Cement composition and method for manufacturing cement composition

A cement composition with controlled gypsum and fly ash ratios enhances strength development by promoting continuous hydration, addressing emission reduction challenges in cement production.

JP2024166353AActive Publication Date: 2024-11-28MITSUBISHI UBE CEMENT CORP
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
JP2024160824
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-28
Estimated Expiration
2040-03-31

AI Technical Summary

Technical Problem

Existing cement compositions face challenges in achieving sufficient strength development when reducing cement clinker content to lower carbon dioxide emissions, as increasing gypsum or fly ash content can lead to reduced strength, and adjusting cement clinker quality requires additional fuel input, increasing emissions.

Method used

A cement composition comprising cement clinker powder, gypsum powder, and fly ash, with specific ratios of limestone powder and fly ash totaling 10.0% by mass or less, and gypsum powder converted to SO3 at 0.6% to 2.4% by mass, promoting hydration reactions and suppressing rapid aluminate hydration.

Benefits of technology

The composition enhances strength development by promoting continuous hydration of fly ash, reducing the need for fuel input and minimizing carbon dioxide emissions during production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166353000001_ABST
    Figure 2024166353000001_ABST
Patent Text Reader

Abstract

To provide a cement composition which is a cement composition comprising a mixture containing cement clinker powder, gypsum powder, limestone powder and fly ash, and is enhanced in strength developability by gypsum powder and fly ash.SOLUTION: A cement composition comprises a mixture M containing cement clinker powder, gypsum powder, limestone powder L and fly ash A. The limestone powder L and the fly ash A are contained in a ratio of 10.0 mass% or less in total in the mixture M. The gypsum powder is contained in a ratio of 0.6 mass% or more and 2.4 mass% or less in terms of SO3 in the mixture M. It is preferable that the SO3 content of the cement clinker powder is 0.80 mass% or more, and the gypsum powder is contained in a ratio of 1.0 mass% or more in terms of SO3 in the mixture M.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cement composition comprising a mixture containing cement clinker powder, gypsum powder, limestone powder and fly ash, and a method for producing the cement composition. [Background technology]

[0002] A cement composition generally consists of a mixture containing "cement clinker powder, gypsum powder, and admixture powder." The following Patent Document 1 (Example 14) discloses a cement composition using limestone powder and fly ash as the admixture powder.

[0003] In recent years, in order to reduce the amount of carbon dioxide emitted from a cement calciner, it has been considered to reduce the amount of cement clinker produced in the cement calciner and to reduce the content of cement clinker powder in the cement composition and to increase the content of gypsum powder or fly ash. However, if the content of gypsum powder or fly ash in the cement composition is increased in this way, there is a risk that the strength development of the cement composition will not be sufficiently high depending on the composition of the cement composition.

[0004] In order to sufficiently increase the strength development of the cement composition, it is possible to adjust the quality of the cement clinker (for example, the composition of each of the multiple minerals in the cement clinker) in the cement firing process. However, when such an adjustment is made, it becomes necessary to input more fuel into the cement kiln, and therefore there is a risk that the amount of carbon dioxide emissions from the cement firing apparatus will increase even if the amount of cement clinker produced in the cement firing apparatus is reduced. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-172497 A Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, an object of the present invention is to provide a cement composition comprising a mixture containing cement clinker powder, gypsum powder, limestone powder and fly ash, in which the strength development is enhanced by the gypsum powder and fly ash. [Means for solving the problem]

[0007] The first aspect of the present invention relates to a cement composition as follows. This cement composition is a mixture containing cement clinker powder, gypsum powder, limestone powder, and fly ash. The limestone powder and the fly ash are contained in the mixture in a total amount of 10.0 mass% or less. The gypsum powder is contained in the mixture in a ratio of 0.6 mass% or more and 2.4 mass% or less in terms of SO3.

[0008] According to the first item, the mixture contains limestone powder and fly ash at a total content of 10.0% by mass or less, and the mixture contains gypsum powder at a content of 2.4% by mass or less in terms of SO3, so that the mixture contains a small amount of gypsum powder and admixture powder (limestone powder and fly ash). In addition, the mixture contains gypsum powder at a content of 0.6% by mass or more in terms of SO3. Therefore, when this mixture is kneaded with water, the hydration reaction of the fly ash is effectively promoted by the SO3 contained in the gypsum powder, and a high-strength cement kneaded product can be produced. In other words, the cement composition according to the first item increases the strength development of the mixture due to the gypsum powder and fly ash contained in the mixture.

[0009] The second aspect of the present invention includes the following in the first aspect. That is, the SO3 content of the cement clinker powder is 0.80 mass% or more (preferably 0.94 mass% or more). The gypsum powder is contained in the mixture at a rate of 1.0 mass% or more in terms of SO3.

[0010] According to the second item, when the mixture is mixed with water, the large amount of SO3 contained in the gypsum powder suppresses the rapid hydration (flash setting) of the aluminate in the cement clinker powder, and the aluminate contained in the cement clinker powder reacts with the limestone powder. As a result, a large amount of SO3 is eluted from the cement clinker powder, and the large amount of SO3 emitted from the cement clinker powder promotes the hydration of the fly ash, producing a high-strength cement mixture. In other words, the cement composition according to the second item further enhances the strength development of the mixture due to the gypsum powder and fly ash contained in the mixture.

[0011] The second item does not specify the composition range of each of the multiple minerals in the cement clinker powder, but specifies the content of a single chemical component (SO3) in the cement clinker powder. The cement clinker powder in the second item (SO3 content of 0.80 mass% or more) can be easily manufactured by using waste with a high SO3 content as a cement raw material in a cement calcination device, and can be manufactured without inputting a large amount of fuel into the cement kiln to adjust the quality of the cement clinker. Therefore, the second item does not emit a large amount of carbon dioxide in the manufacturing process of the cement clinker powder.

[0012] The third aspect of the present invention includes the following content in the above-mentioned second aspect: In other words, the mixture of the third aspect does not contain cement clinker powder having an SO3 content of 0.56 mass% or less.

[0013] According to the third item, the cement clinker powder with an SO3 content of 0.56 mass% or less is not contained in the mixture, so the ratio of cement clinker powder with an SO3 content of 0.80 mass% or more (content in the mixture) is relatively high. Here, even if the cement clinker powder with an SO3 content of 0.56 mass% or less is mixed with water, it cannot elute an amount of SO3 sufficient to promote the hydration of fly ash. Therefore, the cement composition according to the third item has a high ratio of "cement clinker powder that promotes the hydration of fly ash" to the total amount of cement clinker powder, and the strength development of the mixture is further increased by the gypsum powder and fly ash contained in the mixture.

[0014] The fourth aspect of the present invention is any one of the first to third aspects including the following: That is, when SO3 contained in the cement clinker powder is defined as clinker SO3, SO3 contained in the gypsum powder is defined as gypsum SO3, the ratio of the clinker SO3 to the mixture is defined as S1 mass%, and the ratio of the gypsum SO3 to the mixture is defined as S2 mass%, the total value of the S1 mass% and the S2 mass% is 1.90 mass% or more (preferably 2.05 mass% or more), and the ratio of the S2 mass% to the S1 mass% is 0.90 or more and 3.00 or less (preferably 0.998 or more and 2.837 or less).

[0015] According to the fourth item, the mixture contains a large amount of clinker SO3 and a large amount of gypsum SO3 in a balanced manner. Therefore, when this mixture is mixed with water, gypsum SO3 is dissolved from the gypsum powder in the early stage of mixing, and clinker SO3 is dissolved from the cement clinker powder after the early stage of mixing. As a result, SO3 is dissolved continuously without interruption from the gypsum powder and cement clinker powder in the mixing stage, and this SO3 promotes the hydration of the fly ash continuously without interruption. In other words, the cement composition according to the fourth item further enhances the strength development of the mixture due to the gypsum powder and fly ash contained in the mixture.

[0016] The fifth aspect of the present invention is any one of the first to fourth aspects, including the following: When the TiO2 content, MnO content, P2O5 content, Na2O content and K2O content of the cement clinker powder are defined as T mass%, M mass%, P mass%, N mass% and K mass%, respectively, the physical property value "(T+M+P) / (N+0.658×K)" of the cement clinker powder is 0.80 or more and 1.40 or less.

[0017] According to the fifth item, the cement clinker powder contains evenly the promoting elements (Na2O and K2O) that promote the dissolution of SO3 contained in the cement clinker powder to the outside of the cement clinker powder when the cement clinker powder is hydrated, and the inhibiting elements (TiO2, MnO, and P2O5) that inhibit the dissolution. Therefore, when the cement composition is kneaded with water (when the cement clinker powder contained in this cement composition is hydrated), a large amount of SO3 is dissolved from the cement clinker powder by the promoting elements, and the inhibiting elements prevent the dissolution rate of SO3 from the cement clinker powder from becoming excessively fast, so that a large amount of SO3 contained in the cement clinker powder is gradually dissolved from the cement clinker powder over a long period of time. In other words, when the cement composition is kneaded with water, a large amount of SO3 dissolved from the cement clinker powder can be gradually reacted with the limestone powder and fly ash, so that a cement mixture that exhibits high strength and high fluidity for a long period of time can be produced.

[0018] The sixth aspect of the present invention relates to a method for producing a cement composition as follows. This method includes a finishing step and a mixing step. In the finishing step, cement clinker is pulverized together with gypsum to produce a mixed powder. In the mixing step, the mixed powder, limestone powder, and fly ash are mixed to produce a cement composition. The limestone powder and the fly ash are contained in the cement composition in a total amount of 10.0 mass% or less. The gypsum powder is contained in the cement composition in a proportion of 0.6 mass% or more and 2.4 mass% or less in terms of SO3.

[0019] According to the sixth item, the limestone powder and fly ash are contained in the cement composition at a total ratio of 10.0 mass% or less, and the gypsum powder is contained in the cement composition at a ratio of 2.4 mass% or less in terms of SO3, so that the cement composition contains a small amount of gypsum powder and admixture powder (limestone powder and fly ash). In addition, the gypsum powder is contained in the cement composition at a ratio of 0.6 mass% or more in terms of SO3. Therefore, when this cement composition is mixed with water, the hydration reaction of the fly ash is effectively promoted by the SO3 contained in the gypsum powder, and a high-strength cement mixture can be produced. In other words, according to the sixth item, a cement composition in which strength development is enhanced by the gypsum powder and fly ash can be produced.

[0020] A seventh aspect of the present invention is the method according to the sixth aspect, further comprising a calcination step, in which the cement clinker is produced using waste gypsum boards as a cement raw material.

[0021] According to the seventh item, the strength development of the cement composition can be improved by utilizing the SO3 contained in the waste gypsum board, and the waste gypsum board can be effectively used as a raw material for the cement composition. Effect of the Invention

[0022] As described above, according to the present invention, it is possible to provide a cement composition comprising a mixture containing cement clinker powder, gypsum powder, limestone powder, and fly ash, in which the strength development is enhanced by the gypsum powder and fly ash. [Brief description of the drawings]

[0023] [Figure 1] 1 is an overall configuration diagram showing a cement production apparatus for producing a cement composition according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] FIG. 1 is an overall configuration diagram showing a cement manufacturing apparatus 1 for manufacturing a cement composition according to an embodiment of the present invention. As shown in FIG. 1, the cement manufacturing apparatus 1 includes a clinker silo 2, a finishing mill 3, a classifier 4, a mixer 5, and a cement silo 6. The clinker silo 2 stores clinker (not shown) discharged from a cement calciner (not shown). The finishing mill 3 pulverizes the clinker C discharged from the clinker silo 2 together with gypsum G to produce a pulverized material D (mixed powder). The classifier 4 classifies the pulverized material D discharged from the finishing mill 3 and separates it into coarse powder R and fine powder F. The mixer 5 mixes the fine powder F discharged from the classifier 4 together with limestone powder L and fly ash A to produce a mixture M (cement composition). The cement silo 6 stores the mixture M discharged from the mixer 5. The classifier 4 also returns the coarse powder R to the finishing mill 3. When the finishing mill 3 receives the coarse powder R returned from the classifier 4, the finishing mill 3 pulverizes the clinker C together with the gypsum G and the coarse powder R to produce a pulverized product D.

[0025] A cement composition according to one embodiment of the present invention is composed of a mixture M containing a powder of clinker C, a powder of gypsum G, a powder of limestone L, and a fly ash A. The powder of limestone L and the fly ash A are contained in the mixture M in a total amount of 10.0 mass% or less. The powder of gypsum G is contained in the mixture M in a ratio of 0.6 mass% or more and 2.4 mass% or less in terms of SO3. Preferably, the SO3 content of the powder of clinker C is 0.80 mass% or more (preferably 0.94 mass% or more), and the powder of gypsum G is contained in the mixture M in a ratio of 1.0 mass% or more in terms of SO3. More preferably, the mixture M does not contain a cement clinker powder having a SO3 content of 0.56 mass% or less.

[0026] If the SO3 contained in the powder of clinker C is defined as clinker SO3, the SO3 contained in the powder of gypsum G is defined as gypsum SO3, the ratio of clinker SO3 to mixture M is defined as S1 mass%, and the ratio of gypsum SO3 to mixture M is defined as S2 mass%, then in a cement composition according to one embodiment of the present invention, it is preferable that the total value of S1 mass% and S2 mass% is 1.90 mass% or more (preferably 2.05 mass% or more) and the ratio (proportion) of S2 mass% to S1 mass% is 0.90 or more and 3.00 or less (preferably 0.998 or more and 2.837 or less).

[0027] Preferably, when the TiO2 content, MnO content, P2O5 content, Na2O content and K2O content of the powder of clinker C (contained in the pulverized material D) are defined as T mass%, M mass%, P mass%, N mass% and K mass%, respectively, the physical property value of the powder of clinker C, "(T+M+P) / (N+0.658×K)", is 0.80 or more and 1.40 or less.

[0028] As described above, the method for producing a cement composition according to one embodiment of the present invention includes a finishing step (a grinding step using the finishing mill 3 shown in FIG. 1) and a mixing step (a mixing step using the mixer 5 shown in FIG. 1). In the finishing step, cement clinker (clinker C shown in FIG. 1) is ground together with gypsum (gypsum G shown in FIG. 1) to produce a mixed powder (a mixed powder of clinker C and gypsum G shown in FIG. 1, which is included in the ground product D). In the mixing step, the mixed powder (a mixed powder of clinker C and gypsum G shown in FIG. 1, which is included in the fine powder F), limestone powder (limestone powder L shown in FIG. 1), and fly ash (fly ash A shown in FIG. 1) are mixed to produce a cement composition (mixture M shown in FIG. 1). Note that the method for producing a cement composition according to the present invention is not limited to the method using the cement production apparatus 1 shown in FIG. 1.

[0029] The method for producing a cement composition according to one embodiment of the present invention may further include a firing step (a step of producing clinker C shown in FIG. 1 in the upstream stage of the production apparatus 1 shown in FIG. 1). In this case, in this firing step, cement clinker (clinker C shown in FIG. 1) is produced using waste gypsum boards (not shown) as a cement raw material.

[0030] Next, an experimental example of the cement composition according to the present invention will be described. In this experimental example, various cement compositions were produced by mixing cement clinker powder (Cli1 to Cli6), gypsum powder, and admixture powder (limestone powder, fly ash, and blast furnace slag powder) in various ratios, and the "compressive strength at 28 days" of the cement mixture produced from each of these cement compositions was measured. Tables 1 to 4 show the composition or physical properties of the raw materials of the cement compositions used in this experimental example for each raw material. Tables 5 to 11 show the relationship between the composition of the cement composition produced in this experimental example and the strength development for each experimental example. Table 12 shows the physical property values ​​of the cement composition produced in this experimental example for each experimental example.

[0031] In Tables 1 to 12, "clinker" means cement clinker powder, "gypsum" means gypsum powder, "admixture" means admixture powder, "limestone" means limestone powder, and "blast furnace slag" means blast furnace slag powder.

[0032] Table 1 shows the content (mass%) of each compound in the cement clinker powder (corresponding to the powder of clinker C shown in Figure 1) used in the above experimental example. In Table 1, ig.loss (Ignition Loss) means ignition raw material (volatile substance). Na2Oeq means total alkali. Total alkali is a value calculated by the formula "Na2O+0.658×K2O". f.CaO means free calcium oxide. Free calcium oxide refers to calcium oxide that remains without reacting with silicon dioxide or aluminum oxide when cement raw materials are burned.

[0033] [Table 1]

[0034] Table 2 shows the modulus of the cement clinker powder used in the above experimental example. In Table 2, HM (Hydraulic Modulus) indicates the hydraulic modulus, SM (Silica Modulus) indicates the silica modulus, IM (Iron Modulus) indicates the iron modulus, and AI (Activity Index) indicates the activity index. HM is the ratio of CaO to (SiO2 + Al2O3 + Fe2O3). SM is the ratio of SiO2 to (Al2O3 + Fe2O3). IM is the ratio of Al2O3 to Fe2O3. AI is the ratio of SiO2 to Al2O3. As shown in Table 2, the modulus of the cement clinker powder used in the above experimental example is as follows: HM is 2.15 to 2.21, SM is 2.18 to 2.42, IM is 1.87 to 2.18, and AI is 3.19 to 3.70.

[0035] Table 2 also shows the mineral composition of the cement clinker powder used in the above experimental example. The mineral composition shown in Table 2 was calculated by the Bogue formula. In Table 2, C3S is tricalcium silicate (3CaO·SiO2), C2S is dicalcium silicate (2CaO·SiO2), C3A is tricalcium aluminate (3CaO·Al2O3), and C4AF is tetracalcium aluminate ferroaluminate (4CaO·Al2O3·Fe2O3). As shown in Table 2, the mineral composition of the cement clinker powder used in the above experimental example is as follows: C3S is 55.2 mass% or more and 62.0 mass% or less, C2S is 12.7 mass% or more and 18.6 mass% or less, C3A is 10.1 mass% or more and 12.2 mass% or less, and C4AF is 9.1 mass% or more and 9.6 mass% or less.

[0036] Furthermore, Table 2 shows the physical property values ​​of the cement clinker powder used in the above experimental example. These physical property values ​​indicate the ratio of the strength development inhibition index value to the strength development promotion index value in the cement clinker powder. This strength development promotion index value is the total alkali content in the cement clinker powder. This strength development inhibition index value is the total content (mass%) of TiO2, MnO, and P2O5 in the cement clinker powder. As shown in Table 2, the above physical property values ​​of the cement clinker powder used in this experimental example are 0.853 or more and 1.326 or less.

[0037] [Table 2]

[0038] Table 3 shows the chemical compositions of the limestone powder, fly ash, and blast furnace slag powder used in the above experimental examples.

[0039] [Table 3]

[0040] Table 4 shows the specific surface area (Blaine specific surface area) and activity index of the limestone powder, blast furnace slag powder, and fly ash used in the above experimental examples. Here, the activity index is at the time when the material is 28 days old.

[0041] [Table 4]

[0042] Tables 5 to 11 show the type of cement clinker powder used in the cement compositions, the SO3-equivalent gypsum powder content (mass%), limestone powder content (mass%), fly ash content (mass%), total admixture powder content (total content of limestone powder, fly ash, and blast furnace slag powder: mass%) of the cement compositions, and the "compressive strength at 28 days (N / mm 2 )" relationship.

[0043] In Table 5, the set of Experimental Examples A1 to A4 shows the following: In a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, limestone powder, and fly ash, if the gypsum powder content is 0.6 mass% or more and 2.4 mass% or less in terms of SO3, the compressive strength of the cement mixture increases as the gypsum powder content of the cement composition increases. The set of Experimental Examples A5 to A8 shows the following: That is, even when the total content of limestone powder and fly ash (total content of admixture powders) is changed from 7.5 mass% to 10.0 mass% in the set of Experimental Examples A1 to A4, the compressive strength of the cement mixture increases as the gypsum powder content of the cement composition increases.

[0044] In Table 5, the set of Experimental Examples A9 to A12, the set of Experimental Examples A13 to A16, the set of Experimental Examples A17 to A20, and the set of Experimental Examples A21 to A24 show the following: That is, even when the type of clinker is changed in the set of Experimental Examples A1 to A4 and the set of Experimental Examples A5 to A8, the compressive strength of the cement mixture increases as the gypsum powder content of the cement composition increases (or, even when the gypsum powder content of the cement composition increases, the compressive strength of the cement mixture is maintained without decreasing).

[0045] [Table 5]

[0046] In Table 6, the set of Experimental Examples a1 to a24 shows the following: In a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, and limestone powder, even if the gypsum powder content is 1.2 mass% or more and 2.4 mass% or less in terms of SO3, if fly ash is not contained, the compressive strength of the cement mixture decreases as the gypsum powder content or limestone powder content of the cement composition increases.

[0047] [Table 6]

[0048] From the above, the following conclusions can be derived from the experimental examples shown in Tables 5 and 6. In other words, in a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, limestone powder, and fly ash, if the limestone powder and fly ash are contained in a total amount of 10.0 mass% or less, and the gypsum powder is contained in an amount of 0.6 mass% to 2.4 mass% in terms of SO3, when this cement composition is kneaded with water, the hydration reaction of the fly ash is effectively promoted by the SO3 contained in the gypsum powder, and a high-strength cement mixture can be produced. In other words, such a cement composition has a high strength development due to the gypsum powder and fly ash contained in the mixture.

[0049] Table 7 rearranges the experimental examples A1 to A24 shown in Table 5. The set of experimental examples A1 and A5 shows the following: In a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, limestone powder, and fly ash, if the gypsum powder content is 0.6 mass% in terms of SO3, the compressive strength of the cement mixture decreases as the fly ash content of the cement composition increases.

[0050] On the other hand, in Table 7, the set of Experimental Examples A2 and A6, the set of Experimental Examples A3 and A7, and the set of Experimental Examples A4 and A8 show the following: That is, in the sets of Experimental Examples A1 and A5, when the gypsum powder content was set to 1.2 mass%, 1.8 mass%, or 2.4 mass% in terms of SO3, the compressive strength of the cement mixture increased as the fly ash content of the cement composition increased.

[0051] In Table 7, the set of Experimental Examples A9 and A13, the set of Experimental Examples A10 and A14, the set of Experimental Examples A11 and A15, the set of Experimental Examples A12 and A16, the set of Experimental Examples A17 and A21, the set of Experimental Examples A18 and A22, the set of Experimental Examples A19 and A23, and the set of Experimental Examples A20 and A24 show the following: Even when the type of cement clinker powder is changed in the sets of Experimental Examples A1 and A5, if the gypsum powder content is 0.6 mass% in terms of SO3, the compressive strength of the cement mixture decreases as the fly ash content of the cement composition increases, and if the gypsum powder content is 1.2 mass% or more and 2.4 mass% or less in terms of SO3, the compressive strength of the cement mixture increases as the fly ash content of the cement composition increases.

[0052] [Table 7]

[0053] In Table 8, the set of Experimental Examples B1 and B2 shows the following: That is, even when the content of gypsum powder in the cement composition in the set of Experimental Examples A1 and A5 shown in Table 7 is set to 1.0 mass% in terms of SO3, the compressive strength of the cement mixture increases as the fly ash content of the cement composition increases.

[0054] [Table 8]

[0055] Table 9 is a rearrangement of the experimental examples a1 to a24 shown in Table 6. In Table 9, the set of experimental examples a1 to a24 shows the following: In a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, and limestone powder, even if the total content of the admixture powder is 10.0 mass% or less and the content of the gypsum powder is 1.2 mass% or more and 2.4 mass% or less in terms of SO3, if fly ash is not contained, the compressive strength of the cement mixture decreases as the content of the admixture powder in the cement composition increases.

[0056] [Table 9]

[0057] In Table 10, the set of Experimental Examples C1 and C2 shows the following. That is, when Cli5 is used instead of Cli1 in the set of Experimental Examples A2 and A6 shown in Table 7, even if the gypsum powder content is 1.2 mass% in terms of SO3 and the total content of limestone powder and fly ash (total content of admixture powder) is 10.0 mass% or less, the compressive strength of the cement mixture decreases as the fly ash content of the cement composition increases. As shown in Table 1, the SO3 content of Cli1 to Cli4 (cement clinker powder used in Experimental Examples A1 to A24 and Experimental Examples B1 and B2) is 0.94 mass% or more, while the SO3 content of Cli5 used in Experimental Examples C1 and C2 is 0.56 mass%.

[0058] [Table 10]

[0059] From the above, the following conclusions can be derived from the experimental examples shown in Tables 7 to 10. That is, in a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, limestone powder, and fly ash, if the limestone powder and fly ash are contained in a total amount of 10.0 mass% or less, the gypsum powder is contained in a ratio of 1.0 mass% to 2.4 mass% in terms of SO3, and the SO3 content of the cement clinker powder is 0.80 mass% or more (strictly 0.94 mass% or more), when this cement composition is kneaded with water, the rapid hydration (flash setting) of the aluminate in the cement clinker powder is suppressed by the large amount of SO3 contained in the gypsum powder, and the aluminate contained in the cement clinker powder reacts with the limestone powder. As a result, a large amount of SO3 is dissolved from the cement clinker powder, and the hydration of the fly ash is promoted by the large amount of SO3 dissolved from the cement clinker powder, and a high-strength cement mixture is produced. In other words, in such a cement composition, the strength development of the mixture is further increased by the gypsum powder and fly ash contained in the mixture.

[0060] Furthermore, cement clinker powder with an SO3 content of 0.56 mass% or less cannot dissolve an amount of SO3 sufficient to promote the hydration of fly ash even when mixed with water. Therefore, if the cement composition does not contain cement clinker powder with an SO3 content of 0.56 mass% or less, the ratio of "cement clinker powder that promotes the hydration of fly ash" to the total amount of cement clinker powder in the cement composition will be high, and the strength development of the cement composition will be further enhanced by the gypsum powder and fly ash contained in the cement composition.

[0061] In Table 11, the set of Experimental Examples D1 and D2 and the set of Experimental Examples D3 and D4 show the following: In other words, in a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, limestone powder, and fly ash, if the limestone powder and fly ash are contained in a total amount of 10.0 mass% or less, and the gypsum powder is contained in an amount of 0.6 mass% or more and 2.4 mass% or less in terms of SO3, it is considered that the compressive strength of the cement mixture increases as the fly ash content of the cement composition increases, even if blast furnace slag powder is further contained.

[0062] [Table 11]

[0063] Table 12 will be explained next, but before that, Tables 5 and 10 will be mentioned again. Referring to the set of Experimental Examples A1 to A4, the set of Experimental Examples A5 to A8, the set of Experimental Examples A9 to A12, the set of Experimental Examples A13 to A16, the set of Experimental Examples A17 to A20, and the set of Experimental Examples A21 to A24 in Table 5, the compressive strength of the cement mixture increases sharply when the gypsum powder content increases from 0.6% by mass to 1.2% by mass in SO3 conversion, but even if the gypsum powder content increases from 1.2% by mass to 1.8% by mass and to 2.4% by mass in SO3 conversion, the compressive strength of the cement mixture increases only slightly.

[0064] That is, among these experimental examples, "experimental examples in which the gypsum powder content is 1.2 mass%, 1.8 mass%, or 2.4 mass% converted into SO3" (hereinafter referred to as "Experimental Example X Group") maximizes the strength development of the cement composition by the gypsum powder contained in the cement composition. Also, among these experimental examples, "experimental example in which the gypsum powder content is 0.6 mass% converted into SO3" (hereinafter referred to as "Experimental Example Y1 Group") increases the strength development of the cement composition by the gypsum powder contained in the cement composition, but does not maximize it.

[0065] As described above in the explanation of Table 7, in the "experimental examples in which the gypsum powder content is 1.2 mass%, 1.8 mass%, or 2.4 mass% in terms of SO3" (experimental example X group), the compressive strength of the cement mixture increases as the fly ash content of the cement composition increases. In the "experimental example in which the gypsum powder content is 0.6 mass% in terms of SO3" (experimental example Y1 group), the compressive strength of the cement mixture decreases as the fly ash content of the cement composition increases. On the other hand, in the set of experimental examples C1 and C2 shown in Table 10 (hereinafter referred to as "experimental example Y2 group"), even if the gypsum powder content is 1.2 mass% in terms of SO3, the SO3 content of the cement clinker powder is low, so that the compressive strength of the cement mixture decreases as the fly ash content of the cement composition increases.

[0066] Table 12 shows "S1+S2" and "S2 / S1" for each of the experimental examples, group X, group Y1, and group Y2. In the case where the SO3 contained in the cement clinker powder is defined as clinker SO3, the SO3 contained in the gypsum powder is defined as gypsum SO3, the ratio of the clinker SO3 to the cement composition is defined as S1 mass%, and the ratio of the gypsum SO3 to the cement composition is defined as S2 mass%, "S1+S2" is the total value of S1 mass% and S2 mass%, and "S2 / S1" is the ratio (proportion) of S2 mass% to S1 mass%.

[0067] In the experimental example X group, "S1+S2" is 2.05 or more and 3.60 or less, and "S2 / S1" is 0.998 or more and 2.837 or less. In the experimental examples Y1 and Y2 groups, "S1+S2" is 1.80 or less, and "S2 / S1" is 0.499 or more and 2.381 or less. In other words, in the cement composition, "S1+S2" is 2.05 or more and 3.60 or less, and "S2 / S1" is 0.998 or more and 2.837 or less, so that the strength development of the cement composition is maximized by the gypsum powder and fly ash contained in the cement composition.

[0068] In addition, considering that "S1+S2" of Experimental Examples Y1 and Y2 is lower than "S1+S2" of Experimental Example X, even if "S1+S2" exceeds 3.60 in a cement composition, as long as "S2 / S1" is 0.998 or more and 2.837 or less, it is considered that the strength expression of the cement composition can be maximized by the gypsum powder and fly ash contained in the cement composition.

[0069] [Table 12]

[0070] From the above, the following conclusion can be derived from the experimental examples shown in Table 12. That is, in a cement composition consisting of a mixture containing cement clinker powder, gypsum powder, limestone powder, and fly ash, if the limestone powder and fly ash are contained in a total amount of 10.0 mass% or less, the gypsum powder is contained in an amount of 0.6 mass% or more and 2.4 mass% or less in terms of SO3, "S1 + S2" is 1.90 or more (strictly 2.05 or more), and "S2 / S1" is 0.90 or more and 3.00 or less (strictly 0.998 or more and 2.837 or less), then a large amount of clinker SO3 and a large amount of gypsum SO3 are contained in the cement composition in a balanced manner.

[0071] Therefore, when this cement composition is mixed with water, gypsum SO3 is dissolved from the gypsum powder in the initial mixing stage, and clinker SO3 is dissolved from the cement clinker powder after the initial mixing stage. As a result, SO3 is dissolved continuously without interruption from the gypsum powder and cement clinker powder in the mixing stage, and this SO3 promotes the hydration of the fly ash continuously without interruption. Therefore, it is considered that the strength development of such a cement composition is further increased by the gypsum powder and fly ash contained in the mixture. [Explanation of symbols]

[0072] 1. Cement manufacturing equipment 2. Clinker silo 3 Finishing Mill 4 Classifier 5 Mixing device 6. Cement Silo A Fly ash C Clinker D. Crushed material F Fine powder G plaster L limestone powder M mixture R Coarse powder

Claims

1. A cement composition comprising a mixture containing cement clinker powder, gypsum powder, limestone powder and fly ash, The limestone powder and the fly ash are contained in the mixture in a total amount of 10.0% by mass or less, The gypsum powder is added to the mixture. 3 A cement composition characterized in that it contains 0.6 mass% or more and 2.4 mass% or less of sulphuric acid or sulphuric acid.

2. The cement clinker powder SO 3 The content is 0.80% by mass or more, The gypsum powder is added to the mixture. 3 2. The cement composition according to claim 1, characterized in that it is contained in an amount of 1.0 mass% or more in terms of converted value.

3. In the mixture, SO 3 3. The cement composition according to claim 2, characterized in that it does not contain cement clinker powder having a content of 0.56 mass% or less.

4. The SO contained in the cement clinker powder 3 Clinker SO 3 and the SO contained in the gypsum powder is defined as 3 Plaster SO 3 and the clinker SO 3 The ratio of the gypsum SO to the mixture is defined as S1 mass%. 3 When the ratio of is defined as S2 mass%, The total value of the S1 mass% and the S2 mass% is 1.90 mass% or more, and the ratio of the S2 mass% to the S1 mass% is 0.90 to 3.

00. The cement composition according to any one of claims 1 to 3.

5. The cement clinker powder has a TiO 2 content, MnO content, P 2 O 5 Content rate, Na 2 O content and K 2 The cement composition according to any one of claims 1 to 4, characterized in that the physical property value of the cement clinker powder, "(T + M + P) / (N + 0.658 × K)", in which the O contents are defined as T mass%, M mass%, P mass%, N mass% and K mass%, respectively, is 0.80 or more and 1.40 or less.

6. A method for producing a cement composition, comprising: It is equipped with a finishing process and a mixing process, In the finishing step, the cement clinker is ground together with gypsum to produce a mixed powder; In the mixing step, the mixed powder, limestone powder and fly ash are mixed to produce a cement composition, The limestone powder and the fly ash are contained in the cement composition in a total amount of 10.0% by mass or less, The gypsum powder is added to the cement composition to form a SO 3 A method for producing a cement composition, characterized in that the content is 0.6 mass% or more and 2.4 mass% or less, calculated as a percentage.

7. Further comprising a baking step; The method for producing a cement composition according to claim 6, characterized in that in the burning step, the cement clinker is produced using waste gypsum board as a cement raw material.

Citation Information

Patent Citations

  • Cement composition and cement-based solidifying material

    JP2009062260A

  • Hydraulic composition

    JP2011184253A

  • Hydraulic composition

    JP2011225393A

  • Hydraulic composition

    JP2011225394A

  • Cement clinker and cement composition

    JP2012025635A