Battery, and method for manufacturing polymer porous membrane

A porous polymer membrane with a controlled non-porous layer ratio addresses ion permeation and dendrite issues, enhancing battery performance by preventing short circuits.

JP2024166361AActive Publication Date: 2024-11-28TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2024161079
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-28
Estimated Expiration
2042-02-15

AI Technical Summary

Technical Problem

Porous polymer membranes used as separators in batteries often include a non-porous layer that inhibits ion permeation, rendering them ineffective, and the growth of dendrites can lead to short circuits.

Method used

A porous polymer membrane with a first layer having a three-dimensional network structure and a second non-porous layer that accounts for less than 10% of the total membrane thickness, allowing ion permeability and inhibiting dendrite growth, is produced through controlled phase separation.

Benefits of technology

The membrane effectively functions as a separator, improving short circuit resistance and preventing dendrite growth, thereby enhancing battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024166361000001_ABST
    Figure 2024166361000001_ABST
Patent Text Reader

Abstract

To provide a new polymer porous membrane.SOLUTION: A polymer porous membrane includes a first layer and a second layer. The first layer is porous. The first layer has a three-dimensional network structure. The second layer is non-porous in an image at a magnification of 50000 times. The ratio of the second layer is larger than 0% and less than 10%. The ratio of the second layer is determined by the formula "the ratio of the second layer (%)=(t2 / t0)×100." t0 represents the thickness of the polymer porous membrane. t2 represents the thickness of the second layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a porous polymer membrane, a separator for a battery, an electrode unit, an electrode framework, a battery, and a method for producing a porous polymer membrane. [Background technology]

[0002] JP 2020-123453 A (Patent Document 1) discloses forming a separator layer by a phase separation method. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2020-123453 A Summary of the Invention [Problem to be solved by the invention]

[0004] It has been proposed to form a polymer porous membrane by phase separation induced during the drying process of a multi-component solution (hereinafter also referred to as "drying-induced phase separation"). The polymer porous membrane can be used, for example, as a battery separator. Hereinafter, the polymer porous membrane can be abbreviated as "porous membrane".

[0005] The multi-component solution includes a polymeric material, a good solvent, and a poor solvent. When drying, the solvent evaporates from the surface of the solution. This can cause a composition difference between the surface layer of the solution and the bulk of the solution. As a result, the porous membrane can be formed to include a first layer and a second layer. The first layer is a base layer of the porous membrane. The first layer can have a three-dimensional mesh structure. The second layer can be formed on the outermost surface of the porous membrane. The second layer is non-porous. The presence of pores in the second layer cannot be confirmed even in a 50,000x SEM (Scanning Electron Microscope) image.

[0006] In a battery, the second layer (non-porous layer) may inhibit the permeation of ions, i.e., when the porous membrane includes the second layer, the porous membrane may not function as a separator.

[0007] An object of the present disclosure is to provide a novel porous polymer membrane. [Means for solving the problem]

[0008] The technical configuration and effects of the present disclosure will be described below. However, the mechanism of action in this specification includes assumptions. The mechanism of action does not limit the technical scope of the present disclosure.

[0009] 1. The polymeric porous membrane includes a first layer and a second layer. The first layer is porous. The first layer has a three-dimensional network structure. The second layer is non-porous in an image with a magnification of 50,000 times. The proportion of the second layer is greater than 0% and less than 10%. The proportion of the second layer is determined by the following formula (I). Ratio of second layer (%) = (t2 / t0) × 100 (I) "t0" indicates the thickness of the porous polymer membrane. "t2" indicates the thickness of the second layer.

[0010] According to the new findings of the present disclosure, when the proportion of the second layer (non-porous layer) in the entire membrane is less than 10%, the second layer becomes ion permeable. In other words, a porous membrane containing the second layer at a proportion of less than 10% can function as a separator. Furthermore, it has been found that the presence of the second layer provides benefits. In other words, the presence of the second layer is expected to improve the short-circuit resistance of the battery. This is thought to be because the second layer inhibits the growth of dendrites.

[0011] 2. The second layer may have a proportion of, for example, 2 to 8%.

[0012] 3. The second layer may have a thickness of, for example, 0.5 to 1.5 μm.

[0013] 4. The first layer may have an average pore size of, for example, 500 to 2000 nm.

[0014] 5. The three-dimensional network structure may, for example, include an open pore structure.

[0015] For example, bubble-like pores may partially overlap each other to form a three-dimensional network structure.

[0016] 6. The polymer porous membrane may contain, for example, at least one selected from the group consisting of ethylene-vinyl alcohol copolymer (EVOH), polyvinylidene fluoride (PVDF), and polyvinyl alcohol (PVA).

[0017] The raw material of the porous membrane may be a water-insoluble polymer or a water-soluble polymer.

[0018] 7. The porous polymer membrane may have an air permeability of, for example, 32 to 600 s / 100 ml.

[0019] 8. The polymeric porous membrane may have a porosity of, for example, 50 to 72%.

[0020] 9. The polymeric porous membrane may have a thickness of, for example, 16 to 25 μm.

[0021] 10. The battery separator comprises a porous polymer membrane.

[0022] The porous membrane can be used, for example, as a battery separator. Hereinafter, the term "battery separator" may be abbreviated to "separator".

[0023] 11. The electrode unit includes a porous polymer membrane and an electrode. The porous polymer membrane is attached to the surface of the electrode.

[0024] The porous membrane may be used, for example, in an electrode unit, which is a member in which a separator and an electrode are integrated.

[0025] 12. The electrode framework comprises a porous polymeric membrane.

[0026] 13. A battery includes a first electrode, a separator, a second electrode, and an electrolyte. The second electrode has a different polarity than the first electrode. The separator separates the second electrode from the first electrode. The separator includes a porous polymer membrane.

[0027] The battery of "13." above may include at least one of the separator of "10." and the electrode unit of "11.".

[0028] 14. A battery includes a first electrode, a second electrode, and an electrolyte. The second electrode has a different polarity than the first electrode. The second electrode includes an electrode framework. The second electrode is configured to be charged by a deposition reaction of a metal in voids in the first layer, and to be discharged by a dissolution reaction of the metal.

[0029] The present disclosure also provides a new application of the porous membrane. The electrode framework provides a reaction field for the active material (metal) in a dissolution-precipitation type battery. The metal can dissolve and precipitate in the voids in the electrode framework (first layer). Dissolution-precipitation type batteries are expected to have a high capacity. Conventionally, dissolution-precipitation type batteries have a problem with dendrites. That is, the growth of metal dendrites may cause an internal short circuit. For example, it is expected that the metal will not become dendrites but will become lumpy by precipitating the metal in the voids (bubble-like pores) of the first layer. It is also expected that the volume change of the electrode due to the dissolution and precipitation of the metal will be mitigated. Furthermore, it is expected that the presence of the second layer will confine the metal within the first layer.

[0030] 15. A method for producing a porous polymer membrane includes the following steps (a) to (c): (a) A polymer solution is prepared by mixing a polymer material with a good solvent and a poor solvent. (b) Form a liquid film of the polymer solution. (c) The liquid membrane is dried to produce a porous polymer membrane. A poor solvent has a higher boiling point than a good solvent. The polymeric porous membrane includes a first layer and a second layer. The first layer is porous. The first layer has a three-dimensional network structure. The second layer is non-porous in an image with a magnification of 50,000 times. The thickness ratio of the second layer is greater than 0% and less than 10%. The thickness ratio of the second layer is calculated by the above formula (I).

[0031] The porous membrane can be formed by drying-induced phase separation. For example, the ratio of the second layer can be adjusted by combining the "type of polymer material, good solvent, and poor solvent," the "combination of materials," the "mixing ratio of materials," and the "drying conditions."

[0032] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the example do not limit the technical scope of the present disclosure. [Brief description of the drawings]

[0033] [Figure 1] FIG. 1 is an example of a cross-sectional SEM image of a porous polymer membrane in this embodiment. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing a porous polymer membrane in this embodiment. [Diagram 3] FIG. 3 is a schematic flow chart of the method for producing a porous polymer membrane in this embodiment. [Figure 4] FIG. 4 is a schematic cross-sectional view showing the configuration of the first battery in this embodiment. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing the configuration of the second battery in the present embodiment. [Figure 6] FIG. 6 shows cross-sectional and surface SEM images of Nos. 1 to 5. [Figure 7] FIG. 7 shows cross-sectional and surface SEM images of Nos. 6 to 8. [Figure 8] FIG. 8 is a graph showing the measurement results of the DC internal resistance. [Figure 9]FIG. 9 is a graph showing the results of the initial charge and discharge. [Figure 10] FIG. 10 shows cross-sectional SEM images of Nos. 9 to 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] <Definitions of terms, etc.> The words "comprise," "include," "have," and variations thereof (e.g., "consisting of") are open-ended. The open-ended form may or may not include additional elements in addition to the required elements. The words "consisting of" are closed-ended. However, the closed form does not exclude additional elements that are normally associated with the technology or that are unrelated to the technology disclosed. The words "consisting essentially of" are semi-closed. The semi-closed form allows for the addition of elements that do not substantially affect the basic and novel characteristics of the technology disclosed.

[0035] Expressions such as "may" and "may" are used in the permissive sense, meaning "to have the possibility," rather than in the obligatory sense, meaning "to have to."

[0036] Elements expressed in the singular form include the plural form unless otherwise specified. For example, a "particle" can mean not only "one particle" but also "an aggregate of particles (powder, powder, particle group)."

[0037] Unless otherwise specified, the order of execution of the steps, operations, and the like included in various methods is not limited to the order described. For example, the steps may proceed simultaneously. For example, the steps may be performed in sequence.

[0038] For example, a numerical range such as "m to n%" includes the upper limit and the lower limit unless otherwise specified. That is, "m to n%" indicates a numerical range of "m% or more and n% or less". "m% or more and n% or less" also includes "greater than m% and less than n%". "Greater than m%" can also be written as "more than m%". Furthermore, a numerical value arbitrarily selected from within the numerical range may be set as a new upper limit or lower limit. For example, a new numerical range may be set by arbitrarily combining a numerical value within the numerical range with a numerical value described in another part, table, figure, etc. of this specification.

[0039] All numerical values ​​are modified by the term "about." The term "about" may mean, for example, ±5%, ±3%, ±1%, etc. All numerical values ​​may be approximations that may vary depending on the application of the disclosed technology. All numerical values ​​may be expressed with significant figures. Measurements may be average values ​​of multiple measurements. The number of measurements may be three or more, five or more, or ten or more. In general, the more measurements are taken, the more reliable the average value is expected to be. Measurements may be rounded off based on the number of significant figures. Measurements may include errors associated with, for example, the detection limits of the measuring device.

[0040] When a compound is expressed by a stoichiometric composition formula (e.g., "LiCoO2", etc.), the stoichiometric composition formula is merely a representative example of the compound. The compound may have a non-stoichiometric composition. For example, when lithium cobalt oxide is expressed as "LiCoO2", unless otherwise specified, the lithium cobalt oxide is not limited to the composition ratio of "Li / Co / O=1 / 1 / 2" and may contain Li, Co, and O in any composition ratio. Furthermore, doping, substitution, etc. with trace elements may also be allowed.

[0041] Geometric terms (e.g., "parallel," "perpendicular," "orthogonal," etc.) should not be interpreted in a strict sense. For example, "parallel" may deviate slightly from the strict meaning of "parallel." Geometric terms in this specification may include, for example, tolerances, errors, etc. in design, work, manufacturing, etc. The dimensional relationships in each figure may not match the actual dimensional relationships. In order to facilitate understanding of the disclosed technology, the dimensional relationships (length, width, thickness, etc.) in each figure may be changed. Furthermore, some configurations may be omitted.

[0042] The "thickness of the porous membrane" can be measured by a constant pressure thickness measuring device. For example, a product named "PG-01" (or an equivalent product) manufactured by Techlock Co., Ltd. can be used. The measurement pressure is 0.8N.

[0043] The structure of the porous membrane can be identified by the following procedure: A sample of a predetermined size is cut out from the porous membrane. The sample is coated with platinum (Pt) to reduce the charge of the sample. The sample is immersed in liquid nitrogen. The sample is cooled sufficiently. After cooling, the sample is fractured. The fractured surface of the sample is observed with a Field Emission Scanning Electron Microscope (FE-SEM). For example, a JEOL product named "JSM-7100F" (or an equivalent product) may be used.

[0044] FIG. 1 is an example of a cross-sectional SEM image of a polymeric porous membrane in this embodiment. The surface layer of the porous membrane is observed at a magnification of 50,000 times. If there are no open pores opening on the surface of the porous membrane at 10 randomly selected locations, it is considered that a second layer is present that is "non-porous in an image with a magnification of 50,000 times". Since ions pass through the second layer, nanoscale pores that cannot be confirmed at a magnification of 50,000 times may be formed in the second layer. For example, pores having a maximum Feret diameter of 100 nm or less may be formed.

[0045] The thickness (t2) of the second layer is measured. The thickness (t0) of the porous membrane is measured using the constant pressure thickness gauge described above. The proportion of the second layer is calculated using the above formula (I).

[0046] The "average pore diameter" is determined by the following procedure. A cross-sectional SEM image of the first layer is prepared. The magnification of the image may be, for example, 2,000 to 5,000 times. The first layer is observed in the cross-sectional SEM image. The maximum Feret diameter of 100 pores (bubble-like pores) is measured. The arithmetic mean of the 100 maximum Feret diameters is regarded as the average pore diameter.

[0047] "Air permeability" refers to the "air resistance" defined in "JIS P8117". Air permeability can be measured by a Gurley tester. For example, a Gurley densometer (or an equivalent product) manufactured by Toyo Seiki Seisakusho can be used.

[0048] The "porosity" is measured by the following procedure: A sample of a given size is cut out from the porous membrane. For example, a punch or the like may be used. The mass and thickness of the sample are measured. The volume of the sample is calculated from the area and thickness of the sample. The apparent density is calculated from the mass and volume of the sample. The porosity is calculated by the following formula (II). Porosity (%)={1-ρ / ρ0}×100 (II) "ρ" denotes the apparent density of the sample. "ρ0" indicates the true density of the polymer material (the constituent material of the sample).

[0049] Whether a liquid material is a "good solvent" or a "poor solvent" for a polymeric material can be specified by the following criteria: If 2.5 parts by mass or more of the polymeric material can be dissolved in 100 parts by mass of the liquid material, the liquid material is considered to be a good solvent. If 1 part by mass or more of the polymeric material is not dissolved in 100 parts by mass of the liquid material, the liquid material is considered to be a poor solvent.

[0050] The hourly rate of current is represented by the symbol "C." A current of "1C" discharges the rated capacity of the battery in one hour. In charge and discharge conditions, "CC (Constant Current)" refers to the constant current method, and "CCCV (Constant Current - Constant Voltage)" refers to the constant current - constant voltage method.

[0051] The term "electrode" is a general term for positive and negative electrodes. The electrode may be a positive electrode or a negative electrode.

[0052] The "average degree of polymerization" can be measured by a common method. For example, the average degree of polymerization of a polymer material may be measured by NMR (Nuclear Magnetic Resonance).

[0053] A "water-insoluble polymer" refers to a polymer that has a solubility in water at 25°C, in terms of mass fraction, of less than 1%. The solubility of a water-insoluble polymer may be 0.5% or less, 0.2% or less, or 0.1% or less. A "water-soluble polymer" refers to a polymer that has a solubility in water at 25°C, in terms of mass fraction, of 1% or more.

[0054] <Porous polymer membrane> FIG. 2 is a schematic cross-sectional view showing a polymer porous membrane in this embodiment. The porous membrane 5 includes a first layer 1 and a second layer 2. The porous membrane 5 can be used for any purpose. The porous membrane 5 can have any membrane properties depending on the purpose. For example, the separator and the electrode framework described below may have different suitable membrane properties.

[0055] Film Thickness The porous membrane 5 may have a thickness of, for example, 1 to 100 μm, may have a thickness of 5 to 50 μm, may have a thickness of 10 to 30 μm, or may have a thickness of 16 to 25 μm.

[0056] 《Breathability》 The porous membrane 5 may have an air permeability of, for example, 10 to 1000 s / 100 ml, 32 to 600 s / 100 ml, 125 to 385 s / 100 ml, or 125 to 300 s / 100 ml.

[0057] 《Porosity》 The porous membrane 5 may have a porosity of, for example, 10 to 90%, may have a porosity of 40 to 80%, may have a porosity of 50 to 80%, may have a porosity of 50 to 72%, or may have a porosity of 64 to 72%.

[0058] "composition" The porous membrane 5 may be made of any polymeric material. The polymeric material may be, for example, water-insoluble or water-soluble. The polymeric material may be electrically insulating. The polymeric material may be, for example, non-ion conductive. The polymeric material may be, for example, non-swelling. The polymeric material may include, for example, at least one selected from the group consisting of EVOH, PVDF, and PVA.

[0059] 《1st layer》 The first layer 1 is a base layer of the porous film 5. The porous film 5 may include a second layer 2 that is more than 0% and less than 10% of the thickness, and the first layer 1 that is the remainder. The first layer 1 is porous. The first layer 1 has a three-dimensional mesh structure. For example, the three-dimensional mesh structure may be formed by partial overlapping of bubble-like pores. That is, the three-dimensional mesh structure may include a continuous pore structure. The average pore size in the first layer 1 may be, for example, 100 to 5000 nm, 500 to 2000 nm, or 500 to 1000 nm.

[0060] 《Second layer》 The second layer 2 is a surface layer of the porous membrane 5. The second layer 2 is formed on one of the main surfaces of the porous membrane 5. The second layer 2 is laminated on the first layer 1. The second layer 2 is non-porous when observed at 50,000 times. The second layer 2 has ion permeability. The second layer 2 can inhibit the growth of dendrites.

[0061] The proportion of the second layer 2 is more than 0% and less than 10%. The proportion of the second layer 2 may be, for example, 2 to 8%, 2 to 7%, 2 to 6%, or 2 to 5%. The proportion of the second layer 2 may be, for example, 4 to 8%, 5 to 8%, 6 to 8%, or 7 to 8%.

[0062] The second layer 2 may have a thickness of, for example, 0.1 to 2 μm, 0.5 to 1.5 μm, 0.5 to 1.0 μm, or 1.0 to 1.5 μm.

[0063] <Method of manufacturing porous polymer membrane> Fig. 3 is a schematic flow chart of the method for producing a porous polymer membrane in this embodiment. Hereinafter, "the method for producing a porous polymer membrane in this embodiment" may be abbreviated as "this production method". This production method includes "(a) preparation of a polymer solution", "(b) formation of a liquid membrane", and "(c) drying".

[0064] (a) Preparation of polymer solution The present manufacturing method includes preparing a polymer solution by mixing a polymer material with a good solvent and a poor solvent. The polymer material may have an average degree of polymerization of, for example, 70 to 500,000, or 100 to 200,000.

[0065] The good solvent and the poor solvent are selected according to the type of polymer material. The poor solvent has a higher boiling point than the good solvent. The boiling point of the poor solvent may be, for example, 10°C or more higher than the boiling point of the good solvent. The boiling point of the poor solvent may be, for example, 90 to 300°C higher than the boiling point of the good solvent.

[0066] For example, when the polymer material is EVOH, PVA, etc., the good solvent may include at least one selected from the group consisting of water, alcohol, and dimethyl sulfoxide (DMSO). The good solvent may include at least one selected from the group consisting of water, n-propyl alcohol (nPA), and iso-propyl alcohol (iPA). The poor solvent may include at least one selected from the group consisting of cyclic esters, alcohols, diols, and ethers. The poor solvent may include at least one selected from the group consisting of γ-butyrolactone (GBL), hexylene glycol (HG), and diethylene glycol monomethyl ether (DEGEE).

[0067] For example, when the polymer material is PVDF or the like, the good solvent may include at least one selected from the group consisting of N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF) and DMSO. The poor solvent may include at least one selected from the group consisting of alcohol and ether. The poor solvent may include at least one selected from the group consisting of 1,4-butanediol and glycerin.

[0068] The polymer material, the good solvent, and the poor solvent are mixed in a predetermined ratio. The amount of the good solvent may be, for example, 2 to 10 parts by mass, 4 to 8 parts by mass, or 5 to 6.6 parts by mass, relative to 1 part by mass of the polymer material. The amount of the poor solvent may be, for example, 1 to 5 parts by mass, 1 to 3 parts by mass, 1.5 to 2.3 parts by mass, or 1.5 to 2.0 parts by mass, relative to 1 part by mass of the polymer material.

[0069] The polymer material, the good solvent, and the poor solvent are mixed so that the polymer material is completely dissolved. To promote dissolution of the polymer material, for example, the polymer solution may be heated. The heating temperature may be, for example, 80 to 90°C. After the polymer material is dissolved, the polymer solution may be cooled to room temperature (25°C). The polymer solution may form a homogeneous phase.

[0070] (b) Formation of a liquid film The present manufacturing method includes forming a liquid film of a polymer solution. For example, the liquid film may be formed by applying the polymer solution to the surface of a substrate. Any application method may be used. For example, the polymer solution may be applied by a casting method, a spin coating method, or the like. For example, the thickness of the polymer porous film can be adjusted by the thickness of the liquid film. The substrate may be, for example, a metal foil, or the like. The substrate may be, for example, an electrode for a battery.

[0071] 《(c)Drying》 This production method includes producing a polymer porous membrane by drying the liquid membrane. Any drying method may be used. For example, the liquid membrane may be dried on a hot plate. The drying temperature may be, for example, 80 to 150° C. By drying the liquid membrane, a porous membrane 5 can be formed. For example, it is considered that a three-dimensional network structure is formed by the following mechanism.

[0072] During drying, the good solvent may evaporate before the poor solvent. This is because the boiling point of the poor solvent is higher than that of the good solvent. The reduction in the good solvent relatively increases the concentration of the poor solvent in the polymer solution. Since the polymer material is selectively dissolved in the good solvent, separation between a phase consisting of the polymer material and the good solvent and a phase consisting of the poor solvent is promoted. This separation may be spinodal decomposition. The phase separation causes the polymer material to form a skeleton of a three-dimensional network structure. In the early stage of drying, the solvent rich in the good solvent evaporates. As the drying progresses, the ratio of the poor solvent increases. In the later stage of drying, the solvent rich in the poor solvent evaporates. As the solvent decreases, the polymer material precipitates. Furthermore, pores are formed as the poor solvent evaporates.

[0073] The porous membrane 5 is formed to include a first layer 1 and a second layer 2. In this manufacturing method, various conditions are adjusted so that the ratio of the second layer 2 is more than 0% and less than 10%. For example, the ratio of the second layer 2 can be adjusted by combining the "types of polymeric material, good solvent, and poor solvent," the "combination of materials," the "mixing ratio of materials," and the "drying conditions," etc.

[0074] After the porous membrane 5 is formed, the substrate may be removed. For example, when the substrate is a metal foil, the metal foil may be removed by an etching solution. By removing the substrate, the porous membrane 5 (self-supporting membrane) may be formed. For example, the porous membrane 5 may be formed on the surface of an electrode to produce an electrode unit.

[0075] <First battery> The porous membrane 5 can be used as, for example, a separator. FIG. 4 is a schematic cross-sectional view showing the configuration of the first battery in this embodiment. The first battery 100 may be, for example, a lithium ion secondary battery. The first battery 100 may include a sealed container (not shown). The sealed container may contain a first electrode 10, a separator 30, a second electrode 20, and an electrolyte (not shown). The second electrode 20 has a polarity different from that of the first electrode 10. For example, when the first electrode 10 is a positive electrode, the second electrode 20 is a negative electrode. The first electrode 10 may be a negative electrode or a positive electrode. Each electrode includes an active material. Each electrode may include, for example, an insertion material. The positive electrode may include, for example, lithium nickel cobalt manganese oxide (NCM), etc. The negative electrode may include, for example, natural graphite (NG), etc. Each electrode may further include, for example, a conductive material. Each electrode may include, for example, acetylene black (AB) or the like. Each electrode may further include, for example, a binder. Each electrode may include, for example, PVDF, carboxymethyl cellulose (CMC), styrene butadiene rubber (SBR) or the like.

[0076] The electrolyte solution includes, for example, a lithium (Li) salt and a solvent. The Li salt may include, for example, LiPF6. The concentration of the Li salt may be, for example, 0.5 to 2 mol / L. The solvent may include, for example, at least one selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), and diethyl carbonate (DEC).

[0077] <Battery separator> At least a portion of the separator 30 is interposed between the first electrode 10 and the second electrode 20. The separator 30 separates the second electrode 20 from the first electrode 10.

[0078] The separator 30 includes a porous membrane 5. The separator 30 may be composed of a single porous membrane 5. The separator 30 may include a plurality of porous membranes 5. For example, the separator 30 may be formed by stacking a plurality of porous membranes 5. For example, a plurality of porous membranes 5 may be stacked in order such that the first layer 1 is stacked on the second layer 2. For example, two porous membranes 5 may be stacked such that the second layers 2 are in contact with each other. In this case, the second layer 2 is disposed near the center of the separator 30.

[0079] The separator 30 may further include an additional component in addition to the porous membrane 5. For example, a heat-resistant layer (not shown) may be formed on the surface of the porous membrane 5. For example, the heat-resistant layer may be formed by applying ceramic particles to the surface of the porous membrane 5.

[0080] The porous film 5 includes a first layer 1 (porous layer) and a second layer 2 (non-porous layer). By interposing the second layer 2 between the positive electrode and the negative electrode, it is expected that the short circuit resistance will be improved. This is thought to be because the second layer 2 inhibits the growth of dendrites extending from the negative electrode toward the positive electrode. By making the proportion of the second layer 2 less than 10%, a desired battery resistance can be achieved. The second layer 2 may face either the positive electrode or the negative electrode.

[0081] 《Electrode unit》 The separator 30 (porous membrane 5) may be attached to the surface of the first electrode 10. The separator 30 is integrated with the first electrode 10 to form an electrode unit 40. That is, the electrode unit 40 includes the porous membrane 5 and the first electrode 10. Of course, the first electrode 10 may be a positive electrode or a negative electrode. For example, the electrode unit 40 can be manufactured by manufacturing the porous membrane 5 on the surface of the first electrode 10 as a base material. By integrating the separator 30 with the electrode, for example, a reduction in the number of parts and simplification of battery assembly can be expected.

[0082] The first electrode 10 may include, for example, a first current collector 11 and a first active material layer 12. The first current collector 11 may include, for example, a metal foil or the like. The first current collector 11 may include, for example, an aluminum (Al) foil or the like. The first active material layer 12 includes an active material. The active material may be particles. The first active material layer 12 may further include, for example, a conductive material, a binder, or the like. The porous membrane 5 may be attached to, for example, a surface of the first active material layer 12.

[0083] <Second battery> The porous membrane 5 can be used as, for example, an electrode framework. FIG. 5 is a schematic cross-sectional view showing the configuration of the second battery in this embodiment. The second battery 200 is of a dissolution deposition type. The second battery 200 may be, for example, a lithium metal secondary battery. The second battery 200 may include a sealed container (not shown). The first electrode 10, the second electrode 20, and an electrolyte (not shown) may be stored in the sealed container. A separator 30 may be disposed between the first electrode 10 and the second electrode 20. The separator 30 may include, for example, a polyolefin porous membrane, a nonwoven fabric, or the like. The separator 30 may be manufactured by, for example, a stretching method.

[0084] The second electrode 20 has a polarity different from that of the first electrode 10. The second electrode 20 may be, for example, a negative electrode. The second electrode 20 includes an electrode framework 23. The second electrode 20 may further include a second current collector 21. The second current collector 21 may include, for example, a copper (Cu) foil or the like. The electrode framework 23 may be supported by the second current collector 21. The electrode framework 23 may be attached to a surface of the second current collector 21.

[0085] The second electrode 20 contains a dissolution-precipitation type active material. The active material may contain, for example, at least one selected from the group consisting of Li metal, magnesium (Mg) metal, calcium (Ca) metal, and Al metal.

[0086] The electrode framework 23 includes a porous membrane 5. The porous membrane 5 includes a first layer 1 (porous layer) and a second layer 2 (non-porous layer). When the second electrode 20 is charged, a metal (active material) may be precipitated in the voids in the first layer 1. When the second electrode 20 is discharged, a metal may be dissolved in the electrolyte in the voids in the first layer 1. A dissolution-precipitation type active material (metal) tends to easily form dendrites during precipitation. It is expected that the precipitation of the metal in the voids (bubble-like pores) of the first layer 1 will result in the precipitation of the metal in a lump-like form.

[0087] Normally, the volume of a dissolution-precipitation type electrode changes significantly with charging and discharging (dissolution and precipitation of metal). It is expected that the volume change of the second electrode 20 will be mitigated by the occurrence of dissolution and precipitation of metal in the first layer 1 (three-dimensional network structure).

[0088] Furthermore, since the porous film 5 includes the second layer 2 (non-porous layer), it is expected that the metal will be confined within the first layer 1. By confining the metal within the first layer 1, it is expected that, for example, the cycle life will be improved. EXAMPLES

[0089] <Experiment 1> In Experiment 1, porous membranes according to Nos. 1 to 8 were produced using a water-insoluble polymer as a raw material. Hereinafter, for example, the "porous membrane according to No. 1" may be abbreviated as "No. 1."

[0090] <Production of porous membrane> No.1 The following materials were prepared: Polymer material: EVOH (product name "EVAL L171B", manufactured by Kuraray Co., Ltd.) Good solvent: water, nPA, iPA Poor solvent: GBL, HG Base material: Cu foil

[0091] A sample vessel was charged with 1 part by weight of EVOH, 3.3 parts by weight of water, 3.3 parts by weight of iPA, and 2.0 parts by weight of HG. The sample vessel was heated to 80-90°C. The mixture was stirred at 350 rpm until the EVOH was completely dissolved as confirmed by visual inspection. This resulted in a polymer solution. The polymer solution was then cooled to 25°C.

[0092] The cooled polymer solution was applied to the surface of the substrate by a casting method. This formed a liquid film. The substrate with the liquid film was placed in a hot plate dryer (set temperature: 100°C). The liquid film was dried for 20 minutes. The good solvent and poor solvent evaporated, forming a porous film on the surface of the substrate. The porous film was separated from the substrate by an etching solution.

[0093] No.2~8 As shown in Table 1 below, except that the type and amount of good solvent, the type and amount of poor solvent, and the drying temperature were changed, porous membranes were produced in the same manner as in No. 1. It can be seen that the ratio of the second layer changes depending on the various conditions.

[0094] "evaluation" Film properties The "thickness of the porous membrane," "porosity," "air permeability," and "average pore size" were measured by the above-mentioned methods. The results are shown in Table 1 below. In the "air permeability" column, ">600" indicates that the value is greater than 600, and "10<" indicates that the value is less than 10.

[0095] Second layer ratio The "thickness of the second layer" and "proportion of the second layer" were measured by the above-mentioned method. The results are shown in Table 1 below.

[0096] Battery characteristics The DC internal resistance was measured for a test battery (coin cell). The test battery had the following configuration:

[0097] positive electrode Shape: Disc (diameter: 14mm) Composition of active material layer: NCM / AB / PVDF=88.8 / 9.4 / 1.8 (mass ratio) Current collector: Aluminum foil

[0098] Separator Shape: Disc (diameter: 19mm) Composition: Porous membranes related to Nos. 1 to 8 Orientation: The porous membrane is placed between the positive and negative electrodes, with the second layer facing the negative electrode.

[0099] negative electrode Shape: Disc (diameter: 16mm) Composition: NG / SBR / CMC=98.8 / 0.7 / 0.5 (mass ratio) Current collector: Cu foil

[0100] electrolyte Li salt: LiPF6 (concentration: 1.1 mol / L) Solvent: EC / DMC / EMC=3 / 4 / 3 (volume ratio)

[0101] The internal resistance of the test battery was measured under the following conditions. 1C corresponds to 1.5mA.

[0102] First charge / discharge Ambient temperature: 25℃ CCCV charging: 0.2C, 4.1V CC discharge: 0.2C, 3.0V

[0103] Resistance measurement After the initial charge / discharge, the battery was charged / discharged again under the following conditions. Ambient temperature: 25℃ CCCV charging: 0.2C, 4.1V CC discharge: 0.2C, 3.0V

[0104] The DC internal resistance was calculated from the difference between the voltage at the start of discharge and the voltage 10 seconds after the start of discharge. The DC internal resistance component from 0 to 0.1 seconds was considered to be "DC + reaction resistance." The DC internal resistance component from 0.1 to 10 seconds was considered to be "diffusion resistance."

[0105] [Table 1]

[0106] "result" 6 shows SEM images of the cross section and surface of Nos. 1 to 5. In Nos. 1 to 5, a thin second layer (non-porous layer) was formed on the outermost surface of the porous membrane.

[0107] FIG. 7 shows cross-sectional and surface SEM images of Nos. 6 to 8. In No. 6, a thick second layer (non-porous layer) was formed on the outermost surface of the porous membrane. In Nos. 7 and 8, open pores were confirmed on the surface of the porous membrane. That is, in Nos. 7 and 8, the second layer (non-porous layer) was not formed.

[0108] FIG. 8 is a graph showing the measurement results of the DC internal resistance. No. 6 has a very high DC internal resistance. In No. 6, the proportion of the second layer is 10% or more (see Table 1 above). Nos. 1 to 5 showed the desired DC internal resistance. In Nos. 1 to 5, the proportion of the second layer is less than 10% (see Table 1 above). Note that Nos. 7 and 8 were short-circuited during the initial charge, so the DC internal resistance was not measured.

[0109] Figure 9 is a graph showing the results of the initial charge and discharge. No. 7 shorted during charging. No. 7 had a 0% second layer ratio (see Table 1 above). No. 1 was able to be charged and discharged. No. 1 had a 0% second layer ratio (see Table 1 above).

[0110] <Experiment 2> In Experiment 2, porous membranes Nos. 9 to 11 were produced using a water-soluble polymer as a raw material.

[0111] <Production of porous membrane> No.9 The following materials were prepared: Polymer material: PVA (product name "Poval PVA117", manufactured by Kuraray Co., Ltd.) Good solvent: Water Antisolvent: DEGEE Base material: Cu foil

[0112] 1.5 parts by mass of PVA, 10 parts by mass of water, and 6 parts by mass of DEGEE were added to a sample container. The sample container was heated to 80-90°C. The mixture was stirred at 350 rpm until the PVA was completely dissolved as confirmed by visual inspection. This resulted in a polymer solution. The polymer solution was then cooled to 25°C.

[0113] The cooled polymer solution was applied to the surface of the substrate by a casting method. This formed a liquid film. The substrate with the liquid film was placed in a hot plate dryer (set temperature: 140°C). The liquid film was dried for 20 minutes. The good solvent and poor solvent evaporated, forming a porous film on the surface of the substrate. The porous film was separated from the substrate by an etching solution.

[0114] No.10, 11 As shown in Table 2 below, except that the amount of poor solvent used and the drying temperature were changed, a porous membrane was produced in the same manner as in No. 1. It can be seen that the ratio of the second layer changes depending on the various conditions.

[0115] "evaluation" The "thickness of the porous membrane," "porosity," and "proportion of the second layer" were measured by the above-mentioned methods. The results are shown in Table 2 below.

[0116] [Table 2]

[0117] "result" 10 shows cross-sectional SEM images of Nos. 9 to 11. It can be seen that even when a water-soluble polymer is used as the raw material, a porous membrane including a first layer and a second layer can be produced.

[0118] The present embodiment and the present embodiment are illustrative in all respects. The present embodiment and the present embodiment are not restrictive. The technical scope of the present disclosure includes all modifications within the meaning and scope equivalent to the description of the claims. For example, it is also intended from the beginning that any configuration may be extracted from the present embodiment and the present embodiment, and that they may be arbitrarily combined. [Explanation of symbols]

[0119] 1 first layer, 2 second layer, 5 porous membrane, 10 first electrode, 20 second electrode, 21 current collector, 22 active material layer, 23 electrode framework, 30 separator, 40 electrode unit, 100 first battery, 200 second battery.

Claims

1. A first electrode; A second electrode; An electrolyte; Including, the second electrode has a polarity different from that of the first electrode; the second electrode comprises an electrode framework; the electrode framework comprises a porous polymer membrane; The porous polymer membrane includes a first layer and a second layer, the first layer is porous; The first layer has a three-dimensional network structure, the second layer is non-porous in an image magnified at 50,000 times; The following formula (I): Proportion (%) of the second layer = (t 2 / t 0 ) × 100 (I) (t 0 represents the thickness of the porous polymer membrane, and t 2 indicates the thickness of the second layer.) The ratio of the second layer calculated by is greater than 0% and less than 10%, The second electrode is configured to be charged by a deposition reaction of a metal in the voids in the first layer, and to be discharged by a dissolution reaction of the metal. battery.

2. The second layer has a percentage of 2 to 8%.

10. The battery of claim 1.

3. The second layer has a thickness of 0.5 to 1.5 μm. The battery according to claim 1 or 2.

4. The first layer has an average pore size of 500 to 2000 nm. The battery according to any one of claims 1 to 3.

5. The three-dimensional network structure of the polymer porous membrane includes a continuous pore structure. The battery according to any one of claims 1 to 4.

6. The porous polymer membrane contains at least one selected from the group consisting of an ethylene-vinyl alcohol copolymer, polyvinylidene fluoride, and polyvinyl alcohol. The battery according to any one of claims 1 to 5.

7. The porous polymer membrane has an air permeability of 32 to 600 s / 100 ml. The battery of any one of claims 1 to 6.

8. The porous polymer membrane has a porosity of 50 to 72%. The battery of any one of claims 1 to 7.

9. The porous polymer membrane has a thickness of 16 to 25 μm. The battery of any one of claims 1 to 8.

10. (a) preparing a polymer solution by mixing a polymer material with a good solvent and a poor solvent; (b) forming a liquid film of the polymer solution; and (c) drying the liquid membrane to produce a porous polymer membrane; Including, The poor solvent has a boiling point higher than that of the good solvent, The porous polymer membrane includes a first layer and a second layer, the first layer is porous; The first layer has a three-dimensional network structure, the second layer is non-porous in an image magnified at 50,000 times; The following formula (I): Proportion (%) of the second layer = (t 2 / t 0 ) × 100 (I) (t 0 represents the thickness of the porous polymer membrane, and t 2 indicates the thickness of the second layer.) The ratio of the second layer calculated by is greater than 0% and less than 10%. A method for producing a porous polymer membrane.

Citation Information

Patent Citations

  • Fixed dopant p type conducting polymer positive electrode battery

    JP1990174076A

  • Secondary battery

    JP1999097069A

  • Lithium secondary battery

    JP2021005504A

  • Composite hollow fiber membrane and hollow fiber membrane module

    WO2013147187A1

  • Lithium secondary battery

    WO2021039242A1