low GSM anode type cells) FIG. 17 shows the capacity retention versus cycle number for 3E full cells when charged at various rates and discharged at a constant C / 5 rate as indicated. These cells use low GSM (samples 54 and 56) or comparative GSM anodes (samples 53 and 55) made of either hard carbon commercially available from Kuraray or hard carbon commercially available from BTR (grade BHC-240). Comparing the two hard carbon containing cells, it is observed that the low GSM anode cell according to the invention (A3PC268) shows better capacity retention at fast charging rates such as 2C than the comparative GSM cell (A3PC231). This trend is also observed for the hard carbon material available from BTR. Moreover, the low GSM cell according to the invention (A3PC238) can be cycled in a more stable manner than the corresponding comparative GSM anode cell (A3PC225) when charged at fast rates such as 2C.
[0069] In this example, another surprising, important and commercially relevant result is evident for low GSM anodes, namely, that the cells of the invention can be charged more quickly than comparative cells having a GSM of anode material of over 80.
[0070] (Relationship between the weight (GSM) of the anode material and I) the porosity of the anode material, and II) the volume-specific surface area of the anode material) X-ray computed tomography (CT) is a useful tool to non-destructively build a 3D image of the interior of a battery electrode. By building such a 3D map image, CT allows visualization and quantification of the morphology of battery materials at the electrode level. In particular, it can reveal two important physical parameters of a battery electrode. The first is its porosity, which can be determined in %, and is defined as the ratio of the void volume in the electrode to the total volume of the electrode. The second is its volume-specific surface area, VSSA, which is expressed in m 2 / m 3 can be determined in units of
[0071] As the above results show, the low GSM effect of hard carbon is not the result of any change in the active material (type of hard carbon), binder, or electrolyte, but is solely a result of the GSM of the hard carbon used in the anode electrode (when the anode material thickness is less than 100 μm and C / A is in the range of 0.1 to 10). Applicant has investigated how the porosity and VSSA of a hard carbon electrode change with its GSM, and has obtained interesting and completely unexpected results, as will be shown below.
[0072] CT measurements were performed on two samples.
[0073] As detailed in Table 3 below, the sample designated as Comparative Sample 57 uses a GSM anode activity of 99.09 and a coating thickness of 113 μm. The sample designated as Sample 58 is in accordance with the present invention and has a GSM anode activity of 52.91 and a coating thickness of 60 μm. To avoid confusion, it is noted that for both these samples, the CT measurements were performed on hard carbon electrodes (not in an electrochemical cell).
[0074] Table 3 below summarizes the CT scan results.
[0075] [Table 3] As the above results show, Sample 58 exhibits a VSSA value that is nearly twice (1.92) that of Comparative Sample 57. This improved VSSA value helps explain the significantly higher capacity seen with all low GSM hard carbon electrodes according to the present invention. It is clear that the higher capacity of the low GSM anodes is due to their increased surface area per unit volume. This simply means that more hard carbon active material is accessible for sodium storage. In other words, the electrolyte-hard carbon interfacial area is increased for the low GSM anodes, and this access to "more" hard carbon active material per given volume results in a higher sodium storage capacity of the electrode.
[0076] It is important to note that although the VSSA of samples 57 and 58 are quite different, the two samples do not differ significantly in porosity. This is a highly unexpected result, as literature studies tend to attribute differences in porosity (obtained by techniques such as BET on hard carbon powders) to why different hard carbons have different capacities (and different plateau:slope capacity ratios). However, Applicant's results from the CT experiments described above indicate that it is not the porosity that is the important feature, but the VSSA, which largely determines the capacity obtained by a hard carbon electrode, and its plateau:slope capacity ratio. It will be clear to one skilled in the art that the porosity of a hard carbon electrode remains important in determining certain aspects of electrochemical properties, such as first cycle efficiency, density of the electrode, etc. However, as seen in this example, the VSSA is also a very important parameter, and this has been shown for the first time in this application.
[0077] Based on simple linear extrapolation, for an anode active GSM of 80 GSM (threshold GSM value for samples used in the cells of the present invention), the VSSA value is 0.993. However, it should be understood that this VSSA value may have some error, which may vary slightly or significantly depending on the type of hard carbon. It is also expected that the type of carbon additive and binder may affect the VSSA value. It is also expected that such VSSA value may be significantly affected. Thus, the present invention relates to any negative active material (preferably disordered carbon, and more preferably hard carbon)-containing electrode in which the active material layer has a VSSA value greater than 0.80.
Claims
1. A sodium ion secondary battery having a cathode and an anode, the cathode having one or more positive active materials and the anode having a layer of negative active material disposed on an anode substrate; the negative electrode active material comprises one or more disordered carbon-containing materials; i) the mass of the layer of negative electrode active material is 80 g or less per square meter of the anode substrate; ii) the ratio of the mass of the layer of positive electrode active material to the mass of the layer of negative electrode active material is from 0.1 to 10; iii) A sodium ion secondary battery, wherein the thickness of the layer of the negative electrode active material on the anode substrate is 100 μm or less.
2. The mass of the layer of the negative electrode active material per square meter of the anode substrate is 25 gm -2 Super, 80gm -2 The sodium ion secondary battery according to claim 1, wherein the current collector is less than 100 V.
3. The mass of the layer of the negative electrode active material per square meter of the anode substrate is 40 gm -2 ~75gm -2 2. The sodium ion secondary battery according to claim 1,
4. 2. The sodium ion secondary battery according to claim 1, wherein a ratio of the mass of the layer of the positive electrode active material to the mass of the layer of the negative electrode active material is 0.5 to 10.
5. 5. The sodium ion secondary battery according to claim 1, wherein the layer of the negative electrode active material on the anode substrate has a thickness of 80 μm or less.
6. One or more of the positive electrode active materials are represented by the general formula A 1±δ M 1 V M 2 W M 3 X M 4 Y M 5 Z O 2-c is a compound of Where: A is one or more alkali metals selected from sodium, potassium and lithium; M 1 has one or more redox-active metals in the oxidation state +2; M 2 has an oxidation state greater than 0 and a metal in an oxidation state of +4 or greater; M 3 has a metal in the +2 oxidation state, M 4 has a metal with an oxidation state greater than 0 and less than or equal to +4; M 5 has a metal in the oxidation state +3, Where: 0≦δ≦1; V>0; W≧0; X≧0; Y≧0; At least one of W and Y is greater than 0, Z≧0; C is in the range of 0≦c<2, 6. The sodium ion secondary battery according to claim 1 , wherein V, W, X, Y, Z and C are selected to maintain electrochemical neutrality.
7. 2. The sodium ion secondary battery according to claim 1, wherein the structure of the disordered carbon-containing negative electrode active material is a non-graphitizable non-crystalline amorphous structure.
8. 2. The sodium ion secondary battery according to claim 1, wherein the negative electrode active material comprises hard carbon.
9. The negative electrode active material has a hard carbon / X composite, 2. The sodium-ion secondary battery of claim 1, wherein X is one or more selected from phosphorus, sulfur, indium, antimony, tin, lead, iron, manganese, titanium, molybdenum, and germanium, either in elemental or compound form.
10. 2. The sodium-ion secondary battery of claim 1, wherein the negative electrode active material comprises one or more other materials capable of storing sodium ions and selected from non-metals, non-metal-containing compounds, metals, metal-containing compounds, and metal-containing alloys.
11. A cathode and an anode are provided. the cathode comprises one or more positive active materials and the anode comprises a layer, preferably a uniform layer, of a negative active material disposed on an anode substrate; the layer of negative electrode active material comprises one or more disordered carbon-containing materials; 10. The sodium-ion secondary battery of claim 1, wherein the layer of negative electrode active material has a volume specific surface area (VSSA) greater than 0.
8.
12. A method for producing the sodium ion secondary battery according to any one of claims 1 to 11, a. assembling a cathode having one or more positive electrode active materials with an anode having an anode substrate coated with a layer of negative electrode active material, and an electrolyte to form a sodium ion battery; b. cycling the sodium ion battery to a first voltage; having i) the mass of the layer of the negative electrode active material per square meter of the anode substrate is 80 gm -2 is as follows: ii) the ratio of the mass of the layer of the positive electrode active material to the mass of the layer of the negative electrode active material is 0.1 to 10; iii) The method of manufacturing, wherein the thickness of the layer of the negative electrode active material on the anode substrate is 100 μm or less.
13. A battery comprising at least two sodium-ion secondary batteries according to any one of claims 1 to 11.
Citation Information
Patent Citations
Heat-resistant battery and charge / discharge method thereof
JP2014032755A
Sodium ion secondary battery
JP2017010802A
Control method of sodium ion secondary battery, controller for sodium ion secondary battery, and sodium ion secondary battery for use in control method or controller for sodium ion secondary battery
JP2017045600A
Sodium-ion cell
WO2016157934A1
X / hard carbon composite material and method of preparing the x / hard carbon composite material
WO2017060718A1