Semiconductor device

The laminated structure of a metal oxide film with an oxide semiconductor film and an insulating film addresses charge trapping issues in oxide semiconductor transistors, enhancing reliability and stability by suppressing charge accumulation at the interface.

JP2024149594AActive Publication Date: 2024-10-18SEMICON ENERGY LAB CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024124471
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2010-04-09
Filing Date
2024-07-31
Publication Date
2024-10-18
Estimated Expiration
2031-04-06

AI Technical Summary

Technical Problem

Transistors using oxide semiconductors face issues with fluctuating electrical characteristics and low reliability due to charge trapping at the interface between the active layer and the interfacial stabilization layer, particularly when the layers have similar bandgaps, leading to instability and malfunctions.

Method used

A laminated structure is introduced, where a metal oxide film is stacked with an oxide semiconductor film, acting as a channel protective film to suppress charge trapping, and an insulating film is added to capture charges preferentially at the interface, thereby stabilizing the electrical characteristics.

Benefits of technology

This configuration enhances the reliability and stability of semiconductor devices by reducing charge trapping, leading to improved electrical performance and reduced fluctuations in transistor characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149594000001_ABST
    Figure 2024149594000001_ABST
Patent Text Reader

Abstract

To provide stable electrical characteristics to a semiconductor device using an oxide semiconductor to achieve high reliability.SOLUTION: In a transistor including an oxide semiconductor film, provided is a transistor where on a top face part of the oxide semiconductor film, a metal oxide film which functions as a channel protection film and consists of a component similar to that of the oxide semiconductor film is laminated. The oxide semiconductor film used for an active layer of the transistor is the oxide semiconductor film where an impurity such as hydrogen, moisture, a hydrogen group and hydride is excluded by a heat treatment; and the oxide semiconductor film which achieves high purity and electrically i-type (intrinsic) by supplying oxygen which is reduced simultaneously with the impurity exclusion process and which is a principal component material to compose the oxide semiconductor.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a semiconductor device and a method for manufacturing the semiconductor device.

[0002] In this specification, a semiconductor device is a device that can function by utilizing semiconductor characteristics. This term refers to devices in general, and electro-optical devices, semiconductor circuits, and electronic equipment are all classified as semiconductor devices. [Background technology]

[0003] A technology for constructing transistors using a semiconductor thin film formed on a substrate with an insulating surface. The transistor is used in integrated circuits (ICs) and image display devices (display devices). It is widely used in such electronic devices. Silicon-based semiconductor materials are widely known, but oxide semiconductors are also attracting attention as other materials. is.

[0004] For example, a semiconductor with an electron carrier concentration of 10 18 / cm 3 Less than The amorphous oxide containing indium (In), gallium (Ga), and zinc (Zn) is used. A transistor in which this is used has been disclosed (see Patent Document 1).

[0005] Transistors using oxide semiconductors have higher performance than transistors using amorphous silicon. They are faster than silicon-based transistors and easier to manufacture than polysilicon transistors. However, it is known that the electrical characteristics of the light-emitting diode are easily fluctuated and the reliability is low. The threshold voltage of a transistor varies before and after the T test. Patent Document 2 and Patent Document 3 disclose a method for simulating the threshold voltage of a transistor using an oxide semiconductor. In order to suppress the occurrence of the above-mentioned problem, a thin film is provided on at least one of the upper surface and the lower surface of the oxide semiconductor layer. A technology is disclosed that prevents charge trapping at the interface of an oxide semiconductor layer by using an interface stabilization layer. It has been done. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2006-165528 A [Patent Document 2] JP 2010-16347 A [Patent Document 3] JP 2010-16348 A Summary of the Invention [Problem to be solved by the invention]

[0007] However, the transistors disclosed in Patent Document 2 and Patent Document 3 are not interface stabilized. The layer used is a layer having the same properties as the gate insulating layer and the protective layer, and the interface with the active layer is Since the condition of the active layer and the interface stabilization layer cannot be maintained in a good condition, charge trapping between the active layer and the interface stabilization layer is suppressed. In particular, when the interface stabilization layer and the active layer have the same band gap, In this case, charge accumulation can easily occur.

[0008] Therefore, it is believed that transistors using oxide semiconductors still have sufficient reliability. I can't say.

[0009] In view of such problems, a method for imparting stable electrical characteristics to a semiconductor device using an oxide semiconductor is provided. One of the objectives is to achieve high reliability. [Means for solving the problem]

[0010] One embodiment of the disclosed invention is a channel protective film for an oxide semiconductor film, the channel protective film being in contact with the oxide semiconductor film. The metal oxide film has the same type of structure as the oxide semiconductor film. In other words, one embodiment of the disclosed invention is a metal oxide The semiconductor device has a structure in which an oxide semiconductor film and an oxide semiconductor film are stacked. The term "component of the same kind as the oxide semiconductor film" refers to one or more metal elements selected from the constituent elements of the oxide semiconductor film. It means that it contains an element.

[0011] By providing such a laminated structure, it is possible to reduce the electric current generated due to the operation of the semiconductor device. The oxide semiconductor film is preferably formed on the insulating film by a metal oxide layer. This effect can be achieved by using a material that is compatible with the oxide semiconductor film. By providing a metal oxide film in contact with an oxide semiconductor film, the operation of a semiconductor device can be improved. Charges and the like that may be generated due to the above are trapped at the interface between the oxide semiconductor film and the metal oxide film. This is due to the mechanism that can suppress the above.

[0012] In addition, the above-mentioned feature that trapping of charges at the interface of the oxide semiconductor film can be suppressed can be achieved. As a result, malfunctions of the semiconductor device are suppressed and the reliability of the semiconductor device is improved. It is possible.

[0013] In addition to such a stacked structure, a metal oxide film and an oxide semiconductor film different from each other can be used. It is preferable to use a structure in which an insulating film containing the component is provided on and in contact with a metal oxide film. In one embodiment of the disclosed invention, an oxide semiconductor film, a metal oxide film, and an insulating film are stacked. It has a structure that

[0014] In this way, the insulating film made of a material that can form a charge trap center at the interface is gold. By making the oxide semiconductor film exist in a state of contact with the metal oxide film, The charge can be preferentially trapped at the interface between the metal oxide film and the insulating film compared to the surface. That is, by providing an insulating film in contact with the metal oxide film, Charges are preferentially trapped at the interface between the oxide semiconductor film and the insulating film, and charges are preferentially trapped at the interface between the oxide semiconductor film and the metal oxide film. Thus, the trapping of charges in the semiconductor layer can be more effectively suppressed.

[0015] The trapping of charges at the interface of the oxide semiconductor film is suppressed, and the trapping center of the charges is located in the oxide semiconductor film. The above-mentioned effect of being able to keep the semiconductor film away from the semiconductor device prevents malfunctions of the semiconductor device. This makes it possible to suppress the generation of noise and improve the reliability of the semiconductor device.

[0016] In addition, from the above-mentioned mechanism, it is desirable that the metal oxide film has a sufficient thickness. When the metal oxide film is thin, the effect of charges trapped at the interface between the metal oxide film and the insulating film For example, a metal oxide film has a larger thickness than an oxide semiconductor film. It is preferable to make the

[0017] The insulating metal oxide film is connected to the source electrode and the drain electrode and the oxide semiconductor. Since the oxide film is formed in a manner that does not interfere with the connection between the source electrode or drain electrode and the oxide film, An increase in resistance can be prevented compared to when a metal oxide film exists between the semiconductor film and the semiconductor film. Therefore, deterioration in the electrical characteristics of the transistor can be suppressed.

[0018] In the thin film formation process of oxide semiconductors, the stoichiometric composition is changed due to an excess or deficiency of oxygen. If there is a deviation from the normal state or if hydrogen or moisture that forms electron donors gets mixed in, the electrical conductivity This phenomenon is a major problem for transistors using oxide semiconductors. Therefore, hydrogen, moisture, hydroxyl groups or hydrides (hydrogen compounds) are the cause of fluctuations in the mechanical properties. The impurities such as SiO 2 are intentionally removed from the oxide semiconductor, and the oxide semiconductor is By supplying oxygen, which is the main component of oxide semiconductors, the amount of oxygen decreases at the same time. In this way, the oxide semiconductor film is highly purified and made electrically i-type (intrinsic).

[0019] An i-type (intrinsic) oxide semiconductor is an oxide semiconductor that has n-type impurities, i.e., hydrogen, removed from it. By purifying the oxide semiconductor to minimize the amount of impurities other than the main component, i-type i-type (intrinsic) oxide semiconductors or oxide semiconductors that are as close to i-type (intrinsic) as possible. be.

[0020] In the step of making the oxide semiconductor film i-type, It is also possible to simultaneously convert the metal oxide film into an i-type film. The metal oxide films provided on the upper and lower surfaces of the metal oxide semiconductor film are resistant to impurities such as moisture and hydrogen. It is preferable that the metal oxide film is one in which the conductivity is sufficiently reduced and which is electrically i-type.

[0021] A transistor including a highly purified oxide semiconductor film has a low threshold voltage, an on-state current, and the like. The electrical characteristics of the transistors are almost temperature-dependent. There is also little fluctuation.

[0022] One embodiment of the present invention will be specifically described below.

[0023] One embodiment of the disclosed invention is a gate electrode, a gate insulating film covering the gate electrode, an oxide semiconductor film provided on the insulating film in a region overlapping with a gate electrode; a metal oxide film provided in contact with the oxide semiconductor film; a source electrode and a drain electrode in contact with the oxide semiconductor film; A semiconductor device including an oxide of one or more metal elements selected from the constituent elements It is.

[0024] In the above, the semiconductor device includes a metal oxide film covering the source electrode and the drain electrode. The insulating film may be provided on the insulating film. A conductive film may be provided.

[0025] In the above, the width of the metal oxide film in the channel length direction is equal to or larger than the width of the channel of the oxide semiconductor film. The source electrode and the drain electrode are formed on a part of the upper surface of the oxide semiconductor film. In the above structure, the oxide semiconductor film may be in contact with the The end portion may coincide with a side end portion of the metal oxide film in the channel length direction. In the above, the metal oxide film covers at least the oxide semiconductor film and An opening is provided to expose a part of the film, and the source electrode and the drain electrode are provided through the opening. In the above structure, the insulating film may be in contact with the oxide semiconductor film. A structure having a second metal oxide film in contact with a lower surface of the oxide semiconductor film In the above, the metal oxide film preferably functions as a channel protective film. I wish.

[0026] In the above, a source electrode and a drain electrode are provided on and in contact with the metal oxide film. A protective insulating film may be provided in contact with the electrode at a portion of the upper surface. The protective insulating film is used to prevent the chamfering of the oxide semiconductor film during etching of the source and drain electrodes. It functions as a film to protect the panel formation area.

[0027] In the above, the energy gap of the metal oxide film is equal to the energy gap of the oxide semiconductor film. The energy of the bottom of the conduction band of the metal oxide film is preferably larger than the gap. The energy is preferably higher than the minimum energy of the conduction band of the oxide semiconductor film.

[0028] In the above, the metal oxide film may contain gallium oxide.

[0029] In the above, the gate insulating film contains silicon oxide or hafnium oxide. The configuration may be such that

[0030] In the above, the metal oxide film functioning as a channel protection film has a channel length direction The channel length L of the transistor, which is determined by the width, is 10 nm to 10 μm, e.g. For example, the channel length L can be set to 0.1 μm to 0.5 μm. Of course, the channel length L can be set to 1 μm or more. The channel width W may be 10 nm or more. do. Effect of the Invention

[0031] According to one embodiment of the present invention, a transistor having stable electrical characteristics can be manufactured.

[0032] Another embodiment of the present invention is a semiconductor device including a transistor which has favorable electrical characteristics and high reliability. A device can be fabricated. [Brief description of the drawings]

[0033] [Figure 1] 1A and 1B are a plan view and a cross-sectional view illustrating one embodiment of a semiconductor device. [Diagram 2] FIG. 13 is a band diagram of a transistor including an oxide semiconductor film and a metal oxide film. [Diagram 3] 1A and 1B are a plan view and a cross-sectional view illustrating one embodiment of a semiconductor device. [Figure 4] 1A to 1C are diagrams illustrating one embodiment of a semiconductor device. [Diagram 5] 1A to 1C are diagrams illustrating an example of a manufacturing process of a semiconductor device. [Figure 6] 1A to 1C illustrate one embodiment of a semiconductor device. [Figure 7] 1A to 1C illustrate one embodiment of a semiconductor device. [Figure 8] 1A to 1C illustrate one embodiment of a semiconductor device. [Figure 9] 1A to 1C illustrate one embodiment of a semiconductor device. [Figure 10] FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. The present invention is not limited to the following description, and it is understood by those skilled in the art that various changes can be made in form and detail. The present invention is not limited to the description of the following embodiments. It is not something that is done.

[0035] The ordinal numbers such as 1st and 2nd are used for convenience and do not indicate the order of steps or stacking. In addition, the present specification does not indicate the order of the invention. It does not indicate the name.

[0036] (Embodiment 1) In this embodiment mode, one embodiment of a semiconductor device and a manufacturing method thereof will be described with reference to FIGS. This will be explained using:

[0037] <Configuration Example of Semiconductor Device> FIG. 1 shows an example of a semiconductor device, which is a channel protection type (Chip protection type), which is a bottom gate structure. FIG. 1(A) shows a cross-sectional view and a plan view of a transistor having a channel-stop type. 1(B) and 1(C) are plan views, and FIG. 1(B) and FIG. 1(C) are cross sections taken along lines AB and C in FIG. 1(A). In FIG. 1(A), in order to avoid complication, Some of the components of the transistor 310 (such as the gate insulating film 402) are omitted. .

[0038] The transistor 310 shown in FIG. 1A is provided on a substrate 400 having an insulating surface. A gate electrode 401, a gate insulating film 402 covering the gate electrode 401, and a gate The oxide semiconductor film 403 provided in a region overlapping with the electrode 401, A metal oxide film 407 is provided in contact with the metal oxide film 407. The semiconductor device includes a source electrode 405a and a drain electrode 405b that are in contact with a portion of the body membrane 403. In the transistor 310 shown in FIG. 1A, the metal oxide film 407 serves as a channel protective film. The transistor 310 also functions as a gate. 5b and in contact with the metal oxide film 407. is preferred.

[0039] Here, the metal oxide film 407 is formed of an oxide having the same composition as the oxide semiconductor film 403. Specifically, it is preferable to use one or more elements selected from the constituent elements of the oxide semiconductor film. It is preferable to use a film containing an oxide of several metal elements. The metal oxide film 403 has good compatibility with the oxide semiconductor film. This is because the interface condition can be kept good. By using the oxide semiconductor film in FIG. 07, the interface between the oxide semiconductor film and the metal oxide film in contact with the oxide semiconductor film (here, the gold (407) and the oxide semiconductor film (403). can be done.

[0040] Since the oxide semiconductor film 403 is used as an active layer, the energy of the metal oxide film 407 is The energy gap of the oxide semiconductor film 403 is required to be larger than that of the oxide semiconductor film 403. In addition, a thin film is formed between the metal oxide film 407 and the oxide semiconductor film 403 at room temperature (20° C.). In this case, it is necessary to form an energy barrier that is large enough to prevent carriers from flowing out of the oxide semiconductor film 403. For example, the minimum of the conduction band of the metal oxide film 407 and the minimum of the conduction band of the oxide semiconductor film 403 or the energy difference between the top of the valence band of the oxide semiconductor film 403 and that of the gold The energy difference between the upper end of the valence band of the metal oxide film 407 and the valence band of the metal oxide film 407 is preferably 0.5 eV or more. It is more preferable that the electron transport potential is 0.7 eV or more, and more preferable that the electron transport potential is 1.5 eV or less.

[0041] Specifically, for example, an In-Ga-Zn-O-based material is used for the oxide semiconductor film 403. In this case, the metal oxide film 407 may be formed using a material containing gallium oxide or the like. In addition, the energy barrier when gallium oxide is in contact with an In-Ga-Zn-O material is is approximately 0.8 eV on the conduction band side and approximately 0.9 eV on the valence band side.

[0042] Gallium oxide is GaOx Also written as stoichiometric excess of oxygen. For example, it is preferable to set the value of x to 1.4 or more and 2.0 or less. It is preferable that the value of x is 1.5 or more and 1.8 or less. When used as a gallium oxide film, the amount of impurities such as hydrogen and water is sufficiently reduced. However, if the gallium oxide film contains elements from group 3, such as yttrium, hafnium, etc. Group 4 elements such as aluminum, Group 13 elements such as silicon, nitrogen, etc. By adding impurity elements other than hydrogen, the energy gap of gallium oxide can be expanded. The energy gap of a gallium oxide film that does not contain impurities is 4.9 eV, but the above-mentioned impurities are contained, for example, in a range of more than 0 atomic % to 20 atomic % or less. By doing so, the energy gap can be expanded to about 6 eV.

[0043] From the viewpoint of reducing the source of charge generation and trapping centers, the water in the metal oxide film It is desirable to have sufficiently reduced impurities such as silicon and water. This idea is common to the reduction of impurities in conductive films.

[0044] In addition, a channel protective film is formed in a region overlapping with a channel formation region of the oxide semiconductor film 403. Since the metal oxide film 407 functioning as a Damage to the channel formation region due to etching of the drain electrode 405b (e.g., etch This prevents damage caused by plasma or etching agents during etching. In addition, a semiconductor device including an oxide semiconductor and having stable electrical characteristics can be provided. .

[0045] As shown in FIG. 1B, the width of the metal oxide film 407 in the channel length direction is increased by increasing the oxide semiconductor. By making the width of the conductor film 403 shorter than the width in the channel length direction, the source electrode 405a and the drain The in-electrode 405b is in contact with a part of the top surface of the oxide semiconductor film 403. By shortening the width of the film 407 in the channel length direction, the channel length of the transistor 310 is shortened. This shortens the time required for the transistor to operate at high speed and with low power consumption.

[0046] The transistor 310 is a so-called channel etched transistor in which the metal oxide film 407 is not provided. In comparison with the conventional transistor, the source electrode 405a and the drain electrode 405b are Since the contact area with the semiconductor film 403 is reduced, the source electrode 405a and The vicinity of the interface between the drain electrode 405b and the oxide semiconductor film 403 becomes a high-resistance region. This can reduce the concentration of the electric field in the transistor 310. Even when the sta 310 is miniaturized, the short channel effect can be suppressed.

[0047] In addition, in the case where the insulating film 409 is provided on and in contact with the metal oxide film 407, 09, by contacting it with the metal oxide film 407, a charge trap center is generated at the interface. It is preferable to use a material that can be formed by such a method for forming the insulating film 409. Since the charges are preferentially captured at the interface between the insulating film 409 and the metal oxide film 407, the metal oxide Therefore, the charge trapping at the interface between the oxide semiconductor film 403 and the oxide film 407 can be more effectively suppressed. However, there is a possibility that charges may be trapped at the interface between the insulating film 409 and the metal oxide film 407. If many centers are formed, this may actually deteriorate the transistor characteristics. Therefore, the amount of charge trapped is smaller than that at the interface between the oxide semiconductor film 403 and the metal oxide film 407. It is preferable that the concentration be such that the capture center is easily formed.

[0048] Specifically, the insulating film 409 is made of silicon oxide, silicon nitride, aluminum oxide, or nitride. Aluminum oxide, a mixture of these materials, etc. may be used in a single layer or in a laminated state. For example, When the metal oxide film 407 is formed using a material containing gallium oxide, the insulating film 409 is Silicon oxide or silicon nitride is preferably used. Due to the contact relationship, the energy gap of the insulating film 409 is It is preferable that the gap is larger.

[0049] In addition, a charge trap center may be formed at the interface between the insulating film 409 and the metal oxide film 407. If possible, the material of the insulating film 409 does not need to be limited to the above. Even if a treatment is performed to form a charge trap center at the interface between the film 409 and the metal oxide film 407, Such treatments include, for example, plasma treatment and element addition treatment (ion implantation, etc.). etc.).

[0050] In the transistor 310, the metal oxide film 407 is patterned in an island shape. However, the oxide semiconductor film 403 does not necessarily have to be patterned into an island shape. The side end in the channel length direction coincides with the side end in the channel length direction of the metal oxide film 407. In addition, when the insulating film 409 is formed, In this case, the gate electrode 401 is not provided, and A top-gate transistor may be used. In addition, a second metal oxide film may be provided. The width of the oxide semiconductor film 4 in the channel length direction is narrower than the width of the gate electrode 401 in the channel length direction. 3. Also, an insulating film may be provided on the transistor 310. In addition, the source electrode 405a and the drain electrode 405b may be electrically connected to wiring. In order to connect the gate insulating film 402, the metal oxide film 407, the insulating film 409, etc. Note that the oxide semiconductor film 403 is processed into an island shape. It is preferable that the islands are formed in this way, but they do not have to be formed in an island shape.

[0051] FIG. 2 shows the above-mentioned transistor 310, that is, the insulating film, the oxide Energy band diagram (schematic) for a structure in which a semiconductor film, a metal oxide film, and an insulating film are bonded together. (scheme), and E F is the Fermi level of the oxide semiconductor film. We assume an ideal situation in which both the insulating film and the oxide semiconductor film are intrinsic. Silicon oxide (SiO x ) (band gap Eg8eV~9eV) with metal oxide film Gallium oxide (GaO x ) (band gap Eg 4.9 eV) of the oxide semiconductor film (OS) In-Ga-Zn-O non-single crystal film (band gap Eg3.15eV) The vacuum level and the conduction band minimum energy of silicon oxide are The energy difference between the vacuum level and the conduction band edge of gallium oxide is 0.95 eV. 0.5 eV, and the energy difference between the vacuum level and the conduction band edge of the In-Ga-Zn-O non-single crystal film is The difference is 4.3 eV.

[0052] As shown in FIG. 2, the oxide semiconductor film has a gate electrode side (channel side) on which an oxide semiconductor is formed. There are energy barriers of about 3.35 eV and about 2.5 eV at the interfaces between the film and the insulating film. Similarly, an oxide semiconductor is formed on the opposite side (back channel side) of the oxide semiconductor film from the gate electrode. There are energy barriers of about 0.8 eV and about 0.95 eV at the interfaces between the metal film and the metal oxide film. At the interface between the oxide semiconductor film and the insulating film and at the interface between the oxide semiconductor film and the metal oxide film, Due to the existence of such an energy barrier, the oxide semiconductor film and the insulating film The movement of carriers is not hindered at the interface between the oxide semiconductor film and the metal oxide film, and at the interface between the oxide semiconductor film and the metal oxide film. Therefore, the carriers flow from the oxide semiconductor film to the insulating film or from the oxide semiconductor film to the metal oxide film. In other words, the oxide semiconductor film is The material has a larger band gap than the semiconductor film (here, a metal oxide film and an insulating film). By providing the oxide semiconductor film so as to sandwich the oxide semiconductor film, carriers move in the oxide semiconductor film.

[0053] FIG. 3 and FIG. 4(A) to FIG. 4(H) show examples of transistor configurations different from those in FIG. 1. .

[0054] FIG. 3 shows a cross section of a transistor having a structure in which a metal oxide film 407 covers an oxide semiconductor film 403. 3A is a plan view, and FIG. 3B and FIG. 3C are plan views. ) is a cross-sectional view of the AB section and the CD section in FIG. 3(A). In (A), in order to avoid complication, some of the components of the transistor 320 (e.g., For example, gate insulating film 402 and the like are omitted.

[0055] The transistor 320 shown in FIG. 3 includes a gate electrode 401 and a gate insulating film on a substrate 400. 402, an oxide semiconductor film 403, a metal oxide film 407, a source electrode 405a, a drain electrode The transistor 310 shown in FIG. 1 has the same structure as the transistor 310 shown in FIG. The difference between the transistor 320 shown in FIG. 3 and the transistor 310 shown in FIG. The oxide semiconductor film 403 is covered with the oxide semiconductor film 407. 0 was provided in the metal oxide film 407 so that part of the oxide semiconductor film 403 was exposed. Through the openings, the source electrode 405a, the drain electrode 405b, and the oxide semiconductor film 403 The other components are the same as those of the transistor 310 shown in FIG. For details, please refer to the description of Figure 1.

[0056] With this configuration, the transistor 320 is the same as the transistor 31 shown in FIG. 0, the source electrode 405a, the drain electrode 405b, and the oxide semiconductor film 403 Since the contact area between the source electrode 405a and the drain electrode 405b is reduced, The vicinity of the interface between 5b and the oxide semiconductor film 403 becomes a region with higher resistance. Since the concentration of the electric field in the transistor 310 can be further alleviated, Even when the size of 0 is reduced, the short channel effect can be suppressed more effectively.

[0057] The transistors 330 and 340 shown in FIG. 4(A) and FIG. 4(B) are For the configurations of the transistor 310 and the transistor 320, a conductive film 410 is provided in a region overlapping with a channel formation region of the oxide semiconductor film 403. The conductive film 410 may be formed of the same material and by the same method as the gate electrode 401. The other components are the same as the transistors 310 and 320 described above. The same applies. Note that the transistor 350 shown in FIG. 4(C) and FIG. The transistor 360 is configured to further increase the gate voltage of the transistor 330 and the transistor 340. A top-gate transistor is formed by not providing the electrode 401 and the gate insulating film 402. This is what we have decided.

[0058] The transistors 370 and 380 shown in FIG. 4(E) and FIG. 4(F) are For the configuration of the transistor 310 and the transistor 320, The metal oxide film 404 is a metal oxide. The gate insulating film 402 may be formed of the same material and by the same method as the insulating film 407. It is preferable to form the membrane 409 using the same material and method as the membrane 409. are similar to the transistors 310 and 320 described above.

[0059] With this structure, the lower surface of the oxide semiconductor film 403, that is, the oxide semiconductor film Charge capture can also be suppressed at the interface between the metal oxide film 403 and the metal oxide film 404 . Furthermore, as the gate insulating film 402, by contacting with the metal oxide film 404, By using a material in which a charge trapping center can be formed, the charge is transferred to the gate insulating film 402. Since the metal oxide film 404 is preferentially captured at the interface with the oxide semiconductor film 404, the metal oxide film 404 and the oxide semiconductor film Charge trapping at the interface of the conductive film 403 can be more effectively suppressed.

[0060] A transistor 390 shown in FIG. 4G has the following configuration compared to the transistor 310 described above: The width of the oxide semiconductor film 403 in the channel length direction is larger than the width of the gate electrode 401 in the channel length direction. The oxide semiconductor film 403 is patterned so as to be narrower than the other components. The transistor 310 is similar to the transistor 310 described above. Since the oxide semiconductor film 403 can be formed in a flat shape, the oxide semiconductor film 403 and the gate This can prevent carrier scattering at the interface of the gate insulating film 402 and reduce the interface state. .

[0061] The transistor 500 shown in FIG. 4H has the following configuration compared to the transistor 310 described above: A protective insulating film 419 is further provided on and in contact with the metal oxide film 407. The protective insulating film 419 has a part of its upper surface in contact with the source electrode 405a and the drain electrode 405b. The protective insulating film 41 functions as a channel protective film together with the metal oxide film 407. The insulating film 9 may be formed using the same material and method as the insulating film 409. The transistor 310 is similar to the transistor 310 described above.

[0062] With this structure, even if the insulating film 409 is not provided, the metal oxide film 4 07 and contacting it with the metal oxide film 407, a charge trap center is formed at the interface. Therefore, the insulating film 409 can be formed using a material that can be used for the insulating film 409. Even in the case where the metal oxide film 407 is not provided, the interface between the oxide semiconductor film 403 and the metal oxide film 407 is not as thin as that between the oxide semiconductor film 403 and the metal oxide film 407. Therefore, charges are preferentially captured at the interface between the protective insulating film 419 and the metal oxide film 407. Therefore, charge trapping at the interface between the metal oxide film 407 and the oxide semiconductor film 403 can be more effectively achieved. It can be suppressed.

[0063] The above transistor configurations can be used in appropriate combination. Cut.

[0064] <Example of the transistor manufacturing process> An example of a manufacturing process of the transistor shown in FIG. 1, FIG. 3, or FIG. 4 will be described below with reference to FIG. He explains.

[0065] <Fabrication process of transistor 310> An example of a manufacturing process of the transistor 310 shown in FIG. 1 will be described with reference to FIGS. This article explains:

[0066] First, a conductive film is formed on a substrate 400 having an insulating surface, and then a first photolithography process is performed. A gate electrode 401 is formed by a deposition process (see FIG. 5(A)). The resist mask may be formed by an ink-jet method. Since no photomask is used, manufacturing costs can be reduced.

[0067] There is no significant limitation on the substrate that can be used for the substrate 400 having an insulating surface, but at least At the very least, it is necessary for the material to have heat resistance sufficient to withstand subsequent heat treatment. For example, Substrates such as glass substrates, ceramic substrates, quartz substrates, and sapphire substrates can be used. In addition, as long as it has an insulating surface, a single crystal semiconductor substrate such as silicon or silicon carbide, Suitable for polycrystalline semiconductor substrates, compound semiconductor substrates such as silicon germanium, and SOI substrates. It is also possible to use a substrate having a semiconductor element thereon.

[0068] A flexible substrate may be used as the substrate 400. A transistor including the oxide semiconductor film 403 may be directly formed on a conductive substrate. A transistor including an oxide semiconductor film 403 is formed over a substrate, and then the transistor is peeled off and transferred to a flexible substrate. In order to peel and transfer the film from the production substrate to the flexible substrate, the film may be placed on an oxidized substrate. A peeling layer may be provided between the semiconductor film 403 and the transistor.

[0069] An insulating film serving as a base film may be provided between the substrate 400 and the gate electrode 401. The silicon nitride film, the silicon oxide film, and the like have a function of preventing the diffusion of impurity elements from the substrate 400. One or more films selected from a silicon film, a silicon oxide nitride film, and a silicon oxynitride film The insulating film can be formed by a laminate structure.

[0070] The gate electrode 401 may be made of any of molybdenum, titanium, tantalum, tungsten, and aluminum. Metallic materials such as aluminum, copper, neodymium, scandium, etc., or alloy materials that contain these as their main components. It can be used to form a single layer or a laminate.

[0071] Next, a gate insulating film 402 is formed on the gate electrode 401 (see FIG. 5(A)).

[0072] Specifically, the gate insulating film 402 may be a silicon oxide film, a silicon nitride film, or a silicon oxide nitride film. silicon oxide film, silicon oxynitride film, aluminum oxide film, aluminum nitride film, oxynitride film aluminum nitride film, aluminum oxide nitride film, hafnium oxide film, gallium oxide film, etc. It can be formed as a single layer or a laminate.

[0073] The method for producing the gate insulating film 402 is not particularly limited. For example, a plasma CVD method or a spa The gate insulating film 402 can be formed by a deposition method such as a quartz deposition method.

[0074] After the gate insulating film 402 is formed, a metal oxide film 40 is further formed on the gate insulating film 402. 4, the transistor 370 shown in FIG. 4(E) or the transistor 370 shown in FIG. The metal oxide film 404 can be formed as a metal oxide film 4 It can be formed using the same materials and processes as 07.

[0075] Next, an oxide semiconductor film 40 with a thickness of 3 nm to 30 nm is formed on the gate insulating film 402. The oxide semiconductor film 403 is formed by a sputtering method (see FIG. 5A). If the thickness is too large (for example, 50 nm or more), the transistor becomes normally on. Therefore, it is preferable to set the thickness as described above. The oxide semiconductor film 402 and the oxide semiconductor film 403 are preferably formed in succession without exposure to air.

[0076] Note that before the oxide semiconductor film 403 was formed by a sputtering method, argon gas was The reverse sputtering is performed by introducing the ions into the gate insulating film 402 to generate plasma. It is preferable to remove the powdery material (also called particles or dust) that is stuck to the surface. is a method of modifying the surface of the substrate by applying a voltage to the substrate and forming plasma in the vicinity of the substrate. In place of argon, gas such as nitrogen, helium, or oxygen may be used.

[0077] The oxide semiconductor used for the oxide semiconductor film 403 is an In- Sn-Ga-Zn-O oxide semiconductors and ternary metal oxides such as In-Ga-Zn-O In-Sn-Zn-O oxide semiconductors, In-Al-Zn-O oxide semiconductors Semiconductors, Sn-Ga-Zn-O oxide semiconductors, Al-Ga-Zn-O oxide semiconductors, Sn-Al-Zn-O oxide semiconductors and In-Zn-O oxides, which are binary metal oxides, are Semiconductors, Sn-Zn-O oxide semiconductors, Al-Zn-O oxide semiconductors, Zn-Mg -O-based oxide semiconductors, Sn-Mg-O-based oxide semiconductors, In-Mg-O-based oxide semiconductors, In-Ga-O oxide semiconductors, In-O oxide semiconductors, which are single-element metal oxides, and S nO-based oxide semiconductors, Zn-O-based oxide semiconductors, etc. can be used. The oxide semiconductor may contain SiO2. For example, an In-Ga-Zn-O oxide A compound semiconductor is an oxide film containing indium (In), gallium (Ga), and zinc (Zn). The composition ratio is not particularly important. Also, elements other than In, Ga, and Zn may include:

[0078] The oxide semiconductor film 403 is formed of a compound represented by the chemical formula InMO3(ZnO). m (m>0) A thin film having a thickness of 100 nm or less can be used. Here, M is selected from Ga, Al, Mn, and Co. It represents one or more metal elements. For example, M is Ga, Ga and Al, Ga and M n, or Ga and Co.

[0079] In this embodiment, the oxide semiconductor film 403 is an In-Ga-Zn-O-based oxide semiconductor. The oxide semiconductor film 40 is formed by a sputtering method using a film formation target. 3 is a rare gas (typically argon) atmosphere, an oxygen atmosphere, or a mixture of rare gas and oxygen. The film can be formed by a sputtering method in a mixed atmosphere.

[0080] In order to form an In-Ga-Zn-O film as the oxide semiconductor film 403 by a sputtering method, For example, the composition ratio of the target for this purpose is In2O3:Ga2O3:ZnO=1. A target for forming an oxide semiconductor film having a molar ratio of 1:1 can be used. The target material and composition are not limited to, for example, In2O3:Ga2O3:ZnO A target for forming an oxide semiconductor film having a molar ratio of 1:1:2 may be used.

[0081] In addition, when using an In-Zn-O-based material as an oxide semiconductor, the target used The composition ratio is In:Zn=50:1 to 1:2 in atomic ratio (In2O3 In:ZnO=25:1 to 1:4, preferably In:Zn=20:1 to 1:1 (in terms of molar ratio) In2O3:ZnO=10:1 to 1:2), and more preferably In:Zn=15 :1 to 1.5:1 (converted to a molar ratio of In2O3:ZnO=15:2 to 3:4) For example, the target used for forming an In-Zn-O-based oxide semiconductor has an atomic ratio of In When Zn:O=X:Y:Z, Z>1.5X+Y.

[0082] The filling rate of the oxide semiconductor film forming target is 90% or more and 100% or less, preferably The filling rate is 95% or more and 99.9% or less. A target for oxide semiconductor film formation with a high filling rate is used. As a result, the formed oxide semiconductor film 403 can be a dense film.

[0083] The sputtering gas used in forming the oxide semiconductor film 403 includes hydrogen, water, and a hydroxyl group. Alternatively, it is preferable to use a high-purity gas from which impurities such as hydrides have been removed.

[0084] The oxide semiconductor film 403 was formed by holding the substrate 400 in a deposition chamber kept under reduced pressure. The substrate temperature is set to 100° C. or higher and 600° C. or lower, preferably 200° C. or higher and 400° C. or lower. By heating the substrate 400 during the deposition, the oxide semiconductor film 403 contains In addition, the concentration of impurities in the oxide semiconductor film 4 by sputtering can be reduced. Damage to the oxidized layer 03 is reduced. Hydrogen and moisture are removed while removing the residual moisture in the deposition chamber. The sputtering gas was introduced, and the oxide semiconductor film was deposited on the substrate 400 using the target. In order to remove the residual moisture in the deposition chamber, a vacuum pump of the adsorption type, e.g. For example, it is preferable to use a cryopump, an ion pump, or a titanium sublimation pump. The exhaust means may be a turbo pump with a cold trap added. The deposition chamber evacuated using a cryopump contains hydrogen atoms, water (H2O), and other hydrogen gases. Since compounds containing atoms (and more preferably compounds containing carbon atoms) are exhausted, The impurity concentration in the oxide semiconductor film 403 formed in the deposition chamber can be reduced.

[0085] As an example of the deposition conditions, the distance between the substrate and the target is 100 mm, and the pressure is 0.6 P. a. DC power supply 0.5 kW, oxygen (oxygen flow rate 100%) atmosphere In addition, when a pulsed DC power supply is used, the powdery substances (particles, This is preferable because it reduces the amount of dust (also called dirt) and reduces the variation in film thickness.

[0086] After that, the oxide semiconductor film 403 is preferably subjected to heat treatment (first heat treatment). The first heat treatment removes excess hydrogen (including water and a hydroxyl group) from the oxide semiconductor film 403. The structure of the oxide semiconductor film 403 is adjusted, and defect levels in the energy gap are eliminated. The temperature of the first heat treatment is 250° C. or higher and 700° C. or lower, preferably The temperature of the first heat treatment is set to be lower than the distortion point of the substrate. It is preferable that

[0087] The heat treatment is carried out, for example, by placing the workpiece in an electric furnace using a resistance heating element and heating the workpiece in a nitrogen atmosphere. During this time, the oxide semiconductor film 403 is exposed to the air. Avoid contact and ensure that water or hydrogen does not get mixed in.

[0088] The heat treatment device is not limited to an electric furnace, but may be a device that uses heat conduction or heat radiation from a medium such as a heated gas. For example, a device that heats the workpiece by irradiation may be used. Rapid Thermal Anneal (GRTA) equipment, Gas Rapid Thermal Anneal (GRTA) equipment RTA (Rapid Thermal Anneal) equipment l) Equipment can be used. LRTA equipment includes halogen lamps, metal halide lamps, etc. xenon arc lamp, carbon arc lamp, high pressure sodium lamp, high pressure mercury lamp It is a device that heats the workpiece by radiating light (electromagnetic waves) emitted from a lamp such as a The GRTA device is a device that performs heat treatment using high-temperature gas. An inert gas that does not react with the workpiece during heat treatment, such as a rare gas such as benzene or nitrogen. is used.

[0089] For example, in the first heat treatment, the workpiece is placed in a heated inert gas atmosphere and heated for several minutes. After heating for 10 minutes, the workpiece may be removed from the inert gas atmosphere and subjected to GRTA treatment. GRTA treatment enables high-temperature heat treatment in a short time. The present invention can be applied even to temperature conditions exceeding 1000°C. The first heat treatment may be performed in an atmosphere containing oxygen. This is because the defect level in the energy gap caused by oxygen vacancies can be reduced. do.

[0090] The inert gas atmosphere is nitrogen or a rare gas (helium, neon, argon It is preferable to use an atmosphere that contains, as its main component, hydrogen, water, etc. For example, nitrogen and rare gases such as helium, neon, and argon introduced into a heat treatment device. The purity of is 6N (99.9999%) or more, preferably 7N (99.99999%) or more. (That is, the impurity concentration is 1 ppm or less, preferably 0.1 ppm or less).

[0091] In either case, the first heat treatment reduces impurities and produces an i-type (intrinsic) semiconductor or By forming the oxide semiconductor film 403 which is almost the same as a type semiconductor, A transistor can be realized.

[0092] By the way, the above-mentioned heat treatment (first heat treatment) has the effect of removing hydrogen, water, etc. This heat treatment can also be called a dehydration treatment or a dehydrogenation treatment. The dehydrogenation treatment may be performed, for example, after the oxide semiconductor film 403 is processed into an island shape. In addition, such dehydration and dehydrogenation treatments can be carried out in a single process. This may be done multiple times.

[0093] Next, the oxide semiconductor film 403 is subjected to a second photolithography process to form an island-shaped oxide semiconductor film. It is preferable to process the oxide semiconductor film into a conductive film 403 (see FIG. 5A). A resist mask for forming 403 may be formed by an inkjet method. If the mask is formed by the inkjet method, no photomask is used, so manufacturing costs are reduced. The etching of the oxide semiconductor film 403 can be performed by dry etching or wet etching. Alternatively, etching may be performed by first etching or both may be used.

[0094] Note that the width of the island-shaped oxide semiconductor film 403 in the channel length direction is equal to the width of the channel of the gate electrode 401. The oxide semiconductor film 403 is processed so that its width in the longitudinal direction is narrower than that in the longitudinal direction of the oxide semiconductor film 403. A transistor 390 as shown can be formed.

[0095] Then, plasma treatment is performed using gases such as N2O, N2, or Ar to expose the Water adsorbed on the surface of the oxide semiconductor film 403 may be removed by plasma treatment. In the case where the oxide semiconductor film 403 is not exposed to the air after the plasma treatment, It is preferable to form a metal oxide film 407 in contact with the metal oxide film 407 .

[0096] Next, a metal oxide film 427 is formed to cover the oxide semiconductor film 403 (FIG. 5B). The metal oxide film 427 is processed into islands in a later process. This results in a film 407.

[0097] The metal oxide film 427 (metal oxide film 407) has the same composition as the oxide semiconductor film 403. It is preferable to use an oxide containing a main component material of the oxide semiconductor film 403. Such a material is compatible with the oxide semiconductor film 403, and is used for the metal oxide film 407. This is because the state of the interface with the oxide semiconductor film can be kept good. By using the above-mentioned material for the metal oxide film 427 (metal oxide film 407), Therefore, trapping of charges at the interface between the oxide semiconductor film 407 and the oxide semiconductor film 403 can be suppressed. It is.

[0098] The energy gap of the metal oxide film 407 is larger than that of the oxide semiconductor film 403. In addition, the thickness of the metal oxide film 407 and the oxide semiconductor film 403 is required to be larger than the thickness of the metal oxide film 407. The temperature is set to a level at which carriers do not flow out of the oxide semiconductor film 403 at room temperature (20° C.). At a minimum, the formation of an energy barrier of

[0099] From the viewpoint of reducing the source of charge generation and trapping centers, the metal oxide film 407 is It is desirable that impurities such as hydrogen and water in the oxygen-rich water be sufficiently reduced. This idea is common to the idea of ​​reducing impurities in nitride semiconductor films.

[0100] The metal oxide film 427 (metal oxide film 407) is designed to prevent impurities such as water and hydrogen from being mixed in. It is preferable to form the metal oxide film 427 (metal oxide film 407) by using a hydrogen deposition method. When hydrogen is contained, the hydrogen may enter the oxide semiconductor film 403 or the oxide semiconductor film 404 may be damaged. Oxygen is extracted from the oxide semiconductor film 403, and the back channel of the oxide semiconductor film 403 has a low resistance. Therefore, the metal oxide The film 427 (metal oxide film 407) is formed by a film forming method so as to have as little hydrogen as possible. It is important not to use hydrogen for the reaction.

[0101] Therefore, it is preferable to form the metal oxide film 427 by a sputtering method. The sputtering gas used for the deposition does not contain impurities such as hydrogen, water, hydroxyl groups, or hydrides. It is preferable to use a high-purity gas from which

[0102] In order to keep the charge trapping center away from the oxide semiconductor film 403, the metal oxide film 4 It is preferable that the metal oxide film 407 has a sufficient thickness. Oxide film 427 (metal oxide film 407) with a thickness of more than 10 nm and less than 100 nm It is preferable to set the above.

[0103] After the metal oxide film 427 is formed, a protective insulating film 419 is further formed on the metal oxide film 427. By providing the protective insulation, the transistor 500 shown in FIG. The insulating film 419 can be formed of the same material and in the same process as the insulating film 409 described later. The protective insulating film 419 is formed by bonding the metal oxide film 427 to the metal oxide film 407 in a later process. When forming the turn, the pattern can be formed at the same time. Of course, the metal oxide film 4 Pattern formation may be carried out in a separate process from 27.

[0104] Next, a resist mask is formed on the metal oxide film 427 by a third photolithography process. Then, etching is performed to form a metal oxide film 407 that functions as a channel protection film. After that, the resist mask is removed (see FIG. 5(C)). A resist mask for forming the resist film may be formed by an ink-jet method. When the ink jet method is used, no photomask is used, which reduces manufacturing costs. The etching of the metal oxide film 427 here can be either dry etching or wet etching. Alternatively, both may be used.

[0105] The third photolithography process uses ultraviolet light and KrF for exposure when forming the resist mask. Laser light or ArF laser light is preferably used. Metal oxide film that functions as a channel protection film The width of 407 in the channel length direction determines the channel length L of the transistor to be formed later. In addition, when performing exposure with a channel length L of less than 25 nm, for example, a few nm to a few Extreme ultraviolet rays with an extremely short wavelength of 10 nm are used. It is preferable to use the third photolithography process for exposure when forming a resist mask. Exposure to ultraviolet light has high resolution and a large depth of focus. It is possible to reduce the channel length L of the transistor, thereby increasing the operating speed of the circuit.

[0106] Here, the width of the metal oxide film 407 in the channel length direction is equal to the width of the channel of the oxide semiconductor film 403. By forming the pattern so that the width in the long direction is shorter than the width in the long direction, the source electrode The drain electrode 405 a and the drain electrode 405 b are in contact with part of the top surface of the oxide semiconductor film 403 . Therefore, by shortening the width of the metal oxide film 407 in the channel length direction, the transistor This shortens the channel length of the transistor, thereby enabling the transistor to operate at higher speed and consume less power.

[0107] In addition, in the etching process of the metal oxide film 427, the metal oxide film 427 and the oxide When the etching selectivity of the oxide semiconductor film 403 is not sufficient, the gold of the oxide semiconductor film 403 is In some cases, a portion of the region that does not overlap with the metal oxide film 427 may be removed. The thickness of the conductive film 403 in the region not overlapping with the metal oxide film 427 becomes thin.

[0108] Note that in the case where the oxide semiconductor film 403 is not processed into an island shape in the above process, a metal oxide The oxide semiconductor film 403 and the metal oxide film 427 may be processed into islands at the same time. By simultaneously forming a pattern on the oxide film 427, the number of photolithography steps can be reduced. In addition, the oxide semiconductor film 403 and the metal oxide film 427 can be formed using the same mask. By patterning the oxide semiconductor film 403, the side end portions in the channel length direction and The side end of the metal oxide film 407 in the channel length direction is aligned. The insulating film 402, the oxide semiconductor film 403, and the metal oxide film 427 are continuously heated without being exposed to the outside air. It is preferable to deposit the film successively.

[0109] The metal oxide film 427 does not necessarily have to be processed into an island shape. An oxide semiconductor is provided to electrically connect the source electrode 405a and the drain electrode 405b. An opening through which a part of the conductive film 403 is exposed may be provided. 3B, the transistor 340 shown in FIG. 4(D) or the transistor 380 shown in FIG. 4(F). It is possible.

[0110] Next, a source electrode and a A conductive film is formed to form the source and drain electrodes (including wiring formed in the same layer). The conductive film used for the source electrode and the drain electrode is, for example, Al, Cr, Metal film containing an element selected from Cu, Ta, Ti, Mo, and W, or a film containing the above elements as components Metal nitride films (titanium nitride film, molybdenum nitride film, tungsten nitride film, etc.) are used. In addition, T can be applied to either or both of the upper and lower sides of the metal film such as Al or Cu. High melting point metal films such as Ti, Mo, W, etc., or metal nitride films of these metals (titanium nitride film, molybdenum nitride film, etc.) A structure in which a tungsten nitride film, a tungsten nitride film, and a tungsten nitride film are laminated may also be used. The conductive film used for the drain electrode may be formed of a conductive metal oxide. The oxides include indium oxide (In2O3), tin oxide (SnO2), and zinc oxide (Zn O), indium oxide tin oxide alloy (In2O3-SnO2, abbreviated as ITO), oxide Indium zinc oxide alloy (In2O3-ZnO) or oxide systems made of these metal oxide materials It is possible to use one containing a recombinant.

[0111] A resist mask is formed on the conductive film by a fourth photolithography process, and selectively etched. After etching to form the source electrode 405a and the drain electrode 405b, The resist mask in the third photolithography process is then removed (see FIG. 5(D)). When ultraviolet light, KrF laser light, or ArF laser light is used for exposure during formation, the metal oxide film Between the lower end of the source electrode 405a and the lower end of the drain electrode 405b adjacent to each other on 407 Since the spacing becomes narrower, the fourth photolithography process also uses ultraviolet light and KrF It is preferable to use a laser beam or an ArF laser beam.

[0112] In addition, in order to reduce the number of photomasks and steps used in the photolithography process, The resist pattern formed by a multi-tone mask, which is an exposure mask that transmits light with multiple intensities. The etching process may be performed using a resist mask formed using a multi-tone mask. The mask has a shape with multiple film thicknesses, and the shape is further changed by etching. This allows for multiple etching processes to be performed to create different patterns. Therefore, at least two different patterns can be produced using one multi-tone mask. A corresponding resist mask can be formed. This reduces the number of exposure masks. This also eliminates the need for a corresponding photolithography process, making it possible to simplify the process. .

[0113] Here, a region overlapping with a channel formation region of the oxide semiconductor film 403 is Since the conductive film 407 is provided, damage caused by etching of the conductive film (e.g., etching This prevents damage caused by plasma or etching agents during etching. In addition, a semiconductor device including an oxide semiconductor and having stable electrical characteristics can be provided. .

[0114] Next, a metal oxide film 407 is formed on the source electrode 405a and the drain electrode 405b. It is preferable to form the insulating film 409 by using a metal oxide film (see FIG. 5E). By bringing the oxide film 407 and the insulating film 409 into contact with each other, a charge trapping center is formed at the interface. It is preferable to use a material capable of forming the insulating film 409. Since the charges are captured at the interface between the insulating film 409 and the metal oxide film 407, the charges are not captured at the interface between the insulating film 409 and the metal oxide film 407. Charge trapping at the interface between the oxide semiconductor film 407 and the oxide semiconductor film 403 can be sufficiently suppressed. do.

[0115] The insulating film 409 is an inorganic insulating film, and may be a silicon oxide film, a silicon oxynitride film, an oxide film, or a silicon nitride film. an oxide insulating film such as an aluminum oxide nitride film or an aluminum oxynitride film, or a silicon nitride film; Silicon nitride oxide film, aluminum nitride film, aluminum nitride oxide film, and other nitride insulating films For example, a metal oxide film 4 may be formed by sputtering. A silicon oxide film and a silicon nitride film are laminated in this order from the 07 side. The insulating film 409 is In this case, the oxide semiconductor film 403 and the metal oxide film 407 may be different from each other in the structure. In the subsequent heat treatment process for the oxide semiconductor film 403, the metal oxide film 40 In order to efficiently remove impurities such as hydrogen and moisture from the insulating film 409, the insulating film 409 is made of silicon oxide. In addition, since it is in contact with the metal oxide film 407, the insulating film 409 is preferably an ethylene oxide film. The energy gap is preferably larger than the energy gap of the metal oxide film 407. stomach.

[0116] In addition, a charge trap center may be formed at the interface between the insulating film 409 and the metal oxide film 407. If possible, the material of the insulating film 409 does not need to be limited to the above. Even if a treatment is performed to form a charge trap center at the interface between the film 409 and the metal oxide film 407, Such treatments include, for example, plasma treatment and element addition treatment (ion implantation, etc.). etc.).

[0117] Next, a part (channel formation region) of the oxide semiconductor film 403 is in contact with the metal oxide film 407. It is preferable to perform the second heat treatment in this state. The temperature of the second heat treatment is 250° C. or higher and 700° C. or lower. The temperature of the first heat treatment is preferably 450° C. or higher and 600° C. or lower. It is preferably below the strain point of the plate.

[0118] The second heat treatment is carried out in a vacuum of nitrogen, oxygen, or ultra-dry air (with a water content of 20 ppm or less, preferably Air at less than 1 ppm, preferably less than 10 ppb), or rare gases (argon, helium The above-mentioned atmospheres of nitrogen, oxygen, ultra-dry air, rare gas, etc. may be used. It is preferable that the gas does not contain water, hydrogen, etc. Or the purity of the rare gas is 6N (99.9999%) or more, preferably 7N (99.999 99%) or more (i.e., impurity concentration is 1 ppm or less, preferably 0.1 ppm or less). is preferred.

[0119] In the second heat treatment, the oxide semiconductor film 403 and the metal oxide film 407 are in contact with each other. Therefore, the above-mentioned dehydration (or dehydrogenation) process simultaneously reduces Oxygen, one of the main components of oxide semiconductors that may be damaged, is The metal oxide film 407 containing the metal oxide can supply the metal oxide semiconductor film 403. Thus, charge trapping centers in the oxide semiconductor film 403 can be reduced. The oxide semiconductor film 403 can be formed by purifying the oxide semiconductor film 403 and making the oxide semiconductor film 403 electrically i-type (intrinsic). In addition, this heat treatment also removes impurities from the metal oxide film 407, resulting in a highly purified film. It can be done.

[0120] In this embodiment, the second heat treatment is performed after the insulating film 409 is formed. The timing of the heat treatment is not particularly limited as long as it is performed after the formation of the metal oxide film 407 . For example, the second heat treatment may be performed after the formation of the metal oxide film 407. For example, when the silicon oxide film and the silicon nitride film are laminated, the metal oxide After forming a silicon oxide film on the oxide film 407, a second heat treatment is performed, and then a silicon nitride film is formed. Alternatively, the first heat treatment may be followed by a second heat treatment, or the first heat treatment may be followed by a third heat treatment. The first heat treatment may also serve as the second heat treatment, or the second heat treatment may also serve as the first heat treatment. That's fine.

[0121] As described above, by applying at least one of the first heat treatment and the second heat treatment, oxidation The semiconductor film 403 is highly purified so that it contains as few impurities as possible other than its main components. In the highly purified oxide semiconductor film 403, carriers derived from donors are extremely The carrier concentration is 1×10 14 / cm 3 Less than 1x1 0 12 / cm 3 less than 1×10 11 / cm 3 is less than.

[0122] Through the above steps, the transistor 310 is formed (see FIG. 5E). 0 is an oxide made by removing impurities such as hydrogen, water, hydroxyl groups, or hydrides (also called hydrogen compounds). The oxide semiconductor film 403 is intentionally removed from the semiconductor film 403, and the transistor including the oxide semiconductor film 403 is highly purified. Therefore, the transistor 310 has suppressed fluctuations in electrical characteristics, and It is generally stable.

[0123] In addition, in the transistor including the metal oxide film 407, It is possible to prevent the occurrence of a parasitic channel on the channel side. In the above, a parasitic channel on the back channel side of the oxide semiconductor film 403 is prevented from being generated. This suppresses the fluctuation of the threshold voltage, resulting in a more reliable transistor. It is possible.

[0124] After the insulating film 409 is formed, the oxide semiconductor film 403 is formed over the insulating film 409. By providing the conductive film 410 in a region overlapping the channel formation region, the transistor shown in FIG. The transistor 330 or the transistor 340 shown in FIG. Furthermore, by not providing the gate electrode 401 and the gate insulating film 402, 4(C) or the transistor 360 shown in FIG. 4(D). The conductive film 410 can be formed of the same material and in the same process as the gate electrode 401. The conductive film 410 can be formed at a position overlapping with a channel formation region of the oxide semiconductor film 403. By providing a bias-thermal stress test for checking the reliability of the transistor 340, In a thermal stability test (hereinafter referred to as a BT test), the characteristics of the transistor 340 before and after the BT test were The change in the threshold voltage can be further reduced. It may be the same as the first gate electrode 401 or may be different, and serves as a second gate electrode. In addition, the potential of the conductive film 410 may be set to GND, 0 V, or in a floating state. may be also possible.

[0125] Although not shown, a protective insulating film may be further formed to cover the transistor 310. The protective insulating film is preferably a silicon nitride film, a silicon oxynitride film, or an aluminum nitride film. Um etc. can be used.

[0126] A planarization insulating film may be provided over the transistor 310. Acrylic, polyimide, benzocyclobutene, polyamide, epoxy, etc., with heat resistance In addition to the above organic materials, low-k materials can be used. materials), siloxane resin, PSG (phosphorus glass), BPSG (borophosphorus glass), etc. A plurality of insulating films made of these materials may be laminated.

[0127] As described above, in the transistor according to this embodiment, A metal oxide film made of the same kind of component as the oxide semiconductor film is laminated on the oxide semiconductor film. A metal oxide film made of a material compatible with a semiconductor film is brought into contact with an oxide semiconductor film. By making the semiconductor device exist in such a manner, charges that may be generated due to the operation of the semiconductor device are prevented from being transferred to the oxide semiconductor. This sufficiently prevents the particles from being captured at the interface between the solid film and the metal oxide film. Therefore, the influence of charges on the oxide semiconductor film can be reduced, and the charge on the oxide semiconductor film interface can be reduced. Therefore, it is possible to suppress the threshold voltage fluctuation of the transistor caused by the charge trapping.

[0128] Further, a metal oxide film is provided on a surface of the metal oxide film opposite to the surface in contact with the oxide semiconductor film. The insulating film containing a component different from the oxide semiconductor film is provided in contact with the oxide semiconductor film. In addition, an insulator made of a material that can form a charge trapping center at the interface is placed on a metal oxide film. By making the oxide semiconductor film exist in a state of contact with the metal oxide film, the interface This allows the above-mentioned charges to be preferentially captured at the interface between the metal oxide film and the insulator. Since the influence of charges on the oxide semiconductor film can be further reduced by the To more effectively suppress the threshold voltage shift of transistors caused by charge trapping at the interface between the semiconductor and the semiconductor layer. It is possible.

[0129] In addition, the oxide semiconductor film used for the active layer of the transistor is decomposed by hydrogen, moisture, and the like through heat treatment. Impurities such as hydroxyl groups or hydrides (also called hydrogen compounds) are removed from the oxide semiconductor. The main component material of the oxide semiconductor, which is also reduced during the impurity removal process, By supplying oxygen as a material, the oxide semiconductor film is highly purified and electrically becomes i-type ( The transistor including the highly purified oxide semiconductor film is The change in electrical characteristics of the capacitor is suppressed, and the capacitor is electrically stable.

[0130] When charges are trapped at the interface of the oxide semiconductor film, the threshold voltage of the transistor (For example, if a positive charge is trapped in the back channel, the The threshold voltage shifts in the negative direction. One of the causes of this charge trapping is the positive ionization. A model of the movement and trapping of on (or the atoms responsible for it) can be postulated. In a transistor using an oxide semiconductor, In the disclosed invention, a highly purified oxide semiconductor is used, and Since this structure is in contact with a laminated structure of a metal oxide film and an insulating film, This even suppresses the charge trapping caused by hydrogen in the above-mentioned The model is believed to be valid when the ionization rate of hydrogen is, for example, around 10%.

[0131] As described above, a semiconductor device using an oxide semiconductor and having stable electrical characteristics is provided. Therefore, a highly reliable semiconductor device can be provided.

[0132] The configurations, methods, etc. described in this embodiment may be different from the configurations, methods, etc. described in other embodiments. They can be used in appropriate combination.

[0133] (Embodiment 2) A semiconductor device (display device) having a display function using the transistor described in Embodiment 1 In addition, a part or the whole of a driver circuit including a transistor can be manufactured. The body can be integrally formed on the same substrate as the pixel portion to form a system-on-panel.

[0134] In FIG. 6A, a pixel portion 4002 is provided on a first substrate 4001. A sealant 4005 is provided on the substrate 4002, and the substrate 4002 is sealed with a second substrate 4006. In (A), the area surrounded by the sealant 4005 on the first substrate 4001 A single crystal semiconductor film or a polycrystalline semiconductor film is formed on a separately prepared substrate in a region different from the above. A scanning line driver circuit 4004 and a signal line driver circuit 4003 are mounted on the substrate. A signal line driver circuit 4003 and a scanning line driver circuit 4004 or a pixel portion 4002 are provided with a The various signals and potentials are transmitted through the FPC (Flexible Printed Circuit). Powered by FPC4018a and FPC4018b.

[0135] In FIG. 6B and FIG. 6C, the pixel portion 40 is provided on the first substrate 4001. A sealant 4005 is provided so as to surround the gate electrode 4002 and the scanning line driver circuit 4004. In addition, a second substrate 4006 is provided on the pixel portion 4002 and the scanning line driver circuit 4004. Therefore, the pixel portion 4002 and the scanning line driver circuit 4004 are formed on the first substrate 4001. The display element is sealed by a sealant 4005 and a second substrate 4006 . In FIG. 6B and FIG. 6C, the sealing material 4005 on the first substrate 4001 A single crystal semiconductor film or A signal line driver circuit 4003 formed of a polycrystalline semiconductor film is mounted. In FIG. 6(C), a signal line driver circuit 4003 and a scanning line driver circuit 4004 are separately formed. Various signals and potentials applied to the pixel portion 4002 are supplied from the FPC 4018. are being provided.

[0136] In addition, in FIG. 6B and FIG. 6C, a signal line driver circuit 4003 is separately formed. 10, the scanning lens 4001 is mounted on the first substrate 4001, but the present invention is not limited to this configuration. A signal line driver circuit may be formed separately and mounted, or a part of a signal line driver circuit or a scanning line driver circuit may be mounted. Alternatively, only a part of the path may be formed separately and implemented.

[0137] The method of connecting the separately formed drive circuit is not particularly limited, and may be any method such as COG ( hip on glass method, wire bonding method, or TAB (Tape The Automated Bonding method can be used. This is an example in which a signal line driver circuit 4003 and a scanning line driver circuit 4004 are mounted by the COG method. FIG. 6B shows an example of mounting a signal line driver circuit 4003 by the COG method. C) is an example in which the signal line driver circuit 4003 is mounted by the TAB method.

[0138] The display device includes a panel in which a display element is sealed, and a controller for the panel. This includes modules in which ICs, etc., including lasers, are mounted.

[0139] In this specification, the term "display device" refers to an image display device, a display device, or Refers to light sources (including lighting devices). Also refers to connectors, such as FPC or TAB tape. or a module with TCP attached, a printed wiring board on the tip of TAB tape or TCP A module with a display element or a display device with an IC (integrated circuit) directly mounted on it using the COG method. The display device includes all installed modules.

[0140] In addition, the pixel portion and the scanning line driver circuit provided on the first substrate include a plurality of transistors. The transistor shown in Embodiment 1 can be used.

[0141] Examples of display elements provided in the display device include liquid crystal elements (also called liquid crystal display elements), light-emitting elements, and the like. A light-emitting element (also called a light-emitting display element) can be used. This category includes elements whose brightness is controlled by a specific factor, such as inorganic EL (Electroluminescent) devices. Luminescence, organic electroluminescence, etc. Also, electronic ink, etc. A display medium in which the contrast changes depending on the effect can also be used.

[0142] One embodiment of a semiconductor device will be described with reference to FIGS. This corresponds to the cross-sectional view at MN in (B).

[0143] As shown in FIGS. 7 to 9, the semiconductor device has a connection terminal electrode 4015 and a terminal electrode 401 6, and the connection terminal electrode 4015 and the terminal electrode 4016 are The electrode 4014 is electrically connected to a terminal via an anisotropic conductive film 4019 .

[0144] The connection terminal electrode 4015 is formed from the same conductive film as the first electrode layer 4030. 4016 denotes the source and drain electrodes of the transistors 4010 and 4011. It is formed from the same conductive film as the electrodes.

[0145] A pixel portion 4002 and a scanning line driver circuit 4004 are provided on a first substrate 4001. 7 to 9, the transistors included in the pixel portion 4002 are 4010 and a transistor 4011 included in the scanning line driver circuit 4004. is doing.

[0146] In this embodiment, the transistors 4010 and 4011 are The transistor shown in FIG. 1 can be applied to the transistor 4010. The variation in electrical characteristics of the 4011 is suppressed, and the 4011 is electrically stable. As the semiconductor device of this embodiment shown in FIG. 9, a highly reliable semiconductor device can be provided. Cut.

[0147] The transistor 4010 provided in the pixel portion 4002 is electrically connected to a display element. The display element is not particularly limited as long as it can display an image, and various display elements can be used. can be used.

[0148] FIG. 7 shows an example of a liquid crystal display device using a liquid crystal element as a display element. The liquid crystal element 4013 includes a first electrode layer 4030, a second electrode layer 4031, and The liquid crystal layer 4008 is sandwiched between insulating layers that function as alignment layers. The second electrode layer 4031 is provided on the second substrate 4. 4006 side, and the first electrode layer 4030 and the second electrode layer 4031 are disposed on the liquid crystal layer 4008 The structure is such that the electrodes are laminated via a gap.

[0149] The columnar spacers 4035 are obtained by selectively etching the insulating film. The layer 4008 is provided to control the thickness (cell gap) of the layer 4008. A laser may also be used.

[0150] When liquid crystal elements are used as display elements, thermotropic liquid crystal, low molecular weight liquid crystal, high molecular weight liquid crystal, etc. Liquid crystal, polymer dispersed liquid crystal, ferroelectric liquid crystal, antiferroelectric liquid crystal, etc. can be used. These liquid crystal materials can exhibit cholesteric, smectic, cubic, and chromatic phases depending on the conditions. It shows an isotropic phase, an isotropic phase, etc.

[0151] Alternatively, a liquid crystal that exhibits a blue phase without using an alignment film may be used. When the temperature of the cholesteric liquid crystal is increased, the cholesteric phase transitions to the isotropic phase. The blue phase appears only in a narrow temperature range, so it is necessary to improve the temperature range. In order to improve the chirality, a liquid crystal composition containing a chiral agent of several weight percent or more is used for the liquid crystal layer. A liquid crystal composition containing a liquid crystal exhibiting a blue phase and a chiral agent has a response speed of 1 msec or less. Since the liquid crystal display is short and optically isotropic, no alignment treatment is required, and the viewing angle dependency is small. Since there is no need to provide a counter film, rubbing treatment is also unnecessary. This can prevent electrostatic damage caused by electrostatic discharge, and can reduce defects and damage to liquid crystal display devices during the manufacturing process. Therefore, the productivity of the liquid crystal display device can be improved.

[0152] The specific resistivity of the liquid crystal material is 1×10 9 Ω cm or more, preferably 1×10 11 Ω cm or more, and more preferably 1×10 12 Ω·cm or more. The resistivity values ​​in the specification are values ​​measured at 20°C.

[0153] The size of the storage capacitor provided in the liquid crystal display device is determined by the capacitance of the transistor arranged in the pixel portion. The charge is set so that it can be held for a certain period of time, taking into account factors such as the leakage current. By using a transistor having a semiconductor film, the liquid crystal capacitance of each pixel is It is sufficient to provide a storage volume having a size of 1 / 3 or less, preferably 1 / 5 or less, of the capacity of the do.

[0154] The transistor including the purified oxide semiconductor film used in this embodiment has an off-state Therefore, the current value in the OFF state (off-state current value) can be reduced. The signal retention time can be extended, and the write interval can also be set longer when the power is on. This reduces the frequency of refresh operations, which is effective in reducing power consumption. To bear fruit.

[0155] In addition, the transistor including the purified oxide semiconductor film used in this embodiment has the following characteristics: Since a relatively high field effect mobility can be obtained, high speed operation is possible. By using such a transistor in a pixel portion of a display device, a high-quality image can be provided. In addition, the above transistors are separately manufactured for a driver circuit portion and a pixel portion on the same substrate. This makes it possible to reduce the number of components in the liquid crystal display device.

[0156] There are two types of LCD displays: TN (Twisted Nematic) mode, IPS (In- Plane-Switching mode, FFS (Fringe Field Switching) mode tching) mode, ASM(Axially Symmetric aligned) Micro-cell) mode, OCB(Optical Compensated) Birefringence mode, FLC (Ferroelectric Liquid id Crystal) mode, AFLC (AntiFerroelectric Li quid Crystal mode etc. can be used.

[0157] In addition, normally black type liquid crystal display devices, for example, those using a vertical alignment (VA) mode Here, the vertical alignment mode is a mode in which the liquid crystal display panel is This is a method for controlling the arrangement of liquid crystal molecules, and is used to display the liquid crystal on the panel surface when no voltage is applied. In this method, the liquid crystal molecules are oriented vertically. There are several types of vertical alignment modes: For example, MVA (Multi-domain Vertical Alignment) ent) mode, PVA (Patterned Vertical Alignment ) mode, ASV (Advanced Super View) mode, etc. Also, a pixel can be divided into several regions (subpixels), Multi-domain or multi-domain designs that are designed to flip molecules in different directions A method called "a method for reducing the amount of oxygen in the water" can be used.

[0158] In addition, in display devices, black matrices (light-shielding layers), polarizing members, phase difference members, reflectors, Optical members (optical substrates) such as anti-reflection members are provided as appropriate. For example, a polarizing substrate and a phase A circularly polarized light source such as a backlight or a sidelight may be used as the light source. may also be used.

[0159] In addition, multiple light-emitting diodes (LEDs) are used as backlights to display the image in a time-division format. It is also possible to use the field sequential driving method. By applying the Shar driving method, color display is achieved without using color filters. It is possible.

[0160] In addition, the display method in the pixel section uses the progressive method, interlace method, etc. In addition, the color elements controlled by pixels when displaying colors are RGB (RGB=RGB). The color is not limited to the three colors RGBW (W stands for white). ) or RGB plus one or more colors such as yellow, cyan, or magenta. The size of the display area may be different for each dot of the color element. The present invention is not limited to color display devices, but can also be applied to monochrome display devices. It is also possible.

[0161] In addition, a light-emitting device using electroluminescence is used as a display element included in the display device. The light-emitting element that utilizes electroluminescence can be applied to a light-emitting material They are classified according to whether the material is an organic compound or an inorganic compound. The latter is called an inorganic EL element.

[0162] In an organic EL element, electrons and positive electrodes are released from a pair of electrodes by applying a voltage to the light-emitting element. The holes are then injected into a layer containing a light-emitting organic compound, and a current is passed through them. The recombination of carriers (electrons and holes) causes light-emitting organic compounds to form excited states. When the excited state returns to the ground state, light is emitted. Such a light-emitting element is called a current-excitation type light-emitting element.

[0163] Inorganic EL elements are classified into dispersion type inorganic EL elements and thin film type inorganic EL elements depending on the element structure. Dispersion-type inorganic EL elements have a light-emitting layer in which particles of light-emitting material are dispersed in a binder. The emission mechanism is a donor-based ion exchange reaction that utilizes the donor and acceptor levels. This is an acceptor recombination type emission. Thin-film inorganic EL elements sandwich the light-emitting layer between dielectric layers. The structure is sandwiched between electrodes, and the light emission mechanism is the inner shell electron transition of metal ions. This is a localized light emission that utilizes organic EL elements. do.

[0164] The light emitting element only needs to have at least one of the pair of electrodes transparent in order to extract light. Then, a transistor and a light emitting element are formed on the substrate, and light is emitted from the opposite side of the substrate. Top emission, bottom emission, and side emission. There are light emitting devices with a double-sided emission structure that emits light from the side, and light emitting devices with any emission structure are suitable. It can be used.

[0165] An example of a light-emitting device using a light-emitting element as a display element is shown in FIG. The transistor 4513 is electrically connected to the transistor 4010 provided in the pixel portion 4002. The light-emitting element 4513 includes a first electrode layer 4030, an electroluminescent layer 4511, a second The electrode layer 4031 has a stacked structure, but is not limited to the structure shown in the figure. The structure of the light emitting element 4513 can be changed as appropriate according to the direction of extracted light.

[0166] The partition wall 4510 is formed using an organic insulating material or an inorganic insulating material. An opening is formed on the first electrode layer 4030 using a resin material, and the side wall of the opening is continuous. It is preferable to form the inclined surface so as to have a certain curvature.

[0167] The electroluminescent layer 4511 may be composed of a single layer or a plurality of layers may be laminated. It doesn't matter whether it is completed or not.

[0168] In order to prevent oxygen, hydrogen, moisture, carbon dioxide, and the like from entering the light-emitting element 4513, the second electrode A protective film may be formed on the layer 4031 and the partition wall 4510. The protective film may be a silicon nitride film. Con film, silicon oxynitride film, DLC (Diamond-Like Carbon) film, etc. In addition, the first substrate 4001, the second substrate 4006, and the sheet The space sealed by the sealing material 4005 is sealed with a filling material 4514. A protective film (lamination) that is highly airtight and has little outgassing so that it is not exposed to the outside air. packaging (enclosure) in a covering material (such as a protective film or ultraviolet curing resin film) is preferred.

[0169] Filler 4514 can be inert gas such as nitrogen or argon, or ultraviolet curing resin. Alternatively, thermosetting resin can be used, and PVC (polyvinyl chloride), acrylic, poly Imide, epoxy resin, silicone resin, PVB (Polyvinyl Butyral) or EVA ( Ethylene vinyl acetate) can be used. For example, if nitrogen is used as the filler, good.

[0170] If necessary, a polarizing plate or a circular polarizing plate (including an elliptical polarizing plate) may be attached to the light-emitting surface of the light-emitting element. ), retardation plates (lambda / 4 plates, lambda / 2 plates), color filters, and other optical films are appropriately installed. Alternatively, the polarizing plate or the circular polarizing plate may be provided with an anti-reflection film. It is possible to apply an anti-glare treatment that can diffuse reflected light and reduce glare.

[0171] It is also possible to provide electronic paper that drives electronic ink as a display device. Electronic paper is also called an electrophoretic display device (electrophoretic display). It has the same readability as paper, consumes less power than other display devices, and can be made thin and light. This has the advantage that:

[0172] The electrophoretic display device may have various configurations, but the first particles have a positive charge. and a second particle having a negative charge are mixed into a solvent or solute. By applying an electric field to the microcapsules, By moving the particles in a capsule in opposite directions, only the color of the particles that have gathered on one side is displayed. In addition, the first particles or the second particles contain a dye, and in the absence of an electric field, The first particles and the second particles are different in color (including colorless). (Mm).

[0173] In this way, electrophoretic displays are devices in which materials with high dielectric constants move to areas of high electric field. This is a display that utilizes the so-called dielectrophoretic effect.

[0174] The microcapsules dispersed in a solvent are called electronic ink. This electronic ink can be printed on surfaces such as glass, plastic, fabric, and paper. In addition, a color display is possible by using a color filter or particles having a pigment.

[0175] The first particles and the second particles in the microcapsules are made of a conductive material and an insulating material. , semiconductor materials, magnetic materials, liquid crystal materials, ferroelectric materials, electroluminescent materials, A material selected from the group consisting of magnetochromic materials and magnetophoretic materials, or a composite material of these materials. can be used.

[0176] In addition, display devices using the twist ball display method can also be used as electronic paper. The twist ball display method uses black and white spherical particles as display elements. The electrode layer is disposed between the first electrode layer and the second electrode layer, and the first electrode layer and A display method in which a potential difference is generated in the second electrode layer to control the orientation of the spherical particles. It is law.

[0177] FIG. 9 shows an active matrix electronic paper as one mode of a semiconductor device. The electronic paper of No. 9 is an example of a display device using the twisting ball display method.

[0178] A first electrode layer 4030 connected to a transistor 4010 and a second electrode layer 4006 Between the second electrode layer 4031 and the black area 4615a and the white area 4615b, A spherical particle 4613 is provided having a cavity 4612 around which the cavity is filled with liquid. The spherical particles 4613 are filled with a filler 4614 such as resin. The electrode layer 4031 corresponds to a common electrode (opposite electrode). It is electrically connected to the line.

[0179] In addition, in FIG. 7 to FIG. 9, the first substrate 4001 and the second substrate 4006 are made of Ga. In addition to the glass substrate, a flexible substrate can also be used. For example, a light-transmitting plastic substrate can be used. As for plastic, FRP (Fibreglass) is suitable. SS-Reinforced Plastics) plate, PVF (Polyvinyl Fluoride) ) film, polyester film or acrylic resin film can be used. In addition, sheets with a structure in which aluminum foil is sandwiched between PVF film or polyester film are also available. A marker can also be used.

[0180] The insulating layer 4021 can be formed using an inorganic insulating material or an organic insulating material. In addition, acrylic resin, polyimide, benzocyclobutene resin, polyamide, epoxy resin The use of a heat-resistant organic insulating material such as the above is suitable for the planarizing insulating film. In addition to the above organic insulating materials, low-k materials, siloxane resins, and PSG (phosphorus glass), BPSG (boron phosphorus glass), etc. can be used. The insulating layer may be formed by stacking a plurality of insulating films made of the above-mentioned materials.

[0181] The method for forming the insulating layer 4021 is not particularly limited. Depending on the material, the insulating layer 4021 may be formed by a sputtering method, Spin coating, dipping, spray coating, droplet ejection (inkjet method, screen Printing by means of a combination of techniques such as roll coating, card printing, offset printing, etc. The insulating layer 4021 can also be formed by using ten-coating, knife coating, etc. do.

[0182] A display device transmits light from a light source or a display element to perform display. The thin films such as the substrate, insulating film, and conductive film provided in the pixel area are all in the visible light wavelength range. It is translucent to

[0183] A first electrode layer and a second electrode layer (a pixel electrode layer and a common electrode layer) that apply a voltage to the display element , counter electrode layer, etc.), the direction of the light to be extracted, the location of the electrode layer, The light transmitting property or the light reflecting property can be selected depending on the pattern structure of the electrode layer.

[0184] The first electrode layer 4030 and the second electrode layer 4031 are made of indium tungsten oxide. Oxide, indium zinc oxide with tungsten oxide, indium oxide with titanium oxide Indium tin oxide (ITO) ), indium zinc oxide, indium tin oxide doped with silicon oxide, etc. A conductive material having such a property can be used.

[0185] The first electrode layer 4030 and the second electrode layer 4031 are made of tungsten (W) and molybdenum (Mo). Mo, Zirconium (Zr), Hafnium (Hf), Vanadium (V), Niobium ( Nb), Tantalum (Ta), Chromium (Cr), Cobalt (Co), Nickel (Ni), Metals such as tungsten (Ti), platinum (Pt), aluminum (Al), copper (Cu), and silver (Ag) or its alloy or nitride. can.

[0186] The first electrode layer 4030 and the second electrode layer 4031 are made of a conductive polymer (conductive polymer). The conductive polymer may be a conductive composition containing a conductive polymer. For this purpose, a so-called π-electron conjugated conductive polymer can be used. For example, polyaniline or a derivative thereof, polypyrrole or a derivative thereof, polythiophene or a derivative thereof, Or a copolymer consisting of two or more of aniline, pyrrole and thiophene or a derivative thereof Conductors and the like.

[0187] In addition, since transistors are easily damaged by static electricity, etc., It is preferable to provide a protection circuit using a non-linear element.

[0188] As described above, by using the transistor described in Embodiment 1 as an example, a highly reliable semiconductor device can be obtained. The semiconductor device can be provided by using the transistor exemplified in the first embodiment. Not only semiconductor devices with display functions, but also power devices mounted on power supply circuits, LSI semiconductor integrated circuits such as semiconductor devices having an image sensor function for reading information of an object, The present invention can be applied to semiconductor devices having various functions.

[0189] This embodiment can be implemented in appropriate combination with the configurations described in other embodiments. It is Noh.

[0190] (Embodiment 3) The semiconductor device disclosed in this specification can be applied to various electronic devices (including game machines). The electronic device can be, for example, a television device (television or television (also called digital receivers), computer monitors, digital cameras, digital video cameras, etc. Cameras such as digital cameras, digital photo frames, mobile phones (also called mobile phones or mobile phone devices) (c) Portable game machines, personal digital assistants, audio playback devices, large game machines such as pachinko machines, etc. Examples of electronic devices including the semiconductor device described in the above embodiment include explain.

[0191] FIG. 10A shows a notebook personal computer, which includes a main body 3001 and a housing 30 The embodiment is composed of a display unit 3002, a keyboard 3004, etc. Alternatively, by applying the semiconductor device described in Embodiment 2, a highly reliable notebook type It may be a personal computer.

[0192] FIG. 10B shows a portable digital assistant (PDA), and a main body 3021 includes a display unit 3023 and An external interface 3025 and an operation button 3024 are provided. The stylus 3022 is an accessory for the function. By applying this semiconductor device, a more reliable personal digital assistant (PDA) can be achieved. This can be done.

[0193] FIG. 10C shows an example of an electronic book. For example, an electronic book 2700 has a housing 2 The device is made up of two housings, housing 2701 and housing 2703. 03 is integrated with an axis portion 2711, and performs opening and closing operations around the axis portion 2711. This configuration makes it possible to operate like a paper book. .

[0194] A display unit 2705 is incorporated in the housing 2701, and a display unit 2707 is incorporated in the housing 2703. The display unit 2705 and the display unit 2707 are configured to display a continuous screen. Alternatively, a different screen may be displayed. For example, a text is displayed on the right display unit (display unit 2705 in FIG. 10C) and An image can be displayed on the display unit (display unit 2707 in FIG. 10C). By applying the semiconductor device described in the first or second embodiment, a highly reliable electronic book can be obtained. The number of registered employees can be set at 2,700.

[0195] FIG. 10C shows an example in which an operating unit and the like are provided in the housing 2701. For example, In the housing 2701, a power supply 2721, operation keys 2723, a speaker 2725, etc. are arranged. The operation keys 2723 can be used to turn pages. A keyboard, a pointing device, etc. may be provided on one side. On the back and sides of the device, there are external connection terminals (earphone terminal, USB terminal, etc.), a recording medium insertion port, etc. Furthermore, the electronic book 2700 may have a function as an electronic dictionary. It may be configured such that

[0196] The electronic book 2700 may be configured to transmit and receive information wirelessly. The desired book data can be purchased and downloaded from the electronic book server. It is also possible.

[0197] FIG. 10D shows a mobile phone, which is composed of two housings, a housing 2800 and a housing 2801. The housing 2801 includes a display panel 2802, a speaker 2803, a microphone, and a microphone array. Phone 2804, pointing device 2806, camera lens 2807, external connection The housing 2800 is also provided with a terminal 2808 and the like. It is equipped with a solar cell 2810, an external memory slot 2811, etc. Also, an antenna The semiconductor device shown in the first or second embodiment is built in the housing 2801. By applying the device, a highly reliable mobile phone can be obtained.

[0198] The display panel 2802 is equipped with a touch panel, and in FIG. The multiple operation keys 2805 are indicated by dotted lines. It also includes a boost circuit to boost the input voltage to the voltage required by each circuit.

[0199] The display direction of the display panel 2802 changes appropriately depending on the usage mode. The camera lens 2807 is located on the same surface as the camera 2802, so video calls are possible. The speaker 2803 and the microphone 2804 are not limited to voice calls, The housing 2800 and the housing 2801 can be slid apart. As shown in Fig. 10(D), the unfolded state can be folded up into a folded state, making it easy to carry. It is possible to make the device compact enough to meet the requirements.

[0200] The external connection terminal 2808 can be used to connect to various cables such as an AC adapter and a USB cable. It is possible to charge the battery and to communicate with a personal computer, etc. A recording medium can be inserted into the external memory slot 2811 for storing and transferring a larger amount of data. We can handle it.

[0201] In addition to the above functions, it also has infrared communication function, TV reception function, etc. Good too.

[0202] FIG. 10(E) shows a digital video camera, which includes a main body 3051 and a display unit (A) 3057. , eyepiece 3053, operation switch 3054, display unit (B) 3055, battery 3056 The semiconductor device shown in the first or second embodiment is By using this, a highly reliable digital video camera can be obtained.

[0203] FIG. 10(F) shows an example of a television device. The television device 9600 is A display portion 9603 is incorporated in the housing 9601. In addition, in this example, the housing 9601 is supported by a stand 9605. The semiconductor device shown in the first or second embodiment is applied. This makes it possible to provide a highly reliable television set.

[0204] The television device 9600 can be operated using an operation switch provided on the housing 9601 or a separate remote control. This can be done by a remote control device. A display unit for displaying information output from the input unit may be provided.

[0205] The television device 9600 includes a receiver, a modem, and the like. This allows reception of general television broadcasts, and can also be used for wired or wireless reception via a modem. By connecting to a network, communication can be one-way (sender to receiver) or two-way It is also possible to communicate information in both directions (between sender and receiver, or between receivers). .

[0206] This embodiment can be implemented in appropriate combination with the configurations described in other embodiments. It is Noh. [Explanation of symbols]

[0207] 310 Transistor 320 Transistor 330 Transistor 340 Transistor 350 Transistors 360 Transistor 370 Transistors 380 Transistors 390 Transistors 400 Substrates 401 Gate electrode 402 Gate insulating film 403 Oxide Semiconductor Film 404 Metal oxide film 405a Source electrode 405b Drain electrode 407 Metal oxide film 409 Insulating film 410 Conductive Film 419 Protective insulating film 427 Metal oxide film 500 transistors 2700 e-books 2701 Case 2703 Case 2705 ​​Display section 2707 Display section 2711 Shaft 2721 Power supply 2723 Operation key 2725 Speaker 2800 Chassis 2801 Case 2802 Display Panel 2803 Speaker 2804 Microphone 2805 Operation key 2806 Pointing Device 2807 Camera lenses 2808 External connection terminal 2810 Solar Cell 2811 External memory slot 3001 Main unit 3002 Case 3003 Display section 3004 Keyboard 3021 Main unit 3022 Stylus 3023 Display section 3024 Operation button 3025 External Interface 3051 Main unit 3053 Eyepiece 3054 Operation switch 3055 Display section (B) 3056 Battery 3057 Display section (A) 4001 Board 4002 Pixel section 4003 Signal line driver circuit 4004 Scanning line driver circuit 4005 Sealing material 4006 Substrate 4008 Liquid crystal layer 4010 Transistor 4011 Transistor 4013 Liquid crystal element 4015 Connection terminal electrode 4016 Terminal electrode 4018 FPC 4018a FPC 4018b FPC 4019 Anisotropic conductive film 4021 Insulation layer 4030 Electrode layer 4031 Electrode layer 4032 Insulating film 4033 Insulating film 4035 Spacer 4510 Bulkhead 4511 Electroluminescent layer 4513 Light emitting element 4514 Filling material 4612 Cavity 4613 Spherical particles 4614 Filling material 4615a Black area 4615b White area 9600 Television Equipment 9601 Case 9603 Display section 9605 Stand

Claims

1. A first transistor; a second transistor having a top gate structure, A first conductive layer; and a first insulating layer on the first conductive layer; a first oxide semiconductor layer having a channel formation region of the first transistor over the first insulating layer; a second oxide semiconductor layer having a channel formation region of the second transistor over the first insulating layer; an oxide layer having a region in contact with an upper surface of the first oxide semiconductor layer and a region in contact with an upper surface of the second oxide semiconductor layer; a second conductive layer having a region functioning as a gate electrode of the second transistor; a third conductive layer having a region overlapping with the second oxide semiconductor layer; a fourth conductive layer having a region overlapping with the first oxide semiconductor layer; a fifth conductive layer having a region overlapping with the first oxide semiconductor layer, the oxide layer has a region in contact with a channel formation region of the first transistor, the first conductive layer has a region overlapping with a channel formation region of the first transistor, the second conductive layer has a region overlapping with a channel formation region of the second transistor via a second insulating layer; a region of the third conductive layer overlapping with the second oxide semiconductor layer includes a first region in contact with an upper surface of the second oxide semiconductor layer and a second region not in contact with an upper surface of the second oxide semiconductor layer; a region of the fourth conductive layer overlapping with the first oxide semiconductor layer includes a third region in contact with a top surface of the first oxide semiconductor layer and a fourth region not in contact with a top surface of the first oxide semiconductor layer; the fifth conductive layer has a region overlapping with a channel formation region of the first transistor.

2. A first transistor; a second transistor having a top gate structure, A first conductive layer; and a first insulating layer on the first conductive layer; a first oxide semiconductor layer having a channel formation region of the first transistor over the first insulating layer; a second oxide semiconductor layer having a channel formation region of the second transistor over the first insulating layer; an oxide layer having a region in contact with an upper surface of the first oxide semiconductor layer and a region in contact with an upper surface of the second oxide semiconductor layer; a second conductive layer having a region functioning as a gate electrode of the second transistor; a third conductive layer having a region overlapping with the second oxide semiconductor layer; a fourth conductive layer having a region overlapping with the first oxide semiconductor layer; a fifth conductive layer having a region overlapping with the first oxide semiconductor layer, the oxide layer has a region in contact with a channel formation region of the first transistor, the first conductive layer has a region overlapping with a channel formation region of the first transistor, the second conductive layer has a region overlapping with a channel formation region of the second transistor via a second insulating layer; a region of the third conductive layer overlapping with the second oxide semiconductor layer includes a first region in contact with an upper surface of the second oxide semiconductor layer and a second region not in contact with an upper surface of the second oxide semiconductor layer; a region of the fourth conductive layer overlapping with the first oxide semiconductor layer includes a third region in contact with a top surface of the first oxide semiconductor layer and a fourth region not in contact with a top surface of the first oxide semiconductor layer; the fifth conductive layer has a region overlapping a channel formation region of the first transistor, the first oxide semiconductor layer is In—O; The second oxide semiconductor layer is In—O.

3. In claim 1 or 2, the third conductive layer has a region in contact with a top surface of the oxide layer; the third conductive layer does not have a region in contact with a side surface of the second oxide semiconductor layer.

Citation Information

Patent Citations

  • Thin film transistor and method of forming the same

    JP2008205469A

  • Inverter and operation method of the same, and logic circuit including inverter

    JP2010087518A

  • Inverter, method of operating the same and logic circuit comprising inverter

    US20100079169A1

  • Image display

    JP2006165528A

  • Thin film transistor, method of manufacturing the same, and flat panel display device having thin film transistor

    JP2010016347A